Method of manufacturing laminate, resin composition for low-temperature extrusion lamination process, and laminate

A laminate structure using a specific resin composition and lamination temperature range addresses the challenges of energy consumption and recyclability in polyethylene packaging, ensuring strong and recyclable laminates with reduced shrinkage and optical property degradation.

JP2024146308APending Publication Date: 2024-10-15JAPAN POLYETHYLENE CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023059120
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing extrusion lamination processes for polyethylene-based packaging materials face challenges in achieving sufficient lamination strength while reducing energy consumption and maintaining material recyclability, often resulting in delamination, shrinkage, and optical property deterioration due to high processing temperatures.

Method used

A method involving a laminate structure with a base layer, adhesive layer, and polyethylene layer, using a resin composition comprising linear low-density and branched low-density polyethylene resins, laminated at a temperature range of 220°C to 280°C, which includes a polyolefin film on the opposite side to enhance adhesive strength and recyclability.

Benefits of technology

The method achieves energy-efficient lamination with sufficient strength, reduces shrinkage and wrinkles, and maintains optical properties during recycling, providing a monomaterial packaging solution with improved recyclability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146308000001
    Figure 2024146308000001
  • Figure 2024146308000002
    Figure 2024146308000002
Patent Text Reader

Abstract

To provide a method for manufacturing a laminate that can be extrusion laminated at low temperatures and exhibits high laminate adhesive strength, a resin composition for low-temperature extrusion lamination processing for use in the method, and an extrusion laminate manufacturing method using the composition, and furthermore, a laminate, in particular, laminate suitable for mono-material packaging materials using a polyethylene base material.SOLUTION: A method for manufacturing a laminate that includes at least a polyethylene layer containing a linear low-density polyethylene resin (a) having a specific MFR and density and a branched low-density polyethylene resin (b) having a specific MFR and density in a specific ratio, which is extrusion laminated at a low temperature.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a laminate, a resin composition for low-temperature extrusion lamination and a method for producing an extrusion laminate using the same, and further to a laminate. More specifically, the present invention relates to a method for producing a laminate that exhibits high laminate adhesive strength and that can be extrusion laminated at a temperature lower than that generally used in the past, i.e., at a low die lip temperature of 220°C to 280°C, and a resin composition used therefor and a method for producing a low-temperature laminate using the same, and further to a laminate. In particular, the present invention relates to a mono-material packaging material using a polyethylene substrate. [Background technology]

[0002] In recent years, the increased risk of natural disasters due to global warming has been recognized, and there has been increasing interest in reducing greenhouse gas emissions in the production activities of goods and services. This trend is also seen in plastic products, and active efforts are being made to reduce carbon dioxide emissions throughout the entire life cycle of packaging materials, from production to disposal. In addition, with the rise in energy prices due to the instability of the global situation, there is a demand for energy conservation in the packaging material production process. Furthermore, there is a demand for packaging materials that can be recycled, with the aim of reducing actual carbon dioxide emissions by recycling plastic materials.

[0003] Generally, methods for manufacturing packaging materials using polyethylene include inflation processing, extrusion lamination, and dry lamination. Among these, extrusion lamination is highly productive and is used to manufacture a variety of packaging materials, but it is necessary to forcibly oxidize the resin surface at high temperatures to increase the laminate strength, and a lot of heater energy is required to heat and melt the resin. In addition, branched low-density polyethylene is often used to avoid the reduction in the effective width of the film (neck-in) caused by processing at high temperatures. However, if the processing temperature is lowered in order to reduce the energy consumption of the heater during lamination, the oxidation of the resin surface does not progress sufficiently, reducing the laminate strength and causing problems such as delamination and poor seal strength when used as a packaging material. Furthermore, from the perspective of material recyclability, including post-consumer recycling (PCR) and post-industrial recycling (PIR), mono-material packaging materials using polyethylene base materials are also beginning to be developed. When using a polyethylene base material in general extrusion lamination, the processing temperature is overwhelmingly higher than the melting point of the polyethylene base material, which causes problems with shrinkage, sagging, and wrinkles in the polyethylene base material during lamination. For these reasons, it has been difficult to provide a packaging material using branched low-density polyethylene that has sufficient lamination strength while suppressing heater energy consumption during lamination. Moreover, it has been difficult to provide a mono-material packaging material using a polyethylene base material in general high-temperature extrusion lamination.

[0004] A polyolefin resin composition containing a polyolefin resin and a compound having an intramolecular unsaturated bond has been proposed as a method for providing a packaging material that exhibits sufficient laminate strength in low-temperature lamination (Patent Document 1). However, the processing temperature range in this invention is about 280°C, and the effect is limited in terms of reducing heater energy consumption. Also, a mono-material packaging material has been proposed in which a polyethylene substrate and a polyethylene heat seal film are laminated using an adhesive layer made of a resin composition containing a polyester polyol, an isocyanate compound, and a phosphoric acid-modified compound (Patent Document 2). However, since the resin composition constituting the adhesive layer is cured by urethane bonding, the compatibility with polyethylene is poor, and the dispersibility in polyethylene during material recycling is poor, which tends to deteriorate the optical properties. In addition, when laminating a polyethylene substrate and a heat seal film, it is necessary to provide a thick adhesive layer of about 3 μm in order to maintain adhesive strength, and the ratio of the adhesive layer component to the entire packaging material is high, which causes a problem that the optical properties are more likely to deteriorate. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2000-108278 A [Patent Document 2] JP 2020-055157 A Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made with the objective of solving the above-mentioned problems of the conventional technology, and its object is to provide a resin composition that can ensure sufficient laminate strength while suppressing heater power consumption in the manufacturing process by performing extrusion lamination at a temperature lower than the processing temperature in conventional extrusion lamination, specifically at a low temperature of 220°C to 280°C in the die lip, and to provide a low-temperature lamination method and a method for manufacturing a laminate using the same.Furthermore, it is an object of the present invention to provide a polyethylene-based monomaterial laminate with excellent material recyclability. [Means for solving the problem]

[0007] That is, the present invention is as follows. <Invention 1> A method for producing a laminate obtained by extrusion lamination, comprising: at least a base layer (I), an adhesive layer (II), and a polyethylene layer (III) laminated adjacent to each other in this order; a resin temperature in a die lip during lamination of the polyethylene layer (III) is 220°C to 280°C; the polyethylene layer (III) comprises at least a linear low-density polyethylene resin (a) satisfying the following (a-1) and (a-2) and a branched low-density polyethylene resin (b) satisfying the following (b-1) and (b-2); and the polyethylene layer (III) comprises a resin composition in which the branched low-density polyethylene resin (b) accounts for 1 to 85% by weight. Linear low-density polyethylene resin (a) (a-1) MFR (190℃, 21.18N load) is 1-100g / 10min (a-2) Density is 0.918g / cm 3 less than Branched low-density polyethylene resin (b) (b-1) MFR (190℃, 21.18N load) is 1-100g / 10min (b-2) Density is 0.915 to 0.925 g / cm 3 <Invention 2> The method for producing a laminate according to Invention 1, wherein the linear low-density polyethylene resin (a) further satisfies the following (a-3) to (a-4): (a-3) Contains 80 to 98 mol% of structural units derived from ethylene as a major component, 2 to 20 mol% of structural units derived from propylene as an essential minor component, and may contain 4 mol% or less of structural units derived from a third α-olefin other than ethylene and propylene as a minor component (however, when structural units derived from the third α-olefin are contained, the total of the structural units derived from ethylene, the structural units derived from propylene, and the structural units derived from the third α-olefin does not exceed 100 mol%). (a-4) The total amount of vinyl and vinylidene in the ethylene copolymer is 0.35 (pieces / total 1000C) or more. (Note that the number of vinyl and vinylidene units is the number per 1,000 carbon atoms in the main chain and side chains, measured by NMR.) <Invention 3> 3. The method for producing a laminate according to claim 1 or 2, wherein the substrate layer (I) is a stretched substrate made of a polyethylene resin, and the adhesive layer (II) is made of a polyolefin adhesive. <Invention 4> The resin composition is for low-temperature extrusion lamination, in which extrusion lamination is performed at a low temperature in which the resin temperature in the die lip is 220°C to 280°C, and is characterized in that the resin composition contains at least a linear low-density polyethylene resin (a) that satisfies the following (a-1) and (a-2) and a branched low-density polyethylene resin (b) that satisfies the following (b-1) and (b-2), and the branched low-density polyethylene resin (b) is contained in an amount of 1 to 85% by weight. Linear low-density polyethylene resin (a) (a-1) MFR (190℃, 21.18N load) is 1-100g / 10min (a-2) Density is 0.918g / cm 3 less than Branched low-density polyethylene resin (b) (b-1) MFR (190℃, 21.18N load) is 1-100g / 10min (b-2) Density is 0.915 to 0.925 g / cm 3 <Invention 5> 5. The resin composition for low-temperature extrusion lamination according to claim 4, wherein the linear low-density polyethylene resin (a) further satisfies the following (a-3) to (a-4): (a-3) Contains 80 to 98 mol% of structural units derived from ethylene as a major component, 2 to 20 mol% of structural units derived from propylene as an essential minor component, and may contain 4 mol% or less of structural units derived from a third α-olefin other than ethylene and propylene as a minor component (however, when structural units derived from the third α-olefin are contained, the total of the structural units derived from ethylene, the structural units derived from propylene, and the structural units derived from the third α-olefin does not exceed 100 mol%). (a-4) The total amount of vinyl and vinylidene in the ethylene copolymer is 0.35 (pieces / total 1000C) or more. (Note that the number of vinyl and vinylidene units is the number per 1,000 carbon atoms in the main chain and side chains, measured by NMR.) <Invention 6> A method for producing an extrusion laminate, comprising: at least a base layer (I), an adhesive layer (II), and a polyethylene layer (III) laminated adjacent to each other in this order; the polyethylene layer (III) is made of the resin composition of Invention 4 or 5; and the resin temperature during extrusion lamination of the polyethylene layer (III) is a low temperature of 220°C to 280°C in a die lip. <Invention 7> A laminate comprising at least a base layer (I), an adhesive layer (II) and a polyethylene layer (III) laminated adjacent to each other in this order, the base layer (I) being made of a polyethylene film, the adhesive layer (II) being made of a polyolefin adhesive, the polyethylene layer (III) containing at least a linear low-density polyethylene resin (a) satisfying the following (a-1) and (a-2) and a branched low-density polyethylene resin (b) satisfying the following (b-1) and (b-2), and the branched low-density polyethylene resin (b) is contained in an amount of 1 to 85% by weight. Linear low-density polyethylene resin (a) (a-1) MFR (190℃, 21.18N load) is 1-100g / 10min (a-2) Density is 0.918g / cm 3 less than Branched low-density polyethylene resin (b) (b-1) MFR (190℃, 21.18N load) is 1-100g / 10min (b-2) Density is 0.915 to 0.925 g / cm 3 <Invention 8> 8. The laminate according to claim 7, wherein the linear low-density polyethylene resin (a) further satisfies the following (a-3) and (a-4): (a-3) Contains 80 to 98 mol% of structural units derived from ethylene as a major component, 2 to 20 mol% of structural units derived from propylene as an essential minor component, and may contain 4 mol% or less of structural units derived from a third α-olefin other than ethylene and propylene as a minor component (however, when structural units derived from the third α-olefin are contained, the total of the structural units derived from ethylene, the structural units derived from propylene, and the structural units derived from the third α-olefin does not exceed 100 mol%). (a-4) The total amount of vinyl and vinylidene in the ethylene copolymer is 0.35 (pieces / total 1000C) or more. (Note that the number of vinyl and vinylidene units is the number per 1,000 carbon atoms in the main chain and side chains, measured by NMR.) <Invention 9> 9. The laminate according to claim 7 or 8, wherein a polyolefin film (IV) is laminated adjacent to the polyethylene layer (III) on the side opposite to the adhesive layer (II). <Invention 10> A mono-material packaging material using the laminate according to Invention 7 or Invention 8. <Invention 11> A mono-material packaging material using the laminate according to invention 9. Effect of the Invention

[0008] According to the present invention, by performing extrusion lamination at low temperature, it is possible to provide a laminate having excellent energy saving properties and sufficient laminate strength, and a resin composition used therein. Furthermore, it is possible to provide a low-temperature extrusion lamination method using the laminate, and a polyethylene-based monomaterial laminate having excellent material recyclability. It is also possible to provide a laminate that not only reduces the shrinkage, sagging, and wrinkles of the substrate when laminated to a polyethylene substrate, but also suppresses the deterioration of optical properties during material recycling. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, the resin composition for low-temperature extrusion lamination suitable for the laminate manufacturing method of the present invention, the laminate using the same, the laminate manufacturing method, and the packaging material will be described in detail for each item.

[0010] 1. Basic structure of laminate The laminate of the present invention has a laminated structure in which at least a base layer (I) / an adhesive layer (II) / a polyethylene layer (III) are laminated adjacent to each other in this order, and the polyethylene layer (III) is obtained by an extrusion lamination method (hereinafter also referred to as the "laminate of the present invention"). Details of the base layer (I), the adhesive layer (II) and the polyethylene layer (III) will be described later. More preferably, the substrate layer (I) is a substrate (polyethylene film) made of a polyethylene resin, particularly preferably a stretched polyethylene substrate, and further, the adhesive layer (II) is a laminate made of a polyethylene adhesive. As all layers are mono-material materials made of polyethylene, the laminate has excellent material recyclability. A more preferred embodiment of the laminate is a laminate in which a polyolefin film (IV) is laminated adjacent to the polyethylene layer (III) on the side opposite to the adhesive layer (II).

[0011] 1.1 Base material layer (I) Examples of the base layer (I) of the present invention include monolayer films of polyamide, polyester, polypropylene, polyethylene, ethylene-vinyl alcohol copolymer, etc., and laminated films made of the same or different materials. Stretched films of these are also included. The amount of resin, such as polyamide resin or polyester resin, contained in the base layer (I) is, for example, 50% by weight to 100% by weight. It may be combined with other resins.

[0012] 1.2.Polyethylene base film In particular, the laminate of the present invention is preferably a substrate (polyethylene film) made of polyethylene resin, and more preferably a stretched substrate made of polyethylene resin. Substrates made of polyethylene resin and stretched substrates of polyethylene resin are required in monomaterial laminates composed entirely of polyethylene-based resin materials in the recent development of monomaterial recyclable packaging materials. However, in general high-temperature extrusion lamination, it has been difficult to provide a monomaterial packaging material using a polyethylene substrate because the melting point of the polyethylene substrate is low. However, in the present invention, sufficient effects can be achieved by combining with a resin composition that can be subjected to low-temperature extrusion lamination.

[0013] As the substrate film made of a polyethylene resin, an unstretched substrate film, a stretched substrate film, an electron beam crosslinked film, or the like can be used, with an unstretched substrate film and a stretched substrate film being preferred.

[0014] The term "unstretched substrate film" refers to a film obtained by subjecting a polyethylene resin composition to inflation molding or T-die molding. The term "stretched substrate film" refers to a film obtained by stretching a film obtained by subjecting a polyethylene resin composition to inflation molding or T-die molding.

[0015] Polyethylene resin composition used The polyethylene resin composition used for the polyethylene substrate film is not particularly limited, and may be a virgin resin obtained by homopolymerizing ethylene or copolymerizing ethylene and an α-olefin, a recycled resin obtained by mechanically recycling a product whose main component is used polyethylene, or an ethylene polymer produced by adopting a mass balance method certified by ISCC PLUS certification, etc. Classifications include low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), medium-density polyethylene (MDPE), and high-density polyethylene (HDPE), and the resin composition for polyethylene substrate film may be a mixture of these.

[0016] Furthermore, additives generally used for resin compositions, such as antioxidants, heat stabilizers, neutralizing agents, antiblocking agents, tackifiers, antistatic agents, slip agents, nucleating agents, foaming agents, crosslinking agents, biomass resources, and biodegradation promoters, may be blended within the scope of the present invention.

[0017] ·Unstretched polyethylene base film Examples of methods for producing the unstretched polyethylene substrate film include inflation molding, T-die molding, and calendar molding, with inflation molding and T-die molding being preferred from the viewpoints of production speed, ease of production, etc. Furthermore, the film may be a single-layer film or a multi-layer film. The manufacturing conditions for the unstretched polyethylene substrate film are not particularly limited, but the thickness of the film is preferably 5 μm to 100 μm, more preferably 10 μm to 90 μm, and further preferably 15 μm to 80 μm.

[0018] ·Stretched polyethylene base film The stretched polyethylene substrate film is obtained by stretching a raw material. Examples of the method for producing the raw material include inflation molding, T-die molding, and calendar molding, with inflation molding and T-die molding being preferred from the viewpoints of production speed and ease of production. The film may be a single-layer film using a single polyethylene resin composition, or a multi-layer film using multiple polyethylene resin compositions. Although the manufacturing conditions of the raw roll are not particularly limited, the thickness of the raw roll film is preferably 20 μm to 200 μm, more preferably 30 μm to 200 μm, and further preferably 50 μm to 200 μm. · Stretching method for oriented polyethylene base film The stretched polyethylene substrate film may be a uniaxially stretched film or a biaxially stretched film. The stretching method may be any of longitudinal uniaxial stretching, transverse uniaxial stretching, sequential biaxial stretching, and simultaneous biaxial stretching.

[0019] Multilayer oriented film The stretched substrate film made of the polyethylene resin composition may be a multilayer stretched film in which a plurality of films are laminated. Examples of resins that can be used include high density polyethylene (HDPE), medium density polyethylene (MDPE), low density polyethylene (LDPE), linear low density polyethylene (LLDPE), and ultra low density polyethylene (ULDPE). As for the lamination method, a co-extrusion film obtained by co-extrusion molding may be further stretched, or films may be bonded together using an adhesive.

[0020] A method for producing a polyethylene stretched film that can be used as a base layer constituting a laminate is described in, for example, JP 2022-155350 A and JP 2022-039843 A. Other known polyethylene films or stretched films thereof can be used. The substrate layer may be subjected to printing, deposition, various coatings, and the like.

[0021] 1.2 Adhesive layer (II) An adhesive can be used as a constituent of the adhesive layer (II) of the present invention. The adhesive used contains at least one resin composition, but is not particularly limited. Examples of adhesives that can be used include epoxy-based, acrylic-based, and urethane-based adhesives. In addition, there is a polyolefin-based adhesive that has been developed in recent years. In addition, the adhesive containing any of the above resin compositions can be a one-component type, two-component type, or hot melt type, as necessary, but is not particularly limited. In particular, for mono-material packaging materials that are composed entirely of polyethylene resin, for which there has been an increasing need for development in recent years, it is preferable to use a polyolefin-based adhesive. As the polyolefin-based adhesive, for example, a polyolefin resin aqueous dispersion type adhesive as described in Japanese Patent No. 3759160 can be used.

[0022] 1.3 Polyethylene layer (III) The polyethylene layer (III) is a layer provided by extrusion lamination, and in a preferred embodiment of the present invention, the layer is provided by lamination at a low temperature of 220° C. to 280° C., which is not used in general extrusion lamination. The characteristics of the resin composition constituting this layer will be described later.

[0023] 1.4 Polyolefin film (IV) In the laminate of the present application, it is preferable that a polyolefin film (IV) can be further laminated on the polyethylene layer (III). It can be seen that the adhesive strength of the polyethylene layer (III) is significantly improved when sandwich lamination is performed using the polyolefin film (IV). This is thought to be due to the fact that the polyethylene layer (III) is kept warm by placing the polyolefin film (IV) between the polyethylene layer (III) and the cooling roll in the laminated area, slowing down the cooling and solidifying speed, and thus improving the interfacial interaction by increasing the contact time with the adhesive layer (II) in the molten state. Examples of the polyolefin film include unstretched films or uniaxially or biaxially stretched films containing polyethylene, polypropylene or the like as a main component.

[0024] 2. Polyethylene resin composition for low-temperature extrusion lamination constituting the polyethylene layer (III) The polyethylene resin composition of the present invention constituting the polyethylene layer (III) (hereinafter also simply referred to as "resin composition") is characterized in that it comprises at least a linear low-density polyethylene resin (a) satisfying the following (a-1) to (a-2) and a branched low-density polyethylene resin (b) satisfying the following (b-1) to (b-3), and is composed of a resin composition in which the branched low-density polyethylene resin (b) is contained in the polyethylene layer (III) in an amount of 1 to 85% by weight. Linear low-density polyethylene resin (a) (a-1) MFR (190℃, 21.18N load) is 1-100g / 10min (a-2) Density is 0.918g / cm 3 less than Branched low-density polyethylene resin (b) (b-1) MFR (190℃, 21.18N load) is 1-100g / 10min (b-2) Density is 0.915 to 0.925 g / cm 3

[0025] 2.1 Linear low-density polyethylene resin (a) The linear low-density polyethylene resin (a) is a random copolymer of ethylene and an α-olefin other than ethylene, and is usually obtained by a catalytic polymerization method. The α-olefin used as a comonomer of these ethylene-α-olefin copolymers is an α-olefin having 3 to 20 carbon atoms, preferably 3 to 12 carbon atoms, and more preferably 3 to 8 carbon atoms. Specific examples of the α-olefin include propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-heptene, 4-methyl-pentene-1, 4-methyl-hexene-1, and 4,4-dimethylpentene-1. Specific examples of the ethylene-α-olefin copolymer include an ethylene-propylene copolymer, an ethylene-1-butene copolymer, an ethylene-1-hexene copolymer, and an ethylene-1-octene copolymer. The α-olefin used as a comonomer may be one type, or two or more types may be used simultaneously. For example, a multi-component copolymer using two or more types of α-olefins such as a terpolymer can also be used. Specific examples include ethylene-propylene-1-butene terpolymer, ethylene-propylene-1-hexene terpolymer, etc.

[0026] These ethylene-α-olefin copolymers are preferably those containing structural units derived from ethylene as the main component, and have an ethylene content selected from the range of, for example, 50 to 99% by weight, more preferably 60 to 97% by weight, and even more preferably 70 to 95% by weight. The α-olefin content is preferably selected from the range of, for example, 1 to 50% by weight, more preferably 3 to 40% by weight, and even more preferably 5 to 30% by weight. The ethylene content is a value measured by 13C-NMR spectrum analysis, and is measured under conditions of a temperature of 120°C, a frequency of 100 MHz, a spectral width of 20,000 Hz, a pulse repetition time of 10 seconds, and a flip angle of 40 degrees, using hexamethyldisiloxane as a standard substance for a sample (concentration: 300 mg / 2 mL) dissolved in orthodichlorobenzene. The method for producing the ethylene / α-olefin copolymer is not particularly limited as long as it can produce an ethylene / α-olefin copolymer composition that satisfies the physical properties described below, and the copolymer can be produced using a known catalyst such as a Ziegler catalyst or a metallocene catalyst. Among these, it is preferable to use a metallocene catalyst-based ethylene / α-olefin copolymer that has physical properties specific to the metallocene catalyst and is produced using a metallocene catalyst. The polymerization method may be any method that efficiently contacts the catalyst components with each monomer. Specifically, the polymerization may be carried out in the presence of these catalysts, such as a slurry method, a gas-phase fluidized bed method, a solution method, or a method in which the pressure is 200 kg / cm. 2 As mentioned above, examples of the production method include high-pressure bulk polymerization at a polymerization temperature of 100° C. or higher. A preferred production method is high-pressure bulk polymerization. The linear low-density polyethylene resin can be appropriately selected from commercially available products, such as "Affinity" manufactured by DuPont Dow, and "Kernel" and "Harmolex" manufactured by Japan Polyethylene Corporation.

[0027] (a-1)MFR The linear low-density polyethylene resin (a) used in the present invention has a melt flow rate (MFR: 190°C, 21.18N load) of 1 to 100g / 10min, preferably 1 to 80g / 10min, more preferably 3 to 70g / 10min. If the MFR is less than 1g / 10min, the extensibility during molding is poor and the motor load in the extruder is high, which is not preferred. On the other hand, if the MFR exceeds 100g / 10min, the state of the molten film during molding becomes unstable, which is not preferred.

[0028] To adjust the MFR of a polymer, for example, the polymerization temperature, the amount of comonomer, etc. are appropriately adjusted. The MFR of ethylene-propylene copolymer is measured in accordance with JIS-K6922-2:1997 Appendix (190℃, 21.18N load).

[0029] (a-2) Density The linear low-density polyethylene resin (a) used in the present invention has a density of 0.918 g / cm 3 It is necessary that the density is less than 0.85 to 0.918 g / cm. 3 and preferably 0.87 to 0.916 g / cm 3 and more preferably 0.88 to 0.915 g / cm 3 The density is 0.85g / cm 3 If the density is less than 0.918 g / cm3, blocking will be poor, which is not preferable. 3 If it exceeds this value, the adhesiveness becomes poor, which is not preferable.

[0030] The density of the polymer can be adjusted by, for example, adjusting the comonomer content, polymerization temperature, catalyst amount, etc. The density of ethylene-propylene copolymer is measured in accordance with JIS-K6922-2:1997 Appendix (for low-density polyethylene) (measurement temperature 23°C). The copolymer composition may contain three or more types of ethylene-α-olefin copolymers.

[0031] 2.2 Suitable linear low-density polyethylene resin (A) (ethylene-propylene copolymer) Furthermore, the linear low-density polyethylene resin (a) is preferably a special linear low-density polyethylene resin (A) which further satisfies the following (a-3) to (a-4) (hereinafter also referred to as "ethylene-propylene copolymer (A)"). (a-3) Contains 80 to 98 mol% of structural units derived from ethylene as a major component, 2 to 20 mol% of structural units derived from propylene as an essential minor component, and may contain 4 mol% or less of structural units derived from a third α-olefin other than ethylene and propylene as a minor component (however, when structural units derived from the third α-olefin are contained, the total of the structural units derived from ethylene, the structural units derived from propylene, and the structural units derived from the third α-olefin does not exceed 100 mol%). (a-4) The total amount of vinyl and vinylidene in the ethylene copolymer is 0.35 (pieces / total 1000C) or more. (Note that the number of vinyl and vinylidene units is the number per 1,000 carbon atoms in the main chain and side chains, measured by NMR.) Moreover, it is preferable that the following condition (a-7) be satisfied. (a-7) The resin composition contains a linear low-density polyethylene resin (a) at 1 to 90% by weight. (However, if components other than the linear low-density polyethylene resin (a) and the branched low-density polyethylene resin (b) are contained, the total weight percentage of each component does not exceed 100 weight percent.)

[0032] In addition, copolymers consisting of ethylene and propylene include so-called ethylene propylene rubber (EPM), which contains more than 20 mol% propylene and has a density of 0.870 g / cm 3 Rubber-like polymers obtained by the following solution polymerization method are used in the field of elastomers, but the ethylene-propylene copolymer (A) of the present invention is a polymer that is completely different from these ethylene-propylene rubbers in terms of density range, amount of ethylene and propylene contained, and physical properties.

[0033] Further, among propylene polymers, propylene-ethylene copolymers that contain a small amount of ethylene component during the production process are also known, but these also differ greatly in terms of the propylene content, etc., and are polymers that are completely different in physical properties, etc.

[0034] Also, ethylene-α-olefin copolymers (LLDPE) with so-called normal linear molecular structures are often developed for film applications, and so in order to obtain high-strength copolymers, it is common to use C4 or higher α-olefins such as C4 or C6 as the main comonomer components. A copolymer of ethylene and propylene using a C3 comonomer, which has a relatively low strength, as the main comonomer component has a density of 0.87 g / cm. 3 Copolymers exceeding this limit have hardly been commercially available to date.

[0035] Recently, an ethylene-propylene copolymer was experimentally produced using a C3 comonomer in this density range as the main minor component, preferably by a high-pressure ionic polymerization process which enables polymerization at high temperatures, and after various investigations, it was found that the effects of the present invention are particularly favorable in laminates containing polyethylene resin compositions using ethylene-propylene copolymers having physical properties in the new ranges, such as (a-1) to (a-4).

[0036] (i) Characteristics of ethylene-propylene copolymer (A) (a-3) Monomer structure The ethylene-propylene copolymer (A) used in the present invention is an ethylene-propylene copolymer characterized by containing 80-98 mol % of structural units derived from ethylene as a main component and 2-20 mol % of structural units derived from propylene as a secondary component, and specifically, a copolymer obtained by polymerization by catalytic polymerization method, which is a copolymer obtained by substantially linear random polymerization. Specifically, it is a random copolymer of ethylene and propylene. Preferably, the content of structural units derived from ethylene is 80-98 mol %, the content of structural units derived from propylene is 2-20 mol %, and more preferably, the content of structural units derived from ethylene is 85-95 mol %, and the content of structural units derived from propylene is 5-15 mol %. Here, the monomer content such as ethylene content is 13 The values ​​were measured and calculated by C-NMR under the conditions described in the Examples below.

[0037] In addition, it is preferable that the copolymer does not contain any other α-olefins, particularly α-olefins having 4 to 20 carbon atoms, or other monomer components, but may contain such components in a substantially small amount. In this specification, an α-olefin other than ethylene and propylene is referred to as a third α-olefin. The ethylene-propylene copolymer (A) of the present invention may contain, as a minor component, a structural unit derived from a third α-olefin other than ethylene and propylene, for example, in an amount of 4 mol% or less, preferably 2 mol% or less, more preferably 1.5 mol% or less, even more preferably 1 mol% or less, and most preferably 0.5 mol% or less. Here, when the ethylene-propylene copolymer (A) of the present invention contains a structural unit derived from a third α-olefin, the total amount of the structural units derived from ethylene, the structural units derived from propylene, and the structural units derived from the third α-olefin does not exceed 100 mol%. In this case, the content of the structural units derived from propylene is preferably higher than the content of the structural units derived from the third α-olefin. When the ethylene-propylene copolymer (A) of the present invention contains a structural unit derived from a third α-olefin, one or more kinds of the third α-olefin can be used.

[0038] The ethylene-propylene copolymer (A) may be one type or a combination of two or more types, so long as it satisfies (a-1) to (a-4).

[0039] When propylene is used as a secondary component and is an essential comonomer, and in particular when high-pressure ionic polymerization using a metallocene catalyst (described later) is used, it is possible to obtain ethylene-α-olefin copolymers with a specifically high total number of vinyl and vinylidene units. This effect is difficult to obtain when α-olefins such as 1-hexene and 1-octene are polymerized as the main comonomer components.

[0040] (a-1)MFR The ethylene-propylene copolymer (A) used in the present invention has a melt flow rate (MFR: 190°C, 21.18N load) of 1 to 100g / 10min, preferably 1 to 80g / 10min, and more preferably 3 to 70g / 10min. If the MFR is less than 1g / 10min, the extensibility during molding is poor and the motor load in the extruder is high, which is not preferable. On the other hand, if the MFR exceeds 100g / 10min, the state of the molten film during molding becomes unstable, which is not preferable.

[0041] To adjust the MFR of a polymer, for example, the polymerization temperature, the amount of comonomer, etc. are appropriately adjusted. The MFR of ethylene-propylene copolymer is measured in accordance with JIS-K6922-2:1997 Appendix (190℃, 21.18N load).

[0042] (a-2) Density The ethylene-propylene copolymer (A) used in the present invention has a density of 0.918 g / cm 3 and preferably 0.85 to 0.918 g / cm 3 and more preferably 0.87 to 0.916 g / cm 3 and more preferably 0.88 to 0.915 g / cm 3 The density is 0.85g / cm 3 If the density is less than 0.918 g / cm3, blocking will be poor, which is not preferable. 3 If it exceeds this value, the adhesiveness becomes poor, which is not preferable.

[0043] The density of the polymer can be adjusted by, for example, adjusting the comonomer content, polymerization temperature, catalyst amount, etc. The density of ethylene-propylene copolymer is measured in accordance with JIS-K6922-2:1997 Appendix (for low-density polyethylene) (measurement temperature 23°C).

[0044] (a-4) Total number of vinyls and vinylidenes In copolymers obtained by copolymerizing ethylene with one or more α-olefins, even if diene monomers are not actively added, various double bonds (vinyl, vinylidene, cis-vinylene, trans-vinylene, tri-substituted olefins) may be produced due to differences in the mechanisms of the manufacturing process, and the amounts and types of double bonds vary. In the present invention, it was found that, among the various double bonds contained in an ethylene-propylene copolymer, vinyl and vinylidene are particularly important in terms of adhesive strength, and it was also found that a resin composition containing an ethylene-propylene copolymer in which the total number of vinyl and vinylidene is greater than that of a normal ethylene-α-olefin copolymer is particularly suitable as a resin composition for low-temperature lamination and achieves the effects of the present invention, and this has led to the completion of the present invention.

[0045] The ethylene-propylene copolymer (A) used in the present invention has a total amount of vinyl and vinylidene per 1000 carbon atoms in the main chain and side chains, i.e., the total number of vinyl and vinylidene double bonds, measured by NMR, of 0.35 (units / total 1000C) or more, preferably 0.40 to 5.0 (units / total 1000C), more preferably 0.45 to 4.5 (units / total 1000C), and even more preferably 0.50 to 4.0 (units / total 1000C). When the total number of vinyl and vinylidene is within the above range, the resin composition has excellent adhesive strength, and when it is less than 0.35, the adhesive strength is not sufficient. The total number of vinyl and vinylidene can be controlled within the above range by appropriately selecting a suitable metallocene catalyst, adjusting the polymerization temperature, the type of comonomer, and the amount of comonomer. The number of double bonds is per 1,000 carbon atoms in the main chain and side chains combined. 1 The value was calculated using the integrated intensity of a characteristic peak in the H-NMR spectrum, and was measured and calculated under the conditions described in the Examples below. Furthermore, in the present invention, the number of vinyl groups in the ethylene-propylene copolymer (A) preferably satisfies the range of 0.2 (groups / total 1000C) or more. In the present invention, the number of vinylidenes in the ethylene-propylene copolymer preferably satisfies the range of 0.12 (units / total 1000C) or more.

[0046] (a-5) Relationship between the number of branches (Y) and density (X) due to comonomers The ethylene-propylene copolymer (A) used in the present invention preferably has a branch number (Y) and density (X) due to comonomers that satisfy the following formula (1). Formula (1): (Y) ≧ -1157×(X)+1080 When the density and the number of branches satisfy the relationship of the above formula (1), the number of branches due to the comonomer is sufficiently ensured, resulting in a resin composition with excellent adhesive strength. Here, the number of branches due to comonomers (Y) is the number per 1000 total carbon atoms in the main chain and side chains (units / total 1000C) measured by NMR for ethylene-propylene copolymer (A). Furthermore, density (X) is the density of the ethylene-propylene copolymer (A) and is measured as described above. The number of branches (Y) due to comonomers indicates the amount of tertiary carbons contained in the polymer, and is the number per 1000 carbons in total in the main chain and side chains, as measured by NMR. For example, see EW Hansen, R. Blom, and OM Bade, Polymer, Vol. 36, p. 4295 (1997). 13 It can be calculated from the C-NMR spectrum. The relationship between the density and the number of branches can be adjusted by the polymerization conditions such as the type and ratio of the comonomers to be copolymerized and the polymerization temperature.

[0047] (a-6) Relationship between the number of branches (Y) and density (X) due to comonomers The ethylene-propylene copolymer (A) used in the present invention preferably has a branch number (Y) and density (X) based on the comonomer that satisfy the following formula (2). Formula (2): (Y) ≧ -1157×(X)+1084 When the density and the number of branches satisfy the relationship of the above formula (2), the number of branches due to the comonomer is sufficiently ensured, resulting in a resin composition with excellent adhesive strength. Here, the number of branches due to comonomers (Y) is the number per 1000 total carbon atoms in the main chain and side chains (units / total 1000C) measured by NMR for ethylene-propylene copolymer (A).

[0048] (ii) Polymerization catalyst and polymerization method for ethylene-propylene copolymer (A) The catalyst used in the production of the ethylene-propylene copolymer (A) used in the present invention is not particularly limited, but a metallocene catalyst is more preferably used. The metallocene catalyst is not particularly limited, but may be a catalyst containing a metallocene compound such as a zirconium compound coordinated with a group having a cyclopentadienyl skeleton and a cocatalyst as a catalytic component. In particular, it is preferable to use a metallocene compound such as a zirconium compound coordinated with a group having a cyclopentadienyl skeleton. The production method is not particularly limited, and a high-pressure ionic polymerization method, a gas phase method, a solution method, a slurry method, etc. can be used. However, in order to obtain the ethylene-propylene copolymer (A) according to the present invention having adjusted double bonds, it is desirable to carry out the polymerization at a high temperature of 150 to 330°C, and therefore it is preferable to use a high-pressure ionic polymerization method ("Polyethylene Technology Reader", Chapter 4, edited by Kazuo Matsuura and Naotaka Mikami, 2001).

[0049] (iii) Amount of ethylene-propylene copolymer (A) The ethylene-propylene copolymer (A) in the resin composition is preferably 1 to 90% by weight (however, when components other than the linear low-density polyethylene resin (a) and the branched low-density polyethylene resin (b) are contained, the total weight percentage of each component does not exceed 100% by weight). More preferably, it is 20 to 80% by weight. If it exceeds 80% by weight, there is a concern that processability may decrease, and if it is less than 20% by weight, sufficient adhesive strength is not exhibited.

[0050] 2.3 Branched low-density polyethylene resin (b) The branched low-density polyethylene resin (b) can be obtained by high-pressure radical polymerization of ethylene, and is also called high-pressure radical polymerization low-density polyethylene (HPLD). The molecular structure of HPLD is highly branched, and the melt elasticity is high, and it is often used to improve neck-in, especially during extrusion lamination. The physical properties of HPLD are not particularly specified, but the MFR is 1 to 100 g / 10 min, and the density is 0.915 to 0.925 g / cm. 3 Preferably, the above ranges of MFR and density improve the balance between neck-in and extensibility during processing. The amount of HPLD added in the ethylene-α-olefin copolymer composition is preferably 5 to 30% by weight. If the amount of HPLD added is greater than this, low-temperature sealability and hot tackiness are likely to deteriorate.

[0051] (b-1) MFR (190℃, 21.18N load) is 1-100g / 10min The melt flow rate (MFR) of the branched (high pressure radical polymerization method) low density polyethylene (b) used in the present invention is 1 to 100 g / 10 min, preferably 1 to 50 g / 10 min, and more preferably 1 to 30 g / 10 min. If the MFR is less than 1 g / 10 min, the extensibility is insufficient and film breakage occurs during high speed molding. On the other hand, if the MFR exceeds 100 g / 10 min, the molten film becomes unstable. Here, the MFR is a value measured in accordance with JIS-K7210 (190° C., 21.18 N load).

[0052] (b-2) Density The density of the branched low density polyethylene (b) used in the present invention is 0.915 to 0.925 g / cm 3 and preferably 0.916 to 0.925 g / cm 3 and more preferably 0.917 to 0.925 g / cm 3 It is. Here, the density is measured (23° C.) in accordance with JIS-K6922-2:1997 Appendix (for low-density polyethylene).

[0053] The branched low-density polyethylene (b) used in the present invention is generally produced using a tank reactor or a tubular reactor in the presence of a radical generator at a polymerization pressure of 1000 to 3000 kg / cm. 2 It is carried out by polymerizing ethylene at a polymerization temperature of 150 to 300° C. The melt flow rate can be adjusted by using hydrogen or hydrocarbons such as methane and ethane as molecular weight regulators.

[0054] (3) Composition ratio of component (a) and component (b) In the resin composition for low-temperature extrusion lamination used in the present invention, the branched low-density polyethylene resin (b) is contained in an amount of 1 to 85% by weight. More specifically, the ratio of the linear low-density polyethylene resin (a) to the branched low-density polyethylene resin (b) is (a):(b) 15 to 99% by weight: 1 to 85% by weight, preferably 20 to 95% by weight: 5 to 80% by weight, more preferably 30 to 95% by weight: 5 to 70% by weight, and even more preferably 40 to 95% by weight: 5 to 60% by weight. If the linear low-density polyethylene resin (a) is too much, the stability of the molten film is poor, and if the branched low-density polyethylene resin (b) is too much, the adhesive strength is reduced.

[0055] 3.Low temperature extrusion lamination method The method for producing the laminate is not particularly limited, but one of the features of the laminate is to use a so-called extrusion lamination method in which a polyethylene resin composition is melt-extruded and laminated on at least a base layer. The extrusion laminate layer is preferably laminated in one or more layers by a method such as a single layer, sandwich lamination, coextrusion lamination, or tandem lamination. In addition, the method for ensuring the adhesion with the substrate layer is not particularly limited, but for example, the substrate may be subjected to a surface treatment. Examples of the surface treatment method include various treatment methods such as corona discharge treatment, ozone treatment, frame treatment, and low-temperature plasma treatment. Another example is a method of spraying ozone onto a molten resin. In addition, when another substrate layer is provided, it is preferable to perform an anchor coat treatment as necessary.

[0056] By performing extrusion lamination at a temperature lower than that in conventional extrusion lamination, specifically at a low temperature where the resin temperature in the die lip is 220° C. to 280° C., sufficient laminate strength can be ensured while suppressing heater power consumption in the manufacturing process. Furthermore, even when a polyethylene resin substrate is used as the substrate, a laminate having sufficient laminate strength to the substrate can be obtained.

[0057] 4. Mono-material packaging materials Another embodiment of the present invention is a mono-material packaging material using the laminate of the present invention. Another embodiment of the present invention is a mono-material packaging material using the laminate of the present invention, in which a polyolefin film (IV) is laminated adjacent to the polyethylene layer (III) on the side opposite the adhesive layer (II). Hereinafter, these will be collectively referred to as the mono-material packaging material of the present invention.

[0058] Applications of the monomaterial packaging material of the present invention include packaging bags for food, medicines, medical instruments, industrial parts, miscellaneous goods, magazines, etc. EXAMPLES

[0059] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The measurement methods, evaluation methods, and resin materials used in the examples and comparative examples are as follows.

[0060] [Measurement method] MFR: Performed in accordance with JIS K6922-2 (190°C, 21.18N load). Density: Measured in accordance with JIS K6922-2 (23°C). Amount of comonomer, number of branches and number of double bonds due to comonomer: The amount of comonomer and the number of branches due to the comonomer (Y) are 13 By C-NMR, the number of double bonds (vinyl, vinylidene) is 1Measurements were performed by 1 H-NMR under the following conditions, and the number was calculated per 1,000 carbon atoms in total in the main chain and side chains. Equipment: Bruker Biospin AVANCE III cryo-400MHz Solvent: o-dichlorobenzene / bromobenzene = 8 / 2 mixed solution <Sample amount> Sample 460mg / solvent 2.3ml < 13 C-NMR · 1 H decoupling, NOE available Number of scans: 256 Flip angle: 90° · Pulse interval 20 seconds · AQ (acquisition time) = 5.45s D1 (waiting time) = 14.55s < 1 H-NMR> - Number of scans: 1400 Flip angle: 1.03° AQ (acquisition time) = 1.8s D1 (waiting time) = 0.01s Adhesive strength: The obtained laminate was cut into strips 15 mm wide in the machine direction, and peeled at the interface between the base layer (I) and the polyethylene layer (III). The adhesive strength was determined as the peel strength in a T-peel test using 5 specimens at a peel speed of 300 mm / min. Remix film haze: [Press molding] The resulting laminate was press molded as follows, and then cut into small pellet-shaped sample pieces.

[0061] Press molding machine: 100t press Press temperature: 180℃ Cooling temperature: 30℃ Pressing time: Preheat 2 min, pressurize 2 min, cool 3 min Spacer: 20cm long x 20cm wide x 1mm thick [Re-kneading] The pellet-shaped sample pieces obtained by the above-mentioned method were re-kneaded as follows to obtain a film.

[0062] Mixing equipment: Small mixer Xplore MC15 (manufactured by DSM) Set temperature: 200℃ Screw rotation speed: 50 rpm Mixing time: 1 min [Film molding] A T-die unit was attached to the barrel outlet of the above kneading device, and after kneading for a predetermined time, a T-die film was obtained under the following conditions.

[0063] Set temperature: 200℃ Screw rotation speed: 10 rpm Chill roll speed: 1m / min Film thickness: 50μm [Haze measurement] The T-die film obtained by the above method was subjected to JIS K7136 (Method A).

[0064] Measuring equipment: Haze meter HM-150 (manufactured by Murakami Color Research Institute)

[0065] [material] Base material layer (I) Toyobo Ester Film T4102 (thickness 12μm) manufactured by Toyobo Co., Ltd. Mitsui Chemicals Tocello L-Smart C-1 (30μm) Adhesive layer (II) Mitsui Chemicals Takelac A-3210, Takenate A-3075 (Polyurethane adhesive) Unitika Arrow Base SB-5230N (Modified polyolefin resin emulsion) Polyethylene layer (III)

[0066] Linear low-density polyethylene resin (hereinafter referred to as LLDPE) (a) LLDPE (a-1): Ethylene-1-hexene copolymer (metallocene-based linear low-density polyethylene, MFR 16 g / 10 min, density 0.919 g / cm 3 ) LLDPE (a-2): Ethylene-1-hexene copolymer (metallocene-based linear low-density polyethylene, MFR 16 g / 10 min, density 0.898 g / cm 3 ) LLDPE (a-3): Ethylene-propylene-1-hexene copolymer (metallocene-based linear low-density polyethylene, MFR 30 g / 10 min, density 0.880 g / cm 3 ) LLDPE (a-4): Ethylene-propylene copolymer (metallocene-based linear low-density polyethylene, MFR 20 g / 10 min, density 0.887 g / cm 3 ) LLDPE (a-5): Ethylene-propylene copolymer (metallocene-based linear low-density polyethylene, MFR 11g / 10min, density 0.913g / cm 3 )

[0067] Branched low-density polyethylene resin (hereinafter referred to as LDPE) (b) LDPE (b-1): Branched low-density polyethylene (MFR 20 g / 10 min, density 0.917 g / cm 3 ) LDPE (b-2): Branched low-density polyethylene (MFR 4g / 10min, density 0.918g / cm 3 )

[0068] [Table 1]

[0069] 4. Polyolefin film (IV) Futamura Chemical LL-XMTN (30μm)

[0070] [Example 1] [Resin composition: PE1] As LLDPE, (a-2): 80 wt% and as LDPE, (b-2): 20 wt% were used. These resins were thoroughly blended in a blender, melt-extruded and pelletized to obtain a resin composition (PE1). [Preparation of laminate film for evaluation] Using an extrusion laminating device, a 500 mm wide, 12 μm thick ester film T4102 was used as the base layer (I), and a solution of Arrowbase SB-5230N and methanol diluted in a weight ratio of 1:2.3 was applied on top of it with a Bowes roll as the adhesive layer (II), and the resulting mixture was passed through a drying oven at 100°C. Ozone was applied to the laminating section at a rate of 1.5 NL / min (concentration 15 g / m 3 ), the resin composition PE1 was melt extrusion laminated at a take-up speed of 100 m / min and a coating thickness of 30 μm to form a polyethylene layer (III). The extrusion lamination device was set so that the temperature of the resin extruded from a T-die attached to an extruder with a diameter of 90 mm was 250 ° C., and the extrusion amount was adjusted so that the coating thickness was 30 μm when the take-up speed was 100 m / min with a cooling roll surface temperature of 20 ° C., a die width of 560 mm, and a die lip opening of 0.7 mm. The extrusion lamination was carried out without any particular problems. The evaluation results of the obtained laminate film are shown in Table 2.

[0071] [Examples 2, 5 to 9] Except for using the resin compositions (PE2 to PE7) obtained by the following method for the polyethylene layer (III), evaluation films were produced in the same manner as in Example 1. All of them could be extrusion laminated without any particular problems. The evaluation results of the obtained laminate films are shown in Table 2.

[0072] [Resin composition: PE2] As the LLDPE, (a-3): 80 wt% and as the LDPE, (b-2): 20 wt% were used. These resins were thoroughly blended in a blender, melt-extruded and pelletized to obtain a resin composition (PE2). [Resin composition: PE3] As the LLDPE, (a-4): 80 wt% and as the LDPE, (b-2): 20 wt% were used. These resins were thoroughly blended in a blender, melt-extruded and pelletized to obtain a resin composition (PE3). [Resin composition: PE4] As the LLDPE, (a-5): 80 wt% and as the LDPE, (b-2): 20 wt% were used. These resins were thoroughly blended in a blender, melt-extruded and pelletized to obtain a resin composition (PE4). [Resin composition: PE5] The LLDPE used was (a-2): 20 wt%, (a-4): 60 wt%, and the LDPE used was (b-2): 20 wt%. These resins were thoroughly blended in a blender, melt-extruded, and pelletized to obtain a resin composition (PE5). [Resin composition: PE6] As LLDPE, (a-2): 30 wt% and (a-4): 50 wt% were used, and as LDPE, (b-2): 20 wt% were used. These resins were thoroughly blended in a blender, melt-extruded and pelletized to obtain a resin composition (PE6). [Resin composition: PE7] The LLDPE used was (a-2): 40 wt%, (a-4): 40 wt%, and the LDPE used was (b-2): 20 wt%. These resins were thoroughly blended in a blender, melt-extruded, and pelletized to obtain a resin composition (PE7).

[0073] [Example 3] The resin composition (PE3) obtained by the above method was used for the polyethylene layer (III). [Preparation of laminate film for evaluation] Using an extrusion laminating device, a 500 mm wide, 30 μm thick L-Smart C-1 was used as the base layer (I), and a solution of Takelac A3210, Takenate A3075, and NC401 solvent diluted in a weight ratio of 3:1:28 was applied on top of it with a Bowes roll as the adhesive layer (II), and the mixture was passed through a drying oven at 80°C. Ozone was applied to the laminating section at a rate of 1.5 NL / min (concentration 15 g / m 3), the resin composition PE3 was melt extrusion laminated at a take-up speed of 100 m / min and a coating thickness of 30 μm, and a 30 μm LL-XMTN film was sandwich laminated to laminate the polyethylene layer (III) and the polyolefin film (IV). The extrusion lamination device was set so that the temperature of the resin extruded from the T-die attached to the extruder with a diameter of 90 mmΦ was 250 ° C., and the extrusion amount was adjusted so that the coating thickness was 30 μm when the take-up processing speed was 100 m / min with a cooling roll surface temperature of 20 ° C., a die width of 560 mm, and a die lip opening of 0.7 mm. The extrusion lamination was able to be processed without any particular problems. The evaluation results of the obtained laminate film are shown in Table 2.

[0074] [Example 4] A laminate film was obtained in the same manner as in Example 1, except that the resin composition (PE4) obtained by the above method was used for the polyethylene layer (III) and a 30 μm LL-XMTN film was sandwich-laminated. The extrusion lamination process was performed without any particular problems. The evaluation results of the obtained laminate film are shown in Table 2.

[0075] [Example 10] A laminate film was obtained in the same manner as in Example 3, except that a solution of Arrowbase SB-5230N and methanol diluted in a weight ratio of 1:2.3 was used for the adhesive layer (II) and the drying oven was set to 100°C. The extrusion lamination process was performed without any particular problems. The evaluation results of the obtained laminate film are shown in Table 2.

[0076] [Comparative Example 1] [Resin composition: PE8] As the LDPE, (b-1) was used alone. [Preparation of laminate film for evaluation] Using an extrusion laminating device, a 500 mm wide, 12 μm thick ester film T4102 was used as the base layer (I), and a solution of Arrowbase SB-5230N and methanol diluted in a weight ratio of 1:2.3 was applied on top of it with a Bowes roll as the adhesive layer (II), and the resulting mixture was passed through a drying oven at 100°C. Ozone was applied to the laminating section at a rate of 1.5 NL / min (concentration 15 g / m3 ), the resin composition PE8 was melt extrusion laminated at a take-up speed of 100 m / min and a coating thickness of 30 μm to form a polyethylene layer (III). The extrusion lamination device was set so that the temperature of the resin extruded from a T-die attached to an extruder with a diameter of 90 mm was 250°C, and the extrusion amount was adjusted so that the coating thickness was 30 μm when the take-up speed was 100 m / min with a cooling roll surface temperature of 20°C, a die width of 560 mm, and a die lip opening of 0.7 mm. The extrusion lamination was carried out without any particular problems. The evaluation results of the obtained laminate film are shown in Table 2.

[0077] [Comparative Example 2] A laminate film was obtained in the same manner as in Comparative Example 1, except that a 30 μm LL-XMTN film was sandwich-laminated. The extrusion lamination process was carried out without any particular problems. The evaluation results of the obtained laminate film are shown in Table 2.

[0078] [Comparative Example 3] [Resin composition: PE9] As LLDPE, (a-1): 80 wt% and as LDPE, (b-2): 20 wt% were used. These resins were thoroughly blended in a blender, melt-extruded and pelletized to obtain a resin composition (PE9). [Preparation of laminate film for evaluation] A laminate film was obtained in the same manner as in Comparative Example 1, except that the resin composition (PE9) obtained by the above method was used for the polyethylene layer (III). The extrusion lamination process was carried out without any particular problems. The evaluation results of the obtained laminate film are shown in Table 2.

[0079] [Comparative Example 4] A laminate film was obtained in the same manner as in Comparative Example 1, except that the resin composition (PE9) obtained by the above method was used for the polyethylene layer (III) and a 30 μm LL-XMTN film was sandwich-laminated. The extrusion lamination process was performed without any particular problems. The evaluation results of the obtained laminate film are shown in Table 2.

[0080] [Comparative Example 5] A laminate film was obtained in the same manner as in Comparative Example 1, except that the resin composition (PE9) obtained by the above method was used for the polyethylene layer (III), 30 μm of L-Smart C-1 was used for the base layer (I), and a 30 μm LL-XMTN film was sandwich laminated. The extrusion lamination process was performed without any particular problems. The evaluation results of the obtained laminate film are shown in Table 2.

[0081] [Table 2] (Evaluation Results)

[0082] In Comparative Examples 1 to 5, sufficient adhesive strength of 1 N / 15 mm or less was not obtained for both PET and oriented polyethylene substrates in lamination at 250° C. On the other hand, in Examples 1 to 10, high adhesive strength was obtained for both PET and oriented polyethylene substrates in lamination at 250° C. Furthermore, when focusing on the influence of the presence or absence of the polyolefin film (IV) on the adhesive strength due to sandwich lamination, the effect is limited when comparing Comparative Examples 1 and 2, and Comparative Examples 3 and 4. On the other hand, when comparing Examples 4 and 5, it can be confirmed that the adhesive strength is significantly improved when the polyolefin film (IV) is sandwich laminated. This is thought to be due to the fact that the polyethylene layer (III) is kept warm by interposing the polyolefin film (IV) between the polyethylene layer (III) and the cooling roll in the laminated portion, and the cooling and solidifying speed is reduced, thereby lengthening the contact time with the adhesive layer (II) in the molten state, thereby contributing to the improvement of the interfacial interaction. As can be seen from the Examples and Comparative Examples, when the resin composition of the polyethylene layer (III) is composed solely of a branched low-density polyethylene resin, or when the resin composition is composed of a polyethylene layer having a density of 0.918 g / cm 3 When the resin composition is composed of a mixture of the above-mentioned linear low density polyethylene resin and branched low density polyethylene resin, this specific effect is not manifested, and therefore this is considered to be a characteristic performance of the resin composition obtained by the present invention. Furthermore, when comparing Example 3 and Example 10, the haze of the remixed film was lower when a polyolefin-based adhesive was used, so it is believed that a polyolefin-based adhesive is suitable for mono-material packaging materials that are intended for material recycling.

Claims

1. A method for producing a laminate obtained by extrusion lamination, comprising: at least a base material layer (I) / an adhesive layer (II) / a polyethylene layer (III) laminated adjacent to each other in this order; a resin temperature in a die lip during lamination of the polyethylene layer (III) is 220°C to 280°C; the polyethylene layer (III) comprises at least a linear low-density polyethylene resin (a) satisfying the following (a-1) to (a-2) and a branched low-density polyethylene resin (b) satisfying the following (b-1) to (b-2); and the polyethylene layer (III) comprises a resin composition in which the branched low-density polyethylene resin (b) accounts for 1 to 85% by weight. Linear low-density polyethylene resin (a) (a-1) MFR (190°C, 21.18N load) is 1 to 100g / 10min (a-2) Density is 0.918 g / cm 3 less than Branched low-density polyethylene resin (b) (b-1) MFR (190°C, 21.18N load) is 1 to 100g / 10min (b-2) Density is 0.915 to 0.925 g / cm 3

2. The method for producing a laminate according to claim 1, wherein the linear low-density polyethylene resin (a) further satisfies the following (a-3) to (a-4): (a-3) Contains 80 to 98 mol % of structural units derived from ethylene as a main component, 2 to 20 mol % of structural units derived from propylene as an essential minor component, and may contain 4 mol % or less of structural units derived from a third α-olefin other than ethylene and propylene as a minor component (however, when containing structural units derived from the third α-olefin, the total of the structural units derived from ethylene, the structural units derived from propylene, and the structural units derived from the third α-olefin does not exceed 100 mol %). (a-4) The total amount of vinyl and vinylidene in the ethylene copolymer is 0.35 (pieces / total 1000C) or more (Note that the number of vinyl and vinylidene groups is the number per 1,000 carbon atoms in total in the main chain and side chains as measured by NMR.)

3. 3. The method for producing a laminate according to claim 1, wherein the substrate layer (I) is a stretched substrate made of a polyethylene resin, and the adhesive layer (II) is made of a polyolefin adhesive.

4. The resin composition is for low-temperature extrusion lamination, in which extrusion lamination is performed at a low temperature in which the resin temperature in the die lip is 220°C to 280°C, and is characterized in that the resin composition contains at least a linear low-density polyethylene resin (a) that satisfies the following (a-1) to (a-2) and a branched low-density polyethylene resin (b) that satisfies the following (b-1) to (b-2), and the branched low-density polyethylene resin (b) is contained in an amount of 1 to 85% by weight. Linear low-density polyethylene resin (a) (a-1) MFR (190°C, 21.18N load) is 1 to 100g / 10min (a-2) Density is 0.918 g / cm 3 less than Branched low-density polyethylene resin (b) (b-1) MFR (190°C, 21.18N load) is 1 to 100g / 10min (b-2) Density is 0.915 to 0.925 g / cm 3

5. The resin composition for low-temperature extrusion lamination according to claim 4, wherein the linear low-density polyethylene resin (a) further satisfies the following (a-3) to (a-4). (a-3) Contains 80 to 98 mol % of structural units derived from ethylene as a main component, 2 to 20 mol % of structural units derived from propylene as an essential minor component, and may contain 4 mol % or less of structural units derived from a third α-olefin other than ethylene and propylene as a minor component (however, when containing structural units derived from the third α-olefin, the total of the structural units derived from ethylene, the structural units derived from propylene, and the structural units derived from the third α-olefin does not exceed 100 mol %). (a-4) The total amount of vinyl and vinylidene in the ethylene copolymer is 0.35 (pieces / total 1000C) or more (Note that the number of vinyl and vinylidene groups is the number per 1,000 carbon atoms in total in the main chain and side chains as measured by NMR.)

6. A method for producing an extrusion laminate, comprising: at least a base material layer (I) / an adhesive layer (II) / a polyethylene layer (III) laminated adjacent to each other in this order; the polyethylene layer (III) is made of the resin composition according to claim 4 or 5; and the resin temperature during extrusion lamination of the polyethylene layer (III) is low, at 220°C to 280°C, in a die lip.

7. A laminate comprising at least a base material layer (I) / an adhesive layer (II) / a polyethylene layer (III) laminated adjacent to each other in this order, the base material layer (I) being made of a polyethylene-based film, the adhesive layer (II) being made of a polyolefin-based adhesive, the polyethylene layer (III) containing at least a linear low-density polyethylene-based resin (a) satisfying the following (a-1) to (a-2) and a branched low-density polyethylene-based resin (b) satisfying the following (b-1) to (b-2), and the branched low-density polyethylene-based resin (b) being contained in an amount of 1 to 85% by weight. Linear low-density polyethylene resin (a) (a-1) MFR (190°C, 21.18N load) is 1 to 100g / 10min (a-2) Density is 0.918 g / cm 3 less than Branched low-density polyethylene resin (b) (b-1) MFR (190°C, 21.18N load) is 1 to 100g / 10min (b-2) Density is 0.915 to 0.925 g / cm 3

8. The laminate according to claim 7, wherein the linear low-density polyethylene resin (a) further satisfies the following (a-3) to (a-4): (a-3) Contains 80 to 98 mol % of structural units derived from ethylene as a main component, 2 to 20 mol % of structural units derived from propylene as an essential minor component, and may contain 4 mol % or less of structural units derived from a third α-olefin other than ethylene and propylene as a minor component (however, when containing structural units derived from the third α-olefin, the total of the structural units derived from ethylene, the structural units derived from propylene, and the structural units derived from the third α-olefin does not exceed 100 mol %). (a-4) The total amount of vinyl and vinylidene in the ethylene copolymer is 0.35 (pieces / total 1000C) or more (Note that the number of vinyl and vinylidene groups is the number per 1,000 carbon atoms in total in the main chain and side chains as measured by NMR.)

9. 9. The laminate according to claim 7 or 8, wherein a polyolefin film (IV) is laminated adjacent to the polyethylene layer (III) on the side opposite to the adhesive layer (II).

10. A mono-material packaging material using the laminate according to claim 7 or 8.

11. A mono-material packaging material using the laminate according to claim 9.

Citation Information

Patent Citations

  • Film for print laminate

    JP2003062957A

  • Packaging material and liquid packaging bag using the same

    JP2012081615A

  • Multilayer films and laminates containing slip agents

    JP2020529337A

  • Multilayer Films and Laminates Containing Slip Agents

    US20210187812A1

  • Multilayer sealant film

    WO2015166848A1