Polymer thin film and battery

A polymer thin film with specific copolymers addresses dendrite precipitation issues by swelling to fill gaps between electrodes, improving battery efficiency and safety.

JP2024146092APending Publication Date: 2024-10-15LINTEC CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023058807
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The battery separator described in Patent Document 1 fails to prevent dendrite precipitation on the negative electrode active material, leading to irreversible capacity loss and potential short circuits due to gaps between the electrode surface and the separator.

Method used

A polymer thin film containing specific copolymers with structural units represented by general formulas (1) and (2), and optionally (3) and (4), which exhibit high swelling properties in electrolytes, ensuring compatibility and crosslinking to fill gaps and suppress dendrite formation.

Benefits of technology

The polymer thin film achieves high swelling properties in electrolytes, effectively preventing dendrite growth and enhancing the efficiency and safety of batteries by maintaining electrical contact and reducing elution amounts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146092000021
    Figure 2024146092000021
  • Figure 2024146092000022
    Figure 2024146092000022
  • Figure 2024146092000023
    Figure 2024146092000023
Patent Text Reader

Abstract

To provide a polymer thin film having high swelling property in an electrolyte or the like.SOLUTION: There is provided a polymer thin film which contains a copolymer containing a constitutional unit represented by a following general formula (1) and 0.3 mol% or more and 10 mol% or less of a constitutional unit represented by a following general formula (2). (In the general formula (1) and the general formula (2), R1 is a hydrogen atom or an alkyl group having 1 or more and 3 or less carbon atoms, each of L1 and L2 independently is a single bond or an alkylene group having 1 or more and 3 or less carbon atoms, L3 is a single bond, an alkylene group having 1 or more and 5 or less carbon atoms or an oxyalkylene group having 1 or more and 5 or less carbon atoms, X1 is a reactive group.)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thin polymer film and a battery. [Background technology]

[0002] Polymer thin films are used in a variety of applications, including as materials in the battery field, for example as battery separators. For example, Patent Document 1 discloses a battery separator including a microporous polyolefin membrane and a porous layer laminated on at least one surface of the microporous polyolefin membrane. The porous layer contains a vinylidene fluoride-based polymer selected from the group consisting of vinylidene fluoride homopolymers and vinylidene fluoride-hexafluoropropylene copolymers, polyacrylic acid, and inorganic particles. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2022-053727 Summary of the Invention [Problem to be solved by the invention]

[0004] The battery separator described in Patent Document 1 has a problem in that it cannot stop dendrite deposition on the surface of the negative electrode active material. The dendrites formed on the active material surface peel off from the active material surface during charge / discharge cycles, resulting in irreversible capacity. Furthermore, if the dendrites grow and reach the positive electrode, they will cause a short circuit, so it is necessary to suppress the formation of dendrites. On the other hand, the present inventors believe that the dendrite deposition on the surface of the negative electrode active material is caused by gaps between the negative electrode surface and the separator due to fine irregularities. For example, if the separator has high swelling properties in an electrolyte solution, the separator can be made to swell and fill the gaps between the negative electrode surface and the separator.

[0005] An object of the present invention is to provide a polymer thin film having high swelling properties in an electrolyte solution, etc., and a battery. [Means for solving the problem]

[0006] [1] A copolymer containing a constitutional unit represented by the following general formula (1) and 0.3 mol % to 10 mol % of a constitutional unit represented by the following general formula (2): Polymer thin film.

[0007] [ka]

[0008] (In the general formula (1) and the general formula (2), R 1 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and L 1 and L 2 each independently represents a single bond or an alkylene group having 1 to 3 carbon atoms; L 3 is a single bond, an alkylene group having 1 to 5 carbon atoms, or an oxyalkylene group having 1 to 5 carbon atoms; X 1 is any one of the reactive groups represented by the following structural formula (2-1), (2-2), and (2-3).

[0009] [ka]

[0010] [2] The polymer thin film according to [1], -L in the general formula (2) 3 -X 1 is any one of reactive groups represented by the following structural formula (2-4), the following structural formula (2-5), and the following structural formula (2-6): Polymer thin film.

[0011] [ka]

[0012] [3] The polymer thin film according to [1] or [2], The copolymer further contains at least one structural unit selected from the group consisting of a structural unit represented by the following general formula (3) and a structural unit represented by the following general formula (4), in an amount of 0.1 mol % to 30 mol %: Polymer thin film.

[0013] [ka]

[0014] (In the general formula (3) and the general formula (4), R 2 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and L 4 and L 5 each independently represents a single bond or an alkylene group having 1 to 3 carbon atoms; L 6 is a single bond, an alkylene group having 1 to 5 carbon atoms, or an oxyalkylene group having 1 to 5 carbon atoms; X 2 is any one of the reactive groups represented by the following structural formula (4-1), (4-2), and (4-3).

[0015] [ka]

[0016] [4] The polymer thin film according to any one of [1] to [3], the amount of the copolymer eluted in ethyl acetate is 10% or less; The degree of swelling of the copolymer in a mixed solvent of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1 is 100% or more. Polymer thin film.

[0017] [5] A polymer thin film comprising the polymer thin film according to any one of [1] to [4]. battery. Effect of the Invention

[0018] According to one aspect of the present invention, it is possible to provide a polymer thin film having high swelling properties in an electrolyte solution, etc., and a battery. [Brief description of the drawings]

[0019] [Figure 1] 1 is a cross-sectional view illustrating an example of a main part of a battery according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram for explaining the action and effect when the polymer thin film according to the present embodiment is used as a battery separator. [Diagram 3] 1 is a chart showing the results of 1H-NMR measurement of the copolymer produced in Example 1. [Figure 4] 1 is a chart showing the results of 1H-NMR measurement of the copolymer produced in Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The present invention will be described below by taking an embodiment as an example, but the present invention is not limited to the content of the embodiment.

[0021] [Polymer thin film] A preferred example of the polymer thin film according to this embodiment will be described.

[0022] The polymer thin film according to this embodiment contains a copolymer containing a constitutional unit represented by general formula (1) and 0.3 mol % or more and 10.0 mol % or less of a constitutional unit represented by general formula (2).

[0023] According to the polymer thin film of this embodiment, by having the above-mentioned configuration, a polymer thin film having high swelling properties in an electrolyte solution or the like can be obtained. The reason is not clear, but it is thought to be as follows. The copolymer used in the polymer thin film of this embodiment has a carbonate skeleton as the main polymer skeleton, which improves compatibility with the electrolyte solution. Therefore, when assembling a battery, the polymer thin film as a separator can be swollen after the electrolyte solution is injected. And, by containing 0.3 mol % or more and 10.0 mol % or less of the constitutional unit represented by general formula (2) having a crosslinkable functional group (reactive group), the crosslinking reaction proceeds moderately, so that it is possible to achieve both a high degree of swelling and a low amount of elution.

[0024] The polymer thin film according to this embodiment may contain other components as long as it contains the specific copolymer having the above-mentioned structure, as long as the object of the present invention is not impaired.

[0025] The form of the polymer thin film according to the present embodiment is not particularly limited, but is preferably a free-standing film. The free-standing polymer thin film according to the present embodiment refers to a film that can be supported by itself.

[0026] (copolymer) The copolymer contained in the polymer thin film according to this embodiment includes a copolymer containing a constitutional unit represented by the following general formula (1) and 0.3 mol % or more and 10.0 mol % or less of a constitutional unit represented by the following general formula (2).

[0027] [ka]

[0028] In the general formula (1) and the general formula (2), R 1 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, preferably a hydrogen atom or a methyl group, and particularly preferably a methyl group. L 1 and L 2are each independently a single bond or an alkylene group having 1 to 3 carbon atoms, preferably a methylene group or an ethylene group, and particularly preferably a methylene group. L 3 represents a single bond, an alkylene group having 1 to 5 carbon atoms, or an oxyalkylene group having 1 to 5 carbon atoms, preferably a single bond or an oxyalkylene group having 1 to 5 carbon atoms, and particularly preferably a single bond or an oxyalkylene group having 2 to 4 carbon atoms. X 1 is any one of the reactive groups represented by the following structural formula (2-1), (2-2), and (2-3): In addition, the wavy line in the structural formula indicates a bond position.

[0029] [ka]

[0030] From the viewpoint of ease of synthesis, -L in general formula (2) 3 -X 1 is preferably any one of the reactive groups represented by the following structural formula (2-4), (2-5), and (2-6): In addition, the wavy line in the structural formula indicates a bonding position.

[0031] [ka]

[0032] Such a copolymer may be a random copolymer or a block copolymer, but from the viewpoint of ease of synthesis, the copolymer is preferably a random copolymer.

[0033] The copolymer contained in the polymer thin film according to this embodiment, for example, when it is a copolymer consisting of a constitutional unit represented by general formula (1) and a constitutional unit represented by general formula (2), has the following constitutional ratio. The ratio of the structural unit represented by the general formula (2) must be 0.3 mol% or more and 10.0 mol% or less with respect to all structural units. If this ratio is less than 0.3 mol%, the amount of elution will be high. On the other hand, if this ratio exceeds 10.0 mol%, the crosslink density of the copolymer will be high, resulting in a problem of reduced swelling. From the same viewpoint, the ratio of the constitutional unit represented by the general formula (2) is preferably 1.0 mol% or more, and more preferably 1.5 mol% or more. On the other hand, the ratio of the constitutional unit represented by the general formula (2) is preferably 8.0 mol% or less, more preferably 7.0 mol% or less, even more preferably 6.0 mol% or less, and particularly preferably 5.0 mol% or less.

[0034] The ratio of the structural unit represented by general formula (1) must be 90.0 mol% or more and 99.7 mol% or less with respect to all structural units. The ratio of the structural unit represented by general formula (1) is preferably 92.0 mol% or more, more preferably 93.0 mol% or more, even more preferably 94.0 mol% or more, and particularly preferably 95.0 mol% or more. On the other hand, the ratio of the structural unit represented by general formula (1) is preferably 99.0 mol% or less, more preferably 98.5 mol% or less.

[0035] The copolymer contained in the polymer thin film according to this embodiment preferably further contains at least one constitutional unit selected from the group consisting of constitutional units represented by the following general formula (3) and constitutional units represented by the following general formula (4), in an amount of 0.1 mol % or more and 30.0 mol % or less. By forming a copolymer containing an ether skeleton such as the structural unit represented by general formula (3) or (4), the glass transition temperature of the copolymer is lowered and the thin film becomes flexible, which is expected to result in high ionic conductivity.

[0036] [ka]

[0037] In the general formula (3) and the general formula (4), R 2 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, preferably a hydrogen atom or a methyl group, and particularly preferably a methyl group. L 4 and L 5 are each independently a single bond or an alkylene group having 1 to 3 carbon atoms, preferably a methylene group or an ethylene group, and particularly preferably a methylene group. L 6 represents a single bond, an alkylene group having 1 to 5 carbon atoms, or an oxyalkylene group having 1 to 5 carbon atoms, preferably a single bond or an oxyalkylene group having 1 to 5 carbon atoms, and particularly preferably a single bond or an oxyalkylene group having 2 to 4 carbon atoms. X 2 is any one of the reactive groups represented by the following structural formula (4-1), (4-2), and (4-3): In addition, the wavy line in the structural formula indicates a bond position.

[0038] [ka]

[0039] From the viewpoint of ease of synthesis, -L in general formula (4) 6 -X 2 is preferably any one of the reactive groups represented by the following structural formula (4-4), (4-5), and (4-6): In addition, the wavy line in the structural formula indicates a bonding position.

[0040] [ka]

[0041] The copolymer contained in the polymer thin film according to this embodiment, for example, a copolymer consisting of a constitutional unit represented by general formula (1), a constitutional unit represented by general formula (2), a constitutional unit represented by general formula (3), and a constitutional unit represented by general formula (4), has the following constitutional ratio. The ratio of the constitutional units represented by the general formula (2) is as described above. The total ratio of the structural unit represented by general formula (3) and the structural unit represented by general formula (4) is preferably 0.1 mol% or more and 30.0 mol% or less with respect to all structural units.If the total ratio of these is less than 0.1 mol%, the effect of the ether skeleton tends not to be fully exerted.On the other hand, if the total ratio of these is more than 30.0 mol%, the compatibility with the electrolyte tends to be poor, leading to a decrease in the degree of swelling. From the same viewpoint, the total ratio of these is preferably 0.2 mol% or more, and more preferably 0.6 mol% or more, while the total ratio of these is preferably 25.0 mol% or less, more preferably 20.0 mol% or less, and particularly preferably 10.0 mol% or less.

[0042] The ratio of the structural unit represented by the general formula (1) is preferably 60.0 mol% or more and 99.6 mol% or less with respect to all structural units. The ratio of the structural unit represented by the general formula (1) is preferably 65.0 mol% or more, and more preferably 70.0 mol% or more. On the other hand, the ratio of the structural unit represented by the general formula (1) is preferably 98.0 mol% or less, and more preferably 94.0 mol% or less.

[0043] The molecular weight of the copolymer according to this embodiment, measured by the method shown in the measurement example, is preferably 5,000 or more and 5,000,000 or less, and more preferably 10,000 or more and 1,000,000 or less, when expressed as a weight average molecular weight (Mw). Furthermore, the molecular weight of the copolymer according to this embodiment, measured by the method shown in the measurement example, is preferably 3,000 or more and 3,000,000 or less, and more preferably 5,000 or more and 500,000 or less, when expressed as a number average molecular weight (Mn). The ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) is preferably from 1 to 10, and more preferably from 1.1 to 5. When the molecular weight and molecular weight distribution of the copolymer are within the above ranges, the copolymer can have sufficient handleability when molded into a film.

[0044] (Method of Producing Copolymer) The method for producing the copolymer contained in the polymer thin film according to this embodiment is not particularly limited, and the copolymer can be obtained by a known method. For example, the copolymer can be produced by the following method. As described in the Examples below, it can be produced by copolymerizing an epoxide monomer such as propylene oxide with carbon dioxide in the presence of a polymerization catalyst. Specifically, propylene oxide undergoes ring-opening to become a constitutional unit represented by general formula (3), and a part of propylene oxide undergoes ring-opening polymerization with carbon dioxide to become a constitutional unit represented by general formula (1).

[0045] The polymerization catalyst used in producing the copolymer is not particularly limited, and examples thereof include metal salen complex catalysts such as cobalt salen catalysts, and organozinc catalysts.

[0046] The amount of the polymerization catalyst used in the copolymerization reaction of the epoxide monomer with carbon dioxide, for example, in the case of a metal-salen complex catalyst, is preferably 0.05 mol or less, more preferably 0.01 mol or less, and particularly preferably 0.001 mol or less, per 1 mol of the epoxide monomer. Furthermore, when using a metal salen complex catalyst, a co-catalyst can be used. As the co-catalyst, for example, an onium salt compound is preferable. Specific examples of the onium salt compound are not particularly limited, but from the viewpoint of having high reaction activity, bis(triphenylphosphoranylidene)ammonium chloride, piperidine, bis(triphenylphosphoranylidene)ammonium fluoride, ammonium pentafluorobenzoate, and tetra-n-butylammonium chloride are preferable.

[0047] Incidentally, the optimum polymerization conditions vary depending on the type of catalyst, but for example, the pressure of carbon dioxide in the reaction vessel is 0.1 MPa or more and 10 MPa or less, preferably 0.5 MPa or more and 5 MPa or less. Furthermore, in the case of a cobalt salen complex catalyst, for example, the polymerization temperature is preferably about room temperature (25° C.) from the viewpoint of good catalytic activity and accelerated reaction rate.

[0048] In the method of copolymerizing an epoxide monomer with carbon dioxide, examples of the epoxide monomer used as a starting material include ethylene oxide, propylene oxide, 1,2-butylene oxide, allyl glycidyl ether, glycidyl acrylate, glycidyl methacrylate, and 4-hydroxybutyl acrylate glycidyl ether. Note that the molar ratio of the constitutional unit represented by general formula (1) and the constitutional unit represented by general formula (2) in the copolymer may not match the molar mixing ratio of the epoxide monomer serving as the starting material for the constitutional unit represented by general formula (1) and the epoxide monomer serving as the starting material for the constitutional unit represented by general formula (2) due to differences in reactivity.

[0049] (Properties of thin polymer films) In the polymer thin film according to the present embodiment, the amount of copolymer eluted in ethyl acetate is preferably 40% or less, more preferably 20% or less, particularly preferably 10% or less, and very preferably 7% or less. The amount of eluted copolymer is preferably as low as possible because the eluted low molecular weight component becomes an irreversible capacity. The lower limit of the amount of eluted copolymer is not particularly limited, and may be, for example, 1% or more, 0.1% or more, or 0%.

[0050] In the polymer thin film according to this embodiment, it is preferable that the amount of the copolymer eluted into ethyl acetate is within the above range, and the degree of swelling of the copolymer in a mixed solvent of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1 is 100% or more.

[0051] As described above, the polymer thin film according to the present embodiment preferably has high swelling in the electrolyte and the carbonate-based solvent used as the electrolyte solvent. From this viewpoint, the swelling degree of the copolymer in the mixed solvent of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1 is preferably 100% or more, more preferably 200% or more, even more preferably 300% or more, particularly preferably 500% or more, very preferably 700% or more, and most preferably 900% or more. The upper limit of this swelling degree is not particularly limited, and may be, for example, 2000% or less.

[0052] From the viewpoint of film strength, the polymer thin film according to this embodiment has a thickness of preferably 1 μm or more, more preferably 3 μm or more, and even more preferably 5 μm or more. From the viewpoint of reducing the resistance of the film, the polymer thin film according to this embodiment has a thickness of preferably 20 μm or less, more preferably 16 μm or less, and even more preferably 12 μm or less.

[0053] (Method of manufacturing polymer thin film) In the polymer thin film according to the present embodiment, a photopolymerization initiator is preferably used from the viewpoint of facilitating the production of a polymer thin film containing a copolymer. When a photopolymerization initiator is used in the polymer thin film according to the present embodiment, reactive groups (allyl groups and (meth)acryloyl groups) in the side chains of the copolymer in the thin film react to crosslink the thin film containing the copolymer.

[0054] An example of a preferred method for producing the polymer thin film according to this embodiment will be described.

[0055] The method for producing a polymer thin film according to this embodiment includes the following steps. A step of mixing the copolymer and a photopolymerization initiator to prepare a mixture (step 1). A step of forming the mixture to obtain a formed product (step 2). A step (step 3) of irradiating the molded product with energy rays to obtain a polymer thin film containing the copolymer. "Energy rays" refers to electromagnetic waves or charged particle beams that have an energy quantum. Examples of energy rays include ultraviolet rays, radiation, and electron beams. Ultraviolet rays can be irradiated using an electrodeless lamp, a high-pressure mercury lamp, a metal halide lamp, a xenon lamp, a black light, an LED lamp, etc. Electron beams generated by an electron beam accelerator or the like can be irradiated.

[0056] According to one aspect of the method for producing a polymer thin film according to the present embodiment, a thin film containing a copolymer is obtained as the polymer thin film, and a free-standing film of the thin film can be easily obtained.

[0057] (Process 1) Step 1 is a step of mixing raw materials for obtaining a polymer thin film to obtain a mixture. In step 1, first, the above-mentioned copolymer and photopolymerization initiator are prepared as raw materials for obtaining a polymer thin film. The copolymer is obtained, for example, by the above-mentioned manufacturing method. Next, the desired amount of the prepared raw materials is weighed. Thereafter, the weighed raw materials are mixed, and further, a dilution solvent is added as necessary to prepare a mixture. The mixture may be prepared by stirring the raw materials with a known stirring device or the like. The mixture prepared in step 1 is a mixture for forming a polymer thin film.

[0058] The photopolymerization initiator is not particularly limited, and may be a known compound. The photopolymerization initiator is preferably a photopolymerization initiator that is sensitive to ultraviolet light. The photopolymerization initiator may be used alone or in combination of two or more kinds.

[0059] Specific examples of the photopolymerization initiator include α-ketol compounds such as 4-(2-hydroxyethoxy)phenyl(2-hydroxy-2-propyl)ketone, α-hydroxy-α,α'-dimethylacetophenone, 2-methyl-2-hydroxypropiophenone, and 1-hydroxycyclohexylphenyl ketone; acetophenone compounds such as methoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxyacetophenone, and 2-methyl-1-[4-(methylthio)-phenyl]-2-morpholinopropane-1; benzoin ether compounds such as benzoin ethyl ether, benzoin isopropyl ether, and anisoin methyl ether; ketal compounds such as benzyl dimethyl ketal; aromatic sulfonyl chloride compounds such as 2-naphthalenesulfonyl chloride; photoactive oxime compounds such as 1-phenone-1,1-propanedione-2-(o-ethoxycarbonyl)oxime; benzophenone, benzoylbenzoic acid, 3,3'-dimethyl-4-methoxybenzophenone, etc.; thioxanthone compounds (thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, etc.); camphorquinone, halogenated ketones, acylphosphinoxides, acylphosphonates, and oligo[2-hydroxy-2-methyl-1-(4-(1-methylvinyl)phenyl)propanone].

[0060] The content of the photopolymerization initiator is, for example, preferably 0.1 parts by mass or more and 10 parts by mass or less, more preferably 0.5 parts by mass or more and 7.5 parts by mass or less, and even more preferably 1 part by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the copolymer.

[0061] (Process 2) Step 2 is a step of obtaining a molded product from the mixture prepared in step 1. In step 2, the mixture prepared in step 1 is molded to obtain a molded product. The molding of the mixture is not particularly limited, and may be molded, for example, by applying the mixture to the surface of a support to form a coating film. As the support, for example, a release film having a release-treated surface on at least one side of the substrate may be used. The mixture prepared in step 1 may be applied to the release-treated surface of the release film to form a coating film to obtain a molded product. In addition, when a release film is used, a first release film having a release-treated surface on at least one side of the substrate is used, and the mixture prepared in step 1 is applied to the release-treated surface to form a coating film to obtain a molded product, and then the release-treated surface of a second release film having a release-treated surface on at least one side of the substrate may be superimposed on the molded product. The molded product may be sandwiched between the first release film and the second release film and subjected to step 3.

[0062] (Step 3) Step 3 is a step of obtaining a polymer thin film containing the copolymer from the molded product obtained in step 2. In step 3, the molded product molded in step 2 is irradiated with energy rays, whereby the copolymer is crosslinked to obtain a thin film that is a crosslinked product of the copolymer. The type of energy rays is not particularly limited, but ultraviolet rays are preferred in terms of reactivity and workability. The device for irradiating the molded product with ultraviolet rays is not particularly limited, and may be, for example, a device equipped with an ultraviolet LED lamp, a device equipped with a high-pressure mercury lamp, or a device equipped with a metal halide lamp.

[0063] The conditions for irradiating the molded product with ultraviolet light are not particularly limited. The maximum illuminance and the integrated light quantity when irradiating the molded product with ultraviolet light are, for example, as follows: maximum illuminance: 5 to 1000 mW / cm 2 The integrated light amount is preferably 50 to 5000 mJ / cm. 2 It is preferable that:

[0064] The polymer thin film according to the present embodiment is obtained through the above steps 1, 2, and 3. The release film used in step 2 is irradiated with ultraviolet light in step 3, and then the release film is peeled off from the thin film to obtain the polymer thin film according to the present embodiment.

[0065] [How to use polymer thin film] The polymer thin film according to the present embodiment has high swelling properties in an electrolyte solution or the like, and can be used in applications where such properties are required. The polymer thin film according to the present embodiment is preferably used, for example, in batteries. In this case, the polymer thin film according to the present embodiment is preferably used, for example, as a battery separator, and is also preferably used as a battery separator for a secondary battery such as a lithium ion battery.

[0066] [battery] Next, a preferred example of the battery according to this embodiment will be described.

[0067] The battery according to the present embodiment is a battery to which the polymer thin film according to the present embodiment is applied. The battery according to the present embodiment includes, for example, the polymer thin film according to the present embodiment as a battery separator. The battery is composed of a positive electrode, a negative electrode, and an electrolyte layer disposed between the positive electrode and the negative electrode. By adopting such a configuration, a battery excellent in each characteristic can be obtained. In addition, the battery is preferably a secondary battery, and more preferably a secondary battery such as a lithium ion battery. The structure of the battery according to the present embodiment is not particularly limited, and may be a laminated structure or a wound structure.

[0068] Here, an example of a battery using the polymer thin film according to the present embodiment will be described with reference to the drawings. In the drawings, some parts are illustrated enlarged or reduced in size for ease of explanation.

[0069] FIG. 1 shows an example of a battery using the polymer thin film according to the present embodiment. The battery 100 shown in FIG. 1 is a lithium ion secondary battery. As shown in FIG. 1, the battery 100 includes a positive electrode 10, a negative electrode 20, and an electrolyte layer 30 between the positive electrode 10 and the negative electrode 20. The positive electrode 10 is composed of a positive electrode current collector 13 and a positive electrode composite layer 11 laminated on the positive electrode current collector 13, and the negative electrode 20 is composed of a negative electrode current collector 23 and a negative electrode composite layer 21 laminated on the negative electrode current collector 23. The electrolyte layer 30 is composed of an electrolyte 33 and a separator 31 impregnated with the electrolyte 33, and the separator 31 separates the positive electrode 10 side from the negative electrode 20 side. The battery 100 has a laminated structure in which a positive electrode current collector 13, a positive electrode mixture layer 11, an electrolyte layer 30, a negative electrode mixture layer 21, and a negative electrode current collector 23 are laminated in this order from the positive electrode current collector 13 toward the negative electrode current collector 23, and the laminated structure is housed inside a container (not shown). In the battery 100, the polymer thin film according to this embodiment is used as a separator 31.

[0070] According to the battery using the polymer thin film of this embodiment, the above-mentioned configuration can suppress the generation of dendrites. The reason for this is unclear, but it is thought to be as follows. When the polymer thin film of this embodiment is used as the separator 31, when assembling the battery, after the electrolyte is injected, the separator 31 and the electrolyte 33 are separated as shown in FIG. 2(A). In this state, a gap due to fine irregularities exists between the negative electrode mixture layer 21 and the separator 31. Then, dendrites are precipitated in this portion. On the other hand, since the separator 31 using the polymer thin film of this embodiment has high swelling property in the electrolyte 33, the separator 31 swells as shown in FIG. 2(B) after a certain time has passed after the electrolyte is injected. Then, due to such swelling of the separator 31, the gap between the negative electrode mixture layer 21 and the separator 31 disappears as shown in FIG. 2(C). Therefore, when the polymer thin film of this embodiment is used as the separator 31, the generation of dendrites can be suppressed.

[0071] Although an example of the battery according to the present embodiment has been described above with reference to Fig. 1 and Fig. 2, the example of the battery according to the present embodiment is not limited thereto. The battery according to the present embodiment may adopt various forms as long as the polymer thin film according to the present embodiment is used.

[0072] Examples of materials used for the positive electrode current collector and the negative electrode current collector include metal foils or metal plates such as copper, aluminum, nickel, titanium, and stainless steel, as well as carbon sheets and carbon nanotube sheets.

[0073] The positive electrode mixture layer is composed of, for example, a positive electrode active material such as a lithium-containing composite oxide, a conductive assistant such as a carbon-based material, a binder, and the like.

[0074] The negative electrode mixture layer is composed of, for example, a negative electrode active material such as acetylene black, carbon nanotubes, carbon nanofibers, and graphene, a conductive assistant such as a carbon-based material, a binder, and the like.

[0075] The electrolyte layer is composed of, for example, an electrolyte solution and a separator. The separator is as described above.

[0076] In the battery according to this embodiment, the electrolyte preferably contains a lithium salt and a carbonate-based solvent.

[0077] Specific examples of lithium salts include lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium 2-trifluoromethyl-4,5-dicyanoimidazolate, lithium 4,5-dicyano-1,2,3-triazolate, lithium bis(pentafluoroethylsulfonyl)imide, lithium borofluoride, lithium bis(oxalato)borate, lithium nitrate, lithium chloride, lithium bromide, and lithium fluoride. The lithium salt may be one or more of these exemplified lithium salts.

[0078] Examples of the carbonate-based solvent include dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, ethylene carbonate, propylene carbonate, and butylene carbonate. The carbonate-based solvent can be one or more of the lithium salts listed above. Here, the carbonate-based solvent in this embodiment refers to a compound having a carbonate skeleton in its molecular structure.

[0079] The present invention is not limited to the above-described embodiment, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention. EXAMPLES

[0080] The present invention will be described in more detail below by way of examples, but the present invention is not limited to these examples in any way.

[0081] Measurements and evaluations in the following Examples and Comparative Examples were carried out by the methods described below.

[0082] [Measurement of weight average molecular weight (Mw) and number average molecular weight (Mn)] Measurements were carried out under the following conditions using a gel permeation chromatograph (manufactured by Tosoh Corporation, product name "HLC-8320GPC"), and the values ​​measured were converted into standard polystyrene equivalent values. (Measurement conditions) Column: "TSKgel guardcolumn SuperH-H", "TSKgel SuperHM-H", "TSKgel SuperHM-H" and "TSKgel SuperH2000" (all manufactured by Tosoh Corporation) connected in series Column temperature: 40℃ Developing solvent: Tetrahydrofuran (copolymer concentration 1% by mass) Standard material: polystyrene ·Injection volume: 20μL ·Flow rate: 0.60mL / min Detector: Differential refractometer

[0083] [Measurement of elution amount] The thin film obtained in each of the examples and comparative examples described below was weighed to about 300 mg. The mass of the thin film at this time was defined as M0. The thin film was wrapped in a polyester mesh (mesh size 200). The mass of the thin film wrapped in the polyester mesh was weighed, and the mass of the thin film was subtracted to calculate the mass of the polyester mesh alone. Next, the thin film wrapped in the polyester mesh was immersed in ethyl acetate at 23°C for 48 hours. Thereafter, the thin film wrapped in the polyester mesh was taken out of the ethyl acetate, dried in an oven at 120°C for 2 hours, and further air-dried for 2 hours in an environment at a temperature of 23°C and a relative humidity of 50%. The mass after the air drying was weighed, and the mass of the thin film alone after immersion was calculated by subtracting the mass of the polyester mesh alone. The mass at this time was defined as M1. The amount of elution was calculated using the following formula (F1). Elution amount (%)={(M0-M1) / M0}×100 (F1) In formula (F1), M0 represents the mass of the thin film weighed before being wrapped in the polyester mesh, and M1 represents the mass of the thin film alone after being immersed in ethyl acetate.

[0084] [Swelling degree measurement] The thin film obtained in each of the examples and comparative examples described below was cut to about 3 cm (vertical) x about 3 cm (horizontal), and the obtained thin film piece was weighed to be about 1 g. The mass at this time was defined as W0. The thin film piece was wrapped in a polyester mesh (mesh size 200), and the mass of the thin film piece wrapped in the polyester mesh was weighed, and the mass of the thin film piece was subtracted to calculate the mass of the polyester mesh alone. The thin film was immersed in a carbonate-based solvent [composition: mixed solvent of ethylene carbonate / dimethyl carbonate = 1 / 1 (volume ratio)] for 24 hours to cause swelling. Thereafter, the thin film piece wrapped in the polyester mesh was pulled out, the solvent on the surface was wiped with a paper wiper, and the mass was measured, and the mass of the swollen thin film piece was calculated by subtracting the mass of the polyester mesh alone. The mass at this time was defined as W1. The swelling degree was calculated using the following formula (F2). Swelling degree (%) = {(W1-W0) / W0} × 100 (F2) In formula (F2), W0 represents the mass of the thin film piece weighed before being wrapped in the polyester mesh, and W1 represents the mass of only the thin film piece after swelling.

[0085] [Ionic conductivity measurement] For the full cells obtained in each of the Examples and Comparative Examples described below, measurements were performed using the AC impedance method, in which an AC voltage (applied voltage of 10 mV) is applied between the electrodes to measure the resistance component. The ionic conductivity was calculated from the real impedance intercept of the obtained Cole-Cole plot. A potentiostat / galvanostat (VMP-300, manufactured by Biologic) was used for the measurements. Ionic conductivity (σ A ) was calculated using the following formula (F3). σ A =L A / (R A ×S A ) (F3) In formula (F3), σ A is the ionic conductivity (unit: S cm -1 ), R A is resistance (unit: Ω), S A is the cross-sectional area of ​​the solid electrolyte membrane at the time of measurement (unit: cm 2 ), L A indicates the distance between electrodes (unit: cm). In addition, the inter-electrode distance in the examples (swelling separator) was the value after the separator was swollen in the electrolyte. The measurement temperature was 25°C. The ionic conductivity (σ A ) was calculated.

[0086] [Example 1] (Synthesis of Polymerization Catalyst) (R,R)-N,N'-bis(3,5-di-tert-butylsalicylidene)-1.2-diaminocyclohexanecobalt(II) and pentafluorobenzoic acid were weighed out to a molar ratio of 1:1.1 and placed in a flask, to which was added dehydrated toluene. The flask was shielded from light with aluminum foil and allowed to react at room temperature for 20 hours. The chemical reaction formula is as follows. After the reaction was completed, the solvent was removed under reduced pressure and the mixture was washed several times with an excess amount of hexane. It was then vacuum dried at room temperature to obtain a cobalt salen complex.

[0087] [ka]

[0088] (Synthesis of Copolymer A) As the epoxide monomer, a mixture of propylene oxide and glycidyl methacrylate in a molar ratio of 96:4 was used, and the synthesized cobalt salen complex as the polymerization catalyst and bis(triphenylphosphoranylidene)ammonium chloride as the cocatalyst were weighed out in a molar ratio of epoxide monomer:catalyst:cocatalyst = 2000:1:1 and placed in a pressure vessel. Furthermore, after adding 200 ppm of phenothiazine, ethyl acetate was added so that the monomer:ethyl acetate = 50:50 (mass ratio). All of these operations were performed by replacing the inside of the pressure vessel with argon. Next, after purging the inside of the pressure vessel, carbon dioxide was introduced into the pressure vessel by a liquid pump, the pressure in the pressure vessel was set to 2.0 MPa, and the polymerization reaction was carried out at 25 ° C for 20 hours. After the reaction was completed, chloroform was added to the contents of the pressure vessel to prepare a chloroform solution, and 1M hydrochloric acid was added. Next, the chloroform solution was dropped into stirred methanol to precipitate the product. The product was then dried under reduced pressure in a desiccator using a diaphragm pump, and then vacuum dried at 60°C to obtain copolymer A.

[0089] The structure of the obtained copolymer A was confirmed by nuclear magnetic resonance spectroscopy ( 1When H-NMR (Biospin Avance 500, Bruker) was used with a solvent (CDCl3, containing 0.03 volume% tetramethylsilane), the molar ratio of the structural unit represented by general formula (1) (hereinafter also referred to as structural unit (1)), the structural unit represented by general formula (2) (hereinafter also referred to as structural unit (2)), the structural unit represented by general formula (3) (hereinafter also referred to as structural unit (3)), and the structural unit represented by general formula (4) (hereinafter also referred to as structural unit (4)) in copolymer A was structural unit (1):structural unit (2):structural unit (3):structural unit (4)=95.4:4.3:0.3:0 (see FIG. 3). The number average molecular weight Mn of the resulting copolymer A was 35,000, and the molecular weight distribution Mw / Mn was 1.3.

[0090] (Preparation of thin films) To the obtained copolymer A, 1-hydroxycyclohexyl phenyl ketone was added as a photopolymerization initiator so that the copolymer: initiator = 97: 3 mass%, and further diluted with ethyl acetate and stirred to prepare a solution for thin film formation with a solid content concentration of 30 mass%. A first release film (manufactured by Lintec Corporation, product name "SP-PET381031") was prepared, and the prepared solution for thin film formation was applied to the release-treated surface of this release film, and dried at 120 ° C for 1 minute to form a thin film layer with a thickness of 10 μm. Furthermore, a second release film (manufactured by Lintec Corporation, product name "SP-PET382150") was prepared, and the release-treated surface of this release film was attached to the surface of the thin film layer. Thereafter, the thin film laminate sandwiched between the first release film and the second release film was placed on a stainless steel plate, and irradiated with ultraviolet light [illuminance: 200 mW / cm 2 ] at 50 ° C. 2 , Accumulated light intensity: 1000mJ / cm 2 A thin film having a thickness of 6 μm was obtained by measuring the amount of elution and the degree of swelling using an illuminance actinometer (control unit: EYE UV METER UVPF-A2, light receiving unit: EYE UV METER PD-365A2) manufactured by Eye Graphics Co., Ltd. The thin film obtained was a separator. The amount of elution and the degree of swelling of the obtained thin film were measured using the above-mentioned method.

[0091] (Preparation of positive electrode) Cathode active material (Li1+xNi 1 / 2 Co 3 / 5 Mn 2 / 5 O2), a conductive material (acetylene black: AB), and a binder (polyvinylidene fluoride: PVdF) were mixed in a mass ratio of 96:2:2 and dispersed in a dispersion medium (N-methylpyrrolidone: NMP) to prepare a paste for a positive electrode composite. The paste for a positive electrode composite was then applied to a positive electrode current collector (aluminum foil, 15 μm thick), and then dried and rolled to produce a sheet-shaped positive electrode.

[0092] (Preparation of negative electrode) Granular natural graphite (amorphous coated spherical natural graphite) with its surface coated with amorphous carbon was used as the negative electrode active material, and the negative electrode active material was mixed with a conductive assistant (acetylene black: AB), a thickener (carboxymethyl cellulose: CMC), and a binder (styrene butadiene rubber: SBR) in a mass ratio of 96:2:1:1, and dispersed in a dispersion medium (water) to prepare a paste for a negative electrode composite. The paste for a negative electrode composite was then applied to a negative electrode current collector (copper foil, 11 μm thick), which was then dried and rolled to produce a sheet-shaped negative electrode.

[0093] (Preparation of electrolyte) EC (ethylene carbonate) and DMC (dimethyl carbonate) were mixed at a volume ratio of 1:1. LiTFSL was mixed into the EC and DMC mixed solvent to make the concentration 1M, to prepare an electrolyte solution.

[0094] (Preparation of full cell) The thin film prepared above was punched out to a diameter of 19 mm to prepare a separator. A full cell was prepared by sandwiching the separator between the positive and negative electrodes prepared above. The electrolyte prepared above was poured into the prepared cell and allowed to stand for 3 hours, after which the ionic conductivity was measured using the method described above. After the measurement, the cell was disassembled and the thickness of the separator was measured, which was 12 μm.

[0095] [Example 2] (Polymerization of Copolymer B) Copolymer B was obtained by polymerization in the same manner as in Example 1, except that a mixture of propylene oxide and glycidyl methacrylate in a molar ratio of 98.5:1.5 was used as the epoxide monomer. The structure of the obtained copolymer B was confirmed by nuclear magnetic resonance spectroscopy, and the molar ratio in copolymer B was structural unit (1): structural unit (2): structural unit (3): structural unit (4)=97.5:1.6:0.9:0 (see FIG. 4). The number average molecular weight Mn of the resulting copolymer B was 23,000, and the molecular weight distribution Mw / Mn was 1.3.

[0096] (Preparation of thin films) A thin film having a thickness of 7 μm was prepared in the same manner as in Example 1, except for using Copolymer B. The amount of elution and the degree of swelling of the obtained thin film were measured.

[0097] (Preparation of full cell) A full cell was prepared using a thin film prepared from copolymer B in the same manner as in Example 1. An electrolyte solution was poured into the prepared cell, which was then allowed to stand for 3 hours, after which the ionic conductivity was measured. After the measurement, the cell was disassembled and the thickness of the separator was measured, which was 52 μm.

[0098] [Comparative Example 1] (Preparation of full cell) A polyolefin separator (7 μm thick) manufactured by SEMCORP was punched out to a diameter of 19 mm. A full cell was prepared by sandwiching the separator between the positive and negative electrodes prepared above. The electrolyte prepared above was poured into the prepared cell and allowed to stand for 3 hours, after which the ionic conductivity was measured using the method described above. After the measurement, the cell was disassembled and the thickness of the separator was measured, which was 7 μm.

[0099] [Comparative Example 2] (Preparation of thin films) Polypropylene carbonate (product name "QPAC40", manufactured by EMPOWER MATERIALS) was diluted with chloroform to prepare a solution for thin film formation with a solid concentration of 30% by mass. The prepared solution was applied to the release-treated surface of a release film (manufactured by LINTEC CORPORATION, product name "SP-PET381031") and dried at a temperature of 90°C for 1 minute to obtain a thin film with a thickness of 10 μm. The amount of elution and the degree of swelling of the obtained thin film were measured.

[0100] (Preparation of full cell) A full cell was prepared using a thin film prepared from QPAC40 in the same manner as in Example 1. An electrolyte was poured into the prepared cell, and the cell was allowed to stand for 3 hours, after which the ion conductivity was measured, but the measurement was not possible due to a short circuit. Furthermore, when the cell was dismantled after the measurement, the thin film was found to have dissolved and disappeared.

[0101] [Comparative Example 3] (Polymerization of Copolymer C) Copolymer C was obtained by polymerization in the same manner as in Example 1, except that a mixture of propylene oxide and glycidyl methacrylate in a molar ratio of 90:10 was used as the epoxide monomer. The structure of the obtained copolymer C was confirmed by nuclear magnetic resonance spectroscopy, and the molar ratio in copolymer B was structural unit (1): structural unit (2): structural unit (3): structural unit (4) = 83.7:15.0:1.1:0.2. The resulting copolymer C had a number average molecular weight Mn of 20,000 and a molecular weight distribution Mw / Mn of 1.2.

[0102] (Preparation of thin films) A thin film having a thickness of 13 μm was prepared in the same manner as in Example 1, except for using Copolymer C. The amount of elution and the degree of swelling of the obtained thin film were measured.

[0103] (Preparation of full cell) A full cell was prepared using a thin film prepared from copolymer C in the same manner as in Example 1. An electrolyte solution was poured into the prepared cell, and the cell was allowed to stand for 18 hours, after which the ionic conductivity was measured. After the measurement, the cell was disassembled and the thickness of the separator was measured, which was 15 μm.

[0104] [Table 1]

[0105] [Table 2]

[0106] The results shown in Table 2 demonstrate that the polymer thin films obtained in Examples 1 and 2 have high swelling properties in the electrolyte solution. [Explanation of symbols]

[0107] Reference Signs List 10: positive electrode, 11: positive electrode composite layer, 13: positive electrode current collector, 20: negative electrode, 21: negative electrode composite layer, 23: negative electrode current collector, 30: electrolyte layer, 31: separator, 33: electrolyte, 100: battery.

Claims

1. The copolymer includes a structural unit represented by the following general formula (1) and a structural unit represented by the following general formula (2) in an amount of 0.3 mol % to 10.0 mol %: Polymer thin film. 【Chemistry 1】 (In the general formula (1) and the general formula (2), R 1 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms; L 1 and L 2 each independently represents a single bond or an alkylene group having 1 to 3 carbon atoms; L 3 is a single bond, an alkylene group having 1 to 5 carbon atoms, or an oxyalkylene group having 1 to 5 carbon atoms; X 1 is any one of the reactive groups represented by the following structural formula (2-1), the following structural formula (2-2), and the following structural formula (2-3). 【Chemistry 2】

2. The polymer thin film according to claim 1 , -L in the general formula (2) 3 -X 1 is any one of reactive groups represented by the following structural formula (2-4), the following structural formula (2-5), and the following structural formula (2-6): Polymer thin film. 【Chemistry 3】

3. The polymer thin film according to claim 1 or 2, The copolymer further contains at least one structural unit selected from the group consisting of a structural unit represented by the following general formula (3) and a structural unit represented by the following general formula (4), in an amount of 0.1 mol % to 30.0 mol %: Polymer thin film. 【Chemistry 4】 (In the general formula (3) and the general formula (4), R 2 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms; L 4 and L 5 each independently represents a single bond or an alkylene group having 1 to 3 carbon atoms; L 6 is a single bond, an alkylene group having 1 to 5 carbon atoms, or an oxyalkylene group having 1 to 5 carbon atoms; X 2 is any one of the reactive groups represented by the following structural formula (4-1), the following structural formula (4-2), and the following structural formula (4-3). 【Chemistry 5】

4. The polymer thin film according to claim 1 or 2, the amount of the copolymer eluted in ethyl acetate is 10% or less; The degree of swelling of the copolymer in a mixed solvent of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1 is 100% or more. Polymer thin film.

5. The polymer thin film according to claim 1 or 2 is included. battery.

Citation Information

Patent Citations

  • Battery separator, electrode body, non-aqueous electrolyte secondary battery, and manufacturing method of battery separator

    JP2022053727A