Optical glass, optical element, light guide plate and image display device
The optical glass composition with specific ratios of SiO2, B2O3, TiO2, Nb2O5, Y2O3, La2O3, and Gd2O3 suppresses surface devitrification, maintaining high refractive index and quality in optical elements and light guide plates.
Patent Information
- Application Number
- JP2023058566
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Optical glasses with high refractive index often suffer from surface devitrification, which decreases yield and makes quality inspection difficult, especially when processed into lenses or light guide plates.
The optical glass composition includes SiO2, B2O3, TiO2, Nb2O5, Y2O3, La2O3, and Gd2O3, with specific mass ratios and contents that suppress surface devitrification while maintaining a high refractive index, as well as controlling the melting temperature to prevent devitrification.
The solution provides optical glass with a high refractive index that effectively suppresses surface devitrification, ensuring higher yield and quality consistency in optical elements and light guide plates.
Smart Images

Figure 2024145945000006 
Figure 2024145945000007 
Figure 2024145945000008
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical glass, an optical element, a light guide plate, and an image display device. [Background technology]
[0002] For example, Patent Documents 1 and 2 disclose optical glasses with high refractive index. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 5931173 [Patent Document 2] JP 2019-116408 A Summary of the Invention [Problem to be solved by the invention]
[0004] Optical glass with a high refractive index can correct chromatic aberration and compact the optical system by, for example, combining a lens made of this glass with another lens made of glass with a different dispersion to form a cemented lens, and therefore such optical glass is useful as a material for optical elements constituting imaging optical systems and projection optical systems such as projectors.
[0005] Light guide plates, which are components of image display devices, are also manufactured from optical glass. Optical glass with a high refractive index allows the manufacture of light guide plates with a wide viewing angle.
[0006] One of the physical properties desired for optical glass is that the glass surface is resistant to devitrification. When glass with a devitrified surface is processed into lenses, light guide plates, etc., the devitrified parts must be removed. Therefore, surface devitrification causes a decrease in yield. In addition, glass with a devitrified surface has a cloudy glass surface, making it difficult to inspect the quality of the inside of the glass.
[0007] In view of the above, an object of one aspect of the present invention is to provide an optical glass that has a high refractive index and is suppressed from undergoing surface devitrification. [Means for solving the problem]
[0008] One aspect of the present invention is as follows. [1] It contains SiO2, B2O3, TiO2, Nb2O5, Y2O3, La2O3 and Gd2O3 as essential components. On a mass basis, The mass ratio of the B2O3 content to the SiO2 content (B2O3 / SiO2) is less than 1.000; The mass ratio of the Y2O3 content to the total content of Y2O3, La2O3, Gd2O3, and Yb2O3 (Y2O3 / (Y2O3+La2O3+Gd2O3+Yb2O3)) is greater than 0.020; and An optical glass with a refractive index nd exceeding 2.00000. [2] The optical glass according to [1], wherein the mass ratio (Y2O3 / (Y2O3+La2O3+Gd2O3+Yb2O3)) is greater than 0.020 and not greater than 0.100. [3] The optical glass according to [1] or [2], in which the mass ratio of the TiO2 content to the total content of SiO2 and B2O3 (TiO2 / (SiO2+B2O3)) is 1.950 or more. [4] The optical glass according to any one of [1] to [3], wherein the total content of SiO2 and B2O3 (SiO2 + B2O3) is 30.00 mass% or less. [5] The optical glass according to any one of [1] to [4], which has a refractive index nd of 2.08000 or more. [6] The optical glass according to any one of [1] to [5], which has a melt-switching temperature Tl of 1247° C. or lower in differential scanning calorimetry. [7] The optical glass according to any one of [1] to [6], which has a melt-switching temperature Tl in differential scanning calorimetry of 1245° C. or lower. [8] The mass ratio (Y2O3 / (Y2O3+La2O3+Gd2O3+Yb2O3)) is greater than 0.020 and less than or equal to 0.100; The mass ratio of the TiO2 content to the total content of SiO2 and B2O3 (TiO2 / (SiO2+B2O3)) is 1.950 or more; The total content of SiO2 and B2O3 (SiO2 + B2O3) is 12.00 mass% or less, The refractive index nd is 2.08000 or more, The optical glass according to any one of [1] to [7], which has a melt-switching temperature Tl of 1247° C. or lower in differential scanning calorimetry. [9] The optical glass according to [8], which has a melt-switching temperature Tl in differential scanning calorimetry of 1245°C or lower.
[10] An optical element comprising the optical glass according to any one of [1] to [9].
[11] A light guide plate made of the optical glass according to any one of [1] to [9].
[12] An image display element; a light guide plate that guides light emitted from the image display element; Including, The image display device, wherein the light guide plate is the light guide plate according to
[11] . Effect of the Invention
[0009] According to one aspect of the present invention, an optical glass having a high refractive index and suppressed surface devitrification can be provided. According to another aspect of the present invention, there are provided an optical element and a light guide plate made of the above optical glass, and an image display device including the light guide plate. [Brief description of the drawings]
[0010] [Figure 1] 1 is a photograph of a glass block of optical glass of Example 13 (left) and a glass block of optical glass of Comparative Example 1 (right). [Diagram 2] 1 is a schematic diagram illustrating an example of an image device (head mounted display) including an image display element and a light guide plate. [Diagram 3] 3 is a side view diagrammatically illustrating the configuration of the head mounted display 1 shown in FIG. 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] [Optical glass] In the present invention and this specification, the glass composition is expressed as a glass composition based on oxides. Here, "glass composition based on oxides" refers to a glass composition obtained by converting the glass raw materials into oxides that are present in the glass after being completely decomposed during melting. Furthermore, unless otherwise specified, the glass composition is expressed on a mass basis (mass %, mass ratio). The glass composition of the present invention and this specification can be determined by a method such as ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). Quantitative analysis is performed for each element using ICP-AES. The analytical values are then converted into oxide notation. The analytical values obtained by ICP-AES may contain a measurement error of, for example, about ±5% of the analytical value. Therefore, the oxide notation values converted from the analytical values may also contain an error of about ±5%. In the present invention and this specification, the content of a component being 0%, 0.00%, 0.000%, or not being contained or not being introduced means that the component is substantially not contained, and the content of the component is at or below the level of impurities. At or below the level of impurities means, for example, less than 0.01%.
[0012] The optical glass (also simply referred to as "glass") contains SiO2, B2O3, TiO2, Nb2O5, Y2O3, La2O3 and Gd2O3 as essential components. In such glass, the mass ratio of the B2O3 content to the SiO2 content (B2O3 / SiO2) is less than 1.00, and the mass ratio of the Y2O3 content to the total content of Y2O3, La2O3, Gd2O3 and Yb2O3 (Y2O3 / (Y2O3+La2O3+Gd2O3+Yb2O3)) is more than 0.020, which can contribute to suppression of surface devitrification.
[0013] The glass composition of the above optical glass will now be described in more detail.
[0014] <Glass composition> The mass ratio of the B2O3 content to the SiO2 content (B2O3 / SiO2) is less than 1.000, preferably 0.980 or less, more preferably 0.960 or less, 0.950 or less, 0.920 or less, and 0.900 or less, in that order, from the viewpoint of suppressing surface devitrification and reducing Tl, which will be described later. The mass ratio (B2O3 / SiO2) can be, for example, 0.100 or more, 0.200 or more, 0.300 or more, 0.400 or more, 0.500 or more, or 0.600 or more.
[0015] The mass ratio of the Y2O3 content to the total content of Y2O3, La2O3, Gd2O3 and Yb2O3 (Y2O3 / (Y2O3+La2O3+Gd2O3+Yb2O3)) is more than 0.020, preferably 0.021 or more, more preferably 0.022 or more, 0.023 or more, 0.024 or more, and 0.025 or more in this order, from the viewpoint of suppressing surface devitrification and reducing Tl. The mass ratio (Y2O3 / (Y2O3+La2O3+Gd2O3+Yb2O3)) can be, for example, 0.100 or less, 0.090 or less, 0.080 or less, 0.070 or less, 0.060 or less, or 0.050 or less.
[0016] The optical glass contains, as essential components, SiO2, B2O3, TiO2, Nb2O5, Y2O3, La2O3 and Gd2O3.
[0017] SiO2 is a network-forming oxide, and is a component that can contribute to maintaining glass stability, maintaining viscosity suitable for forming molten glass, and improving chemical durability. Increasing glass stability is preferable because it leads to suppressing surface devitrification of glass. The SiO2 content of the optical glass is preferably 0.10% or more, more preferably 0.50% or more, and further preferably 1.00% or more, 2.00% or more, 3.00% or more, 4.00% or more, and 5.00% or more in that order. From the viewpoint of suppressing the decrease in refractive index and maintaining glass meltability, the SiO2 content is preferably 30.00% or less, more preferably 20.00% or less, and further preferably 15.00% or less, 10.00% or less, 8.00% or less, and 6.00% or less in that order.
[0018] B2O3 is a network-forming oxide, and is a component that can contribute to maintaining glass meltability and improving glass stability. The B2O3 content of the optical glass is preferably 0.10% or more, more preferably 0.50% or more, and further preferably 1.00% or more, 2.00% or more, 3.00% or more, 4.00% or more, and 5.00% or more in that order. From the viewpoint of suppressing the decrease in refractive index and the decrease in chemical durability, the B2O3 content is preferably 30.00% or less, more preferably 20.00% or less, and further preferably 15.00% or less, 10.00% or less, 8.00% or less, and 6.00% or less in that order.
[0019] From the viewpoint of improving the stability of the glass, the total content of SiO2 and B2O3 (SiO2+B2O3) is preferably 1.00% or more, more preferably 3.00% or more, and further preferably 5.00% or more, 8.00% or more, and 10.00% or more. From the viewpoint of increasing the refractive index of the glass, the total content (SiO2+B2O3) is preferably 30.00% or less, more preferably 20.00% or less, and further preferably 15.00% or less, 13.00% or less, and 12.00% or less.
[0020] TiO2 is a component that can increase the refractive index of glass and contribute to improving chemical durability. The TiO2 content of the optical glass is preferably 1.00% or more, more preferably 3.00% or more, and more preferably 5.00% or more, 8.00% or more, 10.00% or more, 13.00% or more, 15.00% or more, 18.00% or more, and 20.00% or more in this order. From the viewpoint of suppressing the deterioration of glass stability, the TiO2 content is preferably 50.00% or less, more preferably 45.00% or less, and more preferably 40.00% or less, 35.00% or less, 30.00% or less, 28.00% or less, and 26.00% or less in this order.
[0021] From the viewpoint of increasing the refractive index of the glass, the mass ratio of the TiO2 content to the total content of SiO2 and B2O3 (TiO2 / (SiO2+B2O3)) is preferably 1.950 or more, more preferably 1.960 or more, further preferably 1.970 or more, 1.980 or more, 1.990 or more, or 2.000 or more. From the viewpoint of improving the glass stability, it is preferably 10.000 or less, more preferably 8.000 or less, and further preferably 5.000 or less, 3.000 or less, 2.800 or less, and 2.500 or less in that order.
[0022] Nb2O5 is a component that can increase the refractive index of glass and contribute to improving chemical durability. The Nb2O5 content of the optical glass is preferably 1.00% or more, more preferably 2.00% or more, and further preferably 3.00% or more, 4.00% or more, 5.00% or more, and 6.00% or more in that order. From the viewpoint of suppressing a decrease in glass stability, the Nb2O5 content is preferably 30.00% or less, more preferably 20.00% or less, and further preferably 15.00% or less, 10.00% or less, and 8.00% or less in that order.
[0023] The WO3 content of the optical glass can be 0.00%, 0.00% or more, or more than 0.00%. WO3 is a component that can increase the refractive index of glass and contribute to improving chemical durability. The WO3 content can be, for example, 8.00% or less, 7.00% or less, 6.00% or less, or 5.00% or less.
[0024] From the viewpoint of increasing the refractive index of the glass and improving the chemical durability, the total content of TiO2, Nb2O5 and WO3 (TiO2+Nb2O5+WO3) is preferably 10.00% or more, more preferably 15.00% or more, and further preferably 20.00% or more, 25.00% or more, 28.00% or more, and 30.00% or more in that order. From the viewpoint of improving the glass stability, the total content (TiO2+Nb2O5+WO3) is preferably 60.00% or less, more preferably 55.00% or less, and further preferably 50.00% or less, 45.00% or less, 40.00% or less, 38.00% or less, and 35.00% or less in that order.
[0025] Y2O3 is a component that can contribute to increasing the refractive index of glass, maintaining low dispersion, and improving chemical durability. The Y2O3 content of the optical glass is preferably 0.10% or more, more preferably 0.30% or more, and further preferably 0.50% or more, 0.80% or more, and 1.00% or more in that order. From the viewpoint of suppressing the deterioration of glass stability and suppressing the increase of Tl, the Y2O3 content is preferably 10.00% or less, more preferably 8.00% or less, and further preferably 5.00% or less, and further preferably 3.00% or less in that order.
[0026] La2O3 is also a component that can contribute to increasing the refractive index of the glass, maintaining low dispersion, and improving chemical durability. The La2O3 content of the optical glass is preferably 10.00% or more, more preferably 15.00% or more, and further preferably 20.00% or more, 25.00% or more, 30.00% or more, and 35.00% or more in that order. From the viewpoint of suppressing the deterioration of glass stability and suppressing the increase of Tl, the La2O3 content is preferably 60.00% or less, more preferably 55.00% or less, and further preferably 50.00% or less, 45.00% or less, and 40.00% or less in that order.
[0027] Gd2O3 is also a component that can contribute to increasing the refractive index of the glass, maintaining low dispersion, and improving chemical durability. The Gd2O3 content of the optical glass is preferably 1.00% or more, more preferably 2.00% or more, and further preferably 3.00% or more, 4.00% or more, 5.00% or more, and 6.00% or more in that order. From the viewpoint of suppressing the deterioration of glass stability and suppressing the increase of Tl, the Gd2O3 content is preferably 30.00% or less, more preferably 20.00% or less, and further preferably 15.00% or less, 10.00% or less, and 8.00% or less in that order.
[0028] The Yb2O3 content can be 0.00%, 0.00% or more, or more than 0.00%. Yb2O3 is also a component that can contribute to increasing the refractive index of the glass, maintaining low dispersion, and improving chemical durability. The Yb2O3 content of the optical glass can be, for example, 5.00% or less, 4.00% or less, 3.00% or less, 2.00% or less, 1.00% or less, 0.50% or less, or 0.10% or less.
[0029] The total content of Y2O3, La2O3, Gd2O3 and Yb2O3 (Y2O3+La2O3+Gd2O3+Yb2O3) is preferably 10.00% or more, more preferably 15.00% or more, and more preferably 20.00% or more, 25.00% or more, 30.00% or more, 35.00% or more, 40.00% or more, 43.00% or more, and 45.00% or more in this order, from the viewpoint of suppressing the deterioration of glass stability and suppressing the increase of Tl, the total content (Y2O3+La2O3+Gd2O3+Yb2O3) is preferably 70.00% or less, more preferably 65.00% or less, and more preferably 60.00% or less, 55.00% or less, 53.00% or less, and 50.00% or less in this order.
[0030] The content of each of Li2O, Na2O, K2O, and Cs2O can be 0.00%, 0.00% or more, more than 0.00%, 0.05% or more, or 0.10% or more. Also, the content of each of Li2O, Na2O, K2O, and Cs2O can be, for example, 5.00% or less, 4.00% or less, 3.00% or less, 2.00% or less, or 1.00% or less. Li2O, Na2O, K2O and Cs2O all have the function of improving the thermal stability of the glass, but when their contents increase, the refractive index and chemical durability tend to decrease. Therefore, the contents of Li2O, Na2O, K2O and Cs2O are preferably within the above ranges.
[0031] The content of each of MgO, CaO, SrO, and BaO may be 0.00%, 0.00% or more, more than 0.00%, 0.05% or more, or 0.10% or more. Also, the content of each of MgO, CaO, SrO, and BaO may be, for example, 5.00% or less, 4.00% or less, 3.00% or less, 2.00% or less, or 1.00% or less. Although MgO, CaO, SrO and BaO all have the function of improving the thermal stability of the glass, when the contents of these elements are high, the refractive index tends to decrease, so that the contents of MgO, CaO, SrO and BaO are preferably within the above-mentioned ranges.
[0032] The ZnO content can be 0.00%, 0.00% or more, more than 0.00%, 0.10% or more, or 0.10% or more. The ZnO content can be, for example, 5.00% or less, 4.00% or less, 3.00% or less, or 2.00% or less. ZnO has the function of improving the thermal stability of the glass, but as the ZnO content increases, the specific gravity tends to increase, so the ZnO content is preferably within the above range.
[0033] The ZrO2 content can be 0.00%, 0.00% or more, more than 0.00%, 1.00% or more, 3.00% or more, or 5.00% or more. Also, the ZrO2 content can be, for example, 10.00% or less, or 8.00% or less. ZrO2 has the function of increasing the refractive index of the glass, but as the content of ZrO2 increases, the thermal stability of the glass tends to decrease, so the content of ZrO2 is preferably within the above range.
[0034] The Ta2O5 content can be 0.00%, 0.00% or more, more than 0.00%, 0.10% or more, or 0.10% or more. Also, the Ta2O5 content can be, for example, 5.00% or less, 4.00% or less, 3.00% or less, or 2.00% or less. Ta2O5 has the function of increasing the refractive index of the glass, but as the Ta2O5 content increases, the thermal stability of the glass tends to decrease, so the Ta2O5 content is preferably within the above range.
[0035] The optical glass may further contain one or more of P2O5, Al2O3, and the like in addition to the above components. The P2O5 content can be 0.00% or more, and is preferably 10.00% or less, and more preferably 8.00% or less, 6.00% or less, 4.00% or less, 2.00% or less, 1.00% or less, and 0.50% or less in that order. The Al2O3 content can be 0.00% or more, and is preferably 10.00% or less, and more preferably 8.00% or less, 6.00% or less, 4.00% or less, 2.00% or less, 1.00% or less, and 0.50% or less in that order.
[0036] Pb, As, Cd, Tl, Be, and Se are each toxic, and therefore it is preferable not to include these elements, i.e., not to introduce these elements into the glass as glass components. U, Th, and Ra are all radioactive elements, and therefore it is preferable not to contain these elements, i.e., not to introduce these elements into the glass as glass components. V, Cr, Mn, Fe, Co, Ni, Cu, Pr, Nd, Pm, Sm, Eu, Tb, Dy, Ho, Er, Tm, and Ce are undesirable elements to be contained in glass for optical elements because they increase the coloring of the glass and are sources of fluorescence. Therefore, it is preferable not to contain these elements, i.e., not to introduce these elements into the glass as glass components.
[0037] Sb and Sn are elements that function as fining agents and can be added as desired. The amount of Sb added is, calculated as Sb2O3 and assuming the total content of glass components other than Sb2O3 to be 100 mass%, preferably in the range of 0.000 to 0.100 mass%, more preferably in the range of 0.001 to 0.020 mass%, even more preferably in the range of 0.001 to 0.010 mass%, and even more preferably in the range of 0.001 to 0.005 mass%. The amount of Sn added is, converted to SnO2, preferably in the range of 0.000 to 0.100 mass%, more preferably in the range of 0.000 to 0.020 mass%, even more preferably in the range of 0.000 to 0.010 mass%, and even more preferably in the range of 0.000 to 0.005 mass%, when the total content of glass components other than SnO2 is taken as 100 mass%.
[0038] <Glass properties> (Refractive index nd) The refractive index nd of the optical glass is more than 2.00000, preferably 2.01000 or more, more preferably 2.02000 or more, and more preferably 2.03000 or more, 2.04000 or more, 2.05000 or more, 2.06000 or more, 2.07000 or more, and 2.08000 or more in this order. The refractive index nd of the optical glass can be, for example, 2.20000 or less, 2.15000 or less, 2.14000 or less, 2.13000 or less, 2.12000 or less, 2.11000 or less, or 2.10000 or less. In the present invention and this specification, "refractive index" means "refractive index nd".
[0039] (Abbe number νd) The Abbe number νd is a value that represents the property related to dispersion, and is expressed as νd=(nd-1) / (nF-nC) using the refractive indices nd, nF, and nC at the d-line, F-line, and C-line. From the viewpoint of usefulness as a material for optical elements and a material for light guide plates, the Abbe number νd of the optical glass is preferably 20.00 or more, more preferably 21.00 or more, and further preferably 22.00 or more and 23.00 or more in that order. From the same viewpoint, the Abbe number νd is preferably 30.00 or less, more preferably 28.00 or less, and further preferably 26.00 or less, 25.00 or less, and 24.00 or less in that order.
[0040] (glass transition temperature Tg) From the viewpoint of machinability, the glass transition temperature Tg of the optical glass is preferably 560°C or higher. Glass with a high glass transition temperature is preferred because it tends to be less likely to break during mechanical processing of the glass, such as cutting, milling, grinding, and polishing. From the viewpoint of machinability, the glass transition temperature Tg is more preferably 570°C or higher, and further preferably 580°C or higher, 590°C or higher, and 600°C or higher in that order. On the other hand, from the viewpoint of reducing the load on the annealing furnace and the molding die, the glass transition temperature Tg is preferably 800°C or lower, and more preferably 790°C or lower, 780°C or lower, 770°C or lower, 760°C or lower, and 750°C or lower in that order.
[0041] The glass transition temperature Tg is determined as follows. In differential scanning calorimetry, when a glass sample is heated, an endothermic behavior associated with a change in specific heat, i.e., an endothermic peak appears, and when the temperature is further increased, an exothermic peak appears. In differential scanning calorimetry analysis, a differential scanning calorimetry curve (DSC (Differential Scanning Calorimetry) curve) is obtained, in which the horizontal axis represents temperature and the vertical axis represents the amount corresponding to the heat generation and endothermic heat of the sample. The intersection of the tangent at the point where the slope of the curve becomes maximum when an endothermic peak appears from the baseline and the baseline is taken as the glass transition temperature Tg. The glass transition temperature Tg can be measured by using glass that has been thoroughly crushed in a mortar or the like as a sample and a differential scanning calorimeter at a heating rate of 10°C / min.
[0042] (Temperature Tl) The present inventors have newly found that glass with a low melt-switching temperature Tl in the differential scanning calorimetry is less likely to cause surface devitrification. The Tl of the optical glass is preferably 1247°C or less, more preferably 1246°C or less, and further preferably 1245°C or less, 1244°C or less, 1243°C or less, 1242°C or less, 1241°C or less, and 1240°C or less in this order. The Tl of the optical glass can be, for example, 1200°C or more, 1210°C or more, or 1220°C or more. However, from the viewpoint of suppressing surface devitrification, the lower the Tl, the more preferable, so the Tl of the optical glass may be below the above range.
[0043] The temperature Tl is determined from the DSC curve as the temperature at the intersection between the tangent line at the point where the slope from the top of the endothermic peak due to melting to the baseline is maximum and the baseline. The temperature at the intersection is the temperature h in Figure 5 of "NEW GLASS, Vol.28, No.110 2013".
[0044] (specific gravity) The refractive power of the optical elements that make up an optical system is determined by the refractive index of the glass that makes up the optical element and the curvature of the optical functional surface of the optical element (the surface through which the light rays to be controlled enter and exit). If you try to increase the curvature of the optical functional surface, the thickness of the optical element also increases. As a result, the optical element becomes heavier. In contrast, if glass with a high refractive index is used, it is possible to obtain a large refractive power without increasing the curvature of the optical functional surface. From the above, if the refractive index can be increased while suppressing an increase in the specific gravity of the glass, it will be possible to reduce the weight of an optical element having a certain refractive power. Also, with regard to the glass constituting the light guide plate, a low specific gravity is preferable from the viewpoint of reducing the weight of the light guide plate and the image display device. From the above viewpoints, the specific gravity of the optical glass is preferably 5.30 or less, more preferably 5.20 or less, and even more preferably 5.10 or less. Since a lower specific gravity is more preferable from the viewpoint of reducing the weight of the optical element, the lower limit of the specific gravity of the optical glass is not particularly limited. In one embodiment, the specific gravity can be 4.00 or more, 4.40 or more, or 4.800 or more.
[0045] The optical glass described above is useful as a glass material for optical elements and a glass material for light guide plates.
[0046] <Glass manufacturing method> The optical glass can be obtained by weighing, preparing and thoroughly mixing raw materials such as oxides, carbonates, sulfates, nitrates and hydroxides so as to obtain the desired glass composition, heating and melting the mixture in a melting vessel, degassing and stirring the mixture to produce a homogeneous, bubble-free molten glass, and then molding the glass. Specifically, the glass can be produced by using a known melting method.
[0047] [Glass material for press molding, optical element blanks, and their manufacturing methods] Another aspect of the present invention is a glass material for press molding comprising the optical glass; an optical element blank made of the optical glass; Regarding.
[0048] According to another aspect of the present invention, a method for producing a glass material for press molding, comprising a step of molding the optical glass into a glass material for press molding; a method for producing an optical element blank, comprising a step of press-molding the glass material for optical glass press molding using a press mold to produce an optical element blank; a method for producing an optical element blank, comprising the step of forming the optical glass into an optical element blank; will also be provided.
[0049] An optical element blank is an optical element base material that approximates the shape of a target optical element and has polishing margins (surface layers to be removed by polishing) and, if necessary, grinding margins (surface layers to be removed by grinding) added to the shape of the optical element. The optical element is finished by grinding and polishing the surface of the optical element blank. In one embodiment, the optical element blank can be produced by a method (called a direct press method) in which a molten glass obtained by melting an appropriate amount of the above glass is press-molded. In another embodiment, the optical element blank can also be produced by solidifying a molten glass obtained by melting an appropriate amount of the above glass.
[0050] In another embodiment, a glass material for press molding is prepared, and the prepared glass material for press molding is press molded to produce an optical element blank.
[0051] The press molding of the glass material for press molding can be carried out by a known method in which the glass material for press molding in a heated and softened state is pressed in a press mold. Both heating and press molding can be carried out in the atmosphere. By annealing after press molding to reduce distortion inside the glass, a homogeneous optical element blank can be obtained.
[0052] Glass materials for press molding include not only those called glass gobs for press molding, which are used for press molding as they are to produce optical element blanks, but also those that are mechanically processed such as by cutting, grinding, polishing, etc., and are used for press molding via glass gobs for press molding. Cutting methods include a method in which a groove is formed in the portion of the surface of the glass plate to be cut by a method called scribing, and local pressure is applied to the grooved portion from the back side of the surface on which the groove is formed, thereby breaking the glass plate at the grooved portion, and a method in which the glass plate is cut by a cutting blade. Grinding and polishing methods include barrel polishing, etc.
[0053] The glass material for press molding can be produced, for example, by casting molten glass into a mold to form a glass plate, and cutting this glass plate into a plurality of glass pieces. Alternatively, a suitable amount of molten glass can be molded to produce a glass gob for press molding. An optical element blank can also be produced by reheating, softening, and press-molding the glass gob for press molding. The method of producing an optical element blank by reheating, softening, and press-molding glass is called a reheat press method, as opposed to a direct press method.
[0054] [Optical element and its manufacturing method] Another aspect of the present invention is An optical element made of the above optical glass Regarding. The optical element is produced using the optical glass. In the optical element, the glass surface may be coated with one or more layers of coating, such as a multilayer film including an anti-reflection film.
[0055] According to another aspect of the present invention, A method for producing an optical element, comprising the step of producing an optical element by grinding and / or polishing the optical element blank described above; will also be provided.
[0056] In the above-mentioned method for producing an optical element, known methods may be used for grinding and polishing, and an optical element with high internal quality and surface quality can be obtained by thoroughly cleaning and drying the surface of the optical element after processing. In this manner, an optical element made of the above-mentioned glass can be obtained. Examples of optical elements include various lenses such as spherical lenses, aspherical lenses, and microlenses, and prisms.
[0057] In addition, the optical element made of the optical glass is also suitable as a lens constituting a cemented optical element. Examples of cemented optical elements include a cemented lens formed by cementing lenses together, and a lens and a prism. For example, a cemented optical element can be produced by precisely processing (for example, spherical polishing) the cemented surfaces of two optical elements to be cemented so that the shapes are inverted, applying an ultraviolet-curing adhesive used for bonding the cemented lens, bonding them together, and then irradiating ultraviolet light through the lens to cure the adhesive. In this way, the above glass is preferable for producing a cemented optical element. A plurality of optical elements to be cemented are produced using a plurality of types of glass having different Abbe numbers νd, and cemented together to produce an element suitable for correcting chromatic aberration.
[0058] [Light guide plate, image display device] Another aspect of the present invention is a light guide plate made of the optical glass; an image display device including an image display element and a light guide plate for guiding light emitted from the image display element, the light guide plate being made of any one of the optical glasses described above; A specific embodiment of the image display device will be described later. EXAMPLES
[0059] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the embodiments shown in the examples.
[0060] [Example 1] In order to obtain the glass composition shown in the table below, the corresponding nitrates, sulfates, carbonates, hydroxides, oxides, boric acid, etc. were used as raw materials for introducing each component, and the raw materials were weighed and thoroughly mixed to obtain blended raw materials. The mixed raw materials were placed in a platinum crucible and heated to melt. After melting, the molten glass was poured into a mold and allowed to cool to near the glass transition temperature, then immediately placed in an annealing furnace and annealed for about 1 hour within the glass transition temperature range, and then allowed to cool to room temperature in the furnace to obtain the optical glasses No. 1 to 40 shown in the table below. In the table below, the unit of content is mass %. The Sb2O3 content is the content when the total content of glass components other than Sb2O3 is taken as 100 mass %.
[0061] [Comparative Examples 1 and 2] Glasses having the glass compositions shown in the following table were produced by the method described for Example 1 to obtain the optical glasses of Comparative Examples 1 and 2. Comparative Example 1 corresponds to Example 1 in Japanese Patent No. 5931173 (Patent Document 1), and Comparative Example 2 corresponds to Example 11 in JP 2019-116408 A (Patent Document 2).
[0062] The physical properties of the optical glasses of the Examples and Comparative Examples are shown in the following table. The physical properties of the optical glasses were measured by the methods described below.
[0063] [Evaluation of physical properties of optical glass] (1) Refractive index nd Abbe number νd The glass obtained by cooling at a cooling rate of -30°C / hour was measured for refractive index nd and Abbe number vd by the refractive index measurement method specified by the Japan Optical Glass Industry Association.
[0064] (2) Glass transition temperature Tg, temperature Tl The glass was thoroughly crushed in a mortar and used as a sample, and a differential scanning calorimeter (DSC3300SA) manufactured by NETZSCH was used to perform DSC measurement at a heating rate of 10°C / min to obtain a DSC curve. From the obtained DSC curve, the glass transition temperature Tg and the temperature at which the glass changes to melt Tl were obtained as described above.
[0065] (3) Specific gravity Specific gravity was measured by Archimedes' method.
[0066] The glass blocks of the optical glasses Nos. 1 to 40 of Example 1 and the optical glasses of Comparative Examples 1 and 2 were visually observed. As a result, no surface devitrification was observed in the glass blocks of the optical glasses of Example 1. In contrast, it was confirmed that surface devitrification occurred in the glass blocks of the optical glasses of Comparative Example 1 and Comparative Example 2.
[0067] 1 is a photograph of a glass block of the optical glass of Example 13 (left) and a glass block of the optical glass of Comparative Example 1 (right). It can be seen that surface devitrification has occurred in the glass block of the optical glass of Comparative Example 1.
[0068] [Table 1]
[0069] [Table 2]
[0070] [Table 3]
[0071] [Table 4]
[0072] [Table 5]
[0073] Example 2 Glass gobs for press molding (glass gobs) were prepared using the various glasses obtained in Example 1. The glass gobs were heated and softened in the atmosphere, and press molded in a press mold to prepare lens blanks (optical element blanks). The prepared lens blanks were removed from the press mold, annealed, and machined, including polishing, to prepare spherical lenses made of the optical glasses of Example 1.
[0074] Example 3 A desired amount of the molten glass produced in Example 1 was press molded in a press mold to produce a lens blank (optical element blank). The produced lens blank was removed from the press mold, annealed, and subjected to mechanical processing including polishing to produce a spherical lens made of each optical glass of Example 1.
[0075] Example 4 The molten glass produced in Example 1 was solidified to produce a glass lump (optical element blank), which was then annealed and machined, including polishing, to produce a spherical lens made of each of the optical glasses in Example 1.
[0076] Example 5 The spherical lenses produced in Examples 2 to 4 were bonded to spherical lenses made of other types of glass to produce cemented lenses.
[0077] Example 6 2 is a schematic diagram of a head mounted display, which is an example of an image device including an image display element and a light guide plate. A head mounted display 1 having the configuration shown in FIG. 2 was produced by the following method. Each optical glass of Example 1 was processed into a rectangular thin plate having a length of 50 mm, a width of 20 mm, and a thickness of 1.0 mm to obtain a light guide plate 10. This light guide plate was attached to a head mounted display 1 (hereinafter, abbreviated as "HMD1") shown in FIG. 2. FIG. 2(a) is a front perspective view of the HMD1, and FIG. 2(b) is a rear perspective view of the HMD1. As shown in FIG. 2(a) and FIG. 2(b), a spectacle lens 3 is attached to the front part of a spectacle-type frame 2 worn on the user's head. A backlight 4 for illuminating an image is attached to the mounting part 2a of the spectacle-type frame 2. A signal processing device 5 for projecting an image and a speaker 6 for reproducing sound are provided on the temple part of the spectacle-type frame 2. Flexible printed circuits (FPCs) 7 constituting wiring drawn from the circuit of the signal processing device 5 are wired along the spectacle-type frame 2. A display element unit (e.g., liquid crystal display element) 20 is wired to the center position of the user's eyes by the FPC 7, and is held so that the approximate center of the display element unit 20 is located on the optical axis of the backlight 4. The imager unit 20 is fixed relative to the light guide plate 10 so as to be located approximately at the center of the light guide plate 10. Holographic optical elements (HOEs) 32R and 32L (first optical elements) are fixed in close contact with the first surface 10a of the light guide plate 10 by adhesive or the like at locations in front of the user's eyes. HOEs 52R and 52L are laminated on the second surface 10b of the light guide plate 10 at positions facing the imager unit 20 across the light guide plate 10. 3 is a side view showing a schematic configuration of the HMD 1 shown in FIG. 2. In FIG. 3, in order to clarify the drawing, only the main parts are shown, and the eyeglass-type frame 2 and the like are omitted. As shown in FIG. 3, the HMD 1 has a structure symmetrical on both sides of a center line X connecting the center of the image display element 24 and the light guide plate 10. Furthermore, the light of each wavelength incident on the light guide plate 10 from the image display element 24 is divided into two and guided to the right eye and the left eye of the user, as described later. The optical paths of the light of each wavelength guided to each eye are also approximately symmetrical on both sides of the center line X. As shown in FIG. 3, the backlight 4 has a laser light source 21, a diffusion optical system 22, and a microlens array 23. The display element unit 20 is an image generating unit having an image display element 24, and is driven, for example, by a field sequential method. The laser light source 21 has laser light sources corresponding to the wavelengths of B (wavelength 436 nm), G (wavelength 546 nm), and R (wavelength 633 nm), and sequentially irradiates light of each wavelength at high speed. The light of each wavelength is incident on the diffusion optical system 22 and the microlens array 23, and is converted into a uniform, highly directional parallel light beam without unevenness in the amount of light, and is incident perpendicularly on the display panel surface of the image display element 24. The image display element 24 is, for example, a transmissive liquid crystal (LCDT-LCOS) panel driven by a field sequential method. The image display element 24 modulates the light of each wavelength according to an image signal generated by an image engine (not shown) of the signal processing device 5. The light of each wavelength modulated by the pixels in the effective area of the image display element 24 is incident on the light guide plate 10 with a predetermined light beam cross section (approximately the same shape as the effective area). The image display element 24 can also be replaced with other types of display elements, such as a DMD (Digital Mirror Device), a reflective liquid crystal (LCOS) panel, a MEMS (Micro Electro Mechanical Systems), an organic EL (Electro-Luminescence), or an inorganic EL. The image generating unit of the image display element 20 is not limited to a field sequential type image display element, but may be a simultaneous type image display element (a display element having a predetermined arrangement of RGB color filters in front of the emission surface). In this case, for example, a white light source is used as the light source. As shown in Fig. 3, the light of each wavelength modulated by the image display element 24 is sequentially incident on the inside of the light guide plate 10 from the first surface 10a. HOEs 52R and 52L (second optical elements) are laminated on the second surface 10b of the light guide plate 10. The HOEs 52R and 52L are, for example, reflective volume phase HOEs having a rectangular shape, and are configured by laminating three photopolymer sheets on which interference fringes corresponding to the light of each wavelength of R, G, and B are recorded. In other words, the HOEs 52R and 52L are configured to have a wavelength selection function that diffracts the light of each wavelength of R, G, and B and transmits light of other wavelengths. The HOEs 32R and 32L are also reflective volume phase type HOEs and have the same layer structure as the HOEs 52R and 52L. The HOEs 32R and 32L and the HOEs 52R and 52L may have, for example, approximately the same pitch of the interference fringe patterns. The HOEs 52R and 52L are stacked with their centers aligned and with their interference fringe patterns inverted by 180 degrees. They are then fixed in close contact with the second surface 10b of the light guide plate 10 by adhesive or the like so that their centers in the stacked state are aligned with the center line X. Light of each wavelength modulated by the image display element 24 is sequentially incident on the HOEs 52R and 52L via the light guide plate 10. The HOEs 52R and 52L each diffract the light of each wavelength incident sequentially at a predetermined angle to guide it to the right eye and the left eye. The light of each wavelength diffracted by the HOEs 52R and 52L is repeatedly totally reflected at the interface between the light guide plate 10 and the air, propagates inside the light guide plate 10, and is incident on the HOEs 32R and 32L. Here, the HOEs 52R and 52L give the same diffraction angle to the light of each wavelength. Therefore, all the light of wavelengths that are incident at approximately the same position on the light guide plate 10 (or, in other words, emitted from approximately the same coordinates within the effective area of the image display element 24) propagate through approximately the same optical path inside the light guide plate 10 and are incident on approximately the same position on the HOEs 32R and 32L. From another perspective, the HOEs 52R and 52L diffract the light of each wavelength of RGB so that the pixel positional relationship within the effective area of the image displayed in the effective area of the image display element 24 is faithfully reproduced on the HOEs 32R and 32L. Thus, in this embodiment, HOEs 52R and 52L each diffract light of all wavelengths emitted from approximately the same coordinates within the effective area of image display element 24 so that it is incident on approximately the same position on HOEs 32R and 32L. Alternatively, HOEs 52R and 52L may be configured to diffract light of all wavelengths that originally constitute the same pixel but are relatively shifted within the effective area of image display element 24 so that it is incident on approximately the same position on HOEs 32R and 32L. The light of each wavelength incident on the HOEs 32R and 32L is diffracted by the HOEs 32R and 32L and sequentially emitted from the second surface 10b of the light guide plate 10 in a substantially perpendicular direction to the outside. The light of each wavelength emitted as substantially parallel light in this manner is imaged on the right and left retina of the user as a virtual image I of the image generated by the image display element 24. In addition, a condenser effect may be given to the HOEs 32R and 32L so that the user can observe the virtual image I of the enlarged image. That is, the light incident on the peripheral area of the HOEs 32R and 32L may be emitted at an angle closer to the center of the pupil and imaged on the user's retina. Alternatively, in order to allow the user to observe the virtual image I of the enlarged image, the HOEs 52R and 52L may diffract the light of each wavelength of RGB so that the pixel positional relationship on the HOEs 32R and 32L forms an enlarged similar shape to the pixel positional relationship within the effective area of the image displayed in the effective area of the image display element 24. Since the air-equivalent optical path length of light traveling inside the light guide plate 10 becomes shorter as the refractive index increases, by using each of the above optical glasses having a high refractive index, it is possible to increase the apparent viewing angle relative to the width of the image display element 24. Furthermore, since the specific gravity of a glass having a high refractive index is kept low, it is possible to provide a light guide plate that is lightweight yet provides the above effects. The light guide plate 10 thus obtained was incorporated into the HMD 1, and the image was evaluated at the eyepoint position. As a result, a high-brightness, high-contrast image could be observed over a wide viewing angle. The light guide plates made of the above optical glasses can be used in see-through transmissive head-mounted displays and non-transmissive head-mounted displays. These head mounted displays have a light guide plate made of high refractive index glass, which provides a wide viewing angle and a sense of immersion, making them ideal as image display devices for use in combination with information terminals, for providing AR (Augmented Reality), and for providing movies, games, VR (Virtual Reality), etc. In this embodiment, a head mounted display has been taken as an example for explanation, but the light guide plate may be attached to other image display devices.
[0078] The embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The scope of the present invention is defined by the claims, not the above description, and is intended to include all modifications within the meaning and scope of the claims. For example, by subjecting the glass compositions exemplified above to compositional adjustments as described in the specification, an optical glass according to one aspect of the present invention can be obtained. Furthermore, it is of course possible to arbitrarily combine two or more of the items described in the specification as examples or preferred ranges.
Claims
1. SiO as an essential component 2 , B 2 O 3 , TiO 2 , Nb 2 O 5 , Y 2 O 3 , La 2 O 3 and Gd 2 O 3 Including, On a mass basis, SiO 2 B relative to content 2 O 3 Mass ratio of content (B 2 O 3 / SiO 2 ) is less than 1.000; Y 2 O 3 , La 2 O 3 , Gd 2 O 3 and Yb 2 O 3 Y relative to the total content 2 O 3 Mass ratio of content (Y 2 O 3 / (Y 2 O 3 +La 2 O 3 +Gd 2 O 3 +Yb 2 O 3 ) is greater than 0.020, and An optical glass having a refractive index nd exceeding 2.00000.
2. Mass ratio (Y 2 O 3 / (Y 2 O 3 +La 2 O 3 +Gd 2 O 3 +Yb 2 O 3 2. The optical glass according to claim 1 , wherein n is greater than 0.020 and not greater than 0.
100.
3. SiO 2 and B 2 O 3 TiO relative to the total content 2 Mass ratio of content (TiO 2 / (SiO 2 +B 2 O 3 2. The optical glass according to claim 1 , wherein n is 1.950 or greater.
4. SiO 2 and B 2 O 3 The total content of 2 +B 2 O 3 2. The optical glass according to claim 1, wherein the content of Cd is 30.00 mass % or less.
5. 2. The optical glass according to claim 1, having a refractive index nd of 2.08000 or more.
6. 2. The optical glass according to claim 1, which has a melt-switching temperature Tl in differential scanning calorimetry of 1247° C. or lower.
7. 2. The optical glass according to claim 1, which has a melt-switching temperature Tl in DSC measurement of 1245° C. or lower.
8. Mass ratio (Y 2 O 3 / (Y 2 O 3 +La 2 O 3 +Gd 2 O 3 +Yb 2 O 3 ) is more than 0.020 and not more than 0.100, SiO 2 and B 2 O 3 TiO relative to the total content 2 Mass ratio of content (TiO 2 / (SiO 2 +B 2 O 3 ) is 1.950 or more, SiO 2 and B 2 O 3 The total content of 2 +B 2 O 3 ) is 12.00 mass% or less, The refractive index nd is 2.08000 or more, 2. The optical glass according to claim 1, which has a melt-switching temperature Tl in differential scanning calorimetry of 1247° C. or lower.
9. 9. The optical glass according to claim 8, which has a melt-switching temperature Tl in differential scanning calorimetry of 1245° C. or lower.
10. An optical element comprising the optical glass according to any one of claims 1 to 9.
11. A light guide plate comprising the optical glass according to any one of claims 1 to 9.
12. An image display element; a light guide plate that guides light emitted from the image display element; Including, The image display device, wherein the light guide plate is the light guide plate according to claim 11.
Citation Information
Patent Citations
Apparatus for continuously printing card
JP1984031173A
Optical glass, preform and optical element
JP2019116408A