Resin composition and molded body

A resin composition with cyclic olefin resin, glass fiber, and granular filler addresses fluidity and weld strength issues, providing improved rigidity and weld strength in molded articles for diverse applications.

JP2024146460APending Publication Date: 2024-10-15ZEON CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023059365
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Conventional resin compositions lack sufficient fluidity and exhibit weak welds in molded articles, leading to reduced rigidity and weld strength, particularly in injection-molded parts.

Method used

A resin composition comprising cyclic olefin resin, glass fiber, and granular filler in specific proportions, enhancing fluidity while improving rigidity and weld strength.

Benefits of technology

The composition achieves excellent fluidity and rigidity with strong welds in molded articles, suitable for various applications including medical and analytical device components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146460000001
    Figure 2024146460000001
  • Figure 2024146460000002
    Figure 2024146460000002
Patent Text Reader

Abstract

To provide a resin composition that has excellent flowability and is capable of causing a molded body to demonstrate excellent rigidity and weld strength.SOLUTION: A resin composition includes a cyclic olefin-based resin, a glass fiber, and a granular filler. A content of the cyclic olefin-based resin is 30-90 pts.mass with respect to a total content of 100 pts.mass of the cyclic olefin-based resin and the glass fiber. A content of the granular filler is 0.05 pt.mass or more and less than 5 pts.mass with respect to a total content of 100 pts.mass of the cyclic olefin-based resin and the glass fiber.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition and a molded article. [Background technology]

[0002] 2. Description of the Related Art Conventionally, fillers have been blended into resin compositions that are materials for molded articles in order to reinforce the articles or provide various functions to the articles.

[0003] Specifically, Patent Document 1 discloses a resin composition containing a hydrogenated crystalline cyclic olefin ring-opening polymer, whiskers, and a white pigment in a specific ratio. According to Patent Document 1, the resin composition can be suitably used to obtain a light reflector that is not denatured even in a high-temperature environment and does not decrease in light reflectance. Patent Document 2 discloses a resin composition containing a crystalline hydrogenated cyclic olefin ring-opening polymer and a glass filler in a specific ratio. According to Patent Document 2, the resin composition can be used as a high dielectric constant, low dielectric loss tangent material that can be easily molded and exhibits excellent moldability. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-178580 A [Patent Document 2] JP 2013-256596 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the conventional resin composition still has room for improvement in terms of further improving the fluidity. In addition, the molded article obtained by using the conventional resin composition is also required to have a higher rigidity. In particular, the molded article formed by injection molding using the conventional resin composition may have a problem that a weld occurs at the portion where the molten resin joins in the mold, and the weld is weak (i.e., the molded article has poor weld strength).

[0006] Therefore, an object of the present invention is to provide a resin composition which has excellent flowability and is capable of providing a molded article with excellent rigidity and weld strength. Another object of the present invention is to provide a molded article having excellent rigidity and weld strength. [Means for solving the problem]

[0007] The present inventors have conducted extensive research to solve the above problems, and have found that a resin composition containing a cyclic olefin resin, glass fiber, and a granular filler in a specific ratio has excellent flowability, and that the resin composition can be used to form a molded article having excellent rigidity and weld strength, thereby completing the present invention.

[0008] That is, the present invention aims to advantageously solve the above problems, and provides the following resin compositions [1] to [3] and the following molded article [4].

[0009] [1] A resin composition comprising a cyclic olefin resin, glass fiber, and a granular filler, wherein the content of the cyclic olefin resin is 30 parts by mass or more and 90 parts by mass or less per 100 parts by mass of the total content of the cyclic olefin resin and the glass fiber, and the content of the granular filler is 0.05 parts by mass or more and less than 5 parts by mass per 100 parts by mass of the total content of the cyclic olefin resin and the glass fiber. Thus, the resin composition containing the cyclic olefin resin, the glass fiber, and the particulate filler in the above-mentioned ratio has excellent flowability. Moreover, by using the resin composition, a molded article having excellent rigidity and weld strength can be produced.

[0010] [2] The resin composition according to [1] above, wherein the average particle diameter of the granular filler is 0.01 μm or more and 0.1 μm or less. In the present invention, the "average particle size" of the particulate filler means the arithmetic mean size determined by observation under an electron microscope, and more specifically, it can be measured using the method described in the examples of this specification.

[0011] [3] The resin composition according to [1] or [2] above, wherein the content of the cyclic olefin resin is 35 parts by mass or more and 60 parts by mass or less per 100 parts by mass of the total content of the cyclic olefin resin and the glass fiber. According to a resin composition in which the ratio of the cyclic olefin resin to the glass fiber falls within the above-mentioned range, the rigidity and weld strength of the molded article can be further increased.

[0012] [4] A molded article obtained by molding the resin composition according to any one of [1] to [3] above. Thus, a molded article obtained by molding any of the above-mentioned resin compositions has excellent rigidity and weld strength. Effect of the Invention

[0013] According to the present invention, it is possible to provide a resin composition which has excellent flowability and is capable of providing a molded article with excellent rigidity and weld strength. Moreover, according to the present invention, it is possible to provide a molded article having excellent rigidity and weld strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, an embodiment of the present invention will be described in detail. The resin composition of the present invention can be used when producing the molded article of the present invention. The molded article of the present invention can be used, without particular limitation, as a component constituting a part or the whole of a medical device part or an analytical device part, for example.

[0015] (Resin composition) The resin composition of the present invention is required to contain a cyclic olefin resin, glass fiber, and a particulate filler, and may optionally contain components other than the cyclic olefin resin, glass fiber, and particulate filler (other components).

[0016] The resin composition of the present invention contains a cyclic olefin resin, glass fiber, and granular filler in a predetermined ratio, and therefore has excellent flowability. In addition, the resin composition can be used to produce a molded product having excellent rigidity and weld strength. Although the reason why the above-mentioned effects are obtained by using the resin composition of the present invention is unclear, it is presumed to be as follows.

[0017] First, the resin composition of the present invention contains a cyclic olefin resin having excellent mechanical strength and a filler (glass fiber and granular filler) capable of improving the rigidity of a molded body. It is known that when a filler is blended into a resin composition, the rigidity of the molded body can be improved, but the fluidity of the resin composition is reduced. However, the present inventors have newly discovered that blending two types of fillers having different aspect ratios, namely glass fiber and granular filler, into a cyclic olefin resin in a predetermined ratio can improve the rigidity and weld strength of a molded body without significantly reducing the fluidity of the resin composition. In other words, the resin composition of the present invention is obtained by blending glass fiber and granular filler into a cyclic olefin resin in a predetermined ratio, and therefore can satisfactorily improve the fluidity of the resin composition and the rigidity and weld strength of a molded body.

[0018] <Cyclic olefin resin> Examples of the cyclic olefin resin include a ring-opening polymer of a cyclic olefin, a hydrogenated product of a ring-opening polymer of a cyclic olefin, and a copolymer of a cyclic olefin and a chain olefin, etc. These cyclic olefin resins can be used alone or in combination of two or more kinds. From the viewpoint of further improving the flowability of the resin composition while further increasing the rigidity and weld strength of the molded article, the cyclic olefin resin is preferably a hydrogenated product of a ring-opening polymer of a cyclic olefin.

[0019] <<Ring-opening polymer of cyclic olefin>> The ring-opening polymer of a cyclic olefin is a polymer obtained by ring-opening polymerization of one or more types of cyclic olefins.

[0020] Specific examples of cyclic olefins include, but are not limited to, 1-ring (monocyclic), 2-ring, 3-ring, 4-ring, and 5 or more ring cyclic olefins, as well as derivatives thereof having a substituent on the ring.

[0021] Examples of the one-ring (monocyclic) cyclic olefin include, but are not limited to, cyclopentene, cyclohexene, cycloheptene, cyclooctene, cyclopentadiene, and 1,3-cyclohexadiene.

[0022] Examples of the two-ring cyclic olefin include, but are not limited to, bicyclo[2.2.1]hept-2-ene (common name: norbornene), 5-methyl-bicyclo[2.2.1]hept-2-ene, 5,5-dimethyl-bicyclo[2.2.1]hept-2-ene, 5-ethyl-bicyclo[2.2.1]hept-2-ene, 5-butyl-bicyclo[2.2.1]hept-2-ene, 5-ethylidene-bicyclo[2.2.1]hept-2-ene, and 5-ethylidene-bicyclo[2.2.1]hept-2-ene. ]hept-2-ene, 5-hexyl-bicyclo[2.2.1]hept-2-ene, 5-octyl-bicyclo[2.2.1]hept-2-ene, 5-octadecyl-bicyclo[2.2.1]hept-2-ene, 5-methylidene-bicyclo[2.2.1]hept-2-ene, 5-vinyl-bicyclo[2.2.1]hept-2-ene, 5-propenyl-bicyclo[2.2.1]hept-2-ene, and the like.

[0023] The three-ring cyclic olefin is not particularly limited, but may be a tricyclo[5.2.1.0 2,6 ]deca-3,8-diene (common name: dicyclopentadiene, hereafter sometimes abbreviated as "DCP"), tricyclo[5.2.1.0 2,6 ]dec-3-ene, tricyclo[6.2.1.0 2,7 ]Undeca-3,9-diene, tricyclo[6.2.1.0 2,7 ]Undeca-4,9-diene, tricyclo[6.2.1.0 2,7 ]undec-9-ene, 5-cyclopentyl-bicyclo[2.2.1]hept-2-ene, 5-cyclohexyl-bicyclo[2.2.1]hept-2-ene, 5-cyclohexenylbicyclo[2.2.1]hept-2-ene, 5-phenyl-bicyclo[2.2.1]hept-2-ene, and the like.

[0024] The 4-ring cyclic olefin is not particularly limited, but may be tetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene (also simply called "tetracyclododecene"), 9-methyltetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-ethyltetracyclo[6.2.1.13,6 .0 2,7 ]dodec-4-ene, 9-methylidenetetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-ethylidenetetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-vinyltetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-propenyl-tetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, tetracyclo[9.2.1.0 2,10 .0 3,8 ]tetradeca-3,5,7,12-tetraene (also called 1,4-methano-1,4,4a,9a-tetrahydrofluorene), tetracyclo[10.2.1.0 2,11 .0 4,9 ]Pentadeca-4,6,8,13-tetraene (also called 1,4-methano-1,4,4a,9,9a,10-hexahydroanthracene), and the like.

[0025] The cyclic olefin having five or more rings is not particularly limited, but may be, for example, (E) 9-cyclopentyl-tetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-cyclohexyl-tetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, 9-cyclohexenyl-tetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, pentacyclo[6.6.1.1 3,6 .0 2,7 .0 9,14 ]-4-Hexadecene, Pentacyclo[6.5.1.1 3,6 .0 2,7 .0 9,13 ]-4-Pentadecene, Pentacyclo[7.4.0.0 2,7 .1 3,6 .1 10,13 ]-4-pentadecene, 9-phenyl-cyclopentyl-tetracyclo[6.2.1.1 3,6 .0 2,7]dodec-4-ene, heptacyclo[8.7.0.1 2,9 .1 4,7 .1 11,17 .0 3,8 .0 12,16 ]-5-Eicosene, heptacyclo[8.7.0.1 2,9 .0 3,8 .1 4,7 .0 12,17 .1 13,16 ]-14-Eicosene and the like.

[0026] The substituent that the cyclic olefin derivative has on the ring is not particularly limited, but examples thereof include an alkyl group, an alkylene group, a vinyl group, an alkoxycarbonyl group, and an alkylidene group.

[0027] The cyclic olefin may be used alone or in combination of two or more. As the cyclic olefin, DCP is preferred from the viewpoint of further increasing the rigidity and weld strength of the resulting molded article.

[0028] The method for preparing the ring-opening polymer of the cyclic olefin is not particularly limited, and any known method for ring-opening polymerization of the above-mentioned cyclic olefin, such as metathesis polymerization, can be used.

[0029] The weight average molecular weight (Mw) of the ring-opening polymer of the cyclic olefin is not particularly limited, but is preferably 1,000 or more, more preferably 2,000 or more, and is preferably 1,000,000 or less, more preferably 500,000 or less. The molecular weight distribution (Mw / Mn) of the cyclic olefin ring-opening polymer is not particularly limited, but is preferably 1 or more and 4 or less, more preferably 1.5 or more and 3.5 or less. In the present invention, the weight average molecular weight (Mw) and number average molecular weight (Mn) of polymers such as ring-opening polymers of cyclic olefins are values ​​calculated as standard polyisoprene by gel permeation chromatography (GPC) using cyclohexane as an eluent.

[0030] <<Hydrogenated ring-opening polymers of cyclic olefins>> The hydrogenated product of the ring-opening polymer of the cyclic olefin is obtained by hydrogenating the above-mentioned ring-opening polymer of the cyclic olefin. The method for hydrogenating the ring-opening polymer of a cyclic olefin is not particularly limited, and any known method can be used. For example, a method in which a known hydrogenation catalyst containing a transition metal such as nickel or palladium is added to a solution of the ring-opening polymer of a cyclic olefin to hydrogenate the carbon-carbon double bonds in the ring-opening polymer can be mentioned. The hydrogenation rate is preferably 90% or more, more preferably 95% or more, and even more preferably 99% or more. The hydrogenation rate can be measured by the method described in the Examples of this specification.

[0031] <<Cyclic olefin and chain olefin copolymer>> The copolymer of a cyclic olefin and a chain olefin is usually a polymer obtained by addition copolymerization of a cyclic olefin and a chain olefin.

[0032] As the cyclic olefin, the same cyclic olefins as those used in the preparation of the ring-opening polymer of the cyclic olefin described above can be used. Among them, the cyclic olefin is preferably norbornene.

[0033] Specific examples of the chain olefin are not particularly limited as long as it is copolymerizable with the above-mentioned cyclic olefin, and include, for example, linear or branched olefins having 2 to 20 carbon atoms, such as ethylene, propylene, butene, pentene, hexene, butadiene, pentadiene, and hexadiene. The chain olefin may be used alone or in combination of two or more kinds. Among these, ethylene is preferred as the chain olefin.

[0034] The method for preparing the copolymer of a cyclic olefin and a chain olefin is not particularly limited, and any of the known methods for copolymerizing the above-mentioned cyclic olefin and a chain olefin can be used.

[0035] Here, the cyclic olefin resin contained in the resin composition of the present invention is preferably crystalline from the viewpoint of further increasing the rigidity of the molded article. In the present invention, the cyclic olefin resin is "crystalline" means that the melting point is detected by measurement according to differential scanning calorimetry (DSC) according to JIS K7121.

[0036] <Glass fiber> The form of the glass fiber to be blended in the resin composition of the present invention is not particularly limited, but examples thereof include chopped strands, milled fibers, filaments, cloth, staple yarns, and the like. The glass fibers may be used alone or in combination of two or more.

[0037] Here, the glass fiber contained in the resin composition of the present invention preferably has an average diameter of 5 μm or more, more preferably 10 μm or more, and preferably 20 μm or less, and more preferably 15 μm or less. If the average diameter of the glass fiber in the resin composition is equal to or greater than the lower limit, the flowability of the resin composition can be further improved. Also, if the average diameter of the glass fiber in the resin composition is equal to or less than the upper limit, the rigidity of the molded product can be further increased.

[0038] The glass fibers contained in the resin composition of the present invention preferably have an average length of 0.13 mm or more, more preferably 0.2 mm or more, even more preferably 0.26 mm or more, and preferably 3.2 mm or less, more preferably 2.6 mm or less, and even more preferably 2 mm or less. If the average length of the glass fibers in the resin composition is equal to or greater than the lower limit, the rigidity of the molded product can be further increased. If the average length of the glass fibers in the resin composition is equal to or less than the upper limit, the flowability of the resin composition can be further improved. The "average diameter" and "average length" of the glass fibers contained in the resin composition can be measured by the method described in the examples of this specification.

[0039] The aspect ratio (long axis / short axis) of the glass fiber in the resin composition is preferably 10 or more, more preferably 15 or more, and even more preferably 20 or more, and is preferably 250 or less, more preferably 200 or less, and even more preferably 150 or less. If the aspect ratio of the glass fiber in the resin composition is equal to or more than the lower limit, the rigidity of the molded article can be further increased. If the aspect ratio of the glass fiber in the resin composition is equal to or less than the upper limit, the flowability of the resin composition can be further improved. In the present invention, the "aspect ratio" of the glass fibers can be determined by calculating the ratio of the average length to the average diameter of the glass fibers (average length / average diameter).

[0040] Here, the glass fiber is preferably surface-treated. The surface treatment agent used for the surface treatment is not particularly limited, but examples thereof include silane coupling agents, unsaturated carboxylic acids or their anhydrides, etc. Examples of silane coupling agents include aminosilane, epoxysilane, methyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, vinyltriacetoxysilane, hexamethylsilane, vinyltrimethoxysilane, etc. Examples of unsaturated carboxylic acids or their anhydrides include monocarboxylic acids such as acrylic acid and methacrylic acid; dicarboxylic acids such as maleic acid, fumaric acid, and itaconic acid; dicarboxylic anhydrides such as maleic anhydride and itaconic anhydride; and the like. Among these, dicarboxylic acids and their anhydrides are preferred. The surface treatment agent can be used alone or in combination of two or more types.

[0041] <Granular filler> The particulate filler is not particularly limited, and carbon-based particulate fillers and non-carbon-based particulate fillers can be used. Examples of carbon-based granular fillers include graphite such as artificial graphite, scaly graphite, exfoliated graphite, natural graphite, acid-treated graphite, expandable graphite, and expanded graphite; and carbon black such as graphite black, Ketjen black, and black oxide. Examples of non-carbon-based granular fillers include alumina (Al2O3), talc (Mg3Si4O 10 (OH)2), calcium carbonate (CaCO3), zinc oxide (ZnO), silica (SiO2), titanium(III) oxide (Ti2O3), titanium(IV) oxide (TiO2), potassium titanate (K2O n Examples of suitable hydroxides include TiO2) [n is an integer between 1 and 12.], barium sulfate (BaSO4), antimony trioxide (Sb2O3), aluminum hydroxide (Al(OH)3), and magnesium hydroxide (Mg(OH)2). These particulate fillers can be used alone or in combination of two or more.

[0042] Among the above, as the particulate filler, from the viewpoint of further improving the flowability of the resin composition while further increasing the rigidity and weld strength of the molded body, carbon black and alumina are preferred, and carbon black is more preferred.

[0043] <<Average particle size>> Here, the average particle diameter of the granular filler is preferably 0.01 μm or more, more preferably 0.015 μm or more, and preferably 0.1 μm or less, more preferably 0.08 μm or less, and even more preferably 0.07 μm or less. If the average particle diameter of the granular filler is 0.01 μm or more, the rigidity of the molded body can be further increased. Also, if the average particle diameter of the granular filler is 0.1 μm or less, the flowability of the resin composition can be further improved.

[0044] The aspect ratio (major axis / minor axis) of the granular filler is usually 5 or less, preferably 3 or less, and more preferably 2 or less. If the aspect ratio of the granular filler is the above value or less, the fluidity of the resin composition can be further improved and the weld strength of the molded article can be further increased. The aspect ratio of the granular filler is 1 or more and may be more than 1. In the present invention, the "aspect ratio" of a granular filler can be determined by measuring the maximum diameter (long diameter) and the particle diameter (short diameter) in the direction perpendicular to the maximum diameter for any 50 granular fillers, and calculating the average ratio of the long diameter to the short diameter (long diameter / short diameter). When the diameters are uniform and the long diameter and short diameter cannot be specified, the aspect ratio is 1.

[0045] <Content of each ingredient> Here, the content of the cyclic olefin resin in the resin composition must be 30 parts by mass or more and 90 parts by mass or less per 100 parts by mass of the total content of the cyclic olefin resin and the glass fiber, preferably 35 parts by mass or more, more preferably 40 parts by mass or more, even more preferably 45 parts by mass or more, preferably 80 parts by mass or less, more preferably 70 parts by mass or less, even more preferably 60 parts by mass or less, and particularly preferably less than 55 parts by mass. If the content of the cyclic olefin resin in the resin composition is less than 30 parts by mass per 100 parts by mass of the total content of the cyclic olefin resin and the glass fiber, there is a risk that sufficient kneading cannot be performed when preparing the resin composition, and the weld strength of the molded body is reduced. On the other hand, if the content of the cyclic olefin resin in the resin composition is more than 90 parts by mass per 100 parts by mass of the total content of the cyclic olefin resin and the glass fiber, the rigidity of the molded body is reduced.

[0046] The content of the granular filler in the resin composition must be 0.05 parts by mass or more and less than 5 parts by mass per 100 parts by mass of the total content of the cyclic olefin resin and the glass fiber, and is preferably 0.06 parts by mass or more, more preferably 0.07 parts by mass or more, preferably 4 parts by mass or less, more preferably 3 parts by mass or less, and even more preferably 2 parts by mass or less. If the content of the granular filler in the resin composition is less than 0.05 parts by mass per 100 parts by mass of the total content of the cyclic olefin resin and the glass fiber, the flowability of the resin composition decreases and the weld strength of the molded product decreases. On the other hand, if the content of the granular filler in the resin composition is 5 parts by mass or more per 100 parts by mass of the total content of the cyclic olefin resin and the glass fiber, the flowability of the resin composition decreases.

[0047] <Other ingredients> The other components are not particularly limited, and may include other additives such as antioxidants, moisture-resistant agents, release agents, flame retardants, antibacterial agents, wood flour, coupling agents, plasticizers, colorants, lubricants, silicone oils, foaming agents, surfactants, thermoplastic elastomers, infrared absorbing agents, light stabilizers, etc. The other components may be used alone or in combination of two or more.

[0048] <Method for preparing resin composition> The resin composition of the present invention is not particularly limited, and can be prepared by a method that can well mix the above-mentioned essential components, cyclic olefin polymer, glass fiber, and granular filler, as well as other components that are optionally used. For example, such a method includes a method in which a mixture of cyclic olefin polymer, glass fiber, and granular filler, as well as other components that are optionally used, is fed to a melt kneader, and the cyclic olefin polymer is melted and kneaded. The obtained resin composition may be molded into pellets or the like by any method. For kneading, a melt kneader such as a single screw kneading extruder, a twin screw kneading extruder, a Banbury mixer, a kneader, a roll, a feeder ruder, etc. can be used. The kneading temperature is preferably 200° C. or higher, more preferably 240° C. or higher, and preferably 400° C. or lower, more preferably 350° C. or lower. In addition, when kneading, each component may be kneaded all at once or may be kneaded while adding it in several portions.

[0049] Here, the glass fiber may be cut by mixing when preparing the resin composition, and the aspect ratio may become shorter. In view of keeping the aspect ratio of the glass fiber in the obtained resin composition within the preferred range described above in the section "glass fiber", the aspect ratio of the glass fiber as a material used in preparing the resin composition (i.e., before mixing) is preferably 150 or more, more preferably 180 or more, and even more preferably 200 or more, and is preferably 1000 or less, more preferably 800 or less, and even more preferably 600 or less.

[0050] (Molded body) The molded article of the present invention is obtained by molding the resin composition of the present invention described above. That is, the cyclic olefin polymer, glass fiber, and particulate filler contained in the molded article of the present invention, as well as other components that are optionally used, are as described above in the "resin composition" section. In addition, the content relationship (content ratio) and attributes of the cyclic olefin polymer, glass fiber, and particulate filler contained in the molded article of the present invention are usually the same as the content relationship (content ratio) and attributes of those in the resin composition. Furthermore, the molded article of the present invention is excellent in rigidity and weld strength since it is formed from the above-mentioned resin composition of the present invention.

[0051] The molding method for producing the molded article of the present invention is not particularly limited, and can be appropriately selected from known molding methods according to the desired shape of the molded article. Examples of such known molding methods include extrusion molding, injection molding, inflation molding, blow molding, extrusion blow molding, injection blow molding, press molding, vacuum molding, powder slush molding, calendar molding, foam molding, thermoforming, etc. Among these, it is preferable to use injection molding as the molding method. EXAMPLES

[0052] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples. In the following description, "%" and "parts" expressing amounts are based on mass unless otherwise specified. In addition, in a polymer produced by polymerizing a plurality of types of monomers, the ratio of a monomer unit formed by polymerizing a certain monomer in the polymer is usually the same as the ratio (feed ratio) of the certain monomer to the total monomers used in the polymerization of the polymer, unless otherwise specified. In the examples and comparative examples, the hydrogenation rate of the cyclic olefin resin, the properties (average length, average diameter) of the glass fiber, the average particle size of the granular filler, the MFR improvement rate of the resin composition, and the flexural modulus and weld strength retention rate of the molded product were evaluated by the following methods.

[0053] <Hydrogenation rate> Using deuterated chloroform as a solvent, 1 1H-NMR measurement was performed to calculate the hydrogenation rate in the hydrogenation reaction. <Properties of glass fiber> After burning the resin compositions prepared in the examples and comparative examples at 550 °C to remove the resin components, a solvent was added to the obtained ash to elute the glass fibers, and the glass fibers were made observable by applying them to the surface of the substrate for observation. Then, the diameters (outer diameters) and lengths of 50 randomly selected glass fibers were measured using a scanning electron microscope (SEM). Then, the arithmetic mean value of the lengths of the 50 glass fibers was taken as the average length, and the arithmetic mean value of the diameters of the 50 glass fibers was calculated as the average diameter. <Average particle diameter of granular filler> After burning the resin compositions prepared in the examples and comparative examples at 550 °C to remove the resin components, a solvent was added to the obtained ash to elute the granular fillers, and the individual granular fillers were made observable by applying them to the surface of the substrate for observation. Then, the particle diameters of 50 randomly selected granular fillers were individually observed using a scanning electron microscope (SEM). A circle was drawn on the image of each obtained granular filler with a planar measurement tool, and the maximum and minimum values of the diameter of the drawn circle were measured by linear measurement. Then, the arithmetic mean value of the maximum and minimum values of the diameter was taken as the particle diameter of the granular filler, and the average value of the particle diameters of the 50 granular fillers was taken as the average particle diameter of the granular filler. <MFR improvement rate> The melt mass flow rate (MFR) of the resin compositions prepared in the examples and comparative examples was measured under the conditions of a temperature of 280 °C and a load of 2.16 kg in accordance with JIS K7210 using a melt indexer (manufactured by Toyo Seiki Co., Ltd., product name "F-F01"). Also, the melt mass flow rate (MFR) of the resin component used in the preparation of the resin composition was measured in the same manner under the same conditions. Then, with the MFR of the resin composition as P1 (g / 10 min) and the MFR of the resin component as P2 (g / 10 min), the MFR improvement rate (%) was calculated by the following formula. MFR improvement rate (%) = {(P1 - P2) / P2} × 100 A higher MFR improvement rate indicates that the resin composition has better fluidity. <Flexural modulus> The rigidity of the molded body was evaluated by the flexural modulus. Specifically, for the test pieces (1) as molded bodies prepared in the examples and comparative examples, a bending test was performed at a test speed of 2 mm / min in accordance with JIS K7171 using an autograph (manufactured by Shimadzu Corporation, product name "AGS-5kNJ·TCR2") to measure the flexural modulus (GPa). The larger the value of the flexural modulus, the more rigid the molded body is. <Weld strength retention rate> The bending strength (MPa) of the test pieces (1) and (2) as the molded bodies produced in the examples and comparative examples was measured in accordance with JIS K7171. The bending strength of the test piece (1) (test piece without a weld) was designated as FS1, and the bending strength of the test piece (2) (test piece with a weld in the center) was designated as FS2, and the weld strength retention rate (%) was calculated by the following formula. Weld strength retention rate (%)={(FS2) / (FS1)}×100 A higher value of the weld strength retention rate indicates that the molded article has better weld strength.

[0054] (Production Example 1) <Synthesis of hydrogenated product A of ring-opening polymer of cyclic olefin> In a metal pressure-resistant reaction vessel with the inside replaced with nitrogen, 154.5 parts of cyclohexane as an organic solvent, 42.8 parts of a cyclohexane solution (concentration 70%) of dicyclopentadiene (endo content 99% or more) (30 parts as dicyclopentadiene), and 1.9 parts of 1-hexene as a molecular weight regulator were added, and the total volume was heated to 53 ° C. Meanwhile, 0.014 parts of a tetrachlorotungsten phenylimide (tetrahydrofuran) complex as a metal compound as a ring-opening polymerization catalyst was dissolved in 0.70 parts of toluene (organic solvent) to obtain a solution, and 0.061 parts of an n-hexane solution (concentration 19%) of diethylaluminum ethoxide as an organometallic reducing agent as a ring-opening polymerization catalyst was added and stirred for 10 minutes to prepare a ring-opening polymerization catalyst solution. This ring-opening polymerization catalyst solution was added to the reactor, and a ring-opening polymerization reaction was carried out at 53 ° C. for 4 hours to obtain a solution containing a dicyclopentadiene ring-opening polymer. 0.037 parts of 1,2-ethanediol was added as a terminator to 200 parts of the solution containing the obtained dicyclopentadiene ring-opening polymer, and the mixture was stirred at 60°C for 1 hour to terminate the polymerization reaction. Then, 1 part of a hydrotalcite-like compound (product name "Kyoward (registered trademark) 2000", manufactured by Kyowa Chemical Industry Co., Ltd.) was added as an adsorbent, and the mixture was heated to 60°C and stirred for 1 hour. 0.4 parts of a filter aid (product name "Radiolight (registered trademark) #1500", manufactured by Showa Chemical Industry Co., Ltd.) was added, and the adsorbent was filtered out using a PP pleated cartridge filter (product name "TCP-HX", manufactured by ADVANTEC Toyo Co., Ltd.) to obtain a solution containing a dicyclopentadiene ring-opening polymer. Using a portion of this solution, the molecular weight of the dicyclopentadiene ring-opening polymer was measured, and it was found that the weight average molecular weight (Mw) was 28,100, the number average molecular weight (Mn) was 8,750, and the molecular weight distribution (Mw / Mn) was 3.21. 100 parts of cyclohexane and 0.0043 parts of chlorohydridocarbonyltris(triphenylphosphine)ruthenium were added to 200 parts of the solution containing the obtained dicyclopentadiene ring-opening polymer (polymer content 30 parts), and the hydrogenation reaction was carried out at a hydrogen pressure of 6 MPa and 180°C for 4 hours. The reaction liquid was a slurry liquid in which solids were precipitated. The reaction liquid was centrifuged to separate the solids and the solution, and the solids were dried under reduced pressure at 60°C for 24 hours to obtain 28.5 parts of a dicyclopentadiene ring-opening polymer hydrogenation product A of a ring-opening polymer of a cyclic olefin. The hydrogenation rate of unsaturated bonds in the hydrogenation reaction was 99% or more, the glass transition temperature of the dicyclopentadiene ring-opening polymer hydrogenation product was 98°C, and the melting point was 262°C. The ratio of racemo-dyads was 89%.

[0055] Example 1 <Preparation of Resin Composition> 85 parts of hydrogenated ring-opening polymer A of cyclic olefin (crystalline, hereinafter abbreviated as "COP resin A") as a cyclic olefin resin, 15 parts of glass fiber (manufactured by Nittobo Co., Ltd., product name "General-purpose chopped strand FRTP 3PE-957S", average length 3 mm, average diameter 13 μm, aspect ratio 230.8), 1.5 parts of carbon black (manufactured by Mitsubishi Chemical Corporation, product name "#10", average particle size 0.075 μm, aspect ratio 1) as a granular filler, and 0.2 parts of tetrakis [methylene-3- (3',5'-di-t-butyl-4'-hydroxyphenyl) propionate] methane as an antioxidant were mixed, and then kneaded using a twin-screw kneading extruder (manufactured by Shibaura Machine Co., Ltd., product name "TEM-35B") at 280 ° C. and 100 rpm to obtain a resin composition. The MFR improvement rate of this resin composition was evaluated, and the results are shown in Table 1. <Preparation of Molded Body> Using the obtained resin composition, test pieces (1) and (2) were prepared as molded bodies under the following conditions. Test pieces (1) and (2) were used to evaluate the weld strength retention rate, and test piece (1) was used to evaluate the flexural modulus. The results are shown in Table 1. [Preparation conditions] Injection molding machine: Manufactured by FANUC, product name "S-2000i" Cylinder temperature: 280℃ Mold temperature: 160℃ Injection speed: 30mm / sec Cooling time: 30 seconds Injection pressure (holding pressure): 30MPa Screw rotation speed: 30 rpm Back pressure: 30MPa [Test piece (1)] Test piece without welds (length 80mm x width 10mm x thickness 4mm) [Test piece (2)] Test piece with a weld in the center (length 80 mm x width 10 mm x thickness 4 mm)

[0056] Example 2 In preparing the resin composition, the amount of COP resin A used was changed from 85 parts to 60 parts, the amount of glass fiber used was changed from 15 parts to 40 parts, and carbon black (manufactured by Mitsubishi Chemical Corporation, product name "#10", average particle size 0.075 μm) was replaced with carbon black (manufactured by Mitsubishi Chemical Corporation, product name "#650", average particle size 0.022 μm) as the granular filler. The resin composition and the molded body were prepared or produced in the same manner as in Example 1. Various evaluations were then performed in the same manner as in Example 1. The results are shown in Table 1.

[0057] Example 3 A resin composition and a molded article were prepared or produced in the same manner as in Example 2, except that a copolymer C of a cyclic olefin and a chain olefin (manufactured by Polyplastics Co., Ltd., product name "TOPAS (registered trademark) 6013M", a copolymer of norbornene and ethylene, non-crystalline, hereinafter abbreviated as "COC resin C") was used instead of COP resin A when preparing the resin composition. Various evaluations were then performed in the same manner as in Example 1. The results are shown in Table 1.

[0058] Example 4 A resin composition and a molded product were prepared or produced in the same manner as in Example 2, except that a hydrogenated product B of a ring-opening polymer of a cyclic olefin (manufactured by Zeon Corporation, product name "ZEONEX (registered trademark) 690R", non-crystalline, hereinafter abbreviated as "COP resin B") was used instead of COP resin A when preparing the resin composition. Various evaluations were then performed in the same manner as in Example 1. The results are shown in Table 1.

[0059] Example 5 In preparing the resin composition, the amount of COP resin A used was changed from 60 parts to 45 parts, the amount of glass fiber used was changed from 40 parts to 55 parts, and the amount of carbon black used was changed from 1.5 parts to 0.07 parts, except that the resin composition and the molded body were prepared or produced in the same manner as in Example 2. Then, various evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0060] Example 6 In preparing the resin composition, the amount of COP resin A used was changed from 85 parts to 35 parts, the amount of glass fiber used was changed from 15 parts to 65 parts, and 0.06 parts of carbon black (manufactured by Mitsubishi Chemical Corporation, product name "#2600", average particle size 0.013 μm) was used instead of 1.5 parts of carbon black (manufactured by Mitsubishi Chemical Corporation, product name "#10", average particle size 0.075 μm) as a granular filler. Except for this, the resin composition and the molded body were prepared or produced in the same manner as in Example 1. Then, various evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0061] Example 7 A resin composition and a molded body were prepared or produced in the same manner as in Example 2, except that alumina (MKnano Corp., product name "MKN-Al-020", average particle size 0.02 μm) was used instead of carbon black (Mitsubishi Chemical Corp., product name "#650", average particle size 0.022 μm) as a granular filler when preparing the resin composition. Various evaluations were then performed in the same manner as in Example 1. The results are shown in Table 1.

[0062] Comparative Example 1 A resin composition and a molded body were prepared or produced in the same manner as in Example 1, except that glass fiber and carbon black as a particulate filler were not used when preparing the resin composition. Various evaluations were then performed in the same manner as in Example 1. The results are shown in Table 2.

[0063] Comparative Example 2 A resin composition and a molded body were prepared or produced in the same manner as in Example 2, except that the amount of carbon black used as a particulate filler was changed from 1.5 parts to 0.03 parts when preparing the resin composition. Various evaluations were then performed in the same manner as in Example 1. The results are shown in Table 2.

[0064] Comparative Example 3 A resin composition and a molded product were prepared or produced in the same manner as in Example 2, except that the amount of carbon black used as a particulate filler was changed from 1.5 parts to 12 parts when preparing the resin composition. Various evaluations were then performed in the same manner as in Example 1. The results are shown in Table 2.

[0065] Comparative Example 4 In preparing the resin composition, the amount of COP resin A used as the cyclic olefin resin was changed from 60 parts to 95 parts, and the amount of glass fiber was changed from 40 parts to 5 parts. The resin composition and the molded body were prepared or produced in the same manner as in Example 2. Then, various evaluations were performed in the same manner as in Example 1. The results are shown in Table 2.

[0066] Comparative Example 5 The resin composition was prepared in the same manner as in Example 2, except that the amount of COP resin A used as the cyclic olefin resin was changed from 60 parts to 25 parts, and the amount of glass fiber used was changed from 40 parts to 75 parts. However, sufficient kneading could not be performed during the preparation of the resin composition. Therefore, various evaluations could not be performed.

[0067] Comparative Example 6 A resin composition and a molded body were prepared or produced in the same manner as in Example 2, except that polyphenylene sulfide (PPS) resin D (manufactured by Toray Industries, Inc., product name "Toray PPS resin TORELINA (registered trademark) A900", hereinafter abbreviated as "PPS resin D") was used as another component instead of COP resin A as a cyclic olefin resin when preparing the resin composition. Then, various evaluations were performed in the same manner as in Example 1. The results are shown in Table 2.

[0068] Comparative Example 7 A resin composition and a molded body were prepared or produced in the same manner as in Example 2, except that carbon black was not used as a particulate filler when preparing the resin composition. Various evaluations were then performed in the same manner as in Example 1. The results are shown in Table 2.

[0069] In addition, in Tables 1 and 2 shown below, "COP resin A" refers to a hydrogenated product A of a ring-opening polymer of a cyclic olefin. indicates, "COP resin B" refers to the hydrogenated ring-opening polymer of cyclic olefin. indicates, "COC resin C" refers to copolymer C of cyclic olefin and chain olefin. indicates, "PPS resin D" refers to polyphenylene sulfide resin D. "CB" stands for carbon black, "Not kneadable" indicates that the resin composition could not be kneaded during preparation, and therefore evaluation could not be performed. In addition, in Tables 1 and 2, the aspect ratios of the glass fibers are expressed as values ​​rounded off to one decimal place.

[0070] [Table 1]

[0071] [Table 2]

[0072] As can be seen from Tables 1 and 2, in Examples 1 to 7, which used resin compositions containing cyclic olefin resin, glass fiber, and granular filler in specified proportions, resin compositions with excellent fluidity and molded articles with excellent rigidity and weld strength were produced. On the other hand, in Comparative Example 1, which used a resin composition that did not contain glass fibers and granular filler, and Comparative Example 4, which used a resin composition in which the ratio of cyclic olefin resin to glass fibers was outside the specified range, it was found that the fluidity of the resin composition was reduced and the rigidity of the molded body was reduced compared to Examples 1 to 7. In addition, in Comparative Examples 2 and 3, which used resin compositions in which the ratio of the particulate filler to the total of the cyclic olefin resin and glass fiber was outside the specified range, the fluidity of the resin composition was found to be reduced compared to Examples 1 to 7. Moreover, it is understood that in Comparative Example 5, in which the ratio of the cyclic olefin resin to the glass fiber is outside the predetermined range, the resin composition could not be kneaded. Furthermore, in Comparative Example 6, which used a resin composition that did not contain a cyclic olefin resin, and Comparative Example 7, which used a resin composition that did not contain a particulate filler, it can be seen that the fluidity of the resin composition was reduced and the weld strength of the molded body was reduced compared to Examples 1 to 7. [Industrial Applicability]

[0073] According to the present invention, it is possible to provide a resin composition which has excellent flowability and is capable of providing a molded article with excellent rigidity and weld strength. Moreover, according to the present invention, it is possible to provide a molded article having excellent rigidity and weld strength.

Claims

1. A resin composition comprising a cyclic olefin resin, glass fibers, and a particulate filler, the content of the cyclic olefin resin is 30 parts by mass or more and 90 parts by mass or less per 100 parts by mass of the total content of the cyclic olefin resin and the glass fiber, A resin composition in which the content of the particulate filler is 0.05 parts by mass or more and less than 5 parts by mass per 100 parts by mass of the total content of the cyclic olefin resin and the glass fiber.

2. The resin composition according to claim 1, wherein the average particle size of the particulate filler is 0.01 μm or more and 0.1 μm or less.

3. The resin composition according to claim 1, wherein the content of the cyclic olefin resin is 35 parts by mass or more and 60 parts by mass or less per 100 parts by mass of the total content of the cyclic olefin resin and the glass fiber.

4. A molded article obtained by molding the resin composition according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Cycloolefin polymer-polyphenyl ether resin composition as well as preparation method and application thereof

    CN113583393A

  • Thermoplastic resin composition

    JP1988295655A

  • Conductive composition, conductive molded product, and conductive coating

    JP2004224829A

  • Conductive resin film and method for producing the same

    JP2010077235A

  • Formed article and method for producing the same

    JP2012111872A