Aluminum electric wire and wire harness

The aluminum electric wire design with a specific conductor and insulator configuration enhances flexibility and curlability, addressing the limitations of existing wires and offering reduced weight and cost-effective performance.

JP2024144982AActive Publication Date: 2024-10-15YAZAKI CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023057192
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

Existing aluminum electric wires lack sufficient flexibility and curlability, leading to the need for additional routing measures like band clamps, and their adhesion properties need improvement.

Method used

The aluminum electric wire design includes a conductor composed of a center stranded wire and multiple outer strands, each made of pure aluminum, with specific diameter and adhesion force ranges, and an insulator made of crosslinked polyethylene, ensuring a balanced thickness and twist pitch to enhance flexibility and curlability.

Benefits of technology

The design achieves improved flexibility and curlability, reducing the need for additional routing measures and providing a balance between heat resistance and cost, while maintaining a reduced weight compared to copper wires.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144982000001_ABST
    Figure 2024144982000001_ABST
Patent Text Reader

Abstract

To provide an aluminum electric wire capable of improving flexibility and addictiveness, and a wire harness.SOLUTION: An aluminum electric wire includes a conductor 10 and an insulator 20. The conductor 10 is constituted of a central strand wire 11 and a plurality of outer peripheral strand wires 12 laminated with two or more layers on the outer periphery of the central strand wire 11; the central strand wire 11 and the outer peripheral strand wires 12 are constituted by stranding an element wire consisting of pure aluminum; the element wire has an element wire diameter of 0.21 mm or more and less than 1.0 mm; the conductor 10 and the insulator 20 have an adhesion force of 6 N or more and 45 N or less; and the insulator 20 has a thickness of 0.72 mm or more and 1.80 mm or less.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an aluminum electric wire and a wiring harness. [Background technology]

[0002] Conventionally, aluminum electric wires in which an insulation material is coated on the outer periphery of an aluminum conductor have been proposed (see, for example, Patent Documents 1 to 3). These aluminum electric wires are improved in flexibility by using a specific material for the insulation material. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2012-99412 A [Patent Document 2] JP 2012-104227 A [Patent Document 3] JP 2019-179628 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, the flexibility of an electric wire is determined by the total of various factors such as the material, wire diameter, and twisting configuration of the conductor, the material and thickness of the insulator, and the state of adhesion between the conductor and the insulator, etc. For this reason, the electric wires described in Patent Documents 1 to 3 have room for improvement in flexibility.

[0005] In addition, copper electric wires are difficult to bend, and the bending radius of the wires is large when they are installed. For this reason, when installing copper electric wires, the route is restricted by protectors or band clamps to prevent interference with devices and electric wires. In contrast, aluminum electric wires are more likely to bend than copper electric wires. However, even aluminum electric wires still do not have sufficient bending properties, and in some cases, the route must be restricted by band clamps or the like.

[0006] The present invention has been made to solve the above-mentioned problems in the conventional art, and an object of the invention is to provide an aluminum electric wire and a wiring harness that can improve flexibility and shapeability. [Means for solving the problem]

[0007] An aluminum electric wire according to the present invention comprises a conductor and an insulator covering the conductor, the conductor being composed of a central strand and a plurality of peripheral strands stacked in two or more layers around the central strand, the central strand and the peripheral strand being constructed by twisting strands of pure aluminum, and each of the strands has a diameter of 0.21 mm or more and less than 1.0 mm, the conductor and the insulator have an adhesion strength of 6 N or more and 45 N or less, and the insulator has a thickness of 0.72 mm or more and 1.80 mm or less.

[0008] A wire harness according to the present invention is characterized by including the aluminum electric wire described above. Effect of the Invention

[0009] According to the present invention, it is possible to provide an aluminum electric wire and a wiring harness that can achieve improved flexibility and shapeability. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a perspective view showing an example of a wire harness including an aluminum electric wire according to an embodiment of the present invention. [Diagram 2] 2 is a cross-sectional view showing an example of the aluminum electric wire shown in FIG. 1. [Diagram 3] 3 is a cross-sectional view showing an example of a partial configuration of the aluminum electric wire shown in FIG. 2. [Figure 4] 1 is a first table showing examples and comparative examples. [Diagram 5] 2 is a second table showing examples and comparative examples. [Figure 6]FIG. 2 is a schematic diagram showing a method for measuring adhesion, in which (a) shows a sample for measuring adhesion, and (b) shows the method for measuring adhesion. [Figure 7] FIG. 1 is a conceptual diagram showing a flexibility test. [Figure 8] 1 is a table showing the results of a shape forming test. [Figure 9] 1 is a table showing the results of a comparison between the aluminum electric wire of Example 3 and the copper electric wire of Comparative Example 10. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described below along with preferred embodiments. Note that the present invention is not limited to the embodiments shown below, and can be modified as appropriate within the scope of the present invention. In addition, in the embodiments shown below, some configurations are omitted from illustration and description, but it goes without saying that publicly known or well-known technologies are appropriately applied to the details of the omitted technologies within the scope of the contents described below.

[0012] Fig. 1 is a perspective view showing an example of a wire harness including an aluminum electric wire according to an embodiment of the present invention. As shown in Fig. 1, the wire harness WH is configured to include an aluminum electric wire 1 and another member O. The other member O is, for example, a connector O1, a terminal O2, etc. Note that the other member O is not limited to the connector O1, the terminal O2, etc., and may be another electric wire, etc.

[0013] Fig. 2 is a cross-sectional view showing an example of the aluminum electric wire 1 shown in Fig. 1, and Fig. 3 is a cross-sectional view showing an example of a partial configuration of the aluminum electric wire 1 shown in Fig. 2. As shown in Fig. 2, the aluminum electric wire 1 includes a conductor 10 and an insulator 20 that covers the outer periphery of the conductor 10 in a contacting state.

[0014] The conductor 10 includes a central strand 11 and a plurality of peripheral strands 12. The plurality of peripheral strands 12 are arranged to form two or more layers on the outer circumferential side of the central strand 11. The peripheral strands 12 are assumed to be bunch-twisted around the central strand 11, but are not limited to bunch-twisting and may be concentrically twisted. As shown in FIG. 3, the central strand 11 and the peripheral strand 12 are formed by twisting a plurality of element wires 11a, 12a made of pure aluminum.

[0015] In this embodiment, the wires 11a, 12a constituting the central strand 11 and the peripheral strand 12 have a wire diameter of 0.21 mm or more and less than 1.0 mm. If the wire diameter is less than 0.21 mm, the wires 11a, 12a are too thin and prone to breakage, whereas if the wire diameter is 1.0 mm or more, the wires 11a, 12a are too thick and lose flexibility.

[0016] In this embodiment, the adhesion between the conductor 10 and the insulator 20 is 6N or more and 45N or less. If the adhesion is less than 6N, the conductor 10 and the insulator 20 will move too easily when bending the wire, and the shape forming ability will be significantly reduced. If the adhesion is more than 45N, the adhesion is too high, and the conductor 10 and the insulator 20 will not move easily when bending the wire, and will act like a thick rod, resulting in a loss of flexibility.

[0017] Furthermore, in this embodiment, the insulator 20 has a thickness of 0.72 mm or more and 1.80 mm or less. If the thickness is less than 0.72 mm, the insulator 20 is too thin and abrasion resistance cannot be ensured. If the thickness exceeds 1.80 mm, the insulator 20 is too thick and flexibility cannot be ensured.

[0018] Additionally, in this embodiment, the insulator 20 is preferably made of cross-linked polyethylene, because cross-linked polyethylene provides a good balance between heat resistance and cost, making it easier to provide an aluminum electric wire 1 that is more excellent in heat resistance and cost.

[0019] In addition, the cross-sectional area (size) of the conductor 10 is preferably 30 sq. or more and 230 sq. or less. If the cross-sectional area is less than 30 sq., the weight reduction effect is reduced compared to a copper electric wire of the same size. If the cross-sectional area is more than 230 sq., the size becomes too large and it becomes difficult to apply it to a vehicle, for example.

[0020] Furthermore, it is preferable that the twist pitch of the central stranded wire 11 is 15 to 30 times (preferably 20 times) the twist outer diameter, and the twist pitch of the peripheral stranded wire 12 is 8 to 15 times (preferably 11 times) the outer diameter of the corresponding layer. Here, the corresponding layer is the first layer in the case of the peripheral stranded wire 12 belonging to the first layer, and the second layer in the case of the peripheral stranded wire 12 belonging to the second layer. That is, it is preferable that the twist pitch of the peripheral stranded wire 12 of the first layer is 8 to 15 times the outer diameter of the first layer, and the twist pitch of the peripheral stranded wire 12 of the second layer is 8 to 15 times the outer diameter of the second layer. This is because the adoption of these twist pitches can contribute to preventing the occurrence of wire breakage, twist lift, and twist collapse.

[0021] Next, examples of the present invention and comparative examples will be described. Figures 4 and 5 are diagrams showing the examples and comparative examples.

[0022] First, as shown in Figures 4 and 5, all of the strands constituting the conductor in Example 1 were made of pure aluminum. In Example 1, the conductor size was 50 sq., and the central strand and the outer circumferential strand had 19 strands in the main twist and 32 strands in the bottom twist, with a strand diameter of 0.32 mm. The cross-sectional area of ​​such a conductor was 48.9 mm. 2 The outer diameter was 10.0 mm. In Example 1, the insulator was made of cross-linked PE (polyethylene) and had a thickness of 1.50 mm. The aluminum electric wire according to Example 1 had an outer diameter of 13.0 mm. Furthermore, the adhesion was measured using a measurement method in accordance with ISO19642, which will be described later, and the adhesion was 6 N.

[0023] The aluminum electric wire according to Example 2 was the same as that of Example 1, except that the adhesive force was 45N.

[0024] In Example 3, all the strands were made of pure aluminum. The conductor size was 95 sq., and the central strand and the outer strand had 19 strands in the main strand and 62 strands in the bottom strand, with a strand diameter of 0.32 mm. The cross-sectional area of ​​such a conductor was 94.7 mm. 2 The outer diameter was 13.9 mm. In Example 3, the insulator was made of cross-linked PE and had a thickness of 1.50 mm. The aluminum electric wire according to Example 3 had an outer diameter of 16.9 mm. Furthermore, the adhesion was 9 N.

[0025] On the other hand, in Comparative Example 1, all the strands constituting the conductor were made of pure copper. In Comparative Example 1, the conductor size was 30 sq., and the central strand and the outer strand had 19 strands in the main twist and the bottom twist, with the strand diameter being 0.32 mm. The cross-sectional area of ​​such a conductor was 29.0 mm. 2 The outer diameter was 7.8 mm. In Comparative Example 1, the insulator was made of cross-linked PE and had a thickness of 1.30 mm. The aluminum electric wire according to Comparative Example 1 had an outer diameter of 10.4 mm. Furthermore, the adhesion was 86 N.

[0026] In Comparative Example 2, all the strands constituting the conductor were made of pure copper. The conductor size in Comparative Example 2 was 35 sq., and the central strand and the outer strand had 19 strands in the main twist and 23 strands in the bottom twist, with a strand diameter of 0.32 mm. The cross-sectional area of ​​such a conductor was 35.2 mm. 2 The outer diameter was 8.4 mm. In Comparative Example 2, the insulator was made of cross-linked PE and had a thickness of 1.50 mm. The aluminum electric wire according to Comparative Example 2 had an outer diameter of 11.4 mm. Furthermore, the adhesion was 95 N.

[0027] In Comparative Example 3, all the strands constituting the conductor were made of pure copper. The conductor size in Comparative Example 3 was 40 sq., and the central strand and the outer strand had 19 strands in the main strand and 26 strands in the bottom strand, with a strand diameter of 0.32 mm. The cross-sectional area of ​​such a conductor was 39.7 mm. 2 The outer diameter was 9.1 mm. In Comparative Example 3, the insulator was made of cross-linked PE and had a thickness of 1.40 mm. The electric wire according to Comparative Example 3 had an outer diameter of 11.9 mm. Furthermore, the adhesion was 110 N.

[0028] In Comparative Example 4, all the strands constituting the conductor were made of pure aluminum. The conductor size in Comparative Example 4 was 50 sq., and the central strand and the outer circumferential strand had 19 strands in the main strand and 83 strands in the bottom strand, with a strand diameter of 0.20 mm. The cross-sectional area of ​​such a conductor was 50.6 mm. 2 The outer diameter was 9.9 mm. In Comparative Example 4, the insulator was made of cross-linked PE and had a thickness of 1.50 mm. The aluminum electric wire according to Comparative Example 4 had an outer diameter of 12.9 mm. This aluminum electric wire had a broken wire during production and was not usable as a product, so the adhesion and other properties were not measured.

[0029] In Comparative Example 5, all the strands constituting the conductor were made of pure aluminum. The conductor size in Comparative Example 5 was 50 sq., and the central strand and the outer circumferential strand had 19 strands in the main strand and 32 strands in the bottom strand, with a strand diameter of 0.32 mm. The cross-sectional area of ​​such a conductor was 48.9 mm. 2 and the outer diameter was 10.0 mm. In Comparative Example 5, the insulator was made of cross-linked PE and had a thickness of 0.50 mm. The aluminum electric wire according to Comparative Example 5 had an outer diameter of 11.0 mm. Note that the thickness of the insulator of this aluminum electric wire was too thin to ensure abrasion resistance, and the coating thickness was unstable, so the wire could not be used as a product. For this reason, the adhesion and other properties of Comparative Example 5 were not measured.

[0030] In Comparative Example 6, the conductor was the same as in Comparative Example 5. In Comparative Example 6, the insulator was made of cross-linked PE and had a thickness of 0.72 mm. The aluminum electric wire according to Comparative Example 6 had an outer diameter of 11.4 mm. The adhesion force was 5N.

[0031] In Comparative Example 7, the conductor was the same as in Comparative Example 5. In Comparative Example 7, the insulator was made of cross-linked PE and had a thickness of 1.80 mm. The aluminum electric wire according to Comparative Example 7 had an outer diameter of 13.6 mm. The adhesion force was 52 N.

[0032] In Comparative Example 8, all of the wires constituting the conductor were made of pure aluminum. The conductor size in Comparative Example 8 was 50 sq. m, and the stranded wire was made of 61 strands each having a wire diameter of 1.0 mm. The cross-sectional area of ​​such a conductor was 47.9 mm. 2 The outer diameter was 9.0 mm. In Comparative Example 8, the insulator was made of cross-linked PE and had a thickness of 1.50 mm. The aluminum electric wire according to Comparative Example 8 had an outer diameter of 12.0 mm. Furthermore, the adhesion was 28 N.

[0033] In Comparative Example 9, all the strands constituting the conductor were made of pure aluminum. The conductor size in Comparative Example 9 was 50 sq., and the central strand and the outer circumferential strand had 19 strands in the main strand and 13 strands in the bottom strand, with a strand diameter of 0.5 mm. The cross-sectional area of ​​such a conductor was 48.5 mm. 2 The outer diameter was 9.4 mm. In Comparative Example 9, the insulator was made of cross-linked PE and had a thickness of 1.50 mm. The aluminum electric wire according to Comparative Example 9 had an outer diameter of 12.4 mm. Furthermore, the adhesion was 200 N.

[0034] In Comparative Example 10, all of the strands constituting the conductor were made of pure copper. The conductor size in Comparative Example 10 was 70 sq., and the central strand and the outer circumferential strand had 19 strands in the main strand and 46 strands in the bottom strand, with a strand diameter of 0.32 mm. The cross-sectional area of ​​such a conductor was 70.3 mm. 2The outer diameter was 12.0 mm. In Comparative Example 10, the insulator was made of cross-linked PE and had a thickness of 1.50 mm. The electric wire according to Comparative Example 10 had an outer diameter of 15.0 mm. Furthermore, the adhesion was 120 N.

[0035] In Comparative Example 11, all the strands constituting the conductor were made of pure aluminum. The conductor size in Comparative Example 11 was 95 sq., and the central strand and the outer circumferential strand had 19 strands in the main strand and 25 strands in the bottom strand, with a strand diameter of 0.5 mm. The cross-sectional area of ​​such a conductor was 93.2 mm. 2 The outer diameter was 12.9 mm. In Comparative Example 11, the insulator was made of cross-linked PE and had a thickness of 1.50 mm. The aluminum electric wire according to Comparative Example 11 had an outer diameter of 15.9 mm. Furthermore, the adhesion was 55 N.

[0036] In Comparative Example 12, all of the strands constituting the conductor were made of aluminum alloy. The conductor size in Comparative Example 12 was 50 sq., and the central strand and the outer circumferential strand had 19 strands in the main strand and 32 strands in the bottom strand, with a strand diameter of 0.32 mm. The cross-sectional area of ​​such a conductor was 48.9 mm. 2 The outer diameter was 10.0 mm. In Comparative Example 12, the insulator was made of cross-linked PE and had a thickness of 1.50 mm. The aluminum electric wire according to Comparative Example 12 had an outer diameter of 13.0 mm. Furthermore, the adhesion was 54 N.

[0037] The adhesion was measured as follows: Figure 6 is a schematic diagram showing the method for measuring the adhesion, where (a) shows a sample for measuring the adhesion, and (b) shows the method for measuring the adhesion.

[0038] To measure the adhesion, first, the insulation was stripped off from one end of a 75 mm long electric wire to expose the conductor, as shown in Fig. 6(a).Then, as shown in Fig. 6(b), the conductor was inserted into a hole in a plate material with a diameter of the conductor outer diameter + 0.1 mm, and pulled from the insertion side at a speed of 200 mm / min. The force (maximum value) when the conductor was pulled out until it was separated from the insulation was recorded as the adhesion.

[0039] The electric wires of Examples 1 to 3 and Comparative Examples 1 to 12 were subjected to a flexibility test, and the electric wires of Examples 1 to 3 and Comparative Examples 2 and 6 were subjected to a curling test.

[0040] Figure 7 is a conceptual diagram showing the flexibility test. For the flexibility test, a 400 mm electric wire with an insulator covering the conductor is used as a sample. As shown in Figure 7, the other end of the sample is fixed, and a load is applied from one end. The load at the point when the sample is bent 180 degrees is defined as the flexibility.

[0041] Fig. 8 is a chart showing the results of the shape forming test. In the shape forming test, as shown in Fig. 8, the wire was wound around a cylinder of φ75 and φ50, fixed with a cable tie or the like, left to stand for one minute, and then the fixed part was released, and the degree of spreading of the wire was evaluated. Regarding the evaluation in Fig. 4 and Fig. 5, if the spread of the wire on the line passing through the center of the cylinder (see the dashed line in Fig. 8) was 75 mm or more, the shape forming was marked as "x", and if it was less than 75 mm, the shape forming was marked as "o". The reason for using cylinders of φ75 and φ50 is to check the shape forming ability of the wire at approximately 5 times its diameter.

[0042] As shown in Figs. 4 and 5, in Examples 1 to 3, the flexibility was 7N or more and 11N or less, and the flexibility was excellent. Similarly, in Comparative Examples 1, 2, and 6, the flexibility was also excellent. In particular, it was found that the aluminum electric wires of Examples 1 to 3 were thicker than the copper electric wires of Comparative Examples 1 and 2, but were able to exhibit the same degree of flexibility. On the other hand, in Comparative Examples 3, 7 to 12, the flexibility exceeded 11N, and the flexibility of Examples 1 to 3 was not achieved. Note that Comparative Examples 4 and 5 were not viable as products, and flexibility measurements were not performed.

[0043] 4, 5, and 8, in Examples 1 to 3 (Example 3 is omitted in FIG. 8), the spread of the aluminum electric wire was less than 75 mm, and the shapeability was good, that is, the electric wire did not require path restriction by a protector or band clamp. On the other hand, in Comparative Examples 2 and 6 (Comparative Example 2 is omitted in FIG. 8), the spread of the electric wire was 75 mm or more, and path restriction was required.

[0044] From the above, it was found that the aluminum electric wires according to Examples 1 to 3 were able to achieve improvements in flexibility and shapeability.

[0045] The aluminum electric wire according to the embodiment does not have a large outer diameter compared to the copper electric wire, and therefore can be significantly lighter. Fig. 9 is a table showing the results of a comparison between the aluminum electric wire according to Example 3 and the copper electric wire according to Comparative Example 10. When the ambient temperature was 105°C and a current of 250A was continuously applied, as shown in Fig. 9, the maximum temperature of the conductor of the aluminum electric wire according to Example 3 was 136.9°C, and the maximum temperature of the conductor of the copper electric wire according to Comparative Example 10 was 137.2°C. In other words, the two had approximately the same temperature.

[0046] Comparing the outer diameters of the electric wires, the aluminum electric wire according to Example 3 was 16.9 mm, and the copper electric wire according to Comparative Example 10 was 15.0 mm. That is, the aluminum electric wire according to Example 3 had an outer diameter of about 113.5% of the copper electric wire according to Comparative Example 10, and there was not a large difference between the two.

[0047] In contrast, when comparing the weights, the aluminum electric wire according to Example 3 was 288.5 g / m, and the copper electric wire according to Comparative Example 10 was 731.3 g / m. That is, the weight of the aluminum electric wire according to Example 3 was reduced by approximately 60.6% compared to the copper electric wire of Comparative Example 10.

[0048] Thus, in the aluminum electric wire 1 and the wire harness WH according to this embodiment, the conductor 10 is not only composed of the central stranded wire 11 and the outer peripheral stranded wire 12 formed by twisting the element wires 11a, 12a, but also has a wire diameter of less than 1.0 mm. This prevents the element wires 11a, 12a from becoming too thick and impairing the flexibility of the aluminum electric wire 1. In addition, since the element wire diameter is 0.21 mm or more, the possibility of the electric wire breaking when being bent is reduced.

[0049] Furthermore, since the adhesion between the conductor 10 and the insulator 20 is 6N or more, a certain degree of adhesion is ensured, making it difficult for the conductor 10 and the insulator 20 to move separately, and reducing the loss of shapeability that would occur if each of them moved independently. Also, since the adhesion between the conductor 10 and the insulator 20 is 45N or less, the conductor 10 and the insulator 20 are integrated, reducing the loss of flexibility that would occur when bending a thick object.

[0050] In addition, since the thickness of the insulator 20 is not less than 0.72 mm and not more than 1.80 mm, the insulator 20 is prevented from becoming too thin to ensure wear resistance, or from becoming too thick to reduce flexibility.

[0051] Therefore, it is possible to provide the aluminum electric wire 1 and the wire harness WH that can achieve improved flexibility and shapeability.

[0052] Furthermore, since the insulator 20 is made of cross-linked polyethylene, it is possible to provide an aluminum electric wire 1 that is superior in both heat resistance and cost by achieving a good balance between both.

[0053] In addition, since the conductor 10 has a cross-sectional area of ​​30 sq. or more, the weight reduction effect is somewhat greater than that of a copper wire of the same size, while the cross-sectional area is 230 sq. or less, so the size is not too large and it can be easily applied to, for example, vehicles.

[0054] In addition, the twist pitch of the central stranded wire 11 is 15 to 30 times the twist outer diameter, and the twist pitch of the peripheral stranded wire 12 is 8 to 15 times the twist outer diameter. This greatly reduces the possibility of exceeding the processing limit, which helps prevent wire breakage, loose twists, and loose twists.

[0055] The present invention has been described above based on an embodiment, but the present invention is not limited to the above embodiment, and modifications may be made or well-known and publicly known technologies may be combined without departing from the spirit of the present invention.

[0056] For example, in the wire harness WH according to the present embodiment, the connector O1 and the terminal O2 are exemplified as examples of the other member O, but the other member O is not particularly limited to these and may be, for example, the same type of aluminum electric wire 1 or the like. [Explanation of symbols]

[0057] 1: Aluminum wire 10: Conductor 11: Center strand 12: Outer stranded wire 11a,12a: Plain wire 20: Insulator O: Other materials WH: Wire harness

Claims

1. An aluminum electric wire comprising a conductor and an insulator covering the conductor, the conductor being composed of a central strand and a plurality of peripheral strands laminated in two or more layers around the central strand, the central strand and the peripheral strand being composed of strands of pure aluminum, The wires each have a wire diameter of 0.21 mm or more and less than 1.0 mm, The adhesion strength between the conductor and the insulator is 6 N or more and 45 N or less, The insulator has a thickness of 0.72 mm or more and 1.80 mm or less.

1. An aluminum electric wire comprising:

2. The insulator is cross-linked polyethylene.

2. The aluminum electric wire according to claim 1 .

3. The conductor has a cross-sectional area of ​​30 sq. or more and 230 sq. or less.

2. The aluminum electric wire according to claim 1 .

4. The conductor has a twist pitch of the central strand that is 15 to 30 times the twist outer diameter, and a twist pitch of the peripheral strand that is 8 to 15 times the outer diameter of the corresponding layer.

2. The aluminum electric wire according to claim 1 .

5. A wire harness comprising the aluminum electric wire according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Resin composition and electric wire for automobile covered with the resin composition

    JP2012229343A

  • Electric wire

    JP2013246949A

  • Bending-resistant electric wire and wiring harness

    JP2016197569A

  • Highly flexible insulated wire

    JP2019021560A

  • Insulation wire

    JP2019207811A