Method for forming multi-layer coating film
A multilayer coating film is formed using vapor-deposited aluminum pigment and specific organic solvents to enhance adhesion and achieve a satin-like appearance, addressing adhesion and equipment limitations in existing methods.
Patent Information
- Application Number
- JP2023057172
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing methods for forming plated satin-like appearances on substrates face challenges such as insufficient adhesion to the base material, require additional primer coatings, and are limited by equipment requirements, especially when applying clear paints on uncured metallic coatings.
A method involving the application of a metallic coating containing vapor-deposited aluminum pigment coated with an inorganic oxide, followed by a top coat with specific organic solvents, is used to form a multilayer coating film with excellent adhesion and satin-like appearance, eliminating the need for a primer and utilizing wet-on-wet painting to reduce environmental impact.
The method achieves excellent adhesion to the base material and a high-quality plated satin-like appearance without a primer, while reducing equipment needs and environmental impact through simultaneous drying of uncured films.
Smart Images

Figure 2024144969000001 
Figure 2024144969000002 
Figure 2024144969000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for forming a multi-layer coating film for imparting a plated satin appearance to the surface of a substrate. [Background technology]
[0002] Plated parts are widely used in automobile interior parts, home appliances, bicycles, fishing tackle, etc. to give them a high level of design. However, the production of plated parts requires equipment costs from pre-treatment to wastewater treatment, and the colors and material shapes that can be expressed in terms of design are limited, so methods of painting with a plated look and forming multi-layered paint films with a plated look are being studied. Among them, a satin-plated look has a calm texture and is often used for car interior parts and emblems.
[0003] JP 2010-247055 A (Patent Document 1) describes a coating film forming method in which a metallic base paint containing 30-70% by mass of non-leafing vapor-deposited aluminum pigment based on the paint solid content is applied onto a plastic material, a two-liquid type acrylic urethane clear paint is applied on top of that, and the formed multi-layer coating film is cured at the same time. There is no description of surface treatment for the vapor-deposited aluminum pigment used in the metallic base paint described in Patent Document 1, and there is room for improvement in adhesion to the substrate due to insufficient strength of the coating film. Furthermore, there is also a problem that it is difficult to obtain the desired plated appearance because the clear paint is applied onto an uncured metallic base coating film.
[0004] Japanese Patent Application Laid-Open No. 2003-053260 (Patent Document 2) describes a method for forming a plated coating in which a colored base coating, an active energy ray-curable metallic coating, and a clear coating are applied in this order onto a substrate such as an automobile part. The plated coating described in Patent Document 2 requires a base coating, and when applied directly to a plastic substrate, the adhesion is insufficient. In addition, the metallic coating is cured by active energy rays, so equipment such as an ultraviolet ray irradiation device is required.
[0005] Japanese Patent Application Laid-Open No. 2020-157691 (Patent Document 3) describes a method for manufacturing a decorative film molded body having a satin-plated appearance. The decorative film molded body described in Patent Document 3 forms a metallic layer on an adhesive layer by deposition rather than painting, which requires equipment such as a vacuum deposition device, and also imposes restrictions on the size and shape of the substrate on which the metallic layer is formed. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2010-247055 A [Patent Document 2] JP 2003-053260 A [Patent Document 3] JP 2020-157691 A Summary of the Invention [Problem to be solved by the invention]
[0007] Therefore, an object of the present invention is to provide a method for forming a multilayer coating film that has excellent adhesion to a substrate without the need for a primer coating film and has an excellent plated satin appearance even when a clear paint is applied over an uncured metallic coating film. [Means for solving the problem]
[0008] As a result of intensive research into achieving the above-mentioned object, the inventors have discovered that by applying a metallic paint containing at least a vapor-deposited aluminum pigment coated with an inorganic oxide onto a substrate, and then applying a topcoat paint containing a specific amount of an organic solvent having a specific SP value and evaporation rate, and drying them simultaneously, it is possible to form a multi-layer coating film which has excellent adhesion to the substrate and an excellent plated satin appearance, and have completed the present invention.
[0009] Therefore, one aspect of the present invention is a method for forming a multilayer coating film, which includes at least a metallic coating film forming step of applying a metallic paint (I) onto a substrate to form an uncured metallic coating film, a topcoat coating film forming step of applying a topcoat paint (II) onto the uncured metallic coating film to form an uncured topcoat coating film, and a drying step of simultaneously drying the uncured metallic coating film and the topcoat coating film to form a multilayer coating film, wherein the metallic paint (I) contains a resin (IA), an organic solvent (IB), and at least an evaporated aluminum pigment (IC) coated with an inorganic oxide, and the topcoat paint (II) contains a resin (II-A) and an organic solvent (II-B), and the organic solvent (II-B1) has an SP value of 8.0 to 9.0 and an evaporation rate of 0.1 or more and less than 1.0 when butyl acetate is taken as 1.0, and is 10 to 30 mass % relative to the total amount of the organic solvent (II-B).
[0010] In a preferred embodiment of the method for forming a multilayer coating film in the present invention, the organic solvent (II-B2) having an SP value of 9.0 to 10.0 and an evaporation rate of 2.0 or more and less than 6.0, where butyl acetate is taken as 1.0, is further contained in an amount of 20 to 50 mass % based on the total amount of the organic solvent (II-B).
[0011] In a preferred embodiment of the method for forming a multilayer coating film in the present invention, the water content in the metallic paint (I) is less than 3.0 mass %, and the inorganic oxide coating the vapor-deposited aluminum pigment (IC) contains at least silica. Effect of the Invention
[0012] According to the present invention, a method for forming a multilayer coating film can be provided which has excellent adhesion to a substrate without the need for a primer coating film, and has an excellent plated satin appearance even when a clear paint is applied onto an uncured metallic coating film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The method for forming the multi-layer coating film of the present invention will be explained in detail below, but the present invention is not limited thereto.
[0014] <Method of forming multi-layer coating film> The method for forming a multilayer coating film in the present invention is characterized by having at least a metallic coating film forming step of applying a metallic paint (I) onto a substrate to form an uncured metallic coating film, a topcoat coating film forming step of applying a topcoat paint (II) onto the uncured metallic coating film to form an uncured topcoat coating film, and a drying step of simultaneously drying the uncured metallic coating film and the topcoat coating film to form a multilayer coating film.
[0015] <Metal coating formation process> This step is a step of applying the metallic paint (I) onto a substrate to form an uncured metallic coating film.
[0016] <Base material> The substrate of the present invention is not particularly limited, but is preferably a plastic substrate. Examples of the plastic substrate include polyphenylene ether resins; polystyrene resins; polyolefin resins such as polypropylene and polyethylene; polyester resins such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polycarbonate resins; acrylic resins such as polymethyl methacrylate; and ABS resins. In addition, substrates of various shapes can be selected according to the application of the painted body, and examples thereof include plastic molded bodies used for automobile interior parts and plastic films having an adhesive layer. Furthermore, in order to highlight the appearance of the plated satin tone, it is more preferable that the color of the substrate is black.
[0017] <Metallic paint (I)> The metallic paint (I) of the present invention is characterized by containing a resin (IA), an organic solvent (IB), and at least a vapor-deposited aluminum pigment (IC) coated with an inorganic oxide.
[0018] <<Resin (IA)>> The resin (IA) used in the metallic paint (I) is not particularly limited, and may be a normal acrylic resin, cellulose resin, polyester resin, urethane resin, vinyl chloride resin, etc., and is preferably an acrylic resin or a cellulose resin. The content of the resin (IA) is 10 to 90 mass% of the solid content in the metallic paint (I), and preferably 50 to 90 mass%. Here, the solid content refers to the components remaining in the coating film when the coating film is formed.
[0019] The acrylic resin is preferably a polymer or copolymer mainly composed of an acrylic acid ester or a methacrylic acid ester. Here, the term "main component" means that the resin is contained in an amount of 50 mol% or more. In the present invention, it is preferable that 90 mass% or more of the acrylic resin has a hydroxyl value of less than 5 mg / KOHg, and it is preferable that the acrylic resin has fewer hydroxyl groups. In addition, it is preferable that the glass transition temperature (hereinafter, Tg) is 50° C. or more.
[0020] In the present invention, Tg is calculated using the following FOX formula.
[0021] 1 / Tg=W1 / Tg1+W2 / Tg2+···+Wi / Tgi+···+Wn / Tgn In the above FOX equation, Tg is the glass transition temperature (K) of a polymer consisting of n types of monomers, Tg(1, 2, i, n) is the glass transition temperature (K) of a homopolymer of each monomer, W(1, 2, i, n) is the mass fraction of each monomer, and W1+W2+···+Wi+···+Wn=1.
[0022] Examples of cellulose resins include cellulose ether, cellulose ester, nitrocellulose, acrylic modified cellulose derivatives, polyester modified cellulose derivatives, and polyurethane modified cellulose derivatives, and nitrocellulose is particularly preferred. The nitrogen content of nitrocellulose is preferably 10% or more. Specifically, commercially available industrial nitrocellulose (manufactured by TNC INDUSTRIAL) can be used.
[0023] <<Organic solvent (IB)>> The organic solvent (IB) used in the metallic paint (I) can be any solvent normally used in paints, without any restrictions. For example, aromatic hydrocarbon solvents such as toluene and xylene, ketones such as methyl ethyl ketone, methyl isobutyl ketone, diethyl ketone, butyl methyl ketone, and diisobutyl ketone, ester solvents such as ethyl acetate, butyl acetate, isobutyl acetate, and 2-methoxypropyl acetate, glycol ester solvents such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, and diethylene glycol monobutyl ether, 2-methoxyethyl acetate, 2-ethoxyethyl acetate, 3-methoxy-3-methylbutanol, 3-methoxy-3-methylbutyl acetate, 1-methoxy-2-propanol, 1-methoxypropyl-2-acetate, and 3-methoxy-1-butyl acetate, alcohol solvents such as butyl alcohol, isobutyl alcohol, isopropyl alcohol, and 1-methoxy-2-propanol, molecular formula C n H 2n+2 Examples of the organic solvent include paraffin-based hydrocarbon solvents such as octane, nonane, decane, dodecane, and tetradecane, which are saturated chain compounds having a straight chain or branched structure and can be represented by the formula: and naphthenic hydrocarbon solvents such as cyclohexane and methylcyclohexane. As the organic solvent (IB), it is preferable to use a combination of two or more kinds of organic solvents, taking into consideration the solubility in the resin (IA) and the evaporation rate of the organic solvent.
[0024] Here, the evaporation rate of an organic solvent in the present invention is a value measured based on the relative evaporation rate when butyl acetate is set to 1. The evaporation rate is measured based on ASTM D3539-11.
[0025] The organic solvent (IB) preferably contains an organic solvent having an evaporation rate of 3.0 or more in an amount of 50 to 90 mass% based on the total amount of the organic solvent (IB). If the content of the organic solvent having an evaporation rate of 3.0 or more is within the above range, the volume of the coating film shrinks due to the evaporation of the organic solvent, and the evaporated aluminum pigment (IC) in the metallic coating film is easily oriented, so that a metallic coating film having a better appearance can be formed. In addition, since the amount of the organic solvent (IB) contained in the uncured metallic coating film is reduced, the orientation of the evaporated aluminum pigment (IC) is less likely to be disturbed even when the topcoat paint (II) is applied, so that a multi-layer coating film having a better plated satin appearance can be formed. Examples of organic solvents having an evaporation rate of 3.0 or more include methyl ethyl ketone, methyl acetate, ethyl acetate, cyclohexane, methylcyclohexane, heptane, etc.
[0026] Furthermore, the organic solvent (IB) preferably contains an organic solvent having an evaporation rate of 0.2 or less in an amount of 1.0 to 10 mass % based on the total amount of the organic solvent (IB). If the content of the organic solvent having an evaporation rate of 0.2 or less is within the above range, a small amount of the organic solvent remains in the uncured metallic coating film, so that the vapor-deposited aluminum pigment (IC) is easily distributed uniformly in the resin (IA), and a metallic coating film having an excellent appearance with little color unevenness can be formed. Examples of the organic solvent having an evaporation rate of 0.2 or less include diisobutyl ketone, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, 3-methoxy-3-methylbutanol, 3-methoxy-3-methylbutyl acetate, and 3-methoxy-1-butyl acetate.
[0027] << Vapor-deposited aluminum pigment (IC) >> The vapor-deposited aluminum pigment (IC) used in the metallic paint (I) is a vapor-deposited aluminum pigment having at least a part of its surface coated with an inorganic oxide. By having at least a part of its surface coated with an inorganic oxide, the vapor-deposited aluminum pigment is prevented from coagulating in the coating film, and the coating film strength is improved, making it possible to form a multi-layer coating film with excellent adhesion without the need for a primer coating film. Examples of the inorganic oxide to be coated include silica and titanium oxide, and silica is preferred. In addition to the coating with an inorganic oxide, organic metal treatment using phosphates, molybdates, silane coupling agents, etc. can also be used.
[0028] The vapor-deposited aluminum pigment (IC) preferably has an average particle size of 5 to 15 μm and an aspect ratio of 100 to 5000. Here, the average particle size refers to the 50% particle size (D50) of the volume-based particle size distribution, and can be determined from the particle size distribution measured using a particle size distribution measuring device (for example, a laser diffraction / scattering type particle size distribution measuring device). The particle size of the vapor-deposited aluminum pigment is expressed as the sphere-equivalent diameter measured by the laser diffraction / scattering method. The aspect ratio is expressed as the average particle size / average thickness.
[0029] As the vapor-deposited aluminum pigment (IC) of the present invention, commercially available vapor-deposited aluminum pigments such as METALURE, HYDROSHINE (manufactured by ECKART), SPLENDAL (manufactured by Benda-Lutz), TOYAL SHINE (manufactured by Toyo Aluminum), and DECOMET (manufactured by SCHLENK) can be used. The content of the vapor-deposited aluminum pigment (IC) is 10 to 50 mass % of the solid content in the metallic paint (I), and preferably 15 to 30 mass %. If the content of the vapor-deposited aluminum pigment (IC) is within the above range, a metallic coating film having a better appearance can be formed.
[0030] <<Other additives>> The metallic paint (I) of the present invention can be appropriately blended with additives commonly used in the paint industry, such as surface conditioners, wetting agents, dispersants, emulsifiers, thickeners, anti-settling agents, anti-skinning agents, anti-sagging agents, defoamers, color separation inhibitors, leveling agents, silane coupling agents, drying agents, plasticizers, coloring pigments, extender pigments, rust inhibitors, insecticides, antibacterial agents, antiviral agents, light stabilizers, ultraviolet absorbers, antistatic agents, and conductivity imparting agents, etc., depending on the purpose. The water content in the metallic paint (I) is 3.0% by mass or less, preferably 0.5% by mass or less, based on the total amount of the metallic paint (I), and more preferably substantially free of water.
[0031] <Topcoat film formation process> This process is a topcoat coating film formation process in which a topcoat paint (II) is applied on an uncured metallic coating film to form an uncured topcoat coating film. This process is so-called wet-on-wet painting. By applying wet-on-wet painting, the drying process can be shortened and CO2 emissions can be reduced, which is preferable from the viewpoint of reducing the environmental load.
[0032] <Topcoat paint (II)> The topcoat paint (II) of the present invention is characterized in that it contains a resin (II-A) and an organic solvent (II-B), and contains 10 to 30 mass % of the organic solvent (II-B1) having an SP value of 8.0 to 9.0 and an evaporation rate of 0.1 or more and less than 1.0 when butyl acetate is taken as 1.0, based on the total amount of the organic solvent (II-B).
[0033] Here, the SP value is a guideline for judging compatibility, and there are various calculation and measurement methods. The SP value of the one-liquid coating composition of the present invention is indicated by the solubility parameter calculated by the Hoy method based on the structure. The SP value of the organic solvent is a value calculated using the vapor pressure method proposed by Hoy, in accordance with the method described in the literature [KL Hoy, J. Paint Technology, 42, (541), 76 (1970)].
[0034] <<Resin (II-A)>> The resin (II-A) used in the topcoat paint (II) is not particularly limited, and can be a topcoat paint used for ordinary automobile interior and exterior parts, home appliances, bicycles, fishing tackle, etc. Examples of resins used in the topcoat paint include acrylic resins, fluorine-based resins, urethane resins, epoxy resins, organically modified silicone resins (e.g., acrylic silicone resins), polyester resins, and melamine resins, and it is particularly preferable to use acrylic resins and urethane resins.
[0035] The acrylic resin is not particularly limited, but preferably contains an acrylic resin having a hydroxyl value in the range of 30 to 150 mgKOH / g. When the hydroxyl value is within the above range, it reacts efficiently with a curing agent or a crosslinking agent, making it possible to increase the crosslink density of the coating film, and improving various properties such as water resistance, oil resistance, and chemical resistance.
[0036] The content of the acrylic resin is preferably 40 to 80 mass % based on the paint solid content of the topcoat paint (II). In the present invention, the acrylic resin may be used alone or in combination of two or more kinds.
[0037] In addition, when an acrylic resin is used, an isocyanate resin, an epoxy resin, a melamine resin, etc. can be used as a curing agent. In blending these curing agents, for example, when an isocyanate is used as a curing agent, it is preferable to mix them in the range of OH / NCO=0.5 to 1.5 equivalents.
[0038] Representative examples of isocyanates include diphenylmethane diisocyanate, polymethylene polyphenyl polyisocyanate, toluene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, modified polyisocyanates obtained by modifying these polyisocyanates with urethane, allophanate, carbodiimide or isocyanurate, and mixtures of these.
[0039] <<Organic solvents (II-B)>> The organic solvent (II-B) used in the topcoat paint (II) can be any solvent normally used in paints, without any restrictions. For example, aromatic hydrocarbon solvents such as toluene and xylene, ketones such as methyl ethyl ketone, methyl isobutyl ketone, diethyl ketone, butyl methyl ketone, and diisobutyl ketone, ester solvents such as ethyl acetate, butyl acetate, isobutyl acetate, and 2-methoxypropyl acetate, glycol ester solvents such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, 2-methoxyethyl acetate, 2-ethoxyethyl acetate, 3-methoxy-3-methylbutanol, 3-methoxy-3-methylbutyl acetate, 1-methoxy-2-propanol, 1-methoxypropyl-2-acetate, and 3-methoxy-1-butyl acetate, alcohol solvents such as butyl alcohol, isobutyl alcohol, isopropyl alcohol, and 1-methoxy-2-propanol, molecular formula C n H 2n+2 Examples of the organic solvent include paraffin-based hydrocarbon solvents such as octane, nonane, decane, dodecane, and tetradecane, which are saturated chain compounds having a straight chain and branched structure and can be represented by the formula: and naphthenic hydrocarbon solvents such as cyclohexane and methylcyclohexane. As the organic solvent (II-B), it is preferable to use a combination of two or more kinds, taking into consideration the solubility in the resin (II-A) and the evaporation rate of the organic solvent.
[0040] <<Organic solvents (II-B1)>> The organic solvent (II-B1) is an organic solvent having an SP value of 8.0 to 9.0 and an evaporation rate of 0.1 or more and less than 1.0, and in the present invention, the organic solvent (II-B) contains 10 to 30% by mass based on the total amount of the organic solvent (II-B). The organic solvent (II-B1) does not easily dissolve the resin (IA) contained in the uncured metallic coating film, and has a relatively slow evaporation rate, so that it improves the leveling property of the topcoat paint (II). Therefore, if the organic solvent (II-B1) is in the above range, a multi-layer coating film having an excellent plated satin-like appearance can be formed. If the content of the organic solvent (II-B1) is less than 10% by mass, the uncured metallic coating film is easily dissolved, the orientation of the vapor-deposited aluminum pigment (IC) is disturbed, and an excellent plated satin-like appearance cannot be obtained. On the other hand, if the content of the organic solvent (II-B1) exceeds 30% by mass, the solubility and drying property of the resin (II-A) in the topcoat paint (II) decreases, affecting the workability during painting and the appearance of the coating film after curing. Examples of the organic solvent (II-B1) include xylene (SP value: 9.0, evaporation rate: 0.76) and diisobutyl ketone (SP value: 8.7, evaporation rate: 0.20).
[0041] <<Organic solvents (II-B2)>> The organic solvent (II-B2) is an organic solvent having an SP value of 9.0 to 10.0 and an evaporation rate of 2.0 or more and less than 6.0, and in the present invention, it is preferable that the organic solvent (II-B) contains 20 to 50% by mass based on the total amount of the organic solvent (II-B). Since the organic solvent (II-B2) has high compatibility with the resin (II-A) and a fast evaporation rate, if the organic solvent (II-B2) is in the above range, the drying property and coating workability of the topcoat paint (II) can be improved. Examples of the organic solvent (II-B2) include toluene (SP value: 9.0, evaporation rate: 2.00), benzene (SP value: 9.1, evaporation rate: 4.12), methyl acetate (SP value: 9.7, evaporation rate: 5.10), ethyl acetate (SP value: 9.5, evaporation rate: 4.20), and propyl acetate (SP value: 9.4, evaporation rate: 2.14).
[0042] <<Matte agent>> The topcoat paint (II) of the present invention may contain a matting agent, and the matte finish of the plated satin tone can be adjusted by the amount of the matting agent added. When the matte finish of the plated satin tone is to be enhanced, it is preferable to contain a large amount of the matting agent, and when the matte finish is to be weakened, it is preferable to contain a small amount of the matting agent or to contain no matting agent. When a matting agent is contained, it is preferable that the amount of the matting agent is 0.1 to 10.0 mass % and more preferably 3.0 to 10.0 mass % based on the solid content of the topcoat paint (II).
[0043] The matting agent used in the topcoat paint (II) may be any matting agent commonly used in paints, without any limitation. Examples of the matting agent include silica-based matting agents, resin beads, glass beads, and extender pigments such as talc.
[0044] <<Other additives>> The topcoat paint (II) of the present invention can be appropriately mixed with additives commonly used in the paint industry, such as surface conditioners, wetting agents, dispersants, emulsifiers, thickeners, anti-settling agents, anti-skinning agents, anti-sagging agents, defoamers, color separation inhibitors, leveling agents, silane coupling agents, color pigments, extender pigments, rust inhibitors, drying agents, plasticizers, insecticides, antibacterial agents, antiviral agents, light stabilizers, ultraviolet absorbers, antistatic agents, and conductivity imparting agents, etc., depending on the purpose. In order to obtain a plated satin-like appearance, the topcoat paint (II) is preferably a clear paint that does not substantially contain color pigments or extender pigments, or a color clear paint that contains color pigments, etc. to the extent that it does not lose transparency.
[0045] <Drying process> This process is a process in which the uncured metallic coating film and the topcoat coating film are simultaneously dried to form a multi-layer coating film.
[0046] <<Drying conditions>> In the drying step of the present invention, the substrate is baked and dried at a temperature that does not cause problems such as a decrease in physical strength, thermal deformation, foaming, etc. The baking temperature is preferably 70 to 100°C as the substrate surface temperature, and the baking time is, for example, 10 to 60 minutes, and preferably 20 to 40 minutes.
[0047] <<Painting method>> The coating method is not particularly limited, and includes known coating methods such as dipping, spin coating, flow coating, roll coating, spray coating, blade coating, and air knife coating. Among these, spray coating is preferred from the viewpoint of easy control of the film thickness. The dry film thickness of the metallic coating film in the present invention is 0.1 to 10 μm, and preferably 0.5 to 5 μm. The dry film thickness of the topcoat coating film is 10 to 100 μm, and preferably 15 to 50 μm. EXAMPLES
[0048] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.
[0049] <Preparation of metallic paint (I)> The raw materials were mixed according to the formulation shown in Table 1 and dispersed by a known method to prepare metallic paint (I). The materials used are as follows:
[0050] <<Resin (IA)>> Nitrocellulose solution (industrial nitrocellulose TR7, manufactured by TNC INDUSTRIAL, solid content: 70% by weight, solvent: isopropanol) <<Organic solvent (IB)>> Ethyl acetate (SP value: 9.5, evaporation rate: 4.20) Butyl acetate (SP value: 9.3, evaporation rate: 1.00) Cyclohexane (SP value: 8.8, evaporation rate: 4.50) Isobutanol (SP value: 10.9, evaporation rate: 0.64) Ethylene glycol monobutyl ether (SP value: 11.0, evaporation rate: 0.08) << Vapor-deposited aluminum pigment (IC) >> Vapor-deposited aluminum pigment paste-1 (HYDROSHINE WS-4140, manufactured by BYK Japan, average particle size: 13-15 μm, silica coating, solid content: 10% by mass, solvent: isopropanol / ethylene glycol monobutyl ether) Vapor-deposited aluminum pigment paste-2 (HYDROSHINE WS-4001, manufactured by BYK Japan, average particle size: 9-12 μm, silica coating, solid content: 10% by mass, solvent: isopropanol / ethylene glycol monobutyl ether) Vapor-deposited aluminum pigment paste-3 (Decomet STV2002 12 / 10 S0, manufactured by SCHLENK, average particle size: 12 μm, silica coating and organometallic treatment, solid content: 10% by weight, solvent: isopropanol) <<Other evaporated aluminum pigments>> Vapor-deposited aluminum pigment paste-4 (METALURE C-51010MA, manufactured by ECKART, average particle size: 9 to 11 μm, uncoated, solid content: 10% by mass, solvent: 1-methoxypropyl-2-acetate) Vapor-deposited aluminum pigment paste-5 (METALURE L 55350, manufactured by BYK Japan, average particle size: 11.5 μm, uncoated, solid content: 10% by mass, solvent: ethyl acetate)
[0051] [Table 1]
[0052] <Preparation of topcoat paint (II)> The raw materials were mixed according to the formulation shown in Table 2 and dispersed by a known method to prepare topcoat paint (II). The materials used are as follows. Topcoat paint (II) is used by mixing the base agent, hardener, and diluent immediately before painting.
[0053] [Main ingredient] <<Resin (II-A)>> Acrylic resin solution-1 (Acrydic AC-3734, manufactured by DIC Corporation, hydroxyl value: 13-19 mgKOH / g, solid content: 50% by mass, solvent: isobutyl acetate / butyl acetate) Acrylic resin solution-2 (Acrydic A-851-HP, manufactured by DIC Corporation, hydroxyl value: 66-74 mg KOH / g, solid content: 70% by mass, solvent: butyl acetate) <<Organic solvents (II-B)>> Butyl acetate (SP value: 9.3, evaporation rate: 1.00) <<Additives>> Matting agent (ACEMATT OK607, Evonic, silica) Dispersant (Disparlon DA-7301, manufactured by Kusumoto Chemicals, solid content: 75%) -UV absorber (TINUVIN292, manufactured by BASF) Light stabilizer (TINUVIN384-2, manufactured by BASF)
[0054] [Hardening agent] <<Resin (II-A)>> Isocyanate-based curing agent (Desmodur N3300, manufactured by Sumika Covestro Urethane Co., Ltd., solid content: 100% by mass) <<Organic solvents (II-B)>> Butyl acetate (SP value: 9.3, evaporation rate: 1.00)
[0055] [Diluent] <<Organic solvents (II-B1)>> Diisobutyl ketone (SP value: 8.7, evaporation rate: 0.20) <<Organic solvents (II-B2)>> Ethyl acetate (SP value: 9.5, evaporation rate: 4.20) <<Other organic solvents (II-B)>> Petroleum Hydrocarbons Methyl isobutyl ketone (SP value: 9.0, evaporation rate: 1.60) Cyclohexane (SP value: 8.8, evaporation rate: 4.50) Mineral Spirits (SP value: 8.7) 3-Methoxy-1-butyl acetate (SP value: 9.5, evaporation rate: 0.14)
[0056] [Table 2]
[0057] <Coating film formation method> A metallic paint (I) shown in formulation 1-1 in Table 1 was spray-coated on a black ABS substrate in an amount sufficient to give a dry film thickness of 1.0 μm, and allowed to stand for 7 minutes. Next, a topcoat paint (II) shown in formulation 2-1 in Table 2 was spray-coated on the uncured metallic coating in an amount sufficient to give a dry film thickness of 35 μm, and allowed to stand for 7 minutes. The topcoat was then dried at 80° C. for 30 minutes to form a plated satin-like multi-layer coating film, and the coated body of Example 1 was obtained.
[0058] Using the metallic paint (I) shown in Table 1 and the topcoat paint (II) shown in Table 2 in the combinations shown in Table 3, the coated bodies of Examples 2 to 5 and Comparative Examples 1 to 4 were obtained in the same manner as the coated body of Example 1. These sample coated bodies were used as test bodies to carry out the following tests, and the obtained results are shown in Table 3.
[0059] [Table 3]
[0060] <Adhesion of multi-layer coating> Using the above test specimen, a straight cut was made on the coating surface with a cutter knife at a cutting angle of 60°, reaching the substrate, and another cut was made at an angle of 60° to the first cut. Cellophane tape was then firmly applied to cover the cut, and the cellophane tape was peeled off at an angle of 45° to the coating surface. After peeling off the cellophane tape, the degree of peeling of the coating was visually judged according to the following evaluation criteria. A score of ○ or higher indicates a level suitable for use as a product. ○: No peeling at all. △: There is slight peeling at the cut area. ×: The coating surface at the cut portion was completely peeled off.
[0061] <Satin-plated appearance> The test specimen was visually observed and rated according to the following criteria: Good or better is a level suitable for use as a product. ◎: Shows a satin-finished appearance equivalent to a metal satin-finished plating. ◯: Inferior to metal-plated satin finish, but shows a plated satin appearance superior to that of a normal metallic coating. ×: Sufficient metallic appearance is obtained, but does not achieve a plated satin appearance.
[0062] From the results in Table 3, it is clear that according to the present invention, it is possible to form a multi-layer coating film that has an excellent plated satin appearance and also has excellent adhesion.
Claims
1. The method for forming a multilayer coating film includes at least a metallic coating film forming step of applying a metallic paint (I) onto a substrate to form an uncured metallic coating film, a topcoat coating film forming step of applying a topcoat paint (II) onto the uncured metallic coating film to form an uncured topcoat coating film, and a drying step of simultaneously drying the uncured metallic coating film and the topcoat coating film to form a multilayer coating film, The metallic paint (I) contains a resin (IA), an organic solvent (IB), and a vapor-deposited aluminum pigment (IC) coated with at least an inorganic oxide, The method for forming a multilayer coating film is characterized in that the topcoat paint (II) contains a resin (II-A) and an organic solvent (II-B), and contains 10 to 30 mass % of an organic solvent (II-B1) having an SP value of 8.0 to 9.0 and an evaporation rate of 0.1 or more and less than 1.0 when butyl acetate is taken as 1.0, based on the total amount of the organic solvent (II-B).
2. The method for forming a multilayer coating film according to claim 1, further comprising an organic solvent (II-B2) having an SP value of 9.0 to 10.0 and an evaporation rate of 2.0 or more and less than 6.0, where butyl acetate is taken as 1.0, in an amount of 20 to 50 mass% based on the total amount of the organic solvent (II-B).
3. The method for forming a multilayer coating film according to claim 1 or 2, characterized in that the water content in the metallic paint (I) is less than 3.0 mass%, and the inorganic oxide coating the vapor-deposited aluminum pigment (IC) contains at least silica.
Citation Information
Patent Citations
Plating-like film forming method
JP2003053260A
Method of forming coat, coated article and game implement
JP2010247055A
Decorative film molding, method for producing decorative film molding, satin plating-like product, container, cabinet, and vehicular interior and exterior member
JP2020157691A