Super-hydrophobic self-cleaning radiation cooling composite coating as well as preparation method and application thereof

By covering the superhydrophobic self-cleaning layer on the radiation cooling layer, using materials such as carbon nanotubes and silica aerogel composite particles, the problem of reduced cooling effect and shortened life in outdoor applications is solved, and high efficiency is achieved Building surface cooling and long-term performance maintenance.

CN119039842AActive Publication Date: 2024-11-29CENT SOUTH UNIV

Patent Information

Application Number
CN202411305165.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-29
Estimated Expiration
2044-09-19

AI Technical Summary

Technical Problem

Radiation refrigeration technology in the application of building exterior walls is due to high manufacturing costs, complex processing, and wind, rain, and dust pollution in outdoor environments, resulting in weakening of cooling effect and shortening of service life.

Method used

The superhydrophobic self-cleaning radiation-insulated composite coating adopts a layered architecture. By covering the superhydrophobic self-cleaning layer on the radiation cooling layer, the radiation cooling effect is improved by using carbon nanotubes and silica aerogel composite particles, and the radiation cooling effect is improved by polymerization. Materials such as tetrafluoroethylene nanoparticles and PDMS achieve superhydrophobicity and self-cleaning functions.

Benefits of technology

It improves the cooling performance of the building surface, extends the service life of the radiation-cooled coating, enhances the hydrophobicity and self-cleaning ability of the coating, reduces the difficulty of preparation, and improves construction efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention provides a super-hydrophobic self-cleaning radiation cooling composite coating as well as a preparation method and application thereof, and belongs to the technical field of buildings. The composite coating comprises a radiation cooling layer arranged on the surface of a base body and a super-hydrophobic self-cleaning coating arranged on the outer surface of the radiation cooling layer, and paint of the radiation cooling layer is prepared from, by mass, 10-15 parts of acrylic resin, 2-3 parts of radiation blocking composite particles, 0.5-1 part of a coupling agent, 0.5-1 part of a coalescing agent and 0.5-1 part of a flatting agent; the radiation barrier composite particles are formed by compounding carbon nanotubes and silicon dioxide aerogel. The composite coating provided by the invention has excellent super-hydrophobicity and radiation heat insulation function, can automatically carry out heat radiation heat dissipation and cooling, also can maintain and protect the radiation cooling performance for a longer time due to the self-cleaning function, and is excellent in adhesion property and wear resistance, convenient to construct and high in efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of building technology, and more specifically, to a super-hydrophobic self-cleaning radiation heat-insulating composite coating and a preparation method and application thereof. Background Art

[0002] Radiative cooling technology is a new type of passive, energy-free cooling method. Compared with traditional cooling methods, it has the advantages of no pollution and no emissions, and is of great significance to energy conservation and emission reduction. Radiative cooling technology has always faced problems such as high manufacturing costs and complex processing in outdoor applications such as building exterior walls, which seriously hinders the practical application and large-scale industrialization of the technology. In addition, since radiative cooling materials are in an outdoor working environment for a long time, they face the challenges of wind, rain and dust pollution, which will cause damage to the spectral performance, thereby greatly weakening the radiative cooling performance and even shortening its service life.

[0003] Chinese patent CN116836592A provides a method for preparing a radiation cooling coating, comprising the following steps: S1, dissolving a film-forming material in an organic solvent, heating and stirring for 12 hours to obtain a solution A; S2, adding the ball-milled reflective filler and fluorescent filler to solution A, and adding an auxiliary agent, fully dispersing to obtain a uniformly dispersed slurry B; S3, subjecting the obtained slurry B to ultrasonic treatment for 15 to 20 minutes to obtain a radiation cooling coating. The radiation cooling coating provided by Chinese patent CN114410219A comprises the following components in parts by weight: 5 to 7 parts of polysiloxane resin, 20 to 25 parts of reflective powder, 18 to 22 parts of hydrophobically modified silica, 1 to 3 parts of fiber, 40 to 50 parts of solvent, and 0.25 to 0.7 parts of curing agent. The above-mentioned radiation cooling coating is used to prevent the heat of the sun from accumulating and heating up on the surface of the building, but since the radiation cooling coating needs to be outdoors facing the sky, it is inevitable to be polluted by outdoor dust and soaked in rainwater, which will seriously affect the cooling effect and service life of the radiation material. Therefore, coupling the superhydrophobic function into the radiation cooling coating makes the coating have self-cleaning properties, which is of great significance for maintaining the spectral performance of the radiation cooling coating and extending its service life. Summary of the invention

[0004] Based on the problems existing in the prior art, the present invention proposes a super-hydrophobic self-cleaning radiation insulation composite coating and a preparation method and application thereof. By covering the radiation insulation layer with a super-hydrophobic self-cleaning layer, the composite coating has excellent super-hydrophobicity and self-cleaning ability, thereby effectively improving the cooling performance of the building surface.

[0005] In order to achieve the above object, the technical solution of the present invention is as follows:

[0006] A super-hydrophobic self-cleaning radiation cooling composite coating, comprising a radiation cooling layer arranged on the surface of a substrate and a super-hydrophobic self-cleaning coating arranged on the outer surface of the radiation cooling layer, wherein the coating of the radiation cooling layer comprises the following raw materials in parts by weight: 10 to 15 parts of acrylic resin, 2 to 3 parts of radiation blocking composite particles, 0.5 to 1 part of coupling agent, 0.5 to 1 part of film-forming aid, and 0.5 to 1 part of leveling agent;

[0007] The radiation blocking composite particles are composited from carbon nanotubes and silicon dioxide aerogel.

[0008] Preferably, the acrylic resin has a solid content of 40% to 60% and a viscosity of 100 to 500 mPa·s.

[0009] Preferably, the carbon nanotubes have a diameter range of 8 to 15 nm and a length range of 3 to 12 μm, and the silica aerogel has a particle size range of 10 nm to 200 nm and a density range of 0.05 g / cm 3 ~0.15g / cm 3 .

[0010] Preferably, the preparation process of the radiation blocking composite particles is as follows:

[0011] S11a, calcining the silica aerogel powder at 400-600°C for 2-4h at a heating rate of 3-8°C / min;

[0012] S11b, take 1-2g of calcined silica aerogel powder and add it to 50-100mL of ethanol, ultrasonically treat for 30-60min, and adjust the pH value of the solution to between 3 and 4 with dilute hydrochloric acid after treatment; add 2-5mL of coupling agent, heat in a water bath at 50-80°C; stir, wash, filter, and dry to obtain modified silica aerogel;

[0013] S11c, dispersing carbon nanotubes in 50-100 mL of deionized water and stirring for 24-36 h, dissolving 0.5-1 g of modified silica aerogel in 5-10 mL of anhydrous ethanol solution, then adding the solution to the carbon nanotube suspension, ultrasonically treating at room temperature for 2-3 h, and stirring for 72-96 h;

[0014] S11d, filtering, washing the collected solid, and vacuum drying to obtain radiation blocking composite particles.

[0015] Preferably, the concentration of the dilute hydrochloric acid is 0.1 to 1 mol / L.

[0016] Preferably, the coupling agent may be KH550 (γ-aminopropyltriethoxysilane) or KH570 (γ-methacryloxypropyltrimethoxysilane), and its density is 0.9 g / cm 3~1.0g / cm 3 .

[0017] Preferably, the film-forming aid is alcohol ester dodecahydrate, and the leveling agent is a modified polyurethane rheology modifier.

[0018] Preferably, the method for preparing the above-mentioned radiation cooling layer coating comprises the following steps:

[0019] S11, mixing acrylic resin and radiation-blocking composite particles in proportion, using a magnetic stirrer at room temperature at a rotation speed of 600 to 800 rpm for 30 to 60 minutes, and the obtained dispersion is named A;

[0020] S12. During the stirring process, a coupling agent, a film-forming aid and a leveling agent are added to the dispersion A, and mixed at a speed of 600 to 800 rpm for 5 to 8 hours to ensure uniform mixing, to obtain a radiation cooling layer coating.

[0021] Preferably, the coating of the super hydrophobic self-cleaning layer includes the following raw materials in parts by mass: 0.5 to 1.0 parts of polyvinylidene fluoride (PVDF), 0.5 to 1.0 parts of polydimethylsiloxane (PDMS), 0.1 to 0.2 parts of PDMS curing agent, 6 to 10 parts of N,N-dimethylformamide (DMF), 0.5 to 1.0 parts of tetrahydrofuran (THF), 2 to 3 parts of polytetrafluoroethylene (PTFE) nanoparticles, and 0.1 to 0.2 parts of nano-silicon dioxide (SiO2).

[0022] Preferably, the polyvinylidene fluoride (PVDF) has a purity of ≥99.5% and a relative density of 1.74 to 1.77.

[0023] Preferably, the curing temperature of the polydimethylsiloxane (PDMS) is 20-150° C., and the thermal conductivity is 0.2-0.3 W / mK.

[0024] Preferably, the purity of the N,N-dimethylformamide (DMF) is ≥99% and the density is 1.0-1.1 g / mL.

[0025] Preferably, the purity of tetrahydrofuran (THF) is ≥99.5%, and the density is 0.8-1.0 g / mL.

[0026] Preferably, the average diameter of the polytetrafluoroethylene nanoparticles is 20 to 500 nm, and the average diameter of the nano-SiO2 particles is 20 to 500 nm.

[0027] Preferably, the method for preparing the super hydrophobic self-cleaning layer coating comprises the following steps:

[0028] S21, dissolving the formulated amount of PVDF and PDMS in the formulated amount of DMF and THF, respectively, and then magnetically stirring at room temperature for 1 to 2 hours at a stirring speed of 200 to 300 r / min until PVDF and PDMS are completely dissolved, and the obtained dispersions are named A and B, respectively;

[0029] S22, adding a formulated amount of polytetrafluoroethylene nanoparticles to solution A, and magnetically stirring for 1 to 2 hours at a stirring speed of 200 to 300 r / min to uniformly distribute the particles in solution A. The resulting dispersion is called C;

[0030] S23, add the formulated amount of SiO2 nanoparticles to solution B, stir magnetically for 1 to 2 hours at a stirring speed of 200 to 300 r / min, so that the particles are evenly distributed in solution B. The resulting dispersion is called D;

[0031] S24, mixing liquid C and liquid D, and magnetically stirring at room temperature for 1 to 2 hours at a stirring speed of 200 to 300 r / min to form a dispersion E;

[0032] S25. Add the formulated amount of PDMS curing agent to the dispersion E, stir magnetically for 0.5 to 1 h at a stirring speed of 200 to 300 r / min to obtain a super hydrophobic self-cleaning layer coating.

[0033] As a general technical concept, the present invention provides a method for preparing the above-mentioned super-hydrophobic self-cleaning radiation insulation composite coating, comprising the following steps:

[0034] S1, coating the prepared radiation cooling layer coating on the surface of the substrate to form a flat film layer, drying and curing to obtain a radiation cooling layer;

[0035] S2, spraying the configured super-hydrophobic self-cleaning layer coating onto the surface of the solidified radiation cooling layer;

[0036] S3. After the spraying is completed, a super hydrophobic self-cleaning layer is formed.

[0037] Preferably, in step S1, the coating method can be drip coating, scraping coating, brush coating, etc.

[0038] In the present invention, content refers to mass fraction, such as solid content.

[0039] As a general technical concept, the present invention also provides the use of the above-mentioned super-hydrophobic self-cleaning radiation insulation composite coating in the protection of building exterior walls.

[0040] Compared with the prior art, the advantages of the present invention are:

[0041] (1) In view of the coupling of the radiation cooling function and the super-hydrophobic function, the present invention adopts a layered architecture to separate the two functions and implement them in the bottom layer and the top layer respectively. The super-hydrophobic needs to be attached to the outer surface to play the role of a self-cleaning surface, so it needs to be placed on the top layer, and the radiation cooling coating film layer is used as the bottom layer. The layered structure is more conducive to the regulation and combination of functions, reduces the overlap and mutual influence of the two functions, reduces the difficulty of preparation, and can better ensure the realization of the better performance of the individual functions.

[0042] (2) The radiation cooling layer of the present invention adopts radiation-blocking composite particles composed of carbon nanotubes and silica aerogel as the main filler. The carbon nanotubes have a high emissivity and can effectively release heat into the environment in the form of infrared radiation. At the same time, the thermal conductivity of silica aerogel is extremely low, which can effectively prevent the conduction of heat. The positive synergistic effect of the two particles further enhances the thermal insulation effect of the radiation cooling layer coating.

[0043] (3) The super-hydrophobic self-cleaning layer of the present invention adopts polytetrafluoroethylene (PTFE) nanoparticles as the main filler, PDMS and PVDF as the binder, and a large amount of -CF2, -CH2 and -CH3 chemical groups on the coating surface, so that the coating has excellent super-hydrophobicity and self-cleaning function, thereby solving the phenomenon that the existing thermal insulation coating is affected by surface pollution and the cooling performance of the coating decreases when used outdoors. At the same time, due to the addition of nano-SiO2, the super-hydrophobic self-cleaning layer can also play a positive synergistic role in the spectrum on the radiation cooling layer, which can not only improve the emissivity of the infrared band, but more importantly, it can also reflect short-wave solar radiation when sunlight is incident on the top layer, effectively making up for the intrinsic defect problem of the radiation cooling layer in the short-wave band.

[0044] In summary, the super-hydrophobic self-cleaning radiation heat-insulating composite coating provided by the present invention has excellent super-hydrophobicity and radiation heat-insulating function, can automatically radiate heat to dissipate heat and cool down, and the self-cleaning function can also maintain and protect the radiation cooling performance for a longer time, and has excellent adhesion and wear resistance, convenient construction and high efficiency. The super-hydrophobic self-cleaning radiation heat-insulating composite coating system of the present invention can be used to prevent the heat of the sun from accumulating and heating up on the surface of the building, so as to achieve the purpose of improving the cooling performance of the building surface. DETAILED DESCRIPTION

[0045] Many specific details are set forth in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited to the specific implementation disclosed below.

[0046] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0047] It should be noted that the raw materials, instruments, etc. involved in the present invention are all common commercially available products.

[0048] The following embodiments are only used to more clearly illustrate the technical solutions of the present invention, and are not intended to limit the protection scope of the present invention.

[0049] Example 1

[0050] A super-hydrophobic self-cleaning radiation cooling composite coating, comprising a radiation cooling layer arranged on the surface of a substrate and a super-hydrophobic self-cleaning coating arranged on the outer surface of the radiation cooling layer, wherein the coating of the radiation cooling layer comprises the following raw materials in parts by weight: 10 parts of acrylic resin, 3 parts of radiation blocking composite particles, 1 part of coupling agent, 1 part of film-forming aid, and 1 part of leveling agent;

[0051] In this embodiment, the preparation process of the radiation blocking composite particles is as follows:

[0052] S11a, calcining the silica aerogel powder at 500°C for 3 h at a heating rate of 5°C / min;

[0053] S11b, take 2g of calcined silica aerogel powder and add it to 100mL of ethanol, ultrasonically treat it for 60min, and adjust the pH value of the solution to between 3 and 4 with dilute hydrochloric acid after treatment; add 5mL of coupling agent, and heat it in a water bath at 60°C; stir, wash, filter, and dry to obtain modified silica aerogel;

[0054] S11c, dispersing carbon nanotubes in 100 mL of deionized water and stirring for 24 h, dissolving 1 g of modified silica aerogel in 10 mL of anhydrous ethanol solution, then adding the solution to the carbon nanotube suspension, ultrasonically treating at room temperature for 3 h, and stirring for 96 h;

[0055] S11d, filtering, washing the collected solid, and vacuum drying to obtain radiation blocking composite particles.

[0056] In this embodiment, the preparation method of the radiation cooling layer coating comprises the following steps:

[0057] S11, mixing acrylic resin and radiation-blocking composite particles in proportion, using a magnetic stirrer at room temperature at a rotation speed of 800 rpm for 60 min, and the obtained dispersion is named A;

[0058] S12. During the stirring process, a coupling agent, a film-forming aid and a leveling agent were added to the dispersion A, and the mixture was mixed at a speed of 800 rpm for 6 hours to ensure uniform mixing, thereby obtaining a radiation cooling layer coating.

[0059] In this embodiment, the preparation method of the super hydrophobic self-cleaning layer coating comprises the following steps:

[0060] S21, by mass, 0.7 parts of PVDF and 0.6 parts of PDMS were dissolved in 8 parts of DMF and 0.8 parts of THF, respectively, and then magnetically stirred at room temperature for 2 hours at a stirring speed of 300 r / min until PVDF and PDMS were completely dissolved. The obtained dispersions were named A and B, respectively;

[0061] S22, add 3 parts of polytetrafluoroethylene nanoparticles to solution A, stir magnetically for 2 hours at a stirring speed of 300 r / min, so that the particles are evenly distributed in solution A. The resulting dispersion is called C;

[0062] S23, add 0.2 parts of SiO2 nanoparticles to solution B, stir magnetically for 2 hours at a stirring speed of 300 r / min, so that the particles are evenly distributed in solution B. The resulting dispersion is called D;

[0063] S24, mixing liquid C and liquid D, and magnetically stirring at room temperature for 2 h at a stirring speed of 300 r / min to form dispersion E;

[0064] S25. Add 0.1 parts of PDMS curing agent to the dispersion E, stir magnetically for 1 hour at a stirring speed of 300 r / min to obtain a super hydrophobic self-cleaning layer coating.

[0065] In this embodiment, the preparation method of the super hydrophobic self-cleaning radiation insulation composite coating comprises the following steps:

[0066] S1, coating the prepared radiation cooling layer coating on the surface of the substrate to form a flat film layer, drying and curing to obtain a radiation cooling layer;

[0067] S2, spraying the configured super-hydrophobic self-cleaning layer coating onto the surface of the solidified radiation cooling layer;

[0068] S3. After the spraying is completed, a super hydrophobic self-cleaning layer is formed.

[0069] The performance test results of the super-hydrophobic self-cleaning radiative cooling composite coating are shown in Table 1.

[0070] Example 2

[0071] A super-hydrophobic self-cleaning radiation cooling composite coating, the preparation process of which is substantially the same as that of Example 1, except that in the preparation process of the radiation cooling layer coating, the radiation blocking composite particles used in step S11 are 2 parts. The performance test results of the super-hydrophobic self-cleaning radiation cooling composite coating are shown in Table 1.

[0072] Example 3

[0073] A super-hydrophobic self-cleaning radiation cooling composite coating, the preparation process of which is substantially the same as that of Example 1, except that in the preparation process of the super-hydrophobic self-cleaning layer coating, 2 portions of polytetrafluoroethylene nanoparticles are used in step S22. The performance test results of the super-hydrophobic self-cleaning radiation cooling composite coating are shown in Table 1.

[0074] Comparative Example 1

[0075] A super-hydrophobic self-cleaning radiation cooling composite coating, the preparation process of which is substantially the same as that of Example 1, except that in the preparation process of the radiation cooling layer coating, the radiation blocking composite particles used in step S11 are 1 part. The performance test results of the super-hydrophobic self-cleaning radiation cooling composite coating are shown in Table 1.

[0076] Comparative Example 2

[0077] A super-hydrophobic self-cleaning radiation cooling composite coating, the preparation process of which is substantially the same as that of Example 1, except that in the preparation process of the radiation cooling layer coating, step S11 does not use radiation blocking composite particles. The performance test results of the super-hydrophobic self-cleaning radiation cooling composite coating are shown in Table 1.

[0078] Comparative Example 3

[0079] A super-hydrophobic self-cleaning radiation cooling composite coating, the preparation process of which is substantially the same as that of Example 1, except that in the preparation process of the super-hydrophobic self-cleaning layer coating, the amount of polytetrafluoroethylene nanoparticles used in step S22 is 1 part. The performance test results of the super-hydrophobic self-cleaning radiation cooling composite coating are shown in Table 1.

[0080] Comparative Example 4

[0081] A super-hydrophobic self-cleaning radiation cooling composite coating, the preparation process of which is substantially the same as that of Example 1, except that in the preparation process of the super-hydrophobic self-cleaning layer coating, step S22 does not use polytetrafluoroethylene nanoparticles. The performance test results of the super-hydrophobic self-cleaning radiation cooling composite coating are shown in Table 1.

[0082] Comparative Example 5

[0083] A super-hydrophobic self-cleaning radiation cooling composite coating, the preparation process of which is substantially the same as that of Example 1, except that in the preparation process of the super-hydrophobic self-cleaning layer coating, step S23 does not use nano-SiO2 particles. The performance test results of the super-hydrophobic self-cleaning radiation cooling composite coating are shown in Table 1.

[0084] Comparative Example 6

[0085] A super-hydrophobic self-cleaning radiation cooling composite coating, the preparation process of which is basically the same as that of Example 1, except that: during the preparation of the radiation cooling layer coating, no radiation blocking composite particles are added, and 1.5 parts of carbon nanotubes and 1.5 parts of silica aerogel are added in step S11. The performance test results of the super-hydrophobic self-cleaning radiation cooling composite coating are shown in Table 1.

[0086] Comparative Example 7

[0087] The preparation process of the single radiation insulation layer coating is the same as that of Example 1. The test results of the radiation insulation coating performance are shown in Table 1.

[0088] Comparative Example 8

[0089] The preparation process of a single super-hydrophobic self-cleaning layer coating is the same as that of Example 1. The test results of the super-hydrophobic self-cleaning coating performance are shown in Table 1.

[0090] Comparative Example 9

[0091] The radiation cooling layer coating and the super hydrophobic self-cleaning layer coating were simply mixed to prepare a super hydrophobic self-cleaning radiation cooling hybrid coating, and the performance test results are shown in Table 1.

[0092] Table 1. Test results of coating performance prepared by Examples 1-3 and Comparative Examples 1-9

[0093]

[0094]

[0095] Specific characterization method:

[0096] (1) The water contact angle (WCA) and sliding angle (SA) of the coating are tested according to the relevant contents in standard GB / T30693-2014.

[0097] (2) The infrared emissivity of the coating is tested in accordance with the relevant contents of the standard GJB 5023-2012.

[0098] (3) The thermal conductivity of the coating is tested with reference to the relevant contents in standard GB / T25261-2018.

[0099] (4) The thermal insulation temperature difference of the coating is tested with self-made equipment according to the relevant contents of standard HG / T 4341-2012.

[0100] (5) The bonding strength is tested in accordance with Section 7 of GB / T16777-2008.

[0101] It can be seen from the results of Examples 1 and 2 and Comparative Examples 1 and 2 that by adding radiation blocking composite particles to the coating, the infrared emissivity of the coating system is greatly improved, while the thermal conductivity is greatly reduced, and as the amount of radiation blocking composite particles added increases, the thermal insulation temperature difference of the coating gradually increases.

[0102] It can be seen from the results of Examples 1 and 3 and Comparative Examples 3 and 4 that by adding polytetrafluoroethylene nanoparticles to the coating, the water drop contact angle (WCA) of the coating is greatly improved, the sliding angle (SA) is greatly reduced, and the hydrophobicity of the coating is gradually improved with the addition of polytetrafluoroethylene nanoparticles.

[0103] It can be seen from the results of Example 1 and Comparative Examples 2 and 5 that by adding radiation insulation composite particles to the radiation layer coating and adding nano-SiO2 particles to the super hydrophobic self-cleaning layer, there is an excellent synergistic effect between the two fillers, the infrared emissivity of the coating is higher, and the insulation effect is more significantly improved.

[0104] It can be seen from the results of Example 1 and Comparative Example 6 that the carbon nanotube and silica aerogel particles are compounded to prepare radiation-blocking composite particles, and the positive synergistic effect of the two particles is exerted to further enhance the thermal insulation effect of the radiation cooling layer coating.

[0105] It can be seen from the results of Example 1 and Comparative Examples 7, 8, and 9 that the composite coating system designed by this patent, which includes a super-hydrophobic self-cleaning layer and a radiation cooling layer, has better hydrophobic and thermal insulation properties than a single-layer coating, while reducing the overlap and mutual influence of the two functions. It can automatically radiate heat to dissipate heat and cool down, and the self-cleaning function can also maintain and protect the radiation cooling performance for a longer period of time.

[0106] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A super-hydrophobic self-cleaning radiation cooling composite coating, characterized in that: It comprises a radiation cooling layer arranged on the surface of a substrate and a super hydrophobic self-cleaning coating arranged on the outer surface of the radiation cooling layer, wherein the coating of the radiation cooling layer comprises the following raw materials in parts by weight: 10 to 15 parts of acrylic resin, 2 to 3 parts of radiation blocking composite particles, 0.5 to 1 part of coupling agent, 0.5 to 1 part of film-forming aid, and 0.5 to 1 part of leveling agent; The radiation blocking composite particles are composited from carbon nanotubes and silicon dioxide aerogel.

2. The super-hydrophobic self-cleaning radiation cooling composite coating according to claim 1, characterized in that: The preparation process of the radiation blocking composite particles is as follows: S11a, calcining the silica aerogel powder at 400-600°C for 2-4h at a heating rate of 3-8°C / min; S11b, take 1-2g of calcined silica aerogel powder and add it to 50-100mL of ethanol, ultrasonically treat for 30-60min, and adjust the pH value of the solution to between 3 and 4 with dilute hydrochloric acid after treatment; add 2-5mL of coupling agent, heat in a water bath at 50-80°C; stir, wash, filter, and dry to obtain modified silica aerogel; S11c, dispersing carbon nanotubes in 50-100 mL of deionized water and stirring for 24-36 h, dissolving 0.5-1 g of modified silica aerogel in 5-10 mL of anhydrous ethanol solution, then adding the solution to the carbon nanotube suspension, ultrasonically treating at room temperature for 2-3 h, and stirring for 72-96 h; S11d, filtering, washing the collected solid, and vacuum drying to obtain radiation blocking composite particles. Preferably, the concentration of the dilute hydrochloric acid is 0.1 to 1 mol / L.

3. The super-hydrophobic self-cleaning radiation cooling composite coating according to claim 1, characterized in that: The coupling agent is KH550 or KH570.

4. The super-hydrophobic self-cleaning radiation cooling composite coating according to claim 1, characterized in that: The film-forming aid is alcohol ester dodecapolymer, and the leveling agent is a modified polyurethane rheology modifier.

5. The super-hydrophobic self-cleaning radiation cooling composite coating according to claim 1, characterized in that: The method for preparing the coating of the radiation cooling layer comprises the following steps: S11, mixing acrylic resin and radiation-blocking composite particles in proportion, using a magnetic stirrer at room temperature at a rotation speed of 600 to 800 rpm for 30 to 60 minutes, and the obtained dispersion is named A; S12. During the stirring process, a coupling agent, a film-forming aid and a leveling agent are added to the dispersion A, and mixed at a speed of 600 to 800 rpm for 5 to 8 hours to ensure uniform mixing, to obtain a radiation cooling layer coating.

6. The super-hydrophobic self-cleaning radiation cooling composite coating according to claim 1, characterized in that: The coating of the super-hydrophobic self-cleaning layer comprises the following raw materials in parts by weight: 0.5 to 1.0 parts of polyvinylidene fluoride, 0.5 to 1.0 parts of polydimethylsiloxane, 0.1 to 0.2 parts of PDMS curing agent, 6 to 10 parts of N,N-dimethylformamide, 0.5 to 1.0 parts of tetrahydrofuran, 2 to 3 parts of polytetrafluoroethylene nanoparticles, and 0.1 to 0.2 parts of nano-silicon dioxide.

7. The super-hydrophobic self-cleaning radiation cooling composite coating according to claim 6, characterized in that: The average diameter of the polytetrafluoroethylene nanoparticles is 20 to 500 nm, and the average diameter of the nano-SiO2 particles is 20 to 500 nm.

8. The super-hydrophobic self-cleaning radiation cooling composite coating according to claim 6 or 7, characterized in that: The method for preparing the coating of the super hydrophobic self-cleaning layer comprises the following steps: S21, dissolving the formulated amount of PVDF and PDMS in the formulated amount of DMF and THF, respectively, and then magnetically stirring at room temperature for 1 to 2 hours at a stirring speed of 200 to 300 r / min until PVDF and PDMS are completely dissolved, and the obtained dispersions are named A and B, respectively; S22, adding a formulated amount of polytetrafluoroethylene nanoparticles to solution A, and magnetically stirring for 1 to 2 hours at a stirring speed of 200 to 300 r / min to uniformly distribute the particles in solution A. The resulting dispersion is called C; S23, add the formulated amount of SiO2 nanoparticles to solution B, stir magnetically for 1 to 2 hours at a stirring speed of 200 to 300 r / min, so that the particles are evenly distributed in solution B. The resulting dispersion is called D; S24, mixing liquid C and liquid D, and magnetically stirring at room temperature for 1 to 2 hours at a stirring speed of 200 to 300 r / min to form a dispersion E; S25. Add the formulated amount of PDMS curing agent to the dispersion E, stir magnetically for 0.5 to 1 h at a stirring speed of 200 to 300 r / min to obtain a super hydrophobic self-cleaning layer coating.

9. A method for preparing the super-hydrophobic self-cleaning radiation insulation composite coating according to any one of claims 1 to 8, comprising the following steps: S1, coating the prepared radiation cooling layer coating on the surface of the substrate to form a flat film layer, drying and curing to obtain a radiation cooling layer; S2, spraying the configured super-hydrophobic self-cleaning layer coating onto the surface of the solidified radiation cooling layer; S3. After the spraying is completed, a super hydrophobic self-cleaning layer is formed.

10. Application of the super-hydrophobic self-cleaning radiation heat-insulating composite coating according to any one of claims 1 to 8 in protection of building exterior walls.

Citation Information

Patent Citations

  • Radiation cooling coating and preparation method thereof

    CN114410219A

  • Preparation method of radiation cooling coating

    CN116836592A

  • Passive radiation refrigeration coating and preparation method and coating structure thereof

    CN113292874A

  • Radiation refrigeration coating with self-cleaning function and preparation method and application thereof

    CN113861771A

  • Preparation method of radiation refrigeration coating with super-hydrophobic performance

    CN116102928A

Cited By

  • Anti-condensation and anti-icing membrane material and forming process thereof

    CN120209384A

  • Glass curtain wall radiation refrigeration film and preparation process thereof

    CN122277123A