Semiconductor device inspection method
The semiconductor device inspection method addresses the issue of defective gate insulating films in silicon carbide devices by applying voltages and measuring leakage currents, ensuring the selection of reliable products.
Patent Information
- Application Number
- JP2023057230
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Insulated gate type silicon carbide semiconductor devices suffer from gate insulating films with many defects, leading to potential malfunctions during long-term use due to unstable quality, necessitating an effective inspection method to detect performance degradation.
A semiconductor device inspection method involving voltage application and measurement steps to detect defects in the gate insulating film, including positive and negative voltage applications followed by leakage current measurements to assess the influence of defects.
The method allows for the detection of performance degradation in silicon carbide semiconductor devices by accurately measuring leakage currents, enabling the selection of non-defective products before shipment.
Smart Images

Figure 2024145013000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for inspecting an insulated gate semiconductor device made of silicon carbide. [Background technology]
[0002] Silicon carbide (SiC) has been attracting attention as a semiconductor material that can be used to manufacture power semiconductors with low resistance, high voltage resistance, heat resistance, and high speed characteristics. Power semiconductor devices using silicon carbide include MOSFETs (Metal Oxide Semiconductor Field Effect Transistors) and IGBTs (Insulated Gate Bipolar Transistors) with insulated gate structures. Furthermore, in such semiconductor devices, manufactured elements are subjected to inspection to determine whether they are conforming products or non-conforming products (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 2018-205252 Summary of the Invention [Problem to be solved by the invention]
[0004] However, in an insulated gate SiC semiconductor device, the gate insulating film is likely to contain many defects in the crystal, and the quality of the gate insulating film is less stable than that of a Si semiconductor device. If the gate insulating film contains many defects, problems such as malfunctions are likely to occur during long-term use of the semiconductor device. For this reason, an inspection method capable of detecting performance degradation of the semiconductor device due to defects in the gate insulating film is required for the insulated gate SiC semiconductor device.
[0005] In order to solve the above-mentioned problems, the present invention provides a method for inspecting a semiconductor device that is capable of detecting a performance degradation caused by a defect in a gate insulating film.
[0006] The above and other objects of the present invention and novel features of the present invention will become apparent from the description of this specification and the accompanying drawings. [Means for solving the problem]
[0007] The semiconductor device inspection method of the present invention is a method for inspecting an insulated gate silicon carbide semiconductor device having a gate insulating film, a gate terminal, a source terminal, and a drain terminal. The inspection method includes a positive voltage application step of applying a voltage VGS+ that positively biases the gate terminal with respect to the source terminal, and a positive voltage release step of releasing the application of the voltage VGS+. The inspection method also includes a first measurement step of measuring a leakage current IDSS1 while applying a voltage VDS that positively biases the drain terminal with respect to the source terminal. Effect of the Invention
[0008] According to the present invention, it is possible to provide a method for inspecting a semiconductor device that is capable of detecting a performance degradation caused by a defect in a gate insulating film.
[0009] Problems, configurations and effects other than those described above will become apparent from the following description of the embodiments. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a diagram showing a schematic configuration of a SiC semiconductor device. [Diagram 2] 1 is a flowchart showing a method for inspecting a semiconductor device. [Diagram 3] 1 is a flowchart showing a method for inspecting a semiconductor device. [Figure 4] 1 is a graph showing a characteristic curve of leakage current of a gate insulating film. [Diagram 5] 1 is a graph showing a characteristic curve of leakage current of a gate insulating film. [Figure 6] FIG. 1 is a diagram showing a schematic configuration of an inspection device and a semiconductor device in a wafer state; [Figure 7] FIG. 2 is a plan view of a semiconductor device in a wafer state; [Figure 8] 1 is a cross-sectional view of a semiconductor device in a wafer state; [Figure 9] FIG. 1 is a diagram showing a configuration of an inspection device and an example of a discrete package of a semiconductor device. [Figure 10] FIG. 1 is a diagram showing a configuration of an example of a power module package of a 2-in-1 half-bridge type semiconductor device. [Figure 11] FIG. 1 is a circuit diagram of a 2-in-1 half-bridge type semiconductor device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] An example of a method for inspecting a semiconductor device according to an embodiment of the present invention will be described below with reference to the drawings. Note that the present invention is not limited to the following example. In each of the drawings described below, the same reference numerals are used for common members. In addition, in the drawings used in this specification, the same reference numerals are used for the same or corresponding components, and repeated description of these components may be omitted.
[0012] [Configuration of semiconductor device] The configuration of a SiC semiconductor device that can be applied to the semiconductor device inspection method of this embodiment will be described below. Fig. 1 shows a schematic configuration of a SiC semiconductor device. The semiconductor device 100 shown in Fig. 1 is a planar type MOSFET (Metal Oxide Semiconductor Field Effect Transistor) having an insulated gate using silicon carbide. In the semiconductor device 100 described below, a case of a MOSFET using an n-type SiC substrate is illustrated, but the MOSFET may be a p-type. In that case, the conductivity types of the impurities described below are all reversed.
[0013] The semiconductor device 100 has a semiconductor substrate 10 and a drift layer 11 formed on a main surface of the semiconductor substrate 10. The semiconductor substrate 10 is a compound semiconductor substrate containing carbon and silicon, and is made of silicon carbide (SiC). The drift layer 11 is made of an epitaxial growth layer or the like formed on the semiconductor substrate 10, and is made of SiC like the semiconductor substrate 10. The drift layer 11 has a first conductivity type (n-type) region, and the semiconductor substrate 10 has a first conductivity type (n-type) region containing an n-type dopant at a higher concentration than the drift layer 11. + It has a type) region.
[0014] A second conductivity type (p-type) body region 13 is formed near the surface of the drift layer 11. In addition, an n-type drift layer 11 having a higher concentration of n-type dopants is formed in the p-type body region 13. + In addition, an n-type source region 14 is formed. + A p-type dopant having a higher concentration than the p-type body region 13 is provided adjacent to the end of the source region 14. + A mold contact region 15 is formed.
[0015] On the drift layer 11, + type source region 14 and p + A source terminal 22 is formed in contact with at least a portion of the type contact region 15. In addition, a drain terminal 23 is provided on the back surface of the semiconductor substrate 10 made of SiC. Furthermore, a gate insulating film 20 is provided in contact with the p-type body region 13 near the surface of the drift layer 11. A gate terminal 21 is formed on the gate insulating film 20. That is, the semiconductor device 100 is a semiconductor device including an insulated gate in which the gate terminal 21 is formed on the gate insulating film 20.
[0016] In the semiconductor device 100 having the above-mentioned configuration, when the gate terminal 21 is biased to a certain voltage or more (threshold voltage VGSth) with respect to the source terminal 22, the portion of the p-type body region 13 on the surface side that contacts the lower part of the gate insulating film 20 is inverted to n-type, and a conductive channel is formed. In this state, when the drain terminal 23 is positively biased with respect to the source terminal 22, + Electrons flow from the source region 14 through the conductive channel toward the drain terminal 23 .
[0017] When the gate voltage is equal to or lower than the threshold voltage, no conductive channel is formed below the gate insulating film 20. However, even when the gate voltage is equal to or lower than the threshold voltage VGSth, when a high drain voltage is applied, a depletion region is formed in the drift layer 11, and a very small leakage current flows to the drain terminal 23. In this way, the semiconductor device 100 is capable of turning the current on and off (switching operation) by controlling the gate voltage applied to the gate terminal 21.
[0018] In the semiconductor device 100 having the above configuration, the gate insulating film 20 is formed by oxidizing the SiC constituting the semiconductor substrate 10, or by depositing SiO2 on the semiconductor substrate 10 using a chemical vapor deposition (CVD) method. However, the SiC constituting the semiconductor substrate 10 has crystal polytypes. In addition, SiC has properties such as including many defects in the crystal, and C (carbon) remaining when oxidized to form SiO2. For this reason, the gate insulating film 20 formed on the semiconductor substrate 10 made of SiC may include defects, compared to a gate insulating film formed on a semiconductor substrate made of Si.
[0019] If the gate insulating film 20 contains defects, it will have a degraded performance or adverse effects on the semiconductor device 100, such as a fluctuation in threshold voltage, an increase in leakage current, etc. Furthermore, this may lead to malfunction of the semiconductor device 100 when used for a long period of time. For this reason, in the inspection method of the present embodiment, in the semiconductor device 100 using the semiconductor substrate 10 made of SiC having the above configuration, inspection of the semiconductor device is performed including the influence of defects in the gate insulating film 20. By using this inspection method, it is possible to select products whose performance and reliability do not deteriorate even after long-term use.
[0020] [Method of inspecting semiconductor device (1)] Next, a method for inspecting the semiconductor device 100 using the semiconductor substrate 10 made of SiC described above will be described with reference to Fig. 2. Fig. 2 is a flow chart showing the method for inspecting the semiconductor device 100.
[0021] (Positive voltage application process) First, a positive voltage is applied between the gate terminal 21 and the source terminal 22 of the semiconductor device 100 (step S10). In this step, for example, a positive voltage is applied to the gate terminal 21, and the potential of the source terminal 22 is set to zero, so that a voltage VGS+ is applied to the gate terminal 21 such that the gate terminal 21 is positively biased with respect to the source terminal 22. As a result, in the semiconductor device 100, the gate terminal 21 is positively biased with respect to the source terminal 22. At this time, the drain terminal 23 is floating or has a potential of zero.
[0022] (Positive voltage release process) Next, the application of the positive voltage applied between the gate terminal 21 and the source terminal 22 is released (step S11). Specifically, in the semiconductor device 100, the application of the voltage VGS+ to the gate terminal 21 is released, and the application of the positive voltage that positively biases the gate terminal 21 with respect to the source terminal 22 is released.
[0023] (1st measurement process) Next, a positive voltage is applied between the drain terminal 23 and the source terminal 22 (step S12). Then, a leakage current IDSS1 is measured at the drain terminal 23 (step S13). For example, a positive voltage is applied to the drain terminal 23, and the potential of the source terminal 22 is set to 0, so that a voltage VDS is applied to the drain terminal 23 such that the drain terminal 23 is positively biased with respect to the source terminal 22. Then, with the voltage VDS applied to the drain terminal 23, the leakage current IDSS1 is measured at the drain terminal 23. At this time, the gate terminal 21 is floating or has a potential of 0, thereby being in an off state. Next, after measuring the leakage current IDSS1, the application of the positive voltage applied between the drain terminal 23 and the source terminal 22 is released (step S14). Specifically, the application of the voltage VDS to the drain terminal 23 is released.
[0024] (Sorting process) Next, the measured leakage current IDSS1 is compared with a reference value for determining whether the semiconductor device 100 is conforming or non-conforming in advance, and it is determined whether the leakage current IDSS1 is less than the reference value (step S15). If the leakage current IDSS1 is not less than the reference value (No in step S15), the inspected semiconductor device 100 is screened out as a defective product (step S16). Thus, the semiconductor device 100 inspected in the above series of processes is screened as conforming or non-conforming depending on whether the leakage current IDSS1 exceeds the reference value. When the leakage current IDSS1 is less than the reference value (Yes in step S15), or after the semiconductor device 100 has been out-screened, the process according to this flowchart ends.
[0025] In the above-described inspection method, in step S10, a voltage VGS+ is applied between the gate terminal 21 and the source terminal 22, so that electrons captured by defects contained in the gate insulating film 20 can be discharged to the drift layer 11. After the electrons are discharged from the gate insulating film 20, a voltage VDS is applied between the drain terminal 23 and the source terminal 22 to measure the leakage current IDSS1. Therefore, the measured leakage current IDSS1 is affected by the electrons discharged below the gate insulating film 20. That is, because electrons are discharged from the gate insulating film 20 to the surface side of the p-type body region 13 below the gate insulating film 20, the conductivity of the p-type body region 13 increases. As a result, the value of the leakage current IDSS1 measured between the source terminal 22 and the drain terminal 23 in step S13 increases. Therefore, by performing the above-described inspection method, the leakage current IDSS1 is likely to increase as the number of defects in the gate insulating film 20 increases. Therefore, the above-described inspection method can detect a performance degradation of the semiconductor device 100 caused by defects in the gate insulating film 20.
[0026] In the above-mentioned inspection method, after the voltage VGS+ is released in step S11, the gate terminal 21 is not negatively biased with respect to the source terminal 22 until the voltage VDS is applied in step S12. For example, it is preferable to keep the gate terminal 21 and the source terminal 22 at the same potential by floating the gate terminal 21 or shorting it with the source terminal 22. In the above-mentioned inspection method, the leakage current is measured in a state in which electrons trapped in defects in the gate insulating film 20 are discharged by application of the voltage VGS+. For this reason, after the voltage VGS+ is applied in step S11 to discharge the trapped electrons from the gate insulating film 20, it is necessary to prevent electrons from being recaptured by defects in the gate insulating film 20 until the leakage current IDSS1 is measured in step S12.
[0027] Moreover, it is preferable that the time from step S11 to performing step S12 is within 24 hours. A defect in the gate insulating film 20 is stable in a state in which electrons are trapped. Therefore, even if the gate terminal 21 is left without being negatively biased after the voltage VGS+ is applied to discharge electrons, the gate insulating film 20 may recapture electrons excited by heat or light. Therefore, even if the gate insulating film 20 has a configuration in which there is a defect, there is a possibility that an abnormality in the leakage current IDSS1 is not detected in step S12. Therefore, it is better that the time from releasing the negative bias of the gate terminal 21 in step S11 to measuring the leakage current IDSS1 in step S12 is short, and it is preferable that the time is within 24 hours.
[0028] [Method of inspecting semiconductor device (2)] Next, an application example of the inspection method for the semiconductor device 100 using the semiconductor substrate 10 made of SiC described above will be described with reference to Fig. 3. Fig. 3 is a flowchart showing an application example of the inspection method for the semiconductor device 100. Note that the process of the flowchart shown in Fig. 3 includes the same process as the process of the flowchart shown in Fig. 2 described above. Therefore, detailed description of the process similar to the process of the flowchart shown in Fig. 2 described above will be omitted.
[0029] (Electrification process) First, a current of a predetermined value or more is passed between the source terminal 22 and the drain terminal 23 (step S20). For example, the gate terminal 21 is biased to a voltage (threshold voltage VGSth) or more with respect to the source terminal 22, to form a conductive channel below the gate insulating film 20. In this state, a positive voltage is applied to the drain terminal 23, and the potential of the source terminal 22 is set to 0, thereby passing a current between the source terminal 22 and the drain terminal 23. At this time, it is preferable to pass a current larger than 1 / 10 of the absolute maximum rated current specification of the semiconductor device 100 between the source terminal 22 and the drain terminal 23.
[0030] (Positive voltage application process to first measurement process) Next, the same processes as those from step S10 to step S14 in the flowchart shown in Fig. 2 are performed (steps S21 to S25). Through these processes, in the semiconductor device 100, the leakage current IDSS1 caused by application and release of the voltage VGS+ to the gate terminal 21 and application and release of a positive voltage between the drain terminal 23 and the source terminal 22 is measured.
[0031] (Negative voltage application process) Next, a negative voltage is applied between the gate terminal 21 and the source terminal 22 of the semiconductor device 100 (step S26). For example, a negative voltage is applied to the gate terminal 21, and the potential of the source terminal 22 is set to zero, so that a voltage VGS- is applied to the gate terminal 21 such that the gate terminal 21 is negatively biased with respect to the source terminal 22. As a result, in the semiconductor device 100, the gate terminal 21 is negatively biased with respect to the source terminal 22. At this time, the drain terminal 23 is floating or has a potential of zero.
[0032] (Negative voltage release process) Next, the application of the negative voltage applied between the gate terminal 21 and the source terminal 22 is released (step S27). Specifically, in the semiconductor device 100, the application of the voltage VGS- to the gate terminal 21 is released, and the application of the negative voltage that negatively biases the gate terminal 21 with respect to the source terminal 22 is released.
[0033] (2nd measurement process) Next, a positive voltage is applied between the drain terminal 23 and the source terminal 22 (step S28). Then, the leakage current IDSS2 is measured at the drain terminal 23 (step S29). For example, a positive voltage is applied to the drain terminal 23, and the potential of the source terminal 22 is set to 0, so that a voltage VDS is applied to the drain terminal 23 such that the drain terminal 23 is positively biased with respect to the source terminal 22. Then, with the voltage VDS applied to the drain terminal 23, the leakage current IDSS2 is measured at the drain terminal 23. At this time, the gate terminal 21 is floating or has a potential of 0, bringing it into an off state. Next, after measuring the leakage current IDSS2, the application of the positive voltage between the drain terminal 23 and the source terminal 22 is released (step S30). Specifically, the application of the voltage VDS to the drain terminal 23 is released.
[0034] (Sorting process) Next, the measured leakage currents IDSS1 and IDSS2 are compared to determine whether or not [IDSS1 / IDSS2<2] is satisfied (step S31). If [IDSS1 / IDSS2<2] is not satisfied (No in step S31), the inspected semiconductor device 100 is screened out as a defective product (step S32). Thus, the semiconductor device 100 inspected in the above series of processes is screened as conforming or non-conforming by comparing the leakage currents IDSS1 and IDSS2. If [IDSS1 / IDSS2<2] is satisfied (Yes in step S31), or after the semiconductor device 100 has been out-screened, the process according to this flowchart ends.
[0035] In the above-described inspection method, in step S20, a current equal to or greater than a predetermined value is passed between the source terminal 22 and the drain terminal 23. In this manner, by passing a relatively large current between the source terminal 22 and the drain terminal 23 through the conductive channel, the effect of defects in the gate insulating film 20 on the performance of the semiconductor device 100 can be made more evident. Therefore, in the processes of steps S21 to S25, the value of the leakage current IDSS1 can be made larger when the gate insulating film 20 contains many defects.
[0036] In the above-described inspection method, in step S21, a voltage VGS+ is applied between the gate terminal 21 and the source terminal 22 to discharge electrons trapped in defects contained in the gate insulating film 20. After the electrons are discharged from the gate insulating film 20, a voltage VDS is applied between the drain terminal 23 and the source terminal 22 to measure the leakage current IDSS1. Meanwhile, in step S26, a voltage VGS- is applied between the gate terminal 21 and the source terminal 22 to cause the defects contained in the gate insulating film 20 to recapture electrons. Then, after the electrons are recaptured from the gate insulating film 20, a voltage VDS is applied between the drain terminal 23 and the source terminal 22 to measure the leakage current IDSS2.
[0037] For this reason, in the above-mentioned inspection method, the measurement of the leakage current IDSS1 is affected by electrons discharged below the gate insulating film 20, whereas the measurement of the leakage current IDSS2 is not affected by electrons discharged below the gate insulating film 20. Therefore, by comparing the measured values of the two leakage currents IDSS1 and IDSS2, it is possible to inspect the effect of defects in the gate insulating film 20 on the leakage current IDSS1.
[0038] For example, when leakage current IDSS1 is greater than leakage current IDSS2 by a predetermined ratio or more, it can be determined that the gate insulating film 20 to be determined contains defects. Also, the larger the leakage current ratio calculated by [IDSS1 / IDSS2], the more defects are estimated to be contained in the gate insulating film 20. Therefore, the larger the leakage current ratio, the more likely it is that a malfunction will become apparent during long-term use.
[0039] In the semiconductor device 100, even if only good elements that do not contain defects in the gate insulating film 20 are present, there are cases where it is difficult to set a reference value for selecting good elements in advance because the leakage current IDSS1 varies widely among elements. Also, selection based on a set constant reference value may result in over-selection. In such cases, a method of selecting elements using the leakage current ratio [IDSS1 / IDSS2] is preferable.
[0040] In step S31, [IDSS1 / IDSS2<2] of the semiconductor device 100 is an example of a comparison standard of the leakage currents IDSS1 and IDSS2 for determining defects of the semiconductor device 100, and the ratio of IDSS1 to IDSS2 is not limited to this. The leakage current ratio of [IDSS1 / IDSS2] can be set arbitrarily as necessary.
[0041] In the inspection method of the flowchart shown in Fig. 3, the flow of current between the drain and source in step S20 and the application of voltage VGS- and measurement of IDSS2 in steps S26 to S30 may be performed, or only one of them may be performed. Preferably, both step S20 and steps S26 to S30 are performed as in the flowchart shown in Fig. 3. When both step S20 and steps S26 to S30 are performed, they may be performed consecutively, but it is preferable to perform steps S21 to S25 between step S20 and steps S26 to S30. That is, it is preferable to apply voltage VGS+ (positive voltage application step) and measure IDSS1 (first measurement step) between the current application step and the negative voltage application step. For example, it is preferable to perform the steps S20 to S25 in the order of the flowchart shown in FIG. 3 or after the steps S26 to S30. When the application of the voltage VGS- and the measurement of IDSS2 in steps S26 to S30 are not performed, in step S31, it is determined whether the leakage current IDSS1 is less than the reference value.
[0042] Also in the above-mentioned inspection method, after the voltage VGS+ is released in step S22, until the voltage VDS is applied in step S23, the gate terminal 21 is kept from being negatively biased with respect to the source terminal 22. Similarly, after the voltage VGS- is released in step S27, until the voltage VDS is applied in step S28, the gate terminal 21 is kept from being positively biased with respect to the source terminal 22. Furthermore, the time between step S22 and step S23, and between step S27 and step S28, should be short, preferably within 24 hours.
[0043] [Leakage current characteristics of semiconductor devices] The leakage current IDSS1, leakage current IDSS2, reference value, and leakage current ratio will be described with reference to Fig. 4 and Fig. 5. Fig. 4 and Fig. 5 are graphs showing characteristic curves of leakage current of semiconductor device 100 depending on the presence or absence of defects in gate insulating film 20. In each of Fig. 4 and Fig. 5, the horizontal axis indicates the voltage (drain-source voltage) between drain terminal 23 and source terminal 22, and the vertical axis indicates the value of leakage current (drain current) measured at drain terminal 23.
[0044] Fig. 4 is a graph showing the leakage current IDSS measured in step S13 in the inspection method for the semiconductor device 100 performed according to the above-mentioned flowchart shown in Fig. 2. In Fig. 4, the measured value of the leakage current IDSS of the semiconductor device 100 having no defects in the gate insulating film 20 is shown by a solid line. Also, the measured value of the leakage current IDSS of the semiconductor device 100 having a defect in the gate insulating film 20 is shown by a dashed line.
[0045] As shown in FIG. 4, the leakage current IDSS (dashed line) when the gate insulating film 20 has a defect is relatively high compared to the leakage current IDSS (solid line) when the gate insulating film 20 has no defect. In particular, excluding the low and high drain-source voltage regions, there is a difference in magnitude between the leakage current IDSS (solid line) when the gate insulating film 20 has no defect and the leakage current IDSS (dashed line) when the gate insulating film 20 has a defect. For this reason, the value of the voltage VDS applied in step S12 in the flowchart of FIG. 2 is set at a drain-source voltage where the difference between the leakage current IDSS (solid line) when there is no defect and the leakage current IDSS (dashed line) when there is a defect is large. Then, at this voltage VDS, a reference value used for the judgment in step S15 is set between the value of the leakage current IDSS (solid line) when there is no defect and the value of the leakage current IDSS (dashed line) when there is a defect. Thus, by comparing the leakage current IDSS1 measured at the voltage VDS in step S13 with the reference value, it is possible to detect a defect due to a defect in the gate insulating film 20 in the inspected semiconductor device 100.
[0046] 3. FIG. 5 shows a case where the leakage current IDSS1 and the leakage current IDSS2 are compared in the process of the flowchart shown in FIG. The measurement of leakage current IDSS2 in step S29 is performed after applying voltage VGS- between gate terminal 21 and source terminal 22 in step S26 to cause defects in gate insulating film 20 to recapture electrons. Because electrons are recaptured in the defects in gate insulating film 20, the measurement of leakage current IDSS2 is not affected by the defects in gate insulating film 20. For this reason, regardless of the presence or absence of defects in gate insulating film 20, leakage current IDSS2 approximately matches leakage current IDSS (solid line) when there are no defects in gate insulating film 20, as shown in FIG. Therefore, by comparing the leakage current IDSS1 and the leakage current IDSS2, if the leakage current IDSS1 is larger than the leakage current IDSS2, a defect in the semiconductor device 100 due to a defect in the gate insulating film 20 can be detected.
[0047] The leakage current ratio [IDSS1 / IDSS2] used in the judgment in step S31 can be set from the ratio between the leakage current IDSS (solid line) when there is no defect and the leakage current IDSS (dashed line) when there is a defect, at the voltage VDS applied in steps S23 and S28. Therefore, the reference value of the leakage current ratio [IDSS1 / IDSS2] can be arbitrarily set from the ratio between the leakage current IDSS (solid line) and the leakage current IDSS (dashed line) according to the configuration of the semiconductor device 100.
[0048] Furthermore, even if the leakage current ratio of [IDSS1 / IDSS2] exceeds the reference value, if the measured value of IDSS1 is less than the reference value, the semiconductor device 100 can be determined as a conforming product. For example, when the leakage current of the semiconductor device 100 is small and there are very few defects in the gate insulating film 20, it is possible that both of the leakage currents IDSS1 and IDSS2 will be very small. In this case, even if the ratio of [IDSS1 / IDSS2] does not satisfy the reference value, the measured value of IDSS1 will be less than the reference value. Such a semiconductor device 100 whose measured value of IDSS1 is less than the reference value may be determined as a conforming product regardless of the ratio of [IDSS1 / IDSS2].
[0049] [Examples of application of inspection methods] Next, a description will be given of the configuration of a semiconductor device to which the semiconductor device inspection method can be applied. Semiconductor devices are tested in a number of processes to select non-defective products before being shipped. The semiconductor device inspection method of this embodiment can be applied to semiconductor devices in any form, such as a wafer state, a chip state, or a package state.
[0050] (Wafer or chip testing) The above-mentioned semiconductor device inspection method can be applied to elements in a wafer state or a chip state. A semiconductor device 100 having a planar MOSFET structure as shown in Fig. 1 can be fabricated on a SiC substrate in a wafer state by a known technique such as ion implantation. In the wafer on which the semiconductor devices 100 are formed, the electrical characteristics of each semiconductor device 100 are evaluated by an inspection device, and non-defective products are selected.
[0051] Fig. 6 shows a schematic configuration of an inspection device for inspecting semiconductor devices and a semiconductor device in a wafer state, Fig. 7 shows a plan layout diagram of the semiconductor device in a wafer state, and Fig. 8 shows a cross-sectional view of the semiconductor device in a wafer state. As shown in Fig. 6, a plurality of semiconductor devices 100 are formed on a wafer-shaped semiconductor substrate 10. As shown in Figs. 7 and 8, the semiconductor device 100 formed on the wafer-shaped semiconductor substrate 10 has a gate terminal 21 and a source terminal 22 formed on a first main surface (front surface) of the semiconductor substrate 10. Also, a drain terminal 23 is formed on a second main surface (back surface) of the semiconductor substrate 10. Note that, although the configurations of the gate insulating film 20 and the conductive regions in the semiconductor substrate 10 are omitted in Figs. 7 and 8, the semiconductor device 100 has the same configuration as the semiconductor device 100 shown in Fig. 1.
[0052] 6, the inspection device 200 has a gate voltage source 201, a drain voltage source 202, and a leakage current meter 203. The gate voltage source 201 of the inspection device 200 is connected to the gate terminal 21 of the semiconductor device 100. The drain voltage source 202 is connected to the drain terminal 23 of the semiconductor device 100, and the leakage current meter 203 is provided between the drain voltage source 202 and the drain terminal 23. The inspection device 200 also has a wiring connected to the source terminal 22 of the semiconductor device 100.
[0053] As shown in FIG. 6, by connecting an inspection device 200 to a semiconductor device 100 formed on a wafer-shaped semiconductor substrate 10 and performing the process of the flowchart shown in FIG. 2 or 3 described above, the leakage current IDSS of the semiconductor device 100 can be measured. In addition, when inspecting the semiconductor device 100, it is also possible to measure the gate leakage current, threshold voltage, on-resistance when conductive, etc. using the same inspection equipment 200 before or after the screening process by measuring the leakage current IDSS, and add these to the inspection of the semiconductor device 100.
[0054] The wafer-like semiconductor substrate 10 after the above-mentioned inspection of the semiconductor device 100 is completed is diced into individual chips. The semiconductor device inspection method of this embodiment can be applied to the individual chips. Since SiC is a very hard material, large internal stress may occur during dicing, causing damage to the SiC crystal and the gate insulating film. Therefore, by applying the above-mentioned inspection method to the semiconductor device 100 in the chip state, it becomes possible to select defects that occur after the wafer inspection.
[0055] Another embodiment of the semiconductor device 100 with an insulated gate is a trench structure semiconductor device in which a groove is formed on the surface of SiC and a channel is formed in the vertical direction. Trench type semiconductor devices have the advantage of being able to increase the cell density per area and therefore lower the conduction resistance. The above-mentioned semiconductor device inspection method can be effectively applied to semiconductor device elements with an insulated gate of a trench structure because it can select semiconductor devices that have defects in the gate insulating film.
[0056] (Package testing) The individual chips cut from the wafer are assembled into discrete packages or power module packages. The assembly process includes steps such as soldering the chips to a circuit board or lead frame, wire bonding the surface electrodes, and sealing with insulating resin, and these steps can be performed using known methods. The above-mentioned semiconductor device inspection method can also be applied to screening assembled discrete packages and power module packages. Testing in the packaged state makes it possible to screen out defects that have newly occurred during the assembly process due to heat or stress during chip soldering, for example.
[0057] 9 shows the configuration of an example of a discrete package of a semiconductor device and the configuration of an inspection device 200. Note that the inspection device 200 shown in FIG. 9 has the same configuration as the inspection device 200 shown in FIG.
[0058] In the discrete package 101 shown in Fig. 9, a semiconductor chip (e.g., a semiconductor device 100) is sealed inside resin. A source terminal 103, a gate terminal 102, and a drain terminal 104 are drawn out from the resin sealing portion inside the discrete package 101 to the outside. In such a discrete package 101, a drain voltage source 202, a gate voltage source 201, a leakage current meter 203, and the like of an inspection device 200 are connected to the source terminal 103, the gate terminal 102, and the drain terminal 104. With the discrete package 101 and the inspection device 200 connected, the leakage current IDSS of the semiconductor device in the discrete package 101 can be measured by performing the process of the flowchart shown in Fig. 2 or 3 described above.
[0059] As an example of a power module package having a semiconductor device, there is a configuration in which a plurality of elements are incorporated in one package to form a circuit inside. As an example of this power module package, a 2-in-1 half-bridge type is shown in Figs. 10 and 11. Fig. 10 is a perspective view of a 2-in-1 half-bridge type power module and a configuration diagram of an inspection device 200, and Fig. 11 is a circuit diagram of a 2-in-1 half-bridge type semiconductor device. Note that the inspection device 200 has a similar configuration to the inspection device 200 shown in Fig. 8 described above.
[0060] As shown in Fig. 11, a 2-in-1 half-bridge type power module 130 has two MOSFETs, called an upper arm 110 and a lower arm 120, connected in series. An AC terminal is provided between the upper arm 110 and the lower arm 120. Note that the element shown as one MOSFET in the circuit diagram shown in Fig. 11 may be a plurality of MOSFET chips arranged in parallel.
[0061] 10, the exterior surface of the power module 130 is provided with a G1 terminal 111, an SS1 terminal 112, a P terminal 113, a G2 terminal 121, an SS2 terminal 122, an AC terminal 123, and an N terminal 124, which correspond to the respective terminals in the circuit diagram shown in FIG. 11. The respective terminals of the power module 130 are connected to a drain voltage source 202, a gate voltage source 201, and a leakage current meter 203 of the inspection device 200. In FIG. 10, the connections when inspecting the elements on the upper arm 110 side of the power module 130 are shown by solid lines. The connections when inspecting the elements on the lower arm 120 side are shown by dashed lines.
[0062] 10, leakage current IDSS can also be measured by performing the process of the flowchart shown in Fig. 2 or 3 described above with each terminal of power module 130 connected to inspection device 200. Then, leakage current IDSS is measured for the element on upper arm 110 side and the element on lower arm 120 side, and if both satisfy the conditions, power module 130 is selected as a non-defective product.
[0063] 10 shows a configuration in which elements on the upper arm 110 side and elements on the lower arm 120 side are inspected by changing the method of connection from the inspection device 200. Alternatively, two inspection devices 200 may be prepared and each may be connected to the elements on the upper arm 110 side and the elements on the lower arm 120 side for inspection. In addition to the 2-in-1 type, there are also power module packages such as 4-in-1 and 6-in-1, which package two or three half-bridge circuits, and the above-mentioned semiconductor device inspection method can be applied to each element of such packages as well.
[0064] The present invention is not limited to the above-described embodiments, and various modifications are possible. For example, the above-described embodiments have been described in detail to clearly explain the present invention, and the present invention is not necessarily limited to an embodiment having all of the configurations described. It is also possible to replace a part of the configuration of one embodiment with the configuration of another embodiment. It is also possible to add the configuration of another embodiment to the configuration of one embodiment. It is also possible to delete a part of the configuration of each embodiment, or to add or replace another configuration. [Explanation of symbols]
[0065] 10 semiconductor substrate, 11 drift layer, 13 body region, 14 source region, 15 contact region, 20 gate insulating film, 21, 102 gate terminal, 22, 103 source terminal, 104 drain terminal, 23, drain terminal, 100 semiconductor device, 101 discrete package 101, 110 upper arm 110, 111 G1 terminal 111, 112 SS1 terminal 112, 113 P terminal 113, 120 lower arm 120, 121 G2 terminal 121, 122 SS2 terminal 122, 123 AC terminal 123, 124 N terminal 124, 130 power module 130, 200 inspection device 200, 201 gate voltage source, 202 drain voltage source, 203 ammeter
Claims
1. A method for inspecting an insulated gate silicon carbide semiconductor device having a gate insulating film, a gate terminal, a source terminal, and a drain terminal, comprising the steps of: a positive voltage application step of applying a voltage VGS+ to the gate terminal such that the gate terminal is positively biased with respect to the source terminal; a positive voltage release step of releasing the application of the voltage VGS+; a first measurement step of measuring a leakage current IDSS1 while applying a voltage VDS such that the drain terminal is positively biased with respect to the source terminal. A method for inspecting a semiconductor device.
2. A screening process is included in which the leakage current IDSS1 is compared with a reference value to screen the semiconductor device.
2. The method for inspecting a semiconductor device according to claim 1.
3. Before the positive voltage application step or after the first measurement step, a negative voltage application step of applying a voltage VGS− to the gate terminal such that the gate terminal is negatively biased with respect to the source terminal; a negative voltage release step of releasing the application of the voltage VGS-; a second measuring step of measuring a leakage current I DSS2 while applying a voltage V D S such that the drain terminal is positively biased with respect to the source terminal.
2. The method for inspecting a semiconductor device according to claim 1.
4. A selection step of comparing the leakage current IDSS1 with the leakage current IDSS2 to select the semiconductor device is included.
4. The method for inspecting a semiconductor device according to claim 3.
5. Prior to the positive voltage application step, a current passing step is performed in which a voltage is applied to the gate terminal and a current of a predetermined value or more is passed through the conductive channel to the drain terminal.
4. The method for inspecting a semiconductor device according to claim 1.
6. In the current application step, a current having a value larger than 1 / 10 of the maximum rated current specification of the semiconductor device is applied.
6. The method for inspecting a semiconductor device according to claim 5.
7. After the positive voltage removing step, the gate terminal is maintained in a floating state or in a state shorted to the source terminal until the first measuring step is performed.
4. The method for inspecting a semiconductor device according to claim 1.
8. The time period from the positive voltage removal step to the first measurement step is within 24 hours.
4. The method for inspecting a semiconductor device according to claim 1.
Citation Information
Patent Citations
Method for selecting silicon carbide semiconductor device
JP2018205252A