Deposition method and deposition equipment
The film formation method uses phosphine gas adsorption to control silicon film thickness differences by adjusting incubation time, ensuring uniform deposition on multiple film types.
Patent Information
- Application Number
- JP2023058206
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Existing methods struggle to control film thickness differences when simultaneously forming a silicon film on multiple films, such as an amorphous silicon film and a silicon oxide film, leading to inconsistencies in film deposition.
A film formation method involving a growth inhibition step using phosphine gas to selectively adsorb on one film type, followed by a film forming step with monosilane gas to control the incubation time and thickness of the silicon film, ensuring uniform deposition across different film types.
The method achieves controlled film thickness differences by adjusting the incubation time of the silicon film formation, resulting in uniform film thickness across varying film types.
Smart Images

Figure 2024145726000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a film forming method and a film forming apparatus. [Background technology]
[0002] A technique is known in which the surface layers of a SiO film and a SiN film exposed on the surface of a substrate are nitrided to form a seed layer, and then a SiN film is formed by ALD, thereby aligning the growth of the SiN film on the surface of the SiO film and the surface of the SiN film (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-175106 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present disclosure provides a technique capable of controlling a thickness difference between a silicon film formed on a first film and a silicon film formed on a second film when the silicon films are simultaneously formed on a first film and a second film. [Means for solving the problem]
[0005] A film formation method according to one embodiment of the present disclosure is a film formation method for forming a silicon film on a substrate, the film formation method comprising the steps of: preparing a substrate having a first film and a second film on its surface; supplying a growth-inhibiting gas that inhibits the growth of the silicon film to the substrate and physically adsorbing the growth-inhibiting gas onto the first film; and supplying a silane-based gas having a silicon number of 1 to the substrate with the growth-inhibiting gas physically adsorbed onto the first film, and forming the silicon film on the first film and the second film. Effect of the Invention
[0006] According to the present disclosure, when silicon films are simultaneously formed on a first film and a second film, the difference in thickness between the silicon film formed on the first film and the silicon film formed on the second film can be controlled. [Brief description of the drawings]
[0007] [Figure 1] 2 is a flowchart illustrating a film forming method according to an embodiment. [Diagram 2] 1A to 1C are cross-sectional views illustrating a film forming method according to an embodiment. [Diagram 3] FIG. 2 is a diagram showing a surface reaction when an a-Si film is formed on an a-Si film. [Figure 4] FIG. 1 is a diagram showing a surface reaction when an a-Si film is formed on a SiO2 film. [Diagram 5] 1 is a cross-sectional view showing a film forming apparatus according to an embodiment. [Figure 6] FIG. 13 is a diagram showing the relationship between gas supply time and film thickness when an a-Si film is formed on an a-Si film. [Figure 7] FIG. 13 is a diagram showing the relationship between gas supply time and film thickness when an a-Si film is formed on a SiO 2 film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, non-limiting exemplary embodiments of the present disclosure will be described with reference to the accompanying drawings. In all of the accompanying drawings, the same or corresponding members or parts are designated by the same or corresponding reference numerals, and duplicated descriptions will be omitted.
[0009] [Film formation method] A film forming method according to an embodiment will be described with reference to Figures 1 and 2. As shown in Figure 1, the film forming method according to the embodiment includes a preparation step S10, a growth inhibition step S20, and a film forming step S30.
[0010] The preparation step S10 includes preparing a substrate 101 as shown in FIG. 2(a). The substrate 101 is, for example, a semiconductor wafer such as a silicon wafer. The substrate 101 has an amorphous silicon film (a-Si film) 102 and a silicon oxide film (SiO2 film) 103 on the surface. The a-Si film 102 is an example of a first film. The SiO2 film 103 is an example of a second film. The substrate 101 has a flat portion 104, a first columnar portion 105, and a second columnar portion 106 on the surface. The first columnar portion 105 and the second columnar portion 106 are each provided on the flat portion 104. The first columnar portion 105 and the second columnar portion 106 may each be a plurality of portions. The a-Si film 102 covers the flat portion 104 and the first columnar portion 105. The SiO2 film 103 covers the second columnar portion 106. The substrate 101 may not have the first columnar section 105 and the second columnar section 106. In this case, the a-Si film 102 and the SiO2 film 103 are provided in different regions on the flat section 104. The preparation step S10 may include adjusting and maintaining the substrate 101 at a predetermined temperature. The predetermined temperature may be the same as the processing temperature in the growth inhibition step S20. In this case, there is no need to change the temperature when transitioning from the preparation step S10 to the growth inhibition step S20, thereby improving productivity.
[0011] The growth inhibition step S20 is performed after the preparation step S10. The growth inhibition step S20 includes adjusting and maintaining the substrate 101 at a first processing temperature. The growth inhibition step S20 includes supplying phosphine (PH3) gas to the substrate 101. Phosphine gas is an example of a growth inhibition gas. As shown in FIG. 2(b), the phosphine gas is selectively physically adsorbed on the surface of the a-Si film 102, but is hardly physically adsorbed on the surface of the SiO2 film 103. The reason will be described later. The first processing temperature is preferably a temperature lower than the thermal decomposition temperature of the phosphine gas. In this case, since the phosphine gas can be prevented from being chemically adsorbed on the surface of the a-Si film 102, the phosphine gas present on the surface of the a-Si film 102 in the film formation step S30 is easily removed. Therefore, phosphorus (P) contained in the phosphine gas can be prevented from remaining in the a-Si film 108 described later. As a result, the properties of the a-Si film 108 are not affected. The first treatment temperature is, for example, 470°C.
[0012] The film forming step S30 is performed after the growth inhibition step S20. The film forming step S30 includes adjusting and maintaining the substrate 101 at a second processing temperature. The film forming step S30 includes supplying monosilane (SiH4) gas to the substrate 101 to form the a-Si film 108 on the a-Si film 102 and the SiO2 film 103. The monosilane gas is an example of a silane-based gas with a silicon number of 1. It takes a certain time from when the supply of the monosilane gas to the SiO2 film 103 is started until the film formation starts. When the supply of the monosilane gas to the a-Si film 102 is started, the film formation starts immediately after the supply, but if PH3 is physically adsorbed on the surface, the more the amount of physically adsorbed PH3, the longer the time from when the supply of the monosilane gas is started until the film formation starts. In the film forming step S30, since PH3 is physically adsorbed on the a-Si film 102, an a-Si film 108 having a smaller difference in thickness is formed on the a-Si film 102 and the SiO2 film 103, compared to a case in which PH3 is not physically adsorbed on the a-Si film 102. The second process temperature may be a temperature equal to or higher than the thermal decomposition temperature of the monosilane gas and equal to or lower than 600°C. The second process temperature may be the same as the first process temperature, for example, 470°C.
[0013] With reference to Fig. 3, a surface reaction occurring when an a-Si film 108 is formed on an a-Si film 102 will be described. As shown in Fig. 3(a), the surface of the a-Si film 102 is composed of silicon (Si) having Si-H bonds and dangling bonds. Phosphine (PH3) is easily adsorbed onto a surface having Si-H bonds and silicon having dangling bonds. For this reason, as shown in Fig. 3(b), when phosphine gas is supplied to the a-Si film 102 in the growth inhibition step S20, PH3 is physically adsorbed onto the surface of the a-Si film 102.
[0014] Subsequently, when monosilane gas is supplied in the film forming step S30, the monosilane gas is thermally decomposed to generate SiH2 radicals, as shown in FIG. 3(c). The SiH2 radicals extract hydrogen (H) present on the surface of the a-Si film 102 to return to SiH4 and generate dangling bonds. If PH3 is not physically adsorbed on the surface of the a-Si film 102, another SiH2 radical is adsorbed on the dangling bond and the formation of the a-Si film 108 is started. On the other hand, if PH3 is physically adsorbed on the surface of the a-Si film 102, the adsorption of the SiH2 radicals on the dangling bonds is inhibited by PH3. In this case, if SiH2 radicals are continuously supplied to the surface of the a-Si film 102, PH3 is desorbed from the surface of the a-Si film 102. When PH3 is desorbed from the surface of the a-Si film 102, the SiH2 radical extracts hydrogen (H) present on the surface of the a-Si film 102, returning to SiH4 and making it easier to generate dangling bonds. As a result, another SiH2 radical is adsorbed to the dangling bond, and the formation of the a-Si film 108 begins.
[0015] In this way, for the a-Si film 102 with PH3 physically adsorbed on its surface, the time required from the start of supply of monosilane gas to the start of deposition of the a-Si film 108 (hereinafter also referred to as "incubation time") becomes longer. The incubation time becomes longer as the amount of PH3 physically adsorbed on the surface of the a-Si film 102 increases. Therefore, by changing the supply time of phosphine gas to the substrate 101 in the growth inhibition step S20, the incubation time of the a-Si film 108 on the a-Si film 102 can be controlled.
[0016] With reference to FIG. 4, the surface reaction when the a-Si film 108 is formed on the SiO2 film 103 will be described. As shown in FIG. 4(a), the surface of the SiO2 film 103 has many Si-O bonds, and has less silicon (Si) with Si-H bonds or dangling bonds than the surface of the a-Si film 102. The Si-O bonds have the function of inhibiting the extraction of hydrogen (H) by the SiH2 radicals. Therefore, the time required from the start of the supply of monosilane gas onto the SiO2 film 103 to the start of the formation of the a-Si film 108 is longer than the time required from the start of the supply of monosilane gas onto the a-Si film 102 to the start of the formation of the a-Si film 108. The Si-O bonds have the function of inhibiting the physical adsorption of PH3. Therefore, even if the surface of the SiO2 film 103 is exposed to phosphine gas in the growth inhibition step S20, almost no PH3 is physically adsorbed on the surface of the SiO2 film 103 as shown in FIG. 4(b).
[0017] Subsequently, when monosilane gas is supplied in the film forming process S30, the monosilane gas is thermally decomposed to generate SiH2 radicals, as shown in FIG. 4(c). The SiH2 radicals extract hydrogen (H) present on the surface of the SiO2 film 103 to return to SiH4 and generate dangling bonds. At this time, the surface of the SiO2 film 103 has many Si-O bonds and few Si-H bonds, so that the extraction of hydrogen (H) by the SiH2 radicals is unlikely to occur. Thus, on the surface of the SiO2 film 103, regardless of the presence or absence of physical adsorption of PH3, the time required from the start of the supply of monosilane gas to the start of the growth of the a-Si film 108 becomes long.
[0018] As described above, according to the film forming method of the embodiment, phosphine gas is supplied to the substrate 101 having an a-Si film 102 and a SiO2 film 103 on its surface, and PH3 is physically adsorbed on the surface of the a-Si film 102. Thereafter, monosilane gas is supplied to form an a-Si film 108 on the a-Si film 102 and the SiO2 film 103. This allows the a-Si film 108, with a small thickness difference, to be formed simultaneously on the a-Si film 102 and the SiO2 film 103.
[0019] According to the film forming method of the embodiment, the incubation time of the a-Si film 108 relative to the a-Si film 102 can be controlled by changing the supply time of the phosphine gas to the substrate 101. At this time, the incubation time of the a-Si film 108 relative to the SiO2 film 103 hardly changes. Therefore, the difference in thickness of the a-Si film 108 formed on the a-Si film 102 and the SiO2 film 103 can be controlled.
[0020] [Film forming equipment] A film forming apparatus 1 according to an embodiment will be described with reference to Fig. 5. As shown in Fig. 5, the film forming apparatus 1 is a batch type apparatus that processes a plurality of substrates W at once.
[0021] The film forming apparatus 1 includes a processing chamber 10, a gas supply unit 30, an exhaust unit 40, a heating unit 50, and a control unit 80.
[0022] The processing vessel 10 is capable of reducing the pressure inside. The processing vessel 10 accommodates a substrate W therein. The processing vessel 10 has an inner tube 11 and an outer tube 12. The inner tube 11 and the outer tube 12 have a cylindrical shape with a ceiling and an open lower end. The outer tube 12 covers the outside of the inner tube 11. The inner tube 11 and the outer tube 12 have a double tube structure arranged coaxially. The inner tube 11 and the outer tube 12 are formed of a heat-resistant material such as quartz.
[0023] The ceiling of the inner pipe 11 may be flat, for example. A storage section 13 for storing a gas nozzle is formed along the longitudinal direction (vertical direction) of the inner pipe 11 on one side. For example, a part of the side wall of the inner pipe 11 protrudes outward to form a convex section 14, and the inside of the convex section 14 is formed as the storage section 13.
[0024] In the side wall on the opposite side of the inner tube 11 facing the storage portion 13, a rectangular opening 15 is formed along the longitudinal direction (vertical direction).
[0025] The opening 15 is a gas exhaust port formed so as to be able to exhaust the gas inside the inner tube 11. The length of the opening 15 is the same as the length of the boat 16, or is formed so as to extend longer than the length of the boat 16 in the vertical direction.
[0026] The lower end of the processing vessel 10 is supported by a cylindrical manifold 17. The manifold 17 is made of, for example, stainless steel. A flange 18 is formed at the upper end of the manifold 17. The flange 18 supports the lower end of the outer tube 12. A seal member 19 such as an O-ring is provided between the flange 18 and the lower end of the outer tube 12. This keeps the inside of the outer tube 12 airtight.
[0027] An annular support 20 is provided on the inner wall of the upper part of the manifold 17. The support 20 supports the lower end of the inner tube 11. A lid 21 is air-tightly attached to the opening at the lower end of the manifold 17 via a seal member 22 such as an O-ring. This air-tightly closes the opening at the lower end of the processing vessel 10, i.e., the opening of the manifold 17. The lid 21 is made of, for example, stainless steel.
[0028] A rotating shaft 24 is provided penetrating the center of the lid 21 via a magnetic fluid seal 23. A lower portion of the rotating shaft 24 is rotatably supported by an arm 25A of an elevation mechanism 25 made up of a boat elevator.
[0029] A rotating plate 26 is provided at the upper end of the rotating shaft 24. The boat 16, which holds the substrates W, is placed on the rotating plate 26 via a quartz heat retention stand 27. The boat 16 rotates by rotating the rotating shaft 24. The boat 16 moves up and down together with the lid 21 by raising and lowering the lifting mechanism 25. This allows the boat 16 to be inserted into and removed from the processing vessel 10. The boat 16 can be accommodated within the processing vessel 10. The boat 16 holds a plurality of substrates W (e.g., 50 to 150 substrates) approximately horizontally with a gap between them in the vertical direction.
[0030] The gas supply unit 30 is configured to be able to introduce various process gases used in the above-mentioned film formation method into the inner tube 11. The gas supply unit 30 includes a phosphine supply unit 31 and a monosilane supply unit 32.
[0031] The phosphine supply unit 31 includes a phosphine supply pipe 31a inside the processing vessel 10, and a phosphine supply path 31b outside the processing vessel 10. A phosphine supply source 31c, a mass flow controller 31d, and a valve 31e are provided in the phosphine supply path 31b, in this order from the upstream side to the downstream side in the gas flow direction. Thus, the supply timing of the phosphine gas from the phosphine supply source 31c is controlled by the valve 31e, and the flow rate is adjusted to a predetermined value by the mass flow controller 31d. The phosphine gas flows from the phosphine supply path 31b into the phosphine supply pipe 31a, and is discharged from the phosphine supply pipe 31a into the processing vessel 10.
[0032] The monosilane supply unit 32 includes a monosilane supply pipe 32a inside the processing vessel 10, and a monosilane supply path 32b outside the processing vessel 10. A monosilane source 32c, a mass flow controller 32d, and a valve 32e are provided in the monosilane supply path 32b, in this order from upstream to downstream in the gas flow direction. Thus, the supply timing of the monosilane gas from the monosilane source 32c is controlled by the valve 32e, and the flow rate is adjusted to a predetermined value by the mass flow controller 32d. The monosilane gas flows from the monosilane supply path 32b into the monosilane supply pipe 32a, and is discharged from the monosilane supply pipe 32a into the processing vessel 10.
[0033] Each gas supply pipe (phosphine supply pipe 31a, monosilane supply pipe 32a) is fixed to manifold 17. Each gas supply pipe is made of, for example, quartz. Each gas supply pipe extends linearly in the vertical direction near inner pipe 11, and is bent in an L-shape within manifold 17 to extend horizontally, thereby penetrating manifold 17. Each gas supply pipe is provided side by side along the circumferential direction of inner pipe 11, and is formed at the same height as each other.
[0034] A plurality of phosphine discharge ports 31f are provided in the phosphine supply pipe 31a at a portion located within the inner pipe 11. A plurality of monosilane discharge ports 32f are provided in the monosilane supply pipe 32a at a portion located within the inner pipe 11.
[0035] Each outlet (phosphine outlet 31f, monosilane outlet 32f) is formed at a predetermined interval along the extension direction of each gas supply pipe. Each outlet discharges gas in the horizontal direction. The interval between each outlet is set to be the same as the interval between the substrates W held in the boat 16, for example. The position of each outlet in the height direction is set to the midpoint between the substrates W adjacent in the vertical direction. This allows each outlet to efficiently supply gas to the opposing surfaces between the adjacent substrates W.
[0036] The gas supply unit 30 may mix a plurality of types of gases and discharge the mixed gas from one gas supply pipe. The gas supply pipes (phosphine supply pipe 31a, monosilane supply pipe 32a) may have different shapes and arrangements. The film forming apparatus 1 may further include a gas supply pipe for supplying another gas in addition to the phosphine gas and monosilane gas.
[0037] The exhaust unit 40 exhausts gas that is exhausted from the inner tube 11 through the opening 15 and then exhausted from a gas outlet 41 through a space P1 between the inner tube 11 and the outer tube 12. The gas outlet 41 is formed in an upper side wall of the manifold 17, above the support unit 20. An exhaust passage 42 is connected to the gas outlet 41. A pressure adjustment valve 43 and a vacuum pump 44 are sequentially provided in the exhaust passage 42, so that the inside of the processing vessel 10 can be exhausted.
[0038] The heating part 50 is provided around the outer tube 12. The heating part 50 is provided, for example, on a base plate 28. The heating part 50 has a cylindrical shape so as to cover the outer tube 12. The heating part 50 includes, for example, a heating element, and heats each substrate W in the processing vessel 10.
[0039] The control unit 80 controls the operation of each part of the film forming apparatus 1. The control unit 80 may be, for example, a computer. A computer program for controlling the operation of each part of the film forming apparatus 1 is stored in a storage medium 90. The storage medium 90 may be, for example, a flexible disk, a compact disk, a hard disk, a flash memory, a DVD, or the like.
[0040] [Operation of the Film Forming Apparatus] The operation of the film forming apparatus 1 when carrying out the film forming method according to the embodiment will be described.
[0041] First, the control unit 80 controls the lifting mechanism 25 to load the boat 16 holding the substrates W into the processing vessel 10, and hermetically closes the opening at the bottom of the processing vessel 10 with the lid 21. Next, the control unit 80 controls the exhaust unit 40 to reduce the pressure inside the processing vessel 10, and controls the heating unit 50 to adjust the temperature of the substrates W to the first processing temperature. Each substrate W may be the substrate 101 described above.
[0042] Next, the control unit 80 controls the gas supply unit 30, the exhaust unit 40, and the heating unit 50 to execute the growth inhibition step S20. Specifically, first, the control unit 80 controls the heating unit 50 to maintain the temperature of the substrate W at the first processing temperature, controls the gas supply unit 30 to supply phosphine gas into the processing vessel 10, and controls the exhaust unit 40 to maintain the inside of the processing vessel 10 at the processing pressure. As a result, the phosphine gas is selectively physically adsorbed onto the surface of the a-Si film 102.
[0043] Next, the control unit 80 controls the gas supply unit 30, the exhaust unit 40, and the heating unit 50 to execute the film forming process S30. Specifically, first, the control unit 80 controls the heating unit 50 to adjust and maintain the temperature of the substrate W at the second processing temperature, controls the gas supply unit 30 to supply monosilane gas into the processing vessel 10, and controls the exhaust unit 40 to maintain the inside of the processing vessel 10 at the processing pressure. As a result, an a-Si film 108 having a small thickness difference is formed on the a-Si film 102 and the SiO2 film 103.
[0044] Next, control unit 80 increases the pressure inside processing vessel 10 to atmospheric pressure and decreases the temperature inside processing vessel 10 to the unloading temperature, and then controls lifting mechanism 25 to unload boat 16 from processing vessel 10 .
[0045] [Example] Example 1 In Example 1, a substrate having an a-Si film on its surface was prepared. Then, the prepared substrate was placed in the processing vessel 10 of the above-mentioned film forming apparatus 1, and the above-mentioned growth inhibition step S20 and film forming step S30 were carried out in this order. In the growth inhibition step S20, phosphine gas was supplied to the substrate while the substrate temperature was maintained at 470°C. In the film forming step S30, monosilane gas was supplied to the substrate while the substrate temperature was maintained at 470°C. In Example 1, an a-Si film was formed under a plurality of conditions in which the time for supplying monosilane gas to the substrate was different in the film forming step S30. Then, the thickness of the formed a-Si film was measured.
[0046] Comparative Example 1 As Comparative Example 1, the prepared substrate was placed in the processing vessel 10 of the above-mentioned film formation apparatus 1, and the film formation process S30 was carried out without carrying out the above-mentioned growth inhibition process S20. In the film formation process S30, an a-Si film was formed under the same conditions as in Example 1. Then, the thickness of the formed a-Si film was measured.
[0047] Fig. 6 is a diagram showing the relationship between the gas supply time and the film thickness when an a-Si film is formed on an a-Si film. In Fig. 6, the horizontal axis indicates the gas supply time, and the vertical axis indicates the film thickness of the a-Si film. Fig. 6 shows a solid straight line connecting each point when the film thicknesses of a plurality of a-Si films measured in Example 1 are plotted, and a dashed straight line connecting each point when the film thicknesses of a plurality of a-Si films measured in Comparative Example 1 are plotted.
[0048] As shown by the solid line in Fig. 6, in Example 1, the deposition of the a-Si film is started after a predetermined time X1 has elapsed since the supply of monosilane gas was started. In contrast, as shown by the dashed line in Fig. 6, in Comparative Example 1, the deposition of the a-Si film is started immediately after the supply of monosilane gas is started. This result shows that by performing the growth inhibition step S20 before the deposition step S30, it is possible to lengthen the time required from the start of the supply of monosilane gas to the substrate until the deposition of the a-Si film is started.
[0049] Example 2 In Example 2, a substrate having a SiO2 film on its surface was prepared. Then, the prepared substrate was placed in the processing vessel 10 of the above-mentioned film-forming apparatus 1, and the above-mentioned growth inhibition step S20 and film-forming step S30 were carried out in this order. In the growth inhibition step S20, phosphine gas was supplied to the substrate while the substrate temperature was maintained at 470°C. In the film-forming step S30, monosilane gas was supplied to the substrate while the substrate temperature was maintained at 470°C. In Example 2, an a-Si film was formed under a plurality of conditions in which the time for supplying monosilane gas to the substrate was different in the film-forming step S30. Then, the thickness of the formed a-Si film was measured.
[0050] Comparative Example 2 As Comparative Example 2, the prepared substrate was placed in the processing vessel 10 of the above-mentioned film formation apparatus 1, and the film formation process S30 was carried out without carrying out the above-mentioned growth inhibition process S20. In the film formation process S30, an a-Si film was formed under the same conditions as in Example 2. Then, the thickness of the formed a-Si film was measured.
[0051] Fig. 7 is a diagram showing the relationship between the gas supply time and the film thickness when an a-Si film is formed on a SiO2 film. In Fig. 7, the horizontal axis indicates the gas supply time, and the vertical axis indicates the film thickness of the a-Si film. Fig. 7 shows a solid straight line connecting each point when the film thicknesses of a plurality of a-Si films measured in Example 2 are plotted, and a dashed straight line connecting each point when the film thicknesses of a plurality of a-Si films measured in Comparative Example 1 are plotted.
[0052] As shown by the solid line in FIG. 7, in Example 2, the deposition of the a-Si film is started after a predetermined time X2 has elapsed since the supply of monosilane gas was started. As shown by the dashed line in FIG. 7, in Comparative Example 2, the deposition of the a-Si film is started after a predetermined time Y2 has elapsed since the supply of monosilane gas was started. It is also found that the predetermined time Y2 is almost the same as the predetermined time X2. From this result, it was shown that when the a-Si film is deposited on the SiO2 film, even if the SiO2 film is exposed to phosphine gas before the supply of monosilane gas, the time required from the start of the supply of monosilane gas to the start of the deposition of the a-Si film hardly changes.
[0053] The embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The above-described embodiments may be omitted, substituted, or modified in various forms without departing from the scope and spirit of the appended claims.
[0054] In the above embodiment, the growth inhibition gas is phosphine gas, but the present disclosure is not limited thereto. For example, the growth inhibition gas may be diborane (B2H6) gas.
[0055] In the above embodiment, the case where the silane-based gas having one silicon number is SiH4 gas has been described, but the present disclosure is not limited thereto. For example, the silane-based gas having one silicon number may be a silane-based gas in which a part of the hydrogen (H) in the molecule of SiH4 gas is replaced with a halogen such as fluorine (F), chlorine (Cl), bromine (Br), or iodine (I). For example, the silane-based gas having one silicon number may be SiF4 gas, SiHF3 gas, SiH2F2 gas, SiH3F gas, SiCl4 gas, SiHCl3 gas, SiH2Cl2 (DCS) gas, SiH3Cl gas, Si2Cl6 gas, SiBr4 gas, SiHBr3 gas, SiH2Br2 gas, SiH3Br gas, SiI4 gas, SiHI3 gas, SiH2I2 gas, or SiH3I gas.
[0056] In the above embodiment, the first film is an a-Si film and the second film is a SiO2 film, but the present disclosure is not limited to this. The first film and the second film may be formed of different materials. For example, the first film and the second film are films having different incubation times when forming the a-Si film. For example, the first film may be a silicon nitride film (SiN film) and the second film may be a SiO2 film. For example, the substrate 101 may have another film on its surface in addition to the first film and the second film.
[0057] In the above embodiment, the film forming apparatus is a batch type apparatus that processes a plurality of substrates at once, but the present disclosure is not limited to this. For example, the film forming apparatus may be a single-wafer type apparatus that processes substrates one by one. [Explanation of symbols]
[0058] 1 Film deposition equipment 10 Processing vessel 31 Phosphine Supply Department 32 Monosilane Supply Section 80 Control section S10 Preparation process S20 Growth inhibition step S30 Film formation process
Claims
1. A method for forming a silicon film on a substrate, comprising the steps of: preparing a substrate having a first film and a second film on a surface thereof; supplying a growth-inhibiting gas that inhibits growth of the silicon film to the substrate and physically adsorbing the growth-inhibiting gas onto the first film; supplying a silane-based gas having a silicon number of 1 to the substrate on which the growth-inhibiting gas has been physically adsorbed onto the first film, thereby forming the silicon film on the first film and the second film; The film forming method includes the steps of:
2. The growth inhibiting gas is supplied at a temperature lower than the pyrolysis temperature. The film forming method according to claim 1 .
3. The first film and the second film are films having different incubation times when forming the silicon film. The film forming method according to claim 1 .
4. the incubation time of the second membrane is longer than the incubation time of the first membrane; The film forming method according to claim 3 .
5. the first film is a silicon film or a silicon nitride film, The second film is a silicon oxide film. The film forming method according to claim 4.
6. The growth inhibition gas is phosphine gas or diborane gas. The film forming method according to claim 1 .
7. A film forming apparatus for forming a silicon film on a substrate, comprising: a processing vessel for accommodating the substrate; a gas supply unit for supplying a processing gas into the processing vessel; A control unit; Equipped with the substrate has a first film and a second film on a surface thereof; the processing gas includes a growth inhibition gas that inhibits the growth of the silicon film and a silane-based gas having a silicon number of 1; the control unit is configured to control the gas supply unit to perform a step of supplying the growth inhibition gas to the substrate and physically adsorbing the growth inhibition gas onto the first film; The control unit is configured to control the gas supply unit to supply the silane-based gas to the substrate on which the growth-inhibiting gas is physically adsorbed onto the first film, and to perform a process of forming the silicon film on the first film and the second film. Film deposition equipment.
Citation Information
Patent Citations
Film forming method and film forming apparatus
JP2017175106A
Silicon film forming method and forming device
JP2017183508A
Method and apparatus for forming silicon film
JP2019029576A
Method for producing semiconductor device, substrate treatment device, and program
WO2022054216A1
Deposition methods for high aspect ratio structures using an inhibitor molecule
WO2022081620A1