Laminate

A laminate with a specific ethylene-propylene copolymer, ethylene-α-olefin copolymer, and high-pressure radical polymerized low-density polyethylene composition addresses the issues of poor punching and tearability in paper packaging, offering excellent low-temperature sealing and easy tearability for improved handling and protection.

JP2024146309APending Publication Date: 2024-10-15JAPAN POLYETHYLENE CORP

Patent Information

Application Number
JP2023059121
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Conventional laminates using polyethylene resins for paper packaging face issues with poor punching properties, stretching of the resin layer during punching, poor tearability, and inadequate balance between heat seal strength and tearing, especially in applications requiring easy opening and straw penetration.

Method used

A laminate composed of a specific ethylene-propylene copolymer, ethylene-α-olefin copolymer, and high-pressure radical polymerized low-density polyethylene, optimized for low-temperature heat-sealing, pinhole resistance, and easy tearability, using a combination of ethylene-propylene copolymer (A), ethylene-α-olefin copolymer (B), and high-pressure radical polymerized low-density polyethylene (C), with specific properties and ratios to enhance adhesion and tearability.

Benefits of technology

The laminate achieves excellent low-temperature heat-sealing properties, pinhole resistance, and easy tearability, providing both content protection and ease of handling, suitable for packaging applications such as easily tearable packaging bags and liquid paper containers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146309000001
    Figure 2024146309000001
Patent Text Reader

Abstract

To provide an ethylene resin composition fo lamination that is excellent in adhesiveness to a paper base material or a barrier paper base material and also excellent in easy tearability, pinhole resistance and low temperature sealability, and also to provide a laminate.SOLUTION: A laminate includes: a layer including an ethylene resin composition for lamination (D) having the characteristics of (d-1)-(d-6) and including 5-90 wt.% of an ethylene propylene copolymer having the characteristics of (a-1)-(a-3), (B) 1-50 wt.% of an ethylene-α olefin copolymer including a C6 or more essential component having the characteristics of (b-1)-(b-3) and (C) 5-90 wt.% of a low density polyethylene having the characteristics of (c-1)-(c-2) and obtained by the high-pressure radical polymerization method; and a base material layer (E).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate containing an ethylene resin composition for lamination, and more particularly to a laminate containing a polyethylene resin composition for lamination to be laminated to paper and barrier paper base materials, which laminate has good adhesion to base materials, and further has excellent tearability, pinhole resistance and low-temperature sealability. [Background technology]

[0002] In recent years, efforts to address environmental issues have been expanding worldwide, and in particular efforts to reduce the volume of plastic packaging and containers used for food, beverages, seasonings, medicines, etc. are being promoted. As one of the efforts to reduce the amount of plastic used, the use of paper has been considered as a packaging and container that is a burnable material and has low combustion calories when incinerated. Since paper itself does not have a sealing property and it is difficult to use paper alone as a packaging material, generally, a paper-plastic laminate material that has been given sealing properties is used. From the viewpoints of protecting the contents and convenience during use, it is desired that these packaging and containers have excellent pinhole resistance and are easy to open. Conventional laminates used in packaging and containers are made by laminating polyethylene resins such as high-pressure low-density polyethylene (LDPE) and ethylene-vinyl acetate copolymer (EVA) onto base materials such as paper, biaxially oriented polyamide, polyester, polypropylene, etc., as heat-sealable layer resins, in order to impart the necessary properties to containers, such as heat-sealability and moisture resistance. In recent years, the use of linear low-density polyethylene (LLDPE), in particular LLDPE polymerized with a metallocene catalyst, has been proposed to improve the heat seal strength, low-temperature heat sealability, hot tack property, impact resistance, pinhole resistance, etc. of these laminates.

[0003] LLDPE polymerized with metallocene catalysts can be heat sealed at low temperatures and has the characteristics of high seal strength and high hot tack strength, and has been widely used as a sealant for flexible packaging, liquid paper containers, etc. However, in applications that involve a punching process such as paper cups and paper containers, there are problems such as poor punchability, which makes it difficult to punch through, and poor appearance due to the stretching of the resin layer. In addition, in paper bundling and easy-tear packaging applications, there are problems such as poor tearability, which requires force to open, and the stretching of the resin layer. Furthermore, in containers with straw holes such as liquid paper containers, there are problems such as poor penetration of the straw. Many attempts have been made to solve this problem. For example, a laminate of LLDPE polymerized with a metallocene catalyst and LLDPE polymerized with a Ziegler catalyst has been proposed (see, for example, Patent Document 1). However, although the tearability of this laminate is somewhat improved by the LLDPE polymerized with a Ziegler catalyst, the elongation of the LLDPE layer polymerized with a metallocene catalyst remains unsolved, and this method is not desirable. Furthermore, an invention has been disclosed in which LDPE having a specific swell ratio is blended with LLDPE polymerized with a metallocene catalyst (see, for example, Patent Document 2), but the balance between heat seal strength and tear resistance is not satisfactory.Another invention has been disclosed in which an ethylene terpolymer essentially consisting of ethylene, propylene, and 1-hexene or 1-octene is blended with LDPE (see Patent Document 3), but there has been no disclosure of a product that is excellent in both tearability and pinhole resistance. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 10-24539 [Patent Document 2] JP 2000-212339 A [Patent Document 3] JP 2006-82547 A Summary of the Invention [Problem to be solved by the invention]

[0005] In view of the above problems, an object of the present invention is to provide a laminate that has good adhesion to a paper substrate or a barrier paper substrate, and also has excellent tearability, pinhole resistance, and low-temperature sealability. [Means for solving the problem]

[0006] As a result of intensive investigations aimed at solving the above-mentioned problems, the present inventors have found that a laminate having a base layer and a layer of a polyethylene resin composition containing a specific ethylene-propylene copolymer, a specific ethylene-α-olefin copolymer as an essential component, and a specific low-density polyethylene produced by high-pressure radical polymerization, has excellent low-temperature heat sealability, pinhole resistance, and tearability, and thus provides a laminate which exhibits excellent content protection performance and ease of handling while achieving all of these properties, thereby completing the present invention.

[0007] That is, the first aspect of the present invention relates to a laminate having a layer containing a polyethylene resin composition for lamination (D) having the following characteristics (d-1) to (d-6), and a base layer (E), which contains (A) 5 to 90% by weight of an ethylene-propylene copolymer having the following characteristics (a-1) to (a-3), (B) 1 to 50% by weight of an ethylene-α-olefin copolymer containing an essential component of C6 or higher having the following characteristics (b-1) to (b-3), and (C) 5 to 90% by weight of a low-density polyethylene obtained by a high-pressure radical polymerization method having the following characteristics (c-1) to (c-2): (a-1) Melt flow rate: 1 to 50 g / 10 min (a-2) Density is 0.870 to 0.920 g / cm 3 (a-3) Propylene molar fraction is 5-20 mol% (b-1) Melt flow rate is 0.1 to 100g / 10min (b-2) Density is 0.880 to 0.930 g / cm 3 (b-3) The molar fraction of C6 or higher α-olefins is 1 to 10 mol% (c-1) Melt flow rate is 0.1 to 20g / 10min (c-2) Density is 0.915 to 0.930 g / cm 3 (d-1) Contains 95-98 mol% of ethylene-derived structural units as the main component, 1-5 mol% of propylene-derived structural units as the minor component, and 0.05-0.90 mol% of C6 or higher ethylene-α-olefin-derived structural units other than ethylene and propylene as essential minor components (however, the total content of ethylene-derived structural units, propylene-derived structural units, and ethylene-α-olefin-derived structural units does not exceed 100 mol%). (d-2) Melt flow rate: 1 to 100 g / 10 min (d-3) Density is 0.880 to 0.930 g / cm 3 (d-4) The ratio of the mole fraction of propylene (Mp) to the mole fraction of C6 or higher ethylene-α olefins (Mh) is 5 to 100 (d-5) The density relationship between an ethylene-propylene copolymer (A) and an ethylene-α-olefin copolymer (B) containing an essential component of C6 or higher satisfies the following equation. ·Density of ethylene-propylene copolymer (A) ···ρ(a) ·Density of ethylene-α-olefin copolymer (B) containing essential components of C6 or higher···ρ(b) ρ(a)<ρ(b) Relational expression (3)

[0008] The second invention relates to the laminate of the first invention, characterized in that the ethylene-propylene copolymer (A) in the layer of the polyethylene resin composition for lamination (D) satisfies the following properties (a-4) to (a-5): (a-4) The total amount of vinyl and vinylidene is 0.35 (pieces / total 1000C) or more. (Note that the number of vinyl and vinylidene units is per 1,000 carbon atoms in total in the main chain and side chains as measured by NMR.) (a-5) The number of branches (Y) and density (X) due to comonomers in an ethylene-propylene copolymer satisfy formula (1). (Note that the number of branches is the number per 1,000 carbon atoms in the main chain and side chains measured by NMR.) (Y)≧-1157×(X)+1080 (Equation 1)

[0009] According to a third aspect of the present invention, there is provided a laminate according to the first or second aspect of the present invention, characterized in that the base layer (E) is a paper base.

[0010] The fourth invention relates to a laminate according to the first or second invention, characterized in that the ethylene-propylene copolymer (A) in the layer of the polyethylene resin composition for lamination (D) further satisfies the following property (a-6): (a-6) The number of branches (Y) and density (X) due to comonomers in an ethylene-propylene copolymer satisfy formula (2). (Note that the number of branches is the number per 1,000 carbon atoms in the main chain and side chains measured by NMR.) (Y)≧-1157×(X)+1084 (Equation 2)

[0011] A fifth invention relates to a laminate according to the first or second invention, characterized in that the substrate layer (E) is a barrier paper substrate.

[0012] A sixth invention resides in a laminate having at least a substrate layer (E) and a layer (F) containing the ethylene resin composition for lamination (D) according to either the first or second invention.

[0013] A seventh aspect of the present invention is the laminate according to the sixth aspect of the present invention, characterized in that the laminate is formed by an extrusion coating method. Effect of the Invention

[0014] A laminate containing the laminating resin composition of the present invention has excellent low-temperature heat sealability, pinhole resistance, and tearability, and is a laminate that has excellent content protection performance and ease of handling while achieving both of these properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present invention relates to a laminate having a specific ethylene-propylene copolymer, a specific ethylene α-olefin copolymer as an essential component, and a layer of a polyethylene resin composition containing a specific high-pressure radical polymerization low-density polyethylene, and a substrate layer having a paper or a barrier paper substrate as a surface in contact with the layer. Each component used in the present invention and a laminate for extrusion lamination using them will be described in detail below.

[0016] 1. Polyethylene resin composition for lamination (D) (1) Ethylene-propylene copolymer (A) The ethylene-propylene copolymer (A) of the present invention is characterized in that it satisfies all of the following properties (a-1) to (a-3), and, if necessary, further has properties (a-4) and (a-5), and further properties (a-6). In addition, copolymers consisting of ethylene and propylene include so-called ethylene propylene rubber (EPM), which contains more than 20 mol% propylene and has a density of 0.870 g / cm 3 Rubber-like polymers obtained by the following solution polymerization method are used in the field of elastomers, but the ethylene-propylene copolymer (A) of the present invention is a polymer that is completely different from these ethylene-propylene rubbers in terms of density range, amount of ethylene and propylene contained, and physical properties. Further, among propylene polymers, propylene-ethylene copolymers that contain a small amount of ethylene component during the production process are also known, but these also differ greatly in terms of the propylene content, etc., and are polymers that are completely different in physical properties, etc. In addition, ethylene-α-olefin copolymers (LLDPE) with a so-called normal linear molecular structure have been developed mainly for film applications, and therefore usually contain C4 or higher α-olefins such as C4 or C6 as the main comonomer components to obtain high-strength copolymers. The copolymers made of ethylene and propylene using low-strength C3 comonomers as the main subcomponent have a density of 0.87 g / cm. 3The above copolymers have received little attention up until now. Recently, the present inventors have newly produced an ethylene-propylene copolymer using a C3 comonomer in this density range as the main subcomponent, and conducted various studies, and have found that the effects of the present invention can be obtained in a laminating resin composition using an ethylene-propylene copolymer (A) having physical properties in the new range, particularly (a-1) to (a-3).

[0017] (a-1) Melt flow rate (MFR: 190℃, 21.18N load) The melt flow rate (MFR: 190°C, 21.18N load) of the ethylene-propylene copolymer (A) used in the present invention is 1 to 50g / 10min, preferably 1 to 40g / 10min, more preferably 3 to 30g / 10min. If the MFR is less than 1g / 10min, the extensibility during molding is poor and the motor load in the extruder is high, which is not preferable. On the other hand, if the MFR exceeds 50g / 10min, the state of the molten film during molding becomes unstable, which is not preferable. To adjust the MFR of the ethylene-propylene copolymer, for example, there is a method of appropriately adjusting the polymerization temperature, the amount of comonomer, etc. Here, the MFR is a value measured in accordance with JIS-K6922-2:1997 Appendix (190°C, 21.18 N load).

[0018] (a-2) Density The density of the ethylene-propylene copolymer (A) used in the present invention is 0.870 to 0.920 g / cm 3 and preferably 0.880 to 0.919 g / cm 3 and more preferably 0.885 to 0.918 g / cm 3 The density is 0.870g / cm 3 If the density is less than 0.920 g / cm3, blocking will be poor, which is not preferable. 3If it exceeds this value, the adhesiveness will be poor, which is not desirable. To adjust the density of the polymer, for example, the comonomer content, polymerization temperature, catalyst amount, etc. can be adjusted appropriately. The density of ethylene-propylene copolymer is measured in accordance with JIS-K6922-2:1997 Appendix (for low density polyethylene) (measurement temperature 23°C).

[0019] (a-3) Monomer structure of component (A) The ethylene-propylene copolymer (A) used in the present invention has a propylene molar fraction of 5 to 20 mol %. More specifically, the ethylene-propylene copolymer (A) is an ethylene-propylene copolymer characterized by containing 80-95 mol% of ethylene-derived structural units as a main component and 5-20 mol% of propylene-derived structural units as a secondary component, and specifically, a copolymer obtained by polymerization by catalytic polymerization, which is a copolymer obtained by substantially linear random polymerization, and is a random copolymer of ethylene and propylene. Preferably, the molar fraction of ethylene-derived structural units is 82-94 mol%, the molar fraction of propylene-derived structural units is 6-18 mol%, and more preferably, the molar fraction of ethylene-derived structural units is 85-92 mol%, and the molar fraction of propylene-derived structural units is 8-15 mol%. Here, the monomer content such as the ethylene content is a value measured and calculated by 13C-NMR under the conditions described in the Examples section below. The ethylene-propylene copolymer (A) used in the present invention preferably does not contain any structural units derived from other α-olefins, particularly α-olefins having 4 to 20 carbon atoms, and any other monomer components. The ethylene-propylene copolymer (A) may be one or a combination of two or more, so long as it satisfies (a-1) to (a-3), more preferably (a-4), (a-5) and (a-6). When propylene is used as a secondary component and is an essential comonomer, and in particular when high-pressure ionic polymerization using a metallocene catalyst (described later) is used, it is possible to obtain ethylene-α-olefin copolymers with a specifically high total number of vinyl and vinylidene units. This effect is difficult to obtain when α-olefins such as 1-hexene and 1-octene are polymerized as the main comonomer components.

[0020] (a-4) Total number of vinyls and vinylidenes In copolymers obtained by copolymerizing ethylene with one or more α-olefins, even if diene monomers are not actively added, various double bonds (vinyl, vinylidene, cis-vinylene, trans-vinylene, tri-substituted olefins) may be generated due to differences in the mechanisms of the manufacturing process, and the amount and type of double bonds may also vary. It was previously known that in order to obtain good crosslinking properties as a solar cell encapsulant, the more double bonds contained in the ethylene-α-olefin copolymer, the better the crosslinking properties. However, in the field of lamination resin compositions, the differences due to the amount and type of double bonds had not been studied. In the present invention, it has been discovered that, among the various double bonds contained in an ethylene-propylene copolymer, vinyl and vinylidene are particularly important in achieving both adhesive strength and easy-tear properties, and it has also been discovered that the effects of the present invention can be achieved by producing an ethylene-propylene copolymer in which the total number of vinyl and vinylidene is greater than that of a copolymer usually obtained, and using this ethylene-propylene copolymer as an ethylene-propylene copolymer for a lamination resin composition, and has been completed. The ethylene-propylene copolymer (A) used in the present invention has a total amount of vinyl and vinylidene double bonds per 1000 carbon atoms in the main chain and side chains measured by NMR, i.e., the total number of vinyl and vinylidene double bonds, of 0.35 or more (sometimes expressed as "units / total 1000C"), preferably 0.40 to 5.0 (units / total 1000C), more preferably 0.45 to 4.5 (units / total 1000C), and even more preferably 0.50 to 4.0 (units / total 1000C). When the total number of vinyl and vinylidene is within the above range, the polyethylene resin composition for lamination has excellent adhesive strength, and when it is less than 0.35, the adhesive strength is insufficient. The total number of vinyl and vinylidene can be controlled within the above range by appropriately selecting a suitable metallocene catalyst, adjusting the polymerization temperature, and the type of comonomer. The number of these double bonds is the number per total of 1000 carbon atoms in the main chain and side chain, and is a value calculated using the integrated intensity of the characteristic peak of the 1H-NMR spectrum, and is a value measured and calculated under the conditions described in the Examples section below. The number of vinyl and vinylidene can be adjusted by the production conditions such as the type of comonomer, the amount of comonomer, and the polymerization temperature. Furthermore, in the present invention, it is preferable that the number of vinyl in the ethylene-propylene copolymer (A) satisfies the range of 0.2 (units / total 1000C) or more. In the present invention, the number of vinylidenes in the ethylene-propylene copolymer (A) preferably satisfies the range of 0.12 (units / total 1000C) or more.

[0021] (a-5) Relationship between the number of branches (Y) and density (X) due to comonomers The ethylene-propylene copolymer (A) used in the present invention preferably has a branch number (Y) due to a comonomer and a density (X) that satisfy the following formula (1). (Y)≧-1157×(X)+1080 (Equation 1) When the density and the number of branches satisfy the relationship of the above (Formula 1), the number of branches due to the comonomer is sufficiently secured, and the laminated polyethylene resin composition has excellent tearability and excellent adhesive strength. The number of branches due to the comonomer (Y) indicates the amount of tertiary carbon contained in the polymer, and is the sum of the number of methyl branches and the number of butyl branches per total of 1000 carbon atoms in the main chain and side chain, measured by 13C-NMR under the conditions described in the Examples section below. The density (X) is the density of the ethylene-propylene copolymer (A) and is measured as described above. The relationship between the density and the number of branches can be adjusted by the type and ratio of the comonomer to be copolymerized.

[0022] (a-6) Relationship between the number of branches (Y) and density (X) due to comonomers The ethylene-propylene copolymer (A) used in the present invention preferably has a comonomer branch number (Y) and density (X) that satisfy the following formula (2). (Y)≧-1157×(X)+1084 (Equation 2) The number of branches (Y) and density (X) due to the comonomer in (Formula 2) are as shown in (Formula 1). When the density and the number of branches satisfy the relationship of (Formula 2) above, the number of branches due to the monomer is sufficiently ensured, and the polyethylene resin composition for lamination has excellent tearability and adhesive strength. The relationship between the density and the number of branches can be adjusted by the type and ratio of the comonomer to be copolymerized.

[0023] Polymerization catalyst and polymerization method for component (A) The catalyst used in the production of the ethylene-propylene copolymer (A) used in the present invention is not particularly limited, but more preferably a metallocene catalyst is used. The metallocene catalyst is not particularly limited, but examples thereof include catalysts containing a metallocene compound such as a zirconium compound coordinated with a group having a cyclopentadienyl skeleton and a cocatalyst as catalytic components. In particular, it is preferable to use a metallocene compound such as a zirconium compound coordinated with a group having a cyclopentadienyl skeleton. The production method is not particularly limited, and a high-pressure ionic polymerization method, a gas phase method, a solution method, a slurry method, etc. can be used. However, in order to obtain the ethylene-propylene copolymer (A) according to the present invention having adjusted double bonds, it is desirable to carry out the polymerization at a high temperature of 150 to 330°C, and therefore it is preferable to use a high-pressure ionic polymerization method (Chapter 4 of "Polyethylene Technology Reader," edited by Kazuo Matsuura and Naotaka Mikami, 2001).

[0024] (2) Ethylene-α-olefin copolymer containing essential components of C6 or higher (B) The ethylene-α-olefin copolymer (B) of the present invention containing an essential component of C6 or higher is a random copolymer of ethylene and an α-olefin, mainly composed of structural units derived from ethylene, and is characterized by having the following properties (b-1) to (b-3):

[0025] (b-1) Melt flow rate (MFR: 190℃, 21.18N load) The melt flow rate (MFR: 190°C, 21.18N load) of the ethylene-α-olefin copolymer (B) used in the present invention is 0.1 to 100g / 10min, preferably 1 to 80g / 10min, more preferably 1 to 50g / 10min. If the MFR is less than 0.1g / 10min, the extensibility during molding is poor and the motor load in the extruder is high, which is not preferable. On the other hand, if the MFR exceeds 100g / 10min, the state of the molten film during molding becomes unstable, which is not preferable. To adjust the MFR of the ethylene-propylene copolymer, for example, there is a method of appropriately adjusting the polymerization temperature, the amount of comonomer, etc. Here, the MFR is a value measured in accordance with JIS-K6922-2:1997 Appendix (190°C, 21.18 N load).

[0026] (b-2) Density The density of the ethylene-α-olefin copolymer (B) used in the present invention is 0.880 to 0.930 g / cm 3 and preferably 0.885 to 0.920 g / cm 3 and more preferably 0.890 to 0.919 g / cm 3 The density is 0.880g / cm 3 If the density is less than 0.930 g / cm3, blocking will be poor, which is not preferred. 3 If it exceeds this value, the adhesiveness will be poor, which is not desirable. To adjust the density of the polymer, for example, the α-olefin content, polymerization temperature, catalyst amount, etc. can be adjusted appropriately. The density of ethylene-α-olefin copolymers is measured in accordance with JIS-K6922-2:1997 Appendix (for low density polyethylene) (measurement temperature 23°C).

[0027] (b-3) Monomer composition of component (B) The ethylene / α-olefin copolymer (B) used in the present invention has a molar fraction of C6 or higher α-olefins of 1 to 10 mol %. More specifically, the ethylene-α-olefin copolymer (B) is an ethylene-α-olefin random copolymer characterized by containing 90.0-99.0 mol% of ethylene-derived structural units as a main component and 1.0-10.0 mol% of α-olefin-derived structural units as a secondary component. Preferably, the ethylene-derived structural units are 90.5-98.5 mol%, the α-olefin-derived structural units are 1.5-9.5 mol%, more preferably, the ethylene-derived structural units are 91.0-98.0 mol%, and the α-olefin-derived structural units are 2.0-9.0 mol%. The α-olefin used as a comonomer is preferably an α-olefin having 6-12 carbon atoms. Specific examples include 1-hexene, 1-octene, 1-heptene, 4-methyl-pentene-1, 4-methyl-hexene-1, and 4,4-dimethylpentene-1.

[0028] Polymerization catalyst and polymerization method for component (B) The ethylene-α-olefin copolymer (B) used in the present invention can be produced using a Ziegler catalyst or a metallocene catalyst, preferably a metallocene catalyst, by a high pressure ionic polymerization method, a gas phase method, a solution method, a slurry method, etc.

[0029] The metallocene catalyst is not particularly limited, but may be any of those described in Japanese Patent Publication No. 7-508545. A catalyst similar to that described in the publication, for example, a catalyst solution prepared by adding an equimolar amount of tripentafluorophenyl boron to 2.0 mmol of the complex dimethylsilylenebis(4,5,6,7-tetrahydroindenyl)hafnium dimethyl and diluting the mixture with toluene to 10 L, can be preferably used. Commercially available products include the Harmolex series and Kernel series manufactured by Japan Polyethylene Corporation, the Evolue series manufactured by Prime Polymer Co., Ltd., and the Excellen GMH series and Excellen FX series manufactured by Sumitomo Chemical Co., Ltd.

[0030] (3) Low-density polyethylene produced by high-pressure radical polymerization (C) The low-density polyethylene (C) obtained by high-pressure radical polymerization (also referred to as high-pressure radical polymerization low-density polyethylene (C)) used in the polyethylene resin composition for lamination of the present invention is a low-density polyethylene (LDPE) obtained by high-pressure radical polymerization having the following characteristics (c-1) to (c-2), and is preferably a long-chain branched low-density polyethylene.

[0031] (c-1) Melt flow rate (MFR: 190℃, 21.18N load) The melt flow rate (MFR) of the high pressure radical polymerization low density polyethylene (C) used in the present invention is 0.1 to 20 g / 10 min, preferably 0.5 to 15 g / 10 min, and more preferably 1 to 15 g / 10 min. If the MFR is less than 0.1 g / 10 min, the extensibility is insufficient and film breakage occurs during high speed molding. On the other hand, if the MFR exceeds 20 g / 10 min, the molten film becomes unstable. Here, the MFR is a value measured in accordance with JIS-K6922-2:1997 Appendix (190°C, 21.18 N load).

[0032] (c-2) Density The density of the high-pressure radical polymerization low-density polyethylene (C) used in the present invention is 0.915 to 0.930 g / cm 3 and preferably 0.916 to 0.926 g / cm 3 and more preferably 0.917 to 0.925 g / cm 3 The density is 0.915g / cm 3 If it is less than 0.930g / cm, it will be sticky. 3 If it exceeds this value, the adhesion becomes poor. Here, the density is measured in accordance with JIS-K6922-2:1997 Appendix (for low-density polyethylene) (measurement temperature: 23° C.).

[0033] The low-density polyethylene (C) used in the present invention is generally produced by high-pressure radical polymerization using a tank reactor or a tubular reactor in the presence of a radical generator at a polymerization pressure of 1000 to 3000 kg / cm. 2It is carried out by polymerizing ethylene at a polymerization temperature of 150 to 300° C. The melt flow rate can be adjusted by using hydrogen or hydrocarbons such as methane and ethane as molecular weight regulators.

[0034] (4) Composition ratio of components (A), (B), and (C) In the case where the polyethylene resin composition for lamination (D) used in the present invention contains, in addition to the ethylene-propylene copolymer (A), an ethylene-α-olefin copolymer (B) containing an essential component of C6 or more, and further a high-pressure radical polymerization low-density polyethylene (C), the ratio of the ethylene-propylene copolymer (A), the ethylene-α-olefin copolymer (B) containing an essential component of C6 or more, and further a high-pressure radical polymerization low-density polyethylene (C) is (A):(B):(C) 5-90% by weight:1-50% by weight:5-90% by weight, preferably 5-80% by weight:1-40% by weight:10-90% by weight, more preferably 5-70% by weight:1-30% by weight:20-90% by weight. If the ethylene-propylene copolymer (A) is too much, the molten film may become unstable, and if the ethylene-α-olefin copolymer (B) containing an essential component of C6 or more is too much, the easy tearing property may decrease. Furthermore, if the amount of the high-pressure radical polymerization low-density polyethylene (C) is too large, the adhesiveness may decrease.

[0035] (5) Characteristics of Polyethylene Resin Composition for Lamination (D) (d-1) Monomer structure The lamination polyethylene resin composition (D) used in the present invention is characterized by containing 95.0 to 98.0 mol% of ethylene-derived structural units as main components, 1.0 to 5.0 mol% of propylene-derived subcomponents, and 0.05 to 0.90 mol% of α-olefin-derived structural units as subcomponents, preferably 95.0 to 97.5 mol% of ethylene-derived structural units, 1.5 to 5.0 mol% of propylene-derived subcomponents, and 0.05 to 0.80 mol% of α-olefin-derived structural units as subcomponents, more preferably 95.0 to 97.0 mol% of ethylene-derived structural units, 2.0 to 5.0 mol% of propylene-derived subcomponents, and 0.05 to 0.70 mol% of α-olefin-derived structural units as subcomponents. If the ethylene-derived main component is too high, the low-temperature heat sealability may be reduced, and if the propylene-derived subcomponents are too high, the pinhole resistance may be reduced. Furthermore, if the amount of the secondary component derived from α-olefin is too large, the ease of tearing may decrease.

[0036] (d-2) Melt flow rate (MFR: 190℃, 21.18N load) The melt flow rate (MFR: 190° C., 21.18 N load) of the polyethylene resin composition for lamination (D) used in the present invention is 1 to 100 g / 10 min, preferably 1 to 80 g / 10 min, and more preferably 2 to 70 g / 10 min. If the MFR is less than 1 g / 10 min, the extensibility during molding will be poor and the motor load in the extruder will be high, which is undesirable, whereas if the MFR exceeds 100 g / 10 min, the state of the molten film during molding will be unstable, which is undesirable. Here, the MFR is a value measured in accordance with JIS-K6922-2:1997 Appendix (190°C, 21.18 N load).

[0037] (d-3) Density The density of the polyethylene resin composition for lamination (D) used in the present invention is 0.88 to 0.93 g / cm 3 and preferably 0.885 to 0.925 g / cm 3and more preferably 0.890 to 0.920 g / cm 3 The density is 0.88g / cm 3 If the density is less than 0.93 g / cm3, blocking will be poor, which is not preferable. 3 If it exceeds this value, the adhesiveness becomes poor, which is not preferable. Here, the density is measured in accordance with JIS-K6922-2:1997 Appendix (for low density polyethylene) (measurement temperature: 23° C.).

[0038] (d-4) Ratio of the mole fraction of propylene to the mole fraction of C6 or higher ethylene-α-olefins The ratio (Mp / Mh) of the molar fraction (Mp) of propylene to the molar fraction (Mh) of ethylene-α-olefin in the polyethylene resin composition for lamination (D) used in the present invention is from 5 to 100, preferably from 5 to 60, and more preferably from 5 to 40. If Mp / Mh is less than 5.0, the ease of tearing becomes poor and the ease of opening becomes poor, which is undesirable.

[0039] (d-5) Relationship between density of ethylene-propylene copolymer (A) and ethylene-α-olefin copolymer (B) It is preferable that the densities of the ethylene-propylene copolymer (A) and the ethylene-α-olefin copolymer (B) containing an essential component of C6 or higher in the polyethylene resin composition for lamination (D) used in the present invention satisfy the following relational expression (3): ·Density of ethylene-propylene copolymer (A) ···ρ(a) ·Density of ethylene-α-olefin copolymer (B) containing essential components of C6 or higher···ρ(b) ρ(a)<ρ(b) Relational expression (3) When the densities of the ethylene-propylene copolymer (A) and the ethylene-α-olefin copolymer (B) containing an essential component of C6 or higher in the polyethylene resin composition for lamination (D) satisfy the relational expression (3), the polyethylene resin composition for lamination has excellent tearability and adhesive strength.

[0040] (6) Other ingredients The polyethylene resin composition for lamination (D) used in the present invention or a layer containing the same may contain additives, such as phenol-based or phosphorus-based antioxidants, stabilizers such as metal soaps, antiblocking agents, lubricants, dispersants, pigments such as organic or inorganic colorants, antifogging agents such as unsaturated fatty acid esters, antistatic agents, ultraviolet absorbers, light stabilizers, nucleating agents, etc., which are commonly used in polyethylene resins, as necessary. In addition, other thermoplastic resins, such as polyethylene resins such as LDPE, C4-LLDPE, HAO-LLDPE, ethylene-vinyl acetate copolymer (EVA), ethylene-acrylic acid copolymer (EAA), ethylene-methacrylic acid copolymer (EMAA), ethylene-acrylic acid ester copolymer (EEA, EMA, EMMA, etc.), high density polyethylene (HDPE), adhesive resins such as ethylene-maleic anhydride copolymers, polypropylene resins, polystyrene resins, etc. may be contained within the range that does not impair the properties of the polyethylene resin composition layer. Moreover, it is preferable that the polyethylene resin composition for lamination (D) of the present invention does not contain a crosslinking agent.

[0041] 2. Base material layer (E) The substrate layer (E) used in the present invention may be, for example, a film of polypropylene resin, nylon, polyester, polyethylene, ethylene-vinyl alcohol copolymer, or a laminated film made of the same or different materials, on the surface in contact with at least the layer (F) containing the ethylene resin composition for lamination (D). The film is preferably a stretched film. Examples of the substrate include a single-layer substrate such as paper such as kraft paper, metal foil such as aluminum or copper, a plastic film on which metal, inorganic material, or organic material is vapor-deposited, or a laminated substrate such as paper with a barrier coating. Commercially available paper substrates with a barrier coating include Shield Plus manufactured by Nippon Paper Industries Co., Ltd., Silvio Barrier manufactured by Oji F-Tex Co., Ltd., Protego manufactured by Utsu Shoji Co., Ltd., Hansol EB manufactured by Japan Pulp and Paper Co., Ltd., and Varicoat manufactured by Mitsubishi Paper Mills Co., Ltd., and examples thereof include substrates with improved barrier properties such as water vapor permeability and oxygen permeability, and improved aroma retention.

[0042] 3.Laminate The laminate of the present invention is a laminate having at least a base layer (E) and a layer (F) containing the polyethylene resin composition for lamination (D) of the present invention. The layer (F) containing the polyethylene resin composition for lamination (D) of the present invention is formed on at least one surface of the base layer (E). There are no restrictions on the structure of the laminate, but examples of the laminate include laminates having the following structures. Substrate layer (E) / layer (F) containing polyethylene resin composition for lamination (D), layer (F) containing polyethylene resin composition for lamination (D) / substrate layer (E) / layer (F) containing polyethylene resin composition for lamination (D), substrate layer (E) / layer (F) containing polyethylene resin composition for lamination (D) / substrate layer (E), substrate layer (E) / layer (F) containing polyethylene resin composition for lamination (D) / substrate layer (E), substrate layer (E) / layer (F) containing polyethylene resin composition for lamination (D) / substrate layer (E) / layer (F) containing polyethylene resin composition for lamination (D), substrate layer (E) / layer (F) containing polyethylene resin composition for lamination (D) / substrate layer (E) / layer (F) containing polyethylene resin composition for lamination (D) / substrate layer (E), other resin layer / substrate layer (E) / layer (F) containing polyethylene resin composition for lamination (D), substrate layer (E) / layer (F) containing polyethylene resin composition for lamination (D) / other resin layer Here, the other resin layer is a resin layer different from the layer (F) containing the polyethylene resin composition for lamination (D) of the present invention, and examples thereof include polyethylene resins such as LDPE, C4-LLDPE, HAO-LLDPE, ethylene-vinyl acetate copolymer (EVA), ethylene-acrylic acid copolymer (EAA), ethylene-methacrylic acid copolymer (EMAA), ethylene-acrylic acid ester copolymer (EEA, EMA, EMMA, etc.), high density polyethylene (HDPE), etc., adhesive resins such as ethylene-maleic anhydride copolymer, polypropylene resins, polystyrene resins, etc. As the other resin layer, it is preferable to use a layer containing the above-mentioned high pressure radical polymerization low density polyethylene (C). The method for producing the laminate is not particularly limited, but for example, the so-called extrusion coating method in which the polyethylene resin composition is melt-extruded and laminated on the substrate layer is preferred. The extrusion coating is preferably performed by laminating one or more layers by a method such as single layer, sandwich lamination, coextrusion lamination, or tandem lamination. The polyethylene resin composition layer can be used as an adhesive layer and also as a sealant for the surface layer. According to the present invention, high-speed molding is possible due to good adhesion to the substrate.

[0043] The method for ensuring the adhesion to the substrate layer is not particularly limited, but for example, it is preferable to subject the substrate surface to a surface treatment, and if necessary, an anchor coat treatment. Examples of the surface treatment method include various treatment methods such as a corona discharge treatment method, an ozone treatment method, a flame treatment method, and a low-temperature plasma treatment method. Another example is a method of spraying ozone onto a molten resin.

[0044] The laminate of the present invention has a layer (F) containing the above-mentioned polyethylene resin composition for lamination (D), and is a laminate that has excellent adhesive strength with substrates, etc., as well as good tearability and pinhole resistance, and is excellent in both content protection performance and ease of handling.

[0045] The laminate of the present invention has excellent adhesive strength to substrates and the like, and also has excellent ease of opening properties such as easy tearing properties, and is therefore particularly suitable for use as films for easy-tear packaging bags, food packaging films, paper containers for liquids, paper bundling, paper cups, paper trays, and the like. EXAMPLES

[0046] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. The measurement methods and resins used in the examples and comparative examples are as follows.

[0047] 1.Measurement method (1) Melt flow rate (MFR): The MFR of ethylene-propylene copolymer or ethylene-α-olefin copolymer, high-pressure radical polymerization low-density polyethylene, and polyethylene resin composition was measured in accordance with JIS-K6922-2:1997 Appendix (190°C, 21.18N load). (2) Density: The density of the ethylene-propylene copolymer or ethylene-α-olefin copolymer, the high-pressure radical polymerization low-density polyethylene, and the polyethylene resin composition was measured in accordance with JIS-K6922-2:1997 Appendix (23°C, in the case of low-density polyethylene).

[0048] (3) Monomer amount, number of branches, number of double bonds: <Sample preparation and measurement conditions> 200 mg of sample was dissolved in an NMR sample tube with an inner diameter of 10 mm together with 2.4 ml of o-dichlorobenzene / deuterated bromide benzene = 4 / 1 (volume ratio) and hexamethyldisiloxane as a chemical shift standard substance. NMR measurements were performed using a Bruker Biospin AV400M NMR instrument equipped with a 10 mm diameter cryoprobe. The 13C-NMR measurement conditions were a sample temperature of 120°C, a pulse angle of 90°, a pulse interval of 20 seconds, and an accumulation of 128 times, and the measurement was performed using the broadband decoupling method. The 1H-NMR measurement conditions were a sample temperature of 120°C, a pulse angle of 4.5°, a pulse interval of 2 seconds, and an accumulation of 512 times. <Calculation method> (i) Monomer amount and number of branches due to comonomers The amounts of propylene, hexene, and ethylene were calculated using the signal intensity of the 13C-NMR spectrum according to the following formula. C3(mol%)=I(P)×100 / [I(P)+I(H)+I(E)] C6(mol%)=I(H)×100 / [I(P)+I(H)+I(E)] C2(mol%)=I(E)×100 / [I(P)+I(H)+I(E)] Here, I(P), I(H), and I(H) are quantities expressed by the following formulas, respectively. I(P) = 0.5 × (I 37.69~37.20+I 37.90~37.69 +I 37.97~37.90 +I 43.90~42.68 ) +I 46.60~45.39 I(H) = 0.5 × (I 34.56~34.22 +I 34.94~34.86 +I 43.60~42.68 )+0.5×(I 34.86~34.70 -I 35.80~35.68 ) +I 40.10~39.96 +I 40.80~40.70 I(E)={0.5×(I 34.94~34.86 +I 37.90~37.69 I 37.97~37.90 +I 34.56~34.22 +I 37. 69~37.20 )+0.5×(I 34.86~34.70 -I 35.80~35.68 ) +I 24.90~24.70 +I 24.70~24. 52 +I 24.52~24.32 +I 27.28~26.83 +I 27.50~27.28 +I 31.50~28.50 -I(H)} / 2 I is the integrated intensity, and the subscript number of I indicates the range of chemical shifts. For example, I37.69~37.20 indicates the integrated intensity of the 13C signal detected between 37.69 ppm and 37.20 ppm. The chemical shift was set to 1.98 ppm for the 13C signal of hexamethyldisiloxane, and the chemical shifts of other 13C signals were based on this. The number of branches per 1000 carbon atoms in the main chain and side chain was calculated using the following formula: Number of methyl branches (units / total 1000C) =C3(mol%)×1000 / {C3(mol%)×3+C6(mol%)×6+C2(mol%)×2} Number of butyl branches (pcs / total 1000C) =C6(mol%)×1000 / {C3(mol%)×3+C6(mol%)×6+C2(mol%)×2}

[0049] (ii) Number of double bonds The amount of unsaturated bonds per 1,000 carbon atoms in total in the main chain and side chains was calculated from the signal intensity of the 1H-NMR spectrum according to the following formula. Number of vinylidene units (units / total 1000C) = Ivd x 1000 / Itotal Number of vinyl pieces (pieces / total 1000C) = Ivi x 1000 / Itotal Number of trisubstituted olefins (units / total 1000C) = Itri × 1000 / Itotal Number of vinylenes (pieces / total 1000C) = Ivnl x 1000 / Itotal I is the integrated intensity, and the subscripts on I indicate the range of chemical shifts. Here, Ivd, Ivi, Itri, Ivnl, and Itotal are quantities represented by the following formulas, respectively. Ivd=(I 4.88~4.44 ) / 2 Ivni=(I 5.52~5.30 ) / 2 Ivi=(I 5.05~4.88 +I 5.85~5.70 ) / 3 Itri=I 5.30~5.05 Itotal = (I 0.00~5.85 ) / 2 However, for example, I5.52-5.30 indicates the integrated intensity of the proton signal detected between 5.52 ppm and 5.30 ppm. The chemical shifts were set to 0.09 ppm based on the proton signal of hexamethyldisiloxane, and the chemical shifts of the signals due to other protons were based on this.

[0050] (4) Melt film stability: The stability of the molten film was visually observed with an extruder of 90 mmφ, a T-die of 560 mm width, a lip width of 0.8 mm, an air gap of 115 mm, a molding temperature of 325°C, and a take-off speed of 100 m / min. A case in which the molten film was stable and could be processed was marked with "○", and a case in which the molten film was unstable and could not be processed to a uniform thickness was marked with "×".

[0051] (5) Heat seal strength (N / 15mm) The polyethylene resin composition (D) was extruded from a T-die at a resin temperature of 325°C from a single-screw extrusion laminator having a screw diameter of 90 mm, and Silvio Barua UB unbleached (Oji F-Tex Co., Ltd., basis weight 65 g / m), which is a type of barrier paper base material, was extruded from the extrusion machine. 2 ) was unrolled to form the substrate, and the barrier-coated surface was corona-treated at 30 W·min / m 2 While applying pressure, extrusion lamination was carried out at a take-up speed of 100 m / min to a thickness of 30 μm, to obtain a laminate consisting of a barrier paper base layer (E) and a layer (F) containing the polyethylene resin composition for lamination (D). The obtained laminate was cut in MD to a width of 15 mm, the sealant surfaces were aligned, and the lower seal bar of a Tester Sangyo hot platen heat sealer was kept constant at 30°C, the upper seal bar was heat sealed at 90°C to 140°C in 10°C increments under the conditions of a sealing pressure of 2Mpa and a sealing time of 1 second, and seven samples were obtained for each temperature. The 180° peel strength of the heat-sealed parts of the obtained samples was measured at a tensile speed of 300mm / min using a Toyo Seiki tensile tester. A heat seal curve of heat seal temperature (°C) and strength (N) was created from the measured values, and the heat seal strength was evaluated according to the following criteria. 〇: The temperature at which the heat seal strength reaches 4N is 110℃ or less. ×: The temperature at which the heat seal strength of 4N is reached is 110°C or higher.

[0052] (6) Trouser tear strength In accordance with JIS-K7128-1, the tear load was measured in the direction perpendicular to the direction of take-up (MD) of the sample at a take-up speed of 200 mm / min, and the average tear load was calculated (unit: N). A tear load of less than 1.0 was marked as ◯, and a tear load of 1.0 or more was marked as ×. The sample used was a laminate in which a thickness of 30 μm was laminated on a barrier paper substrate as described in the examples.

[0053] (7) Pinhole resistance Using a Gelbo Flex Tester manufactured by Tester Sangyo Co., Ltd., pinholes were measured after 100 repetitions at 23°C. A laminate having a thickness of 30 μm as described in the examples laminated on a barrier paper substrate was used, and measurements were taken three times in each of the machine direction (MD) and the transverse direction (TD) of the laminate with a size of 20 cm wide x 30 cm long. After a stroke load, a reagent (a colored surfactant aqueous solution containing 1% basic dye and 1% surfactant) was applied to the sealant layer side with a brush, and the number of contaminated areas was checked based on whether the reagent penetrated, and the average value of a total of six measurements was calculated. Pinhole resistance was judged according to the following criteria. ○: Less than 26 contaminated spots ×: 26 or more contamination points

[0054] 2.Resin materials (1) Ethylene-propylene copolymer (A) and ethylene-α-olefin copolymer (B) The ethylene-propylene copolymer and ethylene-α-olefin copolymer obtained by the following manufacturing method were used as component (A), (PE-1) to (PE-3). Their physical properties are shown in Table 1.

[0055] Production method of (PE-1) to (PE-3) (i) Preparation of catalyst A catalyst solution was prepared by adding an equimolar amount of “N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate” to 0.05 moles of the complex “rac-dimethylsilylenebisindenylhafnium dimethyl” prepared by the method described in JP-A-10-218921, and diluting the mixture to 50 L with toluene.

[0056] (ii) Polymerization method A 5.0-liter stirred autoclave continuous reactor was used, and the pressure inside the reactor was kept at 80 MPa. The feed gas was continuously supplied at a rate of 40 kg / hour while appropriately adjusting the amounts of ethylene, propylene, and 1-hexene. The catalyst solution described in the above section "(i) Preparation of catalyst" was continuously supplied, and the polymerization temperature was appropriately adjusted within the range of 150 to 250°C to obtain an ethylene-α-olefin copolymer. The physical properties of the obtained ethylene-propylene copolymer and ethylene-α-olefin copolymer are shown in Table 1.

[0057] (2) Low-density polyethylene produced by high-pressure radical polymerization The low-density polyethylenes (PE-4) to (PE-8) produced by high-pressure radical polymerization and having the physical properties shown in Table 1 were used.

[0058] Example 1 The mixture consisted of 28.3% by weight of ethylene-propylene copolymer (A) (PE-1), 3.4% by weight of ethylene-α-olefin copolymer (B) (PE-2), and high-pressure low-density polyethylene (C), with a MFR of 13 g / 10 min and a density of 0.918 g / cm. 3 A polyethylene resin composition (D) consisting of 68.3% by weight of the long-chain branched low-density polyethylene (PE-4) prepared by high-pressure radical polymerization was pelletized in a 40 mm single-screw extruder to obtain pellets of the polyethylene composition. Using the pellets obtained above, a polyethylene resin composition (D) was extruded from a T-die at a resin temperature of 325°C from a single-screw extrusion laminator having a screw diameter of 90 mm, and the polyethylene resin composition (D) was fed from a feeder to Silvio Barua UB unbleached (manufactured by Oji F-Tex Co., Ltd., basis weight 65 g / m), which is a type of barrier paper base material. 2 ) was unwound and used as the substrate, and extrusion lamination was performed at a take-up speed of 100 m / min and a thickness of 30 μm while subjecting the barrier-coated surface to a corona treatment of 30 W·min / m2. The laminate consisting of the obtained barrier paper base layer (E) and the layer (F) containing the polyethylene resin composition for lamination (D) was subjected to various evaluations. The evaluation results of the laminate are shown in Table 1. The melt film stability, tearability, pinhole resistance, and low-temperature sealability were all good.

[0059] Example 2 Pellets were prepared and evaluated in the same manner as in Example 1, except that the blending ratio of the ethylene-α-olefin copolymer (B) (PE-2) was changed to 5.9% by weight and the blending ratio of the high-pressure low-density polyethylene (C) (PE-4) was changed to 65.8% by weight. The evaluation results of the laminate are shown in Table 1. The melt film stability, tearability, pinhole resistance, and low-temperature sealability were all good.

[0060] Example 3 In Example 1, the blending ratio of the ethylene-propylene copolymer (A) (PE-1) was 26.1% by weight, the blending ratio of the ethylene-α-olefin copolymer (B) (PE-2) was 5.0% by weight, the MFR was 10 g / 10 min, and the density was 0.918 g / cm 3 Pellets were prepared and evaluated in the same manner as in Example 1, except that the blending ratio of the long-chain branched low-density polyethylene (PE-5) prepared by high-pressure radical polymerization was changed to 68.9% by weight. The evaluation results of the laminate are shown in Table 1. The melt film stability, tearability, pinhole resistance, and low-temperature sealability were all good.

[0061] Comparative Example 1 In Example 1, the ethylene-α-olefin copolymer (B) was not used, and the blending ratio of the ethylene-propylene copolymer (A) (PE-1) was set to 20.0 wt%, the MFR was 8.0 g / 10 min, and the density was 0.919 g / cm 3 Pellets were prepared and evaluated in the same manner as in Example 1, except that the blending ratio of the long-chain branched low-density polyethylene (PE-6) prepared by high-pressure radical polymerization was changed to 80.0% by weight. The evaluation results of the laminate are shown in Table 1. The melt film stability, tearability, and low-temperature sealability were good, but the pinhole resistance was insufficient.

[0062] Comparative Example 2 In Example 1, the ethylene-propylene copolymer (A) and the ethylene-α-olefin copolymer (B) were not used, and the MFR was 7.0 g / 10 min and the density was 0.918 g / cm 3A laminate was evaluated using only the long-chain branched low-density polyethylene (PE-7) prepared by high-pressure radical polymerization. The evaluation results of the laminate are shown in Table 1. The melt film stability and tearability were good, but the low-temperature sealability and pinhole resistance were insufficient.

[0063] Comparative Example 3 In Example 1, the ethylene-propylene copolymer (A) and the ethylene-α-olefin copolymer (B) were not used, and the MFR was 27 g / 10 min and the density was 0.908 g / cm 3 The evaluation was carried out in the same manner as in Example 1, except that the polyethylene resin composition (D) was made into pellets of a polyethylene composition consisting of a polyethylene resin composition (D) containing 67.0% by weight of an ethylene-based terpolymer (PE-3) of ethylene, propylene and 1-hexene and 33.0% by weight of a long-chain branched low-density polyethylene (PE-8) produced by a high-pressure radical polymerization method having an MFR of 4.0 g / 10 min and a density of 0.918 g / cm3. The evaluation results of the laminate are shown in Table 1. The melt film stability, pinhole resistance and low-temperature sealability were good, but the tearability was insufficient.

[0064] [Table 1]

[0065] [Industrial Applicability] The laminate of the present invention can be used as an easy-tear packaging paper container, a barrier packaging paper container, paper bundling, paper cups, paper trays, and the like.

Claims

1. (A) 5 to 90% by weight of an ethylene-propylene copolymer having the following characteristics (a-1) to (a-3), (B) 1 to 50% by weight of an ethylene / α-olefin copolymer containing an essential component of C6 or higher and having the following characteristics (b-1) to (b-3), and (C) 5 to 90% by weight of low-density polyethylene obtained by high-pressure radical polymerization and having the following characteristics (c-1) to (c-2): A layer containing a polyethylene resin composition for lamination (D) having the following properties (d-1) to (d-6), A laminate having a substrate layer (E). (a-1) Melt flow rate is 1 to 50 g / 10 min (a-2) Density is 0.870 to 0.920 g / cm 3 (a-3) Propylene molar fraction is 5 to 20 mol% (b-1) Melt flow rate is 0.1 to 100 g / 10 min (b-2) Density is 0.880 to 0.930 g / cm 3 (b-3) The molar fraction of C6 or higher α-olefins is 1 to 10 mol% (c-1) Melt flow rate is 0.1 to 20 g / 10 min (c-2) Density is 0.915 to 0.930 g / cm 3 (d-1) Contains 95 to 98 mol% of structural units derived from ethylene as a major component, 1 to 5 mol% of structural units derived from propylene as a minor component, and contains 0.05 to 0.90 mol% of structural units derived from ethylene-α-olefins of C6 or more other than ethylene and propylene as essential minor components (however, the total content of structural units derived from ethylene, structural units derived from propylene, and structural units derived from ethylene-α-olefins does not exceed 100 mol%). (d-2) Melt flow rate is 1 to 100 g / 10 min (d-3) Density is 0.880 to 0.930 g / cm 3 (d-4) The ratio of the molar fraction of propylene (Mp) to the molar fraction of C6 or higher ethylene-α-olefins (Mh) is 5 to 100 (d-5) The relational equation of the densities of the ethylene-propylene copolymer (A) and the ethylene-α-olefin copolymer (B) containing an essential component of C6 or higher satisfies the following formula: Density of ethylene-propylene copolymer (A)...ρ(a) Density of ethylene-α-olefin copolymer (B) containing essential components of C6 or more ... ρ (b) ρ(a)<ρ(b) Relational expression (3)

2. 2. The laminate according to claim 1, wherein the ethylene-propylene copolymer (A) in the layer of the polyethylene resin composition for lamination (D) satisfies the following properties (a-4) to (a-5): (a-4) The total amount of vinyl and vinylidene is 0.35 (pieces / total 1000C) or more. (Note that the number of vinyl and vinylidene units is per 1,000 total carbon atoms in the main chain and side chains as measured by NMR.) (a-5) The number of branches (Y) and density (X) due to comonomers in an ethylene-propylene copolymer satisfy formula (1). (Note that the number of branches is the number per 1,000 total carbon atoms in the main chain and side chains as measured by NMR.) (Y) ≧−1157×(X)+1080 (Formula (1))

3. 3. The laminate according to claim 1, wherein the substrate layer (E) is a paper substrate.

4. 3. The laminate according to claim 1, wherein the ethylene-propylene copolymer (A) in the layer of the polyethylene resin composition for lamination (D) further satisfies the following characteristic (a-6): (a-6) The number of branches (Y) and density (X) due to comonomers in an ethylene-propylene copolymer satisfy formula (2). (Note that the number of branches is the number per 1,000 total carbon atoms in the main chain and side chains measured by NMR.) (Y) ≧−1157×(X)+1084 (Formula (2))

5. 3. The laminate according to claim 1 or 2, wherein the substrate layer (E) is a barrier paper substrate.

6. A laminate comprising at least a substrate layer (E) and a layer (F) containing the ethylene resin composition for lamination (D) according to claim 1 or 2.

7. 7. The laminate of claim 6, wherein the laminate is formed by extrusion coating.

Citation Information

Patent Citations

  • Resin composition for sealant, and packaging film

    JP2016191012A

  • Polyethylene resin composition for lamination and laminate

    JP2019104248A

  • Laminate for heat lamination

    JP2022155390A

  • Packaging material with good tearing property

    JP1998024539A

  • Ethylene-based polymer composition for easily tearing film and the same film

    JP2000212339A

Cited By

  • Heavy duty tire

    EP4703150A1