Support plate, support tool, and method for manufacturing semiconductor substrate

The use of a support plate and tool with grooves and dummy boards facilitates the formation of high-quality SiC polycrystalline growth layers on semiconductor substrates, addressing the high costs associated with polishing and support materials in semiconductor manufacturing, enabling cost-effective batch production.

JP2024145699AInactive Publication Date: 2024-10-15ROHM CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023058163
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The polishing process for bonding single-crystalline SiC semiconductor substrates to polycrystalline SiC semiconductor substrates is expensive, and the cost of supporting film-forming substrates during chemical vapor deposition (CVD) is high, hindering cost reduction in semiconductor manufacturing.

Method used

A support plate and support tool with grooves and dummy boards are used to support a temporary substrate, allowing for the formation of a SiC polycrystalline growth layer on a semiconductor substrate, which includes a method for forming an SiC epitaxial growth layer on a SiC single crystal substrate, attaching it to a temporary substrate, and then removing it, using a graphite substrate that can be reused.

Benefits of technology

This approach enables the production of high-quality semiconductor substrates at a lower cost by reducing the need for expensive polishing and support materials, allowing for batch processing and reusing the support structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145699000001_ABST
    Figure 2024145699000001_ABST
Patent Text Reader

Abstract

To provide a support tool capable of manufacturing a semiconductor substrate with high quality and at low cost.SOLUTION: A support tool 1 includes: a first dummy substrate 6 and a second dummy substrate 7; and a support 2, supporting the first dummy substrate 6 and the second dummy substrate 7, and including at least three of the support plates 3, 4, 5, the support plate 3, 4, 5 being fitted with the first dummy substrate 6 through a first groove 3a1, 4a1, 5a1 and fitted with the second dummy substrate 7 through a second groove 3a2, 4a2, 5a2 of a plurality of grooves 3a, 4a, 5a. The support 2 supports a temporary substrate 9 inserted into a third groove 3a3, 4a3, 5a3 of the plurality of grooves 3a, 4a, 5a of the support plate 3, 4, 5 excluding the first groove 3a1, 4a1, 5a1 and the second groove 3a2, 4a2, 5a2.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a support plate, a support tool, and a method for manufacturing a semiconductor substrate. [Background technology]

[0002] Conventionally, SiC power devices such as Schottky barrier diodes (SBDs), metal-oxide-semiconductor field effect transistors (MOSFETs), and insulated gate bipolar transistors (IGBTs) have been provided for power control applications. In order to reduce manufacturing costs and provide desired physical properties, SiC semiconductor substrates on which such SiC devices are formed have been fabricated by bonding a single-crystal SiC semiconductor substrate to a polycrystalline SiC semiconductor substrate. Patent Document 1 describes a technique for bonding a single-crystal SiC semiconductor substrate to a polycrystalline SiC semiconductor substrate without defects in order to grow an epitaxial layer on the single-crystal SiC semiconductor substrate bonded to the polycrystalline SiC semiconductor substrate. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] U.S. Patent No. 8,916,451 Summary of the Invention [Problem to be solved by the invention]

[0004] However, the polishing process required to ensure the surface roughness required to attach a single-crystal SiC semiconductor substrate to a polycrystalline SiC semiconductor substrate by room temperature bonding or diffusion bonding is costly, and when manufacturing a polycrystalline SiC semiconductor free-standing substrate by chemical vapor deposition (CVD), the support tool for supporting the film-formed substrate is expensive, making it difficult to achieve the required cost reduction.

[0005] The present disclosure has been proposed in consideration of the above-mentioned circumstances, and aims to provide a support plate and support tool, as well as a method for manufacturing a semiconductor substrate, that enable the provision of semiconductor substrates of high quality and at low cost. [Means for solving the problem]

[0006] A support plate of one embodiment of the present disclosure is a support plate that supports a temporary substrate and enables a SiC polycrystalline growth layer to be formed on a semiconductor substrate supported on a major surface of the temporary substrate, the support plate including a plurality of grooves formed on one edge thereof, the plurality of grooves being configured to support the temporary substrate inserted in an orientation such that the major surface is perpendicular to the direction in which one edge extends.

[0007] A support device according to one embodiment of the present disclosure uses a support plate and includes a first dummy substrate and a second dummy substrate, and pillars supporting the first dummy substrate and the second dummy substrate, the support plate including, for a plurality of grooves, pillars that engage with the first dummy substrate in the first groove and that engage with the second dummy substrate in the second groove, the pillars being configured to support a semiconductor substrate inserted into a third groove, excluding the first groove and the second groove, among the plurality of grooves of the support plate.

[0008] A manufacturing method for a semiconductor substrate according to one embodiment of the present disclosure uses a support tool and includes the steps of forming a SiC epitaxial growth layer on the Si face of a SiC single crystal substrate, attaching the Si face of the SiC epitaxial growth layer to a temporary substrate, removing the SiC epitaxial growth layer from the SiC single crystal substrate, supporting the temporary substrate with the SiC epitaxial growth layer attached thereto with the support tool, forming a SiC polycrystalline growth layer on the C face of the SiC epitaxial growth layer attached to the temporary substrate, removing the temporary substrate with the SiC polycrystalline growth layer formed thereon from the support tool, and removing the temporary substrate. Effect of the Invention

[0009] According to the present disclosure, it is possible to provide a support plate, a support tool, and a method for manufacturing a semiconductor substrate that enable the provision of a high-quality semiconductor substrate at low cost. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 shows an overhead view of the support. [Diagram 2] FIG. 2 shows a front view of the support. [Diagram 3] FIG. 3 shows a plan view of the support. [Figure 4] FIG. 4 shows an overhead view of the support that houses the temporary substrate. [Diagram 5] FIG. 5 shows a front view of the support that houses the temporary substrate. [Figure 6] FIG. 6 shows three views of the support plate. [Figure 7A] FIG. 7A shows a plan view of the dummy substrate. [Figure 7B] FIG. 7B shows a side view of the dummy substrate. [Figure 8] FIG. 8 shows three views of a modified support plate. [Figure 9] FIG. 9 shows a cross-sectional view of a SiC single crystal substrate. [Figure 10A] FIG. 10A shows a plan view illustrating the crystal planes of a SiC wafer. [Figure 10B] FIG. 10B shows a side view illustrating the crystal planes of a SiC wafer. [Figure 11A] FIG. 11A shows an overhead view of a unit cell of a 4H—SiC crystal. [Figure 11B] FIG. 11B shows a schematic diagram of a two-layer portion of a 4H—SiC crystal. [Figure 11C] FIG. 11C shows a schematic diagram of a four-layer portion of a 4H—SiC crystal. [Figure 12] FIG. 12 shows a configuration diagram of the unit cell of the 4H—SiC crystal shown in FIG. 11A, viewed from directly above the (0001) plane. [Figure 13] FIG. 13 shows a cross-sectional view of a structure in which a first graphene layer is formed on a SiC single crystal substrate. [Figure 14]FIG. 14 shows a cross-sectional view of a structure in which a SiC epitaxial growth layer is formed on a first graphene layer. [Figure 15] FIG. 15 shows a cross-sectional view of a structure in which a stress layer is formed on a SiC epitaxial growth layer. [Figure 16] FIG. 16 shows a cross-sectional view of a structure in which a graphite substrate is bonded onto a stress layer via an adhesive layer. [Figure 17A] FIG. 17A shows a cross-sectional view of the SiC epitaxial growth layer side of a structure in which a graphite substrate is bonded onto a stress layer via an adhesive layer, and the SiC epitaxial growth layer and the graphene layer are peeled off at the interface between them. [Figure 17B] FIG. 17B shows a cross-sectional view of the graphene layer side of a structure in which a graphite substrate is bonded onto a stress layer via an adhesive layer, and the SiC epitaxial growth layer and the graphene layer are peeled off at the interface between them. [Figure 18] FIG. 18 shows a cross-sectional view of a structure in which the peelable structure of FIG. 17A is attached to both sides of a graphite substrate and the adhesive layers are carbonized by annealing. [Figure 19] FIG. 19 shows a cross-sectional view of the structure of FIG. 18 supported by a support. [Figure 20] FIG. 20 shows a cross-sectional view of a structure in which a SiC polycrystalline growth layer is formed by the CVD method. [Figure 21] FIG. 21 is a plan view of a structure in which a SiC polycrystalline growth layer is formed by the CVD method. [Figure 22] FIG. 22 shows a cross-sectional view of the structure of FIG. 21 separated from the support. [Figure 23] FIG. 23 shows a cross-sectional view of the structure of FIG. 18 supported by a modified support. [Figure 24] FIG. 24 shows a cross-sectional view of the structure of FIG. 18 removed from the modified support after a SiC polycrystalline growth layer has been formed by CVD. [Diagram 25] FIG. 25 shows a cross-sectional view of the structure after removal of the graphite substrate and the carbonized adhesive layer by combustion. [Figure 26] FIG. 26 shows a cross-sectional view of the structure of a SiC composite substrate after removing the peripheral SiC polycrystalline growth layer and stress layer. [Figure 27]FIG. 27 shows a cross-sectional view of a SiC composite substrate. [Figure 28] FIG. 28 shows an overhead view of a SiC composite substrate (wafer). [Figure 29] FIG. 29 shows a cross-sectional view of a structure in which a hydrogen ion implanted layer is formed on the Si surface of a SiC single crystal substrate. [Diagram 30] FIG. 30 shows a cross-sectional view of a structure in which a thinned single-crystal SiC layer is formed by weakening the hydrogen ion implanted layer through annealing, and then a SiC epitaxial growth layer is formed on the Si surface of the thinned single-crystal SiC layer. [Diagram 31] FIG. 31 shows a cross-sectional view of a structure in which a graphite substrate is attached to the Si surface of a SiC epitaxial growth layer via an adhesive layer. [Diagram 32] FIG. 32 shows a cross-sectional view of a structure that has been peeled off and separated from a SiC single crystal substrate via a thin single crystal SiC layer formed by embrittlement annealing. [Diagram 33] FIG. 33 shows a cross-sectional view of the structure in which the peeled surface of the thinned single crystal SiC layer has been smoothed. [Diagram 34] FIG. 34 shows a cross-sectional view of the structure of FIG. 33 supported by a support. [Diagram 35] FIG. 35 shows a cross-sectional view of a structure in which a SiC polycrystalline growth layer is formed by the CVD method. [Diagram 36] FIG. 36 shows a cross-sectional view of the structure of FIG. 35 separated from the support. [Figure 37] FIG. 37 shows a cross-sectional view of the structure of FIG. 36 after the graphite substrate has been removed by combustion. [Figure 38] FIG. 38 shows a cross-sectional view of a SiC composite substrate obtained by removing the peripheral SiC polycrystalline growth layer and stress layer from the structure in the upper part of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Next, an embodiment will be described with reference to the drawings. In the description of the drawings described below, the same or similar parts are given the same or similar reference numerals. The drawings are schematic. Furthermore, the embodiment shown below is an example of an apparatus or method for embodying a technical idea, and does not specify the material, shape, structure, arrangement, etc. of parts. Various modifications can be made to the embodiment.

[0012] (Support plate and support) Fig. 1 shows an overhead view of a support 1 according to an embodiment. Fig. 2 shows a front view of the support 1, and Fig. 3 shows a plan view of the support 1. The support 1 accommodates and supports a temporary substrate having a main surface on which a semiconductor substrate is supported, and enables a SiC polycrystalline growth layer to be formed on the surface of the semiconductor substrate by CVD. A first support plate 3, a second support plate 4, and a third support plate 5, which are support plates according to an embodiment, constitute a support column 2 that supports the temporary substrate accommodated in the support 1 by surrounding it from three sides.

[0013] The support 1 has a support pillar 2 composed of a first support plate 3, a second support plate 4, and a third support plate 5, and a first dummy substrate 6 and a second dummy substrate 7 fitted with the support pillar 2. The support pillar 2, the first dummy substrate 6, and the second dummy substrate 7 are fitted and fixed to each other to form the support 1. The support 1 forms a space surrounded by the support pillar 2, the first dummy substrate 6, and the second dummy substrate 7 so as to accommodate and support a temporary substrate.

[0014] The first support plate 3, the second support plate 4, and the third support plate 5 constituting the support 2 are rectangular plate-like, and each has a plurality of grooves 3a, 4a, and 5a formed in a comb-like shape along one long side. The first support plate 3, the second support plate 4, and the third support plate 5 are arranged so that one long side is parallel to each other, and a first dummy substrate 6 having a disk-like shape is inserted and fitted into the first groove 3a1, 4a1, and 5a1 at one end along one long side of the plurality of grooves 3a, 4a, and 5a, with its main surface being inserted and fitted in a direction perpendicular to one long side. In addition, a second dummy substrate 7 having a disk-like shape similar to the first dummy substrate 6 is inserted and fitted into the second groove 3a2, 4a2, and 5a2 at the other end along one long side, with its main surface being inserted and fitted in a direction perpendicular to one long side. The first dummy substrate 6 and the second dummy substrate 7 are held parallel to each other by the first support plate 3, the second support plate 4, and the third support plate 5 arranged along the periphery. Among the multiple grooves 3a, 4a, 5a, the third grooves 3a3, 4a3, 5a3 excluding the first grooves 3a1, 4a1, 5a1 and the second grooves 3a2, 4a2, 5a2 receive the temporary substrate and support it in the direction of one long side when the temporary substrate having a disk-like shape like the first dummy substrate 6 and the second dummy substrate 7 is inserted in an orientation such that the bottom surface and / or the bottom surface serving as the main surface is perpendicular to the direction of one long side.

[0015] The support 2 has an opening at the front of the support 1 so that a temporary substrate can be inserted from outside the support 1 into the space surrounded by the support 2, the first dummy substrate 6, and the second dummy substrate 7 and stored therein. Among the first support plate 3, the second support plate 4, and the third support plate 5 constituting the support 2, for example, a pair of the first support plate 3 and the third support plate 5 are arranged at positions facing each other with the first dummy substrate 6 and the second dummy substrate 7 in between, and the remaining second support plate 4 is arranged on one side opposite the front of the support 1 with respect to a plane including the first support plate 3 and the third support plate 5. With such an arrangement of the support 2, it is ensured that a temporary substrate whose main surface has an orientation perpendicular to one long side is inserted from the front of the support 1 toward the second support plate 4 through an opening between the pair of the first support plate 3 and the third support plate 5 of the support 2, and stored in the space surrounded by the support 2, the first dummy substrate 6, and the second dummy substrate 7.

[0016] Fig. 4 shows an overhead view of the support 1 housing the temporary substrates 9. Fig. 5 shows a front view of the support 1 housing the temporary substrates 9. In the support 1, a plurality of temporary substrates 9 are housed in a space surrounded by the support posts 2, the first dummy substrate 6, and the second dummy substrate 7. In this space, the temporary substrates 9 are inserted into the third grooves 3a3, 4a3, and 5a3 of the plurality of grooves 3a, 4a, and 5a, excluding the first grooves 3a1, 4a1, and 5a1 and the second grooves 3a2, 4a2, and 5a2 that fit into the first dummy substrate 6 and the second dummy substrate 7, respectively, with their main surfaces inserted in an orientation perpendicular to one long side, and are supported in the direction of one long side.

[0017] The temporary substrate 9 of the embodiment has a disk-like shape having a predetermined diameter and thickness, and supports the first semiconductor substrate 9a on the bottom surface and the second semiconductor substrate 9b on the top surface as shown in FIG. 5. The temporary substrate 9 is made of graphite, but may be made of other materials such as SiC. The first semiconductor substrate 9a and the second semiconductor substrate 9b are semiconductor substrates of a laminate including a SiC single crystal substrate as described later. The first semiconductor substrate 9a and the second semiconductor substrate 9b are arranged in an area excluding the edge portion up to a predetermined distance from the outer periphery on the bottom surface and the top surface of the temporary substrate 9, respectively. In other words, the bottom surface and the top surface of the temporary substrate 9 form an edge portion where the first semiconductor substrate 9a and the second semiconductor substrate 9b are not arranged in a predetermined range from the outer periphery. In FIG. 5, the first semiconductor substrate 9a and the second semiconductor substrate 9b are supported on the bottom surface and the top surface of the temporary substrate 9, respectively, but the temporary substrate 9 may support only one of the first semiconductor substrate 9a on the bottom surface and the second semiconductor substrate 9b on the top surface.

[0018] FIG. 6 shows a three-view diagram of the first support plate 3. The first support plate 3 is a graphite plate having a rectangular plate shape, and may be, for example, 25 mm×250 mm in length and 2 mm in thickness. A plurality of grooves 3a are formed in a comb shape at a predetermined interval along one long side of the first support plate 3. Among the plurality of grooves 3a, the third groove 3a3, excluding the first groove 3a1 that fits with the first dummy substrate 6 and the second groove 3a2 that fits with the second dummy substrate 7, is formed to a size that supports the inserted temporary substrate 9. For example, the width of the third groove 3a3 can be 2.1 mm when the thickness of the temporary substrate 9 is 2 mm, and the depth can be (diameter of temporary substrate 9)−(diameter of first semiconductor substrate 9a or second semiconductor substrate 9b) / 2−2 mm. The number and pitch of the third grooves 3a3 that support the temporary substrates 9 are adjusted according to the number of temporary substrates 9 to be accommodated in the support 1, the size of the first semiconductor substrate 9a and the second semiconductor substrate 9b, and the like. For example, if the first semiconductor substrate 9a and the second semiconductor substrate 9b are 4-inch wafers and 25 temporary substrates 9 are accommodated in the support 1, the number of third grooves 3a supporting the temporary substrates 9 can be at least 27, and the pitch can be at least 8 mm.

[0019] The first groove 3a1 and the second groove 3a2, which respectively fit the first dummy substrate 6 and the second dummy substrate 7, are formed with a width and depth that allow them to fit the first dummy substrate 6 and the second dummy substrate 7, which are inserted in a direction perpendicular to the direction of one of the long sides, so that the first support plate 3, the first dummy substrate 6, and the second dummy substrate 7 are fitted and fixed to each other without rattling. Note that a SiC coating may be formed on the first support plate 3 by CVD as necessary, and in that case, the width of the groove 3a is set in consideration of the thickness of the SiC coating. Here, the first support plate 3 has been described with reference to FIG. 6, but the same applies to the second support plate 4 and the third support plate 5.

[0020] FIG. 7A shows a plan view of the first dummy substrate 6, and FIG. 7B shows a side view of the first dummy substrate 6. The first dummy substrate 6 is a graphite plate having a disk-like shape, and may have a thickness of, for example, 2 mm or more. The first dummy substrate 6 may be the same size as the temporary substrate 9. Note that, if necessary, a SiC coating may be formed on the first dummy substrate 6 by CVD. Also, the first dummy substrate 6 is not limited to graphite, and may be made of other materials such as SiC. Here, the first dummy substrate 6 has been described with reference to FIG. 7, but the same applies to the second dummy substrate 7.

[0021] The support 1 having the above-mentioned configuration can be assembled by the following procedure. A rectangular graphite plate having a predetermined size is prepared, and a plurality of grooves 3a, 4a, 5a are formed in a comb-like shape with a predetermined pitch, width, and depth along one long side to produce the first support plate 3, the second support plate 4, and the third support plate 5 constituting the support 2. A disk-shaped graphite plate having a predetermined size is also prepared to serve as the first dummy substrate 6 and the second dummy substrate 7. If necessary, a SiC coating may be formed by CVD on the first support plate 3, the second support plate 4, the third support plate 5, and the first dummy substrate 6 and the second dummy substrate 7. Then, the first support plate 3, the second support plate 4, and the third support plate 5 are assembled so that the first grooves 3a1, 4a1, 5a1 and the second grooves 3a2, 4a2, 5a2 formed in the first support plate 3, the second support plate 4, and the third support plate 5 are fitted around the peripheries of the first dummy substrate 6 and the second dummy substrate 7, respectively. In the assembled support 1, the first support plate 3, the second support plate 4 and the third support plate 5 are fixed to one another so that one long side is parallel to each other, and the first dummy substrate 6 and the second dummy substrate 7 are parallel to each other.

[0022] In the embodiment, the first support plate 3, the second support plate 4, and the third support plate 5 have a rectangular plate shape, but are not limited to a rectangular plate shape as long as they are columnar members capable of forming the support 2 of the support 1 and have a plurality of grooves formed on one edge. In the first support plate 3, the second support plate 4, and the third support plate 5, the first groove 3a1, 4a1, 5a1 for fitting the first dummy substrate 6 is formed at one end along one long side among the plurality of grooves 3a, 4a, 5a formed on one long side of the rectangular plate-shaped first support plate 3, the second support plate 4, and the third support plate 5, and the second groove 3a2, 4a2, 5a2 for fitting the second dummy substrate 7 is formed at the other end along one long side among the plurality of grooves 3a, 4a, 5a, but are not limited to these positions. The first grooves 3a1, 4a1, 5a1 and the second grooves 3a2, 4a2, 5a2 may be included in the multiple grooves 3a, 4a, 5a, and the third grooves 3a3, 4a3, 5a3 supporting the temporary substrate 9 may be the remaining grooves 3a, 4a, 5a among the multiple grooves 3a, 4a, 5a excluding the first grooves 3a1, 4a1, 5a1 which fit the first dummy substrate 6 and the second grooves 3a2, 4a2, 5a2 which fit the second dummy substrate 7.

[0023] Although the first dummy substrate 6 and the second dummy substrate 7 have been described as having a disk shape, they may be other shapes, such as a rectangular plate, so long as they are similar in shape to the temporary substrate 9 housed in the support 1. Furthermore, the first dummy substrate 6 and the second dummy substrate 7 are not limited to being one piece each, and the first dummy substrate 6 and the second dummy substrate 7 may each be formed by stacking a plurality of substrates.

[0024] The temporary substrate 9 supports the first semiconductor substrate 9a and the second semiconductor substrate 9b on its bottom and top surfaces, which serve as its main surfaces, respectively. However, the semiconductor substrates supported by the temporary substrate 9 may be only the first semiconductor substrate 9a on the bottom surface, or only the second semiconductor substrate 9b on the top surface.

[0025] As described above, the first support plate 3, the second support plate 4, and the third support plate 5 of the embodiment are inexpensive because they are made of graphite plates. In addition, the support 1 of the embodiment is inexpensive because it is made of the first support plate 3, the second support plate 4, and the third support plate 5 made of graphite plates, and the first dummy substrate 6 and the second dummy substrate 7 also made of graphite plates. Therefore, when a SiC polycrystalline growth layer is formed by CVD on the first semiconductor substrate 9a and the second semiconductor substrate 9b supported by the temporary substrate 9 in the support 1, the support 1 can be separated and disposable together with the end of the temporary substrate 9 fixed to the support 1. Since the support 1 is inexpensive and disposable in this way, the cost of the manufacturing method of the semiconductor substrate can also be reduced.

[0026] The support 1 of the embodiment can accommodate a plurality of temporary substrates 9, each having a first semiconductor substrate 9a and a second semiconductor substrate 9b supported on its bottom and top surfaces, in a space surrounded by the support 2, the first dummy substrate 6, and the second dummy substrate 7. In the support 1, the plurality of temporary substrates 9 are supported at a predetermined interval by third grooves 3a3, 4a3, and 5a3 formed on one long side of the first support plate 3, the second support plate 4, and the third support plate 5 constituting the support 2. In addition, the plurality of temporary substrates 9 supported by the support 1 are open in the in-plane direction of the main surface, except for the direction blocked by the first support plate 3, the second support plate 4, and the third support plate 5 of the support 2. For this reason, a uniform atmosphere can be provided for the plurality of temporary substrates 9 accommodated in the support 1 in the CVD process, and a high-quality SiC polycrystalline growth layer 16 can be formed on the first semiconductor substrate 9a and the second semiconductor substrate 9b supported on the bottom and top surfaces of the temporary substrate 9, respectively. Furthermore, the support 1 can accommodate a plurality of temporary substrates 9, and the temporary substrates 9 support a first semiconductor substrate 9a and a second semiconductor substrate 9b on their bottom and top surfaces, respectively. This allows the CVD processing of a large number of semiconductor substrates to be performed in a batch, thereby reducing the cost of the semiconductor substrate manufacturing method.

[0027] Next, a description will be given of a support 1 according to a modification of the embodiment. The support 1 according to the modification is different from the support 1 according to the embodiment in that an expanded graphite sheet is attached to a range including the third grooves 3a3, 4a3, 5a3 that support the temporary substrate 9 in a region where a plurality of grooves 3a, 4a, 5a are formed in a comb shape on one long side of the first support plate 3, the second support plate 4, and the third support plate 5, but the other configurations are the same as the support 1 according to the embodiment.

[0028] FIG. 8 shows the first support plate 3 of the modified example. The first support plate 3 of the modified example is a graphite plate having a rectangular plate shape, similar to the first support plate of the embodiment, and a plurality of grooves 3a are formed in a comb shape at a predetermined interval along one long side. The first support plate 3 of the modified example has an expanded graphite sheet 8 attached to a range including the third groove 3a3 supporting the temporary substrate 9, excluding the first groove 3a1 and the second groove 3a2 that fit with the first dummy substrate 6 and the second dummy substrate 7, respectively, among the plurality of grooves 3a formed along one long side. The expanded graphite sheet 8 is formed by pressing expanded graphite obtained by expanding a laminate of graphene, and has properties such as being very soft and flexible, excellent in compressive strength, elasticity, and heat resistance, and is used as a sealing material that requires heat resistance. In the first support plate 3 of the modified example, the expanded graphite sheet 8 is attached to a region including the third groove 3a3 along one long side, so that the gap between the third groove 3a3 and the inserted temporary substrate 9 can be filled.

[0029] In the first support plate 3 of the modified example, the expanded graphite sheet 8 fills the gap between the third groove 3a3 and the temporary substrate 9, so that when a SiC polycrystalline growth layer is formed by CVD on the surfaces of the first semiconductor substrate 9a and the second semiconductor substrate 9b supported by the temporary substrate 9, the SiC polycrystalline growth layer is prevented from being formed between the temporary substrate 9 and the third groove 3a, and the temporary substrate 9 and the third groove 3a3 are prevented from being fixed to each other. Even when a SiC polycrystalline growth layer is formed between the temporary substrate 9 and the first support plate 3 via the graphite substrate 19 inserted into the third groove 3a3, and the graphite substrate 19 and the first support plate 3 are fixed to each other, the expanded graphite sheet 8 is attached to a range including the third groove 3a3 along one long side, and the SiC polycrystalline growth layer is formed on the first support plate 3 with the expanded graphite sheet 8 interposed therebetween, so that the SiC polycrystalline growth layer can be easily removed by peeling off the expanded graphite sheet 8 along the graphene layer. In this manner, in the modified example, the first support plate 3 can be removed from the temporary substrate 9 after the CVD process and can be used repeatedly. Therefore, in the modified example, the cost of the semiconductor manufacturing method can be reduced. Here, the first support plate 3 of the modified example has been described with reference to Fig. 8, but the same applies to the second support plate 4 and the third support plate 5 of the modified example.

[0030] (Method of manufacturing semiconductor substrate) Next, a description will be given of a method for manufacturing a semiconductor substrate using the support 1 of the embodiment. The semiconductor manufacturing method of the embodiment uses a remote epitaxial method that enables peeling of the SiC epitaxial growth layer transferred via the graphene layer by forming an SiC epitaxial growth layer on the surface of a SiC single crystal substrate serving as a seed substrate via a graphene layer, and uses the support 1 of the embodiment in a process of forming a SiC polycrystalline growth layer by CVD.

[0031] FIG. 9 is a cross-sectional view of a SiC single crystal substrate (SiCSB) 11 serving as a seed crystal. In the embodiment, the SiC single crystal substrate 11 will be described taking a 4H-SiC substrate as an example, but it may be either a hexagonal crystal system (4H, 6H) or a cubic crystal system (3C). The thickness of the SiC single crystal substrate 11 may be, for example, about 300 μm to 600 μm. In FIG. 9, [C] indicates the C-face of SiC, and [S] indicates the Si-face of SiC. The same applies to the following figures.

[0032] Fig. 10 is a diagram for explaining the crystal planes of a SiC wafer 110 applicable as a SiC single crystal substrate 11. The plan view of Fig. 10A shows a Si surface 113 of a SiC wafer 110 on which a primary orientation flat 111 and a secondary orientation flat 112 are formed. In the side view of Fig. 10B seen from the [-1100] orientation, a Si surface 113 with a

[0001] orientation is formed on the upper surface, and a C surface 114 with a [000-1] orientation is formed on the lower surface.

[0033] A schematic overhead configuration of a unit cell of a 4H-SiC crystal is shown as in Fig. 11A, a schematic configuration of a two-layer portion of a 4H-SiC crystal is shown as in Fig. 11B, and a schematic configuration of a four-layer portion of a 4H-SiC crystal is shown as in Fig. 11C. Moreover, a schematic configuration of the unit cell of the 4H-SiC crystal structure shown in Fig. 11A viewed from directly above the (0001) plane is shown as in Fig. 12.

[0034] As shown in Fig. 11A to Fig. 11C, the crystal structure of 4H-SiC can be approximated by a hexagonal system, in which one Si atom is bonded to four C atoms. The four C atoms are located at the four vertices of a regular tetrahedron with a Si atom at the center. Of these four C atoms, one Si atom is located in the

[0001] axial direction relative to the C atom, and the other three C atoms are located on the [000-1] axial side relative to the Si atom. In Fig. 11A, the off-angle θ is, for example, about 4 degrees or less.

[0035] The

[0001] and [000-1] axes are aligned along the axial direction of the hexagonal prism, and the surface (top surface of the hexagonal prism) normalized to the

[0001] axis is the (0001) surface (Si surface). Meanwhile, the surface (bottom surface of the hexagonal prism) normalized to the [000-1] axis is the (000-1) surface (C surface). In addition, the directions perpendicular to the

[0001] axis and passing through non-adjacent vertices of the hexagonal prism when viewed from directly above the (0001) surface are the a1 axis [2-1-10], a2 axis [-12-10], and a3 axis [-1-120], respectively.

[0036] As shown in FIG. 12, the direction passing through the vertex between the a1 axis and the a2 axis is the [11-20] axis, the direction passing through the vertex between the a2 axis and the a3 axis is the [-2110] axis, and the direction passing through the vertex between the a3 axis and the a1 axis is the [1-210] axis. Between each of the six axes passing through each vertex of the hexagonal prism, the axes inclined at an angle of 30° to the axes on both sides and normal to each side of the hexagonal prism are, in order clockwise from between the a1 axis and the [11-20] axis, the [10-10] axis, the [1-100] axis, the [0-110] axis, the [-1010] axis, the [-1100] axis, and the [01-10] axis. Each face (side face of the hexagonal prism) having these axes as normals is a crystal face perpendicular to the (0001) plane and the (000-1) plane.

[0037] 13, a graphene layer (GR) 12 of up to several molecular layers is formed on the (0001) Si surface of the SiC single crystal substrate 11. The graphene layer 12 can be formed by pyrolysis on the Si surface of the SiC single crystal substrate 11 by annealing the SiC single crystal substrate 11 at about 1700° C. in an argon gas atmosphere at atmospheric pressure. The graphene layer 12 may also be formed by stacking on the SiC single crystal substrate 11 by CVD.

[0038] The graphene layer 12 has a stacked structure of graphite sheets. The graphite sheets on each side of the stacked structure have many hexagonal carbon (C) covalent bonds, and the graphite sheets on each side are bonded by van der Waals forces. The graphene layer 12 may be a 0 layer as a buffer layer, or a single layer structure.

[0039] As shown in Fig. 14, a SiC epitaxial growth layer (SiC-epi) 13 is formed on a graphene layer 12. The SiC epitaxial growth layer 13 is formed by remote epitaxial growth on the graphene layer 12 formed on the Si surface of a SiC single crystal substrate 11. The SiC epitaxial growth layer 13 is a single crystal SiC thin film. The surface of the SiC epitaxial growth layer 13 in contact with the graphene layer 12 is the C-plane, and the surface of the SiC epitaxial growth layer 13 is the Si-plane.

[0040] As shown in FIG. 15, a stress layer 14 is formed on a SiC epitaxial growth layer 13. The stress layer 14 is made of a nickel (Ni) thin film. The nickel thin film may be formed by vapor deposition or plating. The stress layer 14 is adjusted to a size such that the internal stress facilitates peeling of the graphene layer 12 and the SiC epitaxial growth layer 13. Therefore, the stress generated between the graphene layer 12 and the SiC epitaxial growth layer 13 facilitates peeling of the graphene layer 12 and the SiC epitaxial growth layer 13.

[0041] Next, as shown in FIG. 16, an adhesive layer 15 is formed on the stress layer 14, and the applied surface of the adhesive layer 15 is attached to one or both sides of a graphite substrate 19, which is a temporary substrate having an outer size slightly larger than that of the SiC single crystal substrate 11, to form a first composite (11 (SiCSB), 12 (GR), 13 (SiC-epi), 14, 15, 19). For example, a carbon adhesive may be used for the adhesive layer 15. The carbon adhesive is an adhesive that contains phenol resin and can maintain its bonding strength even at high temperatures by carbonizing the adhesive itself. The graphite substrate 19 may be in the form of a disk or a rectangular plate. The graphite substrate 19 having an outer size slightly larger than that of the SiC single crystal substrate 11 may have an outer size of 1 mm or more larger than that of the SiC single crystal substrate 11. For example, if the SiC single crystal substrate 11 has a diameter of about 10 cm, a graphite substrate 19 having an outer size approximately 10 mm larger than that of the SiC single crystal substrate 11 may have a diameter of about 11 cm. For example, if the SiC single crystal substrate 11 has a diameter of about 15 cm, a graphite substrate 19 having an outer diameter of about 16 cm may be used.

[0042] Then, the first composite is heated in an inert gas atmosphere in a thermal annealing furnace or the like to carbonize the adhesive layer 15. At this time, by gradually heating with a temperature gradient that allows the gas generated when the carbon adhesive of the adhesive layer 15 decomposes to be gradually removed, the adhesive surface is prevented from peeling off when the adhesive layer 15 is carbonized. The graphite substrate 19 may have a glassy carbon coating on its surface. Since the glassy carbon coating has a strong adhesive force with the carbon adhesive of the adhesive layer 15, it is possible to easily peel off the SiC epitaxial growth layer 13 from the graphene layer 12 and the SiC single crystal substrate 11, and the yield can be improved. Note that, although FIG. 10 shows an example in which the adhesive layer 15 is attached to one side of the graphite substrate 19 to form the first composite, the adhesive layer 15 may be attached to both sides of the graphite substrate 19 to form the first composite.

[0043] As shown in Fig. 17, after carbonizing the adhesive layer 15 of the first composite of Fig. 16, the SiC epitaxial growth layer 13 is physically peeled off and separated from the graphene layer 12 interface on one or both sides of the first composite using an adhesive peeling tape, a debonder device, or the like. Fig. 17A is a cross-sectional view of the structure peeled off to the SiC epitaxial growth layer 13 side from the first composite shown in Fig. 16, and Fig. 17B is a cross-sectional view of the structure peeled off to the graphene layer 12 side. The peeled structure on the SiC epitaxial growth layer 13 side shown in Fig. 17A forms a second composite (13 (SiC-epi), 14, 15, 19). The graphene layer 12 is bonded by van der Waals forces, and the stress generated by the stress layer 14 is adjusted to a magnitude that facilitates peeling of the graphene layer 12 and the SiC epitaxial growth layer 13. Therefore, by applying a force in the shear direction, peeling can be easily caused at the interface between the graphene layer 12 and the SiC epitaxial growth layer 13.

[0044] In the structure shown in FIG. 17B where the graphene layer 12 is peeled off, the graphene layer 12 on the SiC single crystal substrate 11 is removed by etching or polishing. In the etching process of the graphene layer 12, for example, a plasma asher using oxygen plasma can be applied. Since the Si surface of the SiC single crystal substrate 11 from which the graphene layer 12 has been etched by oxygen plasma is oxidized, wet etching using hydrogen fluoride (HF) is performed. In the polishing process of the graphene layer 12, the graphene layer 12 is removed by, for example, chemical mechanical polishing (CMP). Here, the Si surface of the SiC single crystal substrate 11 has an average surface roughness Ra of, for example, about 1 nm or less due to the above-mentioned wet etching process. As a result, the SiC single crystal substrate 11 becomes reusable.

[0045] 18 shows an example in which the release structure of FIG. 11A is attached to both sides of a graphite substrate 19, and SiC epitaxial growth layers 131, 132 are formed on both sides. In this case, the second composite (131 (SiC-epi), 141, 151, 19, 152, 142, 132 (SiC-epi)) is heated in a thermal annealing furnace to carbonize the adhesive layers 151, 152.

[0046] As shown in FIG. 19, the second composite is accommodated in the support 1 of the embodiment. As shown in FIG. 1 to FIG. 3, the support 1 has a space in which the second composite including the graphite substrate 19 of the temporary substrate 9 can be accommodated by the first support plate 3, the second support plate 4, and the third support plate 5 constituting the support 2, and the first dummy substrate 6 and the second dummy substrate 7. The third grooves 3a3, 4a3, and 5a3 among the multiple grooves 3a, 4a, and 5a formed in a comb-like shape along one long side of the first support plate 3, the second support plate 4, and the third support plate 5 can support the graphite substrate 19 of the inserted second composite in the direction of one long side. As shown in FIG. 4 and FIG. 5, the second composite is accommodated by being inserted from the front side of the support 1 into the opening formed by the first support plate 3, the third support plate 5, the first dummy substrate 6, and the second dummy substrate 7 in an orientation such that the main surface of the graphite substrate 19 is perpendicular to one long side. The second complex is supported in the direction of one of its long sides by graphite substrate 19 inserted into third grooves 3a3, 4a3, 5a3, and a predetermined distance is maintained between the second complex, first dummy substrate 6, or second dummy substrate 7 adjacent thereto.

[0047] As shown in FIG. 20, a SiC polycrystalline growth layer 16 is formed on the (000-1) C plane of the SiC epitaxial growth layers 131, 132 provided on one or both sides of the second composite. The SiC polycrystalline growth layer 16 can be formed by CVD technology. After the support 1 containing the second composite is placed in a CVD furnace, the furnace is evacuated and heated to about 1400°C to 1500°C. Then, the SiC polycrystalline growth layer 16 is deposited by simultaneously flowing, as material gases, SiCl4 (silicon tetrachloride) gas, CH4 (methane) gas, and H2 (hydrogen) gas, and adjusting the pressure. The SiC polycrystalline growth layer 16 has a 3C (cubic) structure. The thickness of the deposited SiC polycrystalline growth layer 16 can be set according to the thickness of the final SiC composite substrate. For example, when the overall thickness of the SiC composite substrate is to be 350 μm, if the thickness of the SiC epitaxial growth layer 13 is 10 μm, the deposited thickness of the SiC polycrystalline growth layer 16 may be set to 340 μm.

[0048] 20, a third composite (16 (SiC-poly CVD), 131 (SiC-epi), 141, 151, 19, 152, 142, 132 (SiC-epi), 16 (SiC-poly CVD)) is formed by depositing a SiC polycrystalline growth layer 16 on the second composite. The third composite is fixed to the support 1 by the SiC polycrystalline growth layer 16 extending from the graphite substrate 19 to the support 1 it contains.

[0049] As shown in the plan view of Fig. 21, the graphite substrate 19 and the SiC polycrystalline growth layer 16 are cut along the cutting line C2 between the third composite and the second support plate 4 as well as the cutting line C1 between the third composite and the first support plate 3 and the cutting line C3 between the third composite and the third support plate 5 shown in Fig. 20, thereby separating the third composite from the support 1. A chain saw may be used to cut the graphite substrate 19 and the SiC polycrystalline growth layer 16 along the cutting lines C1, C2, and C3. After separating the third composite, the remaining support 1 to which the graphite substrate 19 and the like are fixed is disposed of.

[0050] 22 shows the third composite separated from the support 1. The third composite was separated by cutting the graphite substrate 19 inserted in the third grooves 3a3, 4a3, 5a3 of the first support plate 3, the second support plate 4, and the third support plate 5, together with the SiC polycrystalline growth layer 16 formed and extending on the support 1. As a result, the cut surface of the graphite substrate 19 is exposed from the third composite.

[0051] As shown in Fig. 23, the second composite can also be accommodated in the modified support 1. In the modified support 1, as shown in Fig. 8, the expanded graphite sheets 8 are attached to the ranges including the third grooves 3a3, 4a3, and 5a3 that support the graphite substrate 19 among the multiple grooves 3a formed along one long side of the first support plate 3, the second support plate 4, and the third support plate 5. Even when the modified support 1 is used, the SiC polycrystalline growth layer 16 is deposited on the second composite, thereby forming the third composite (16 (SiC-poly CVD), 131 (SiC-epi), 141, 151, 19, 152, 142, 132 (SiC-epi), 16 (SiC-poly CVD)).

[0052] In the modified support 1, the expanded graphite sheet 8 fills the gaps between the graphite substrate 19 and the third grooves 3a3, 4a3, 5a3. Therefore, when the SiC polycrystalline growth layer 16 is formed in the second composite, the SiC polycrystalline growth layer 16 is formed between the graphite substrate 19 and the third grooves 3a3, 4a3, 5a3, preventing adhesion between the temporary substrate 9 and the third grooves 3a3, 4a3, 5a3. In addition, even when the SiC polycrystalline growth layer 16 is formed between the graphite substrate 19 and the first support plate 3, the second support plate 4, and the third support plate 5, and the graphite substrate 19 is fixed to the first support plate 3, the second support plate 4, and the third support plate 5, the expanded graphite sheet 8 is attached along one long side in an area including the third grooves 3a3, 4a3, and 5a3, so that the SiC polycrystalline growth layer 16 is formed on the first support plate 3, the second support plate 4, and the third support plate 5 with the expanded graphite sheet 8 interposed therebetween, and can be easily removed by peeling off the expanded graphite sheet 8 along the graphene layer. The support 1 of the modified example can be reused after the formed SiC polycrystalline growth layer 16 is removed.

[0053] Fig. 24 is a diagram showing the third composite removed from the support 1 of the modified example. The SiC polycrystalline growth layer 16 formed and extending from the graphite substrate 19 to the support 1 has also been removed from the support 1 of the modified example together with the third composite. The SiC polycrystalline growth layer 16 extending from the third composite to the support 1 along the graphite substrate 19 is unnecessary, so it is cut and removed along the cutting lines C1, C2 in the figure, etc., to obtain the third composite as shown in Fig. 22.

[0054] As shown in Fig. 25, the third composite with the exposed graphite substrate 19 shown in Fig. 22 is heated to about 900°C to 1000°C in an atmospheric furnace capable of heating in an atmospheric atmosphere while flowing air, so that the graphite substrate 19 and the carbonized adhesive layers 151 and 152 inside the third composite are burned and completely removed. Then, the fourth composite (16 (SiC-poly CVD), 131 (siC-epi), 141, 142, 132 (SiC-epi), 162 (SiC-poly CVD)) is taken out.

[0055] 26, the SiC polycrystalline growth layers 161, 162 on the periphery of the fourth composite are removed by grinding and polishing with a beveling device, and the stress layers 141, 142 are removed by etching or polishing, thereby obtaining a SiC composite substrate 10 configured by laminating the SiC polycrystalline growth layer 161 and the SiC epitaxial growth layer 131, and a SiC composite substrate 10 configured by laminating the SiC epitaxial growth layer 132 and the SiC polycrystalline growth layer 162. Furthermore, these SiC composite substrates 10 are processed to the required dimensions and surface condition.

[0056] As shown in Fig. 27, the SiC composite substrate 10 is configured by laminating a SiC polycrystalline growth layer (SiC-poly CVD) 16 and a SiC epitaxial growth layer (SiC-epi) 13. Fig. 28 is a schematic bird's-eye view of the SiC composite substrate (wafer) 10. In the SiC composite substrate 10, the surface of the SiC epitaxial growth layer 13 may be a Si face of 4H-SiC with a

[0001] orientation, and the face in contact with the SiC polycrystalline growth layer 16 may be a C face of 4H-SiC with a [000-1] orientation.

[0057] As described above, in the manufacturing method of the semiconductor of the embodiment, in the step of forming the SiC polycrystalline growth layer 16 on the SiC epitaxial growth layer 13 by CVD, the graphite substrate 19 serving as the temporary substrate 9 supporting the SiC epitaxial growth layer 13 is accommodated in the support 1 of the embodiment. The support 1 of the embodiment is inexpensive because it is composed of the first support plate 3, the second support plate 4, and the third support plate 5 made of graphite plates, and the first dummy substrate 6 and the second dummy substrate 7 also made of graphite plates. Therefore, after the SiC polycrystalline growth layer is formed on the first semiconductor substrate 9a and the second semiconductor substrate 9b supported by the temporary substrate 9 in the support 1 by CVD, the support 1 can be cut off together with the end of the graphite substrate 19 fixed thereto and can be used for disposal. Since the support 1 is inexpensive and disposable in this way, the cost of the manufacturing method of the semiconductor substrate can also be reduced.

[0058] In the semiconductor manufacturing method of the embodiment, the support 1 of the embodiment used in the step of forming the SiC polycrystalline growth layer 16 on the SiC epitaxial growth layer 13 by CVD can accommodate a plurality of temporary substrates 9 having the first semiconductor substrate 9a and the second semiconductor substrate 9b supported on the bottom and top surfaces, respectively, in a space surrounded by the support 2, the first dummy substrate 6, and the second dummy substrate 7. In the support 1, the plurality of temporary substrates 9 are supported at a predetermined interval by the third grooves 3a3, 4a3, and 5a3 formed on one long side of the first support plate 3, the second support plate 4, and the third support plate 5 constituting the support 2. In addition, the graphite substrates 19 of the plurality of temporary substrates 9 supported by the support 1 are open in the in-plane direction of the main surface except for the direction blocked by the first support plate 3, the second support plate 4, and the third support plate 5 of the support 2. Therefore, a uniform atmosphere can be provided in the CVD process for the multiple temporary substrates 9 housed in the support 1, and a high-quality SiC polycrystalline growth layer 16 can be formed on the first semiconductor substrate 9a and the second semiconductor substrate 9b supported on the bottom and top surfaces of the temporary substrates 9, respectively. Furthermore, the support 1 can house multiple temporary substrates 9, and the temporary substrates 9 support the first semiconductor substrate 9a and the second semiconductor substrate 9b on their bottom and top surfaces, respectively. Therefore, the CVD process can be performed on a large number of semiconductor substrates in a batch, and the cost of the semiconductor substrate manufacturing method can be reduced.

[0059] According to the semiconductor manufacturing method of the embodiment, before forming SiC polycrystalline growth layer 16 by CVD method, SiC single crystal substrate 11 is separated and replaced with graphite substrate 19, which is a highly heat-resistant temporary substrate, thereby preventing unnecessary adhesion of SiC polycrystals to SiC single crystal substrate 11, improving the reusability of SiC single crystal substrate 11, and enabling cost reduction.

[0060] According to the semiconductor manufacturing method of the embodiment, by using graphite substrate 19, which is a highly heat-resistant temporary substrate that is slightly larger than SiC single crystal substrate 11, it is inserted into support 1 of the embodiment and stored therein, enabling one-sided or two-sided epitaxial growth, and achieving high throughput and low-cost production without increasing the growth rate.

[0061] According to the semiconductor manufacturing method of the embodiment, by carbonizing a highly heat-resistant substrate such as graphite substrate 19 and adhesive layer 15, the semiconductor substrate structures formed on both sides of graphite substrate 19 can be separated inexpensively by simply baking them in an oxidation furnace or the like.

[0062] According to the semiconductor manufacturing method of the embodiment, remote epitaxial growth of SiC is performed via graphene formed on the SiC single crystal substrate 11, and the SiC polycrystalline growth layer 16 and the like are formed directly thereon by CVD, which makes substrate bonding unnecessary and eliminates defects caused by substrate bonding. In addition, since the epitaxial growth layer is formed via the graphene layer 12, it becomes easy to separate the SiC single crystal substrate 11 and the SiC epitaxial growth layer 13, simplifying the process steps.

[0063] According to the semiconductor manufacturing method of the embodiment, after the SiC single crystal substrate is removed, the support 1 with the graphite substrate 19, which is a highly heat-resistant handle substrate, inserted therein is placed in a high-temperature LP-CVD apparatus, and the SiC polycrystalline growth layer 16 and the like are grown directly on the SiC epitaxial growth layer 13. This eliminates the steps of transporting the epitaxial growth layer having a thickness of several μm from the handle substrate to the support substrate and bonding it to the support substrate, thereby making it possible to avoid defects such as wrinkles, crystal transition, and voids due to thin film transportation and bonding.

[0064] According to the semiconductor manufacturing method of the embodiment, the graphene layer 12 formed on the SiC single crystal substrate 11 is not transferred, but epitaxial growth is performed directly on the graphene layer 12. This makes it possible to avoid defects such as wrinkles and cracks caused by the transfer of graphene.

[0065] According to the semiconductor manufacturing method of the embodiment, since the SiC single crystal substrate 11 is used as a base, hexagonal SiC with little deterioration in crystallinity can be obtained. In addition, the SiC single crystal substrate 11 is expensive and difficult to remove by polishing or etching, but by using remote epitaxial growth via the graphene layer 12, the obtained high-performance single crystal layer can be easily separated, making removal by polishing or etching unnecessary. Since the expensive SiC single crystal substrate 11 can be reused after separation, a large cost advantage is obtained.

[0066] The SiC epitaxial growth layer 13 may include at least one type or a plurality of types selected from the group consisting of Group IV element semiconductors, Group III-V compound semiconductors, and Group II-VI compound semiconductors.

[0067] Furthermore, the SiC single crystal substrate 11 and the SiC epitaxial growth layer 13 may be made of any one of 4H-SiC, 6H-SiC, and 2H-SiC materials.

[0068] Furthermore, the SiC single crystal substrate 11 and the SiC epitaxial growth layer 13 may comprise, as a material other than SiC, at least one selected from the group consisting of GaN, BN, AlN, Al2O3, Ga2O3, diamond, carbon, and graphite.

[0069] The SiC composite substrate 10 uses a low-cost SiC polycrystalline growth layer 16 instead of a high-cost SiC single crystal substrate 11 on the Si surface that serves as the device surface.

[0070] (Modification of semiconductor manufacturing method) Next, a modified example of the semiconductor manufacturing method of the embodiment will be described. The modified semiconductor manufacturing method uses a hydrogen ion implantation delamination method that implants hydrogen ions into a SiC single crystal substrate to form an embrittled layer, thereby enabling delamination of a thinned layer on the surface. The modified semiconductor manufacturing method is the same as the semiconductor manufacturing method of the embodiment, except that the hydrogen ion implantation delamination method is used in the manufacturing method of the semiconductor substrate.

[0071] Hydrogen ions are implanted into the Si surface of the SiC single crystal substrate (SiCSB) 11 shown in Fig. 9 for the ion implantation delamination method to form a hydrogen ion implanted layer 11c having a specified depth (for example, about 1 µm). Fig. 29 shows the SiC single crystal substrate 11 on which the hydrogen ion implanted layer 11c has been formed. Here, the ion implantation conditions are, for example, an acceleration energy of about 100 keV and a dose of about 2.0 × 10 17 / cm 2 The hydrogen ion implanted layer 11c is then subjected to a high temperature treatment to embrittle the hydrogen ion implanted layer 11c. After the hydrogen ion implantation, embrittlement thermal annealing is required to generate hydrogen microbubbles and make the hydrogen ion implanted layer 11c easier to break.

[0072] As shown in Fig. 30, a SiC epitaxial growth layer 13 is formed by CVD on the Si surface of the hydrogen ion implanted layer 11c. Then, as shown in Fig. 31, a graphite substrate 19 serving as a temporary substrate is attached to the Si surface of the SiC epitaxial growth layer 13 via an adhesive layer 15 made of a carbon adhesive, and the adhesive layer 15 is carbonized by heating in a thermal annealing furnace or the like.

[0073] The embrittled hydrogen ion implanted layer 11c is divided along the separation surface indicated by the line BB in FIG. 31, and the SiC single crystal substrate 11 is removed. As shown in FIG. 32, the side of the divided hydrogen ion implanted layer 11c in contact with the SiC epitaxial growth layer 13 forms a thinned SiC single crystal layer 11d formed by thinning the SiC single crystal substrate 11. Meanwhile, the uneven structure formed by separation on the Si surface of the main body of the SiC single crystal substrate 11 divided by the hydrogen ion implanted layer 11c is smoothed by mechanical polishing, mechanical chemical polishing, or the like. The average surface roughness Ra of the Si surface of the SiC single crystal substrate 11 is reduced to, for example, about 1 nm or less by the above process. As a result, the SiC single crystal substrate 11 becomes reusable.

[0074] As shown in Fig. 33, the peeled surface of the laminate of the thinned SiC single crystal layer 11d and the SiC epitaxial growth layer 13 bonded to the graphite substrate 19 has an uneven structure smoothed out by mechanical polishing, mechanical chemical polishing, etc. The structure shown in Fig. 33 forms a fifth composite (19, 15, 13 (SiC-epi), 11d).

[0075] As shown in FIG. 34, the fifth composite is accommodated in the support 1 of the embodiment. As shown in FIG. 1 to FIG. 3, the support 1 has a space in which the fifth composite including the graphite substrate 19 of the temporary substrate 9 can be accommodated by the first support plate 3, the second support plate 4, and the third support plate 5 constituting the support 2, and the first dummy substrate 6 and the second dummy substrate 7. The third grooves 3a3, 4a3, and 5a3 among the multiple grooves 3a, 4a, and 5a formed in a comb-like shape along one long side of the first support plate 3, the second support plate 4, and the third support plate 5 can support the graphite substrate 19, which becomes the temporary substrate 9 of the inserted fifth composite, in the direction of one long side. As shown in FIG. 4 and FIG. 5, the fifth composite is accommodated by being inserted from the front side of the support 1 into the opening formed by the first support plate 3, the third support plate 5, the first dummy substrate 6, and the second dummy substrate 7 in an orientation such that the main surface of the graphite substrate 19 is perpendicular to one long side. The fifth complex is supported in the direction of one of its long sides by graphite substrate 19 inserted into third grooves 3a3, 4a3, 5a3, and a predetermined distance is maintained between the fifth complex, the first dummy substrate 6, or the second dummy substrate 7 adjacent thereto.

[0076] 35, a sixth composite (16 (SiC-poly CVD), 19, 15, 13 (SiC-epi), 11c, 16 (SiC-poly CVD)) is formed by forming a SiC polycrystalline growth layer 16 by CVD technology on the C-face of the thinned SiC single crystal layer 11d of the fifth composite. The sixth composite is fixed to the support 1 by the SiC polycrystalline growth layer 16 extending from the graphite substrate 19 to the support 1 it contains.

[0077] 35, the graphite substrate 19 and the SiC polycrystalline growth layer 16 are cut along a cutting line C1 between the sixth composite and the first support plate 3 and a cutting line C3 between the sixth composite and the third support plate 5, etc., to separate the sixth composite from the support 1. After the sixth composite is separated, the remaining support 1 to which the graphite substrate 19 and the like are fixed is disposed of.

[0078] 36 shows the sixth composite separated from the support 1. The sixth composite was separated by cutting the graphite substrate 19 together with the SiC polycrystalline growth layer 16 formed extending on the support 1. Therefore, the cut surface of the graphite substrate 19 is exposed from the sixth composite.

[0079] As shown in Figure 37, by removing the graphite substrate 19 and carbonized adhesive layer 15 inside the sixth composite by oxidative combustion, a seventh composite (13 (SiC-epi), 11c, 16 (SiC-poly CVD)) in which a SiC epitaxial growth layer 13, a thinned SiC single crystal layer 11d and a SiC polycrystalline growth layer 16 are stacked, and the SiC polycrystalline growth layer 16 is separated from the seventh composite.

[0080] 38, the SiC polycrystalline growth layer 16 on the periphery of the seventh composite is ground and polished to remove it, thereby obtaining a SiC composite substrate 10. The SiC composite substrate 10 of the modified example is similar to the SiC composite substrate 10 of the embodiment, except that a thinned SiC single crystal layer 11d is interposed between the SiC epitaxial growth layer 13 and the SiC polycrystalline growth layer.

[0081] As shown in Figure 37, a substrate consisting of a single-layer SiC polycrystalline growth layer 16 is obtained by oxidatively burning the graphite substrate 19 and the adhesive layer 15. Since this substrate has the same dimensions as the SiC composite substrate 10, such as the diameter and thickness, it can be used as the first dummy substrate 6 or the second dummy substrate 7 in the support 1.

[0082] The manufacturing method of the semiconductor substrate of the modified example can also produce the SiC composite substrate 10 in the same manner as the manufacturing method of the semiconductor of the embodiment. Therefore, the same effect as the manufacturing method of the semiconductor of the embodiment can be obtained in the modified example. Furthermore, since epitaxial growth is performed directly on the Si surface of the SiC single crystal substrate 11 without the intermediation of a graphene layer, the SiC epitaxial growth layer 13 having a good crystal structure can be formed. In addition, according to the modified example, a substrate made of a single layer of SiC polycrystalline growth layer having the same size as the SiC composite substrate 10 can be obtained at the same time as the SiC composite substrate 10, and this substrate can be used for the first dummy substrate 6 or the second dummy substrate 7.

[0083] (Additional Note 1) A support plate 3, 4, 5 supports a temporary substrate 9 and enables a SiC polycrystalline growth layer to be formed on a semiconductor substrate supported on a main surface of the temporary substrate 9, and includes a plurality of grooves 3a, 4a, 5a formed on one edge thereof, the plurality of grooves 3a, 4a, 5a including grooves 3a3, 4a3, 5a3 configured to support the temporary substrate 9 inserted in an orientation such that the main surface is perpendicular to the direction in which the one edge extends. The temporary substrate 9 can be supported by the grooves 3a3, 4a3, 5a3.

[0084] (Appendix 2) The support plates 3, 4, and 5 described in appendix 1 are made of graphite. Since they are made of graphite, they are inexpensive.

[0085] (Supplementary Note 3) The support plate 3, 4, 5 according to Supplementary Note 1 has one edge extending in the longitudinal direction and formed in a comb shape by a plurality of grooves 3a, 4a, 5a. The plurality of grooves 3a, 4a, 5a can form a plurality of grooves 3a3, 4a3, 5a3 for supporting a temporary substrate 9.

[0086] (Appendix 4) The support plates 3, 4, and 5 according to appendix 3 have a rectangular plate shape, and one edge is one long side of the rectangular plate shape. Because of the rectangular plate shape, it is easy to manufacture.

[0087] (Appendix 5) The support plate 3, 4, 5 according to appendix 3 or 4, wherein an expanded graphite sheet is attached to at least a part of one edge on which a plurality of comb-tooth-shaped grooves 3a, 4a, 5a are formed. Even if a temporary substrate 9 is fixed to the support plate 3, 4, 5 by the CVD process, it can be easily peeled off by the expanded graphite sheet.

[0088] (Appendix 6) A support 1 for a temporary substrate 9 using the support plates 3, 4, 5 described in Appendix 1, comprising a first dummy substrate 6 and a second dummy substrate 7, and a support pillar 2 supporting the first dummy substrate 6 and the second dummy substrate 7, the support plates 3, 4, 5 including at least three support plates 3, 4, 5, the support plates 3, 4, 5 including, for a plurality of grooves 3a, 4a, 5a, a support pillar 2 that fits with the first dummy substrate 6 in the first groove 3a1, 4a1, 5a1 and fits with the second dummy substrate 7 in the second groove 3a2, 4a2, 5a2, the support pillar 2 is configured to support the temporary substrate 9 inserted into the third groove 3a3, 4a3, 5a3 of the plurality of grooves 3a, 4a, 5a of the support plates 3, 4, 5, excluding the first groove 3a1, 4a1, 5a1 and the second groove 3a2, 4a2, 5a2. The structure of the support tool 1 can be formed by the first dummy substrate 6, the second dummy substrate 7, and the support posts 2 including the support plates 3, 4, and 5.

[0089] (Supplementary Note 7) In the support 1 described in Supplementary Note 6, the first dummy substrate 6 and the second dummy substrate 7 are fixed to be parallel to each other by the support pillars 2. The first dummy substrate 6, the second dummy substrate 7 and the support pillars 2 can form a space for accommodating the temporary substrate 9.

[0090] (Appendix 8) In the support 1 described in appendix 6, the support pillars 2 are arranged along the periphery of the first dummy substrate 6 and the second dummy substrate 7 so that the directions in which one edges of the support plates 3, 4, and 5 extend are parallel to each other. By fitting with the first dummy substrate 6 and the second dummy substrate 7, the structure of the support 1 can be formed.

[0091] (Appendix 9) The support 1 described in appendix 6, wherein the first grooves 3a1, 4a1, 5a1 are grooves at one end in a direction in which one edge extends for the plurality of grooves 3a, 4a, 5a, and the second grooves 3a2, 4a2, 5a2 are grooves at the other end in that direction. The third grooves 3a3, 4a3, 5a3 into which the temporary substrate 9 is inserted can be secured in the center of one edge.

[0092] (Supplementary Note 10) In the support 1 according to any one of Supplementary Notes 6 to 9, at least one of the first dummy substrate 6 and the second dummy substrate 7 is made of graphite. Since it is made of graphite, it is inexpensive.

[0093] (Supplementary Note 11) The support 1 according to any one of Supplementary Notes 6 to 9, wherein at least one of the first dummy substrate 6 and the second dummy substrate 7 is made of SiC. Since it is made of SiC, it is inexpensive.

[0094] (Supplementary Note 12) In the support 1 according to any one of Supplementary Notes 6 to 9, the first dummy substrate 6 and the second dummy substrate 7 are disk-shaped or rectangular plate-shaped. They can be selected to correspond to the temporary substrate 9 having a disk-shaped or rectangular plate-shaped configuration.

[0095] (Appendix 13) The support 1 according to any one of appendices 6 to 9, wherein a pair of support plates 3, 4, 5 face each other across a first dummy substrate 6 and a second dummy substrate 7, and the remaining support plates 3, 4, 5 are on one side of a plane that includes the opposing pair of support plates 3, 4, 5. A temporary substrate 9 can be inserted from the front of the support 1.

[0096] (Appendix 14) A method for manufacturing a semiconductor substrate using the support 1 described in appendix 6, comprising the steps of forming a SiC epitaxial growth layer 13 on the Si face of a SiC single crystal substrate 11, attaching the Si face of the SiC epitaxial growth layer 13 to a graphite substrate 19, removing the SiC epitaxial growth layer 13 from the SiC single crystal substrate 11, supporting the graphite substrate 19 with the SiC epitaxial growth layer 13 attached thereto with the support 1, forming a SiC polycrystalline growth layer 16 on the C face of the SiC epitaxial growth layer 13 attached to the graphite substrate 19, removing the graphite substrate 19 with the SiC polycrystalline growth layer 16 formed thereon from the support 1, and removing the graphite substrate 19. By using the support 1, a semiconductor substrate can be manufactured with high quality and at low cost.

[0097] (Appendix 15) The method for producing a semiconductor substrate according to appendix 14 further includes a step of forming a graphene layer 12 on a Si surface of the SiC single crystal substrate 11, and the step of forming the SiC epitaxial growth layer 13 forms the SiC epitaxial growth layer 13 on the Si surface of the SiC single crystal substrate 11 via the graphene layer 12. This makes it possible to peel off the graphene layer 12 and the SiC epitaxial growth layer 13.

[0098] (Appendix 16) In the method for producing a semiconductor substrate according to appendix 15, the step of removing the SiC epitaxial growth layer 13 from the SiC single crystal substrate 11 peels the SiC epitaxial growth layer 13 from the graphene layer 12. This makes it possible to reuse the SiC single crystal substrate 11.

[0099] (Appendix 17) The method for producing a semiconductor substrate according to appendix 15 further includes a step of forming a stress layer 14 on a Si face of the SiC epitaxial growth layer 13, the stress layer 14 generating a stress for peeling the SiC epitaxial growth layer 13 from the graphene layer 12, and the step of attaching the Si face of the SiC epitaxial growth layer 13 to the graphite substrate 19 attaches the Si face of the SiC epitaxial growth layer 13 to the graphite substrate 19 via the stress layer 14. The stress generated by the stress layer 14 makes it easy to peel the SiC epitaxial growth layer 13 and the graphene layer 12 from each other.

[0100] (Appendix 18) The method for manufacturing a semiconductor substrate according to appendix 14 further includes a step of forming a hydrogen ion implanted layer 11c at a predetermined depth from the Si face of the SiC single crystal substrate 11, and the step of removing the SiC epitaxial growth layer 13 from the SiC single crystal substrate 11 embrittles the hydrogen ion implanted layer 11c to peel off the SiC epitaxial growth layer 13 together with the thinned SiC single crystal layer 11d separated by the hydrogen ion implanted layer 11c from the SiC single crystal substrate 11. Separation is made possible by embrittling the hydrogen ion implanted layer 11c of the SiC single crystal substrate 11.

[0101] (Appendix 19) The method for manufacturing a semiconductor substrate according to appendix 18 further includes a step of polishing a C-face of the thinned SiC single crystal layer 11d peeled off together with the SiC epitaxial growth layer 13. This makes it possible to smooth out the uneven structure formed by the division of the hydrogen ion implanted layer 11c.

[0102] (Appendix 20) In the method for manufacturing a semiconductor substrate according to any one of appendices 14 to 19, the temporary substrate 9 is made of graphite. This enables removal of the graphite substrate 19, which is the temporary substrate 9, by burning.

[0103] (Appendix 21) The method for manufacturing a semiconductor substrate according to any one of Appendices 14 to 19, wherein the graphite substrate 19 has an outer size larger than that of the SiC single crystal substrate 11. The graphite substrate 19 can be supported by being inserted into the support 1.

[0104] (Appendix 22) In the method for producing a semiconductor substrate according to any one of Appendices 14 to 19, graphite substrate 19 includes a glassy carbon coating formed on the surface thereof. Since the glassy carbon coating has a strong adhesive force with the carbon adhesive of adhesive layer 15, graphene layer 12 and SiC epitaxial growth layer 13 can be reliably peeled off from each other.

[0105] (Supplementary Note 23) In the method for producing a semiconductor substrate according to any one of Supplementary Notes 14 to 19, the step of removing the graphite substrate 19 removes the graphite substrate 19 by burning it. Since the graphite substrate 19 is a graphite substrate, it can be removed by burning it in an air atmosphere or the like.

[0106] (Appendix 24) In the method for producing a semiconductor substrate according to appendix 23, in the step of attaching the graphite substrate 19 to the C-face of the SiC epitaxial growth layer, the SiC epitaxial growth layer 13 and the graphite substrate 19 are attached via an adhesive layer 15 made of a carbon adhesive. Since the carbon adhesive has a strong adhesive force, the graphene layer 12 and the SiC epitaxial growth layer 13 can be reliably peeled off.

[0107] (Appendix 25) In the method for producing a semiconductor substrate according to appendix 24, the step of removing the graphite substrate 19 includes burning and removing the adhesive layer 15 together with the graphite substrate 19. The adhesive layer 15 can be burned and removed together with the graphite substrate 19 in an air atmosphere or the like.

[0108] (Other embodiments) As described above, several embodiments have been described, but the descriptions and drawings forming part of the disclosure are illustrative and should not be understood as limiting. From this disclosure, various alternative embodiments, examples and operating techniques will become apparent to those skilled in the art. Thus, the embodiments include various embodiments not described herein. [Industrial Applicability]

[0109] The present disclosure can be used in various semiconductor module technologies, such as IGBT modules, diode modules, and MOS modules (SiC, GaN, AlN, gallium oxide), and can be applied to a wide range of application fields, such as power modules for inverter circuits that drive electric motors used as power sources for electric vehicles (including hybrid vehicles), trains, industrial robots, etc., and power modules for inverter circuits that convert power generated by solar cells, wind turbines, and other power generation devices (especially private power generation devices) into power from commercial power sources. [Explanation of symbols]

[0110] 1 Support 2 pillars 3, 4, 5 Support plate 2a, 3a, 4a groove 3a1, 4a1, 5a1 1st groove 3a2, 4a2, 5a2 2nd groove 3a3, 4a3, 5a3 3rd groove 6, 7 Dummy board 9 Temporary board 10 SiC composite substrate 11 SiC single crystal substrate 12 Graphene layers 13. SiC epitaxial growth layer 14 Stress Layer 15 Adhesive layer 19 Graphite Substrate

Claims

1. A support plate that supports a temporary substrate and enables a SiC polycrystalline growth layer to be formed on a semiconductor substrate supported on a main surface of the temporary substrate, A support plate including a plurality of grooves formed in one edge thereof, the plurality of grooves being configured to support the temporary substrate inserted in an orientation such that the main surface is perpendicular to the direction in which the one edge extends.

2. 2. The support plate of claim 1, which is comprised of graphite.

3. The support plate according to claim 1 , wherein the one edge extends in the longitudinal direction and is formed into a comb-like shape by the plurality of grooves.

4. 4. The support plate according to claim 3, having a rectangular plate shape, said one edge being one long side of said rectangular plate shape.

5. 5. The support plate according to claim 3, further comprising an expanded graphite sheet attached to at least a portion of the edge on which the plurality of comb-tooth grooves are formed.

6. A support for the temporary substrate using the support plate according to claim 1, A first dummy substrate and a second dummy substrate; a support plate for supporting the first dummy substrate and the second dummy substrate, the support plate including at least three support plates, the support plate including a support plate for engaging with the first dummy substrate in a first groove and a support plate for engaging with the second dummy substrate in a second groove, Including, The support pillar is a support configured to support the temporary substrate inserted into a third groove, which is one of the multiple grooves of the support plate, excluding the first groove and the second groove.

7. The support according to claim 6 , wherein the first dummy substrate and the second dummy substrate are fixed by the support pillars so as to be parallel to each other.

8. The support according to claim 6 , wherein the support pillars are arranged along the peripheries of the first dummy substrate and the second dummy substrate such that the directions in which the one edge of the support plate extends are parallel to each other.

9. The support according to claim 6 , wherein the first groove is a groove at one end of the plurality of grooves in a direction in which the one edge extends, and the second groove is a groove at the other end in the direction.

10. The support according to claim 6 , wherein at least one of the first dummy substrate and the second dummy substrate is made of graphite.

11. The support according to claim 6 , wherein at least one of the first dummy substrate and the second dummy substrate is made of SiC.

12. The support according to claim 6 , wherein the first dummy substrate and the second dummy substrate are in the shape of a circular plate or a rectangular plate.

13. A support device as described in any one of claims 6 to 9, wherein a pair of support plates face each other across the first dummy substrate and the second dummy substrate, and the remaining support plate is on one side of a plane containing the opposing pair of support plates.

14. A method for manufacturing a semiconductor substrate using the support according to claim 6, comprising the steps of: forming a SiC epitaxial growth layer on the Si surface of the SiC single crystal substrate; attaching a Si surface of the SiC epitaxial growth layer to the temporary substrate; removing the SiC epitaxial growth layer from the SiC single crystal substrate; supporting the temporary substrate to which the SiC epitaxial growth layer is attached with the support; forming a SiC polycrystalline growth layer on a C surface of the SiC epitaxial growth layer attached to the temporary substrate; removing the temporary substrate on which the SiC polycrystalline growth layer is formed from the support; removing the temporary substrate; A method for manufacturing a semiconductor substrate comprising the steps of:

15. 15. The method for producing a semiconductor substrate according to claim 14, further comprising the step of forming a graphene layer on a Si surface of the SiC single crystal substrate, wherein the step of forming the SiC epitaxial growth layer forms the SiC epitaxial growth layer on the Si surface of the SiC single crystal substrate via the graphene layer.

16. The method for producing a semiconductor substrate according to claim 15 , wherein the step of removing the SiC epitaxial growth layer from the SiC single crystal substrate comprises peeling the SiC epitaxial growth layer from the graphene layer.

17. 16. The method for producing a semiconductor substrate according to claim 15, further comprising the step of forming a stress layer on a Si surface of the SiC epitaxial growth layer, the stress layer generating a stress that peels the SiC epitaxial growth layer from the graphene layer, and the step of attaching the Si surface of the SiC epitaxial growth layer to the temporary substrate comprises attaching the Si surface of the SiC epitaxial growth layer to the temporary substrate via the stress layer.

18. 15. The method for manufacturing a semiconductor substrate according to claim 14, further comprising the step of forming a hydrogen ion implanted layer at a predetermined depth from a Si-face of the SiC single crystal substrate, and the step of removing the SiC epitaxial growth layer from the SiC single crystal substrate comprises embrittling the hydrogen ion implanted layer to peel off the SiC epitaxial growth layer together with the thinned SiC single crystal layer divided by the hydrogen ion implanted layer from the SiC single crystal substrate.

19. The method for producing a semiconductor substrate according to claim 18 , further comprising the step of polishing a C-plane of the thinned SiC single crystal layer that has been peeled off together with the SiC epitaxial growth layer.

20. The method for manufacturing a semiconductor substrate according to claim 14 , wherein the temporary substrate is made of graphite.

21. The method for manufacturing a semiconductor substrate according to claim 14 , wherein the temporary substrate has an outer size larger than that of the SiC single crystal substrate.

22. The method for manufacturing a semiconductor substrate according to claim 14 , wherein the temporary substrate includes a glassy carbon coating formed on a surface thereof.

23. The method for manufacturing a semiconductor substrate according to claim 14 , wherein the step of removing the temporary substrate comprises burning the temporary substrate to remove it.

24. 24. The method for manufacturing a semiconductor substrate according to claim 23, wherein the step of attaching the temporary substrate to the C surface of the SiC epitaxial growth layer includes attaching the SiC epitaxial growth layer and the temporary substrate via an adhesive layer made of a carbon adhesive.

25. The method for manufacturing a semiconductor substrate according to claim 24 , wherein the step of removing the temporary substrate includes burning and removing the adhesive layer together with the temporary substrate.

Citation Information

Patent Citations

  • Thin film wafer transfer and structure for electronic devices

    US8916451B2