Shotcrete
A concrete composition with specific ratios of cement, aggregate, gypsum, and rapid setting admixtures like calcium aluminate and sulfates enhances initial strength development in shotcrete, addressing unexpected strength increases and ensuring consistent performance across different construction sites.
Patent Information
- Application Number
- JP2023057282
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing shotcrete technologies face challenges in achieving high initial strength development without unexpected strength increases, which can lead to increased costs and time requirements, especially in varying construction site environments.
A concrete composition comprising cement, aggregate, gypsum, and a rapid setting admixture, with specific ratios and types of components, including calcium aluminate, alkali metal sulfate, and alkaline earth metal sulfate, is used to enhance initial strength development.
The composition achieves high initial and long-term strength development with improved adhesion, regardless of the type of quick-setting admixture, suitable for various construction environments.
Smart Images

Figure 2024145050000001
Abstract
Description
[Technical field]
[0001] The present invention relates to sprayed concrete. [Background technology]
[0002] In tunnels, mining pits, underground spaces, etc., sprayed concrete is used to prevent the collapse of excavation surfaces and to reinforce the ground during or after excavation. The quick setting properties of sprayed concrete ensure adhesion to the construction target, contributing to the reinforcement of the construction target.
[0003] In order to give quick-setting properties, quick-setting components are mixed into the sprayed concrete. Among them, powder quick-setting agents containing calcium aluminate, sodium aluminate, etc. as active ingredients can give strong quick-setting properties and can also obtain high strength. In the wet spraying method, which is a general application method for sprayed concrete, for example, at least cement, water, and aggregate are weighed and mixed to prepare base concrete, and then pumped to a spraying device via an agitator vehicle or the like during application. In the spraying device, a separate powder or liquid quick-setting agent is added to the base concrete being pumped, and mixing is carried out in the spraying nozzle of the spraying device to form sprayed concrete, which is then sprayed from the nozzle end hole. Mixing is carried out while the quick-setting components in the spraying device move from the point where they come into contact with water (water contact point) to the discharge hole at the end of the spraying nozzle, and the sprayed concrete is formed. The distance used for mixing is usually several tens of centimeters to several meters, and the travel time is the mixing time. Generally, the longer this distance, the more mixing progresses, the better the mixability, and the easier it is to obtain a more uniform concrete in terms of structure and properties.
[0004] In order to obtain such a sprayed concrete, the powdered quick-setting admixture mixed with the base concrete is generally the quick-setting component described above with various components added to adjust various properties. For example, a typical conventional powdered quick-setting admixture is made by mixing calcium aluminate with a high CaO content as a chemical component with gypsum to accelerate hardening, to which sodium aluminate to enhance early strength development and sodium carbonate to accelerate setting are added (for example, see Patent Documents 1 to 4). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2012-121763 A [Patent Document 2] JP 2003-012356 A [Patent Document 3] Patent No. 5129955 [Patent Document 4] JP 2020-011891 A Summary of the Invention [Problem to be solved by the invention]
[0006] In recent years, depending on the application and the environment of the construction site, there are cases where even higher early strength development than conventional shotcrete is required. In order to achieve high early strength development, it is possible to prepare high-strength shotcrete using a high-strength quick-setting additive, but there are also cases where an unexpected need for increased strength arises just before the start of construction or during construction. In such cases, it is necessary to prepare new materials, which can be costly and time-consuming.
[0007] Therefore, an object of the present invention is to provide a shotcrete that exhibits high early strength development regardless of the type of quick-setting admixture. [Means for solving the problem]
[0008] As a result of intensive research by the present inventors into the above-mentioned problems, it was discovered that by adjusting the amount of cement and then adding gypsum, a sprayed concrete with improved initial strength development can be obtained.
[0009] That is, the present invention is as follows. [1] A concrete composition containing cement, aggregate and gypsum, a quick-setting admixture and water, wherein the unit volume mass of the cement is 300 to 500 kg / m 3 The gypsum content is 1 to 10 parts by mass, calculated as an anhydride content, per 100 parts by mass of cement. [2] The sprayed concrete according to [1], wherein the quick-setting admixture comprises calcium aluminate, alkali metal sulfate, alkaline earth metal sulfate, and aluminum sulfate. [3] The sprayed concrete according to [1] or [2], wherein the fine aggregate ratio of the aggregate is 45 to 70 volume %. [4] The sprayed concrete according to [1] or [2], wherein the water-cement ratio is 40 to 70 mass %. Effect of the Invention
[0010] According to the present invention, it is possible to provide a shotcrete that exhibits high early strength development regardless of the type of quick-setting admixture. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the present invention will be described in detail. In this specification, the contents and the like are all calculated on a solid content basis and on an anhydrous basis.
[0012] The sprayed concrete of the present embodiment contains a concrete composition including cement, aggregate, and gypsum, a quick-setting admixture, and water.
[0013] [Concrete composition] The concrete composition includes cement, aggregate, and gypsum. Various types of cement can be used, for example, various types of Portland cement such as ordinary, early strength, ultra-early strength, low heat and moderate heat, ecocement, ultra-rapid hardening cement, fly ash cement, etc. One type of cement may be used alone, or two or more types may be used in combination. The cement is preferably Portland cement. When using Portland cement, the particle size is not particularly limited, for example, 2500 cm according to the JIS standard (JIS R 5210:2019). 2 / g or more.
[0014] The unit mass of cement is 300-500kg / m 3 If the unit mass of the cement is outside the above range, the initial and long-term strength development is reduced. From the viewpoint of further improving the initial and long-term strength development and further improving the adhesion, the unit mass of the cement is preferably 330 to 480 kg / m 3 is preferably 350 to 450 kg / m 3 It is more preferable that:
[0015] Examples of aggregates include fine aggregate and coarse aggregate. The fine aggregate is not particularly limited as long as it is a fine aggregate that can be used in mortar or concrete. The coarse aggregate is not particularly limited as long as it is a coarse aggregate that can be used in concrete. Both fine aggregate and coarse aggregate are preferred because they can easily secure a predetermined aggregate strength and are less likely to cause material separation due to their small specific gravity difference with other contained components, and therefore have a surface dry density of 2.3 to 2.9 g / cm. 3 It is preferable to use aggregates such as those mentioned above. Specific examples of such aggregates include fine aggregates such as natural aggregates, such as silica sand and limestone sand, and crushed sands, such as andesite, sandstone, and basalt, and coarse aggregates such as crushed stone and gravel, such as silica stone, limestone, andesite, sandstone, and basalt. One type of aggregate may be used alone, or two or more types may be used in combination.
[0016] The unit mass of fine aggregate is 700 to 1300 kg / m 3 is preferably 800 to 1200 kg / m 3 More preferably, it is 900 to 1100 kg / m 3When the unit volume mass of the fine aggregate is within the above range, the initial and long-term strength development is further improved. The unit mass of coarse aggregate is 400-900kg / m 3 is preferably 500 to 850 kg / m 3 More preferably, it is 600 to 800 kg / m 3 When the unit volume mass of the coarse aggregate is within the above range, the initial and long-term strength development is further improved.
[0017] The fine aggregate ratio of the aggregate ([volume of fine aggregate / volume of total aggregate]×100) is preferably 45 to 70 volume %, more preferably 50 to 68 volume %, and even more preferably 55 to 65 volume %. If the fine aggregate ratio of the aggregate is within the above range, pumpability during construction is further improved, and initial and long-term strength development is further improved.
[0018] Examples of gypsum include anhydrous gypsum, hemihydrate gypsum, and dihydrate gypsum. As the gypsum, anhydrous gypsum is preferable from the viewpoint of further improving the strength development. The gypsum may be used alone or in combination of two or more kinds. The fineness of the gypsum is preferably 3200 to 18000 cm in terms of Blaine specific surface area from the viewpoint of further improving the initial strength development. 2 / g, and 5000 to 15000 cm 2 / g, and more preferably 5500 to 14000 cm 2 / g, and more preferably 7000 to 12000 cm 2 / g is particularly preferred.
[0019] The content of the gypsum is 1 to 10 parts by mass, calculated as an anhydride, relative to 100 parts by mass of cement. If the content of the gypsum is outside the above range, initial and long-term strength development is insufficient. From the viewpoint of further improving initial and long-term strength development and adhesion, the content of the gypsum is preferably 1.5 to 9 parts by mass, more preferably 2 to 7 parts by mass, calculated as an anhydride, relative to 100 parts by mass of cement.
[0020] Various admixtures (materials) may be blended into the concrete composition as long as the effects of the present invention are not impaired. Examples of admixtures (materials) include water-reducing agents, expansive agents, defoamers, waterproofing agents, rust inhibitors, shrinkage reducing agents, thickeners, water retention agents, pigments, water repellents, efflorescence inhibitors, fibers, and pozzolanic substances.
[0021] The concrete composition can be prepared by mixing the above-mentioned components using a commonly used mixing tool, and the tool is not particularly limited. Examples of the mixing tool include a concrete mixer.
[0022] [Quick setting admixture] The quick-setting admixture may be either a powder or a liquid. From the viewpoint of high quick-setting property, the quick-setting admixture is preferably a powder. Examples of the powder quick-setting admixture include those containing calcium aluminate, alkali metal sulfate, alkaline earth metal sulfate, and aluminum sulfate. Examples of the liquid quick-setting admixture include those containing aluminum sulfate as a main component in addition to alkali metal carbonate, and commercially available liquid quick-setting admixtures can also be used.
[0023] Calcium aluminate is an inorganic hydration active material whose main chemical components are CaO and Al2O3, and the molar ratio of CaO to Al2O3 (CaO / Al2O3) is preferably 2.0 to 2.7, more preferably 2.1 to 2.65, and more preferably 2.15 to 2.6. If the molar ratio of CaO to Al2O3 is within the above range, it becomes easier to achieve both quick setting and workability. Calcium aluminate may contain other components such as impurities other than CaO and Al2O3 derived from the raw materials, regardless of their form of existence, as long as they do not impair the effects of the present invention.
[0024] Calcium aluminate may be crystalline, amorphous, or a mixture thereof. From the viewpoint of obtaining a better quick-setting property, calcium aluminate preferably has a vitrification rate, which is the degree of amorphization, of 60% by mass or more, more preferably 80% by mass or more, and even more preferably 95% by mass or more. The fineness of calcium aluminate is not particularly limited, but since it is easy to obtain an appropriate reaction activity when used as a quick-setting admixture for concrete, it is preferable that the fineness is the same as or higher than that of the cement in the base concrete to be mixed, and for example, a Blaine specific surface area of 3000 to 6500 cm 2 The powder size is 0.1 to 1.0 μm / g.
[0025] Calcium aluminate can be obtained, for example, by heating a mixture of raw materials, which are a CaO source and an Al2O3 source, so as to obtain a molar ratio of CaO and Al2O3 as the desired chemical components, until it melts. In addition, since the structural state of calcium aluminate after cooling varies depending on the cooling process after heating during production, the vitrification rate, which is the degree of amorphization, can be adjusted depending on the cooling conditions such as the cooling rate.
[0026] The content of calcium aluminate is preferably 55 to 85 mass%, more preferably 58 to 83 mass%, further preferably 60 to 80 mass%, and particularly preferably 65 to 78 mass%, based on the total mass of the quick-setting admixture. If the content of calcium aluminate is within the above range, it is easy to achieve both quick-setting property and mixability.
[0027] The alkali metal sulfate is not particularly limited and any one can be used, and anhydride is preferable because it has excellent reactivity. Examples of the alkali metal include lithium, sodium, potassium, etc., and sodium is preferable. The alkali metal sulfate may be used alone or in combination of two or more kinds.
[0028] The content of the alkali metal sulfate is preferably 1 to 20 parts by mass, more preferably 3 to 18 parts by mass, further preferably 5 to 15 parts by mass, and particularly preferably 6 to 14 parts by mass, based on 100 parts by mass of calcium aluminate in anhydride equivalent. When the content of the alkali metal sulfate is within the above range, the quick-setting property and the initial and long-term strength development are likely to be excellent.
[0029] The alkaline earth metal sulfate is not particularly limited and any of them can be used, and it is preferable that it is anhydrous because it has excellent reactivity. Examples of alkaline earth metals include magnesium and calcium, and among them, calcium is preferable. The alkaline earth metal sulfate may be used alone or in combination of two or more kinds. The particle size and grain size of the alkaline earth metal sulfate are also not particularly limited, and for example, the Blaine specific surface area is 4000 to 8500 cm. 2 / g.
[0030] The content of the alkaline earth metal sulfate is preferably 10 to 65 parts by mass, more preferably 11 to 60 parts by mass, further preferably 12 to 50 parts by mass, and particularly preferably 13 to 35 parts by mass, calculated as an anhydride, relative to 100 parts by mass of calcium aluminate. When the content of the alkaline earth metal sulfate is within the above range, the long-term strength development is likely to be excellent.
[0031] The mass ratio of the alkali metal sulfate and the alkaline earth metal sulfate in the quick-setting admixture ([mass of the alkaline earth metal sulfate] / [mass of the alkali metal sulfate]) is preferably 1.1 to 5, more preferably 1.2 to 4, even more preferably 1.3 to 3, and particularly preferably 1.4 to 2.5, calculated on an anhydride basis. When the mass ratio of the alkali metal sulfate and the alkaline earth metal sulfate is within the above range, quick-setting properties, mixability, and long-term strength development are easily obtained.
[0032] Aluminum sulfate may be in any form, for example, 16-hydrate, anhydrous form, etc., with the 16-hydrate being preferred. The content of aluminum sulfate is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 8 parts by mass, and even more preferably 1 to 5 parts by mass, calculated as an anhydride, relative to 100 parts by mass of calcium aluminate. If the content of aluminum sulfate is within the above range, it is easy to ensure long-term strength development even when the quick-setting property is increased in a low-temperature environment.
[0033] The mass ratio of the alkali metal sulfate to aluminum sulfate in the quick-setting admixture ([mass of aluminum sulfate] / [mass of alkali metal sulfate]) is preferably 0.05 to 2, more preferably 0.1 to 1.8, and even more preferably 0.14 to 1.5, calculated on anhydrous basis. When the mass ratio of the alkali metal sulfate to aluminum sulfate is within the above range, quick-setting properties, mixability, and strength development are easily obtained.
[0034] The quick-setting admixture is produced by mixing the above-mentioned components. The mixing method is not particularly limited, and for example, a general-purpose mixer such as a tilting mixer, a pan mixer, a twin-shaft mixer, a grout mixer, a Hobart mixer, an Omni mixer, or a Henschel mixer can be used.
[0035] The amount of the quick-setting admixture is preferably 5 to 15 parts by mass, more preferably 6 to 14 parts by mass, and even more preferably 7 to 13 parts by mass, relative to 100 parts by mass of cement. If the amount of the quick-setting admixture added is within the above range, it is easy to achieve both quick-setting properties and mixability.
[0036] [Sprayed concrete] For example, sprayed concrete may be produced by a wet spraying method in which each material except for the quick-setting admixture and water are mixed in a concrete mixer or the like to form base concrete, and the base concrete and the quick-setting admixture are mixed at the tip of a spray nozzle and sprayed, or it may be produced by a dry spraying method in which each material including the quick-setting admixture is mixed to form a base composition, and the base composition and water are mixed at the tip of a spray nozzle and sprayed. It is preferable to produce sprayed concrete by the wet spraying method, from the viewpoint that dust and rebound are more easily reduced and the materials can be mixed more uniformly.
[0037] The amount of water in sprayed concrete can be adjusted appropriately depending on factors such as the purpose and location of use. The unit volume mass of water is 100 to 350 kg / m 3 is preferably 150 to 300 kg / m 3 More preferably, it is 170 to 250 kg / m 3 It is more preferable that the unit volume mass of water is within the above range. When the unit volume mass of water is within the above range, pumpability during construction is further improved, and high strength development is easily ensured. The amount of water can be adjusted within the above range whether the wet spraying method or the dry spraying method is used.
[0038] The water-cement ratio of the sprayed concrete ([mass of water / mass of cement]×100) is preferably 40-70 mass%, more preferably 45-65 mass%, and even more preferably 50-60 mass%. If the water-cement ratio is within the above range, the initial and long-term strength development and adhesion are further improved.
[0039] When the sprayed concrete hardens, the compressive strength at 15 minutes measured at 20℃ in accordance with the Japan Society of Civil Engineers standard JSCE-G561:2010 is 1.15N / m 2 It is preferable that the resistance is 1.3N / m or more. 2 More preferably, it is 1.45 N / m or more. 2 More preferably, the compressive strength at 15 minutes is 2.5N / m 2If the compressive strength of the sprayed concrete at an age of 15 minutes is within the above range, the initial strength development will be even better.
[0040] The sprayed concrete of the present embodiment has excellent initial and long-term strength development and good adhesion. In addition, even if a commonly used quick-setting admixture is used, the initial strength development can be easily improved by adjusting the mix ratio of the concrete composition. Therefore, the sprayed concrete of the present embodiment can be suitably used for spraying on tunnel walls, slopes, environments with spring water, environments with soft ground, etc. EXAMPLES
[0041] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. The examples were carried out in an environment of 20±1° C. unless otherwise specified. In the examples, the contents and the like are all calculated on a solid content basis and on an anhydrous basis.
[0042] [material] ·Rapid setting admixture Calcium aluminate: CaO / Al2O3 is 2.5, Blaine specific surface area is 5400cm 2 / g, vitrification rate 95% by mass Sodium sulfate reagent: anhydrous sodium sulfate Calcium sulfate reagent: anhydrite Aluminum sulfate reagent: 16-hydrate Base concrete Cement: Ordinary Portland cement, Blaine specific surface area 3200cm 2 / g, density 3.15g / cm 3 Aggregate: Mixture of fine and coarse aggregate (fine aggregate ratio 60% by volume) Fine aggregate: Limestone fine aggregate (surface dry density: 2.65g / cm 3 , center grain size; 0.6mm) Coarse aggregate: crushed stone (surface dry density: 2.74 g / cm 3 , particle size 5~15mm) Gypsum: Anhydrous gypsum, Brain specific surface area 11000cm 2 / g
[0043] [Preparation of quick-setting admixture] The mixture was designed to contain 100 parts by mass of calcium aluminate, 1.7 parts by mass of aluminum sulfate, 10.8 parts by mass of sodium sulfate, and 20 parts by mass of calcium sulfate, and was mixed in a Henschel mixer to produce a quick-setting admixture.
[0044] [Preparation of base concrete] The cement, aggregate, water, and gypsum were mixed to the unit volume and parts by mass shown in Table 1, and each material was mixed for 2 minutes in a concrete mixer to prepare base concrete. The amount of gypsum is based on 100 parts by mass of cement.
[0045] [Preparation of sprayed concrete] The base concrete was put into a supply tank immediately after mixing, and was pumped from there to the spraying device via a resin hose about 10 m long and 6 cm in inner diameter. The spraying device is a commercially available product whose basic components are a pressure pipe with an inner diameter of 2 inches through which the base concrete is pressure-fed, a cylindrical side pipe (air supply section) that is connected to the side of the pressure pipe at an inclination angle of about 30 degrees to supply and add air to the base concrete, a cylindrical side pipe (quick-setting admixture supply section) that is connected to the side of the pressure pipe at an inclination angle of about 30 degrees to supply and add additives (quick-setting admixture) to the base concrete, and a spray nozzle with an inner diameter (tip hole diameter) of 2 inches for spraying the shotcrete. The side pipe, which supplies the quick-setting admixture, was formed by placing a steel T-shaped pipe (three-way pipe) between the main pressure pipe and the injection nozzle. The main pressure pipe and the injection nozzle were connected to two of the pipe openings located on a straight line of the T-shaped pipe, respectively, and the remaining pipe opening was connected to a supply pipe for the quick-setting admixture, which was sent separately. The base concrete and the quick-setting admixture were mixed in the distance from the addition position of the quick-setting admixture to the base concrete inside the T-shaped pipe (the joining point of the base concrete and the quick-setting admixture) to the end of the injection nozzle hole, and this distance (hereinafter referred to as the mixing distance) was 3m. The quick-setting admixture is added to the base concrete being pumped in the spraying device by pumping a specified amount of it with compressed air. The added concrete is mixed while traveling a specified mixing distance to produce the sprayed concrete. The amount of quick-setting admixture to be added is 8 parts by mass per 100 parts by mass of cement.
[0046] [Evaluation method] The various evaluation methods for the shotcrete are as follows. The evaluation results are shown in Table 1. -Evaluation of strength development of sprayed concrete The shotcrete prepared with a mixing distance of 3 m was immediately sprayed into a molding form with inner dimensions of 30 x 40 x 20 cm after preparation, so as to fill the form. This was placed in a thermostatic chamber at 20°C (±1°C) and after a specified time had elapsed, a cylindrical specimen with a diameter of 5 cm and a height of 10 cm was taken from the hardened concrete in the form using a core drill, and a specimen with a material age of 28 days was obtained. The unconfined compressive strength of this 28-day-old specimen was measured using an Amsler type compressive strength tester. In addition, using a pull-out test form and embedding tool specified in the Japan Society of Civil Engineers standard JSCE-G561:2010, shotcrete prepared in the same manner was subjected to a pull-out test in accordance with JSCE-G561:2010. The compressive strength of the shotcrete at 15 minutes and 24 hours was measured by this test.
[0047] -Evaluation of adhesion of sprayed concrete The above-mentioned spraying device was used to immediately spray the obtained sprayed concrete. The sprayed concrete was sprayed from a 10m hole toward a 9 mm thick, 3 m square concrete flat surface that was vertically installed at a point about 100 cm away from the nozzle end of the spraying device. 3 The sprayed concrete was sprayed at a flow rate of 1 / hour. The adhesion of the sprayed concrete was evaluated by visual observation as follows. ◎: Smooth pressure delivery, little dripping or rebounding, and thick spraying possible ○: No pulsation or bursting during pumping, no peeling, no adhesion
[0048] [Table 1]
[0049] The sprayed concrete of the Example showed high strength development from the early stage to the long term, and also had good adhesion. The sprayed concrete of the Comparative Example did not show good strength development, especially in the early stage such as 15 minutes.
Claims
1. A concrete composition including cement, aggregate, and gypsum, a quick-setting admixture, and water, The unit volume mass of the cement is 300 to 500 kg / m 3 and The sprayed concrete has a gypsum content of 1 to 10 parts by mass, calculated as an anhydride content, per 100 parts by mass of the cement.
2. 2. The sprayed concrete of claim 1, wherein the quick-setting admixture comprises calcium aluminate, alkali metal sulfate, alkaline earth metal sulfate, and aluminum sulfate.
3. The sprayed concrete according to claim 1 or 2, wherein the fine aggregate ratio of the aggregate is 45 to 70 volume %.
4. The sprayed concrete according to claim 1 or 2, wherein the water-cement ratio is 40 to 70 mass%.
Citation Information
Patent Citations
Itonohinshitsuhyokasochi
JP1976029955A
Quick setting agent for shotcrete
JP2003012356A
Quick setting agent for spraying and sprayed concrete using the same, and spraying method
JP2012121763A
High strength concrete for spraying
JP2020011891A