Cement compositions, method for manufacturing cement composition, mortar composition, and concrete composition

A cement composition with controlled limestone content, Blaine specific surface area, and gypsum hemihydration rate addresses the strength and heat issues in mortar and concrete, enhancing performance and environmental sustainability.

JP2024145508APending Publication Date: 2024-10-15MITSUBISHI UBE CEMENT CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023057892
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The incorporation of limestone beyond 5% by mass in cement compositions leads to a decrease in compressive strength of cured mortar and concrete compositions, and increased heat of hydration, which is undesirable for environmental and performance reasons.

Method used

A cement composition comprising cement clinker, gypsum, and limestone, with specific ranges for limestone content, Blaine specific surface area, particle size distribution, and chemical composition, including controlled hemihydration rate of gypsum, to maintain strength and reduce hydration heat.

Benefits of technology

The solution enhances the compressive strength of cured mortar and concrete products while keeping hydration heat low, thereby improving performance and reducing environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145508000001
    Figure 2024145508000001
  • Figure 2024145508000002
    Figure 2024145508000002
  • Figure 2024145508000003
    Figure 2024145508000003
Patent Text Reader

Abstract

To provide a cement composition that contains more than 5 mass% of limestone, capable of improving compressive strength of hardened bodies of not only a concrete composition but also a mortar composition, and exhibiting sufficiently low heat of hydration.SOLUTION: A cement composition includes a cement clinker, gypsum, and limestone. The limestone content is more than 5 mass% and 15 mass% or less. The cement composition has a Blaine specific surface area of 3,500 cm2 / g or more and 4,000 cm2 / g or less. In a particle size distribution of the cement composition, Rc calculated by the formula Rc=R35.1 / (R10.9-R35.1) is 0.27 or more and 0.40 or less. The content of SO3 in the cement clinker is 0.3 mass% or more and 1.5 mass% or less. The degree of semi-hydration of gypsum is 25 mass% or more and 90 mass% or less. The apparent viscosity of the mortar composition containing the cement composition at a shear rate of 1 s-1 is 1 Pa_s or more and 8 Pa_s or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a cement composition, a method for producing a cement composition, a mortar composition, and a concrete composition. [Background technology]

[0002] A part of the cement clinker that constitutes the cement composition such as ordinary Portland cement may be replaced by an admixture, and limestone is widely used as an admixture. The content of admixtures added to ordinary Portland cement is set at 5% by mass or less according to the JIS standard.

[0003] However, since the production of cement clinker involves a relatively large amount of CO2 emissions, it is desirable to replace a larger proportion of cement clinker with admixtures from the perspective of preventing global warming and reducing carbon emissions. For example, Non-Patent Document 1 discusses a cement composition containing an admixture content exceeding 5 mass% as specified by the JIS standard. [Prior art documents] [Non-patent literature]

[0004] [Non-Patent Document 1] Ayuka Nakaguchi et al., "Quality evaluation of cement with increased amounts of minor mixed components", Abstracts of the Cement Technology Conference, 2018, pp.270-271 Summary of the Invention [Problem to be solved by the invention]

[0005] However, when the content of limestone as an admixture exceeds 5% by mass, the compressive strength of the hardened body of the mortar composition or concrete composition tends to decrease. Even if the Blaine specific surface area of ​​the cement composition is increased, there is a problem that the compressive strength of the hardened body of the concrete composition, especially the hardened body of the mortar composition, tends to decrease with age when the content of limestone is large. In addition, it is also desired that the heat of hydration associated with mixing the cement composition with water is low.

[0006] The present disclosure relates to a cement composition that can improve the compressive strength of a hardened body of not only a concrete composition but also a mortar composition while containing limestone in a content of more than 5 mass %, and that exhibits a sufficiently low heat of hydration. [Means for solving the problem]

[0007] The present disclosure includes the following. [1] A cement composition comprising cement clinker, gypsum, and limestone, Based on the mass of the cement composition, the content of the limestone is more than 5 mass% and 15 mass% or less, and the total content of the cement clinker and the gypsum is 85 mass% or more and less than 95 mass%, The cement composition has a viscosity of 3500 cm 2 / g or more 4000cm 2 / g or less, In the particle size distribution of the cement composition by the laser diffraction / scattering method, the ratio of particles with a particle size of 10.9 μm or more is R 10.9 [%], the percentage of grains with a particle size of 35.1 μm or more is R 35.1 When [%], Formula: Rc=R 35.1 / (R 10.9 -R 35.1 ) Rc calculated by is 0.27 or more and 0.40 or less, In the cement clinker, the SO3 content is 0.3 mass% or more and 1.5 mass% or less based on the mass of the cement clinker, the C3S content is 50 mass% or more and 64 mass% or less, and the C3A content is 9.0 mass% or more and 12 mass% or less, and the C3S content and the C3A content are values ​​calculated by the Bogue formula, Formula: Hemihydration rate = 100 × mass of gypsum hemihydrate / (mass of gypsum hemihydrate + mass of gypsum dihydrate) wherein the mass of gypsum hemihydrate and the mass of gypsum dihydrate in the formula are masses converted into SO3; the hemihydration rate of the gypsum is 25% by mass or more and 90% by mass or less; The mortar composition containing only the cement composition, water and silica sand is subjected to a temperature of 20°C and a shear rate of 1 s -1 The apparent viscosity at is 1 Pa s or more and 8 Pa s or less, The apparent viscosity is a value obtained by forming a mortar composition by kneading a mixture containing only 100 g of the cement composition, 50 g of water, and 100 g of silica sand with a chemical mixer at a rotation speed of 500 rpm for 3 minutes, and measuring the apparent viscosity of the mortar composition 5 minutes after the start of kneading with a double cylinder rheometer. Cement compositions. [2] The cement composition has a viscosity of 3800 cm 2 / g and above 4000 cm 2 The cement composition according to [1], which is a powder having a Blaine specific surface area of ​​0.1 to 1.0 μm / g or less. [3] The cement composition according to [1] or [2], wherein the hemihydration rate of the gypsum is 40% by mass or more and 90% by mass or less. [4] In the particle size distribution of the cement composition, the ratio of the particle size of 2.0 μm or more is R 2.0 When Formula: Rf = R 2.0 -R 10.9 The cement composition according to any one of [1] to [3], wherein Rf calculated by the above formula is 30.0% or more and 35.7% or less. [5] A method for producing a cement composition according to any one of [1] to [4], The method includes forming the cement composition by mixing cement clinker, gypsum, and limestone. [6] A mortar composition comprising the cement composition according to any one of [1] to [4], a fine aggregate, and water. [7] The density of the mortar hardened body formed from the mortar composition without the addition of any admixtures at 24 hours in accordance with JIS R 5201:2015 "Physical Test Methods for Cement" is 2.230g / cm 3 More than 2.280g / cm 3 The mortar composition according to [6], [8] A concrete composition comprising the cement composition according to any one of [1] to [4], fine aggregate, coarse aggregate, and water. Effect of the Invention

[0008] A cement composition can be provided which contains more than 5 mass % limestone and yet can improve the compressive strength of hardened concrete compositions as well as mortar compositions and exhibit a sufficiently low heat of hydration. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The following embodiments are examples for explaining the present disclosure, and are not intended to limit the present disclosure to the following examples.

[0010] Unless otherwise specified, the materials exemplified in this specification can be used alone or in combination of two or more. When a plurality of substances corresponding to each component are present in the composition, the content of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified.

[0011] An example of a cement composition according to the present disclosure includes cement clinker, gypsum, and limestone. Based on the mass of the cement composition, the content of limestone is more than 5 mass% and not more than 15 mass%, and the total content of cement clinker and gypsum is 85 mass% or more and less than 95 mass%. A cement composition containing more than 5 mass% limestone is beneficial from the viewpoint of reducing environmental load.

[0012] The cement composition is 3500 cm 2 / g or more 4000cm 2 / g or less. The Blaine specific surface area of ​​the cement composition is 3550 cm 2 / g or more, 3600cm 2 / g or more, 3650cm 2 / g or more, 3700cm 2 / g or more, 3750cm 2 / g or more, or 3800 cm 2 / g or more, and 2 / g. The Blaine specific surface area of ​​the cement composition is measured in accordance with JIS R 5201:2015 "Physical Testing Methods for Cement". When the Blaine specific surface area is large, the compressive strength of the hardened body of the mortar composition or concrete composition tends to be improved. When the Blaine specific surface area of ​​the cement composition is 3950 cm 2 / g or less, or 3900cm 2 / g or less.

[0013] The density of the cement composition is preferably 3.04 to 3.14, more preferably 3.06 to 3.13, further preferably 3.08 to 3.12, and particularly preferably 3.10 to 3.11. The density of the cement composition is measured in accordance with JIS R 5201:2015 "Physical testing methods for cement".

[0014] In the particle size distribution of the cement composition measured by the laser diffraction and scattering method, the ratio of particles with a particle size of 10.9 μm or more is R 10.9 [%], the percentage of grains with a particle size of 35.1 μm or more is R 35.1 When [%], Formula: Rc=R 35.1 / (R 10.9 -R 35.1 ) Rc calculated by is 0.27 or more and 0.40 or less. Rc corresponds to the ratio of the part with a particle size of 35.1 μm or more to the part with a particle size of 10.9 μm or more in the particle size distribution. When Rc is 0.27 or more and 0.40 or less, the hydration heat generated when the cement composition is mixed with water tends to be small and good strength is obtained. From the same viewpoint, Rc may be 0.28 or more, 0.29 or more, 0.29 or more, 0.30 or more, 0.31 or more, 0.32 or more, 0.33 or more, 0.34 or more, or 0.35 or more. R 10.9 may be, for example, 54.5 or more and 60.0 or less.

[0015] In the particle size distribution of the cement composition measured by the laser diffraction and scattering method, the ratio of particles with a particle size of 2.0 μm or more is R 2.0 When Formula: Rf = R 2.0 -R 10.9 Rf calculated by may be 30.0% or more and 35.7% or less. Rf may be 31.0% or more, 35.0% or less, 34.5% or less, or 34.0% or less. Rf being within these ranges is also advantageous in terms of reducing heat of hydration.

[0016] The particle size distribution of a cement composition is a value calculated based on, for example, the Rosin-Rammler equation, and can also be determined by the n value, which indicates the uniformity of particle size. The Rosin-Rammler equation is an equation that represents the cumulative distribution of a cement composition on a sieve, and is expressed by the following equation. Formula: R(x)=exp(-bx) n In the above formula, b and n are constants. x is the representative particle diameter D of the precipitated calcium carbonate. 50The larger the n value calculated based on the formula, the narrower the particle size distribution and the more uniform the particle size. Although the Rosin-Rammler formula is usually considered to be a formula based on mass, in this specification, for the purpose of comparing particles of the same quality, the Rosin-Rammler formula is also considered to be valid on a volume basis, and the particle diameters D 50 The n value is calculated using the integrated volumetric value for

[0017] The n value of the Rosin-Rammler equation in the particle size distribution of the cement composition is preferably 0.90 or more, more preferably 0.95 or more, and even more preferably 1.00 or more. An n value of 2.2 or more is preferable because it reduces the amount of fine particles in the cement composition, thereby improving the fluidity of the cement composition.

[0018] The n value of the Rosin-Rammler equation in the particle size distribution of the precipitated calcium carbonate is preferably 1.12 or less, more preferably 1.06 or less, even more preferably 1.06 or less, particularly preferably 1.04 or less, and most preferably 1.02 or less. The n value of 1.12 or less is preferable from the viewpoint of the heat of hydration of the cement composition.

[0019] The particle size distribution of the cement composition can be adjusted to within the above range by subjecting the cement composition to pulverization, classification, sieving, etc., without departing from the spirit of the present disclosure. Alternatively, the particle size distribution of the cement composition may be adjusted by mixing a plurality of types of cement compositions having different particle size distributions. Alternatively, the cement composition may be obtained by the manufacturing method described below.

[0020] The cement clinker may be, for example, normal Portland cement clinker, high-early-strength Portland cement clinker, moderate-heat Portland cement clinker, low-heat Portland cement clinker, oil well cement clinker, or a combination thereof. From the viewpoint of availability and improving the strength at an early age, the cement clinker may include at least one of normal Portland cement clinker and high-early-strength Portland cement clinker, or may include normal Portland cement.

[0021] Cement clinker usually contains C3S (tricalcium silicate, 3CaO·SiO2), C2S (dicalcium silicate (2CaO·SiO2), C3A (tricalcium aluminate, 3CaO·Al2O3), and C4AF (tetracalcium aluminate ferroferrate, 4CaO·Al2O3·Fe2O3). The amounts of C3S, C2S, C3A, and C4AF can be calculated using the following Bogue formula. Bogue style: C3S amount [mass %] = (4.07 × CaO content [mass %]) - (7.60 × SiO2 content [mass %]) - (6.72 × Al2O3 content [mass %]) - (1.43 × Fe2O3 content [mass %]) - (2.85 × SO3 content [mass %]) C2S amount [mass %] = (2.87 x SiO2 content [mass %]) - (0.754 x C3S amount [mass %]) C3A amount [mass%] = (2.65 x Al2O3 content [mass%]) - (1.69 x Fe2O3 content [mass%]) C4AF amount [mass%] = 3.04×Fe2O3 content [mass%]

[0022] The Bogue formula is a widely used formula for calculating the content of major minerals in cement clinker from the content of each compound, CaO, SiO2, Al2O3, Fe2O3, and SO3. The content of each compound used in the Bogue formula calculation is obtained from chemical analysis values ​​according to JIS R 5204:2019 "Method for X-ray fluorescence analysis of cement".

[0023] In one example of cement clinker, the C3S content is 50% by mass or more and 64% by mass or less. The C3S content may be 51.0% by mass or more, 52.0% by mass or more, 53.0% by mass or more, or 54.0% by mass or more, and may be 63.0% by mass or less, 62.0% by mass or less, 61.0% by mass or less, 60.0% by mass or less, or 59.0% by mass or less. When the C3S content is large, the early strength of the hardened body of the concrete composition or mortar composition tends to be improved. When the C3S content is small, the heat generation accompanying the hardening of the concrete composition or mortar composition tends to be suppressed.

[0024] In one example of cement clinker, the C3A content is 9.0% by mass or more and 12% by mass or less. The C3A content may be 10.4% by mass or less, or 9.6% by mass or less. If the C3A content is large, the amount of waste and by-products such as coal ash used as raw materials for cement clinker can be increased. If the C3A content is small, the regeneration of ettringite (a compound represented by 3CaO·Al2O3·3CaSO4·32H2O) tends to be suppressed. In addition, if the C3A content is small, the adiabatic temperature of the hardened body of the concrete composition or mortar composition tends to be difficult to increase.

[0025] In one example of cement clinker, the C2S content may be 5.0% by mass or more and 65.0% by mass or less. The C2S content may be 10.0% by mass or more or 15.0% by mass or more, and may be 50.0% by mass or less, 40.0% by mass or less, 30.0% by mass or less, or 25.0% by mass or less. When the C2S content is large, the strength of the hardened body of the concrete composition or mortar composition after a long period of time tends to be improved. When the C2S content is small, the initial strength of the hardened body of the concrete composition or mortar composition tends to be improved.

[0026] In one example of cement clinker, the C4AF amount may be 7.0% by mass or more, 8.0% by mass or more, 9.0% by mass or more, 9.5% by mass or more, or 9.8% by mass or more. A large C4AF amount can increase the amount of waste and by-products such as coal ash used as raw materials for cement clinker. The C4AF amount may be 14.0% by mass or less, 12.0% by mass or less, 11.0% by mass or less, 10.5% by mass, or 10.0% by mass or less. A small C4AF amount tends to suppress heat generation associated with hardening of the concrete composition or mortar composition.

[0027] The content of SO3 in one example of cement clinker is 0.3 mass% or more and 1.5 mass% or less based on the mass of the cement clinker. When the content of SO3 is within this range, the heat of hydration generated when the cement composition is mixed with water tends to be small. From the same viewpoint, the content of SO3 may be 0.4 mass% or more, or 0.5 mass% or more, and may be 1.4 mass% or less, 1.3 mass% or less, 1.2 mass% or less, 1.1 mass% or less, 1.0 mass% or less, 0.9 mass% or less, 0.8 mass% or less, 0.7 mass% or less, or 0.6 mass% or less.

[0028] In one example of the cement composition, the hemihydration rate of the gypsum is 25% by mass or more and 90% by mass or less. Formula: Hemihydration rate = 100 × mass of gypsum hemihydrate / (mass of gypsum hemihydrate + mass of gypsum dihydrate) The value calculated by the formula is as follows. The mass of gypsum hemihydrate and the mass of gypsum dihydrate in the formula are masses converted into SO3. When the hemihydration rate is within the above range, the viscosity of the mortar composition decreases, which can contribute to improving the compressive strength of the hardened body of the mortar composition. From the same viewpoint, the hemihydration rate of gypsum may be 30% by mass or more, 32% by mass or more, 34% by mass or more, 36% by mass or more, 38% by mass or more, 40% by mass or more, 42% by mass or more, 44% by mass or more, 46% by mass or more, 48% by mass or more, 50% by mass or more, 52% by mass or more, 54% by mass or more, 56% by mass or more, 58% by mass or more, 60% by mass or more, 62% by mass or more, 64% by mass or more, 66% by mass or more, 68% by mass or more, or 70% by mass or more, and may be 88% by mass or less, 86% by mass or less, 84% by mass or less, 82% by mass or less, 80% by mass or less, or 78% by mass or less.

[0029] The hemihydration rate of gypsum is determined by measuring the weight change when a cement composition placed in a measuring pan with holes is heated at a heating rate of 5°C / min by simultaneous differential thermal analysis and thermogravimetry (TG-DTA) in the range of about 120°C to about 220°C in a nitrogen gas flow environment. In the differential thermogravimetry (DTG) curve obtained by this measurement, two peaks, a first peak and a second peak, are observed, and the hemihydration rate can be calculated by the following formula. The first peak is the peak on the low temperature side in the DTG curve, and the second peak is the peak on the high temperature side in the DTG curve. Hemihydration rate (%) = (weight loss at second peak) x 172.2 / 9.0 - (weight loss at first peak) x 172.2 / (1.5 x 18.0) x 145.1 / 172.2

[0030] The hemihydration rate of gypsum can be adjusted within the range of 25% by mass or more and 90% by mass or less based on the hemihydration rate of the gypsum used as a raw material, as well as by adjusting the temperature inside the mill in the production process of the cement composition, mixing cements with different hemihydration rates, etc.

[0031] The limestone is a powder mainly composed of calcium carbonate, and may be, for example, limestone powder or kansui stone powder. The limestone may be one that conforms to the minor mixing components described in JIS R 5210:2019 "Portland Cement". The Blaine specific surface area of ​​the cement composition can also be adjusted by combining limestones with different particle size distributions.

[0032] In one example of the cement composition, the limestone content is greater than 5% by mass and not more than 15% by mass, based on the mass of the cement composition. The limestone content may be 6% by mass or more, 7% by mass or more, 8% by mass or more, or 9% by mass or more, and may be 14% by mass or less, 13% by mass or less, 12% by mass or less, 11% by mass or less, or 10% by mass or less.

[0033] In one example of the cement composition, the total content of cement clinker and gypsum is 85 mass% or more and less than 95 mass% based on the mass of the cement composition. The total content of cement clinker and gypsum may be 86 mass% or more, 87 mass% or more, 88 mass% or more, 89 mass% or more, or 90 mass% or more, or 94 mass% or less, 93 mass% or less, 92 mass% or less, or 91 mass% or less. Here, the gypsum content is the amount converted into SO3.

[0034] The gypsum content in terms of SO3 in one example of the cement composition may be, for example, 0.5% by mass or more and 3.5% by mass or less based on the mass of the cement composition. The gypsum content in terms of SO3 may be 0.7% by mass or more or 1.0% by mass or more based on the mass of the cement composition, and may be 3.0% by mass or less, 2.0% by mass or less, or 1.5% by mass or less.

[0035] The cement clinker content in one example of the cement composition may be, for example, 70% by mass or more and 95% by mass or less, based on the mass of the cement composition. The cement clinker content may be 75% by mass or more or 85% by mass or more, and 93% by mass or less or 90% by mass or less, based on the mass of the cement composition.

[0036] The mortar composition formed from the cement composition can have a moderately low viscosity. Specifically, a mortar composition containing only the cement composition, water, and silica sand is mixed at a temperature of 20° C. and a shear rate of 1 s -1 The apparent viscosity of the mortar composition may be 1 Pa·s or more and 8 Pa·s or less at a shear rate of 1 s. The low viscosity of the mortar composition can contribute to improving the compressive strength of the hardened body of the mortar composition. -1 may be 2 Pa·s or more, 3 Pa·s or more, 4 Pa·s or more, or 5 Pa·s or more.

[0037] The apparent viscosity of a mortar composition is a value obtained by forming a mortar composition by kneading a mixture containing only 100 g of cement composition, 50 g of water, and 100 g of silica sand with a chemical mixer at a rotation speed of 500 rpm for 3 minutes, and measuring the apparent viscosity of the mortar composition 5 minutes after the start of mixing using a double cylinder rheometer. In the mortar composition for measuring the apparent viscosity, the water-cement ratio (W / C) is 0.50 and the sand-cement ratio is 1.0. The water-cement ratio is the mass ratio of the water content to the cement clinker content in the mortar composition. The sand-cement ratio is the mass ratio of the silica sand content to the cement clinker content in the mortar composition. The silica sand contained in the mortar composition for measuring the apparent viscosity can be silica sand (e.g., Toyoura silica sand) having a particle size distribution in which the proportion of the portion having a particle size that passes through a sieve with a mesh size of 0.3 mm but not through a sieve with a mesh size of 0.15 mm is 95% by mass or more, and the proportion of the portion having a particle size that passes through a sieve with a mesh size of 0.063 mm or less is 1% by mass.

[0038] In addition to cement clinker, gypsum, and limestone, the cement composition may further contain other components within the scope of the present disclosure. Examples of other components include allophane, calcium hydroxide, silica powder, powder containing calcium (excluding gypsum and limestone), water reducer for concrete, accelerator, and retarder.

[0039] The above-exemplified cement compositions can be produced by a method including mixing cement clinker, gypsum, and limestone to form a cement composition. The method for producing the cement composition may include adjusting the temperature during grinding and mixing of the mixture including cement clinker, gypsum, and limestone so that the hemihydration rate of the gypsum is 25% by mass or more and 90% by mass or less.

[0040] The cement composition can be used to prepare a mortar composition or a concrete composition. The mortar composition includes the cement composition, a fine aggregate, and water. The concrete composition includes the cement composition, a fine aggregate, a coarse aggregate, and water.

[0041] The fine aggregate may be a fine aggregate as defined in JIS A 5005:2020 "Crushed stone and crushed sand for concrete". The fine aggregate may include, for example, river sand, land sand, mountain sand, sea sand, crushed sand, silica sand, limestone aggregate, blast furnace slag fine aggregate, copper slag fine aggregate, electric furnace oxidized slag fine aggregate, or a combination thereof. The mass ratio (sand-cement ratio) of the content of the fine aggregate to the content of the cement composition in the mortar composition may be, for example, 0.5 to 10.0, preferably 0.8 to 5.0, and more preferably 1.0 to 3.0. The content of the fine aggregate to the content of the cement composition in the concrete composition is, for example, 200 kg / m based on the volume of the concrete composition. 3 More than 1500kg / m 3 It may be the following.

[0042] Coarse aggregate is specified in JIS A 5005:2020 "Crushed stone and crushed sand for concrete" The coarse aggregate may be, for example, gravel, crushed stone, limestone aggregate, blast furnace slag coarse aggregate, electric furnace oxidizing slag coarse aggregate, or a combination thereof. The content of the coarse aggregate in the concrete composition is, for example, 200 kg / m based on the volume of the concrete composition. 3 More than 1500kg / m 3 It may be the following.

[0043] The water constituting the mortar composition or concrete composition may be, for example, tap water, distilled water, or deionized water. The mass ratio of the water content to the cement composition content (water-cement ratio) is preferably 0.10 to 5.00, more preferably 0.20 to 3.00, even more preferably 0.30 to 1.00, and particularly preferably 0.40 to 0.60.

[0044] The mortar composition containing the cement composition according to the present disclosure has a density of 2.230 g / cm3 of a hardened mortar body containing no admixtures at 24 hours of age, which is formed in accordance with JIS R 5201:2015 "Physical Testing Methods for Cement". 3 More than 2.280g / cm 3 It may form a hardened body which is: Mortar compositions having high density tend to exhibit high compressive strength. EXAMPLES

[0045] The present invention is not limited to the following examples.

[0046] 1. Raw materials for cement composition Cement clinker Cement clinkers A to F were prepared having the mineral composition and SO3 content according to the Bogue formula shown in Table 1. The chemical composition of the cement clinker, including the SO3 content, used in the calculations according to the Bogue formula was measured in accordance with the method described in JIS R 5204 "Fluorescent X-ray analysis method for cement."

[0047] [Table 1]

[0048] plaster Gypsum satisfying the requirements described in JIS R 9151:2009 "Natural gypsum for cement" was prepared.

[0049] limestone Limestone with a calcium carbonate content of 90% by mass or more and an aluminum oxide content of 1.0% by mass or less, which meets the requirements for minor mixed components described in JIS R 5210:2019 "Portland cement", and its crushed material (Ube Material Industries: limestone fine powder 325 mesh product, Blaine specific surface area value: 7470 cm 2 / g) was prepared.

[0050] 2. Cement composition Preparation of cement compositions A cement composition containing cement clinker, gypsum and limestone in the mixing ratio shown in Table 2 was prepared. The SO3 content shown in the table corresponds to the total ratio of the SO3 content of the cement clinker and the SO3 content of the gypsum. The cement composition containing uncrushed limestone and its crushed product was produced by mixing the cement clinker and uncrushed limestone while crushing them with a ball mill, and then mixing the crushed mixture with the crushed limestone with a mixer. The cement composition not containing the crushed limestone was produced by mixing the cement clinker and uncrushed limestone while crushing them with a ball mill. The cement composition of Example 1 was produced by mixing the cement composition of Comparative Example 1, which was heated at 110 ° C., with the cement composition of Comparative Example 1.

[0051] The Blaine specific surface area values ​​of the cement compositions of Examples 1 to 3 and Comparative Examples 1 and 2 were 3800±50 cm 2 , mainly based on the ratio of uncrushed limestone to crushed limestone. 2 The Blaine specific surface area was measured in accordance with the description of JIS R 5201:2015 "Physical measurement method of cement". The cement composition of Reference Example 1 is a cement that conforms to JIS R 5210:2019 ordinary Portland cement.

[0052] Limestone Content The limestone content in the cement composition was calculated by assuming that the carbon content measured using a carbon-sulfur analyzer (manufacturer: LECO Japan, LLC, device name: Carbon-Sulfur Analyzer CS744) was entirely derived from limestone (CaCO3) and calculated using the following formula. Limestone content (mass%) = carbon content x 100.1 / 12.0

[0053] Half-hydration rate A sample of the cement composition was placed in a measuring pan with holes, and the weight change due to heating at a heating rate of 5°C / min was measured by simultaneous differential thermal analysis and thermogravimetry (TG-DTA) under a nitrogen gas flow environment. Based on the weight loss at the first and second peaks confirmed in the DTG curve in the range of about 120°C to about 220°C, the hemihydration rate of gypsum was calculated using the following formula. Hemihydration rate (%) = (weight loss at second peak) x 172.2 / 9.0 - (weight loss at first peak) x 172.2 / (1.5 x 18.0) x 145.1 / 172.2

[0054] Particle size distribution The particle size distribution of the cement composition was measured by the laser diffraction / scattering method. In the obtained particle size distribution, the percentage of the part with a particle size of 35.1 μm or more (%, R 35.1 ), the percentage of particles with a particle size of 10.0 μm or more (%, R 10.9 ), and the percentage of particles with a particle size of 2.0 μ or more (%, R 2.0 ) was obtained. Rc and Rf were calculated using the following formula. The n value of the Rosin-Rammler formula (RR) was calculated within the particle size distribution range of 1.0 to 49.1 μm. Rc=R 35.1 / (R 10.9 -R 35.1 ) Rf=R 2.0 -R 10.9

[0055] [Table 2]

[0056] 3. Mortar composition Apparent viscosity of mortar composition Silica sand (Toyoura Silica Sand (trade name), Toyoura Silica Industry Co., Ltd.) having the particle size distribution shown in Table 3 was prepared. 100 g of each produced cement composition and 100 g of silica sand were added to 50 g of water in that order, and mixed for 3 minutes at a rotation speed of 500 rpm using a small mixer (manufacturer: Shindo Scientific Co., Ltd., model number: HEIDON Three-One Motor BL600) to form a mortar composition. In the mortar composition, the mass ratio of water to the cement composition (W / C) was 0.50, and the mass ratio of silica sand to the cement composition was 1.00. The formed mortar composition was left to stand for 5 minutes after the start of mixing. The apparent viscosity was measured using a sample taken from the mortar composition at that time. The apparent viscosity was measured using a coaxial double cylinder rheometer (manufactured by Anton Paar, product name: MCR101, fixture: CC27 / T200 / SS and CC27 / P6) in a constant temperature room at 20°C, with a shear rate of 10 -5 From 10 3 s -1 The measurements were performed under conditions that were gradually changed from -5 From 10 3 s -1 The apparent viscosity was measured by applying shear to the sample for 5 seconds at 36 shear rates, which equally divide the range of shear rate change from 10 to 180 on a logarithmic axis. The increase in shear rate and the viscosity measurement were repeated for a total of 180 seconds. -5 From 10 3 s -1 The shear rate was then gradually decreased to 1 s. The apparent viscosity was then measured at 36 shear rates to obtain a viscosity curve showing the relationship between the apparent viscosity and the shear rate. -1 The apparent viscosity was determined when a shear force of 1000 Hz was applied for 5 seconds.

[0057] [Table 3]

[0058] density The mortar composition was introduced into a 40 x 40 x 160 mm formwork in accordance with JIS R 5201:2015 "Physical Testing Methods for Cement," and after 24 hours, the formwork was removed to obtain a hardened mortar composition. The density of the hardened body at 24 hours was calculated from the weight and volume of the hardened body obtained.

[0059] Compressive strength The compressive strength of the hardened bodies aged 7 or 28 days was measured using 40 x 40 x 160 mm mortar specimens in accordance with the method described in JIS R 5201:2015 "Physical Testing Methods for Cement". Specifically, the mass ratio of water to cement composition (W / C) was 0.50, the mass of standard sand (JIS R5201 standard sand for strength testing) to the cement composition was 3.00, and the mortar composition for forming the mortar specimens was prepared by kneading these without adding any admixtures.

[0060] 4. Concrete composition Fine aggregate, coarse aggregate, and admixtures shown in Table 4 were prepared. Water (tap water), fine aggregate, coarse aggregate, and admixtures were mixed in the proportions shown in Table 5 to prepare concrete compositions of Reference Examples 1 and 2. In the concrete compositions, the mass ratio of water to cement composition (W / C) was 0.55, the air content was 4.5±0.5%, and the amount of AE water-reducing agent and AE agent was adjusted so that the slump value was 18 cm±1 cm. In the cement compositions of the Examples and Comparative Examples, the unit water content and W / C were constant in the proportions in Table 5, the amount of cement composition was determined according to the change in cement density, and the amount of the fine aggregate was used to adjust the variation.

[0061] In a thermostatic room at 20°C, the coarse aggregate, fine aggregate, and cement were added to a forced mixing horizontal twin-shaft mixer (volume 55 L) in that order, and the mixture was dry mixed for 30 seconds. After that, water containing admixtures was added, and the mixture was mixed for 90 seconds, and the formed concrete composition was discharged from the mixer. The compressive strength of the concrete specimens aged 7 days and 28 days was measured in accordance with JIS A 1108:2018 "Test method for compressive strength of concrete".

[0062] [Table 4]

[0063] [Table 5]

[0064] 5. Heat of hydration The heat of hydration was measured at ages of 7 and 28 days in accordance with JIS R 5203:2015 "Method for measuring heat of hydration of cement."

[0065] [Table 6]

[0066] The evaluation results are shown in Table 6. The limestone content in the cement compositions of Examples 1 to 4 and Comparative Example 1 is 9 mass%, and the Blaine specific surface area of ​​these cement compositions is also approximately the same. Despite this, the compressive strength at 28 days of the mortar composition containing the cement composition of each Example was up to 4 N / mm 2 Even when compared with Reference Example 1, which corresponds to the current ordinary Portland cement, Examples 1 to 3 exhibited compressive strengths equal to or greater than those at an age of 28 days.

[0067] On the other hand, in the case of the concrete composition, the hardened bodies (concrete specimens) obtained from the cement compositions of the Examples and Comparative Examples all exhibited compressive strengths approximately equal to that of the Reference Example.

[0068] The mortar compositions containing the cement compositions of Examples 1 to 4 exhibited lower apparent viscosities compared to the mortar composition containing the cement composition of Comparative Example 1. It is presumed that the lower apparent viscosity enhances the filling property of the mortar composition into a mold, resulting in the formation of a dense hardened body exhibiting high compressive strength.

[0069] Compared with the cement composition of Comparative Example 2, the cement compositions of Examples 1 to 4 had low heat of hydration at ages of 7 and 28 days, and were able to achieve both good heat generation properties and strength development.

Claims

1. A cement composition comprising cement clinker, gypsum, and limestone, Based on the mass of the cement composition, the content of the limestone is more than 5 mass% and 15 mass% or less, and the total content of the cement clinker and the gypsum is 85 mass% or more and less than 95 mass%, The cement composition has a viscosity of 3500 cm 2 / g or more 4000cm 2 / g or less, In the particle size distribution of the cement composition as determined by the laser diffraction / scattering method, the ratio of particles with a particle size of 10.9 μm or more is R 10.9 [%], the ratio of grains with a particle size of 35.1 μm or more is R 35.1 When [%], Formula: Rc=R 35.1 / (R 10.9 -R 35.1 ) Rc calculated by is 0.27 or more and 0.40 or less, In the cement clinker, SO 3 The content of is 0.3 mass% or more and 1.5 mass% or less based on the mass of the cement clinker, 3 The amount of S is 50% by mass or more and 64% by mass or less, and C 3 The amount of A is 9.0 mass% or more and 12 mass% or less, and C 3 S amount and C 3 The amount A is a value calculated by the Bogue formula, Formula: Hemihydration rate = 100 × mass of hemihydrate gypsum / (mass of hemihydrate gypsum + mass of dihydrate gypsum) In the above formula, the mass of gypsum hemihydrate and the mass of gypsum dihydrate are calculated by SO 3 The hemihydration rate of the gypsum, which is the converted mass, is 25% by mass or more and 90% by mass or less, The mortar composition containing only the cement composition, water and silica sand is subjected to a temperature of 20°C and a shear rate of 1s -1 The apparent viscosity is 1 Pa s or more and 8 Pa s or less, The apparent viscosity is a value obtained by mixing a mixture containing only 100 g of the cement composition, 50 g of water, and 100 g of silica sand with a chemical mixer at a rotation speed of 500 rpm for 3 minutes to form a mortar composition, and measuring the apparent viscosity of the mortar composition 5 minutes after the start of mixing with a double cylinder rheometer. Cement compositions.

2. The cement composition has a viscosity of 3800 cm 2 / g and above 4000 cm 2 The cement composition according to claim 1, which is a powder having a Blaine specific surface area of ​​0.1 to 1.0 μm / g or less.

3. The cement composition according to claim 1, wherein the hemihydration rate of the gypsum is 40% by mass or more and 90% by mass or less.

4. In the particle size distribution of the cement composition, the ratio of the part with a particle size of 2.0 μm or more is R 2.0 When Formula: Rf=R 2.0 -R 10.9 The cement composition according to claim 1, wherein Rf calculated by the above formula is 30.0% or more and 35.7% or less.

5. 13. A method for producing the cement composition of claim 1, comprising: The method includes forming the cement composition by mixing cement clinker, gypsum, and limestone.

6. A mortar composition comprising the cement composition of claim 1, fine aggregate and water.

7. The density of the mortar hardened body formed from the mortar composition without the addition of any admixtures at a material age of 24 hours in accordance with JIS R 5201:2015 "Physical test methods for cement" is 2.230 g / cm 3 2.280g / cm or more 3 7. The mortar composition according to claim 6, wherein:

8. A concrete composition comprising the cement composition of claim 1, fine aggregate, coarse aggregate and water.