Resin sheet

The resin sheet, composed of 4-methyl-1-pentene polymer and a thermoplastic elastomer, addresses the rapid contraction issue of rubber bands by controlling tensile stress paths, enabling a stretch band that reduces excessive load and provides a gentle, relaxing exercise experience.

JP2024145789AInactive Publication Date: 2024-10-15MITSUI FINE CHEM
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023058287
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional rubber-based stretch bands require excessive force for recovery and can cause rapid contraction, leading to stress on joints during exercise.

Method used

A resin sheet composed of a 4-methyl-1-pentene polymer and a thermoplastic elastomer, designed to control the outward and return paths of tensile stress, reducing excessive load during recovery.

Benefits of technology

The resin sheet allows for a stretch band that can be stretched with appropriate force and slowly recover, reducing excessive load during recovery, providing a gentle stretching and relaxing effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145789000002
    Figure 2024145789000002
  • Figure 2024145789000003
    Figure 2024145789000003
  • Figure 2024145789000004
    Figure 2024145789000004
Patent Text Reader

Abstract

To provide a resin sheet from which a stretch band capable of reducing an excessive load at the time of recovery can be obtained.SOLUTION: A resin sheet is composed of a resin composition containing a 4-methyl-1-pentene-based polymer (A) and a thermoplastic elastomer (B) having a melting point of 130 to 180°C, wherein the 4-methyl-1-pentene-based polymer (A) contains a constitutional unit (a1) derived from 4-methyl-1-pentene and a constitutional unit (a2) derived from linear α-olefin having 2 to 3 carbon atoms, and a ratio (M2 / M1×100)(%) determined by the following procedure is 10% or more and 80% or less. [Procedure] A test piece is created using the resin sheet so that a long direction becomes a MD direction of the resin sheet, an initial inter-chuck distance is set at 30 mm and an inter-chuck distance at the time of elongation is set at 45 mm, and an elongation recovery test is performed at an environment temperature of 23°C and a deformation volume of 1,000% / min. A ratio (M2 / M1×100)(%) of tensile stress M1 of an approach route and tensile stress M2 of a return route at the time of a tensile strain amount of 30% is determined with the tensile strain amount (%) as an axis of abscissa and the tensile stress (MPa) as an axis of ordinate.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin sheet, and more particularly to a resin sheet, a fabric laminate using the resin sheet, and an exercise machine. [Background technology]

[0002] Resin sheets using 4-methyl-1-pentene polymers containing 4-methyl-1-pentene as the main constituent monomer have excellent flexibility and elasticity, and provide a good feel on the skin, and are therefore expected to be widely used in various applications such as hygiene materials, clothing materials, medical materials, etc. For example, Patent Document 1 (International Publication No. 2018 / 143411) discloses an example in which a sheet foamed from a 4-methyl-1-pentene polymer is used as it is for a pressure supporter.

[0003] On the other hand, in light exercise and stretching exercises performed for health promotion, etc., it is desirable to apply a moderate load to muscles and joints. For example, Patent Document 2 (JP 2020-028689 A) discloses a stretch band made of a rubber material. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2018 / 143411 [Patent Document 2] JP 2020-028689 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, conventional stretch bands made of rubber material, such as those disclosed in Patent Document 2, have problems in that when they are stretched by applying force, they rapidly contract if the force is released even slightly, putting stress on the joints and requiring excessive force to slowly return to their original position. [Means for solving the problem]

[0006] Therefore, the present inventors have focused on a new use of a resin sheet using a 4-methyl-1-pentene polymer, that is, as a stretch band, which is not disclosed in Patent Document 1 and the like. They have conducted extensive research into reducing the excessive load during recovery in a stretch band using a conventional rubber material as disclosed in Patent Document 2, and have devised a new index relating to the forward and backward tensile stress of a resin sheet. In other words, they have found that a stretch band capable of reducing the excessive load during recovery can be obtained by producing a resin sheet so as to simultaneously control the forward and backward tensile stress paths, and have completed the present invention.

[0007] That is, according to the present invention, there are provided the following resin sheet and related techniques.

[0008] [1] A resin sheet made of a resin composition containing a 4-methyl-1-pentene polymer (A) and a thermoplastic elastomer (B), The 4-methyl-1-pentene polymer (A) contains a structural unit (a1) derived from 4-methyl-1-pentene and a structural unit (a2) derived from a linear α-olefin having 2 to 3 carbon atoms, A resin sheet in which the ratio (M2 / M1×100) (%) calculated by the following procedure is 10% or more and 80% or less. [procedure] Using the resin sheet, a test piece is prepared so that the long direction is the MD direction of the resin sheet, and an elongation recovery test is performed at an environmental temperature of 23°C and a deformation speed of 1000% / min with an initial chuck distance of 30 mm and an elongation chuck distance of 45 mm. The horizontal axis is the tensile strain amount (%) and the vertical axis is the tensile stress (MPa), and the ratio (M2 / M1 x 100) (%) of the tensile stress M1 on the outward path to the tensile stress M2 on the return path when the tensile strain amount is 30% is calculated. [2] The resin sheet according to [1], wherein in the above-mentioned procedure, the tensile stress (MPa) in the outward path when the tensile strain amount is 10% is 0.1 MPa or more and 1.0 MPa or less. [3] The resin sheet according to [1] or [2], wherein, in the step, the maximum value of the tensile stress (MPa) is 0.4 MPa or more and 1.8 MPa or less. [4] The resin sheet according to any one of [1] to [3], wherein in the above-mentioned procedure, the tensile stress (MPa) in the return path when the tensile strain amount is 40% is 0.1 MPa or more and 1.0 MPa or less. [5] A resin sheet according to any one of [1] to [4], wherein the permanent deformation of the test piece measured under the following conditions is 1% or less. <Condition> Using the resin sheet, a test piece with a width of 25 mm is prepared so that the long direction is the MD direction of the resin sheet, and a gauge line (initial gauge length L0 = 50 mm) is provided. The test piece is pulled with an initial chuck distance of 100 mm, a chuck distance during elongation of 200 mm, a tensile speed of 300 mm / min, and an environmental temperature of 23°C, and after holding the stretched state for 20 minutes, it is immediately returned to the initial chuck distance at 300 mm / min, the test piece is removed, and the gauge length L1 is measured after leaving it on a flat table for 1 hour. The rate of change (L1-L0) / L0 (%) between the initial gauge length L0 and the gauge length L1 after leaving it on the flat table for 1 hour is defined as the permanent strain. [6] The resin sheet according to any one of [1] to [5], wherein the resin sheet has a thickness of 0.1 mm to 10 mm. [7] The density of the resin sheet is 0.1 g / cm 3 ~1.0g / cm 3 The resin sheet according to any one of [1] to [6], [8] The content of the 4-methyl-1-pentene polymer (A) is 40 to 80 mass% based on the total amount of the resin composition; The resin sheet according to any one of [1] to [7], wherein the content of the thermoplastic elastomer (B) is 20 to 60% by mass based on the total amount of the resin composition. [9] The resin sheet according to any one of [1] to [8], wherein the thermoplastic elastomer (B) is one or more selected from the group consisting of thermoplastic styrene-based elastomers, thermoplastic polyamide-based elastomers, thermoplastic polyurethane-based elastomers, and thermoplastic polyester-based elastomers.

[10] The resin sheet according to any one of [1] to [9], wherein the thermoplastic elastomer (B) has a Shore A hardness of A20 to A80.

[11] The resin sheet according to any one of [1] to

[10] , wherein the content of the mineral oil is 5% by mass or more and 20% by mass or less based on the total amount of the resin composition.

[12] A fabric laminate having a fabric bonded to at least one surface of the resin sheet described in any one of [1] to

[10] .

[13] An exercise machine using the resin sheet described in any one of [1] to

[10] . Effect of the Invention

[0009] According to the present invention, it is possible to provide a resin sheet that can provide a stretch band that can reduce excessive load during recovery, and a technique relating to the same. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a graph showing the results of the tensile recovery tests of Examples 1 to 5. [Diagram 2] FIG. 2 is a graph showing the results of the tensile recovery tests of Comparative Examples 1 and 2. [Diagram 3] FIG. 1 is a graph showing the results of the tensile recovery test of Comparative Examples 3 and 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] In this specification, the expression "a to b" in the explanation of a numerical range means from a to b, unless otherwise specified. For example, "1 to 5% by mass" means "1% by mass to 5% by mass."

[0012] In this specification, MD direction stands for machine direction and refers to the flow direction of a resin or sheet, and TD direction stands for transverse direction and refers to the direction perpendicular to the flow direction.

[0013] <Resin sheet> The resin sheet of the present embodiment is constituted by a resin composition containing a 4-methyl-1-pentene polymer (A) and a thermoplastic elastomer (B). The 4-methyl-1-pentene polymer (A) contains a structural unit (a1) derived from 4-methyl-1-pentene and a structural unit (a2) derived from a linear α-olefin having 2 to 3 carbon atoms, and the ratio (M2 / M1×100) (%) calculated by the following procedure is 10% or more and 80% or less.

[0014] [procedure] Using the resin sheet, a test piece is prepared so that the long direction is the MD direction of the resin sheet, and an elongation recovery test is performed at an environmental temperature of 23°C and a deformation speed of 1000% / min with an initial chuck distance of 30 mm and an elongation chuck distance of 45 mm. The horizontal axis is the tensile strain amount (%) and the vertical axis is the tensile stress (MPa), and the ratio (M2 / M1 x 100) (%) of the tensile stress M1 on the outward path to the tensile stress M2 on the return path when the tensile strain amount is 30% is calculated.

[0015] This allows the resin sheet to realize a stretch band that can reduce excessive load during recovery. That is, a normal rubber band can be stretched when force is applied, but when the force is removed, it instantly shrinks and returns to its original state. In contrast, the resin sheet of the present embodiment can be stretched by applying a moderate force, and can slowly recover to its original state even if the force is reduced. As a result, the stretch band using the resin sheet can reduce excessive load during recovery. Furthermore, since the resin sheet contains the 4-methyl-1-pentene polymer (A), it has excellent flexibility and texture, and can provide a good feel when a user grips the stretch band.

[0016] Furthermore, one of the expected effects of a stretch band made using the resin sheet of this embodiment is that after a person stretches the stretch band by hand, the stretch band quickly releases stress and contracts at a slow rate. Therefore, when imagining an exercise in which a person stretches and contracts the stretch band, the user can inhale when stretching the stretch band, and exhale slowly in time with the speed at which the stretch band contracts when it contracts, which is expected to have the effect of regulating the user's breathing. Similarly, when the resin sheet of this embodiment is wrapped around a part of the torso of the body, the resin sheet expands when the user inhales and contracts when the user exhales, which is expected to induce slower breathing in the user and provide a relaxing effect to the user.

[0017] Although the details of the mechanism of the relationship between the configuration of the resin sheet of this embodiment and the action and effect are not clear, it is speculated as follows. First, in the elongation recovery test of the resin sheet of this embodiment, a tensile strain of 30% is considered to correspond to a state in which the user is moving moderately during light exercise or stretching exercise using a stretch band. Therefore, it is speculated that the load felt by the user can be effectively controlled by focusing on the tensile strain of 30%. In addition, the larger the ratio (M2 / M1×100) (%) of the tensile stress M1 in the forward path to the tensile stress M2 in the return path, the smaller the tensile stress in the return path is intended to be relative to the tensile stress in the forward path, and the stretched resin sheet is intended to slowly return to its original length. In other words, since the tensile stress in the return path of the conventional rubber band is as large as that in the forward path, it is likely to shrink rapidly and increase the load on the user.

[0018] The above ratio (M2 / M1×100) (%) is preferably 10% to 60%, and more preferably 15% to 40%, in order to make the load during extension and contraction more suitable.

[0019] Furthermore, in the above procedure, in order to feel an appropriate load at the beginning of tension, the tensile stress (MPa) in the outward movement when the tensile strain amount is 10% is preferably 0.2 MPa to 0.8 MPa, and more preferably 0.3 MPa to 0.8 MPa.

[0020] Furthermore, in the above procedure, in order to further reduce the load during contraction by slowly contracting while feeling a moderate load until the material is fully stretched, the tensile stress (MPa) on the return path when the tensile strain amount is 40% is preferably 0.2 MPa to 0.8 MPa, and more preferably 0.3 MPa to 0.8 MPa.

[0021] Furthermore, in the above procedure, in order to allow a moderate load to be felt until the material is fully pulled, the maximum value of the tensile stress (MPa) is preferably 0.4 MPa to 1.5 MPa, and more preferably 0.8 MPa to 1.3 MPa.

[0022] Moreover, the resin sheet of this embodiment has a test piece with a permanent set of 1% or less measured under the following conditions. This prevents the resin sheet from becoming worn even if it is repeatedly stretched and contracted, and makes it easier to return to its original state.

[0023] <Condition> Using the resin sheet, a test piece with a width of 25 mm is prepared so that the long direction is the MD direction of the resin sheet, and a gauge line (initial gauge distance L0 = 50 mm) is provided. The test piece is pulled with an initial chuck distance of 100 mm, a chuck distance during elongation of 200 mm, a tensile speed of 300 mm / min, and an environmental temperature of 23°C, and after holding the test piece in the elongated state for 20 minutes, it is immediately returned to the initial chuck distance at 300 mm / min, the test piece is removed, and the gauge distance L1 is measured after leaving the test piece on a flat table for 1 hour. The rate of change (L1-L0) / L0 (%) between the initial gauge distance L0 and the gauge distance L1 after leaving the test piece on the flat table for 1 hour is defined as the permanent strain.

[0024] Furthermore, a resin sheet having the above-described tensile stress and its behavior can be realized by selecting the materials constituting the resin sheet, adjusting the blending amounts, and devising a method for manufacturing the resin sheet that combines known methods.

[0025] Next, the physical properties of the resin sheet will be described.

[0026] [Loss tangent (tanδ)] It is preferable that the resin sheet has at least one maximum temperature of loss tangent (tan δ) in the range of 10°C to 100°C, as determined by dynamic viscoelasticity measurement under conditions of a heating rate of 4°C / min, a frequency of 1.59 Hz, and a distortion of 0.1%, and that the maximum value of the loss tangent is 0.5 to 3.5.

[0027] The temperature at which the loss tangent (tan δ) of dynamic viscoelasticity shows a maximum value is preferably at least one in the range of 10°C or higher and 40°C or lower, more preferably at least one in the range of 15°C or higher and 38°C or lower, and even more preferably at least one in the range of 15°C or higher and 38°C or lower. The maximum value of the loss tangent (tan δ) of the dynamic viscoelasticity is preferably 0.8 or more and 4.0 or less, more preferably 1.2 or more and 3.5 or less, and further preferably 1.5 or more and 3.0 or less.

[0028] In this embodiment, the maximum value of the loss tangent of the 4-methyl-1-pentene polymer (a) is preferably 0.8 or more, more preferably 1.0 or more, and even more preferably 1.2 or more. In this embodiment, the maximum value of the loss tangent is preferably 3.0 or less, and more preferably 2.8 or less.

[0029] The dynamic viscoelasticity measurement can be performed, for example, by preparing a test piece of 30 mm length × 10 mm width from the resin sheet of this embodiment and using a rheometer under the following conditions: frequency 1.59 Hz, heating rate 4°C / min, measurement temperature range 0°C to 110°C, distortion amount 0.1%, chuck distance 20 mm, and torsion mode.

[0030] The loss tangent of the resin sheet can be controlled within the above range by appropriately adjusting, for example, the type and blending ratio of the 4-methyl-1-pentene polymer (A), the presence or absence of crosslinking, the molding method of the composition, and the like.

[0031] Thickness The average thickness of the resin sheet is not particularly limited, but is preferably in the range of 0.1 mm to 10 mm, more preferably in the range of 0.2 mm to 5 mm, and even more preferably in the range of 0.3 mm to 3 mm. By setting the average thickness of the resin sheet to be equal to or more than the above lower limit, the feeling of use of the resin sheet can be improved, and the mechanical strength can be improved, thereby expanding the degree of freedom in design. On the other hand, by setting the average thickness of the resin sheet to be equal to or less than the above upper limit, the load during expansion and contraction can be easily improved.

[0032] [density] The density of the resin sheet measured according to ASTM D 1505 (underwater displacement method) is preferably 0.1 to 1.0 g / cm 3 , more preferably 0.3 to 0.9 g / cm 3 , and more preferably 0.5 to 0.8 g / cm 3 It is. By setting the density of the resin sheet to be equal to or higher than the lower limit, the feeling of use of the resin sheet can be improved, the mechanical strength can be improved, and the degree of freedom in design can be widened. On the other hand, by setting the density of the resin sheet to be equal to or lower than the upper limit, the weight can be reduced and the load during expansion and contraction can be easily improved. The density of the resin sheet can be adjusted by the selection of the materials for the resin composition as well as by whether or not the resin sheet is foamed and the degree of foaming.

[0033] [form] The resin sheet of the present embodiment may be in the form of a foam containing air bubbles, or may not be foamed. By using a foam, the stretchability and cushioning properties of the resin sheet are improved, and the feel of the stretch band is improved. The expansion ratio is not particularly limited, and can be appropriately determined taking into consideration the application of the resin sheet, etc. In this embodiment, the resin sheet being a foam refers to a resin sheet having a large number of air bubbles (cavities) therein.

[0034] [Resin composition] Next, the resin composition constituting the resin sheet will be described. The resin composition constituting the resin sheet contains a 4-methyl-1-pentene polymer (A) and a thermoplastic elastomer (B). The 4-methyl-1-pentene polymer (A) and the thermoplastic elastomer (B) may be used alone or as a compound with other components.

[0035] [4-Methyl-1-pentene polymer (A)] The 4-methyl-1-pentene polymer (A) contains, for example, a structural unit (a1) derived from 4-methyl-1-pentene and a structural unit (a2) derived from an α-olefin having 2 to 3 carbon atoms other than 4-methyl-1-pentene.

[0036] In the 4-methyl-1-pentene polymer (A) according to this embodiment, from the viewpoint of further improving the flexibility of the resin sheet, when the sum of the structural units (a1) and (a2) is taken as 100 mol %, it is preferable that the content of the structural unit (a1) is 10 mol % or more and 90 mol % or less, and the content of the structural unit (a2) is 10 mol % or more and 90 mol % or less. In addition, in the 4-methyl-1-pentene polymer (A) according to this embodiment, from the viewpoint of improving the flexibility and mechanical properties of the resin sheet, when the sum of the structural units (a1) and (a2) is taken as 100 mol%, the content of the structural unit (a1) is more preferably 30 mol% or more and 90 mol% or less, and the content of the structural unit (a2) is more preferably 10 mol% or more and 70 mol% or less, the content of the structural unit (a1) is even more preferably 50 mol% or more and 90 mol% or less, and the content of the structural unit (a2) is even more preferably 10 mol% or more and 50 mol% or less, the content of the structural unit (a1) is even more preferably 60 mol% or more and 90 mol% or less, and the content of the structural unit (a2) is even more preferably 10 mol% or more and 40 mol% or less, and the content of the structural unit (a1) is particularly preferably 65 mol% or more and 90 mol% or less, and the content of the structural unit (a2) is particularly preferably 10 mol% or more and 35 mol% or less.

[0037] Examples of the structural unit (a2) derived from a linear α-olefin having 2 to 3 carbon atoms include ethylene and propylene, with propylene being preferred from the viewpoint of obtaining flexibility while maintaining mechanical strength.

[0038] The 4-methyl-1-pentene polymer (A) may contain structural units other than the structural units (a1) and (a2) as long as the object of the present invention is not impaired. Examples of other structural units include structural units derived from non-conjugated polyenes. Examples of the non-conjugated polyene include linear, branched or cyclic dienes having preferably 5 to 20 carbon atoms, more preferably 5 to 10 carbon atoms, various norbornenes, norbornadienes, etc. Among these, 5-vinylidene-2-norbornene and 5-ethylidene-2-norbornene are preferred.

[0039] The 4-methyl-1-pentene polymer (A) according to this embodiment has an intrinsic viscosity [η] in decalin at 135° C. of preferably 0.01 to 5.0 dL / g, more preferably 0.1 to 4.0 dL / g, even more preferably 0.5 to 3.0 dL / g, and particularly preferably 1.0 to 2.8 dL / g, from the viewpoint of improving the flexibility and mechanical strength of the resin sheet.

[0040] The density of the 4-methyl-1-pentene polymer (A) according to this embodiment, measured according to ASTM D 1505 (water displacement method), is preferably 0.810 to 0.850 g / cm 3 , more preferably 0.820 to 0.850 g / cm 3 , and more preferably 0.830 to 0.850 g / cm 3 It is.

[0041] The 4-methyl-1-pentene polymer (A) according to the present embodiment can be produced by various methods. For example, it can be produced by using known catalysts such as magnesium-supported titanium catalysts; metallocene catalysts described in International Publication No. 01 / 53369, International Publication No. 01 / 027124, JP-A-3-193796, and JP-A-02-41303; and olefin polymerization catalysts containing metallocene compounds described in International Publication No. 2011 / 055803.

[0042] The content of the 4-methyl-1-pentene polymer (A) is preferably 40 to 80% by mass based on the total amount of the resin composition, which makes it possible to obtain a resin sheet having a better balance between breathability and mechanical properties.

[0043] [Thermoplastic elastomer (B)] The thermoplastic elastomer (B) has good compatibility with the 4-methyl-1-pentene polymer (A), and therefore, it becomes possible to obtain stable extensibility and shrinkability while maintaining mechanical strength.

[0044] The Shore A hardness of the thermoplastic elastomer (B) is preferably A20 to A80. By setting the Shore A hardness of the thermoplastic elastomer (B) within the above range, it becomes easier to control the appropriate load during elongation and contraction.

[0045] The Shore A hardness of the thermoplastic elastomer (B) can be measured in accordance with JIS K6253.

[0046] The thermoplastic elastomer (B) preferably contains, for example, one or more selected from thermoplastic styrene-based elastomers, thermoplastic polyurethane-based elastomers, thermoplastic polyamide-based elastomers, and thermoplastic polyester-based elastomers.

[0047] Examples of thermoplastic styrene-based elastomers include hydrogenated styrene-isoprene block copolymers (SEPS), hydrogenated styrene-butadiene block copolymers (SEBS), and hydrogenated styrene-isoprene-butadiene block copolymers (SEEPS).

[0048] The content of the thermoplastic elastomer (B) is preferably 20 to 90% by mass, more preferably 30 to 80% by mass, based on the total amount of the resin composition, which allows for good control of the load during elongation and contraction.

[0049] The total content of the 4-methyl-1-pentene polymer (A) and the thermoplastic elastomer (B) is preferably 60% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more, or may be 100% by mass, based on the total amount of the resin composition, which allows the load during elongation and contraction to be well controlled.

[0050] [Other ingredients] The resin sheet according to the present embodiment may contain components other than the 4-methyl-1-pentene polymer (A) and the thermoplastic elastomer (B) as necessary, within the scope that does not impair the effects of the present invention.

[0051] The resin sheet of the present embodiment may contain mineral oil. Examples of mineral oil include aromatic (aromatic) hydrocarbon compounds, naphthenic (cyclocyclic) hydrocarbon compounds, paraffinic (aliphatic) hydrocarbon compounds, and mixtures thereof. The kinetic viscosity of mineral oil at 40°C is 120mm 2 / s or more 800mm 2 Specifically, the kinetic viscosity at 40°C may be 120 mm 2 / s or more 800mm 2 As a result, it is possible to obtain a resin sheet that satisfactorily controls the load during expansion and contraction. 2 / s~600mm 2 It is preferable to use liquid paraffin having a molecular weight of 1000 to 15000. When the resin sheet contains mineral oil, the content of the mineral oil is preferably 20% by mass or less, more preferably 18% by mass or less, and more preferably 5% by mass or more, based on the total amount of the resin composition, thereby obtaining a resin sheet that can withstand an appropriate load during elongation and contraction. In this embodiment, the mineral oil may be one component contained in the mixture containing the thermoplastic elastomer (B).

[0052] In addition, the resin sheet of the present embodiment has an inorganic particle content of preferably 5% by mass or less, more preferably 3% by mass or less, and further preferably 1% by mass or less, based on the total amount of the resin composition, thereby obtaining a resin sheet that can withstand an appropriate load during elongation and contraction.

[0053] Specific examples of inorganic particles include carbon black or carbon black that has been surface-treated with graphite or a silane coupling agent, finely powdered silicic acid, silica (including fumed silica, precipitated silica, diatomaceous earth, and quartz), oxide-based fillers including alumina, iron oxide, ferrite, magnesium oxide, titanium oxide, antimony trioxide, zirconium oxide, barium oxide, and calcium oxide, hydroxide-based fillers including aluminum hydroxide and magnesium hydroxide, silicate-based fillers including aluminum silicate (clay), magnesium silicate (talc), mica, kaolin, calcium silicate, glass fiber, glass flakes, and glass beads, sedimentary rock-based fillers including diatomaceous earth and limestone, montmorillonite, magnesian montmorillonite, and the like. Examples of suitable fillers include clay mineral-based fillers such as quartz, ferromontmorillonite, ferromagnesianmontmorillonite, beidellite, aluminianbeidellite, nontronite, aluminiannontronite, saponite, aluminiansaponite, hectorite, sauconite, stevensite, and bentonite; magnetic fillers such as ferrite, iron, and cobalt; conductive fillers such as silver, gold, copper, and alloys thereof; thermally conductive fillers such as aluminum nitride, boron nitride, and silicone carbide; sulfate-based fillers such as aluminum sulfate, magnesium sulfate, barium sulfate, and calcium sulfate; sulfite-based fillers such as calcium sulfite; calcium carbonate, basic magnesium carbonate, dolomite, barium titanate, and potassium titanate.

[0054] Moreover, it is preferable that the resin sheet of the present embodiment does not contain inorganic particles having an average particle size of 0.01 to 100 μm.

[0055] The resin sheet according to this embodiment may contain additives such as foaming agents, foaming modifiers, heat stabilizers, antioxidants, UV absorbers, pigments, antistatic agents, copper damage inhibitors, flame retardants, neutralizing agents, plasticizers, nucleating agents, weather stabilizers, light stabilizers, anti-aging agents, fatty acid metal salts, softeners, dispersants, colorants, lubricants, natural oils, synthetic oils, and waxes.

[0056] (foaming agent) The foaming agent includes chemical foaming agents and physical foaming agents. Chemical foaming agents include sodium bicarbonate, ammonium bicarbonate, various carboxylates, sodium borohydride, azodicarboxamide, N,N-dinitrosopentamethylenetetramine, P,P-oxybis(benzenesulfonyl hydrazide), azobisisobutyronitrile, paratoluenesulfonyl hydrazide, and sodium hydrogen carbonate. Physical blowing agents include carbon dioxide, nitrogen, or a mixture of carbon dioxide and nitrogen, any of which can be supplied in gaseous, liquid, or supercritical state.

[0057] [Manufacturing method of resin sheet] The resin sheet of this embodiment can be produced by mixing or melt-kneading the raw materials, 4-methyl-1-pentene polymer (A), thermoplastic elastomer (B), and other optional components, by a known method such as dry blending, a tumbler mixer, a Banbury mixer, a single screw extruder, a twin screw extruder, a high-speed twin screw extruder, or a heat roll to prepare a resin composition, and extruding the resin composition into a sheet by a known method. The extruded sheet is cooled by a cooling roll and taken up by a take-up machine.

[0058] Examples of the method for foaming the resin sheet include the following methods. When a chemical foaming agent is used, a resin composition other than the chemical foaming agent is charged into an extruder together with the chemical foaming agent, and the mixture is mixed uniformly, and then foamed while being extruded into a sheet. In addition, when carbon dioxide is used as a physical foaming agent, a method can be mentioned in which the resin composition is charged into an extrusion molding machine, kneaded in the extrusion molding machine, and after the resin composition is plasticized, carbon dioxide is directly injected into the extrusion molding machine to foam the resin composition while extruding it into a sheet.

[0059] <Fabric laminate> The fabric laminate of this embodiment is a resin sheet composed of a resin composition containing a 4-methyl-1-pentene polymer (A) and a thermoplastic elastomer (B), the 4-methyl-1-pentene polymer (A) containing a structural unit (a1) derived from 4-methyl-1-pentene and a structural unit (a2) derived from a linear α-olefin having 2 to 3 carbon atoms, and the ratio (M2 / M1×100) (%) obtained by the above procedure is 10% or more and 80% or less, and a fabric is laminated on at least one surface of the resin sheet. This makes it possible to realize a fabric laminate that can reduce excessive load during recovery. In addition, even if the resin sheet has self-adhesiveness, the self-adhesiveness can be prevented by covering the surface of the resin sheet with the fabric.

[0060] The fabric is a material obtained by processing fibers such as natural fibers, synthetic fibers, and chemical fibers into thin pieces, and examples of the fabric include woven fabrics such as woven cloth, nonwoven fabrics, etc. Specific examples of the fabric include knitted fabrics having a weft knitting structure such as plain knit, milling, smooth, and double knit, knitted fabrics having a warp knitting structure such as tricot and raschel, and woven fabrics having a structure such as plain weave, twill, and satin.

[0061] From the viewpoints of adhesion to the resin sheet and maintaining the properties of the resin sheet, the thickness of the material is preferably 0.2 to 1.0 mm, more preferably 0.2 to 0.8 mm, and even more preferably 0.2 to 0.6 mm.

[0062] The basis weight of the fabric is not particularly limited from the viewpoint of adhesiveness and heat resistance, but is preferably 75 to 300 g / m2 from the viewpoint of handling. 2 It is preferable that the thickness is 90 to 250 g / m 2 More preferably, the thickness is 100 to 200 g / m 2 It is even more preferable that:

[0063] Fabric materials include natural fibers such as cotton, linen, wool, and silk; regenerated fibers such as rayon and cupra; semi-synthetic fibers such as acetate and triacetate; synthetic fibers such as nylon, polyester, polyurethane, acrylic, and rayon, as well as chemical fiber products made from blends of these synthetic fibers. Of these, synthetic fibers are preferred, and one or more types selected from nylon, polyester, polyurethane, acrylic, and rayon are more preferred.

[0064] The fabric laminate may be a resin sheet having fabrics laminated on both sides thereof. In this case, the fabric on one side of the resin sheet and the fabric on the other side of the resin sheet may be made of the same material or different materials. The fabric laminate may be one in which fabric is laminated on the entire surface or a portion of the surface of a resin sheet, or one in which a resin sheet is laminated on the entire surface or a portion of the surface of the fabric.

[0065] The thickness of the fabric laminate of this embodiment is appropriately adjusted taking into consideration flexibility, processability, ease of sewing, and the like.

[0066] [Method of manufacturing fabric laminate] The method of manufacturing the fabric laminate includes the following steps. (Step) A fabric is laid on at least one surface of the resin sheet and heat-sealed under conditions of 140 to 190° C. and 1.0 to 1.8 MPa to obtain a fabric laminate.

[0067] Among them, when laminating with the fabric, it is preferable to perform lamination at 140 to 190°C and 1.0 to 1.8 MPa. The lamination time is 30 seconds to 10 minutes, which provides good production efficiency. This makes it possible to obtain a fabric laminate while maintaining the properties of the sheet composition of the present embodiment. In order to improve the stretchability of the laminate, it is more preferable to laminate the resin sheets so that the MD direction of the resin sheet is parallel to the warp direction of the fabric, but this is not limited thereto. The resin sheets may be laminated so that the TD direction of the resin sheet is parallel to the warp direction of the fabric.

[0068] <Application> The resin sheet and fabric laminate according to the present embodiment are widely used regardless of the field, but because of their excellent elasticity, they are suitable for use in medical products such as rehabilitation, health care, and nursing care support products, and exercise equipment for training, supporters, massage, sports, etc. Specific examples of exercise equipment include stretch bands, stretch belts, exercise bands, training bands, and training belts.

[0069] The form of the resin sheet and the fabric laminate is not particularly limited, but may be, for example, a strip, a loop or a ring, a partly branched, a partly loop or ring, etc. The length and width of the resin sheet and the fabric laminate can be appropriately set depending on the application and the method of use.

[0070] Furthermore, the resin sheet and the fabric laminate may have a gripping portion, a hooking portion, a fitting portion, a joining portion, etc., depending on the application and the method of use, etc. Furthermore, they may have a length / size adjustment function, an auxiliary function, etc.

[0071] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above may also be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention. EXAMPLES

[0072] The present embodiment will be described in detail below with reference to examples and comparative examples, but the present embodiment is not limited to the descriptions of these examples.

[0073] (1)Measurement method Composition of 4-methyl-1-pentene polymer (A) The contents of 4-methyl-1-pentene and α-olefin in 4-methyl-1-pentene polymers are 13 Quantitative analysis was performed using C-NMR.

[0074] (2) Raw materials [4-Methyl-1-pentene polymer (A)] Copolymer of 4-methyl-1-pentene and propylene (content of 4-methyl-1-pentene-derived structural units (a1): 72 mol%, content of propylene-derived structural units (a2): 28 mol%) Glass transition temperature: 30°C, intrinsic viscosity [η] in decalin at 135°C: 1.5 dL / g, MFR: 10 g / 10 min

[0075] [Thermoplastic elastomer (B)] Thermoplastic elastomer (B)-1: "Hybra 7311F" hydrogenated styrene-isoprene-butadiene block copolymer (SEEPS), manufactured by Kuraray Co., Ltd., Shore A hardness A41 Thermoplastic elastomer (B)-2: "Septon 2004F" hydrogenated styrene-isoprene block copolymer (SEPS) manufactured by Kuraray Co., Ltd., Shore A hardness A67 Thermoplastic elastomer (B)-3: "Tuftec H1272" mineral oil-containing styrene-based elastomer compound, manufactured by Asahi Kasei Corporation, Shore A hardness A35, mineral oil content 36% by mass Thermoplastic elastomer (B)-4: "Arneston CJ102NS" mineral oil-containing styrene-based elastomer compound, manufactured by Kuraray Plastics Co., Ltd., Shore A hardness A35, mineral oil content 45% by mass Thermoplastic elastomer (B)-5: "Arneston JH28NS" mineral oil-containing styrene-based elastomer compound, manufactured by Kuraray Plastics Co., Ltd., Shore A hardness A37, mineral oil content 55% by mass Thermoplastic elastomer (B)-6: "Kraton G4609" mineral oil-containing styrene-based elastomer compound, manufactured by Kraton Polymer Japan, Shore A hardness A22, mineral oil content 45% by mass

[0076] [others] Foaming agent 1: "EE275F" Polythrene, manufactured by Eiwa Kasei Co., Ltd. Natural rubber band 1; "Latex Band EX Super Hard" made by IGNIO, thickness 0.7mm, width 25mm Natural rubber band 2; "O-Band #35" made by Kyowasha, thickness 1.1mm, width 21mm

[0077] (3) Preparation of resin sheet <Example 1> The molding machine used was a single-screw extruder (cylinder inner diameter D: 50 mm, full-flight screw, L / D: 32 mm when L is the effective screw length, T-die (die width: 320 mm, lip opening: 0.5 to 1.8 mm), cooling roll (outer diameter 50 mm, made of steel with mirror-finished hard chrome plating surface treatment, water-cooled), and a take-up machine. First, the raw materials were dry-blended in the proportions shown in Table 1 (the units in the table are parts by mass), and the resulting mixture was placed in a hopper. The raw material components were melted and kneaded under conditions of a temperature of 120-250°C in each part of the cylinder and a screw rotation speed of 40-70 rpm, and extruded from a T-die so that the resin temperature at the cylinder head was 120-200°C and the extrusion rate was 10-13 kg / hr. The extruded foam sheet was taken up using a take-up machine (take-up speed 0.4-2.3 m / min) to obtain a resin sheet with a sheet width of approximately 300 mm.

[0078] <Examples 2 to 5, Comparative Examples 1 to 2> A resin sheet was obtained under the same processing conditions as in Example 1, except that the raw materials and raw material compositions were changed to those shown in Table 1.

[0079] (4) Evaluation and measurement The following evaluations and measurements were carried out using the resin sheets of the Examples obtained in (3) above. In addition, the resin sheets were replaced with the rubber pads of the Comparative Examples, and the same evaluations and measurements were carried out. The results are shown in Table 1.

[0080] [Elongation recovery test] Using each resin sheet, a test piece was prepared so that the long direction was the MD direction of the resin sheet, and an elongation recovery test was performed at an environmental temperature of 23°C and a deformation rate of 1000% / min with an initial chuck distance of 30 mm and an elongation chuck distance of 45 mm, to obtain a tensile curve with the tensile strain amount (%) on the horizontal axis and the tensile stress (MPa) on the vertical axis. The tensile curves are shown in Figures 1 to 3. In addition, the ratio (M2 / M1 x 100) (%) of the tensile stress M1 on the outward path when the tensile strain amount is 30% to the tensile stress M2 on the return path, the tensile stress (MPa) on the outward path when the tensile strain amount is 10%, the maximum tensile stress (MPa), and the tensile stress (MPa) on the return path when the tensile strain amount is 40% were also calculated. In addition, the above deformation rate was changed to 100% / min and 500% / min, and similar tests were performed to determine (M2' / M1' x 100) (%) and (M2'' / M1'' x 100) (%) at each deformation rate.

[0081] [Permanent set] Using each resin sheet, a test piece of 25 mm width was prepared so that the long direction was the MD direction of the resin sheet, and a gauge line (initial gauge distance L0 = 50 mm) was provided. The test piece was pulled with an initial chuck distance of 100 mm, a chuck distance during elongation of 200 mm, a tensile speed of 300 mm / min, and an environmental temperature of 23 ° C., and held in the elongated state for 20 minutes, and then immediately returned to the initial chuck distance at 300 mm / min, the test piece was removed, and the gauge distance L1 was measured after leaving it on a flat table for 1 hour. The rate of change (L1-L0) / L0 (%) between the initial gauge distance and the gauge distance L1 after leaving it on the flat table for 1 hour was taken as the permanent strain.

[0082] [density] The weight was calculated from the weight of the resin sheet measured in water and in air using an ALFA MIRAGE electronic specific gravity meter MD-300S in accordance with ASTM D 1505 (underwater displacement method).

[0083] [Appropriate load evaluation during extension and contraction] The resin sheet was cut to a width of 50 mm and a length of 1 m. Five panelists (men in their 20s to 60s) held the resulting long sheet in both hands and performed arm stretching exercises, stretching and contracting it 30 times until the maximum extension length was approximately 1.5 m. Each of the five panelists evaluated the sheet according to the following criteria, and the sheet with the most votes was recorded as the evaluation result. (standard) A: Although I felt slight fatigue in my arms, the load during contraction (on the return trip) was just right and I was able to exercise. B: The load was weaker during extension (forward travel) and stronger during contraction (return travel). C1: Too much force was applied during contraction (return stroke) and this put strain on the arm. C2: There was no load during elongation (on the way forward), so it did not result in a stretching exercise.

[0084] [Table 1]

Claims

1. A resin sheet made of a resin composition containing a 4-methyl-1-pentene polymer (A) and a thermoplastic elastomer (B), the 4-methyl-1-pentene polymer (A) contains a structural unit (a1) derived from 4-methyl-1-pentene and a structural unit (a2) derived from a linear α-olefin having 2 to 3 carbon atoms; A resin sheet, in which a ratio (M2 / M1×100) (%) calculated by the following procedure is 10% or more and 80% or less. [procedure] Using the resin sheet, a test piece is prepared so that the long direction is the MD direction of the resin sheet, and an elongation recovery test is performed with an initial chuck distance of 30 mm and an elongation chuck distance of 45 mm at an environmental temperature of 23° C. and a deformation rate of 1000% / min. The horizontal axis represents the tensile strain amount (%) and the vertical axis represents the tensile stress (MPa), and the ratio (M2 / M1×100) (%) of the tensile stress M1 on the outward path to the tensile stress M2 on the return path when the tensile strain amount is 30% is calculated.

2. The resin sheet according to claim 1 , wherein in the step, a tensile stress (MPa) in a forward path when a tensile strain amount is 10% is 0.1 MPa or more and 1.0 MPa or less.

3. The resin sheet according to claim 1 or 2, wherein in the step, the maximum value of the tensile stress (MPa) is 0.4 MPa or more and 1.8 MPa or less.

4. The resin sheet according to claim 1 or 2, wherein in the procedure, a tensile stress (MPa) in the return path when the tensile strain amount is 40% is 0.1 MPa or more and 1.0 MPa or less.

5. The resin sheet according to claim 1 or 2, wherein the test piece has a permanent deformation of 1% or less when measured under the following conditions. <Conditions> Using the resin sheet, a test piece of 25 mm width is prepared so that the long direction is the MD direction of the resin sheet, and a gauge line (initial gauge distance L0 = 50 mm) is provided. The test piece is pulled with an initial chuck distance of 100 mm, a chuck distance during elongation of 200 mm, a tensile speed of 300 mm / min, and an environmental temperature of 23 ° C., and after holding the stretched state for 20 minutes, it is immediately returned to the initial chuck distance at 300 mm / min, the test piece is removed, and the gauge distance L1 after being left on a flat table for 1 hour is measured. The rate of change (L1-L0) / L0 (%) between the initial gauge distance L0 and the gauge distance L1 after being left on the flat table for 1 hour is defined as the permanent strain.

6. The resin sheet according to claim 1 or 2, wherein the resin sheet has a thickness of 0.1 mm to 10 mm.

7. The density of the resin sheet is 0.1 g / cm 3 ~1.0 g / cm 3 The resin sheet according to claim 1 or 2,

8. The content of the 4-methyl-1-pentene polymer (A) is 40 to 80% by mass based on the total amount of the resin composition, The resin sheet according to claim 1 or 2, wherein the content of the thermoplastic elastomer (B) is 20 to 60 mass% based on the total amount of the resin composition.

9. 3. The resin sheet according to claim 1, wherein the thermoplastic elastomer (B) is one or more selected from the group consisting of thermoplastic styrene-based elastomers, thermoplastic amide-based elastomers, thermoplastic urethane-based elastomers, and thermoplastic ester-based elastomers.

10. The resin sheet according to claim 1 or 2, wherein the thermoplastic elastomer (B) has a Shore A hardness of A20 to A80.

11. The resin sheet according to claim 1 or 2, wherein a content of the mineral oil is 5% by mass or more and 20% by mass or less with respect to a total amount of the resin composition.

12. A fabric laminate comprising the resin sheet according to claim 1 or 2 and a fabric laminated to at least one surface of the resin sheet.

13. An exercise machine using the resin sheet according to claim 1 or 2.

Citation Information

Patent Citations

  • Massage device used also as stretch device

    JP2020028689A

  • Foam body, polyolefin-based foam sheet and complex

    WO2018143411A1