Light diffusion device, backlight device and image display device
By introducing a low refractive index layer between the light source and diffusion film, the device achieves improved uniformity of in-plane luminance by reducing directivity and enhancing interfacial reflection, thus addressing the non-uniformity issues in PDLC-based light diffusion devices.
Patent Information
- Application Number
- JP2023057696
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing light diffusion devices using PDLC films in direct type backlight devices suffer from insufficient uniformity of in-plane luminance due to interfacial reflection and adhesion issues with surface-type diffusion films, leading to non-uniform light emission.
Incorporating a low refractive index layer between the light source layer and the diffusion film, which reduces directivity of light and enhances uniformity by increasing interfacial reflection, using a configuration that includes a light source layer, sealing resin layer, and a diffusion film with a polymer matrix and dispersed liquid crystal particles.
The low refractive index layer improves the uniformity of in-plane brightness by diffusing light more uniformly across the surface, addressing the non-uniformity issues in existing devices.
Smart Images

Figure 2024145373000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a light diffusion device including a diffusion film, and a backlight device and an image display device using the light diffusion device. [Background technology]
[0002] A PDLC film having a polymer dispersed liquid crystal (hereinafter sometimes referred to as "PDLC") layer between a pair of transparent electrode layers is a type of light control film, and can switch between a light scattering state (scattering state) and a light transmitting state (non-scattering state or transparent state) by switching between a voltage application state and a non-voltage application state. Specifically, the PDLC layer includes a polymer matrix and droplets of a liquid crystal compound (hereinafter sometimes referred to as "liquid crystal droplets") dispersed in the polymer matrix, and the liquid crystal droplets become scattering particles and can cause light scattering due to the difference in refractive index between the liquid crystal compound in the liquid crystal droplets and the polymer matrix, etc.
[0003] Moreover, in recent years, display devices and lighting devices that use light-emitting diodes (hereinafter referred to as LEDs) as light sources have become widespread due to their low power consumption and ability to be made smaller and thinner, and one or more diffusion films are placed over the light source to obtain uniform surface light emission.
[0004] The above-mentioned diffusion film includes a surface-type diffusion film in which a diffusion pattern is formed on the surface by uneven processing, dot printing, etc. When a surface-type diffusion film is laminated to an adjacent member without an adhesive layer, the adjacent member may be scratched by rubbing, the diffusion pattern may change over time, etc., and when the surface-type diffusion film is laminated to an adjacent member via an adhesive layer, the diffusion pattern may change or disappear due to the adhesive, and air bubbles may be generated in the uneven parts, etc.
[0005] Another type of diffusion film is an internal diffusion film that contains scattering particles inside. A PDLC film can be used as an internal diffusion film by utilizing the scattering effect of the liquid crystal droplets (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent Publication No. 2021-077534 Summary of the Invention [Problem to be solved by the invention]
[0007] A light diffusion device including a light source and a PDLC film as a diffusion film can be applied to a backlight device in an image display device, but when applied to a direct-type backlight device, the uniformity of the in-plane luminance may be insufficient. Therefore, the main object of the present invention is to provide a light diffusion device having a diffusion film and capable of realizing more uniform surface emission. [Means for solving the problem]
[0008] [1] A light diffusion device according to an embodiment of the present invention has, in this order, a light source layer including a light source unit and a sealing resin layer that seals the light source unit, a first low refractive index layer having a lower refractive index than the sealing resin layer, and a first diffusion film including a diffusion layer, the diffusion layer including a polymer matrix and dispersed particles including at least one type selected from a liquid crystal compound and a liquid crystal polymer, the dispersion particles being dispersed in the polymer matrix. [2] In the above [1], the refractive index of the first low refractive index layer may be lower than the refractive index of the first diffusion film. [3] In the above [1] or [2], the first low refractive index layer may be a layer including voids or an air layer. [4] In any one of the above [1] to [3], the sealing resin layer may contain at least one resin selected from a silicone resin and an epoxy resin. [5] In any one of the above [1] to [4], the first diffusion film may further include a transparent substrate disposed on at least one side of the diffusion layer. [6] In any one of the above [1] to [5], the light source unit may include a plurality of point light sources. [7] In any one of the above items [1] to [6], the dispersed particles may contain at least the liquid crystal polymer. [8] In the above [7], the first diffusion film may have a plurality of regions having different hazes in a plan view. [9] In the above [7] or [8], the multiple regions may be arranged in a predetermined pattern.
[10] In any of [1] to [9] above, a second low refractive index layer and a second diffusion film may be arranged in this order on the side of the first diffusion film opposite to the side on which the first low refractive index layer is arranged, the second diffusion film may include a diffusion layer including a polymer matrix and dispersed particles dispersed in the polymer matrix and including at least one type selected from a liquid crystal compound and a liquid crystal polymer, and the refractive index of the second low refractive index layer may be lower than those of the first diffusion film and the second diffusion film.
[11] A backlight device according to an embodiment of the present invention includes the light diffusing device according to any one of [1] to
[10] above.
[12] An image display device according to an embodiment of the present invention includes the backlight device described in
[11] above and a display element. Effect of the Invention
[0009] In the manufacture of image display devices, in order to ensure good visibility, generally, adjacent optical films are bonded to each other using an adhesive layer having a relatively high refractive index similar to that of the adjacent optical films themselves to reduce interface reflection, whereas according to the embodiment of the present invention, a low refractive index layer is disposed between the light source layer and the diffusion film, thereby obtaining a light diffusion device with improved uniformity of in-plane luminance. The reason for obtaining such an effect is presumed to be as follows, although this does not limit the present invention in any way. That is, by disposing a low refractive index layer between the light source layer and the diffusion film, the interface reflection between the light source layer and the low refractive index layer increases. As a result, light with reduced directivity enters the diffusion film compared to a configuration in which the light source layer and the diffusion film are directly laminated. It is presumed that the light with reduced directivity is further diffused by the diffusion film, resulting in improved uniformity of in-plane luminance. [Brief description of the drawings]
[0010] [Figure 1] 1 is a schematic cross-sectional view showing a configuration of a light diffusing device according to one embodiment of the present invention. [Diagram 2] 1 is a schematic cross-sectional view showing a configuration of a light diffusing device according to one embodiment of the present invention. [Diagram 3] FIG. 1(a) is a schematic plan view of a diffusion film that can be used in the present invention, and FIG. 1(b) is a schematic cross-sectional view of the diffusion film shown in (a). [Figure 4] FIG. 11 is a schematic diagram illustrating step C of the manufacturing method of the diffusion film. [Diagram 5] FIG. 2 is a schematic cross-sectional view illustrating an electrode having a protrusion. [Figure 6A] 1 is a schematic cross-sectional view of an example of a diffusion film that can be used in the present invention. [Figure 6B] 1 is a schematic cross-sectional view of an example of a diffusion film that can be used in the present invention. [Figure 6C] 1 is a schematic cross-sectional view of an example of a diffusion film that can be used in the present invention. [Figure 7A] FIG. 2 is a schematic cross-sectional view illustrating an example of a low refractive index layer that is an air layer. [Figure 7B] FIG. 2 is a schematic cross-sectional view illustrating an example of a low refractive index layer that is an air layer. [Figure 8] 1 is a schematic cross-sectional view of an image display device according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, preferred embodiments of the present invention will be described, but the present invention is not limited to these embodiments. In this specification, the term "to" indicating a range of values includes the upper and lower limits.
[0012] A. Light diffusion device A light diffusion device according to an embodiment of the present invention has, in this order, a light source layer including a light source unit and a sealing resin layer that seals the light source unit, a first low refractive index layer having a refractive index lower than that of the sealing resin layer, and a first diffusion film including a diffusion layer, the diffusion layer including a polymer matrix and dispersed particles dispersed in the polymer matrix and including at least one type selected from a liquid crystal compound and a liquid crystal polymer.
[0013] 1 is a schematic cross-sectional view showing the configuration of a light diffusion device according to one embodiment of the present invention. The light diffusion device 100A has a light source layer 10 including a light source section 12 and a sealing resin layer 14 sealing the light source section 12, a first diffusion film 20, and a first low refractive index layer 30 disposed therebetween. The first low refractive index layer 30 has a refractive index lower than that of the sealing resin layer 14. Although not shown, the light diffusion device 100A may further have a reflective layer on the side of the light source layer 10 opposite to the side on which the first low refractive index layer 30 is disposed.
[0014] 2 is a schematic cross-sectional view showing the configuration of a light diffusion device according to another embodiment of the present invention. The light diffusion device 100B has a light source layer 10 including a light source section 12 and a sealing resin layer 14 sealing the light source section 12, a first low refractive index layer 30 having a refractive index lower than that of the sealing resin layer 14, a first diffusion film 20, a second low refractive index layer 40, and a second diffusion film 50, in this order. In other words, the light diffusion device 100B has a configuration in which the second low refractive index layer 40 and the second diffusion film 50 are arranged in this order on the first diffusion film 20 of the light diffusion device 100A. The second low refractive index layer 40 preferably has a refractive index lower than that of the first diffusion film 20 and the second diffusion film 50. By laminating the second low refractive index layer 40 and the second diffusion film 50 on the first low refractive index layer 30 and the first diffusion film 20, the effect of improving the uniformity of the in-plane luminance can be more suitably obtained. Although not shown, the light diffusing device 100B may further include a reflective layer on the side of the light source layer 10 opposite to the side on which the first low refractive index layer 30 is disposed.
[0015] A-1.Light source layer The light source layer 10 includes a light source section 12 and a sealing resin layer 14 that seals the light source section 12 .
[0016] The light source 12 is typically composed of a plurality of point light sources 12a. The plurality of point light sources are, for example, arranged two-dimensionally in a predetermined pattern. As the point light source, a light source that emits light with high directivity is preferable, and for example, an LED element can be used.
[0017] Examples of the resin forming the sealing resin layer 14 include thermosetting resins such as silicone resin, epoxy resin, polyester resin, urethane resin, and ethylene vinyl acetate, ultraviolet curing resins such as acrylic resin, urethane resin, vinyl ester resin, and alkyd resin, and thermoplastic resins such as polyolefin, polystyrene, polyisobutylene, and isobutylene-based elastomer. Among them, silicone resin and epoxy resin are preferred, and silicone resin is more preferred, because they have high adhesion to resin films in general and the effects of the present invention can be suitably obtained. The sealing resin layer may be formed using a single resin, or may be formed using two or more resins in combination.
[0018] The Young's modulus of the sealing resin layer (23°C, 50RH%) may be, for example, 5 GPa or less, more specifically, 0.1 GPa to 4 GPa. Since a sealing resin layer having such a Young's modulus tends to have high adhesion to resin films in general, when a PDLC layer or a PDLC film is used as a diffusion film, the interface reflection is reduced, and as a result, the in-plane luminance may not be uniform enough. In contrast, according to an embodiment of the present invention, the first low refractive index layer is provided, so that the in-plane luminance uniformity effect can be suitably obtained. The Young's modulus can be measured, for example, in accordance with JIS K 7127.
[0019] A-2. First diffusion film The first diffusion film includes a diffusion layer and may further include a transparent substrate on one or both sides thereof. The diffusion layer includes a polymer matrix and dispersed particles that are dispersed in the polymer matrix and include at least one selected from a liquid crystal compound and a liquid crystal polymer. In one embodiment (also referred to as "embodiment I"), the diffusion layer has a plurality of regions with different hazes in plan view. In the diffusion layer having a plurality of regions with different hazes, the dispersed particles typically include at least a liquid crystal polymer. The liquid crystal polymer may exist in a different orientation state according to the haze in each region with different haze. In another embodiment (also referred to as "embodiment II"), the diffusion layer has a substantially uniform haze in plan view.
[0020] A-2-1.Embodiment I FIG. 3 is a diagram illustrating an example of a diffusion film including a diffusion layer having a plurality of regions with different hazes in plan view. FIG. 3(a) is a schematic plan view of the diffusion film, and FIG. 3(b) is a schematic cross-sectional view of the diffusion film shown in FIG. 3(a). The diffusion film 20a includes a diffusion layer 22 including a polymer matrix 22a and dispersed particles 22b including a liquid crystal compound 23a and a liquid crystal polymer 23b dispersed in the polymer matrix 22a, a first transparent substrate 24 disposed on one side of the diffusion layer 22, and a second transparent substrate 26 disposed on the other side. The diffusion layer 22 and the first transparent substrate 24 and / or the second transparent substrate 26 may be laminated via an adhesive layer or a pressure-sensitive adhesive layer, or may be laminated directly without the adhesive layer or pressure-sensitive adhesive layer. Depending on the purpose, one or both of the first transparent substrate 24 and the second transparent substrate 26 may be omitted.
[0021] The diffusion layer 22 has five regions (A1, A2, B1, B2, C). Among these regions, the orientation states of the liquid crystal polymer 23b in the regions A1 and A2 are the same as each other, the orientation states of the liquid crystal polymer 23b in the regions B1 and B2 are the same as each other, and the orientation states of the liquid crystal polymer 23b in the regions A1 and A2, the regions B1 and B2, and the region C are different from each other (relationship of the orientation states of the liquid crystal polymer in each region: A1=A2≠B1=B2≠C, A1≠C).
[0022] Specifically, the liquid crystal polymer 23b in the dispersed particles 22b is oriented approximately perpendicular to the main surface of the diffusion film 20a (diffusion layer 22) in the regions A1 and A2, is non-oriented in the region C, and is oriented in an intermediate state in the regions B1 and B2. The liquid crystal compound 23a in the dispersed particles 22b is oriented along the liquid crystal polymer 23b, and is oriented in the same state as the orientation state of the liquid crystal polymer 23b. Therefore, the dispersed particles in these multiple regions (A1, A2, B1, B2, C) may exhibit different scattering properties in each region due to differences in the orientation state of the liquid crystal polymer and / or the liquid crystal compound. As a result, the diffusion film 20a exhibits the smallest haze (diffusion degree) in the regions corresponding to the regions A1 and A2 in a plan view, the largest haze in the region corresponding to the region C, and an intermediate haze in the region corresponding to the regions B1 and B2.
[0023] In the diffusion film 20a, the dispersed particles 22b contain a liquid crystal compound 23a and a liquid crystal polymer 23b, but the dispersed particles 22b may not contain the liquid crystal compound 23a. In addition, in the diffusion film, the orientation of the liquid crystal compound in the dispersed particles can be controlled by the liquid crystal polymer, so there is no need to control the orientation of the liquid crystal compound by applying a voltage. Therefore, the diffusion film does not need to have an electrode layer, regardless of whether the dispersed particles contain a liquid crystal compound or not.
[0024] In the diffusion layer of the illustrated example, the liquid crystal polymer in the dispersed particles has three orientation states, but is not limited to this embodiment. Specifically, the orientation state of the liquid crystal polymer is not particularly limited as long as it is two or more. In addition, the orientation state of the liquid crystal polymer in a plurality of regions in which the orientation state of the liquid crystal polymer is different (in other words, the scattering property of the dispersed particles in the region or the haze of the region) is not limited, and each region may have a desired orientation state independently. Furthermore, the arrangement pattern of these regions is not limited, and can be freely designed as a predetermined pattern. Therefore, the above-mentioned diffusion film can show a desired haze in a desired pattern. In one embodiment, the diffusion layer is configured to have a haze pattern corresponding to the arrangement pattern of the point light source. For example, the diffusion layer is configured so that the haze is high in the region close to the point light source, and the haze decreases as the distance from the point light source increases. According to such a configuration, it is possible to preferably uniformize the in-plane brightness even for a direct-type LED light source.
[0025] In the illustrated diffusion layer, each of the regions (A1, A2, B1, B2, C) in which the orientation state of the liquid crystal polymer in the dispersed particles is different has a certain area, but the region does not need to have an area of a predetermined value or more. For example, in this specification, even if the orientation state of the liquid crystal polymer changes continuously in the in-plane direction and a site in a specific orientation state in a planar view cannot be specified as a region having a certain area, it is treated as "the diffusion layer has multiple regions in which the orientation state of the liquid crystal polymer is different." In one embodiment, when the haze of the diffusion film (more specifically, the diffusion layer) changes continuously in the in-plane direction in a planar view, it is treated as "the diffusion layer has multiple regions with different hazes" and the orientation state of the liquid crystal polymer can be considered to change continuously in the in-plane direction.
[0026] <Diffusion layer> The diffusion layer includes a polymer matrix and dispersed particles that are dispersed in the polymer matrix and contain at least a liquid crystal polymer, and has a plurality of regions with different hazes in plan view. The liquid crystal polymer may be present in different orientation states according to the haze in each region with different haze. As described above, the dispersed particles may further include a liquid crystal compound. In the diffusion film of embodiment I, a non-polymerizable liquid crystal compound is typically used as the liquid crystal compound that may be contained in the dispersed particles. A method for producing the plurality of regions will be described later.
[0027] The haze in each of the multiple regions of the diffusion layer can be appropriately set according to the purpose. The maximum value, minimum value, and difference between the haze in each of the multiple regions of the diffusion layer can be set so as to obtain the maximum value, minimum value, and difference between the haze desired for the diffusion film. The haze of the highest haze region of the diffusion film is, for example, 30% to 100%. The haze of the lowest haze region is, for example, 0% to 70%. The difference between the maximum and minimum haze values of the diffusion film typically exceeds 0%, and is, for example, 5% or more, preferably 10% or more, more preferably 20% to 100%, and even more preferably 30% to 100%. The total light transmittance of the region with the highest haze of the diffusion film is, for example, 10% to 70%, preferably 10% to 50%, and the total light transmittance of the portion with the lowest haze is, for example, 60% to 100%, preferably 80% to 100%.
[0028] The polymer matrix may be composed of any suitable resin. The resin for forming the polymer matrix may be appropriately selected depending on the light transmittance, the refractive index of the liquid crystal polymer or liquid crystal compound, the adhesion to the substrate, and the like. For example, water-soluble or water-dispersible resins such as urethane-based resins, polyvinyl alcohol-based resins, polyethylene-based resins, polypropylene-based resins, and acrylic-based resins may be preferably used. The resin for forming the polymer matrix may be used alone or in combination.
[0029] The content of the polymer matrix in the diffusion layer is, for example, 30% by weight to 70% by weight, preferably 35% by weight to 65% by weight, and more preferably 40% by weight to 60% by weight. If the content of the polymer matrix is within this range, it is possible to obtain effects such as good mechanical strength and prevention of liquid crystal leakage from the edges.
[0030] A liquid crystal polymer is a polymer of a polymerizable liquid crystal compound and is non-liquid crystal, i.e., the liquid crystal polymer does not undergo transition to a liquid crystal phase, a glass phase, or a crystalline phase due to temperature changes, which is characteristic of liquid crystal compounds.
[0031] The polymerizable liquid crystal compound constituting the liquid crystal polymer can be appropriately selected according to the light transmittance, the compatibility with the non-polymerizable liquid crystal compound, and the like. The polymerizable liquid crystal compound may be a crosslinked type having two or more functionalities. As the polymerizable liquid crystal compound, for example, the polymerizable mesogen compounds described in JP-A-2002-533742 (WO00 / 37585), EP358208 (US5211877), EP66137 (US4388453), WO93 / 22397, EP0261712, DE19504224, DE4408171, and GB2280445, etc., can be used. As the polymerizable liquid crystal compound, for example, a nematic type liquid crystal monomer is preferable. The birefringence Δn (=ne-no; ne is the refractive index of the liquid crystal compound molecule in the major axis direction, and no is the refractive index of the liquid crystal compound molecule in the minor axis direction) of the polymerizable liquid crystal compound at a wavelength of 589 nm is preferably 0.05 to 0.50, and more preferably 0.10 to 0.45.
[0032] As the liquid crystal compound, any suitable non-polymerizable liquid crystal compound can be used. As described later, the diffusion layer can be formed by carrying out a polymerization reaction while controlling the orientation of the polymerizable liquid crystal compound. In this case, by using a non-polymerizable liquid crystal compound in combination with a polymerizable liquid crystal compound, the temperature range of the liquid crystal phase (for example, nematic phase) can be expanded, and the orientation can be more suitably controlled. As the liquid crystal compound, a non-polymerizable liquid crystal compound having a birefringence Δn (=ne-no; ne is the refractive index of the liquid crystal compound molecule in the long axis direction, and no is the refractive index of the liquid crystal compound molecule in the short axis direction) of 0.05 to 0.50 at a wavelength of 589 nm, more preferably a birefringence Δn of 0.10 to 0.45, is used.
[0033] The dielectric anisotropy of the non-polymerizable liquid crystal compound may be positive or negative. The non-polymerizable liquid crystal compound may be, for example, a nematic type, a smectic type, or a cholesteric type liquid crystal compound. It is preferable to use a nematic type liquid crystal compound because it can achieve excellent transparency in the transparent state.
[0034] Examples of nematic liquid crystal compounds include biphenyl-based compounds, phenylbenzoate-based compounds, cyclohexylbenzene-based compounds, azoxybenzene-based compounds, azobenzene-based compounds, azomethine-based compounds, terphenyl-based compounds, biphenylbenzoate-based compounds, cyclohexylbiphenyl-based compounds, phenylpyridine-based compounds, cyclohexylpyrimidine-based compounds, cholesterol-based compounds, fluorine-based compounds, etc. These low molecular weight liquid crystal compounds may be used alone or in combination.
[0035] The total content ratio of the liquid crystal polymer and the liquid crystal compound in the diffusion layer when present (the content ratio of the liquid crystal polymer when the liquid crystal compound is not present) is, for example, 30% by weight to 70% by weight, preferably 35% by weight to 65% by weight, more preferably 40% by weight to 60% by weight. The content ratio of the liquid crystal polymer to the total content of the liquid crystal polymer and the liquid crystal compound in the diffusion layer (more specifically, the dispersed particles) is, for example, 5% by weight or more, preferably 7% by weight or more, more preferably 10% by weight or more, and may be, for example, 100% by weight or less, preferably 80% by weight or less, more preferably 50% by weight or less. The total content ratio of the polymer matrix, the liquid crystal polymer, and the liquid crystal compound in the diffusion layer when present may be, for example, 90% by weight to 99.9% by weight, preferably 95% by weight to 99.9% by weight.
[0036] As described later, in the preparation of the diffusion film of embodiment I, the diffusion layer can be formed by preparing a PDLC layer containing liquid crystal droplets containing a polymerizable liquid crystal compound and a non-polymerizable liquid crystal compound as an optional component, and polymerizing the polymerizable liquid crystal compound while applying a voltage from the first main surface side and the second main surface side of the PDLC layer so that regions with different electric field strengths are generated. Thus, the diffusion layer (more specifically, the dispersed particles) can further contain a polymerization initiator. The type and content of the polymerization initiator will be described later. In addition, unreacted polymerizable liquid crystal compound may remain in the dispersed particles. The content of the unreacted polymerizable liquid crystal compound in the diffusion layer is, for example, 3% by weight or less, preferably 1% by weight or less.
[0037] The average particle diameter of the dispersed particles may be, for example, 0.2 μm to 9 μm, preferably 0.3 μm to 8 μm. If the average particle diameter of the dispersed particles is too small, the dispersed particle size is smaller than the wavelength of light, so that the light passes through the dispersed particles without being scattered, and as a result, a problem may occur in which sufficient haze cannot be obtained. If the average particle diameter is too large, the dispersed particle size is too large than the wavelength of light, so that a problem may occur in which sufficient haze cannot be obtained. The average particle diameter of the dispersed particles in the diffusion layer is the volume average particle diameter of the dispersed particles when viewed from a direction perpendicular to the main surface of the diffusion film.
[0038] The thickness of the diffusion layer is, for example, 20 μm to 150 μm, preferably 30 μm to 120 μm, and more preferably 40 μm to 100 μm.
[0039] <First transparent substrate> The first transparent substrate 24 includes a first transparent film. The first transparent substrate may have a hard coat (HC) layer on one or both sides of the first transparent film, if necessary.
[0040] The haze of the first transparent substrate is preferably 20% or less, more preferably 10% or less, and further preferably 0.1% to 10%.
[0041] The total light transmittance of the first transparent substrate is preferably 30% or more, more preferably 60% or more, and further preferably 80% or more. The total light transmittance can be measured according to JIS K 7361.
[0042] The first transparent film can be formed using any suitable material. Specific examples include glass film and polymer film. Polymer film is preferable because it has excellent smoothness and can greatly improve productivity by continuous production using rolls.
[0043] The polymer film is typically a polymer film mainly composed of a thermoplastic resin. Examples of the thermoplastic resin include polyester resins; cycloolefin resins such as polynorbornene; acrylic resins; polycarbonate resins; and cellulose resins. Among them, polyester resins, cycloolefin resins, and acrylic resins are preferred. These resins are excellent in transparency, mechanical strength, thermal stability, and moisture shielding properties. The above-mentioned thermoplastic resins may be used alone or in combination of two or more. In addition, optical films such as those used in polarizing plates, such as low retardation substrates, high retardation substrates, retardation plates, absorptive polarizing films, and polarized selective reflection films, can also be used as the first transparent film.
[0044] The total light transmittance of the first transparent film is preferably 30% or more, more preferably 60% or more, and further preferably 80% or more.
[0045] The thickness of the first transparent substrate (thickness including the HC layer if the substrate has an HC layer) is preferably 200 μm or less, more preferably 3 μm to 150 μm, and further preferably 5 μm to 100 μm.
[0046] <Second transparent substrate> The second transparent substrate 26 includes a second transparent film. The second transparent substrate may have a hard coat layer on one or both sides of the second transparent film, if necessary.
[0047] The haze of the second transparent substrate is preferably 20% or less, more preferably 10% or less, and further preferably 0.1% to 10%.
[0048] The total light transmittance of the second transparent substrate is preferably 30% or more, more preferably 60% or more, and further preferably 80% or more.
[0049] The thickness of the second transparent base material (thickness including the HC layer if the second transparent base material has an HC layer) is preferably 200 μm or less, more preferably 3 μm to 150 μm, and further preferably 5 μm to 100 μm.
[0050] The second transparent film can be described in the same manner as the first transparent film. The second transparent substrate may have the same structure as the first transparent substrate, or may have a different structure.
[0051] <Production method> The diffusion film can be manufactured by any suitable manufacturing method. The diffusion film can be manufactured by, for example, (Step A) applying a coating liquid containing a polymer matrix-forming resin, a polymerizable liquid crystal compound, and a solvent to a first substrate to obtain a coating layer; (Step B) drying the coating layer to obtain a PDLC layer including a polymer matrix and droplets including the polymerizable liquid crystal compound dispersed in the polymer matrix; and (Step C) polymerizing the polymerizable liquid crystal compound while applying a voltage from the first principal surface side and the second principal surface side of the PDLC layer so as to generate regions with different electric field intensities, thereby obtaining a diffusion layer; Includes. The method for producing the diffusion film may further include, as necessary, disposing a second substrate on the side of the PDLC layer or the diffusion layer opposite to the side on which the first substrate is provided before or after polymerizing the polymerizable liquid crystal compound (step D). According to the method for producing the diffusion film, the polymerizable liquid crystal compound is polymerized in different orientation states according to the electric field strength in each region with different electric field strength. As a result, a diffusion layer having a plurality of regions with different orientation states of the liquid crystal polymer in the dispersed particles (as a result, a diffusion layer having a plurality of regions with different hazes) may be formed.
[0052] (Process A) In step A, a coating liquid containing a polymer matrix-forming resin, a polymerizable liquid crystal compound, and a solvent is applied to a first substrate to obtain a coating layer. The coating liquid may further contain a non-polymerizable liquid crystal compound.
[0053] The coating liquid is preferably an emulsion containing a polymerizable liquid crystal compound and liquid crystal particles as a dispersoid, which may further contain a non-polymerizable liquid crystal compound (hereinafter, this may be referred to as an "emulsion coating liquid"). In one embodiment, the coating liquid is an emulsion coating liquid in which polymer matrix forming resin particles and liquid crystal particles containing a polymerizable liquid crystal compound and optionally a non-polymerizable liquid crystal compound are dispersed in a solvent. The emulsion coating liquid preferably further contains a polymerization initiator in the liquid crystal particles, and may further contain any appropriate additive depending on the purpose.
[0054] As the solvent, water or a mixed solvent of water and a water-miscible organic solvent can be preferably used. As the water-miscible organic solvent, C1-3 alcohol, acetone, DMSO, etc. can be mentioned. The polymerizable liquid crystal compound, the non-polymerizable liquid crystal compound, and the resin for forming the polymer matrix are as described above. As the optional additive, a dispersant, a leveling agent, a crosslinking agent, etc. can be mentioned.
[0055] The content of the liquid crystal compound in the solid content of the coating liquid (the total content of the polymerizable liquid crystal compound and the non-polymerizable liquid crystal compound, if present) can be, for example, 30% by weight to 70% by weight, preferably 35% by weight to 65% by weight, and more preferably 40% by weight to 60% by weight.
[0056] The weight ratio of the polymerizable liquid crystal compound to the non-polymerizable liquid crystal compound in the coating liquid (polymerizable liquid crystal compound:non-polymerizable liquid crystal compound) may be, for example, 5:95 to 100:0, preferably 7:93 to 80:20, and more preferably 10:90 to 50:50.
[0057] The content of the polymer matrix-forming resin in the solid content of the coating liquid can be, for example, 30% by weight to 70% by weight, preferably 35% by weight to 65% by weight, and more preferably 40% by weight to 60% by weight.
[0058] The weight ratio of the content of the liquid crystal compound (total content of the polymerizable liquid crystal compound and the non-polymerizable liquid crystal compound when present) to the content of the resin for forming a polymer matrix (liquid crystal compound:resin for forming a polymer matrix) in the coating liquid may be, for example, 30:70 to 70:30, preferably 35:65 to 65:35, and more preferably 40:60 to 60:40. The total content ratio of the resin for forming a polymer matrix and the polymerizable liquid crystal compound and the non-polymerizable liquid crystal compound when present in the solid content of the coating liquid may be, for example, 90% by weight to 99.9% by weight, and preferably 95% by weight to 99.9% by weight.
[0059] The average particle diameter of the liquid crystal particles is preferably 0.2 μm or more, more preferably 0.3 μm or more. The average particle diameter of the liquid crystal particles is preferably 9 μm or less, more preferably 8 μm or less. If the average particle diameter of the liquid crystal particles is within this range, the average particle diameter of the dispersed particles in the diffusion layer can be set to a desired range. The average particle diameter of the liquid crystal particles is a volume average particle diameter.
[0060] The average particle size of the liquid crystal particles preferably has a relatively narrow particle size distribution. The coefficient of variation (CV value) of the average particle size of the liquid crystal particles may be, for example, less than 0.40, preferably 0.35 or less, and more preferably 0.30 or less. In one embodiment, an emulsion coating liquid that is substantially free of liquid crystal particles having a particle size of less than 0.2 μm or more than 9 μm (for example, an emulsion coating liquid in which the volume ratio of liquid crystal particles having a particle size of less than 0.2 μm or more than 9 μm to the total volume of liquid crystal particles is 10% or less) may be used.
[0061] The average particle diameter of the resin particles for forming a polymer matrix is preferably 10 nm to 500 nm, more preferably 30 nm to 300 nm, and further preferably 50 nm to 200 nm. Two or more kinds of resin particles having different resin types and / or average particle diameters may be used. The average particle diameter of the resin particles for forming a polymer matrix means the volume average particle diameter, and can be measured using a dynamic light scattering particle size distribution measuring device.
[0062] As the polymerization initiator, any appropriate photopolymerization initiator or thermal polymerization initiator can be used depending on the purpose, desired properties, etc., and a photopolymerization initiator is preferably used. Specific examples of photopolymerization initiators include 2,2-dimethoxy-2-phenylacetophenone, acetophenone, benzophenone, xanthone, 3-methylacetophenone, 4-chlorobenzophenone, 4,4'-dimethoxybenzophenone, benzoin propyl ether, benzyl dimethyl ketal, N,N,N',N'-tetramethyl-4,4'-diaminobenzophenone, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis-(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-2,4-dipentoxyphenylphosphine oxide, bis(2,6-dimethoxy-benzoyl)-(2,4,4-trimethyl-pentyl)-phosphine oxide, and thioxanthone compounds. The polymerization initiators may be used alone or in combination of two or more. The content of the polymerization initiator is preferably 0.1 to 10 parts by weight, and more preferably 0.5 to 5 parts by weight, based on 100 parts by weight of the polymerizable liquid crystal compound.
[0063] Examples of the dispersant include anionic surfactants, cationic surfactants, amphoteric surfactants, nonionic surfactants, etc. The content of the dispersant is preferably 0.05 to 10 parts by weight, more preferably 0.1 to 1 part by weight, relative to 100 parts by weight of the coating liquid.
[0064] Examples of the leveling agent include an acrylic leveling agent, a fluorine-based leveling agent, a silicone-based leveling agent, etc. The content of the leveling agent is preferably 0.05 to 10 parts by weight, more preferably 0.1 to 1 part by weight, relative to 100 parts by weight of the coating liquid.
[0065] Examples of the crosslinking agent include aziridine-based crosslinking agents, isocyanate-based crosslinking agents, etc. The content of the crosslinking agent is preferably 0.5 to 10 parts by weight, more preferably 0.8 to 5 parts by weight, relative to 100 parts by weight of the coating liquid.
[0066] The coating liquid, preferably the emulsion coating liquid, can be prepared, for example, by mixing a resin emulsion or a resin particle dispersion containing resin particles for forming a polymer matrix, a liquid crystal emulsion containing liquid crystal particles containing a polymerizable liquid crystal compound, a polymerization initiator, and optionally a non-polymerizable liquid crystal compound, and any additives (for example, a dispersant, a leveling agent, a crosslinking agent). If necessary, a solvent may be further added during mixing. Alternatively, the emulsion coating liquid can also be prepared by adding a polymerizable liquid crystal compound, a resin for forming a polymer matrix, a polymerization initiator, and optionally a non-polymerizable liquid crystal compound and additives to a solvent, and mechanically dispersing the mixture.
[0067] The resin emulsion and liquid crystal emulsion can be prepared, for example, by a mechanical emulsification method, an ultrasonic emulsification method, a microchannel method, a membrane emulsification method, or the like.
[0068] The solids concentration of the coating liquid may be, for example, 20% by weight to 60% by weight, and preferably 30% by weight to 50% by weight.
[0069] The viscosity of the coating liquid can be appropriately adjusted so that the coating liquid is applied to the first substrate in a suitable manner. The viscosity of the coating liquid during application is preferably 20 mPas to 400 mPas, more preferably 30 mPas to 300 mPas, and even more preferably 40 mPas to 200 mPas. If the viscosity is less than 20 mPas, convection of the solvent becomes significant when the solvent is dried, and the thickness of the PDLC layer (as a result, the diffusion layer) may become unstable. If the viscosity exceeds 400 mPas, the bead of the coating liquid may become unstable. The viscosity of the coating liquid can be measured, for example, by a rheometer MCR302 manufactured by Anton Paar. The viscosity used here is the shear viscosity value under the conditions of 20°C and a shear rate of 1000 (1 / s).
[0070] Any suitable substrate can be used as the first substrate. By using the first transparent substrate as the first substrate, a diffusion film having the first transparent substrate and a diffusion layer can be suitably obtained. Depending on the purpose, the first substrate may be peeled off from the diffusion layer after the end of step C.
[0071] Any appropriate method can be used as the coating method, for example, roll coating, spin coating, wire bar coating, dip coating, die coating, curtain coating, spray coating, knife coating (comma coating, etc.), etc.
[0072] The thickness of the coating layer is preferably 40 μm to 300 μm, more preferably 60 μm to 240 μm, and further preferably 80 μm to 200 μm. Within such a range, a diffusion layer having excellent in-plane luminance improving effect and excellent thickness uniformity can be obtained.
[0073] (Process B) In step B, the coating layer is dried to obtain a PDLC layer containing a polymer matrix and droplets containing a polymerizable liquid crystal compound and optionally a non-polymerizable liquid crystal compound dispersed in the polymer matrix. The solvent is removed from the coating layer by drying, and the resin particles for forming the polymer matrix are fused to each other to form a PDLC layer having a structure in which liquid crystal droplets are dispersed in a polymer matrix.
[0074] The coating layer can be dried by any appropriate method. Specific examples of the drying method include natural drying, heat drying, hot air drying, etc. When the coating liquid contains a crosslinking agent, a crosslinked structure of the polymer matrix can be formed during drying.
[0075] The drying temperature is preferably 20° C. to 150° C., and more preferably 25° C. to 80° C. The drying time is preferably 1 minute to 100 minutes.
[0076] (Process C) In step C, the polymerizable liquid crystal compound is polymerized while applying a voltage from the first and second main surfaces of the PDLC layer so as to generate regions with different electric field strengths, thereby forming a diffusion layer including a polymer matrix and dispersed particles that are dispersed in the polymer matrix and contain a liquid crystal polymer, which is a polymer of the polymerizable liquid crystal compound.
[0077] The polymerization of the polymerizable liquid crystal compound is carried out by irradiation with active energy rays, heating, or a combination of these, and is preferably carried out by irradiation with active energy rays.
[0078] Examples of the active energy rays include ultraviolet rays, infrared rays, X-rays, α rays, β rays, γ rays, and electron beams. Among these, ultraviolet rays are preferred. Moreover, the active energy rays are preferably collimated light that has a high linearity from the irradiation source.
[0079] The ultraviolet irradiation conditions can be appropriately set depending on the type of polymerizable liquid crystal compound, the transmittance of the substrate, the absorption wavelength of the photopolymerization initiator, etc. The irradiation intensity is, for example, 0.1 mW / cm 2~1000mW / cm 2 , preferably 1 mW / cm 2 ~100mW / cm 2 The irradiation dose can be, for example, 10 mJ / cm 2 ~10000mJ / cm 2 , preferably 100 mJ / cm 2 ~5000mJ / cm 2 The irradiation temperature may be, for example, from -20°C to 80°C, and preferably from -20°C to 60°C.
[0080] In one embodiment, the voltage is applied using a first electrode arranged on the first principal surface side of the PDLC layer and a second electrode arranged on the second principal surface side, and the distance between the first electrode and the second electrode is controlled to form regions with different electric field strengths. Hereinafter, step C will be described with reference to FIG. 4. In the embodiment shown in FIG. 4, step D is performed before step C, and a first transparent substrate 24 is arranged as a first substrate on the first principal surface side of the PDLC layer 22', and a second transparent substrate 26 is arranged as a second substrate on the second principal surface side. Unlike the illustrated example, the first principal surface and / or the second principal surface of the PDLC layer may be exposed.
[0081] FIG. 4(a) is a schematic cross-sectional view showing the PDLC layer obtained in step B in a state where no voltage is applied. The PDLC layer 22' includes a polymer matrix 22a and liquid crystal droplets 22b' dispersed in the polymer matrix 22a, and the liquid crystal droplets 22b' include a non-polymerizable liquid crystal compound 23a and a polymerizable liquid crystal compound 23c. A first electrode 310 is disposed on the outside (opposite side to the side where the PDLC layer is disposed) of the first transparent substrate 24, and a second electrode 320 is disposed on the outside (opposite side to the side where the PDLC layer is disposed) of the second transparent substrate 26. Since no voltage is applied from a power source 330 to the electrodes 310 and 320 and no electric field is generated between them, the non-polymerizable liquid crystal compound 23a and the polymerizable liquid crystal compound 23c in the liquid crystal droplets 22b' are present in a non-oriented state. In addition, the first electrode 310 is formed so that the surface height on the PDLC layer 22' side varies depending on the location, and thus regions with different inter-electrode distances are formed.
[0082] The region with different inter-electrode distances can be freely designed, for example, by changing the surface shape of the first electrode and / or the second electrode on the PDLC layer side. Specifically, a desired inter-electrode distance can be realized in a desired pattern by providing the surface of the first electrode and / or the second electrode with unevenness, steps, inclinations, etc. in an arbitrary pattern. For example, as shown in FIG. 5, by providing tapered convex portions 312 on the surface of electrode 310a, the inter-electrode distance can be continuously changed, and as a result, the orientation state of the polymerizable liquid crystal compound and the non-polymerizable liquid crystal compound in the liquid crystal droplet can be continuously changed in the plane. At this time, by changing the height H and the inclination angle θ, the amount and rate of change of the inter-electrode distance can be controlled, and as a result, the obtained diffusion film can have a haze with an arbitrary gradient. The height H and the inclination angle θ can each be set to any appropriate value according to the haze pattern desired for the diffusion film.
[0083] FIG. 4(b) is a schematic diagram showing an embodiment in which the polymerizable liquid crystal compound 23c is polymerized by UV irradiation. UV irradiation is performed in a state where a voltage is applied between the first electrode 310 and the second electrode 320 from the power source 330. The application of the voltage generates an electric field between the first electrode 310 and the second electrode 320, the strength of which depends on the distance between them, and as a result, a plurality of regions with different electric field strengths are generated. In each of the plurality of regions, the non-polymerizable liquid crystal compound 23a and the polymerizable liquid crystal compound 23c in the liquid crystal droplet 22b' are aligned according to the electric field strength. Specifically, in the region where the distance between the first electrode 310 and the second electrode 320 is the smallest, the non-polymerizable liquid crystal compound 23a and the polymerizable liquid crystal compound 23c are aligned approximately perpendicular to the main surface of the PDLC layer 22', and as the distance between them increases, the degree of alignment becomes weaker. By polymerizing the polymerizable liquid crystal compound 23c under such conditions, a diffusion layer 22 is formed having multiple regions in which the orientation state of the liquid crystal polymer 23b in the dispersed particles 22b is different (as a result, multiple regions with different haze), as shown in Figure 4(c).
[0084] The voltage applied during polymerization is not limited as long as the polymerizable liquid crystal compound exhibits the desired alignment, and can be appropriately set according to the haze desired for the diffusion film, the distance between the electrodes, etc. The voltage can be, for example, 10 V to 100 kV, and preferably 100 V to 10 kV.
[0085] (Process D) In step D, a second substrate is disposed on the side (second main surface side) of the PDLC layer or the diffusion layer opposite to the side (first main surface side) on which the first substrate is provided. Any appropriate substrate may be used as the second substrate, and the above-mentioned second transparent substrate may be preferably used. The timing of carrying out step D may be before step C, i.e., before polymerizing the polymerizable liquid crystal compound, or after step C, i.e., after polymerizing the polymerizable liquid crystal compound.
[0086] According to the method for manufacturing a diffusion film including steps A to D, by using the above-mentioned first transparent substrate and the above-mentioned second transparent substrate as the first substrate and the second substrate, respectively, a diffusion film having the first transparent substrate and the second transparent substrate and a diffusion layer directly sandwiched therebetween can be obtained.
[0087] In order to obtain sufficient adhesion, the second substrate is laminated on the second main surface side of the PDLC layer or the diffusion layer, preferably using a laminator, while applying a lamination pressure of 0.006 MPa / m to 7 MPa / m, more preferably 0.06 MPa / m to 0.7 MPa / m.
[0088] A-2-2.Embodiment II The diffusion film 20b shown in FIG. 6A includes a diffusion layer 22 including a polymer matrix 22a and dispersed particles 22b including a liquid crystal compound 23a and a liquid crystal polymer 23b dispersed in the polymer matrix 22a, a first transparent substrate 24 disposed on one side of the diffusion layer 22, and a second transparent substrate 26 disposed on the other side. The diffusion layer 22 and the first transparent substrate 24 and / or the second transparent substrate 26 may be laminated via an adhesive layer or a pressure-sensitive adhesive layer, or may be laminated directly without the adhesive layer or pressure-sensitive adhesive layer. Depending on the purpose, one or both of the first transparent substrate 24 and the second transparent substrate 26 may be omitted. In the diffusion film of embodiment II, the diffusion layer may include dispersed particles including a liquid crystal polymer and not including a liquid crystal compound, or may include dispersed particles including a liquid crystal compound and not including a liquid crystal polymer. For example, the diffusion film 20c shown in Fig. 6B includes a diffusion layer 22 including a polymer matrix 22a and dispersed particles 22b that are dispersed in the polymer matrix 22a and include a liquid crystal polymer 23b and do not include a liquid crystal compound, a first transparent substrate 24 disposed on one side of the diffusion layer 22, and a second transparent substrate 26 disposed on the other side. Also, for example, the diffusion film 20d shown in Fig. 6C includes a diffusion layer 22 including a polymer matrix 22a and dispersed particles 22b that are dispersed in the polymer matrix 22a and include a liquid crystal compound 23a and do not include a liquid crystal polymer, a first transparent substrate 24 disposed on one side of the diffusion layer 22, and a second transparent substrate 26 disposed on the other side.
[0089] In the diffusion film of embodiment II, typically, the orientation state of the liquid crystal compound and / or liquid crystal polymer in the dispersed particles is substantially uniform throughout the entire diffusion layer, and as a result, the diffusion layer can have a substantially uniform haze when viewed in a plane.
[0090] Due to the diffusion layer having a substantially uniform haze, the diffusion film of embodiment II (e.g., diffusion films 20b to 20d) also have a substantially uniform haze. The difference between the maximum and minimum haze values in the diffusion film of embodiment II is, for example, less than 10%, preferably less than 5%. The haze of the diffusion film of embodiment II is, for example, 50% to 80%, and for example, 70% to 100%, respectively.
[0091] The same explanation as for the diffusion film of embodiment I can be applied to the diffusion film of embodiment II, except that the orientation state of the liquid crystal compound and / or liquid crystal polymer in the dispersed particles is substantially uniform throughout the diffusion layer. For example, in the diffusion films 20b and 20c, the liquid crystal compound 23a and / or the liquid crystal polymer 23b may be in a predetermined orientation state or in a non-oriented state. Also, for example, in the diffusion film 20d, the liquid crystal compound 23a may be in a non-oriented state.
[0092] A diffusion film in which dispersed particles contain a liquid crystal polymer (e.g., diffusion film 20b or 20c) can be obtained in the same manner as the diffusion film of embodiment I, except that in step C above, the polymerizable liquid crystal compound is polymerized without applying a voltage to the PDLC layer or while applying a predetermined voltage so that the electric field strength between the electrodes is constant. For example, a diffusion film with high haze can be obtained by performing polymerization without applying a voltage. Also, for example, the haze of the resulting diffusion film can be reduced by increasing the electric field strength between the electrodes during polymerization.
[0093] A diffusion film in which the dispersed particles contain a liquid crystal compound and do not contain a liquid crystal polymer (e.g., diffusion film 20d) can be obtained by a method similar to that of the diffusion film of embodiment I, except that step C is not performed. In such a diffusion film, the liquid crystal compound may be a polymerizable liquid crystal compound, a non-polymerizable liquid crystal compound, or a combination of both. In one embodiment, a coating liquid containing a non-polymerizable liquid crystal compound and not containing a polymerizable liquid crystal compound and a polymerization initiator may be used.
[0094] A-3. First low refractive index layer The first low refractive index layer 30 has a refractive index lower than that of the sealing resin layer 14. The refractive index of the first low refractive index layer is, for example, 1.30 or less, preferably 1.20 or less, more preferably 1.15 or less, and more preferably corresponds to the refractive index of air (1.00). The lower limit of the refractive index of the first low refractive index layer is, for example, the refractive index of air (1.00). If the refractive index of the first low refractive index layer is in such a range, the interfacial reflection at the interface with the light source layer is increased, thereby realizing a light diffusion device with high uniformity of in-plane luminance. The difference between the refractive index of the first low refractive index layer and the refractive index of the sealing resin layer is, for example, 0.1 or more and 0.4 or less, preferably 0.2 or more and 0.4 or less.
[0095] The first low refractive index layer preferably has a refractive index lower than that of the first diffusion film. The difference between the refractive index of the first low refractive index layer and that of the first diffusion film is, for example, 0.2 to 0.6, preferably 0.3 to 0.6. The phrase "the first low refractive index layer has a refractive index lower than that of the first diffusion film" means that the refractive index of the first low refractive index layer is lower than the refractive index of the surface of the first diffusion film on the first low refractive index layer side, and therefore means that when the first diffusion film has a transparent substrate on the light source layer side of the diffusion layer, the refractive index is lower than that of the transparent substrate, and when the first diffusion film does not have a transparent substrate, the refractive index is lower than that of the polymer matrix. The refractive index of the polymer matrix is usually 1.49 to 1.60, for example 1.49 to 1.55. The refractive index of the transparent substrate is usually 1.49 to 1.65, for example 1.49 to 1.58.
[0096] The first low refractive index layer can have any structure as long as it has the above refractive index. In one embodiment, the first low refractive index layer is a low refractive index layer having a void therein. In another embodiment, the first low refractive index layer is an air layer.
[0097] A-3-1. Low refractive index layer with internal voids The porosity of the low refractive index layer having voids therein can be any appropriate value. The porosity is, for example, 5% to 99%, and preferably 25% to 95%. When the porosity is within the above range, the refractive index of the low refractive index layer can be sufficiently low and high mechanical strength can be obtained. Air typically exists in the voids.
[0098] The low refractive index layer may be formed of at least one of a particle-like, fibrous, and flat-shaped structure. The particle-like structure (structural unit) may be a solid particle or a hollow particle, and specifically includes silicone particles, silicone particles having micropores, hollow silica nanoparticles, and hollow silica nanoballoons. The fibrous structural unit may be, for example, a nanofiber having a nano-sized diameter, and specifically includes cellulose nanofibers and alumina nanofibers. The flat structural unit may be, for example, nanoclay, and specifically includes nano-sized bentonite (for example, Kunipia F [trade name]). In addition, in the void structure of the low refractive index layer, the structural units of a single type or a plurality of types forming the void structure include a portion that is chemically bonded, for example, directly or indirectly, via a catalytic action. In addition, in the present invention, the structural units are "indirectly bonded" to each other, which means that the structural units are bonded to each other via a small amount of binder component that is equal to or less than the amount of the structural unit. The phrase "constituent units are directly bonded" means that the constituent units are directly bonded to each other without the intervention of a binder component or the like.
[0099] Any suitable material may be used as the material constituting the low refractive index layer. For example, the materials described in International Publication No. 2004 / 113966, JP 2013-254183, and JP 2012-189802 may be used as the material. Specifically, for example, silica-based compounds; hydrolyzable silanes, and their partial hydrolyzates and dehydration condensates; organic polymers; silicon compounds containing silanol groups; activated silica obtained by contacting silicate with acid or ion exchange resin; polymerizable monomers (e.g., (meth)acrylic monomers and styrene monomers); curable resins (e.g., (meth)acrylic resins, fluorine-containing resins, and urethane resins); and combinations thereof may be used.
[0100] Examples of the organic polymer include polyolefins (e.g., polyethylene and polypropylene), polyurethanes, fluorine-containing polymers (e.g., fluorine-containing copolymers having, as constituent components, a fluorine-containing monomer unit and a constituent unit for imparting crosslinking reactivity), polyesters (e.g., poly(meth)acrylic acid derivatives (in this specification, (meth)acrylic acid means acrylic acid and methacrylic acid, and "(meth)" is used in this sense in all cases)), polyethers, polyamides, polyimides, polyureas, and polycarbonates.
[0101] The above-mentioned material preferably includes a silica-based compound; hydrolyzable silanes, and partial hydrolyzates and dehydrated condensates thereof.
[0102] Examples of the silica-based compounds include SiO2 (silicic anhydride); compounds containing SiO2 and at least one compound selected from the group consisting of Na2O-B2O3 (borosilicate), Al2O3 (alumina), B2O3, TiO2, ZrO2, SnO2, Ce2O3, P2O5, Sb2O3, MoO3, ZnO2, WO3, TiO2-Al2O3, TiO2-ZrO2, In2O3-SnO2, and Sb2O3-SnO2 (the "-" above indicates a composite oxide);
[0103] The hydrolyzable silanes include, for example, hydrolyzable silanes containing an alkyl group which may have a substituent (e.g., fluorine). The hydrolyzable silanes and their partial hydrolyzates and dehydration condensates are preferably alkoxysilanes and silsesquioxanes.
[0104] The alkoxysilane may be a monomer or an oligomer. The alkoxysilane monomer preferably has three or more alkoxyl groups. Examples of the alkoxysilane monomer include methyltrimethoxysilane, methyltriethoxysilane, phenyltriethoxysilane, tetramethoxysilane, tetraethoxysilane, tetrabutoxysilane, tetrapropoxysilane, diethoxydimethoxysilane, dimethyldimethoxysilane, and dimethyldiethoxysilane. The alkoxysilane oligomer is preferably a polycondensate obtained by hydrolysis and polycondensation of the above monomer. By using an alkoxysilane as the material, a low refractive index layer having excellent uniformity can be obtained.
[0105] Silsesquioxanes have the general formula RSiO 1.5 (wherein R represents an organic functional group). Examples of R include an alkyl group (which may be linear or branched and has 1 to 6 carbon atoms), a phenyl group, and an alkoxy group (e.g., a methoxy group and an ethoxy group). Examples of the silsesquioxane structure include a ladder type and a cage type. By using silsesquioxane as the material, a low refractive index layer having excellent uniformity, weather resistance, transparency, and hardness can be obtained.
[0106] As the particles, any appropriate particles can be adopted. The particles are typically made of a silica-based compound.
[0107] The shape of the silica particles can be confirmed, for example, by observation with a transmission electron microscope. The average particle size of the particles is, for example, 5 nm to 200 nm, and preferably 10 nm to 200 nm. By having the above-mentioned constitution, it is possible to obtain a low refractive index layer having a sufficiently low refractive index, and to maintain the transparency of the low refractive index layer. Here, the average particle size of the particles is the specific surface area (m2) measured by a nitrogen adsorption method (BET method). 2 / g), the average particle size is defined as the value given by the formula: average particle size=(2720 / specific surface area) (see JP-A-1-317115).
[0108] The haze of the low refractive index layer is, for example, 0.1% to 30%, and preferably 0.2% to 10%.
[0109] The low refractive index layer preferably has a mechanical strength of, for example, a scratch resistance of 60% to 100% as measured by Bemcot (registered trademark).
[0110] The low refractive index layer has a thickness of preferably 0.1 μm to 100 μm, more preferably 0.2 μm to 30 μm, and further preferably 1 μm to 20 μm. If the thickness is less than 0.1 μm, the effect of the low refractive index layer may not be sufficiently obtained. If the thickness is more than 100 μm, there is a problem that the thickness of the light diffusing device becomes large.
[0111] Examples of the method for obtaining the low refractive index layer include those described in JP 2010-189212 A, JP 2008-040171 A, JP 2006-011175 A, WO 2004 / 113966 A, and references thereto.Specific examples include a method of hydrolyzing and polycondensing at least one of silica-based compounds, hydrolyzable silanes, and their partial hydrolyzates and dehydration condensates, a method of using porous particles and / or hollow fine particles, a method of generating an aerogel layer by utilizing the springback phenomenon, a method of crushing a gel obtained by sol-gel and chemically bonding the microporous particles in the crushed liquid with a catalyst, etc.
[0112] The low refractive index layer may be formed on a substrate film and supported by the substrate film. The same explanation as for the first transparent film in A-2 can be applied to the substrate film. As long as the effect of the present invention can be obtained, the refractive index of the substrate film is not particularly limited.
[0113] A-3-2. Low refractive index layer that is an air gap In one embodiment, the air layer as the low refractive index layer 30 can be formed spontaneously between the resin film 32 and the diffusion film 20 by disposing the resin film 32 on the light source layer 10 and laminating the diffusion film 20 thereon without an adhesive layer, as shown in Fig. 7A. The thickness of the air layer formed in this embodiment is not particularly limited, but is, for example, 0.1 µm to 3 µm, and preferably 1 µm to 3 µm.
[0114] As the resin film, a film having low adhesion to the diffusion film is preferably used. The arithmetic mean roughness (Ra) of the resin film surface is, for example, 10 nm or more, preferably 50 nm or more. The upper limit of Ra of the resin film is not particularly limited, but may be, for example, 100 nm or less. One or both sides of the resin film may be subjected to a surface roughening treatment. In this case, Ra of the resin film may be 1 μm to 2 μm. Ra can be measured in accordance with JIS B 0601.
[0115] The resin forming the resin film is not limited as long as the effects of the present invention can be obtained, and examples thereof include polyester resins such as polyethylene terephthalate (PET), cycloolefin resins such as polynorbornene, acrylic resins, polycarbonate resins, and cellulose resins. These resins may be used alone or in combination of two or more. The thickness of the resin film is, for example, 10 μm to 100 μm.
[0116] In another embodiment, the air layer as the low refractive index layer 30 can be formed as a space having a height according to the diameter of the spacer between the light source layer 10 and the diffusion film 20 by laminating the diffusion film 20 on the light source layer 10 via a spacer 34, as shown in Fig. 7B. The spacer 34 may be fixed to the light source layer 10 and / or the diffusion film 20 by an adhesive, or may be interposed between the light source layer 10 and the diffusion film 20 without being fixed by an adhesive. The thickness of the air layer formed in this embodiment is not particularly limited, but is, for example, 1 µm to 20 µm, preferably 5 µm to 20 µm, depending on the particle size of the spacer.
[0117] A-4. Second diffusion film The second diffusion film 50 includes, for example, a diffusion layer, a third transparent substrate disposed on one side of the diffusion layer, and a fourth transparent substrate disposed on the other side. As long as the effects of the present invention are obtained, one or both of the third transparent substrate and the fourth transparent substrate may be omitted.
[0118] The second diffusion film 50 can be described in the same manner as the first diffusion film 20. The first diffusion film and the second diffusion film may have the same configuration or different configurations. For example, both the first diffusion film and the second diffusion film may have a substantially uniform haze in a planar view, or both the first diffusion film and the second diffusion film may have a non-uniform haze in a planar view (in other words, they may have a plurality of regions with different hazes). Also, for example, one of the first diffusion film and the second diffusion film may have a substantially uniform haze in a planar view, and the other may have a non-uniform haze.
[0119] A-5. Second low refractive index layer The second low refractive index layer 40 typically has a refractive index lower than that of the first diffusion film 20 and the second diffusion film 50. The refractive index of the second low refractive index layer 40 is, for example, 1.30 or less, preferably 1.20 or less, more preferably 1.15 or less, and more preferably corresponds to the refractive index of air (1.00). The lower limit of the refractive index of the second low refractive index layer is, for example, the refractive index of air (1.00). If the refractive index of the second low refractive index layer is in such a range, the interfacial reflection at the interface with the first diffusion film is increased, and thus a light diffusion device with higher uniformity of in-plane luminance can be realized. Note that "the second low refractive index layer has a refractive index lower than that of the first diffusion film" means that the refractive index of the second low refractive index layer is lower than the refractive index of the surface of the first diffusion film on the second low refractive index layer side, and therefore means that when the first diffusion film has a transparent substrate on the second low refractive index layer side of the diffusion layer, the refractive index is lower than that of the transparent substrate, and when the first diffusion film does not have a transparent substrate, the refractive index is lower than that of the polymer matrix. The same meaning applies to "the second low refractive index layer has a refractive index lower than that of the second diffusion film".
[0120] The difference between the refractive index of the second low refractive index layer and the refractive index of the first diffusion film 20 is, for example, 0.2 or more and 0.6 or less, preferably 0.3 or more and 0.6 or less. The difference between the refractive index of the second low refractive index layer and the refractive index of the second diffusion film 50 is, for example, 0.2 or more and 0.6 or less, preferably 0.3 or more and 0.6 or less. The refractive index of the polymer matrix is usually 1.49 to 1.60, for example, 1.49 to 1.55. The refractive index of the transparent substrate is usually 1.49 to 1.65, for example, 1.49 to 1.58.
[0121] The same explanation as for the first low refractive index layer 30 can be applied to the second low refractive index layer 40. The first low refractive index layer and the second low refractive index layer may have the same configuration or different configurations.
[0122] A-6.Reflective layer Any suitable configuration may be adopted as the reflective layer. For example, the reflective layer may be a specular reflective layer or a diffuse reflective layer. Specific examples of the reflective layer include a resin sheet (e.g., an acrylic plate) having a high reflectance mixed with a white pigment, a thin metal plate or metal foil such as aluminum or stainless steel, a vapor deposition sheet in which aluminum, silver, or the like is vapor-deposited on a substrate such as a resin film such as polyester, a laminate of a substrate such as a resin film such as polyester and a metal foil such as aluminum, and a resin film in which voids are formed inside.
[0123] A-7. Method for making a light diffusion device The light diffusing device can be obtained by stacking the above-mentioned members. A light diffusion device using an air layer as a low refractive index layer can be obtained, for example, by laminating a resin film on a light source layer with or without an adhesive layer; and laminating a diffusion film on the resin film without an adhesive layer. Alternatively, a light diffusion device using an air layer as a low refractive index layer can be obtained, for example, by distributing spacers on the light source layer; and laminating a diffusion film on the spacers. An adhesive may or may not be present between the spacer and the light source layer and / or the diffusion film. A light diffusion device using a low refractive index layer that is not an air layer can be obtained, for example, by laminating a low refractive index layer on a light source layer with or without an adhesive layer; and laminating a diffusion film on the low refractive index layer with or without an adhesive layer. The adhesive layer may be a pressure-sensitive adhesive layer, an adhesive layer, etc., and among these, an acrylic pressure-sensitive adhesive layer is preferably used. By fixing each member with an adhesive layer, problems such as deterioration due to friction between members, undulation of members, and generation of water marks can be prevented.
[0124] B. Backlight device The light diffusion device described in Section A can be used in a backlight device in an image display device. Therefore, a backlight device according to an embodiment of the present invention includes the light diffusion device described in Section A.
[0125] C. Image display device An image display device according to an embodiment of the present invention includes a backlight device and a display element described in Section B. In other words, an image display device according to an embodiment of the present invention includes a light diffusion device and a display element described in Section A. The display element is preferably a liquid crystal panel. In one embodiment, the image display device is a liquid crystal display device 200 including a light diffusion device 100 described in Section A and a liquid crystal panel 110 arranged on the viewing side thereof, as shown in FIG. 8. EXAMPLES
[0126] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring the various properties are as follows. In addition, unless otherwise specified, "parts" and "%" in the examples and comparative examples are based on weight.
[0127] (1) Thickness The measurement was performed using a digital micrometer (manufactured by Anritsu Corporation, product name "KC-351C"). (2) Volume average particle size of liquid crystal particles in liquid crystal emulsion The volume average particle diameter was calculated using a particle size distribution measuring device (Microtrac, "MT3300EXII"). (3) Average particle size of resin particles A few drops of the resin dispersion were added to 100 mL of water to prepare a measurement sample. Using a dynamic light scattering particle size distribution analyzer (Microtrac, device name "Nanotrac150"), the measurement sample was placed in the measurement holder of the device, and the device monitor was used to confirm that the concentration was measurable, after which the measurement was performed. (4) Hayes Measurements were carried out in accordance with JIS K 7136 using a Nippon Denshoku product called "NDH4000." (5) Refractive index of low refractive index layer After forming a low refractive index layer on the acrylic film, it was cut to a size of 50 mm x 50 mm and attached to the surface of a glass plate (thickness: 3 mm) via an adhesive layer. The center of the back surface of the glass plate (diameter: about 20 mm) was filled with black marker to make a sample that does not reflect on the back surface of the glass plate. The sample was set in an ellipsometer (JA Woollam Japan: VASE) and the refractive index was measured under the conditions of a wavelength of 500 nm and an incident angle of 50 to 80 degrees. (6) Refractive index of other materials The refractive indexes of the members other than the low refractive index layer were measured using a Metricon Prism Coupler Model 2010 / M.
[0128] [Production Example 1: Diffusion Film A] (Preparation of emulsion coating liquid) A liquid crystal emulsion was prepared by mixing 34.1 parts of a non-polymerizable liquid crystal compound (JNC, product name "JC-5240XX", birefringence Δn = 0.252 (ne = 1.766, no = 1.514), viscosity = 75 mPa·s), 3.8 parts of a polymerizable liquid crystal compound (BASF, product name "PALIOCOLOR LC-242"), 0.1 parts of a photopolymerization initiator (IGM, product name "OMNIRAD651"), 60.0 parts of pure water, and 2.0 parts of a dispersant (Dai-ichi Kogyo Seiyaku, "Noigen ET159"), and irradiating the mixture with ultrasonic waves at a frequency of 24 kHz for 1 minute using an ultrasonic homogenizer (Hielscher ultrasonics, UP-200S). The average particle size of the liquid crystal particles in the obtained liquid crystal emulsion was 0.8 μm. An emulsion coating liquid was obtained by mixing 19.03 parts of the above liquid crystal emulsion, 9.16 parts of a polyether-based polyurethane resin aqueous dispersion (manufactured by DSM, product name "NeoRez R967", average polymer particle size: 80 nm, solid content: 40 wt%), 8.12 parts of a polyester-based polyurethane resin aqueous dispersion (manufactured by Sanyo Chemical Industries, product name "Eucoat C-102", average polymer particle size: 168 nm, solid content: 45 wt%), 0.38 parts of a leveling agent (manufactured by DIC, product name "F-444"), 1.23 parts of a crosslinking agent (tris[3-(2-methylaziridin-1-yl)propionic acid]=propylidinetrimethyl), and 62.0 parts of pure water.
[0129] (Application and drying of emulsion coating liquid) The emulsion coating liquid was applied to one side of a PET film (thickness: 25 μm, refractive index: 1.49) as a first transparent substrate to form a coating layer having a thickness of 150 μm using a wire bar, and then the coating layer was dried at 25° C. for 90 minutes to form a PDLC layer having a thickness of 46 μm.
[0130] (Lamination of second transparent substrate) A PET film (thickness 25 μm, refractive index 1.49) was laminated as a second transparent substrate on the PDLC layer while applying a lamination pressure of 0.4 MPa / m using a laminator. This resulted in a laminate having a structure of [first transparent substrate / PDLC layer / second transparent substrate]. The obtained laminate showed a uniform haze (haze: 99%) over the entire main surface.
[0131] (UV irradiation) A flat metal electrode having a recess of 2 mm in depth on its upper surface was used as the first electrode. The recesses were arranged to correspond to the point light sources in the light source section described below. The laminate was placed so that the first transparent base material was in contact with the upper surface of the first electrode, and a glass substrate with ITO was placed on top of it as the second electrode so that the ITO surface was in contact with the second transparent base material. Next, a voltage of 1.3 kV was applied to these electrodes using a high-voltage power supply, while emitting 20 mW / cm under a UV-LED lamp (manufactured by Hamamatsu Photonics, product name "C11924-101", peak wavelength 365 nm). 2 The film was exposed to light at 25°C for 3 minutes. This caused the polymerizable liquid crystal compound to polymerize, and a diffusion film A having a structure of [first transparent substrate / diffusion layer / second transparent substrate] was obtained. The refractive index of the polymer matrix of the diffusion layer was 1.49 to 1.58.
[0132] The haze of the obtained diffusion film A was measured, and the haze in the region (region I) corresponding to the recesses of the first electrode was 99%, while the haze in the region (region II) corresponding to the other parts of the first electrode other than the recesses was 37%. This shows that the orientation state of the liquid crystal polymer and liquid crystal compound in the dispersed particles in region I of the diffusion layer is different from the orientation state of the liquid crystal polymer and liquid crystal compound in the dispersed particles in region II, and more specifically, the degree of orientation of the liquid crystal polymer and liquid crystal compound in the dispersed particles in region I is lower than the degree of orientation of these in region II.
[0133] [Production Example 2: Low Refractive Index Layer A] A low refractive index layer was formed on the surface of an acrylic film (manufactured by Toyo Kohan Co., Ltd., product name "RX-30NC", thickness: 30 μm) as follows. 0.95 g of methyltrimethoxysilane (MTMS), a precursor of a silicon compound, was dissolved in 2.2 g of dimethyl sulfoxide (DMSO) and 0.5 g of 0.01 mol / L oxalic acid solution was added to the mixture, which was stirred at room temperature for 30 minutes to hydrolyze MTMS and generate tris(hydroxy)methylsilane. After that, 0.38 g of 28% ammonia water and 0.2 g of pure water were added to 5.5 g of DMSO, and the hydrolyzed mixture was further added and stirred at room temperature for 15 minutes to gel tris(hydroxy)methylsilane and obtain a gel-like silicon compound. The mixture that had undergone the gelation treatment was incubated at 40° C. for 20 hours to perform aging treatment. Next, the gel-like silicon compound that had been aged was crushed into granules of a few mm to a few cm in size using a spatula. 40 g of isopropyl alcohol (IPA) was added thereto, and after light stirring, the mixture was left to stand at room temperature for 6 hours, and the solvent and catalyst in the gel were decanted. The same decantation process was repeated three times to complete the solvent replacement. Then, the gel-like silicon compound in the mixture was pulverized. The pulverization process was carried out using a homogenizer (product name "UH-50", manufactured by SMT Co., Ltd.) with a 5 cm 3 1.18g of gel and 1.14g of IPA were weighed into a screw bottle, and then crushed for 2 minutes under the conditions of 50W and 20kHz. The gel-like silicon compound in the mixed liquid was crushed by the crushing process, and as a result, the mixed liquid became a sol liquid of the crushed matter. The volume average particle diameter indicating the particle size variation of the crushed matter contained in the mixed liquid was confirmed to be 0.5μm to 0.7μm. Furthermore, a 0.3 wt% KOH aqueous solution was prepared, and 0.02g of KOH was added to 0.5g of the sol liquid to prepare a coating liquid. A silane coupling agent (manufactured by Shin-Etsu Silicone Co., Ltd., product name "KBM-403") was formed on the acrylic film surface to a thickness of 40nm, and the coating liquid was further formed thereon by spray coating, and dried at 80℃ for 1 minute to obtain a laminate A of an acrylic film and a low refractive index layer A. The film thickness and refractive index of the low refractive index layer A were evaluated to be 1000nm and 1.20, respectively.
[0134] [Example 1] A light source layer including a light source unit and a silicone resin layer sealing the light source unit was taken out from a liquid crystal display device (Apple Inc., "iPad Pro (registered trademark) 12.9 inch (5th generation)") and used as light source layer A. The light source unit was composed of mini-LEDs arranged two-dimensionally in 119 rows and 88 columns. The refractive index of the silicone resin layer was 1.43. A PET film (manufactured by Toray Industries, product name "Lumirror S10", thickness 25 μm) was laminated on top of the light source layer A without an adhesive layer, and then a diffusion film A was laminated on top of that without an adhesive layer to form an air layer between the PET film and the diffusion film A. This resulted in a light diffusion device having a configuration of [light source layer A / PET film / air layer / diffusion film A]. In the obtained light diffusion device, region I of the diffusion film corresponded to the arrangement positions of each LED in a planar view.
[0135] [Example 2] A diffusion film A was laminated on the low refractive index layer A side of the laminate A obtained in Production Example 2 via an acrylic adhesive (thickness 10 μm) to obtain a laminate B having a structure of [acrylic film / low refractive index layer A / adhesive layer / diffusion film A]. The laminate B was laminated on the same light source layer A as in Example 1 without an adhesive layer so that the acrylic film was on the light source layer A side. This resulted in a light diffusion device having a structure of [light source layer A / acrylic film / low refractive index layer A / adhesive layer / diffusion film A]. In the obtained light diffusion device, region I of the diffusion film corresponded to the arrangement positions of each LED in a planar view.
[0136] [Example 3] Resin particles with a uniform particle size (manufactured by Sekisui Chemical Co., Ltd., product name "Micropearl SP-220", particle size 20 μm) were placed on top of the light source layer A without using an adhesive, and the diffusion film A was further laminated on top of that without an adhesive layer. This formed a low refractive index layer (air layer) between the light source layer A and the diffusion film A. One layer of resin particles was randomly laminated on the light source layer A, and the area occupied by the resin particles on the light source layer A when observed from the perpendicular direction to the surface was 20%. This resulted in a light diffusion device with a configuration of [light source layer A / resin particles+air layer / diffusion film A]. In the obtained light diffusion device, area I of the diffusion film corresponded to the arrangement positions of each LED when viewed in a plan view.
[0137] [Comparative Example 1] The same light source layer A as in Example 1 was used as a light diffusing device.
[0138] [Comparative Example 2] A diffusion film A was laminated on the same light source layer A as in Example 1 without an adhesive layer. This resulted in a light diffusion device having a configuration of [light source layer A / diffusion film A]. The diffusion film A was in close contact with the light source layer A, and no air layer was formed at the interface between them. In the obtained light diffusion device, region I of the diffusion film corresponded to the arrangement positions of each LED in a plan view.
[0139] [Reference example 1] A diffusion film B (a surface-type diffusion film having a prism shape on its surface, thickness 132 μm) was laminated on the same light source layer A as in Example 1 without an adhesive layer, so that the surface having the prism shape faced the light source layer A. This resulted in a light diffusion device having a configuration of [light source layer A / diffusion film B].
[0140] [Reference example 2] A PET film (manufactured by Toray Industries, product name "Lumirror S10", thickness 25 μm) was laminated on the light source layer A similar to that in Example 1 without an adhesive layer. Next, a diffusion film B was laminated on the PET film without an adhesive layer so that the surface having the prism shape was on the light source layer A side. This resulted in a light diffusion device having a configuration of [light source layer A / PET film / diffusion film B].
[0141] The light diffusion devices obtained in the above Examples, Comparative Examples, and Reference Examples were turned on, and the uniformity of in-plane luminance was evaluated as follows. The results are shown in Table 1. <In-plane luminance uniformity> The luminance of the surface on the diffusion film side of the light diffusion device was measured with a 2D spectroradiometer (Topcon Technohouse, "SR-5000HS") with a resolution of 0.2 mm x 0.2 mm, and the maximum luminance (Lmax) and minimum luminance (Lmin) were substituted into the following formula to calculate the in-plane luminance uniformity. In-plane luminance uniformity (%) = [1-(Lmax-Lmin) / (Lmax+Lmin)] x 100 [Table 1]
[0142] A comparison between the Examples and Comparative Examples shows that the uniformity of in-plane luminance is greatly improved by disposing a low refractive index layer having a lower refractive index than the light source layer between the light source layer and the diffusion film. On the other hand, such an effect is not obtained in the Reference Example. This is thought to be because, in the surface-type diffusion film, the adhesion between the diffusion film and the light source layer is low, and sufficient interfacial reflection occurs even in the absence of a low refractive index layer. [Industrial Applicability]
[0143] The light diffusing device of the present invention is suitably used in display devices such as liquid crystal display devices. [Explanation of symbols]
[0144] 10 Light source layer 12 Light source section 14 Sealing resin layer 20 First diffusion film 22 Diffusion Layer 22a Polymer matrix 22b Dispersed particles 30 First low refractive index layer 40 Second low refractive index layer 50 Secondary diffusion film 100 Light Diffuser 200 LCD display device
Claims
1. a light source layer including a light source unit and a sealing resin layer sealing the light source unit, a first low refractive index layer having a refractive index lower than that of the sealing resin layer, and a first diffusion film including a diffusion layer, in this order; The diffusion layer includes a polymer matrix and dispersed particles dispersed in the polymer matrix, the dispersed particles including at least one selected from a liquid crystal compound and a liquid crystal polymer. Light diffuser.
2. The light diffusing device of claim 1 , wherein the refractive index of the first low refractive index layer is lower than the refractive index of the first diffusion film.
3. The light diffusing device according to claim 1 , wherein the first low refractive index layer is a layer including voids or an air layer.
4. The light diffusing device according to claim 1 , wherein the sealing resin layer contains at least one resin selected from a silicone resin and an epoxy resin.
5. The light diffusing device of claim 1 , wherein the first diffusion film further comprises a transparent substrate disposed on at least one side of the diffusion layer.
6. The light diffusing device according to claim 1 , wherein the light source section includes a plurality of point light sources.
7. The light diffusing device of claim 1 , wherein the dispersed particles include at least the liquid crystal polymer.
8. The light diffusing device according to claim 7 , wherein the first diffusion film has a plurality of regions having different hazes in a plan view.
9. The light diffusing device of claim 7 , wherein the plurality of regions are arranged in a predetermined pattern.
10. a second low refractive index layer and a second diffusion film are disposed in this order on a side of the first diffusion film opposite to a side on which the first low refractive index layer is disposed, the second diffusion film includes a diffusion layer including a polymer matrix and dispersed particles that are dispersed in the polymer matrix and include at least one selected from a liquid crystal compound and a liquid crystal polymer; The light diffusing device of claim 1 , wherein the second low refractive index layer has a refractive index lower than the first diffusion film and the second diffusion film.
11. A backlight device comprising the light diffusing device according to any one of claims 1 to 10.
12. An image display device comprising the backlight device according to claim 11 and a display element.