Anchor coating agent for vapor deposition and method for producing substrate for vapor deposition
The anchor coating agent, composed of specific solvents and resins, addresses the issues of residue-induced adhesion problems and short pot life by enhancing blocking resistance and adhesion, ensuring stable film formation and extended usability.
Patent Information
- Application Number
- JP2023057372
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing anchor coating agents for vapor deposition suffer from issues such as sticky residues leading to adhesion or delamination between deposition substrates and metal films, due to incomplete crosslinking reactions and short pot life, which affect the blocking resistance and adhesion of metal films.
An anchor coating agent comprising an alcoholic solvent, an aprotic solvent, a polyisocyanate compound, and an acrylic resin with a glass transition temperature above 50°C, formulated to provide a balanced composition that enhances blocking resistance and adhesion, with a long pot life.
The solution results in an anchor coat layer with excellent blocking resistance and adhesion to metal films, ensuring stable film formation and prolonged usability of the coating agent.
Smart Images

Figure 2024145124000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an anchor coating agent for deposition that can be used for metal deposition, and a method for producing a substrate for deposition using the same. [Background technology]
[0002] Surface processing technology by vapor deposition is capable of forming thin metal films on a variety of substrates, such as various resin substrates and glass substrates, and is therefore used in applications such as conductive materials, food barrier films, surface decoration, etc. In general, when forming a thin metal film on a substrate by vapor deposition, an anchor coat layer is often provided on the substrate in advance, and the thin metal film is formed on the anchor coat layer to ensure adhesion between the metal and the substrate.
[0003] For example, JP 2010-229291 A (Patent Document 1) discloses a deposition film having an anchor coat layer formed using an aqueous polyurethane resin, and JP 2021-178899 A (Patent Document 2) discloses an anchor coat agent containing a glycidyl group-containing (meth)acrylic resin, an isocyanate compound, and an organic solvent.
[0004] Generally, a tough coating film can be obtained by a crosslinking reaction, and therefore resin compositions such as paints and adhesives containing a polyisocyanate compound are widely known, as in Patent Document 2. However, since the crosslinking reaction between a polyisocyanate compound and a resin proceeds gradually even in a solution or dispersion, these resin compositions generally have a life span (pot life) during which sufficient coating film performance can be obtained after production.
[0005] As a measure to extend the pot life of a resin composition containing a polyisocyanate compound, JP 2006-97018 A (Patent Document 3) and JP 2020-147644 A (Patent Document 4) disclose compositions containing an isocyanate group blocking agent or a water-absorbent filler. In addition, JP 2013-199582 A (Patent Document 5), JP 2015-166404 A (Patent Document 6), and JP 2016-74780 A (Patent Document 7) disclose compositions and adhesives in which the reactivity of a urethane metal catalyst is controlled by a chelating agent or the like.
[0006] Although the method described in the above document is capable of achieving both a long pot life and high crosslinking reactivity, various additives in the resin composition often remain in the coating film. If the anchor coat layer contains a large amount of residues other than the resin, the anchor coat layer becomes sticky, which may cause adhesion or layer peeling between the stacked deposition substrates (blocking), or may reduce the adhesion between the deposition substrate and the deposited metal film, and therefore improvements have been required. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2010-229291 A [Patent Document 2] Patent Publication No. 2021-178899 [Patent Document 3] JP 2006-97018 A [Patent Document 4] JP 2020-147644 A [Patent Document 5] JP 2013-199582 A [Patent Document 6] JP 2015-166404 A [Patent Document 7] JP 2016-74780 A Summary of the Invention [Problem to be solved by the invention]
[0008] The problem that the present invention aims to solve is to provide an anchor coating agent for deposition that can form an anchor coating layer that is excellent in blocking resistance and adhesion to a metal film on a deposition substrate and has a long pot life, and a method for producing a deposition substrate that can obtain an anchor coating layer that is excellent in blocking resistance and adhesion to a metal film. [Means for solving the problem]
[0009] The object of the present invention has been achieved by the following means. (1) An anchor coating agent for vapor deposition containing at least an alcohol-based solvent, an aprotic solvent, a polyisocyanate compound, and an acrylic resin having a glass transition temperature higher than 50°C, wherein the proportion of the alcohol-based solvent in the entire anchor coating agent is 25 to 63 mass%. (2) A method for producing a substrate for deposition, comprising applying the anchor coating agent for deposition according to (1) above to a surface of a substrate and drying the same to form an anchor coating layer. Effect of the Invention
[0010] The present invention can provide an anchor coating agent for deposition that can form an anchor coating layer that is excellent in blocking resistance and adhesion to a metal film and has a long pot life, and a method for producing a substrate for deposition that can provide an anchor coating layer that is excellent in blocking resistance and adhesion to a metal film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention will be described in detail below.
[0012] The anchor coating agent for deposition of the present invention contains an alcohol-based solvent. The alcohol-based solvent in the present invention is an organic solvent having one or more hydroxyl groups in the molecule, and known alcohol-based solvents such as methanol, ethanol, denatured ethanol, isopropyl alcohol, butanol, tertiary butanol, pentanol, benzyl alcohol, and ethylene glycol can be used as such an organic solvent. Among them, alcohol-based solvents having 5 or less carbon atoms are preferred, and alcohol-based solvents having 3 or less carbon atoms are particularly preferred, because they are easily removed in the drying process when forming the anchor coat layer.
[0013] The proportion of the alcohol-based solvent in the entire anchor coating agent for deposition of the present invention is 25 to 63 mass%. If the proportion of the alcohol-based solvent is less than 25 mass%, the pot life of the anchor coating agent for deposition is shortened, and the agent becomes highly viscous and gels over time. In addition, the tackiness of the surface of the formed anchor coating layer increases over time, making blocking more likely to occur. Conversely, if the proportion of the alcohol-based solvent exceeds 63 mass%, good blocking resistance cannot be obtained.
[0014] The anchor coating agent for deposition of the present invention contains an aprotic solvent. The aprotic solvent in the present invention is not particularly limited except that it is an organic solvent that does not have a proton-donating functional group, but it is preferable that it is a solvent that dissolves or disperses components such as acrylic resins that coexist in the anchor coating agent for deposition and has a glass transition temperature higher than 50°C, and is miscible with alcohol-based solvents. Specifically, known aprotic solvents can be used, such as ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, ester-based solvents such as ethyl acetate, propyl acetate, butyl acetate, and γ-butyrolactone, ether-based solvents such as diethyl ether, diisopropyl ether, 1,4-dioxane, and tetrahydrofuran, hydrocarbon-based solvents such as toluene, xylene, and solvent naphtha, amide-based solvents such as dimethylformamide, dimethylacetamide, and N-methylpyrrolidone, nitrile-based solvents such as acetonitrile, and halogen-based solvents such as dichloromethane, chloroform, and 1,2-dichloroethane.
[0015] The volatility of the alcohol-based solvent and the aprotic solvent in the present invention is not particularly limited, but it is preferable that they are removed by evaporation in a general drying process because of the convenience of forming an anchor coat layer by coating and drying, etc. From this viewpoint, alcohol-based solvents and aprotic solvents having a vapor pressure of 2 kPa or more at 20°C are preferable. In addition, it is preferable that the boiling point is 120°C or less.
[0016] The anchor coating agent for deposition of the present invention contains an acrylic resin having a glass transition temperature (Tg) of higher than 50° C. The acrylic resin in the present invention is not particularly limited as long as it is an acrylic resin having a Tg of higher than 50° C., but in order to toughen the anchor coating layer by a crosslinking reaction with a polyisocyanate compound, it is preferable that the acrylic resin has a functional group (hydroxy group, carboxy group, amino group, etc.) that reacts with an isocyanate group, and it is particularly preferable that the acrylic polyol resin has a hydroxy group. These may be synthesized by a polymerization reaction of acrylic acid and methacrylic acid derivatives, or commercially available products may be used. As a commercially available product, acrylic resins dissolved or dispersed in various organic solvents are known. For example, known commercially available products such as ACRYDIC (registered trademark) (54-270, A-814, A-817, A-859-B, AU-7005, AU-7007, BU-955, FU-1031, WBU-1218, WFU-289, WFU-580, WLU-738, WNL-200, WNU-533, WXU-880-BA, WZU-591) manufactured by DIC Corporation, and COATAX (registered trademark) LH (408, 601, 613, 629) manufactured by Toray Fine Chemicals Co., Ltd. can be used. In order to improve the blocking resistance of the deposition substrate and the pot life, the hydroxyl value of the acrylic resin in the present invention is preferably 60 mgKOH / g or less, more preferably 45 mgKOH / g or less, and particularly preferably 40 mgKOH / g or less. The preferred lower limit of the hydroxyl value is 5 mgKOH / g or more. Similarly, in order to improve the blocking resistance, the particularly preferred Tg of the acrylic resin in the present invention is 80° C. or more.
[0017] The anchor coating agent for deposition of the present invention contains a polyisocyanate compound. The polyisocyanate compound in the present invention is a compound containing two or more isocyanate groups in the molecule, and the compound itself or a commercially available product in which the compound is dissolved or dispersed in a solvent may be used. Specifically, known polyisocyanate compounds such as Burnock (registered trademark) (DN-950, DN-980, DN-981) manufactured by DIC Corporation and Duranate (registered trademark) (24A-100, TPA-100, P301-75E) manufactured by Asahi Kasei Corporation can be used. Polyisocyanate compounds are known to be of the isocyanurate type, adduct type, biuret type, and other types depending on the molecular structure, and among them, the isocyanurate type is preferred because of its excellent drying properties of the coating film.
[0018] The proportion of the polyisocyanate compound in the present invention is not particularly limited, but in order to form a tough anchor coat layer by crosslinking reaction with the acrylic resin, it is preferable that the content is 1% by mass or more, more preferably 5% by mass or more, based on the acrylic resin in terms of solid content. The upper limit is preferably 50% by mass or less. The retention rate of the isocyanate group (NCO) of the polyisocyanate compound is not particularly limited, but is preferably 10% by mass or more of the polyisocyanate compound.
[0019] In the present invention, the alcohol-based solvent, the aprotic solvent, the polyisocyanate compound, and the acrylic resin may each be used alone or in combination of two or more kinds.
[0020] The anchor coating agent for vapor deposition of the present invention may contain various components such as a protic solvent such as water, a resin other than acrylic resin, inorganic particles, a surfactant, an ultraviolet absorber, a pH adjuster, in addition to the alcohol-based solvent, the aprotic solvent, the polyisocyanate compound, and the acrylic resin.
[0021] The anchor coating agent for deposition of the present invention can be produced by mixing the above-mentioned components. The mixing method is not particularly limited, and a known mixing method can be used. For example, after mixing the desired alcohol solvent and aprotic solvent, the above-mentioned acrylic resin and polyisocyanate compound are added, and the mixture can be obtained by performing a known mixing process such as stirrer stirring, propeller stirring, turbine type stirring, homomixer type stirring, media mill, pressure type disperser, ultrasonic disperser, micromixer, static mixer, etc. The solid content concentration of the anchor coating agent for deposition is not particularly limited, but since a high solid content concentration increases the viscosity of the coating liquid and makes it difficult to form a uniform layer, it is preferably 50 mass% or less, more preferably 30 mass% or less. The lower limit is preferably 5 mass% or more.
[0022] Next, the method for producing the substrate for deposition in the present invention will be described. The substrate to which the anchor coating agent for deposition is applied is not particularly limited, and known substrates such as polyester resin, diacetate resin, triacetate resin, acrylic resin, polycarbonate resin, polyvinylidene fluoride resin, cellophane, celluloid, cycloolefin, and glass can be used. In particular, the alcohol-based solvent contained in the anchor coating agent for deposition of the present invention is unlikely to corrode the resin substrate, so it can be suitably used for resin substrates with low solvent resistance such as polycarbonate resin.
[0023] In the present invention, the method of applying the anchor coating agent for deposition to the surface of a substrate is not particularly limited, and examples thereof include known coating methods such as bar coating, spin coating, slit coating, die coating, blade coating, gravure coating, curtain coating, spray coating, and kiss coating, and known printing methods such as gravure printing, flexographic printing, inkjet printing, screen printing, offset printing, gravure offset printing, dispenser printing, and pad printing. Furthermore, after coating or printing by these methods, it is possible to obtain a substrate for deposition having an anchor coating layer laminated on the substrate surface by drying by a known method such as hot air drying, infrared drying, and natural drying.
[0024] When the deposition substrate is manufactured by the present invention, the thickness of the anchor coat layer is not particularly limited, but in order to ensure sufficient adhesion of the metal film, the dry thickness is preferably 5 μm or less, more preferably 1 μm or less. In addition, the lower limit is practically 0.01 μm or more. The drying temperature is also not limited, but it is preferable to heat and dry at 60° C. or more.
[0025] In the production of the deposition substrate according to the present invention, it is preferable to heat the deposition substrate after drying in order to promote curing of the anchor coat layer by the crosslinking reaction between the acrylic resin and the polyisocyanate compound. The heating conditions are not particularly limited, but it is preferable to heat the substrate at a temperature of 40° C. or higher for 15 hours or longer.
[0026] There is no limitation on the metal material that can be vapor-deposited on the vapor deposition base material obtained by the present invention, and known metal materials such as aluminum, chromium, zinc, gold, silver, platinum, nickel, etc. The vapor deposition method of the metal material is also not particularly limited, and known vapor deposition methods such as vacuum vapor deposition can be used. EXAMPLES
[0027] The present invention will be described in detail below using examples, but the present invention is not limited to the following examples as long as it does not deviate from the gist of the present invention. In addition, percentages in the description are based on mass unless otherwise specified.
[0028] "Preparation of deposition substrate 1" The following components were mixed and stirred for 3 minutes at 100 rpm using a magnetic stirrer to prepare anchor coating agent 1 for deposition. Methanol (vapor pressure 13.3 kPa at 20°C, boiling point 64.5°C) 28 g Methyl ethyl ketone (vapor pressure 9.5 kPa at 20°C, boiling point 79.6°C) 28 g DN-980 (DIC Corporation isocyanurate type polyisocyanate, solid content 75%, contains ethyl acetate as a solvent component) 2.4g WXU-880-BA (acrylic resin manufactured by DIC Corporation, Tg 90°C, hydroxyl value 7.0-13.0 mgKOH / g, solid content concentration 50%, contains isobutyl acetate and methyl isobutyl ketone as a solvent) 20 g (Alcohol-based solvent ratio: 36%)
[0029] On the side not having the protective film of Technoloy (registered trademark) C000 (polycarbonate film manufactured by Sumitomo Chemical Co., Ltd., with a protective film on one side), the anchor coating agent 1 for deposition immediately after preparation was applied by a bar coating method so as to have a dry film thickness of 0.5 μm, and dried for 1 minute in a dryer at 95° C. The dried film was heated at 50° C. for 24 hours to prepare the substrate 1 for deposition.
[0030] "Preparation of deposition substrate 2" A substrate for deposition 2 was prepared in the same manner as in the preparation of the substrate for deposition 1, except that the anchor coating agent 1 for deposition was changed to the anchor coating agent 2 for deposition described below.
[0031] <Anchor coating agent for vapor deposition 2> Ethanol (vapor pressure 6.4 kPa at 20°C, boiling point 78.3°C) 28 g Methyl ethyl ketone 28g DN-980 2.4g WXU-880-BA 20g (Alcohol-based solvent ratio: 36%)
[0032] "Preparation of deposition substrate 3" A substrate for deposition 3 was prepared in the same manner as in the preparation of the substrate for deposition 1, except that the anchor coating agent 1 for deposition was changed to the anchor coating agent 3 for deposition described below.
[0033] <Anchor coating agent for vapor deposition 3> Isopropyl alcohol (vapor pressure 4.3 kPa at 20°C, boiling point 82.3°C) 28 g Methyl ethyl ketone 28g DN-980 2.4g WXU-880-BA 20g (Alcohol-based solvent ratio: 36%)
[0034] "Preparation of deposition substrate 4" A substrate for deposition 4 was prepared in the same manner as in the preparation of the substrate for deposition 1, except that the anchor coating agent 1 for deposition was changed to the anchor coating agent 4 for deposition described below.
[0035] <Anchor coating agent for vapor deposition 4> 28g isopropyl alcohol Ethyl acetate (vapor pressure 9.7 kPa at 20°C, boiling point 77°C) 28 g DN-980 2.4g WXU-880-BA 20g (Alcohol-based solvent ratio: 36%)
[0036] "Preparation of deposition substrate 5" A substrate for deposition 5 was prepared in the same manner as in the preparation of the substrate for deposition 1, except that the anchor coating agent 1 for deposition was changed to the anchor coating agent 5 for deposition described below.
[0037] <Anchor coating agent for vapor deposition 5> 28g isopropyl alcohol Toluene (vapor pressure 2.9 kPa at 20°C, boiling point 110.6°C) 28 g DN-980 2.4g WXU-880-BA 20g (Alcohol-based solvent ratio: 36%)
[0038] "Preparation of deposition substrate 6" A substrate for deposition 6 was prepared in the same manner as in the preparation of the substrate for deposition 1, except that the anchor coating agent 1 for deposition was changed to the anchor coating agent for deposition 6 described below.
[0039] <Anchor coating agent for vapor deposition 6> 45g isopropyl alcohol Methyl ethyl ketone 11g DN-980 2.4g WXU-880-BA 20g (Alcohol-based solvent content: 57%)
[0040] "Preparation of deposition substrate 7" A substrate for deposition 7 was prepared in the same manner as in the preparation of the substrate for deposition 1, except that the anchor coating agent 1 for deposition was changed to the anchor coating agent 7 for deposition described below.
[0041] <Anchor coating agent for vapor deposition 7> 28g isopropyl alcohol Methyl ethyl ketone 28g DN-950 (DIC Corporation adduct type polyisocyanate, solid content 75%, contains ethyl acetate as a solvent) 2.4g WXU-880-BA 20g (Alcohol-based solvent ratio: 36%)
[0042] "Preparation of deposition substrate 8" A substrate for deposition 8 was prepared in the same manner as in the preparation of the substrate for deposition 1, except that the anchor coating agent 1 for deposition was changed to the anchor coating agent 8 for deposition described below.
[0043] <Anchor coating agent for vapor deposition 8> 28g isopropyl alcohol Methyl ethyl ketone 28g 24A-100 (biuret type polyisocyanate manufactured by Asahi Kasei Corporation, solid content concentration 100%) 1.8g WXU-880-BA 20g (Alcohol-based solvent ratio: 36%)
[0044] "Preparation of deposition substrate 9" A substrate for deposition 9 was prepared in the same manner as in the preparation of the substrate for deposition 1, except that the anchor coating agent for deposition 1 was changed to the anchor coating agent for deposition 9 described below.
[0045] <Anchor coating agent for vapor deposition 9> 28g isopropyl alcohol Methyl ethyl ketone 28g DN-980 2.4g WZU-591 (acrylic resin manufactured by DIC Corporation, Tg 55°C, hydroxyl value 37.0-43.0 mgKOH / g, solid content concentration 55%, contains butyl acetate as a solvent) 18.2 g (Alcohol-based solvent ratio: 37%)
[0046] "Preparation of deposition substrate 10" A substrate 10 for deposition was prepared in the same manner as in the preparation of the substrate 1 for deposition, except that the anchor coating agent 1 for deposition was changed to the anchor coating agent 10 for deposition described below.
[0047] <Anchor Coating Agent for Vapor Deposition 10> 28g isopropyl alcohol Methyl ethyl ketone 28g DN-980 2.4g WFU-580 (DIC Corporation acrylic resin, Tg 70°C, hydroxyl value 51.0-57.0 mgKOH / g, solid content 60%, contains butyl acetate as a solvent) 16.7 g (Alcohol-based solvent ratio: 37%)
[0048] "Preparation of deposition substrate 11" A substrate for deposition 11 was prepared in the same manner as in the preparation of the substrate for deposition 1, except that the anchor coating agent 1 for deposition was changed to the anchor coating agent for deposition 11 described below.
[0049] <Anchor coating agent for vapor deposition 11> 28g isopropyl alcohol Methyl ethyl ketone 28g DN-980 2.4g FU-1031 (acrylic resin manufactured by DIC Corporation, Tg 80°C, hydroxyl value 32.0-38.0 mgKOH / g, solid content concentration 50%, contains xylene, butyl acetate, and toluene as solvents) 20 g (Alcohol-based solvent ratio: 36%)
[0050] "Preparation of deposition substrate 12" A substrate for deposition 12 was prepared in the same manner as in the preparation of the substrate for deposition 1, except that the anchor coating agent 1 for deposition was changed to the anchor coating agent for deposition 12 described below.
[0051] <Anchor coating agent for vapor deposition 12> 28g isopropyl alcohol Methyl ethyl ketone 28g DN-980 2.4g A-817 (acrylic resin manufactured by DIC Corporation, Tg 95°C, hydroxyl value 27.0-33.0 mgKOH / g, solid content concentration 50%, contains toluene and butyl acetate as a solvent) 20 g (Alcohol-based solvent ratio: 36%)
[0052] "Preparation of deposition substrate 13" A substrate for deposition 13 was prepared in the same manner as in the preparation of the substrate for deposition 1, except that the anchor coating agent 1 for deposition was changed to the anchor coating agent for deposition 13 described below.
[0053] <Anchor coating agent for vapor deposition 13> 28g isopropyl alcohol Methyl ethyl ketone 28g DN-980 2.4g A-817 10g WXU-880-BA 10g (Alcohol-based solvent ratio: 36%)
[0054] "Preparation of deposition substrate 14" A substrate for deposition 14 was prepared in the same manner as in the preparation of the substrate for deposition 1, except that the anchor coating agent 1 for deposition was changed to the anchor coating agent for deposition 14 described below.
[0055] <Anchor coating agent for vapor deposition 14> 28g isopropyl alcohol Methyl ethyl ketone 28g DN-980 2.4g WBU-1218 (acrylic resin manufactured by DIC Corporation, Tg 100°C, hydroxyl value 7.0-13.0 mgKOH / g, solid content concentration 30%, contains butyl acetate as a solvent) 33.3 g (Alcohol-based solvent content: 31%)
[0056] "Preparation of deposition substrate 15" A substrate for deposition 15 was prepared in the same manner as in the preparation of the substrate for deposition 1, except that the anchor coating agent 1 for deposition was changed to the anchor coating agent for deposition 15 described below.
[0057] <Anchor coating agent for vapor deposition 15> 28g isopropyl alcohol Methyl ethyl ketone 28g DN-980 2.4g LH-601 (Toray Fine Chemicals Co., Ltd. acrylic resin, Tg 68°C, hydroxyl value 20mgKOH / g, solid content concentration 50%, contains butyl acetate and toluene as a solvent) 20g (Alcohol-based solvent ratio: 36%)
[0058] "Preparation of deposition substrate 16" A deposition substrate 16 was prepared in the same manner as in preparation of the deposition substrate 3, except that Technoloy C000 was changed to Lumirror (registered trademark) U48 (a polyester film manufactured by Toray Industries, Inc.).
[0059] "Preparation of deposition substrate 17" A substrate for deposition 17 was prepared in the same manner as in the preparation of the substrate for deposition 1, except that the anchor coating agent 1 for deposition was changed to the anchor coating agent for deposition 17 described below.
[0060] <Anchor coating agent for vapor deposition 17> Methyl ethyl ketone 56g DN-980 2.4g WXU-880-BA 20g (0% alcohol-based solvent)
[0061] "Preparation of deposition substrate 18" A substrate for deposition 18 was prepared in the same manner as in the preparation of the substrate for deposition 1, except that the anchor coating agent 1 for deposition was changed to the anchor coating agent for deposition 18 described below.
[0062] <Anchor coating agent for vapor deposition 18> 14g isopropyl alcohol Methyl ethyl ketone 42g DN-980 2.4g WXU-880-BA 20g (Alcohol-based solvent content: 18%)
[0063] "Preparation of deposition substrate 19" A substrate for deposition 19 was prepared in the same manner as in the preparation of the substrate for deposition 1, except that the anchor coating agent 1 for deposition was changed to the anchor coating agent for deposition 19 described below.
[0064] <Anchor coating agent for vapor deposition 19> 53g isopropyl alcohol Methyl ethyl ketone 3g DN-980 2.4g WXU-880-BA 20g (Alcohol-based solvent content: 68%)
[0065] "Preparation of deposition substrate 20" A substrate for deposition 20 was prepared in the same manner as in the preparation of the substrate for deposition 1, except that the anchor coating agent for deposition 1 was changed to the anchor coating agent for deposition 20 described below.
[0066] <Anchor Coating Agent 20 for Vapor Deposition> 28g isopropyl alcohol Methyl ethyl ketone 28g WXU-880-BA 20g (Alcohol-based solvent ratio: 37%)
[0067] "Preparation of deposition substrate 21" A substrate for deposition 21 was prepared in the same manner as in the preparation of the substrate for deposition 1, except that the anchor coating agent 1 for deposition was changed to the anchor coating agent for deposition 21 described below.
[0068] <Anchor Coating Agent for Vapor Deposition 21> 28g isopropyl alcohol Methyl ethyl ketone 28g DN-980 2.4g A-875-55 (acrylic resin manufactured by DIC Corporation, Tg 45°C, hydroxyl value 19.0-25.0 mgKOH / g, solids concentration 55%, contains mineral spirits and Solvesso 100 as solvents) 18.2 g (Alcohol-based solvent ratio: 37%)
[0069] "Preparation of deposition substrate 22" Technoloy C000 was used as the deposition substrate 22 as it was.
[0070] "Preparation of deposition substrate 23" Lumirror U48 was used as the deposition substrate 23 as it was.
[0071] The various anchor coating agents for deposition obtained as described above and the anchor coating layers obtained by applying the anchor coating agents to the surfaces of substrates were evaluated as follows. The anchor coating layers of the deposition substrates 1 to 6, 9 to 19, and 21 using the isocyanurate-type polyisocyanate compound were superior in drying property and good in film-forming property compared to the other anchor coating layers.
[0072] <Evaluation of blocking resistance of deposition substrate> Two sheets of each of the deposition substrates 1 to 23 were stacked, a load of 1 kg was applied using an iron plate, and the sheets were stored at 50°C for 24 hours. The stacked deposition substrates were then peeled off. Blocking resistance was evaluated as follows: ◯ if the deposition substrates were peeled off without resistance, △ if there was resistance but the anchor coat layer did not peel off, and × if the anchor coat layer peeled off. The results are shown in Table 1.
[0073] <Metal film adhesion evaluation> Using a vacuum deposition apparatus E-230A manufactured by Shimadzu Corporation, aluminum was deposited to a thickness of 300 nm on the anchor coat layer-coated surfaces of deposition substrates 1 to 21 and on deposition substrates 22 and 23. The adhesion of the deposited aluminum film was tested in accordance with the cross-cut method specified in JIS K 5600-5-6:1999, and the test results were recorded as classifications 0 to 5. In this evaluation, classification 0 is the best, and as the classification number increases, the results become worse, with classification 5 being the worst. The results are shown in Table 1.
[0074] <Pot life evaluation> The anchor coating agents for deposition used for the deposition substrates 1 to 21 were observed 24 hours after preparation, and the change in appearance from immediately after preparation was recorded. When the anchor coating agent for deposition had become highly viscous or gelled, the change in appearance during the pot life was evaluated as ×, and when there was no change, it was evaluated as ◯. The results are shown in Table 1 as the change in appearance of the anchor coating agent. Furthermore, a deposition substrate was prepared using the anchor coating agent for deposition 24 hours after preparation, and the blocking resistance was evaluated in the same manner as the blocking resistance evaluation of the deposition substrate described above. The results are shown in Table 1.
[0075] [Table 1]
[0076] Table 1 shows the effectiveness of the present invention.
Claims
1. The anchor coating agent for vapor deposition contains at least an alcohol-based solvent, an aprotic solvent, a polyisocyanate compound, and an acrylic resin having a glass transition temperature of higher than 50°C, and the proportion of the alcohol-based solvent in the entire anchor coating agent is 25 to 63 mass%.
2. A method for producing a substrate for deposition, comprising applying the anchor coating agent for deposition according to claim 1 to a surface of a substrate and drying the agent to form an anchor coating layer.
Citation Information
Patent Citations
Reactive composition containing blocked polyurethane prepolymer
JP2006097018A
Film for vapor deposition film and gas barrier film
JP2010229291A
Resin composition
JP2013199582A
Two-component polyurethane adhesive, laminate obtained by using the same, and protective sheet for solar cell
JP2015166404A
Urethanization catalyst, polyol mixture, adhesive and laminate film
JP2016074780A