Manufacturing method of moldings
The method stabilizes modeled objects on a modeling sheet with adjusted peel strength, addressing the challenge of fixing and separating objects in material extrusion 3D printing, improving efficiency by ensuring stable adhesion during printing and easy post-print separation.
Patent Information
- Application Number
- JP2023059205
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The challenge in material extrusion 3D printing is the difficulty in stabilizing the modeled object on the modeling stage during printing while ensuring easy separation after completion, which affects production efficiency due to either weak adhesion leading to peeling or strong adhesion requiring excessive time for separation.
A method involving a modeling sheet fixed to the stage using adhesive, mechanical fastening, or vacuum chuck, with adjusted peel strength between 0.5 N/cm to 20 N/cm, utilizing thermoplastic resins and inorganic fillers to stabilize the object during printing and facilitate easy separation post-printing.
Ensures stable fixation of the object during printing and efficient separation after completion, reducing the time required for separation and enhancing production efficiency.
Smart Images

Figure 2024146359000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for manufacturing a shaped object. [Background technology]
[0002] In recent years, material extrusion (MEX) has been attracting attention as an efficient modeling technology. In the material extrusion method, based on 3D model data, molten material for the modeling layer is extruded from an extrusion nozzle to form a modeling layer, and the modeling layers are stacked to materialize the model.
[0003] A 3D printer used in the material extrusion method is equipped with a modeling stage having a mounting surface for placing a model. The model, on which the modeling layers are stacked, needs to be fixed on the modeling stage. In addition, the object being printed may warp and may try to peel off from the printing stage, so the object needs to be attached to the printing stage with a certain amount of force.
[0004] A modeling sheet is used to increase the adhesion between the modeling stage and the model. The modeling sheet is fixed to the support surface of the modeling stage, and the model is layered on the surface of the modeling sheet, with the first modeling layer being fused to the modeling sheet. Once modeling is complete, the object welded to the modeling sheet is removed from the modeling stage together with the modeling sheet, and is manually separated from the modeling sheet using, for example, a scraper.
[0005] As an example of a modeling sheet used when manufacturing a modeled object by a material extrusion method, Patent Document 1 discloses an adhesive sheet for a modeling stage having an adhesive layer containing an adhesive, the adhesive strength of which can be reduced by adhesive strength reducing measures such as heating, cooling, application of electromagnetic waves, and application of voltage. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2017 / 187800 Summary of the Invention [Problem to be solved by the invention]
[0007] When manufacturing a molded object on a modeling sheet using the material extrusion method, the object needs to be fixed to the modeling stage during modeling. However, since the object will be separated from the modeling sheet after modeling is complete, from the standpoint of workability it is desirable that the object is not firmly fixed to the modeling sheet. However, the object that is layered on the surface of the modeling sheet is strongly welded to the modeling sheet. Therefore, it may take a long time to separate the object that is welded to the modeling sheet from the modeling sheet. For example, it may take more than five hours to manually separate a rectangular parallelepiped object (size: 400 mm wide x 400 mm deep) that is welded to the modeling sheet from the modeling sheet using a scraper.
[0008] In particular, when manufacturing large objects (e.g., objects with long sides of 200 mm or more), if the adhesion between the modeling sheet and the object is too weak, the object will easily peel off from the modeling sheet or become deformed during modeling, and if the adhesion is too strong, it will take a long time to remove the object from the modeling sheet after modeling is complete, resulting in reduced production efficiency.
[0009] An object of the present disclosure is to provide a method for manufacturing a molded object by a material extrusion method, which allows the molded object to be stably fixed to the molding stage via a molding sheet until molding is completed, and which makes it easy to separate the molded object from the molding sheet after molding is completed. [Means for solving the problem]
[0010] Specific means for solving the problems include the following aspects.
[0011] <1> A manufacturing method of a molded object, which molds a molded object on a molding stage by a material extrusion method, comprising the steps of: a shaping sheet fixing step of fixing a shaping sheet on the shaping stage; a modeling step of stacking modeling layers on a surface of the modeling sheet fixed on the modeling stage using a molten modeling material to form the model; a separation step of separating the shaping sheet and the shaped object after the shaping step; Including, A method for manufacturing a shaped object, wherein a peel strength between the shaping sheet and the shaped object in the separation step is adjusted to a range of 0.5 N / cm to 20 N / cm. <2> In the shaping sheet fixing step, the shaping sheet is fixed on the shaping stage by at least one means selected from adhesion, mechanical fastening, and a vacuum chuck. <1> A method for producing a shaped object according to claim 1. <3> The peel strength between the modeling sheet and the modeled object is adjusted by at least one means selected from the composition of the modeling sheet, the melting point or glass transition point of the material of the modeling sheet, the elastic modulus of the modeling sheet, the thickness of the modeling sheet, and the surface treatment of the modeling sheet. <1> or <2> A method for producing a shaped object according to claim 1. <4> The modeling stage includes a temperature adjustment mechanism, and a peel strength between the modeling sheet and the modeled object is adjusted by a temperature of the modeling stage. <1> ~ <3> 13. A method for manufacturing a shaped object according to any one of the above items. <5> The molding material is a material containing an olefin-based polymer, or a material containing an olefin-based polymer and an inorganic filler. <1> ~ <4> 13. A method for manufacturing a shaped object according to any one of the above items. <6> A selection process is included in advance for selecting a modeling sheet for the modeling material used in the modeling process such that the peel strength between the modeling sheet and the modeled object in the separation process is within a range of 0.5 N / cm to 20 N / cm. <1> ~ <5> 13. A method for manufacturing a shaped object according to any one of the above items. Effect of the Invention
[0012] According to the present disclosure, when manufacturing a molded object by a material extrusion method, a manufacturing method is provided in which the molded object can be stably fixed to the molding stage via the molding sheet until molding is completed, and the molded object and the molding sheet can be easily separated after molding is completed. [Brief description of the drawings]
[0013] [Figure 1] 1A to 1C are schematic diagrams for explaining an example of a method for manufacturing a shaped object according to the present disclosure. [Diagram 2] 10A to 10C are schematic diagrams showing an example of a method for fixing a modeling sheet to a modeling stage. [Diagram 3] 3 is an enlarged view of a part of a cross section taken along line AA in FIG. 2. [Figure 4] FIG. 1 is a schematic diagram showing an example of a state in which a model is manufactured using a 3D printer by the manufacturing method for a model according to the present disclosure. [Figure 5A] 2 is a schematic diagram showing an example of a layer structure of a modeling sheet. FIG. [Figure 5B] 11 is a schematic diagram showing another example of the layer structure of the shaping sheet. FIG. [Figure 5C] 11 is a schematic diagram showing another example of the layer structure of the shaping sheet. FIG. [Figure 5D] 11 is a schematic diagram showing another example of the layer structure of the shaping sheet. FIG. [Figure 5E] 11 is a schematic diagram showing another example of the layer structure of the shaping sheet. FIG. [Figure 6A] FIG. 2 is a diagram showing a shaped object produced in the examples to evaluate the ease of removing the shaped sheet from the shaped object. [Figure 6B] FIG. 13 is a diagram showing a state in which a part of the modeling sheet is removed from the model in the embodiment. [Figure 7A] FIG. 2 is a diagram showing a shaped object produced in the examples in order to measure the peel stress when removing a shaping sheet from the shaped object. [Figure 7B] 10A to 10C are diagrams for explaining a method for measuring a peel stress when removing a modeling sheet from a model in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. The embodiments and examples described below are intended to exemplify the method for manufacturing a shaped object according to the present disclosure, and are not intended to limit the method for manufacturing a shaped object according to the present disclosure. Note that in the following description, reference numerals will be omitted as appropriate.
[0015] In this specification, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits. In the numerical ranges described in stages in this disclosure, the upper limit value described in one numerical range may be replaced by the upper limit value of another numerical range described in stages, and the same applies to the lower limit value. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit of the numerical ranges may be replaced with values shown in the examples.
[0016] In the present disclosure, each component may contain multiple types of corresponding substances. When referring to the amount of each component in a composition in the present disclosure, if multiple substances corresponding to each component are present in the composition, the total amount of the multiple substances present in the composition is meant unless otherwise specified. In the present disclosure, combinations of two or more preferred embodiments are more preferred embodiments. In addition, in the present disclosure, the term "process" includes not only an independent process, but also a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process is achieved.
[0017] When manufacturing a model using the material extrusion method, it is desirable for the model to be firmly fixed to the sheet fixed to the modeling stage during modeling in order to prevent deformation such as "warping" of the model, but from the perspective of workability when removing the model from the modeling sheet after modeling is completed, it is desirable for the model to not be firmly fixed to the modeling sheet. For example, the adhesion strength between an object modeled using modeling sheet A and modeling material B is different from the adhesion strength between an object modeled using modeling sheet A and modeling material C, and modeling sheet A is not necessarily suitable for some modeling materials. Therefore, the inventors of the present disclosure conducted extensive research and experiments to resolve these two conflicting demands depending on the situation, and discovered that, regardless of the type of modeling material or modeling sheet, as long as the peel strength between the modeling sheet and the modeled object during the separation process is adjusted to be within the range of 0.5 N / cm to 20 N / cm, the modeled object can be stably fixed to the modeling stage via the modeling sheet until modeling is completed, and after modeling is completed, the modeled object and the modeling sheet can be easily separated, thereby shortening the separation work time and improving production efficiency.
[0018] In other words, the method for manufacturing a molded object according to the present disclosure is a method for manufacturing a molded object by forming a molded object on a mold stage by a material extrusion method, and includes a molded object fixing process for fixing a molded object sheet onto the mold stage, a molded object forming process for laminating molded layers using molten mold material on the surface of the molded object sheet fixed onto the mold stage, and a separation process for separating the molded object from the molded object after the molded object forming process, and the peel strength between the molded object and the molded object in the separation process is adjusted to be within the range of 0.5 N / cm to 20 N / cm.
[0019] If the peel strength between the modeling sheet and the object is 0.5 N / cm or more, the object can be stably fixed to the modeling stage via the modeling sheet until the object is completed by the material extrusion method. From this viewpoint, the peel strength between the modeling sheet and the object is preferably 1 N / cm or more, more preferably 5 N / cm or more, and even more preferably 10 N / cm or more. On the other hand, if the peel strength between the modeling sheet and the object is 20 N / cm or less, the object can be easily separated from the modeling sheet after modeling is completed, and the work time for the separation process can be shortened. From this perspective, the peel strength between the modeling sheet and the object is preferably 10 N / cm or less, more preferably 5 N / cm or less, and even more preferably 1 N / cm or less.
[0020] The 3D printer used for modeling, for example, extrudes a molten material from a nozzle onto the surface of a modeling sheet based on multiple pieces of two-dimensional data, thereby materializing the 3D model data. The multiple pieces of two-dimensional data are generated, for example, by slicing the 3D model data into slices using slicer software. The multiple pieces of two-dimensional data include, for example, G-code data.
[0021] The 3D printer used in the method for manufacturing a molded object according to the present disclosure may be a known device.
[0022] The modeling stage has a mounting surface on which an object to be modeled is placed. The mounting surface is, for example, flat. The modeling stage includes, for example, an aluminum plate.
[0023] A modeling sheet is fixed to the mounting surface of the modeling stage, and peeling and deformation (especially warping) of the modeled object during modeling are suppressed by the adhesion between the modeling stage and the modeling sheet via the modeling sheet.
[0024] The method for fixing the modeling sheet to the support surface of the modeling stage is not particularly limited, but examples include methods for fixing the modeling sheet to the front modeling stage by at least one means selected from adhesive, mechanical fastening, and vacuum chucks.
[0025] Fig. 1 is a schematic diagram for explaining an example of a manufacturing method of a modeled object according to the present disclosure. The 3D printer (three-dimensional modeled object manufacturing device) 100 shown in Fig. 1 includes a hopper 30, a cylinder 32, an extrusion nozzle 36, a modeling stage 10, and the like. The cylinder 32 includes a heater (not shown) for heating the modeling material 40 supplied from the hopper 30, and a screw 34 for kneading the modeling material 40 and extruding it from a nozzle 36 is provided inside the cylinder 32. A control unit (not shown) controls the extrusion amount of the molten modeling material (melt) extruded from the nozzle 36, and the movement of the nozzle 36 in the X-axis, Y-axis, and Z-axis directions relative to a reference plane of the modeling stage 10.
[0026] [Modeling sheet fixing process] In the modeling sheet fixing step, the modeling sheet 50 is fixed onto the modeling stage 10.
[0027] <Modeling sheet> The modeling sheet 50 is a sheet for fixing the model 20A during modeling.
[0028] The shaping sheet 50 is configured to contain, for example, a thermoplastic resin. Fig. 5A shows an example of the shaping sheet 50. As shown in Fig. 5A, for example, a single-layer resin sheet 50A can be used. Examples of the thermoplastic resin include the same ones as those described below as thermoplastic resins contained in the shaping material. The shaping sheet 50 may further contain an inorganic filler. Examples of the inorganic filler include the same inorganic fillers contained in the shaping material as those described below.
[0029] The shaping sheet 50 may be subjected to a surface treatment to adjust the adhesion to the shaped object 20. Examples of the surface treatment include physical treatments such as embossing, corona treatment, and plasma treatment, and chemical treatments such as undercoating.
[0030] The size of the shaping sheet 50 is appropriately selected depending on the dimensions of the object to be shaped, etc. The thickness of the shaping sheet 50 depends on the material, but from the standpoint of strength, ease of handling, etc., it is preferably 0.01 mm or more and 10.00 mm or less, more preferably 0.05 mm or more and 5.00 mm or less, and even more preferably 0.10 mm or more and 3.00 mm or less.
[0031] Fig. 2 is a schematic diagram showing an example of a method for fixing the modeling sheet 50 to the modeling stage 10, and Fig. 3 is an enlarged view of a part of the cross section taken along line AA in Fig. 2. The mounting surface on which the modeling object 20 is placed on the modeling stage 10 is provided with vacuum holes 12 for fixing the modeling sheet 50 by a vacuum chuck (vacuum drawing). The peripheral portion of the modeling sheet 50 is attached to the modeling stage 10 via masking tape 60, and when modeling is performed, the modeling sheet 50 is further firmly fixed to the modeling stage 10 by a vacuum chuck via the vacuum holes 12.
[0032] The means for fixing the modeling sheet 50 on the modeling stage 10 is not limited to a vacuum chuck or masking tape, and examples of mechanical fastening include a means for holding the periphery of the modeling sheet 50 placed on the modeling stage 10 with metal fittings or the like. Also, the modeling sheet 50 may be removably adhered to the modeling stage 10 via an adhesive or the like.
[0033] 5B to 5E each show another example of the configuration of a shaping sheet that can be used in the manufacturing method of a shaped object according to the present disclosure.
[0034] The shaping sheet 50B shown in FIG. 5B has an adhesive layer 54 disposed on one surface of a base material 52. In the modeling sheet 50C shown in FIG. 5C, adhesive layers 54 and 56 are disposed on both sides of a base material 52, respectively. The shaping sheet 50D shown in FIG. 5D is composed of only an adhesive layer 54. A shaping sheet 50E shown in FIG. 5E has a configuration in which adhesive layers 54 and 56 are laminated together without a base material therebetween.
[0035] Examples of materials that can be used to form the base material 52 include paper, nonwoven fabric, and plastic film. Examples of paper materials include Japanese paper, crepe paper, craft paper, glassine paper, and synthetic paper. Examples of materials for nonwoven fabrics include pulp such as hemp pulp and wood pulp, rayon, acetate fibers, polyester fibers, polyamide fibers, polyolefin fibers, and polyvinyl alcohol fibers. Examples of resins constituting the plastic film include polyolefins, polyesters, polyurethanes, polyimide resins, polyamide resins, soft vinyl chloride resins, and vinyl acetate resins.
[0036] Examples of adhesives constituting the adhesive layers 54, 56 include acrylic adhesives, natural rubber, synthetic rubber, vinyl alkyl ether adhesives, silicone adhesives, polyester adhesives, polyamide adhesives, and urethane adhesives. The adhesive layers 54 and 56 may be made of the same adhesive or different adhesives.
[0037] In the manufacturing method of a molded object according to the present disclosure, since the adhesion strength between the molded object 20 and the molded sheet 50 varies depending on the molding material used, it is sufficient to select a molded sheet such that the peel strength between the molded object 20 and the molded sheet 50 is within the range of 0.5 N / cm to 20 N / cm depending on the molding material used. The means for adjusting the peel strength between the modeling sheet 50 and the modeled object 20 according to the modeling material is not particularly limited, but can be suitably adjusted by at least one means selected from the composition of the modeling sheet 50, the melting point or glass transition point of the material of the modeling sheet 50, the elastic modulus of the modeling sheet 50, the thickness of the modeling sheet 50, and the surface treatment of the modeling sheet 50.
[0038] [Modeling process] In the modeling process, modeling layers are stacked on the surface of a modeling sheet 50 fixed on a modeling stage 10 using a melt 42 of a modeling material 40 to form a model 20.
[0039] A 3D printer is used for the modeling process. When manufacturing a model 20 using the 3D printer 100 shown in Fig. 1, a modeling material 40 is put into a hopper 30, and the modeling material 40 is supplied from the hopper 30 into a cylinder 32. In the cylinder 32, the modeling material 40 is heated and melted by the rotation of a heater and a screw 34, and is extruded as a molten material 42 from an extrusion nozzle 36 toward a modeling sheet 50 fixed on a modeling stage 10. As the molten material 42 is extruded from the nozzle 34 and the nozzle 34 moves relative to the modeling stage 10, a modeling layer is formed by the molten material 42, and the modeling layers are sequentially stacked to form a model 20 on the modeling sheet 50.
[0040] When the molten material 42 of the modeling material 40 forms modeling layers on the surface of the modeling sheet 50 , the bottom layer of the modeling layers is welded to the modeling sheet 50 . The nozzle temperature of the extrusion nozzle 36 may be any temperature at which the modeling material melts, and is adjusted appropriately depending on the type of modeling material, etc. The temperature at which the modeling material melts may be, for example, a temperature of +10°C to +150°C based on the higher of the melting point or the glass transition point (Tg) of the thermoplastic resin. Thermoplastic resins will be described later. The layer pitch of the modeling layers is adjusted appropriately according to the dimensions of the modeled object, etc. From the viewpoint of adhesion strength, the layer pitch of the modeling layers is preferably 3 / 4 or less of the nozzle diameter, more preferably 1 / 2 or less of the nozzle diameter. The layer pitch of the modeling layers corresponds to the thickness of each modeling layer. The filling rate of the modeling layer may be 100% or less than 100%. The filling rate indicates the ratio of the volume of the modeling layer material to the unit space volume. The total thickness of the modeling layers is adjusted appropriately depending on the size of the model, etc. The number of layers of the modeling layers is appropriately selected depending on the thickness of the modeling layers, the lamination pitch of the modeling layers, etc., and may be one layer or two or more layers.
[0041] <Modeling materials> From the viewpoint of ease of molding by the material extrusion method, the molding material 40 is preferably a material containing a thermoplastic resin, and from the viewpoint of mechanical properties of the manufactured object, it is more preferable that the molding material 40 is a material containing a thermoplastic resin and an inorganic filler. Note that an olefin-based polymer is preferable as the thermoplastic resin.
[0042] (thermoplastic resin) The thermoplastic resin preferably contains at least one of a thermoplastic plastic and a thermoplastic elastomer, and more preferably contains both a thermoplastic plastic and a thermoplastic elastomer. When the thermoplastic resin contains a thermoplastic plastic and a thermoplastic elastomer, deformation of the modeling layer is more effectively suppressed.
[0043] The thermoplastic resin preferably contains a crystalline thermoplastic resin from the viewpoints of further suppressing warping of the shaped object and separating the shaped object from the shaping sheet in a shorter time.
[0044] Thermoplastics have a tensile modulus of elasticity of 6.0 x 10 at 25°C. 8 The tensile modulus of elasticity at 25°C is 6.0×10 Pa or more. 8 This indicates a thermoplastic resin having a compressive strength of less than Pa. The tensile modulus is a measurement value conforming to JIS K7161-2:2014.
[0045] Thermoplastics Thermoplastic plastics have little rubber-like elasticity and are difficult to deform. Rubber-like elasticity refers to the property that the shape of a resin changes when a load is applied to the resin, and the shape of the resin returns to its original shape when the load is removed.
[0046] The thermoplastic plastic is not particularly limited, and any known thermoplastic plastic can be used. The thermoplastic plastic may be used alone or in combination of two or more kinds. For example, thermoplastics include general-purpose plastics, engineering plastics, and super engineering plastics. Examples of general-purpose plastics include high-density polyethylene (HDPE), low-density polyethylene (LDPE), propylene-based polymers (propylene homopolymer (PP)), polyvinyl chloride (PVC), polyvinylidene chloride, polystyrene (PS), polyvinyl acetate (PVAc), polytetrafluoroethylene (PTFE), acrylonitrile butadiene styrene resin (ABS resin), styrene-acrylonitrile copolymer (AS resin), and acrylic resin (PMMA, etc.). Engineering plastics include polyamide (PA), polyacetal (POM), polycarbonate (PC), modified polyphenylene ether (m-PPE, modified PPE, PPO), polybutylene terephthalate (PBT), polyethylene terephthalate (PET), syndiotactic polystyrene (SPS), and cyclic polyolefin (COP). Examples of super engineering plastics include polyphenylene sulfide (PPS), polytetrafluoroethylene (PTFE), polysulfone (PSF), polyethersulfone (PES), amorphous polyarylate (PAR), polyetheretherketone (PEEK), thermoplastic polyimide (PI), and polyamideimide (PAI). In particular, from the viewpoint of further suppressing warping of the molded object and separating the molded object from the molding sheet in a shorter time, it is preferable that the thermoplastic contains one or more types selected from the group consisting of high-density polyethylene (HDPE), propylene-based polymers, polyamide (PA), polybutylene terephthalate (PBT), syndiotactic polystyrene (SPS), polyphenylene sulfide (PPS) and polyacetal (POM), and it is more preferable that the thermoplastic contains a propylene-based polymer.
[0047] From the viewpoint of further suppressing warpage of the molded object, the thermoplastic preferably contains at least one of a crystalline thermoplastic and an amorphous thermoplastic, and more preferably contains a crystalline thermoplastic. When the thermoplastic contains a crystalline thermoplastic, the molded object has an excellent balance between mechanical strength and impact resistance. The crystalline thermoplastic is an example of a crystalline thermoplastic resin. The crystalline thermoplastic more preferably includes at least one selected from the group consisting of high density polyethylene (HDPE), a propylene-based polymer, polyamide (PA), polybutylene terephthalate (PBT), syndiotactic polystyrene (SPS), polyphenylene sulfide (PPS), and polyacetal (POM), and further preferably includes a propylene-based polymer. The "crystalline" nature of a thermoplastic refers to the presence of an endothermic peak in differential scanning calorimetry. The "amorphous" nature of a thermoplastic refers to the absence of a clear endothermic peak in differential scanning calorimetry.
[0048] The propylene polymer is a polymer having at least propylene as a constituent unit. The propylene-based polymer may be a homopolymer of propylene or a copolymer of propylene and another monomer. When the propylene-based polymer is a copolymer, for example, a copolymer of propylene and an α-olefin having 2 to 20 carbon atoms (excluding propylene) can be mentioned. For example, a copolymer of propylene and an α-olefin having 2 to 20 carbon atoms can be mentioned, for example, a propylene-ethylene copolymer, a propylene-1-butene copolymer, a propylene-ethylene-1-butene copolymer, a propylene-4-methyl-1-pentene copolymer, a mixture thereof, and the like.
[0049] When the propylene-based polymer is a copolymer, the propylene-based polymer may be any one of a random copolymer, an alternating copolymer, a block copolymer, and a graft copolymer.
[0050] When the propylene-based polymer is a copolymer, the ratio of the structural units derived from propylene in the propylene-based polymer may be appropriately designed according to the desired properties of the modeling layer. For example, the ratio of the structural units derived from propylene in the propylene-based polymer is preferably 50 mol% or more, more preferably 70 mol% to 99.5 mol%, and even more preferably 80 mol% to 98 mol%, based on 100 mol% of all structural units in the propylene-based polymer.
[0051] The stereoregularity of the propylene polymer may be any of isotactic, syndiotactic and a mixture thereof.
[0052] The content of the propylene-based polymer is preferably 95.0% by mass or more, more preferably 98.0% by mass or more, and even more preferably 99.9% by mass or more, based on 100% by mass of the total amount of thermoplastics.
[0053] The upper limit of the crystallization temperature (Tc) of the thermoplastic is preferably 140° C. or lower, more preferably 130° C. or lower. The lower limit of the crystallization temperature (Tc) of the thermoplastic is preferably 90° C. or higher, more preferably 110° C. or higher. The crystallization temperature of a thermoplastic plastic is measured by a differential scanning calorimeter (DSC) at a temperature drop rate of 10° C. / min.
[0054] The upper limit of the crystallinity of the thermoplastic is preferably 80% or less, more preferably 75% or less. The lower limit of the crystallinity of the thermoplastic is preferably 2% or more, more preferably 5% or more. The degree of crystallinity of a thermoplastic is calculated from the heat of fusion resulting from the melting of the main component in the heat flow curve obtained using a differential scanning calorimeter (DSC). The heat flow curve is obtained by holding the thermoplastic at -40°C for 5 minutes under a nitrogen atmosphere, then raising the temperature at 10°C / min. Specifically, a differential scanning calorimeter (Perkin-Elmer, DSC-7) is used to obtain a heat flow curve by holding 5 mg of a sample at -40°C for 5 minutes under a nitrogen atmosphere, then raising the temperature at 10°C / min. The heat of fusion is calculated from the heat of fusion resulting from the melting of the main component in the obtained heat flow curve using the following formula. Crystallinity = (ΔH / ΔH0)×100(%) In the formula, ΔH is the heat of fusion (J / g) calculated from the heat of fusion curve resulting from the melting of the main component of the thermoplastic, and ΔH0 is the heat of fusion (J / g) of perfect crystallization of the main component. For example, if the main component is ethylene, ΔH0 is 293 J / g, and if the main component is propylene, ΔH0 is 210 J / g.
[0055] The upper limit of the melting point of the thermoplastic is preferably 200° C. or lower, more preferably 180° C. or lower. The lower limit of the melting point of the thermoplastic is preferably 90° C. or higher, more preferably 110° C. or higher. The melting point can be measured in the same manner as in the measurement of the melting point of a thermoplastic elastomer described below.
[0056] ·Thermoplastic elastomer The thermoplastic elastomer has rubber-like elasticity.
[0057] The thermoplastic elastomer is preferably a copolymer containing structural units derived from an α-olefin and structural units derived from an olefin different from the α-olefin.
[0058] The α-olefin may generally contain one kind of α-olefin having 2 to 20 carbon atoms alone or two or more kinds of α-olefins in combination. Among them, the α-olefin is preferably an α-olefin having 3 or more carbon atoms, and more preferably an α-olefin having 3 to 8 carbon atoms.
[0059] Examples of the α-olefin include 1-butene, 1-pentene, 1-hexene, 3-methyl-1-butene, 3,3-dimethyl-1-butene, 4-methyl-1-pentene, 1-octene, etc. One or more of the α-olefins are used. Among these, from the viewpoint of availability, 1-butene, 1-pentene, 1-hexene, and 4-methyl-1-pentene are preferred as the α-olefin.
[0060] The olefin other than the α-olefin is preferably an olefin having 2 to 4 carbon atoms, and examples of the olefin include ethylene, propylene, butene, etc. Among them, the olefin other than the α-olefin is more preferably an olefin having 2 to 3 carbon atoms.
[0061] Examples of copolymers that are thermoplastic elastomers include ethylene-α-olefin copolymers, propylene-α-olefin copolymers, and butene-α-olefin copolymers.
[0062] Examples of thermoplastic elastomers include ethylene-propylene copolymers (EPR), ethylene-1-butene copolymers (EBR), ethylene-1-pentene copolymers, ethylene-1-octene copolymers (EOR), propylene-1-butene copolymers (PBR), propylene-1-pentene copolymers, and propylene-1-octene copolymers (POR).
[0063] Among these, the thermoplastic elastomer is preferably a copolymer containing a structural unit derived from an α-olefin having 2 to 8 carbon atoms and a structural unit derived from an olefin having 2 to 3 carbon atoms, and a propylene-based elastomer is preferred because it is easily welded to thermoplastic plastics (especially propylene-based polymers) and deformation of the modeling layer is further suppressed.
[0064] Furthermore, the α-olefins may form random copolymers or block copolymers.
[0065] The melting point Tm of the thermoplastic elastomer is preferably 30°C or higher and 120°C or lower. When the melting point of the thermoplastic elastomer is between 30°C and 120°C, the thermoplastic elastomer acts as an adhesive between the modeling layers formed by the material extrusion method, thereby improving the adhesive strength between the modeling layers. The melting point is the value determined as the temperature Tm at the melting peak position that appears on the endothermic curve by differential scanning calorimetry (DSC). The melting point is determined from the endothermic curve when a sample is packed in an aluminum pan, heated to 230°C at 100°C / min, held at 230°C for 5 minutes, cooled to -70°C at -10°C / min, and then heated at 10°C / min.
[0066] The melt flow rate (MFR; 230° C., 2.16 kg load) of the thermoplastic elastomer is preferably 0.5 g / 10 min or more, more preferably 1 g / 10 min or more, further preferably 2 g / 10 min or more, and particularly preferably 5 g / 10 min or more. The upper limit of the melt flow rate (MFR; 230° C., 2.16 kg load) of the thermoplastic elastomer is preferably 70 g / 10 min or less, more preferably 35 g / 10 min or less, and further preferably 30 g / 10 min or less. When the upper and lower limits of the MFR of the thermoplastic elastomer are within this range, deformation of the modeling layer can be more effectively suppressed. The melt flow rate (MFR) is a value measured in accordance with ASTM D1238-65T under conditions of 230° C. and a load of 2.16 kg.
[0067] The upper limit of the Shore D hardness of the thermoplastic elastomer is preferably not more than 60. The lower limit of the Shore D hardness of the thermoplastic elastomer is preferably 30 or more, more preferably 40 or more, and even more preferably 50 or more. When the hardness of the thermoplastic elastomer is 30 or more in Shore D hardness, the thermoplastic elastomer is less likely to deform. In other words, the shape of the thermoplastic elastomer is more likely to be maintained. Therefore, when a modeling layer is formed using a 3D printer described later, the thermoplastic elastomer is more likely to enter the screw of the cylinder. As a result, the discharge efficiency of the molten modeling material is improved. This makes it easier to obtain a model with a smooth surface and excellent appearance. The Shore D hardness is a value measured in accordance with the method described in ASTM D2240.
[0068] Specific examples of thermoplastic elastomers include the TAFMER (registered trademark) series manufactured by Mitsui Chemicals, Inc. (e.g., TAFMER DF605, TAFMER DF610, TAFMER DF640, TAFMER DF710, TAFMER DF740, TAFMER DF7350, TAFMER DF810, TAFMER DF840, TAFMER DF8200, TAFMER DF940, TAFMER DF9200, TAFMER DF110, TAFMER H-0530S ... Examples of such polyimide resins include TAFMER H-1030S, TAFMER H-5030S, TAFMER XM-7070, TAFMER XM-7080, TAFMER XM-7090, TAFMER BL2491M, TAFMER BL2481M, TAFMER BL3110M, TAFMER BL3450M, TAFMER MA8510, TAFMER MH7010, TAFMER MH7020, TAFMER MH5020, TAFMER PN-2070, and TAFMER PN-3560. Among the above, the Toughmer XM series, which is a propylene-based elastomer, is preferred because it is easily welded to thermoplastics (particularly propylene-based polymers) and deformation of the modeling layer is further suppressed. The Toughmer XM series is easily welded to thermoplastics (especially propylene-based polymers) and can maintain the breaking stress α required for the modeling layers. This improves the adhesive strength between modeling layers created by the material extrusion method.
[0069] The thermoplastic elastomer is preferably a propylene-based elastomer. The propylene-based elastomer is a thermoplastic elastomer having at least propylene as a constituent unit. The thermoplastic elastomer is preferably a propylene-based elastomer having a melting point of 80°C to 120°C, a Shore D hardness of 40 to 60, and an MFR of 2g / 10min to 20g / 10min, which makes the modeling layer less susceptible to stress distortion and warping. An example of a propylene-based elastomer having a melting point of 80° C. to 120° C., a Shore D hardness of 40 to 60, and an MFR of 2 g / 10 min to 20 g / 10 min is Toughmer XM-7090.
[0070] (Inorganic filler) The material of the inorganic filler is not particularly limited as long as it is an inorganic compound, and known inorganic fillers can be used. Examples of inorganic fillers include oxide-based fillers, hydroxide-based fillers, silicate-based fillers, sedimentary rock-based fillers, clay mineral-based fillers, magnetic fillers, conductive fillers, thermally conductive fillers, sulfate-based fillers, sulfite-based fillers, carbonate-based fillers, and titanate-based fillers. Examples of oxide-based fillers include carbon black that has been surface-treated with a silane coupling agent, carbon black, graphite, finely powdered silicic acid, silica, alumina, iron oxide, ferrite, magnesium oxide, titanium oxide, antimony trioxide, zirconium oxide, barium oxide, and calcium oxide. Examples of silica include fumed silica, precipitated silica, diatomaceous earth, and quartz. Examples of hydroxide-based fillers include aluminum hydroxide and magnesium hydroxide. Examples of silicate-based fillers include aluminum silicate (hereinafter also referred to as "clay", including hydrated aluminum silicate), magnesium silicate (including hydrated magnesium silicate (hereinafter also referred to as "talc")), mica, kaolin, calcium silicate (including hydrated calcium silicate), glass fiber, glass flakes, and glass beads. Sedimentary rock-based fillers include diatomaceous earth and limestone. Examples of clay mineral fillers include montmorillonite, magnesian montmorillonite, tesla montmorillonite, tesla magnesian montmorillonite, beidellite, aluminian beidellite, nontronite, aluminian nontronite, saponite (i.e., saponite), aluminian saponite, hectorite, sauconite, stevensite, and bentonite. The magnetic filler may include ferrite, iron, and cobalt. The conductive filler may include silver, gold, copper, and alloys thereof. Thermally conductive fillers include aluminum nitride, boron nitride, and silicone carbide. Examples of the sulfate-based filler include aluminum sulfate, magnesium sulfate, barium sulfate, and calcium sulfate. An example of the sulfite-based filler is calcium sulfite. Examples of carbonate-based fillers include calcium carbonate, basic magnesium carbonate, and dolomite. Examples of titanate-based fillers include barium titanate and potassium titanate.
[0071] The inorganic filler preferably contains at least one selected from the group consisting of talc, calcium carbonate, and magnesium sulfate. Since the inorganic filler does not undergo volumetric change at the nozzle temperature of the extrusion nozzle and the thermal expansion coefficient of the inorganic filler is lower than that of the thermoplastic resin, deformation (particularly warping) of a molded object molded using a molding material containing an inorganic filler is more suppressed. The fact that the inorganic filler does not undergo volumetric change at the nozzle temperature of the extrusion nozzle means that the inorganic filler does not melt, does not dissolve, and does not undergo phase transition at the nozzle temperature of the extrusion nozzle. A model formed using a modeling material containing talc has an excellent smooth appearance after the modeling sheet is removed. A molded object made using a molding material containing calcium carbonate is more suppressed from warping. In addition, a molded object made using a molding material containing calcium carbonate has excellent whiteness and high designability. A molded object formed using a molding material containing magnesium sulfate is more suppressed from warping.
[0072] The shape of the inorganic filler is not particularly limited, and examples thereof include spherical, plate-like, scaly, needle-like, and fibrous shapes. The upper limit of the volume average particle diameter of the inorganic filler is preferably 30 μm or less, more preferably 10 μm or less.The lower limit of the volume average particle diameter of the inorganic filler is preferably 0.5 μm or more, more preferably 1 μm or more. The volume average particle size of an inorganic filler is defined as the particle size value at which the cumulative volume of each particle, measured in a dispersed state in water using a particle size analyzer such as a laser diffraction / scattering particle size analyzer, is 50% of the total volume when the volume of each particle is cumulatively calculated from the smallest particle size.
[0073] (Other ingredients) The molding material may contain other components in addition to the thermoplastic resin and the inorganic filler, such as ultraviolet absorbers, stabilizers, antioxidants, plasticizers, colorants, tinting agents, flame retardants, antistatic agents, fluorescent brighteners, matting agents, and impact strength improvers. The molding material may also contain biomass-derived raw materials.
[0074] [Separation process] In the separation step, after the modeling step, the modeling sheet and the shaped object are separated from each other. In the method for manufacturing a shaped object according to the present disclosure, the peel strength between the modeling sheet and the shaped object in the separation step is adjusted to a range of 0.5 N / cm to 20 N / cm.
[0075] 4 is a schematic diagram showing an example of a state in which a model is manufactured using a 3D printer. After modeling is completed, for example, the vacuum chuck is released, the masking tape 60 is peeled off, and the model 20 modeled on the modeling sheet 50 is taken out together with the modeling sheet 50 from the modeling stage 10.
[0076] There is no particular limitation on the method for separating the object 20 welded to the shaping sheet 50 from the shaping sheet 50, but for example, it is preferable to use a scraper to scrape the interface between the shaping sheet 50 and the object 20 to separate the shaping sheet 50 from the object 20 welded to the shaping sheet 50. At this time, since the peel strength between the shaping sheet 50 and the object 20 is in the range of 0.5 N / cm to 20 N / cm, the object 20 welded to the shaping sheet 50 can be separated from the shaping sheet 50 in a short time using the scraper.
[0077] The modeling stage 10 shown in Fig. 4 is provided with a temperature adjustment mechanism 14. If, for example, a heater is provided as the temperature adjustment mechanism 14, after modeling is completed, the modeling sheet 50 is heated by the heater via the modeling stage 10, which softens the modeling sheet 50 and reduces the adhesive force between the modeling sheet 50 and the modeled object 20. This reduces the work of separating the modeling sheet 50 and the modeled object 20 in the separation process, allowing them to be separated in a shorter time.
[0078] The temperature adjustment mechanism 14 of the modeling stage 10 is not limited to a heating means such as a heater, and may be, for example, a means for cooling the modeling stage 10. After modeling is completed, the modeling sheet 50 may be cooled via the modeling stage 10 to harden the modeling sheet 50, thereby reducing the adhesive force between the modeling sheet 50 and the modeled object 20.
[0079] [Other processes] The method for manufacturing a shaped object according to the present disclosure may further include, for example, a processing step in which the shaped object produced in the modeling step is processed.
[0080] In addition, in order to select a modeling sheet appropriate for the modeling material used in the modeling process, the manufacturing method of a modeled object according to the present disclosure may include a selection process for pre-selecting a modeling sheet such that the peel strength between the modeling sheet and the model in the separation process is within the range of 0.5 N / cm to 20 N / cm. For example, multiple resin sheets of different materials that can be used as modeling sheets for the modeling material to be used are prepared. Then, the above-mentioned modeling sheet fixing step and modeling step are performed using each resin sheet. Then, a peel stress test described later in the examples is performed to measure the peel stress between the resin sheet and the model, and a resin sheet with a peel strength in the range of 0.5 N / cm to 20 N / cm is selected as the modeling sheet to be used in the manufacturing method of a modeled object according to the present disclosure. EXAMPLES
[0081] Hereinafter, the present disclosure will be described in more detail with reference to examples, but the present disclosure is not limited to the following examples as long as it does not deviate from the gist of the disclosure. In addition, unless otherwise specified, "parts" are based on mass.
[0082] <Preparing modeling materials> The thermoplastic elastomer (40 parts by mass), thermoplastic plastic (20 parts by mass), and inorganic filler (40 parts by mass) shown below were blended and kneaded using an extruder (model number KTX-30, manufactured by Kobe Steel, Ltd.) to obtain a PP compound.
[0083] (Thermoplastic elastomer) "Tafmer (registered trademark) XM-7090", manufactured by Mitsui Chemicals, Inc., material: propylene polymer, melting point Tm: 98°C, Shore D hardness: 58, MFR: 7.0g / min, tensile modulus at 25°C: less than 6.0×108 Pa The melting point Tm, Shore D hardness, and MFR are all catalog values.
[0084] (Thermoplastics) "Prime Polypro (registered trademark) J-105G", manufactured by Prime Polymer Co., Ltd., material: propylene homopolymer, crystallization temperature Tc: 116.4°C, crystallinity: 52.2%, tensile modulus at 25°C: 6.0 x 108 Pa or more The values of the crystallization temperature Tc and the Shore D hardness are catalog values.
[0085] (Inorganic filler) Talc, volume average particle size: 5μm~10μm
[0086] The obtained PP compound was extruded from a nozzle and cut at 4 mm intervals to obtain granular molding material measuring 4 mm x 3 mm x 2 mm. The extruder conditions were as follows: cylinder temperature: C1 = 50°C, C2 = 90°C, C3 = 100°C, C4 = 120°C, C5 = 180°C, C6 = 200°C, C7 to C14 = 200°C, die temperature: 200°C, screw rotation speed: 500 rpm, extrusion rate: 40 kg / h.
[0087] <Fixing the modeling sheet> A material extrusion 3D printer ("EXF-12" manufactured by Extrabold Co., Ltd.) and application software ("UltimakerCURA" manufactured by Ultimaker) were used. Next, the modeling sheet was placed on the modeling stage, the outer periphery of the modeling sheet was fixed with masking tape, and a vacuum was drawn using a vacuum pump through holes provided on the surface of the modeling stage to fix the modeling sheet in place.
[0088] <Additive Manufacturing> Next, the molding material was put into the hopper, and the molding material was supplied into the cylinder through the hopper. Next, the molding material was heated to a temperature of 180° C. to 240° C. by a heater provided in the cylinder, and the molding material was melted.
[0089] Next, the application software was used to slice the 3D model data below to generate multiple 2D data sets. Based on the multiple 2D data sets, the application software's parameters were set as follows:
[0090] (Model for measuring removability) <3D model data> - Rectangular prism of 80mmD x 80mmW x 50mmH <Printing layer setting parameters> Nozzle diameter: 3mm - Build speed: 360mm / min Nozzle temperature: 200℃ Layer pitch: 1.5mm ·Number of layers: 33 layers -Building stage temperature: 60℃
[0091] (For peel stress measurement) <3D model data> - Rectangular prism of 80mmD x 28mmW x 3mmH <Printing layer setting parameters> Nozzle diameter: 3mm - Build speed: 360mm / min Nozzle temperature: 200℃ Layer pitch: 1.5mm ·Number of layers: 2 layers -Building stage temperature: 60℃
[0092] Next, based on the 2D data, the molten modeling material was extruded from an extrusion nozzle (nozzle diameter: 3 mm) onto the surface of the modeling sheet to obtain a modeled object S1 for measuring removability with the size and shape shown in Fig. 6A and a modeled object S2 for measuring peel stress shown in Fig. 7A. Both models could be modeled without peeling off from the modeling sheet until modeling was completed.
[0093] In this manner, a shaped object S1 for measuring removability and a shaped object S2 for measuring peel stress were obtained, each of which was welded to the modeling sheet.
[0094] <Removing the modeling sheet from the model> The modeling sheet on which the object S1 for removability measurement was formed was removed from the modeling stage, and the modeling sheet 50 was manually pulled and peeled off from the object S1 for removability measurement, as shown in Fig. 6B. The removability of the modeling sheet was good for all of the objects for removability measurement.
[0095] <Measurement of peel stress> 7A, one end C of the object S2 for peel stress measurement, which was in close contact with the modeling sheet 50, was peeled off from the modeling sheet 50 and chucked. The modeling sheet 50 peeled off from the one end C of the object S2 for peel stress measurement was pulled in the direction D of the end opposite to the chuck, and the peel stress was measured under the following conditions.
[0096] Test equipment: Intesco 201X Load cell: 100N Measurement temperature: 23℃ Test speed: 300.0mm / min Test method: 180° peel
[0097] The results are shown in Table 1.
[0098] [Table 1]
[0099] In both cases, the peel strength between the modeling sheet and the model was within the range of 0.5 N / cm to 20 N / cm, the model was stably fixed during modeling, and the model could be easily removed by hand from the modeling sheet after modeling was completed, demonstrating good removability. [Explanation of symbols]
[0100] 10 Modeling Stage 12 holes 14 Temperature adjustment mechanism 20 Sculptures 30 Hopper 32 cylinders 34 Screw 36 Extrusion Nozzle 40 Modeling Materials 42 Melt 50 Modeling Sheet 52 Base material 54,56 Adhesive layer 60 Masking Tape 100 3D Printers
Claims
1. A manufacturing method of a molded object, which molds a molded object on a molding stage by a material extrusion method, comprising the steps of: a shaping sheet fixing step of fixing a shaping sheet on the shaping stage; a modeling step of stacking modeling layers on a surface of the modeling sheet fixed on the modeling stage using a molten modeling material to form the model; a separation step of separating the shaping sheet and the shaped object after the shaping step; Including, A method for manufacturing a shaped object, wherein a peel strength between the shaping sheet and the shaped object in the separation step is adjusted to a range of 0.5 N / cm to 20 N / cm.
2. The method for manufacturing a shaped object according to claim 1 , wherein in the shaping sheet fixing step, the shaping sheet is fixed onto the shaping stage by at least one means selected from the group consisting of adhesive, mechanical fastening, and a vacuum chuck.
3. The method for manufacturing a molded object described in claim 1, wherein the peel strength between the molding sheet and the molded object is adjusted depending on the molding material by at least one means selected from the composition of the molding sheet, the melting point or glass transition point of the material of the molding sheet, the elastic modulus of the molding sheet, the thickness of the molding sheet, and the surface treatment of the molding sheet.
4. The method for manufacturing a shaped object according to claim 1 , wherein the shaping stage includes a temperature adjustment mechanism, and a peel strength between the shaping sheet and the shaped object is adjusted by a temperature of the shaping stage.
5. The method for manufacturing a shaped object according to claim 1 , wherein the shaping material is a material containing an olefin-based polymer or a material containing an olefin-based polymer and an inorganic filler.
6. The method for manufacturing a molded object according to claim 1, further comprising a selection step of preselecting a molding sheet for the molding material used in the molding step such that the peel strength between the molding sheet and the molded object in the separation step is within a range of 0.5 N / cm to 20 N / cm.
Citation Information
Patent Citations
Shaping-stage adhesive sheet and lamination shaping device
WO2017187800A1
Cited By
Printer head for 3D printer and its driving method
JP2026156382A