A biochar-blended adhesive powder composite water-based slurry additive and its preparation method
By modifying a water-based slurry additive that combines biochar and elastic rubber powder, and combining it with multi-dimensional synergistic effects, the problems of uneven dispersion, poor stability, and high-temperature performance degradation of water-based slurries are solved, achieving high efficiency in rheological properties and long-term storage stability, making it suitable for industrial biomass liquid fuels.
Patent Information
- Application Number
- CN202611628470.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-21
- Publication Date
- 2026-11-17
AI Technical Summary
Existing water-based slurry fuel additives have shortcomings in terms of dispersion, flowability, stability and temperature resistance, resulting in low combustion efficiency, short storage period and poor environmental performance. In addition, traditional additives rely on chemically synthesized raw materials, resulting in high production costs.
A composite water-based slurry additive of biochar and elastic rubber powder is adopted. Through the compound system of modified biochar, polyether modified polydimethylsiloxane and polyaspartic acid, combined with plasma treatment and inorganic-organic crosslinking technology, a multi-dimensional synergistic effect is formed to improve the particle dispersion stability and high-temperature viscosity retention rate.
It significantly improves the rheological properties, long-term storage stability and high-temperature resistance of water-based slurries, and solves the problems of uneven dispersion, easy sedimentation and high-temperature performance degradation of traditional additives, making it suitable for industrial preparation and high-temperature combustion conditions.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This application relates to the field of water-based slurry fuel additives, and more specifically, it relates to a biochar-blended rubber powder composite water-based slurry additive and its preparation method. Background Technology
[0002] Biomass liquid fuels and water-based fuel slurries represent an important development direction for new clean energy, possessing advantages such as low carbon emissions, environmental friendliness, renewable raw materials, and low combustion pollution, making them suitable for various applications including industrial heating and residential fuel. The core performance of water-based slurry fuels depends on the additive system, which directly determines the slurry's dispersion stability, rheological properties, slurry concentration, and storage period, making it a key material for ensuring efficient fuel utilization. Currently, most commercially available water-based slurry additives use single polymeric surfactants, starch-based, or lignin-based auxiliaries, resulting in limited composition and function, and significant technological shortcomings.
[0003] In practical applications, existing conventional additives have several drawbacks. First, they have poor coating and dispersion effects on biomass raw material powders, resulting in water-based slurries with high viscosity and insufficient fluidity, making it impossible to achieve high-concentration slurry formation and significantly reducing fuel calorific value and combustion efficiency. Second, the slurries exhibit poor suspension stability, easily leading to stratification, sedimentation, and agglomeration during long-term storage, resulting in short storage periods and poor compatibility. Furthermore, traditional additives have weak temperature and acid / alkali resistance, poor adaptability to various operating conditions, and mostly rely on chemically synthesized raw materials, leading to high production costs and insufficient environmental friendliness, which does not align with the low-carbon and circular development concept of biomass fuels.
[0004] Existing biochar-based additives rely solely on the porous adsorption properties of biochar, neglecting the bonding and toughening advantages of adhesive powder. This results in poor interfacial compatibility, leading to agglomeration and failure issues after simple blending, and failing to simultaneously address slurry flowability, stability, and structural strength. To address the shortcomings of existing technologies, such as unreasonable component combinations, lack of synergistic effects, limited overall performance, and crude preparation processes, there is an urgent need to develop a biochar-adhesive powder composite water-based slurry additive. Through precise formulation and modification processes, this additive should achieve synergistic effects across multiple components, while also considering slurry performance, storage stability, and environmental and economic benefits, making it suitable for large-scale production and application of biomass liquid fuels. Summary of the Invention
[0005] To address the technical problems mentioned in the background section, this application provides a biochar-blended adhesive powder composite water-based slurry additive and its preparation method.
[0006] In the first aspect, this application provides a biochar-blended adhesive powder composite water-based slurry additive, employing the following technical solution: 1. A biochar-blended adhesive powder composite water-based slurry additive, characterized in that it comprises the following raw materials in parts by weight: 20-40 parts modified biochar, 15-30 parts elastic adhesive powder, 3-8 parts dispersant, 2-6 parts stabilizer, 3-5 parts temperature-resistant modifier, 0.5-2 parts pH adjuster, and 30-50 parts deionized water. The method for preparing the modified biochar includes the following preparation steps: S1. Select agricultural and forestry waste mixed with straw and wood chips, dry and crush it, and then sieve it to obtain biomass powder; S2. Under nitrogen protection, biomass powder is carbonized at high temperature and then cooled to obtain biochar. S3. Activate the biochar by plasma treatment to obtain activated biochar; S4. Add activated biochar to the modified polymer solution and stir to react. After the reaction is complete, filter, wash and dry in sequence to obtain modified biochar. The high-temperature carbonization process in step S2 is specifically as follows: the temperature is increased to 450-550℃ at a heating rate of 5-8℃ / min, and high-temperature carbonization is carried out for 2-4 hours. During the carbonization process, the nitrogen flow rate is controlled at 80-120mL / min. In step S4, the modified polymer solution is composed of polyether-modified polydimethylsiloxane, polyaspartic acid, and deionized water in a mass ratio of 8-12:3-5:80-100; in step S4, the stirring reaction temperature is 55-65℃ and the reaction time is 2-3h.
[0007] Preferably, in step S3, the plasma treatment power is 150-250W and the activation treatment time is 15-30min.
[0008] Preferably, the elastic adhesive powder is composed of ethylene-vinyl acetate copolymer adhesive powder and styrene-butadiene resin powder in a mass ratio of 4-7:1-3.
[0009] Preferably, the dispersant is one or more of sodium dodecylbenzenesulfonate, polycarboxylate dispersant, and sodium lignosulfonate.
[0010] Preferably, the stabilizer is one or more of hydroxyethyl cellulose, xanthan gum, and carboxymethyl cellulose.
[0011] Preferably, the pH adjuster is one or more of triethanolamine, sodium bicarbonate, and diethanolamine.
[0012] Preferably, the preparation method of the temperature-resistant modifier includes the following preparation steps: Nano-alumina, potassium hexatitanate whiskers, and isopropanol were added to deionized water and ultrasonically treated to obtain an inorganic high-temperature resistant composite dispersion. The inorganic high-temperature resistant composite dispersion was heated to 45-55℃, and glycidyl methacrylate was added dropwise while stirring to react. Then, an organoboron crosslinking agent and waterborne polyurethane emulsion were added and crosslinked at a constant temperature. After the reaction was completed, the mixture was cooled, allowed to stand for aging, dried, pulverized, and sieved to obtain a heat-resistant modifier.
[0013] Preferably, the mass ratio of the deionized water, nano-alumina, potassium hexatitanate whiskers, and isopropanol is 50-70:8-15:5-10:20-25.
[0014] Preferably, the mass ratio of the inorganic high-temperature resistant composite dispersion, glycidyl methacrylate, organic boron crosslinking agent, and aqueous polyurethane emulsion is 80-100:6-12:3-6:15-25.
[0015] Secondly, this application also provides a method for preparing a biochar-blended adhesive powder composite water-based slurry additive, employing the following technical solution: A method for preparing a biochar-blended adhesive powder composite water-based slurry additive includes the following preparation steps: Dispersant and elastic adhesive powder are added to deionized water and stirred evenly to obtain a stable base liquid. Modified biochar is added to the stable base liquid and stirred evenly. Then, stabilizer is added and stirred evenly again. Then, heat-resistant modifier and pH adjuster are added and stirred to react. After stirring, high-speed homogenization and defoaming treatment is carried out. After filtration and cooling, biochar-blended adhesive powder composite water-based slurry additive is obtained.
[0016] In summary, this application has the following beneficial effects: This application employs an elastic adhesive powder system composed of ethylene-vinyl acetate copolymer powder and styrene-butadiene resin powder. The two powder components can exert a complementary and synergistic effect. The ethylene-vinyl acetate copolymer powder can impart excellent film-forming toughness and suspension support to the slurry, while the styrene-butadiene resin powder can enhance the elasticity and shear resistance of the colloid. This elastic adhesive powder system effectively improves the defects of loose colloid structure and easy delamination in single adhesive powder systems, and can reduce the apparent viscosity and yield stress of the slurry, reduce pipeline pumping resistance, and ensure the stability of low-speed start-up and high-speed transportation.
[0017] Meanwhile, this application employs a binary polymeric compound system of polyether-modified polydimethylsiloxane and polyaspartic acid to synergistically modify biochar. Among them, polyether-modified polydimethylsiloxane can optimize the surface wettability and dispersibility of biochar, while polyaspartic acid can enhance the interfacial bonding force between biochar and slurry system through chelation adsorption. Combined with plasma treatment activation process, it can effectively enrich the pore structure of biochar, increase surface active sites, solve the problems of easy agglomeration and poor interfacial compatibility of traditional biochar, significantly improve particle dispersion stability, and reduce long-term static sedimentation rate.
[0018] Furthermore, this application prepares a heat-resistant modifier through inorganic powder composite dispersion and organic cross-linking polymerization modification. The inorganic heat-resistant framework structure of nano-alumina and potassium hexatitanate whiskers is combined with an organic network structure formed by cross-linking waterborne polyurethane and organic boron to construct an inorganic-organic cross-linked composite heat-resistant system. This system effectively inhibits the decomposition and failure of the colloidal structure at high temperatures and significantly improves the high-temperature viscosity retention rate of the slurry. The various modified systems and the compounded colloidal system form a multi-dimensional synergistic effect, enabling the prepared water-based slurry to possess excellent rheological properties, long-term storage stability, high-temperature resistance, and sedimentation and redispersibility. This effectively solves the technical pain points of traditional biomass water-based slurries, such as easy settling and caking, rapid high-temperature performance degradation, and poor pumpability, making it suitable for industrial preparation and high-temperature combustion conditions. Detailed Implementation
[0019] The present application will be further described in detail below with reference to the embodiments.
[0020] The ethylene-vinyl acetate copolymer powder used in the embodiments and comparative examples of this invention was purchased from Qingdao Tengyun Chemical Technology Co., Ltd.; styrene-butadiene resin powder (brand name: SL-803G) was purchased from Dongguan Xinrui New Materials Co., Ltd.; polyether-modified polydimethylsiloxane and polyaspartic acid were both purchased from Hubei Langbowan Biomedical Co., Ltd.; polycarboxylate dispersant (model: BG1900) was purchased from Nanjing Baiju Technology Co., Ltd.; nano alumina (particle size: 200 mesh) was purchased from Shijiazhuang Jinghuang Technology Co., Ltd.; potassium hexatitanate whiskers were purchased from Jinan Zian Chemical Co., Ltd.; organoboron crosslinking agent was purchased from Suzhou Senfida Chemical Co., Ltd.; and waterborne polyurethane emulsion (model: AH-1128-2) was purchased from Anhui Dawei Huatai New Materials Technology Co., Ltd.
[0021] Examples 1-3 provide a biochar-blended adhesive powder composite water-based slurry additive and its preparation method.
[0022] Example 1 A biochar-blended adhesive powder composite water-based slurry additive comprises the following raw materials in parts by weight: 20 parts modified biochar, 15 parts elastic adhesive powder, 3 parts dispersant, 2 parts stabilizer, 3 parts temperature-resistant modifier, 0.5 parts pH adjuster, and 30 parts deionized water; wherein the elastic adhesive powder is composed of ethylene-vinyl acetate copolymer adhesive powder and styrene-butadiene resin powder in a mass ratio of 4:1; the dispersant is sodium dodecylbenzenesulfonate; the stabilizer is hydroxyethyl cellulose; and the pH adjuster is triethanolamine.
[0023] The preparation method of modified biochar includes the following steps: S1. Select agricultural and forestry waste mixed with straw and sawdust in a mass ratio of 1:1, remove stones, mud and sand impurities, dry at 50℃ for 10 hours, crush and pass through a 20-mesh sieve to obtain biomass powder. S2. Under nitrogen protection, the biomass powder is heated to 450℃ at a heating rate of 5℃ / min and carbonized at high temperature for 2 hours. During the carbonization process, the nitrogen flow rate is controlled at 80mL / min. The mixture is then naturally cooled to room temperature to obtain biochar. S3. Argon gas is introduced as the activation gas under a vacuum of 0.08 MPa, and the argon gas flow rate is set to 30 mL / min. The biochar is activated by plasma treatment with a plasma treatment power of 150 W and room temperature etching activation treatment for 15 min to obtain activated biochar. S4. Control the mass ratio of activated biochar to modified polymer solution to 1:5. Add activated biochar to modified polymer solution and stir at 55℃ for 2 hours at a stirring speed of 100 rpm. After the reaction is completed, filter through a 200-mesh filter, wash three times with deionized water, and dry at 50℃ for 10 hours to obtain modified biochar. The modified polymer solution is composed of polyether-modified polydimethylsiloxane, polyaspartic acid and deionized water in a mass ratio of 8:3:80.
[0024] The preparation method of the temperature-resistant modifier includes the following preparation steps: The mass ratio of deionized water, nano-alumina, potassium hexatitanate whiskers, and isopropanol was controlled at 50:8:5:20. Nano-alumina, potassium hexatitanate whiskers, and isopropanol were added to the deionized water, and the mixture was ultrasonically treated at room temperature for 30 min at an ultrasonic power of 100 W and an ultrasonic frequency of 40 kHz to obtain an inorganic high-temperature resistant composite dispersion. The inorganic high-temperature resistant composite dispersion was heated to 45 °C, and glycidyl methacrylate was added dropwise over a period of 1 h. After the addition was completed, the mixture was stirred at 200 rpm for 2 h. Subsequently, an organoboron crosslinking agent and an aqueous polyurethane emulsion were added, and the mixture was subjected to a constant temperature crosslinking reaction at 50 °C for 1.5 h. After the reaction was completed, the mixture was naturally cooled to room temperature, allowed to stand for 5 h, dried at 50 °C for 8 h, and pulverized through a 200-mesh sieve to obtain a heat-resistant modifier. The mass ratio of the inorganic high-temperature resistant composite dispersion, glycidyl methacrylate, organoboron crosslinking agent, and aqueous polyurethane emulsion was 80:6:3:15.
[0025] A method for preparing a biochar-blended adhesive powder composite water-based slurry additive includes the following preparation steps: Dispersant and elastic adhesive powder were added to deionized water and stirred at 200 rpm for 20 minutes at 40°C until homogeneous, resulting in a stable base liquid. Modified biochar was added to the stable base liquid and stirred at 200 rpm for 20 minutes at 50°C until homogeneous. Stabilizer was then added and stirred for another 10 minutes. Heat-resistant modifier and pH adjuster were added and stirred at 200 rpm for 10 minutes at 40°C until homogeneous. High-speed homogenization and defoaming treatment was then performed at 8000 rpm for 20 minutes at 40°C. The mixture was then filtered through a 300-mesh filter and allowed to cool naturally to room temperature to obtain a biochar-blended adhesive powder composite water-based slurry additive.
[0026] Example 2 A biochar-blended adhesive powder composite water-based slurry additive comprises the following raw materials in parts by weight: 30 parts modified biochar, 22 parts elastic adhesive powder, 5 parts dispersant, 4 parts stabilizer, 4 parts temperature-resistant modifier, 1 part pH adjuster, and 40 parts deionized water; wherein the elastic adhesive powder is composed of ethylene-vinyl acetate copolymer adhesive powder and styrene-butadiene resin powder in a mass ratio of 5.5:2; the dispersant is a polycarboxylate dispersant; the stabilizer is xanthan gum; and the pH adjuster is sodium bicarbonate.
[0027] The preparation method of modified biochar includes the following steps: S1. Select agricultural and forestry waste mixed with straw and sawdust in a mass ratio of 1:1, remove stones, mud and sand impurities, dry at 70℃ for 11 hours, crush and pass through a 40-mesh sieve to obtain biomass powder. S2. Under nitrogen protection, the biomass powder is heated to 500℃ at a heating rate of 7℃ / min and carbonized at high temperature for 3 hours. During the carbonization process, the nitrogen flow rate is controlled at 100mL / min. The mixture is then naturally cooled to room temperature to obtain biochar. S3. Argon gas is introduced as the activation gas under a vacuum of 0.1 MPa, and the argon gas flow rate is set to 40 mL / min. The biochar is activated by plasma treatment with a plasma treatment power of 200 W and room temperature etching activation treatment for 22 min to obtain activated biochar. S4. Controlling the mass ratio of activated biochar to modified polymer solution to 2:7, the activated biochar is added to the modified polymer solution, and the mixture is stirred at 200 rpm for 2.5 h at 60 °C. After the reaction is completed, the mixture is filtered through a 250-mesh filter, washed four times with deionized water, and dried at 55 °C for 11 h to obtain modified biochar. The modified polymer solution is composed of polyether-modified polydimethylsiloxane, polyaspartic acid, and deionized water in a mass ratio of 10:4:90.
[0028] The preparation method of the temperature-resistant modifier includes the following preparation steps: The mass ratio of deionized water, nano-alumina, potassium hexatitanate whiskers, and isopropanol was controlled at 60:12:8:22. Nano-alumina, potassium hexatitanate whiskers, and isopropanol were added to the deionized water, and the mixture was ultrasonically treated at room temperature for 35 minutes at an ultrasonic power of 110W and an ultrasonic frequency of 50kHz to obtain an inorganic high-temperature resistant composite dispersion. The inorganic high-temperature resistant composite dispersion was heated to 50℃, and glycidyl methacrylate was added dropwise over a time of 1.1 hours. After the addition was complete... The mixture was stirred at 250 rpm for 2.5 hours. Then, an organoboron crosslinking agent and an aqueous polyurethane emulsion were added, and the mixture was subjected to a constant temperature crosslinking reaction at 55°C for 2 hours. After the reaction was completed, the mixture was allowed to cool naturally to room temperature, allowed to stand for 7 hours to mature, dried at 55°C for 9 hours, and then pulverized through a 300-mesh sieve to obtain a heat-resistant modifier. The mass ratio of the inorganic high-temperature resistant composite dispersion, glycidyl methacrylate, organoboron crosslinking agent, and aqueous polyurethane emulsion was 90:9:4.5:20.
[0029] A method for preparing a biochar-blended adhesive powder composite water-based slurry additive includes the following preparation steps: Dispersant and elastic adhesive powder were added to deionized water and stirred at 300 rpm for 30 minutes at 45°C until homogeneous, resulting in a stable base liquid. Modified biochar was added to the stable base liquid and stirred at 300 rpm for 30 minutes at 55°C until homogeneous. Stabilizer was then added and stirring was continued for 20 minutes. Heat-resistant modifier and pH adjuster were then added and stirred at 300 rpm for 20 minutes at 45°C until homogeneous. High-speed homogenization and defoaming treatment was then performed at 9000 rpm at 45°C for 30 minutes. The mixture was then filtered through a 400-mesh filter and allowed to cool naturally to room temperature to obtain a biochar-blended adhesive powder composite water-based slurry additive.
[0030] Example 3 A biochar-blended adhesive powder composite water-based slurry additive comprises the following raw materials in parts by weight: 40 parts modified biochar, 30 parts elastic adhesive powder, 8 parts dispersant, 6 parts stabilizer, 5 parts temperature-resistant modifier, 2 parts pH adjuster, and 50 parts deionized water; wherein the elastic adhesive powder is composed of ethylene-vinyl acetate copolymer adhesive powder and styrene-butadiene resin powder in a mass ratio of 7:3; the dispersant is sodium lignosulfonate; the stabilizer is carboxymethyl cellulose; and the pH adjuster is diethanolamine.
[0031] The preparation method of modified biochar includes the following steps: S1. Select agricultural and forestry waste mixed with straw and sawdust in a mass ratio of 1:1, remove stones, mud and sand impurities, dry at 80℃ for 12 hours, crush and pass through a 50-mesh sieve to obtain biomass powder. S2. Under nitrogen protection, the biomass powder is heated to 550℃ at a heating rate of 8℃ / min and carbonized at high temperature for 4 hours. During the carbonization process, the nitrogen flow rate is controlled at 120mL / min. The mixture is then naturally cooled to room temperature to obtain biochar. S3. Argon gas is introduced as the activation gas under a vacuum of 0.12 MPa, and the argon gas flow rate is set to 50 mL / min. The biochar is activated by plasma treatment with a plasma treatment power of 250 W and room temperature etching activation treatment for 30 min to obtain activated biochar. S4. Control the mass ratio of activated biochar to modified polymer solution to 3:8. Add activated biochar to modified polymer solution and stir at 300 rpm for 3 hours at 65°C. After the reaction, filter through a 300-mesh filter, wash 5 times with deionized water, and dry at 60°C for 12 hours to obtain modified biochar. The modified polymer solution is composed of polyether-modified polydimethylsiloxane, polyaspartic acid, and deionized water in a mass ratio of 12:5:100.
[0032] The preparation method of the temperature-resistant modifier includes the following preparation steps: The mass ratio of deionized water, nano-alumina, potassium hexatitanate whiskers, and isopropanol was controlled at 70:15:10:25. Nano-alumina, potassium hexatitanate whiskers, and isopropanol were added to the deionized water, and the mixture was ultrasonically treated at room temperature for 40 min at an ultrasonic power of 120 W and an ultrasonic frequency of 60 kHz to obtain an inorganic high-temperature resistant composite dispersion. The inorganic high-temperature resistant composite dispersion was heated to 55 °C, and glycidyl methacrylate was added dropwise over a time of 1.2 h. After the addition was complete... The mixture was stirred at 300 rpm for 3 hours. Then, an organoboron crosslinking agent and an aqueous polyurethane emulsion were added, and the mixture was subjected to a constant temperature crosslinking reaction at 60°C for 2.5 hours. After the reaction was completed, the mixture was allowed to cool naturally to room temperature, allowed to stand for 8 hours, dried at 60°C for 10 hours, and then pulverized through a 400-mesh sieve to obtain a heat-resistant modifier. The mass ratio of the inorganic high-temperature resistant composite dispersion, glycidyl methacrylate, organoboron crosslinking agent, and aqueous polyurethane emulsion was 100:12:6:25.
[0033] A method for preparing a biochar-blended adhesive powder composite water-based slurry additive includes the following preparation steps: Dispersant and elastic adhesive powder were added to deionized water and stirred at 400 rpm for 40 minutes at 50°C until homogeneous, resulting in a stable base liquid. Modified biochar was added to the stable base liquid and stirred at 400 rpm for 40 minutes at 60°C until homogeneous. Stabilizer was then added and stirring was continued for 30 minutes. Heat-resistant modifier and pH adjuster were then added and stirred at 400 rpm for 30 minutes at 50°C until homogeneous. High-speed homogenization and defoaming treatment was then performed at 10,000 rpm at 50°C for 40 minutes. The mixture was then filtered through a 500-mesh filter and allowed to cool naturally to room temperature to obtain a biochar-blended adhesive powder composite water-based slurry additive.
[0034] Comparative Example 1 A biochar-blended adhesive powder composite water-based slurry additive comprises the following raw materials in parts by weight: 20 parts modified biochar, 15 parts elastic adhesive powder, 3 parts dispersant, 2 parts stabilizer, 3 parts temperature-resistant modifier, 0.5 parts pH adjuster, and 30 parts deionized water; wherein the elastic adhesive powder is ethylene-vinyl acetate copolymer adhesive powder; the dispersant is sodium dodecylbenzenesulfonate; the stabilizer is hydroxyethyl cellulose; and the pH adjuster is triethanolamine.
[0035] The preparation method of modified biochar includes the following steps: S1. Select agricultural and forestry waste mixed with straw and sawdust in a mass ratio of 1:1, remove stones, mud and sand impurities, dry at 50℃ for 10 hours, crush and pass through a 20-mesh sieve to obtain biomass powder. S2. Under nitrogen protection, the biomass powder is heated to 450℃ at a heating rate of 5℃ / min and carbonized at high temperature for 2 hours. During the carbonization process, the nitrogen flow rate is controlled at 80mL / min. The mixture is then naturally cooled to room temperature to obtain biochar. S3. Argon gas is introduced as the activation gas under a vacuum of 0.08 MPa, and the argon gas flow rate is set to 30 mL / min. The biochar is activated by plasma treatment with a plasma treatment power of 150 W and room temperature etching activation treatment for 15 min to obtain activated biochar. S4. Control the mass ratio of activated biochar to modified polymer solution to 1:5. Add activated biochar to modified polymer solution and stir at 55℃ for 2 hours at a stirring speed of 100 rpm. After the reaction is completed, filter through a 200-mesh filter, wash three times with deionized water, and dry at 50℃ for 10 hours to obtain modified biochar. The modified polymer solution is composed of polyether-modified polydimethylsiloxane, polyaspartic acid and deionized water in a mass ratio of 8:3:80.
[0036] The preparation method of the temperature-resistant modifier includes the following preparation steps: The mass ratio of deionized water, nano-alumina, potassium hexatitanate whiskers, and isopropanol was controlled at 50:8:5:20. Nano-alumina, potassium hexatitanate whiskers, and isopropanol were added to the deionized water, and the mixture was ultrasonically treated at room temperature for 30 min at an ultrasonic power of 100 W and an ultrasonic frequency of 40 kHz to obtain an inorganic high-temperature resistant composite dispersion. The inorganic high-temperature resistant composite dispersion was heated to 45 °C, and glycidyl methacrylate was added dropwise over a period of 1 h. After the addition was completed, the mixture was stirred at 200 rpm for 2 h. Subsequently, an organoboron crosslinking agent and an aqueous polyurethane emulsion were added, and the mixture was subjected to a constant temperature crosslinking reaction at 50 °C for 1.5 h. After the reaction was completed, the mixture was naturally cooled to room temperature, allowed to stand for 5 h, dried at 50 °C for 8 h, and pulverized through a 200-mesh sieve to obtain a heat-resistant modifier. The mass ratio of the inorganic high-temperature resistant composite dispersion, glycidyl methacrylate, organoboron crosslinking agent, and aqueous polyurethane emulsion was 80:6:3:15.
[0037] A method for preparing a biochar-blended adhesive powder composite water-based slurry additive includes the following preparation steps: Dispersant and elastic adhesive powder were added to deionized water and stirred at 200 rpm for 20 minutes at 40°C until homogeneous, resulting in a stable base liquid. Modified biochar was added to the stable base liquid and stirred at 200 rpm for 20 minutes at 50°C until homogeneous. Stabilizer was then added and stirred for another 10 minutes. Heat-resistant modifier and pH adjuster were added and stirred at 200 rpm for 10 minutes at 40°C until homogeneous. High-speed homogenization and defoaming treatment was then performed at 8000 rpm for 20 minutes at 40°C. The mixture was then filtered through a 300-mesh filter and allowed to cool naturally to room temperature to obtain a biochar-blended adhesive powder composite water-based slurry additive.
[0038] Comparative Example 2 A biochar-blended adhesive powder composite water-based slurry additive comprises the following raw materials in parts by weight: 20 parts modified biochar, 15 parts elastic adhesive powder, 3 parts dispersant, 2 parts stabilizer, 3 parts temperature-resistant modifier, 0.5 parts pH adjuster, and 30 parts deionized water; wherein the elastic adhesive powder is styrene-butadiene resin powder; the dispersant is sodium dodecylbenzenesulfonate; the stabilizer is hydroxyethyl cellulose; and the pH adjuster is triethanolamine.
[0039] The preparation method of modified biochar includes the following steps: S1. Select agricultural and forestry waste mixed with straw and sawdust in a mass ratio of 1:1, remove stones, mud and sand impurities, dry at 50℃ for 10 hours, crush and pass through a 20-mesh sieve to obtain biomass powder. S2. Under nitrogen protection, the biomass powder is heated to 450℃ at a heating rate of 5℃ / min and carbonized at high temperature for 2 hours. During the carbonization process, the nitrogen flow rate is controlled at 80mL / min. The mixture is then naturally cooled to room temperature to obtain biochar. S3. Argon gas is introduced as the activation gas under a vacuum of 0.08 MPa, and the argon gas flow rate is set to 30 mL / min. The biochar is activated by plasma treatment with a plasma treatment power of 150 W and room temperature etching activation treatment for 15 min to obtain activated biochar. S4. Control the mass ratio of activated biochar to modified polymer solution to 1:5. Add activated biochar to modified polymer solution and stir at 55℃ for 2 hours at a stirring speed of 100 rpm. After the reaction is completed, filter through a 200-mesh filter, wash three times with deionized water, and dry at 50℃ for 10 hours to obtain modified biochar. The modified polymer solution is composed of polyether-modified polydimethylsiloxane, polyaspartic acid and deionized water in a mass ratio of 8:3:80.
[0040] The preparation method of the temperature-resistant modifier includes the following preparation steps: The mass ratio of deionized water, nano-alumina, potassium hexatitanate whiskers, and isopropanol was controlled at 50:8:5:20. Nano-alumina, potassium hexatitanate whiskers, and isopropanol were added to the deionized water, and the mixture was ultrasonically treated at room temperature for 30 min at an ultrasonic power of 100 W and an ultrasonic frequency of 40 kHz to obtain an inorganic high-temperature resistant composite dispersion. The inorganic high-temperature resistant composite dispersion was heated to 45 °C, and glycidyl methacrylate was added dropwise over a period of 1 h. After the addition was completed, the mixture was stirred at 200 rpm for 2 h. Subsequently, an organoboron crosslinking agent and an aqueous polyurethane emulsion were added, and the mixture was subjected to a constant temperature crosslinking reaction at 50 °C for 1.5 h. After the reaction was completed, the mixture was naturally cooled to room temperature, allowed to stand for 5 h, dried at 50 °C for 8 h, and pulverized through a 200-mesh sieve to obtain a heat-resistant modifier. The mass ratio of the inorganic high-temperature resistant composite dispersion, glycidyl methacrylate, organoboron crosslinking agent, and aqueous polyurethane emulsion was 80:6:3:15.
[0041] A method for preparing a biochar-blended adhesive powder composite water-based slurry additive includes the following preparation steps: Dispersant and elastic adhesive powder were added to deionized water and stirred at 200 rpm for 20 minutes at 40°C until homogeneous, resulting in a stable base liquid. Modified biochar was added to the stable base liquid and stirred at 200 rpm for 20 minutes at 50°C until homogeneous. Stabilizer was then added and stirred for another 10 minutes. Heat-resistant modifier and pH adjuster were added and stirred at 200 rpm for 10 minutes at 40°C until homogeneous. High-speed homogenization and defoaming treatment was then performed at 8000 rpm for 20 minutes at 40°C. The mixture was then filtered through a 300-mesh filter and allowed to cool naturally to room temperature to obtain a biochar-blended adhesive powder composite water-based slurry additive.
[0042] Comparative Example 3 A biochar-blended adhesive powder composite water-based slurry additive comprises the following raw materials in parts by weight: 20 parts modified biochar, 15 parts elastic adhesive powder, 3 parts dispersant, 2 parts stabilizer, 3 parts temperature-resistant modifier, 0.5 parts pH adjuster, and 30 parts deionized water; wherein the elastic adhesive powder is composed of ethylene-vinyl acetate copolymer adhesive powder and styrene-butadiene resin powder in a mass ratio of 4:1; the dispersant is sodium dodecylbenzenesulfonate; the stabilizer is hydroxyethyl cellulose; and the pH adjuster is triethanolamine.
[0043] The preparation method of modified biochar includes the following steps: S1. Select agricultural and forestry waste mixed with straw and sawdust in a mass ratio of 1:1, remove stones, mud and sand impurities, dry at 50℃ for 10 hours, crush and pass through a 20-mesh sieve to obtain biomass powder. S2. Under nitrogen protection, the biomass powder is heated to 450℃ at a heating rate of 5℃ / min and carbonized at high temperature for 2 hours. During the carbonization process, the nitrogen flow rate is controlled at 80mL / min. The mixture is then naturally cooled to room temperature to obtain biochar. S3. Argon gas is introduced as the activation gas under a vacuum of 0.08 MPa, and the argon gas flow rate is set to 30 mL / min. The biochar is activated by plasma treatment with a plasma treatment power of 150 W and room temperature etching activation treatment for 15 min to obtain activated biochar. S4. Control the mass ratio of activated biochar to modified polymer solution to 1:5. Add activated biochar to modified polymer solution and stir at 55℃ for 2 hours at a stirring speed of 100 rpm. After the reaction is completed, filter through a 200-mesh filter, wash three times with deionized water, and dry at 50℃ for 10 hours to obtain modified biochar. The modified polymer solution is composed of polyaspartic acid and deionized water in a mass ratio of 11:80.
[0044] The preparation method of the temperature-resistant modifier includes the following preparation steps: The mass ratio of deionized water, nano-alumina, potassium hexatitanate whiskers, and isopropanol was controlled at 50:8:5:20. Nano-alumina, potassium hexatitanate whiskers, and isopropanol were added to the deionized water, and the mixture was ultrasonically treated at room temperature for 30 min at an ultrasonic power of 100 W and an ultrasonic frequency of 40 kHz to obtain an inorganic high-temperature resistant composite dispersion. The inorganic high-temperature resistant composite dispersion was heated to 45 °C, and glycidyl methacrylate was added dropwise over a period of 1 h. After the addition was completed, the mixture was stirred at 200 rpm for 2 h. Subsequently, an organoboron crosslinking agent and an aqueous polyurethane emulsion were added, and the mixture was subjected to a constant temperature crosslinking reaction at 50 °C for 1.5 h. After the reaction was completed, the mixture was naturally cooled to room temperature, allowed to stand for 5 h, dried at 50 °C for 8 h, and pulverized through a 200-mesh sieve to obtain a heat-resistant modifier. The mass ratio of the inorganic high-temperature resistant composite dispersion, glycidyl methacrylate, organoboron crosslinking agent, and aqueous polyurethane emulsion was 80:6:3:15.
[0045] A method for preparing a biochar-blended adhesive powder composite water-based slurry additive includes the following preparation steps: Dispersant and elastic adhesive powder were added to deionized water and stirred at 200 rpm for 20 minutes at 40°C until homogeneous, resulting in a stable base liquid. Modified biochar was added to the stable base liquid and stirred at 200 rpm for 20 minutes at 50°C until homogeneous. Stabilizer was then added and stirred for another 10 minutes. Heat-resistant modifier and pH adjuster were added and stirred at 200 rpm for 10 minutes at 40°C until homogeneous. High-speed homogenization and defoaming treatment was then performed at 8000 rpm for 20 minutes at 40°C. The mixture was then filtered through a 300-mesh filter and allowed to cool naturally to room temperature to obtain a biochar-blended adhesive powder composite water-based slurry additive.
[0046] Comparative Example 4 A biochar-blended adhesive powder composite water-based slurry additive comprises the following raw materials in parts by weight: 20 parts modified biochar, 15 parts elastic adhesive powder, 3 parts dispersant, 2 parts stabilizer, 3 parts temperature-resistant modifier, 0.5 parts pH adjuster, and 30 parts deionized water; wherein the elastic adhesive powder is composed of ethylene-vinyl acetate copolymer adhesive powder and styrene-butadiene resin powder in a mass ratio of 4:1; the dispersant is sodium dodecylbenzenesulfonate; the stabilizer is hydroxyethyl cellulose; and the pH adjuster is triethanolamine.
[0047] The preparation method of modified biochar includes the following steps: S1. Select agricultural and forestry waste mixed with straw and sawdust in a mass ratio of 1:1, remove stones, mud and sand impurities, dry at 50℃ for 10 hours, crush and pass through a 20-mesh sieve to obtain biomass powder. S2. Under nitrogen protection, the biomass powder is heated to 450℃ at a heating rate of 5℃ / min and carbonized at high temperature for 2 hours. During the carbonization process, the nitrogen flow rate is controlled at 80mL / min. The mixture is then naturally cooled to room temperature to obtain biochar. S3. Argon gas is introduced as the activation gas under a vacuum of 0.08 MPa, and the argon gas flow rate is set to 30 mL / min. The biochar is activated by plasma treatment with a plasma treatment power of 150 W and room temperature etching activation treatment for 15 min to obtain activated biochar. S4. Control the mass ratio of activated biochar to modified polymer solution to 1:5. Add activated biochar to modified polymer solution and stir at 55℃ for 2 hours at a stirring speed of 100 rpm. After the reaction is completed, filter through a 200-mesh filter, wash three times with deionized water, and dry at 50℃ for 10 hours to obtain modified biochar. The modified polymer solution is composed of polyether-modified polydimethylsiloxane and deionized water in a mass ratio of 11:80.
[0048] The preparation method of the temperature-resistant modifier includes the following preparation steps: The mass ratio of deionized water, nano-alumina, potassium hexatitanate whiskers, and isopropanol was controlled at 50:8:5:20. Nano-alumina, potassium hexatitanate whiskers, and isopropanol were added to the deionized water, and the mixture was ultrasonically treated at room temperature for 30 min at an ultrasonic power of 100 W and an ultrasonic frequency of 40 kHz to obtain an inorganic high-temperature resistant composite dispersion. The inorganic high-temperature resistant composite dispersion was heated to 45 °C, and glycidyl methacrylate was added dropwise over a period of 1 h. After the addition was completed, the mixture was stirred at 200 rpm for 2 h. Subsequently, an organoboron crosslinking agent and an aqueous polyurethane emulsion were added, and the mixture was subjected to a constant temperature crosslinking reaction at 50 °C for 1.5 h. After the reaction was completed, the mixture was naturally cooled to room temperature, allowed to stand for 5 h, dried at 50 °C for 8 h, and pulverized through a 200-mesh sieve to obtain a heat-resistant modifier. The mass ratio of the inorganic high-temperature resistant composite dispersion, glycidyl methacrylate, organoboron crosslinking agent, and aqueous polyurethane emulsion was 80:6:3:15.
[0049] A method for preparing a biochar-blended adhesive powder composite water-based slurry additive includes the following preparation steps: Dispersant and elastic adhesive powder were added to deionized water and stirred at 200 rpm for 20 minutes at 40°C until homogeneous, resulting in a stable base liquid. Modified biochar was added to the stable base liquid and stirred at 200 rpm for 20 minutes at 50°C until homogeneous. Stabilizer was then added and stirred for another 10 minutes. Heat-resistant modifier and pH adjuster were added and stirred at 200 rpm for 10 minutes at 40°C until homogeneous. High-speed homogenization and defoaming treatment was then performed at 8000 rpm for 20 minutes at 40°C. The mixture was then filtered through a 300-mesh filter and allowed to cool naturally to room temperature to obtain a biochar-blended adhesive powder composite water-based slurry additive.
[0050] Comparative Example 5 A biochar-blended adhesive powder composite water-based slurry additive comprises the following raw materials in parts by weight: 20 parts modified biochar, 15 parts elastic adhesive powder, 3 parts dispersant, 2 parts stabilizer, 3 parts temperature-resistant modifier, 0.5 parts pH adjuster, and 30 parts deionized water; wherein the elastic adhesive powder is composed of ethylene-vinyl acetate copolymer adhesive powder and styrene-butadiene resin powder in a mass ratio of 4:1; the dispersant is sodium dodecylbenzenesulfonate; the stabilizer is hydroxyethyl cellulose; and the pH adjuster is triethanolamine.
[0051] The preparation method of modified biochar includes the following steps: S1. Select agricultural and forestry waste mixed with straw and sawdust in a mass ratio of 1:1, remove stones, mud and sand impurities, dry at 50℃ for 10 hours, crush and pass through a 20-mesh sieve to obtain biomass powder. S2. Under nitrogen protection, the biomass powder is heated to 450℃ at a heating rate of 5℃ / min and carbonized at high temperature for 2 hours. During the carbonization process, the nitrogen flow rate is controlled at 80mL / min. The mixture is then naturally cooled to room temperature to obtain biochar. S3. Argon gas is introduced as the activation gas under a vacuum of 0.08 MPa, and the argon gas flow rate is set to 30 mL / min. The biochar is activated by plasma treatment with a plasma treatment power of 150 W and etched at room temperature for 15 min to obtain modified biochar.
[0052] The preparation method of the temperature-resistant modifier includes the following preparation steps: The mass ratio of deionized water, nano-alumina, potassium hexatitanate whiskers, and isopropanol was controlled at 50:8:5:20. Nano-alumina, potassium hexatitanate whiskers, and isopropanol were added to the deionized water, and the mixture was ultrasonically treated at room temperature for 30 min at an ultrasonic power of 100 W and an ultrasonic frequency of 40 kHz to obtain an inorganic high-temperature resistant composite dispersion. The inorganic high-temperature resistant composite dispersion was heated to 45 °C, and glycidyl methacrylate was added dropwise over a period of 1 h. After the addition was completed, the mixture was stirred at 200 rpm for 2 h. Subsequently, an organoboron crosslinking agent and an aqueous polyurethane emulsion were added, and the mixture was subjected to a constant temperature crosslinking reaction at 50 °C for 1.5 h. After the reaction was completed, the mixture was naturally cooled to room temperature, allowed to stand for 5 h, dried at 50 °C for 8 h, and pulverized through a 200-mesh sieve to obtain a heat-resistant modifier. The mass ratio of the inorganic high-temperature resistant composite dispersion, glycidyl methacrylate, organoboron crosslinking agent, and aqueous polyurethane emulsion was 80:6:3:15.
[0053] A method for preparing a biochar-blended adhesive powder composite water-based slurry additive includes the following preparation steps: Dispersant and elastic adhesive powder were added to deionized water and stirred at 200 rpm for 20 minutes at 40°C until homogeneous, resulting in a stable base liquid. Modified biochar was added to the stable base liquid and stirred at 200 rpm for 20 minutes at 50°C until homogeneous. Stabilizer was then added and stirred for another 10 minutes. Heat-resistant modifier and pH adjuster were added and stirred at 200 rpm for 10 minutes at 40°C until homogeneous. High-speed homogenization and defoaming treatment was then performed at 8000 rpm for 20 minutes at 40°C. The mixture was then filtered through a 300-mesh filter and allowed to cool naturally to room temperature to obtain a biochar-blended adhesive powder composite water-based slurry additive.
[0054] Comparative Example 6 A biochar-blended adhesive powder composite water-based slurry additive comprises the following raw materials in parts by weight: 20 parts modified biochar, 15 parts elastic adhesive powder, 3 parts dispersant, 2 parts stabilizer, 3 parts temperature-resistant modifier, 0.5 parts pH adjuster, and 30 parts deionized water; wherein, the elastic adhesive powder is composed of ethylene-vinyl acetate copolymer adhesive powder and styrene-butadiene resin powder in a mass ratio of 4:1; the dispersant is sodium dodecylbenzenesulfonate; the stabilizer is hydroxyethyl cellulose; the pH adjuster is triethanolamine; and the temperature-resistant modifier is composed of nano-alumina and potassium hexatitanate whiskers in a mass ratio of 8:5.
[0055] The preparation method of modified biochar includes the following steps: S1. Select agricultural and forestry waste mixed with straw and sawdust in a mass ratio of 1:1, remove stones, mud and sand impurities, dry at 50℃ for 10 hours, crush and pass through a 20-mesh sieve to obtain biomass powder. S2. Under nitrogen protection, the biomass powder is heated to 450℃ at a heating rate of 5℃ / min and carbonized at high temperature for 2 hours. During the carbonization process, the nitrogen flow rate is controlled at 80mL / min. The mixture is then naturally cooled to room temperature to obtain biochar. S3. Argon gas is introduced as the activation gas under a vacuum of 0.08 MPa, and the argon gas flow rate is set to 30 mL / min. The biochar is activated by plasma treatment with a plasma treatment power of 150 W and room temperature etching activation treatment for 15 min to obtain activated biochar. S4. Control the mass ratio of activated biochar to modified polymer solution to 1:5. Add activated biochar to modified polymer solution and stir at 55℃ for 2 hours at a stirring speed of 100 rpm. After the reaction is completed, filter through a 200-mesh filter, wash three times with deionized water, and dry at 50℃ for 10 hours to obtain modified biochar. The modified polymer solution is composed of polyether-modified polydimethylsiloxane, polyaspartic acid and deionized water in a mass ratio of 8:3:80.
[0056] A method for preparing a biochar-blended adhesive powder composite water-based slurry additive includes the following preparation steps: Dispersant and elastic adhesive powder were added to deionized water and stirred at 200 rpm for 20 minutes at 40°C until homogeneous, resulting in a stable base liquid. Modified biochar was added to the stable base liquid and stirred at 200 rpm for 20 minutes at 50°C until homogeneous. Stabilizer was then added and stirred for another 10 minutes. Heat-resistant modifier and pH adjuster were added and stirred at 200 rpm for 10 minutes at 40°C until homogeneous. High-speed homogenization and defoaming treatment was then performed at 8000 rpm for 20 minutes at 40°C. The mixture was then filtered through a 300-mesh filter and allowed to cool naturally to room temperature to obtain a biochar-blended adhesive powder composite water-based slurry additive.
[0057] Performance testing The comprehensive performance of the biochar-blended adhesive powder composite water-based slurry additives prepared in Examples 1-3 and Comparative Examples 1-6 of this application was tested. The specific test contents are as follows: I. Preparation method of biomass-based fuel slurry to be tested The biochar-blended adhesive powder composite water-based slurry additives prepared in Examples 1-3 and Comparative Examples 1-6 were added to the biomass water-based slurry raw material system at a uniform addition amount to prepare the biomass water-based fuel slurry to be tested. The specific slurry preparation method, performance testing methods, and evaluation standards are as follows: Preparation method of biomass water-based fuel slurry to be tested: Straw and sawdust are mixed evenly at a mass ratio of 1:1. Impurities such as stones and mud are removed from the raw materials. The raw materials are dried in an 80℃ oven until the moisture content of the raw materials is ≤2wt%. After being crushed by a pulverizer, the particle size distribution is carried out, and the proportion of 20-80 mesh particles is controlled at 40wt% and the proportion of 80-200 mesh particles is controlled at 60wt% to obtain biomass composite powder. The mass ratio of biomass composite powder to deionized water was controlled at 62:38. Biomass composite powder was added to deionized water and stirred at 300 rpm for 30 min at room temperature to obtain blank biomass water-based slurry. Biochar-blended polymer powder composite water-based slurry additives prepared in Examples 1-3 and Comparative Examples 1-6 were added to blank biomass water-based slurry, with the amount of additives fixed at 1.2 wt% of the biomass composite powder mass. Stirring was continued for 20 min at 45°C and 400 rpm, followed by high-speed shear homogenization at 6000 rpm for 10 min to break up air bubbles and agglomerated particles. After homogenization, the slurry was filtered through a 100-mesh standard filter to remove trace large particles. It was then naturally cooled to room temperature, sealed, and allowed to stand for 24 h in the dark to mature, yielding the biomass water-based fuel slurry corresponding to each example and comparative example. The blank biomass water-based slurry without any biochar-blended polymer powder composite water-based slurry additive was the blank group.
[0058] II. Performance Test Methods and Judgment Criteria Apparent viscosity and yield stress test at 25℃: The biomass-based fuel slurry and blank group corresponding to the additives prepared in Examples 1-3 and Comparative Examples 1-6 were placed in the test chamber of the rheometer and kept at 25℃ for 5 minutes to eliminate residual shear stress. The shear rate was set to 100 s. -1 The apparent viscosity of the slurry was obtained by steady-state shear testing; the rheological curve of the slurry was measured by stress scanning mode of a rheometer, and the yield stress was calculated by fitting.
[0059] Performance evaluation: The lower the apparent viscosity, the better the slurry flow performance and the lower the pipeline pumping resistance; the lower the yield stress, the easier it is to start the pump.
[0060] 14-day static settling rate test at room temperature: The biomass water-based fuel slurry and blank group corresponding to the additives prepared in Examples 1-3 and Comparative Examples 1-6 were respectively placed into sealed measuring cylinders of the same specifications. The initial total volume of the slurry was recorded. The slurry was sealed and allowed to stand at room temperature for 14 days. After standing, the volume of the upper clarified liquid was read. The slurry settling rate was calculated according to the following formula: Settling rate = (initial total volume of slurry - volume of upper clarified liquid / initial total volume of slurry) × 100%.
[0061] Performance assessment: The smaller the sedimentation rate, the better the dispersion stability of the biomass particles, the better the anti-sedimentation and anti-stratification performance of the slurry, and the better the long-term storage stability.
[0062] High-temperature viscosity retention rate test: First, the initial apparent viscosity of the biomass water-based fuel slurry and blank group corresponding to the additives prepared in Examples 1-3 and Comparative Examples 1-6 was tested at 25℃. Then, the slurry was placed in a constant temperature environment of 90℃ and kept for 30 minutes. After the temperature was maintained, it was naturally cooled to 25℃, and the apparent viscosity of the slurry was tested again. The high-temperature viscosity retention rate was calculated as follows: Viscosity retention rate = (apparent viscosity after high-temperature treatment / initial apparent viscosity) × 100%; Performance assessment: The higher the viscosity retention rate, the less likely the additive is to decompose and fail at high temperatures, and the better the high temperature resistance and heat aging resistance of the slurry, making it suitable for high temperature preparation and combustion conditions.
[0063] Sediment redispersion performance test: After completing the 14-day room temperature static sedimentation test, the sediment slurry formed at the bottom of the measuring cylinder was mechanically stirred at a low speed of 300 rpm for 5 minutes without adding additional water, and the dispersion state of the sediment layer was observed. Evaluation criteria: Divided into three levels: excellent, good, and poor. Specifically: Excellent: The sediment layer is completely dispersed, the slurry returns to a uniform state, and there are no hard lumps; Good: Most of the sediment is dispersed, with a small amount of fine particles agglomerated; Poor: Hard sediment cake is formed and cannot be dispersed by stirring.
[0064] The specific test results are shown in Table 1.
[0065] Table 1 Performance parameters of biochar-blended adhesive powder composite water-based slurry additive As shown in Table 1, the biochar-blended adhesive powder composite water-based slurry additives prepared in Examples 1-3 of this application exhibit excellent comprehensive performance. Compared with the blank group and the comparative examples, the water-based slurry with the biochar-blended adhesive powder composite water-based slurry additive prepared in this application has lower apparent viscosity and yield stress, and lower pumping flow resistance; the 14-day static settling rate at room temperature is significantly reduced, and the particles have good anti-settling and storage stability; moreover, the high-temperature viscosity retention rate is higher, and it is not prone to failure under high-temperature conditions; the slurry sediment can be quickly disintegrated after low-speed stirring, with no hard sediment, indicating excellent redispersibility. This additive has good application prospects.
[0066] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.
Claims
1. A biochar-blended adhesive powder composite water-based slurry additive, characterized in that, The raw materials include the following parts by weight: 20-40 parts modified biochar, 15-30 parts elastic rubber powder, 3-8 parts dispersant, 2-6 parts stabilizer, 3-5 parts heat-resistant modifier, 0.5-2 parts pH adjuster, and 30-50 parts deionized water. The method for preparing the modified biochar includes the following preparation steps: S1. Select agricultural and forestry waste mixed with straw and wood chips, dry and crush it, and then sieve it to obtain biomass powder; S2. Under nitrogen protection, biomass powder is carbonized at high temperature and then cooled to obtain biochar. S3. Activate the biochar by plasma treatment to obtain activated biochar; S4. Add activated biochar to the modified polymer solution and stir to react. After the reaction is complete, filter, wash and dry in sequence to obtain modified biochar. The high-temperature carbonization process in step S2 is specifically as follows: the temperature is increased to 450-550℃ at a heating rate of 5-8℃ / min, and high-temperature carbonization is carried out for 2-4 hours. During the carbonization process, the nitrogen flow rate is controlled at 80-120mL / min. In step S4, the modified polymer solution is composed of polyether-modified polydimethylsiloxane, polyaspartic acid, and deionized water in a mass ratio of 8-12:3-5:80-100; in step S4, the stirring reaction temperature is 55-65℃ and the reaction time is 2-3h.
2. The biochar-blended adhesive powder composite water-based slurry additive according to claim 1, characterized in that, The elastic adhesive powder is composed of ethylene-vinyl acetate copolymer adhesive powder and styrene-butadiene resin powder in a mass ratio of 4-7:1-3.
3. The biochar-blended adhesive powder composite water-based slurry additive according to claim 1, characterized in that, The dispersant is one or more of sodium dodecylbenzenesulfonate, polycarboxylate dispersant, and sodium lignosulfonate; the stabilizer is one or more of hydroxyethyl cellulose, xanthan gum, and carboxymethyl cellulose.
4. The biochar-blended adhesive powder composite water-based slurry additive according to claim 1, characterized in that, The preparation method of the temperature-resistant modifier includes the following preparation steps: Nano-alumina, potassium hexatitanate whiskers, and isopropanol were added to deionized water and ultrasonically treated to obtain an inorganic high-temperature resistant composite dispersion. The inorganic high-temperature resistant composite dispersion was heated to 45-55℃, and glycidyl methacrylate was added dropwise while stirring to react. Then, an organoboron crosslinking agent and waterborne polyurethane emulsion were added and crosslinked at a constant temperature. After the reaction was completed, the mixture was cooled, allowed to stand for aging, dried, pulverized, and sieved to obtain a heat-resistant modifier.
5. The biochar-blended adhesive powder composite water-based slurry additive according to claim 4, characterized in that, The mass ratio of deionized water, nano-alumina, potassium hexatitanate whiskers, and isopropanol is 50-70:8-15:5-10:20-25.
6. The biochar-blended adhesive powder composite water-based slurry additive according to claim 4, characterized in that, The mass ratio of the inorganic high-temperature resistant composite dispersion, glycidyl methacrylate, organic boron crosslinking agent, and waterborne polyurethane emulsion is 80-100:6-12:3-6:15-25.
7. A method for preparing a biochar-blended adhesive powder composite water-based slurry additive as described in any one of claims 1-6, characterized in that, The preparation steps include the following: Dispersant and elastic adhesive powder are added to deionized water and stirred evenly to obtain a stable base liquid. Modified biochar is added to the stable base liquid and stirred evenly. Then, stabilizer is added and stirred evenly again. Then, heat-resistant modifier and pH adjuster are added and stirred to react. After stirring, high-speed homogenization and defoaming treatment is carried out. After filtration and cooling, biochar-blended adhesive powder composite water-based slurry additive is obtained.