Granule production method
The described method addresses the challenge of continuous production in polymer fine particle processing by incorporating a spraying interruption-cleaning-spraying restart process and coagulant solution spraying, resulting in narrow particle size distribution and improved operational efficiency.
Patent Information
- Application Number
- JP2023059453
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional methods for producing powder and granular materials of polymer fine particles are not suitable for continuous implementation, leading to wider particle size distribution and operational inefficiencies.
A method involving a spraying interruption-cleaning-spraying restart process, where latex is interrupted and cleaned with water at specific pressures, combined with coagulant solution spraying to form droplets in a gas phase, allowing for continuous production of polymer fine particles.
Enables the production of polymer fine particles with a narrow particle size distribution, improving workability and reducing dust generation while maintaining high packing ratios and transportation efficiency.
Smart Images

Figure 2024146503000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing powder or granular material. [Background technology]
[0002] Powder particles of polymer fine particles are used as resin modifiers such as impact resistance modifiers, etc. As a method for producing such powder particles, for example, the technique disclosed in Patent Document 1 is known.
[0003] Furthermore, the technology of Patent Document 2 is known as a technology relating to an apparatus for producing fine particles such as toner fine particles for electrophotography. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2000-279857 A [Patent Document 2] JP 2015-027657 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the above-mentioned conventional techniques are not sufficient from the viewpoint of continuous implementation, and there is room for further improvement.
[0006] One embodiment of the present invention has been made in consideration of the above problems, and an object of the invention is to provide a novel method for producing powder or granular material that can be carried out continuously. [Means for solving the problem]
[0007] The present inventors conducted extensive research to solve the above problems and have now completed the present invention.
[0008] That is, one embodiment of the present invention includes the following configuration. [1] A method for producing a powder or granule of polymer microparticles, comprising a spraying step of spraying and / or dropping latex containing the polymer microparticles from a first sprayer, and a spraying interruption-washing-spraying restart step is carried out in the spraying step, wherein the spraying interruption-washing-spraying restart step is a step of interrupting the spraying and / or dropping of the latex from the first sprayer, spraying washing water from the first sprayer at a pressure of 0.05 MPa to 50.00 MPa, and restarting the spraying and / or dropping of the latex from the first sprayer. [2] The method for producing powder or granular material according to [1], wherein the first sprayer has a nozzle, and the orifice diameter of the nozzle is 2.3 mm to 6.0 mm. [3] The method for producing powder or granular material described in [1] or [2], wherein in the spraying step, the spraying interruption-cleaning-spraying restart steps are carried out within 50 minutes from the start of the spraying step. [4] The method for producing powder or granular material according to any one of [1] to [3], wherein in the spraying step, the spraying time of the cleaning water is 10 seconds or longer. [5] The method for producing a powder or granular material according to any one of [1] to [4], wherein the polymer fine particles have an elastomer and a graft portion grafted to the elastomer. [6] The method for producing powder or granular material according to [5], wherein the elastic body contains at least one type selected from the group consisting of diene-based rubbers, (meth)acrylate-based rubbers, and organosiloxane-based rubbers. [7] The method for producing a powder or granular material according to [5] or [6], wherein the graft portion contains one or more structural units selected from the group consisting of an aromatic vinyl unit, a vinyl cyan unit, and a (meth)acrylate unit. [8] The method for producing a powder or granular material according to any one of [1] to [7], wherein in the spraying step, a coagulant solution containing a coagulant is further sprayed and / or dropped from a second sprayer to bring the droplets of the latex into contact with the droplets of the coagulant solution in a gas phase. [9] The method for producing powder or granular material according to [8], wherein in the spraying step, the coagulant solution is sprayed in a horizontal direction.
[10] The method for producing a powder or granular material according to any one of [1] to [7], wherein in the spraying step, agglomerates of the polymer fine particles are generated by evaporating a solvent from droplets of the latex produced by spraying. Effect of the Invention
[0009] Advantageous Effects of Invention According to one aspect of the present invention, an effect is achieved in that a novel method for producing powder or granular material that can be carried out continuously can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] An embodiment of the present invention will be described below, but the present invention is not limited thereto. The present invention is not limited to each configuration described below, and various modifications are possible within the scope of the claims. In addition, embodiments or examples obtained by appropriately combining the technical means disclosed in different embodiments or examples are also included in the technical scope of the present invention. Furthermore, new technical features can be formed by combining the technical means disclosed in each embodiment. All academic documents and patent documents described in this specification are incorporated herein by reference. In addition, unless otherwise specified in this specification, "A to B" representing a numerical range means "A or more (including A and greater than A) and B or less (including B and smaller than B)".
[0011] In this specification, a "structural unit derived from an X monomer" contained in a polymer, copolymer, or resin may be referred to as an "X unit".
[0012] 2. Manufacturing method of powder and granular material A method for producing powder or granular material according to one embodiment of the present invention is a method for producing powder or granular material of polymer microparticles, comprising a spraying step of spraying and / or dropping latex containing the polymer microparticles from a first sprayer, and a spraying interruption-washing-spraying restart step is carried out in the spraying step: the spraying interruption-washing-spraying restart step is a step of interrupting the spraying and / or dropping of the latex from the first sprayer, spraying washing water from the first sprayer at a pressure of 0.05 MPa to 50.00 MPa, and restarting the spraying and / or dropping of the latex from the first sprayer.
[0013] In this specification, a "latex containing polymer microparticles" or a "latex of polymer microparticles" may be simply referred to as a "latex", an "aggregate of polymer microparticles" may be simply referred to as an "aggregate", and a "powder of polymer microparticles" may be simply referred to as a "powder". In this specification, a "production method for a powder according to one embodiment of the present invention" may be simply referred to as the "production method".
[0014] Since the present manufacturing method has the above-mentioned configuration, it has an advantage that it can be carried out continuously.
[0015] In addition to the problem that the conventional powder and granular material manufacturing method cannot be carried out continuously, the present inventor independently found that the particle size distribution of the obtained powder and granular material tends to become wider as the method is carried out continuously. The reason for this is unclear, but it is thought to be due to the gradual adhesion of scale around the nozzle. The smaller the amount of fine powder in the powder and granular material, the less dusting there is, and the better the workability and the higher the packing rate during packaging, so that the transportation cost is lower. The present inventor independently found that, surprisingly, the present manufacturing method having the above-mentioned configuration can obtain powder and granular material having a narrow particle size distribution. That is, the present manufacturing method has the above-mentioned configuration, and therefore has the advantage of being able to obtain powder and granular material having a narrow particle size distribution.
[0016] Regarding the production method of powders and granules, the following three methods are known from the viewpoint of obtaining aggregates of polymer fine particles: (1) A method of mixing latex containing polymer fine particles with a coagulant solution and coagulating the polymer fine particles in the mixed liquid; (2) A method in which a latex containing fine polymer particles and a coagulant solution are each sprayed into a gas phase, and droplets of the latex are brought into contact with droplets of the coagulant solution in the gas phase, thereby coagulating the fine polymer particles in the gas phase; (3) A method in which latex containing fine polymer particles is sprayed into a gas phase and the solvent in the latex is evaporated to coagulate the fine polymer particles in the gas phase.
[0017] In the above-mentioned methods (2) and (3), latex containing fine polymer particles is sprayed. One embodiment of the present invention can be suitably used in the above-mentioned methods (2) and (3).
[0018] In a preferred embodiment of the present invention, the method for producing powder or granular material may further include the following configuration (a) or (b); (a) the spraying step further includes spraying and / or dropping a coagulant solution containing a coagulant from a second sprayer to bring droplets of the latex into contact with droplets of the coagulant solution in a gas phase; (b) In the spraying step, the solvent is evaporated from the droplets of the latex produced by spraying, thereby forming aggregates of the polymer fine particles.
[0019] The manufacturing method having the configuration (a) may be referred to as a "first manufacturing method." That is, the first manufacturing method according to one embodiment of the present invention may have the following configuration: A method for producing a powder of polymer fine particles, comprising the steps of: A spraying step of spraying and / or dropping the latex containing the polymer fine particles from a first sprayer, In the spraying step, a spray interruption-cleaning-spraying restart step is carried out, In the spraying step, a coagulant solution containing a coagulant is further sprayed and / or dropped from a second sprayer to bring the droplets of the latex into contact with the droplets of the coagulant solution in a gas phase. Here, the spraying interruption-washing-spraying resumption process is a process of interrupting the spraying and / or dripping of the latex from the first sprayer, spraying washing water from the first sprayer at a pressure of 0.05 MPa to 50.00 MPa, and resuming the spraying and / or dripping of the latex from the first sprayer.
[0020] The manufacturing method having the configuration of (b) above may be referred to as a "second manufacturing method." That is, the second manufacturing method according to one embodiment of the present invention may have the following configuration: A method for producing a powder of polymer fine particles, comprising the steps of: A spraying step of spraying and / or dropping the latex containing the polymer fine particles from a first sprayer, In the spraying step, a spray interruption-cleaning-spraying restart step is carried out, In the spraying step, a solvent is evaporated from droplets of the latex produced by spraying to generate aggregates of the polymer fine particles. Here, the spraying interruption-washing-spraying resumption process is a process of interrupting the spraying and / or dripping of the latex from the first sprayer, spraying washing water from the first sprayer at a pressure of 0.05 MPa to 50.00 MPa, and resuming the spraying and / or dripping of the latex from the first sprayer.
[0021] In this specification, "a production method according to one embodiment of the present invention", in other words, "this production method" can be said to be a general term that encompasses both the "first production method" and the "second production method".
[0022] The raw materials (components) used in this production method will be described in detail below, and then each step of this production method will be described.
[0023] (2-1.Latex) In this specification, the term "latex" refers to a solution that includes a solvent and polymer fine particles, and in which the polymer fine particles are dispersed in the solvent. The solvent for latex is not particularly limited, but may be water, for example. Latex in which the solvent is water is sometimes called "aqueous latex." In the solvent for latex, the polymer fine particles are preferably dispersed in the form of primary particles.
[0024] The concentration (amount) of the polymer microparticles in the latex is not particularly limited, but is preferably 10% to 55% by weight, more preferably 20% to 50% by weight, even more preferably 30% to 50% by weight, and particularly preferably 30% to 40% by weight, based on 100% by weight of the latex. When the concentration of the polymer microparticles in the latex is within the above range, the resulting aggregate can provide a powder having a better bulk density. The concentration of the polymer microparticles in the latex can be adjusted by appropriately changing the amount of the solvent (e.g., water) used in the production process of the polymer microparticles and the amount of the monomer used.
[0025] The concentration of polymer particles in latex can be calculated, for example, by the following method: 0.5 g of latex is placed in a hot air convection dryer at 120°C for 3 hours to evaporate the water, the weight W(g) of the residue (solid content) after drying is measured, the obtained value (W(g)) is divided by the weight of the latex before drying, 0.5 g, and the obtained value is multiplied by 100. By such an operation, the "concentration of solid content in latex" can be calculated. The residue after drying latex, i.e., the solid content, mainly contains polymer particles, but may also contain components other than polymer particles. On the other hand, the amount of components in latex that can become solid content other than polymer particles is extremely small. Therefore, the "concentration of solid content in latex" calculated by the above-mentioned method can be regarded as the "concentration of polymer particles in latex".
[0026] The latex containing polymer fine particles can be produced by a known method, for example, an emulsion polymerization method of polymer fine particles, or a method of suspending polymer fine particles and an emulsifier in a solvent, etc. The emulsion polymerization method of polymer fine particles will be described in detail in the section (2-3. Production method of polymer fine particles) below.
[0027] (2-2. Polymer microparticles) The polymer microparticles are not particularly limited in other aspects as long as they are microparticles obtained by polymerization. The polymer microparticles may be (a) made of only one type of polymer (first polymer), or (b) made of two or more types of polymers having a second polymer covering the first polymer. In addition, these polymers may have a graft portion.
[0028] In addition to the first polymer and the second polymer covering it, the polymer microparticles may further contain other components such as other commonly used processing aids. When the polymer microparticles contain two or more types of polymers, the polymer microparticles may have a layer structure (multilayer structure), for example, each of the multiple polymers contained in the polymer microparticles may form each layer. When the polymer microparticles contain two or more types of polymers, each polymer (for example, each of the first polymer and the second polymer) may have a single-layer structure, a multilayer structure, or a combination of a single-layer structure and a multilayer structure. When the polymer microparticles contain the first polymer and the second polymer, it is preferable that the second polymer is present so as to cover at least a part of the first polymer, in other words, it is preferable that the second polymer is present outside the first polymer in the polymer microparticles. In this case, it is preferable that the first polymer and the second polymer are not chemically bonded to each other.
[0029] The polymer microparticles preferably have an elastomer and a graft portion grafted to the elastomer. A polymer having an elastomer and a graft portion grafted to the elastomer may also be called a "rubber-containing graft copolymer". That is, the polymer microparticles are preferably rubber-containing graft copolymers. When the polymer microparticles are rubber-containing graft copolymers, the polymer microparticles have the advantage of being able to exhibit suitable behavior in the manufacturing method of the present disclosure. Hereinafter, an embodiment of the present invention will be described taking the case where the polymer microparticles are rubber-containing graft copolymers as an example.
[0030] (Elastic body) The elastic body preferably contains one or more selected from the group consisting of diene rubber, (meth)acrylate rubber, and organosiloxane rubber. The elastic body may contain natural rubber in addition to the above-mentioned rubber. The elastic body may also be called an elastic portion or rubber particles.
[0031] The case where the elastomer contains a diene rubber (case A) will be described. In case A, the obtained resin composition can provide a molded article or cured product having excellent toughness and impact resistance. A molded article or cured product having excellent toughness and / or impact resistance can also be said to be a molded article or cured product having excellent durability.
[0032] The diene rubber is an elastomer containing, as a constituent unit, a constituent unit derived from a diene monomer. The diene monomer can also be called a conjugated diene monomer. In case A, the diene rubber may contain, in 100% by weight of the constituent units, 50 to 100% by weight of constituent units derived from diene monomers and 0 to 50% by weight of constituent units derived from vinyl monomers other than diene monomers copolymerizable with the diene monomers. In case A, the diene rubber may contain, as a constituent unit, a constituent unit derived from a (meth)acrylate monomer in an amount less than the constituent units derived from the diene monomers.
[0033] Examples of the diene monomer include 1,3-butadiene, isoprene (2-methyl-1,3-butadiene), 2-chloro-1,3-butadiene, etc. These diene monomers may be used alone or in combination of two or more.
[0034] Examples of vinyl monomers other than diene monomers that can be copolymerized with diene monomers (hereinafter, also referred to as vinyl monomer A) include vinyl arenes such as styrene, α-methylstyrene, monochlorostyrene, and dichlorostyrene; vinyl carboxylic acids such as acrylic acid and methacrylic acid; vinyl cyanides such as acrylonitrile and methacrylonitrile; vinyl halides such as vinyl chloride, vinyl bromide, and chloroprene; vinyl acetate; alkenes such as ethylene, propylene, butylene, and isobutylene; and polyfunctional monomers such as diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, and divinylbenzene. The above-mentioned vinyl monomer A may be used alone or in combination of two or more kinds. Among the above-mentioned vinyl monomers A, styrene is particularly preferred. In the diene rubber in case A, the constituent unit derived from the vinyl monomer A is an optional component. In case A, the diene rubber may be composed only of structural units derived from diene monomers.
[0035] In case A, the diene rubber is preferably butadiene rubber (also called polybutadiene rubber) consisting of structural units derived from 1,3-butadiene, or butadiene-styrene rubber (also called polystyrene-butadiene) which is a copolymer of 1,3-butadiene and styrene, and butadiene rubber is more preferable. According to the above configuration, the desired effect of the polymer microparticles containing the diene rubber can be more effectively exhibited. In addition, butadiene-styrene rubber is more preferable in that the transparency of the obtained molded body or cured product can be increased by adjusting the refractive index.
[0036] In one embodiment of the present invention, the elastomer preferably contains 30% by weight or more of diene rubber, more preferably 40% by weight or more, more preferably 50% by weight or more, more preferably 60% by weight or more, more preferably 70% by weight or more, preferably 80% by weight or more, even more preferably 90% by weight or more, particularly preferably 95% by weight or more, and most preferably 100% by weight. In other words, it is most preferable that the elastomer is composed only of diene rubber.
[0037] In one embodiment of the present invention, the elastomer contains butadiene rubber and / or butadiene-styrene rubber, and in 100% by weight of the elastomer, the total of butadiene rubber and butadiene-styrene rubber is preferably 30% by weight or more, more preferably 40% by weight or more, more preferably 50% by weight or more, more preferably 60% by weight or more, more preferably 70% by weight or more, more preferably 80% by weight or more, even more preferably 90% by weight or more, particularly preferably 95% by weight or more, and most preferably 100% by weight. In other words, the elastomer is most preferably composed of only butadiene rubber, only butadiene-styrene rubber, or only butadiene rubber and butadiene-styrene rubber.
[0038] The case where the elastomer contains a (meth)acrylate rubber (Case B) will be described. In Case B, a wide range of polymer designs for the elastomer are possible by combining a variety of monomers.
[0039] The (meth)acrylate rubber is an elastomer containing, as a structural unit, a structural unit derived from a (meth)acrylate monomer. In case B, the (meth)acrylate rubber may contain, in 100% by weight of structural units, 50 to 100% by weight of structural units derived from a (meth)acrylate monomer, and 0 to 50% by weight of structural units derived from a vinyl monomer other than the (meth)acrylate monomer that is copolymerizable with the (meth)acrylate monomer. In case B, the (meth)acrylate rubber may contain, as a structural unit, a structural unit derived from a diene monomer in an amount less than the structural unit derived from the (meth)acrylate monomer.
[0040] Examples of the (meth)acrylate monomer include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, dodecyl (meth)acrylate, stearyl (meth)acrylate, and behenyl (meth)acrylate; aromatic ring-containing (meth)acrylates such as phenoxyethyl (meth)acrylate and benzyl (meth)acrylate; 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and the like. Examples of the monomers include hydroxyalkyl (meth)acrylates such as acrylate; glycidyl (meth)acrylates such as glycidyl (meth)acrylate and glycidyl alkyl (meth)acrylate; alkoxyalkyl (meth)acrylates; allyl alkyl (meth)acrylates such as allyl (meth)acrylate and allyl alkyl (meth)acrylate; and polyfunctional (meth)acrylates such as monoethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, and tetraethylene glycol di(meth)acrylate. These (meth)acrylate monomers may be used alone or in combination of two or more. Among these (meth)acrylate monomers, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate are preferred, and methyl (meth)acrylate and butyl (meth)acrylate are more preferred.
[0041] In case B, the (meth)acrylate rubber is preferably one or more selected from the group consisting of methyl (meth)acrylate rubber, ethyl (meth)acrylate rubber, butyl (meth)acrylate rubber, and 2-ethylhexyl (meth)acrylate rubber, more preferably one or more selected from the group consisting of methyl (meth)acrylate rubber and butyl (meth)acrylate rubber, even more preferably one or more selected from the group consisting of butyl (meth)acrylate rubber, and particularly preferably butyl acrylate. The methyl (meth)acrylate rubber is a rubber containing 50% or more by weight of methyl (meth)acrylate units in 100% by weight of rubber, the ethyl (meth)acrylate rubber is a rubber containing 50% or more by weight of ethyl (meth)acrylate units in 100% by weight of rubber, the butyl (meth)acrylate rubber is a rubber containing 50% or more by weight of butyl (meth)acrylate units in 100% by weight of rubber, the butyl acrylate rubber is a rubber containing 50% or more by weight of butyl acrylate units in 100% by weight of rubber, and the 2-ethylhexyl (meth)acrylate rubber is a rubber containing 50% or more by weight of 2-ethylhexyl (meth)acrylate units in 100% by weight of rubber. According to this configuration, the glass transition temperature (Tg) of the elastomer is lowered, so that polymer microparticles and resin compositions with low Tg can be obtained. As a result, (i) the resulting resin composition can provide a molded article or cured product having excellent toughness, and (ii) the viscosity of the resin composition can be reduced.
[0042] In one embodiment of the present invention, the elastomer preferably contains 60% by weight or more of (meth)acrylate rubber, more preferably 70% by weight or more, more preferably 80% by weight or more, even more preferably 90% by weight or more, particularly preferably 95% by weight or more, and most preferably 100% by weight. In other words, the elastomer is most preferably composed only of (meth)acrylate rubber. This configuration has the advantage of being able to provide a molded or cured product with a good balance of physical properties such as color tone, tensile strength, impact resistance, dispersibility, and compatibility.
[0043] In one embodiment of the present invention, the elastomer preferably contains 30% by weight or more of butyl (meth)acrylate rubber, more preferably 40% by weight or more, more preferably 50% by weight or more, even more preferably 60% by weight or more, and particularly preferably 65% by weight or more, based on 100% by weight of the elastomer. This configuration has the advantage of being able to provide a molded or cured product with a good balance of physical properties such as color tone, tensile strength, impact resistance, dispersibility, and compatibility.
[0044] In one embodiment of the present invention, the elastomer preferably contains 30% by weight or more of (meth)acrylate rubber, more preferably 40% by weight or more, more preferably 50% by weight or more, more preferably 60% by weight or more, more preferably 70% by weight or more, more preferably 80% by weight or more, even more preferably 90% by weight or more, particularly preferably 95% by weight or more, and most preferably 100% by weight. In other words, the elastomer is most preferably composed only of (meth)acrylate rubber. This configuration has the advantage of being able to provide a molded or cured product with a good balance of physical properties such as color tone, tensile strength, impact resistance, dispersibility, and compatibility. Specifically, depending on the type of resin (matrix resin) into which the powder particles are to be blended, when the elastomer contains 60% by weight or more of a (meth)acrylate-based rubber out of 100% by weight of the elastomer, compared with when the elastomer contains a large amount (e.g., 60% by weight or more out of 100% by weight of the elastomer) of diene-based rubber (e.g., polybutadiene rubber), the resulting resin composition or a molded or cured product obtained from the resin composition has the advantage of being better in color, tensile strength, impact resistance, dispersibility and / or compatibility.
[0045] In one embodiment of the present invention, the elastomer preferably contains 30% by weight or more of butyl (meth)acrylate rubber, more preferably 40% by weight or more, more preferably 50% by weight or more, more preferably 60% by weight or more, more preferably 70% by weight or more, more preferably 80% by weight or more, even more preferably 90% by weight or more, particularly preferably 95% by weight or more, and most preferably 100% by weight. In other words, the elastomer is most preferably composed of only butyl (meth)acrylate rubber. This configuration has the advantage of being able to provide a molded or cured product with a good balance of physical properties such as color tone, tensile strength, impact resistance, dispersibility, and compatibility. Specifically, depending on the type of resin (matrix resin) into which the powder particles are to be blended, when the elastomer contains 60% by weight or more of butyl (meth)acrylate rubber out of 100% by weight of the elastomer, compared with when the elastomer contains a large amount (e.g., 60% by weight or more out of 100% by weight of the elastomer) of diene rubber (e.g., polybutadiene rubber), the resulting resin composition or a molded or cured product obtained from the resin composition has the advantage of being better in color, tensile strength, impact resistance, dispersibility and / or compatibility.
[0046] Examples of vinyl monomers other than (meth)acrylate monomers copolymerizable with (meth)acrylate monomers (hereinafter also referred to as vinyl monomer B) include the monomers listed in the vinyl monomer A. Only one type of vinyl monomer B may be used, or two or more types may be used in combination. Among the vinyl monomers B, styrene is particularly preferred. In the (meth)acrylate rubber in case B, the constituent unit derived from the vinyl monomer B is an optional component. In case B, the (meth)acrylate rubber may be composed only of constituent units derived from (meth)acrylate monomers.
[0047] The case where the elastomer contains an organosiloxane-based rubber (Case C) will be described below. In Case C, the resulting resin composition can provide a molded article or cured product having sufficient heat resistance and excellent impact resistance at low temperatures.
[0048] Examples of organosiloxane rubbers include (i) organosiloxane polymers composed of alkyl or aryl disubstituted silyloxy units, such as dimethylsilyloxy, diethylsilyloxy, methylphenylsilyloxy, diphenylsilyloxy, and dimethylsilyloxy-diphenylsilyloxy, and (ii) organosiloxane polymers composed of alkyl or aryl monosubstituted silyloxy units, such as organohydrogensilyloxy in which a portion of the alkyl in the side chain is replaced with a hydrogen atom. These organosiloxane polymers may be used alone or in combination of two or more.
[0049] In this specification, a polymer composed of dimethylsilyloxy units is referred to as dimethylsilyloxy rubber, a polymer composed of methylphenylsilyloxy units is referred to as methylphenylsilyloxy rubber, and a polymer composed of dimethylsilyloxy units and diphenylsilyloxy units is referred to as dimethylsilyloxy-diphenylsilyloxy rubber. In case C, the organosiloxane rubber is preferably one or more selected from the group consisting of dimethylsilyloxy rubber, methylphenylsilyloxy rubber, and dimethylsilyloxy-diphenylsilyloxy rubber, since (i) the resin composition containing the obtained powdery material can provide a molded product or cured product having excellent heat resistance, and (ii) dimethylsilyloxy rubber is more preferable, since it is easily available and economical.
[0050] In one embodiment of the present invention, the elastomer preferably contains 30% by weight or more of organosiloxane rubber, more preferably 40% by weight or more, more preferably 50% by weight or more, more preferably 60% by weight or more, more preferably 70% by weight or more, more preferably 80% by weight or more, even more preferably 90% by weight or more, particularly preferably 95% by weight or more, and most preferably 100% by weight. In other words, it is most preferable that the elastomer is composed only of organosiloxane rubber. According to the above-mentioned configuration, the obtained resin composition can provide a molded body or cured product having excellent heat resistance.
[0051] (Elastomeric bridge structure) From the viewpoint of maintaining the dispersion stability of the polymer microparticles in the thermosetting resin, it is preferable that a crosslinked structure is introduced into the elastomer. A commonly used method can be adopted as a method for introducing a crosslinked structure into the elastomer, and examples thereof include the following methods. That is, in the production of the elastomer, a method is exemplified in which a crosslinkable monomer such as a multifunctional monomer and / or a mercapto group-containing compound is mixed with a monomer capable of constituting the elastomer, and then polymerized. In this specification, the production of a polymer such as an elastomer is also referred to as polymerizing a polymer.
[0052] Methods for introducing a crosslinked structure into an organosiloxane rubber include the following: (A) a method of using a polyfunctional alkoxysilane compound in combination with other materials when polymerizing an organosiloxane rubber; (B) a method of introducing reactive groups (e.g., (i) a mercapto group and (ii) a reactive vinyl group, etc.) into an organosiloxane rubber, and then adding (i) an organic peroxide or (ii) a polymerizable vinyl monomer, etc., to the resulting reaction product to cause a radical reaction; and (C) a method of mixing a crosslinkable monomer such as a polyfunctional monomer and / or a mercapto group-containing compound with other materials when polymerizing an organosiloxane rubber, and then polymerizing the rubber.
[0053] A polyfunctional monomer can be said to be a monomer having two or more radically polymerizable reactive groups in the same molecule. The radically polymerizable reactive group is preferably a carbon-carbon double bond. Examples of polyfunctional monomers include (meth)acrylates having ethylenically unsaturated double bonds, such as allyl alkyl (meth)acrylates and allyloxy alkyl (meth)acrylates, and do not include butadiene. Examples of monomers having two (meth)acrylic groups include ethylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate, butane diol di(meth)acrylate, hexane diol di(meth)acrylate, cyclohexane dimethanol di(meth)acrylate, and polyethylene glycol di(meth)acrylates. Examples of the polyethylene glycol di(meth)acrylates include triethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, and polyethylene glycol (600) di(meth)acrylate. Examples of monomers having three (meth)acrylic groups include alkoxylated trimethylolpropane tri(meth)acrylates, glycerol propoxy tri(meth)acrylate, pentaerythritol tri(meth)acrylate, and tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate. Examples of the alkoxylated trimethylolpropane tri(meth)acrylates include trimethylolpropane tri(meth)acrylate and trimethylolpropane triethoxy tri(meth)acrylate. Further, examples of monomers having four (meth)acrylic groups include pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, etc. Further, examples of monomers having five (meth)acrylic groups include dipentaerythritol penta(meth)acrylate, etc. Further, examples of monomers having six (meth)acrylic groups include ditrimethylolpropane hexa(meth)acrylate, etc.Polyfunctional monomers also include diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, divinylbenzene, and the like.
[0054] Among the above-mentioned polyfunctional monomers, polyfunctional monomers that can be preferably used for introducing a crosslinked structure into the elastomer include allyl methacrylate, ethylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate (e.g., 1,3-butylene glycol dimethacrylate, etc.), butanediol di(meth)acrylate, hexanediol di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate, and polyethylene glycol di(meth)acrylates. These polyfunctional monomers may be used alone or in combination of two or more.
[0055] (Volume average particle size of elastic body) The volume average particle diameter of the elastic body is preferably 0.03 μm to 50.00 μm, more preferably 0.05 μm to 10.00 μm, more preferably 0.08 μm to 2.00 μm, even more preferably 0.10 μm to 1.00 μm, even more preferably 0.10 μm to 0.80 μm, and particularly preferably 0.10 μm to 0.50 μm. When the volume average particle diameter of the elastic body is (i) 0.03 μm or more, an elastic body having a desired volume average particle diameter can be stably obtained, and (ii) when it is 50.00 μm or less, the heat resistance and impact resistance of the obtained molded body or cured product become good. The volume average particle diameter of the elastic body can be measured using a dynamic light scattering type particle size distribution measuring device or the like, using an aqueous latex containing the elastic body as a sample. The method for measuring the volume average particle diameter of the elastic body will be described in detail in the following examples.
[0056] (Ratio of elastic body) The proportion of the elastomer in the polymer microparticles is preferably 40 to 97% by weight, more preferably 60 to 95% by weight, and even more preferably 70 to 93% by weight, based on 100% by weight of the entire polymer microparticles. When the proportion of the elastomer is (i) 40% by weight or more, the resulting resin composition can provide a molded article or cured product having excellent toughness and impact resistance, and (ii) when the proportion is 97% by weight or less, the polymer microparticles do not easily aggregate, so that the resin composition does not become highly viscous, and as a result, the resulting resin composition can be easy to handle.
[0057] In one embodiment of the present invention, the "elastic body" of the polymer microparticles may consist of only one type of elastomer having the same composition of constitutional units.
[0058] (Graft part) The graft moiety preferably contains one or more structural units selected from the group consisting of aromatic vinyl units, vinylcyan units, and (meth)acrylate units. The graft moiety having such a structure can play various roles. The "various roles" include, for example, (i) improving the compatibility between the polymer microparticles and the matrix resin, (ii) improving the dispersibility of the polymer microparticles in the matrix resin, and (iii) enabling the polymer microparticles to be dispersed in the form of primary particles in a resin composition containing a matrix resin and polymer microparticles (hereinafter also simply referred to as "resin composition"), or in a molded product or cured product thereof.
[0059] Specific examples of monomers from which the aromatic vinyl units are derived include styrene, α-methylstyrene, p-methylstyrene, and divinylbenzene.
[0060] Specific examples of monomers from which vinylcyan units are derived include acrylonitrile and methacrylonitrile.
[0061] Specific examples of monomers from which (meth)acrylate units are derived include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, hydroxyethyl (meth)acrylate, and hydroxybutyl (meth)acrylate, etc. In this specification, (meth)acrylate refers to acrylate and / or methacrylate.
[0062] The one or more monomers selected from the group consisting of the aromatic vinyl monomer, the vinyl cyan monomer, and the (meth)acrylate monomer may be used alone or in combination of two or more.
[0063] The graft portion preferably contains 10 to 95% by weight of aromatic vinyl units, vinylcyan units and (meth)acrylate units in total, based on 100% by weight of the graft portion, more preferably 30 to 92% by weight, even more preferably 50 to 90% by weight, particularly preferably 60 to 87% by weight, and most preferably 70 to 85% by weight.
[0064] The graft portion preferably contains, as a constituent unit, a constituent unit derived from a monomer having a reactive group. The monomer having a reactive group is preferably a monomer having one or more reactive groups selected from the group consisting of an epoxy group, an oxetane group, a hydroxyl group, an amino group, an imide group, a carboxylic acid group, a carboxylic anhydride group, a cyclic ester, a cyclic amide, a benzoxazine group, and a cyanate ester group, more preferably a monomer having one or more reactive groups selected from the group consisting of an epoxy group, a hydroxyl group, and a carboxylic acid group, and most preferably a monomer having an epoxy group. According to the above configuration, the graft portion of the polymer fine particles can be chemically bonded to the matrix resin in the resin composition. This allows the polymer fine particles to be maintained in a good dispersion state without agglomerating in the resin composition or in a molded or cured product thereof.
[0065] Specific examples of monomers having an epoxy group include glycidyl group-containing vinyl monomers such as glycidyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, and allyl glycidyl ether.
[0066] Specific examples of monomers having a hydroxyl group include, for example, (i) hydroxy linear alkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate (particularly, hydroxy linear C1-6 alkyl (meth)acrylates); (ii) caprolactone-modified hydroxy (meth)acrylates; (iii) hydroxy branched alkyl (meth)acrylates such as α-(hydroxymethyl)methyl acrylate and α-(hydroxymethyl)ethyl acrylate; and (iv) hydroxyl group-containing (meth)acrylates such as mono(meth)acrylates of polyester diols (particularly saturated polyester diols) obtained from divalent carboxylic acids (such as phthalic acid) and dihydric alcohols (such as propylene glycol).
[0067] Specific examples of the monomer having a carboxylic acid group include monocarboxylic acids such as acrylic acid, methacrylic acid, and crotonic acid, and dicarboxylic acids such as maleic acid, fumaric acid, and itaconic acid. As the monomer having a carboxylic acid group, the above-mentioned monocarboxylic acids are preferably used.
[0068] The above-mentioned monomers having a reactive group may be used alone or in combination of two or more kinds.
[0069] The graft portion preferably contains 0.5% by weight to 90.0% by weight of a structural unit derived from a monomer having a reactive group, more preferably 1.0% by weight to 50.0% by weight, even more preferably 2.0% by weight to 35.0% by weight, and particularly preferably 3.0% by weight to 20.0% by weight, based on 100% by weight of the graft portion. When the graft portion contains (i) 0.5% by weight or more of a structural unit derived from a monomer having a reactive group, the resulting resin composition can provide a molded article or cured product having sufficient impact resistance, and (ii) when the graft portion contains 90.0% by weight or less, the resulting resin composition can provide a molded article or cured product having sufficient impact resistance, and has the advantage of having good storage stability of the resin composition.
[0070] The structural unit derived from a monomer having a reactive group is preferably contained in the graft portion, and more preferably contained only in the graft portion.
[0071] The graft portion may contain a structural unit derived from a polyfunctional monomer as a structural unit. When the graft portion contains a structural unit derived from a polyfunctional monomer, it has the following advantages: (i) swelling of the polymer fine particles in the resin composition can be prevented, (ii) the viscosity of the resin composition is reduced, so that the handleability of the resin composition tends to be improved, and (iii) the dispersibility of the polymer fine particles in the matrix resin is improved.
[0072] When the graft portion does not contain a structural unit derived from a polyfunctional monomer, the resulting resin composition can provide a molded article or cured product that is more excellent in toughness and impact resistance, compared to when the graft portion contains a structural unit derived from a polyfunctional monomer.
[0073] Specific examples of the polyfunctional monomer are the same as those explained in the section (Elastomer) above, so the explanation therefor is incorporated by reference and will not be repeated here.
[0074] Among the polyfunctional monomers, polyfunctional monomers that can be preferably used for polymerization of the graft portion include allyl methacrylate, ethylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate, and polyethylene glycol di(meth)acrylates. These polyfunctional monomers may be used alone or in combination of two or more.
[0075] The graft portion preferably contains 1 to 20% by weight, and more preferably 5 to 15% by weight, of structural units derived from polyfunctional monomers, based on 100% by weight of the graft portion.
[0076] In the polymerization of the graft portion, the above-mentioned monomers may be used alone or in combination of two or more. The graft portion may contain, as a constituent unit, a constituent unit derived from another monomer in addition to the constituent unit derived from the above-mentioned monomer.
[0077] In one embodiment of the present invention, the graft portion may be composed of only one type of graft portion having structural units of the same composition. In one embodiment of the present invention, the graft portion may be composed of multiple types of graft portions each having a structural unit of a different composition.
[0078] The graft portion may cover at least a portion of the elastic body, or may cover the entire elastic body. A portion of the graft portion may penetrate into the inside of the elastic body. It is preferable that at least a portion of the graft portion covers at least a portion of the elastic body. In other words, it is preferable that at least a portion of the graft portion is present on the outermost side of the polymer microparticle.
[0079] The polymer microparticles may form a layer structure. For example, one embodiment of the present invention is one in which the elastomer forms the innermost layer (also referred to as a core layer) and a layer of the graft portion is formed as the outermost layer (also referred to as a shell layer) on the outside of the elastomer. A structure in which the elastomer forms the core layer and the graft portion forms the shell layer can also be called a core-shell structure. In one embodiment of the present invention, the polymer microparticles may have a core-shell structure.
[0080] (Surface crosslinked polymer) The rubber-containing graft copolymer preferably further has a surface cross-linked polymer in addition to the elastomer and the graft portion grafted to the elastomer. In other words, the polymer microparticle preferably further has a surface cross-linked polymer in addition to the elastomer and the graft portion grafted to the elastomer. Hereinafter, an embodiment of the present invention will be described taking as an example a case where the polymer microparticle (e.g., rubber-containing graft copolymer) further has a surface cross-linked polymer. In this case, (i) the blocking resistance can be improved in the production of the polymer microparticles, and (ii) the dispersibility of the polymer microparticles in the thermosetting resin becomes better. The reasons for this are not particularly limited, but can be assumed as follows: By covering at least a part of the elastomer with the surface cross-linked polymer, the exposure of the elastomer part of the polymer microparticles is reduced, and as a result, the elastomers are less likely to stick to each other, and the dispersibility of the polymer microparticles is improved.
[0081] When the polymer microparticles have a surface-crosslinked polymer, they can also have the following effects: (i) the effect of reducing the viscosity of the resin composition, (ii) the effect of increasing the crosslink density in the elastomer, and (iii) the effect of increasing the graft efficiency of the grafted portion. The crosslink density in the elastomer refers to the degree of the number of crosslinked structures in the entire elastomer.
[0082] The surface cross-linked polymer is composed of a polymer containing, as structural units, 30 to 100% by weight of structural units derived from polyfunctional monomers and 0 to 70% by weight of structural units derived from other vinyl monomers, totaling 100% by weight.
[0083] The polyfunctional monomer that can be used for the polymerization of the surface cross-linked polymer includes the same monomer as the polyfunctional monomer described above. Among these polyfunctional monomers, the polyfunctional monomer that can be preferably used for the polymerization of the surface cross-linked polymer includes allyl methacrylate, ethylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate (e.g., 1,3-butylene glycol dimethacrylate, etc.), butanediol di(meth)acrylate, hexanediol di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate, and polyethylene glycol di(meth)acrylates. These polyfunctional monomers may be used alone or in combination of two or more.
[0084] The polymer microparticles may contain a surface cross-linked polymer polymerized independently of the polymerization of the rubber-containing graft copolymer, or may contain a surface cross-linked polymer polymerized together with the rubber-containing graft copolymer. The polymer microparticles may be a multi-stage polymer obtained by multi-stage polymerization of an elastomer, a surface cross-linked polymer, and a graft portion in this order. In any of these embodiments, the surface cross-linked polymer can cover at least a part of the elastomer.
[0085] The surface cross-linked polymer can be regarded as a part of the elastomer. In other words, the surface cross-linked polymer can be regarded as a part of the rubber-containing graft copolymer, and can also be called a surface cross-linked polymerization part. When the polymer microparticles contain a surface cross-linked polymer, the graft part may be (i) grafted to an elastomer other than the surface cross-linked polymer, (ii) grafted to a surface cross-linked polymer, or (iii) grafted to both an elastomer other than the surface cross-linked polymer and a surface cross-linked polymer. When the polymer microparticles contain a surface cross-linked polymer, the volume average particle diameter of the elastomer mentioned above refers to the volume average particle diameter of the elastomer containing the surface cross-linked polymer.
[0086] The case where the polymer microparticle is a multi-stage polymer obtained by multi-stage polymerization of an elastomer, a surface cross-linked polymer, and a graft portion in this order (case D) will be described. In case D, the surface cross-linked polymer may cover a part of the elastomer, or may cover the whole of the elastomer. In case D, a part of the surface cross-linked polymer may penetrate into the inside of the elastomer. In case D, the graft portion may cover a part of the surface cross-linked polymer, or may cover the whole of the surface cross-linked polymer. In case D, a part of the graft portion may penetrate into the inside of the surface cross-linked polymer. In case D, the elastomer, the surface cross-linked polymer, and the graft portion may have a layer structure. For example, an embodiment in which the elastomer is the innermost layer (core layer), a layer of the surface cross-linked polymer exists outside the elastomer as an intermediate layer, and a layer of the graft portion exists outside the surface cross-linked polymer as an outermost layer (shell layer) is also one embodiment of the present invention.
[0087] (Volume average particle size of polymer particles (Mv)) The volume average particle diameter (Mv) of the polymer microparticles is preferably 0.03 μm to 50.00 μm, more preferably 0.05 μm to 10.00 μm, more preferably 0.08 μm to 2.00 μm, even more preferably 0.10 μm to 1.00 μm, even more preferably 0.10 μm to 0.80 μm, and particularly preferably 0.10 μm to 0.50 μm, since a resin composition having a desired viscosity and high stability can be obtained. When the volume average particle diameter (Mv) of the polymer microparticles is within the above range, there is also an advantage that the dispersibility of the polymer microparticles in the matrix resin is improved. In this specification, the "volume average particle diameter (Mv) of the polymer microparticles" refers to the volume average particle diameter of the primary particles of the polymer microparticles, unless otherwise specified. The volume average particle diameter of the polymer microparticles can be measured using a dynamic light scattering particle size distribution measuring device or the like, using an aqueous latex containing the polymer microparticles as a sample.
[0088] (2-3. Method for producing polymer microparticles) An example of a method for producing polymer microparticles will be described below, taking as an example a case where the polymer microparticles are a rubber-containing graft copolymer having an elastomer and a graft portion grafted to the elastomer. The polymer microparticles can be produced, for example, by polymerizing an elastomer, and then graft polymerizing a polymer constituting the graft portion to the elastomer in the presence of the elastomer.
[0089] The polymer microparticles can be produced by known methods, such as emulsion polymerization, suspension polymerization, and microsuspension polymerization. Specifically, the polymerization of the elastomer in the polymer microparticles and the polymerization of the graft portion (graft polymerization) can be carried out by known methods, such as emulsion polymerization, suspension polymerization, and microsuspension polymerization. Among these, the emulsion polymerization method is particularly preferred as a method for producing polymer microparticles. By producing polymer microparticles by emulsion polymerization, latex (e.g., aqueous latex) containing polymer microparticles can be obtained. In this specification, the latex obtained by emulsion polymerization may be referred to as "emulsion-polymerized latex". The emulsion polymerization method has the advantages of (i) easy composition design of polymer microparticles, (ii) easy industrial production of polymer microparticles, and (iii) easy production of latex suitable for use in this production method.
[0090] When emulsion polymerization is employed as a method for producing polymer fine particles, a known emulsifier (dispersant) can be used as the emulsifier (dispersant) for producing the polymer fine particles.
[0091] The emulsifier used in the production of polymer microparticles is not particularly limited, but examples thereof include anionic emulsifiers, nonionic emulsifiers, polyvinyl alcohol, alkyl-substituted cellulose, polyvinylpyrrolidone, polyacrylic acid derivatives, etc. Examples of the anionic emulsifier include sulfur-based emulsifiers, phosphorus-based emulsifiers, sarcosinic acid-based emulsifiers, and carboxylic acid-based emulsifiers. Examples of the sulfur-based emulsifier include sodium dodecylbenzenesulfonate (abbreviation: SDBS). Examples of the phosphorus-based emulsifier include sodium polyoxyethylene lauryl ether phosphate. Examples of the sarcosinic acid-based emulsifier include sodium N-lauroyl sarcosinate. Examples of the carboxylic acid-based emulsifier include alkyl ether carboxylates.
[0092] In the method for producing polymer microparticles, the emulsifier is preferably one or more selected from the group consisting of sulfur-based emulsifiers, phosphorus-based emulsifiers, sarcosinic acid-based emulsifiers, and carboxylic acid-based emulsifiers, more preferably one or more selected from the group consisting of sodium dodecylbenzenesulfonate, polyoxyethylene lauryl ether sodium phosphate, sodium N-lauroyl sarcosinate, and alkyl ether carboxylates, even more preferably one or more selected from the group consisting of sodium dodecylbenzenesulfonate, polyoxyethylene lauryl ether sodium phosphate, sodium N-lauroyl sarcosinate, and alkyl ether carboxylates, and particularly preferably sodium N-lauroyl sarcosinate. This configuration has the advantage of high emulsifying power.
[0093] When a polyfunctional monomer is used in the polymerization of the elastomer or the graft portion for the purpose of introducing a crosslinked structure into the elastomer or the graft portion, a known chain transfer agent can be used in a known amount range. By using the chain transfer agent, the molecular weight and / or degree of crosslinking of the obtained elastomer or the graft portion can be easily adjusted.
[0094] In the production of the polymer microparticles, in addition to the above-mentioned components, a surfactant may be further used. The type and amount of the surfactant used are within the known ranges.
[0095] In the production of polymer microparticles, the polymerization conditions such as polymerization temperature, pressure, and deoxidation may be appropriately set within known numerical ranges.
[0096] A latex containing polymer fine particles can be obtained by the above-mentioned method for producing polymer fine particles. That is, the description in the section (Method for producing polymer fine particles) can be used as a description regarding the method for producing latex.
[0097] (2-4. Washing water) The washing water is not particularly limited, but may be, for example, water.
[0098] In the first manufacturing method, the washing water may be water (aqueous solution) containing a coagulant, but the smaller the amount of coagulant in the washing water, the more preferable it is to reduce the risk of the polymer microparticles coagulating and clogging. In the first manufacturing method, the concentration (amount) of the coagulant in the washing water is, for example, preferably 10% by weight or less, more preferably 1% by weight or less, even more preferably 0.1% by weight or less, and particularly preferably 0.01% by weight or less, based on the total amount of the washing water (100% by weight). This configuration has the advantage that the sprayer (e.g., the nozzle of the sprayer) is less likely to be clogged.
[0099] The cleaning water preferably does not contain an organic solvent. Specifically, the amount of the organic solvent in the cleaning water is preferably 10% by weight or less, more preferably 1% by weight or less, even more preferably 0.1% by weight or less, and particularly preferably 0.01% by weight or less, based on the total amount of the cleaning water (100% by weight). This configuration has the advantage that the sprayer (e.g., the nozzle of the sprayer) is less likely to be clogged.
[0100] (2-5. Coagulant solution) In the first manufacturing method, a coagulant solution containing a coagulant is sprayed and / or dropped from the second sprayer. The "coagulant solution" used in the first manufacturing method refers to a liquid coagulant and a solution containing a solvent and a coagulant. In this specification, the coagulant solution according to one embodiment of the present invention (the coagulant solution used in the first manufacturing method) may be referred to as "the present coagulant solution". In the present coagulant solution, the coagulant may be dispersed or dissolved in the solvent.
[0101] In this specification, a liquid coagulant refers to a liquid substance that functions as a coagulant (i.e., a substance in which the solute itself is liquid without being dissolved or dispersed in a solvent). When using a liquid substance as a coagulant, the substance (coagulant) may be used after being dissolved or dispersed in a solvent to form a solution, or the substance (coagulant) may be used (sprayed) as a coagulant solution without being dissolved or dispersed in a solvent. In other words, the "coagulant solution" in the first manufacturing method also includes the liquid substance itself that functions as a coagulant.
[0102] When a solution containing a solvent and a coagulant is used as the coagulant solution, the solvent for the coagulant solution is not particularly limited, but may be, for example, water.
[0103] The coagulant contained in the coagulant solution may be any substance that has the property of coagulating and coagulating polymer particles in a solution containing latex and additives. Examples of the coagulant include (i) inorganic acids (salts) and / or organic acids (salts) and (ii) polymer coagulants. One of these coagulants may be used alone, or two or more may be used in combination. In this specification, inorganic acids (salts) mean "inorganic acids and their salts," and organic acids (salts) mean "organic acids and their salts."
[0104] The coagulant solution is preferably an aqueous solution containing one or more substances selected from the group consisting of monovalent inorganic acids, salts of monovalent inorganic acids, divalent inorganic acids, salts of divalent inorganic acids, trivalent inorganic acids, salts of trivalent inorganic acids, etc. as coagulants. Examples of monovalent inorganic acids include (a) halogen acids such as chloric acid, bromic acid, and iodic acid, and (b) nitric acid, etc. Examples of divalent inorganic acids include sulfuric acid, etc. Examples of trivalent inorganic acids include phosphoric acid, etc. Examples of cationic elements or molecules that can form salts with these inorganic acids include alkali metals, alkaline earth metals, transition metals (especially iron and zinc), metals of Group 13 such as aluminum, and ammonium, etc.
[0105] The coagulant solution preferably contains, as a coagulant, one or more substances selected from the group consisting of monovalent organic acids, monovalent organic acid salts, divalent organic acids, divalent organic acid salts, etc. Examples of monovalent organic acids include formic acid, acetic acid, etc. Examples of monovalent organic acid salts include salts of formic acid, acetic acid, etc. with alkali metals, etc. Examples of divalent organic acids include oxalic acid, malic acid, maleic acid, malonic acid, tartaric acid, etc. Examples of divalent organic acid salts include salts of acetic acid, formic acid, etc. with alkaline earth metals, etc.
[0106] (i) Specific examples of inorganic acids (salts) and / or organic acids (salts) include: (a) Alkali metal halides, such as sodium chloride, potassium chloride, lithium chloride, sodium bromide, potassium bromide, lithium bromide, potassium iodide, and sodium iodide; alkali metal sulfides, such as potassium sulfate, sodium sulfate, and ammonium sulfate; ammonium chloride; alkali metal nitrates, such as sodium nitrate, potassium nitrate, and other inorganic salts, such as calcium chloride, ferrous sulfate, magnesium sulfate, zinc sulfate, copper sulfate, barium chloride, ferrous chloride, ferric chloride, magnesium chloride, ferric sulfate, aluminum sulfate, potassium alum, and iron alum; (b) Inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid, and phosphoric acid; (c) organic acids such as acetic acid, formic acid, and the like; and (d) Organic acid salts such as sodium acetate, calcium acetate, sodium formate, calcium formate, and the like, and salts of these organic acids;
[0107] The polymer coagulant is not particularly limited as long as it is a polymer compound having a hydrophilic group and a hydrophobic group. Examples of the polymer coagulant include anionic polymer coagulants, cationic polymer coagulants, and nonionic polymer coagulants. Among these, cationic polymer coagulants are preferred because they have the advantage of neutralizing the charge of the polymer particles.
[0108] The cationic polymer coagulant is preferably a polymer coagulant having a cationic group in the molecule, that is, a polymer coagulant that exhibits cationicity when dissolved in water. Specific examples of cationic polymer coagulants include polyamines, polydicyandiamides, cationic starch, cationic poly(meth)acrylamide, water-soluble aniline resins, polythiourea, polyethyleneimine, quaternary ammonium salts, polyvinylpyridines, chitosan, etc.
[0109] As the coagulant, among those mentioned above, (a) an aqueous solution of a monovalent or divalent inorganic acid salt such as sodium chloride, potassium chloride, sodium sulfate, ammonium chloride, calcium chloride, magnesium chloride, magnesium sulfate, or barium chloride, or (b) an aqueous solution of a monovalent or divalent inorganic acid such as hydrochloric acid or sulfuric acid, can be preferably used, since it can provide a powder or grain having a higher bulk density and a smaller amount of fine powder.
[0110] The concentration (amount) of the coagulant in the coagulant solution is not particularly limited, but for example, in the total amount of the coagulant solution (100% by weight), it is preferably 0.1% by weight to 45.0% by weight, more preferably 5.0% by weight to 40.0% by weight, even more preferably 10.0% by weight to 40.0% by weight, even more preferably 20.0% by weight to 40.0% by weight, and particularly preferably 30.0% by weight to 40.0% by weight. According to this configuration, the coagulant is more likely to exert its coagulation action on the polymer fine particles, and the amount of coagulant used in the second contact step can be reduced. As a result, there is an advantage that the production cost of the aggregate and powder can be reduced, and the amount of impurities derived from the coagulant contained in the obtained aggregate and powder can be reduced.
[0111] When the coagulant is a substance in a solid (e.g., powder) state, the concentration (wt%) of the coagulant in the coagulant solution can be calculated, for example, by the following method: 0.5 g of the coagulant solution is placed in a hot air convection dryer at a temperature higher than the boiling point of the solvent (e.g., the boiling point of the solvent + 20°C) for 3 hours to evaporate the solvent. Then, the weight (g) of the residue (solid content) after drying is measured. Next, the obtained value is divided by the weight of the coagulant solution before drying, 0.5 g, and the obtained value is further multiplied by 100. In addition, when the coagulant is in a liquid state, the concentration of the coagulant in the coagulant solution can also be measured by performing fractional distillation.
[0112] The coagulant solution can be obtained, for example, by mixing a solid (e.g., powder) substance that functions as a coagulant with a solvent. When mixing multiple types of coagulants, each coagulant may be (a) mixed with the solvent all at once, or (b) mixed individually. In addition, a commercially available coagulant that is dissolved or dispersed in a solvent in advance may be (a) used as it is as a coagulant solution, or (b) further mixed with a solvent before use.
[0113] (2-6. Equipment) The apparatus used in the present production method (hereinafter, sometimes referred to as production apparatus or apparatus) is not particularly limited, but may be an apparatus equipped with a container having a substantially vertical inner wall. The container includes at least a gas phase region. In this specification, the vertically extending inner wall of the container may be referred to as a "side wall." The container preferably includes a first sprayer on the upper portion (top) or side wall surface of the container for spraying and / or dropping latex into the gas phase.
[0114] In the first manufacturing method, the container preferably further includes a second sprayer on the upper portion (top) or side wall surface of the container for spraying and / or dropping a coagulant solution containing a coagulant into the gas phase. In the first manufacturing method, in the gas phase region, latex containing polymer fine particles is sprayed and / or dropped from the first sprayer, and further, coagulant solution containing a coagulant is sprayed and / or dropped from the second sprayer. Thereby, in the first manufacturing method, droplets of latex and droplets of coagulant solution come into contact with each other in the gas phase. As a result, in the first manufacturing method, aggregates of polymer fine particles may be generated in the gas phase.
[0115] The shape of the container is not particularly limited, but is preferably cylindrical. When the container is cylindrical, the diameter thereof is preferably, for example, 30 cm to 500 cm.
[0116] In the first production method, the container may have a receiving tank having a liquid phase region at the bottom. In the first production method, when the container has a receiving tank having a liquid phase region, the aggregates of polymer microparticles generated in the gas phase may fall into the liquid phase of the receiving tank. In other words, in the first production method, the aggregates may be collected in the liquid phase. In the first production method, when the container has a receiving tank having a liquid phase region, the height from the top of the container to the liquid level of the liquid phase in the receiving tank at the bottom is preferably 50 cm to 10 m, more preferably 1 m to 5 m, and even more preferably 2 m to 3 m, from the viewpoint of appropriately progressing coagulation of the polymer microparticles in the latex in the gas phase.
[0117] In the second production method, the height from the top of the container to the bottom surface of the bottom is preferably 50 cm to 10 m, more preferably 1 m to 5 m, and even more preferably 2 m to 3 m, from the viewpoint of appropriately progressing drying.
[0118] In the first manufacturing method, the container may be connected, as necessary, to a recovery device for recovering the obtained agglomerate from the container, a drying device for drying the recovered agglomerate to obtain a powder or granular product, and a temperature control device for controlling the temperature inside the container or the temperature of each solution and liquid phase sprayed and / or dropped into the container.
[0119] In the second production method, the container may be connected, as necessary, to a recovery device for recovering the obtained aggregate from the container, a temperature control device for controlling the temperature inside the container or the temperature of the latex sprayed and / or dropped into the container, and the like.
[0120] (2-7.Liquid phase) As described above, in the first manufacturing method, the container may have a receiving tank having a liquid phase region at the bottom. The liquid phase is not particularly limited, but may be, for example, water or water (aqueous solution) containing a coagulant. The liquid phase may be a coagulant solution. In other words, the liquid phase may contain a coagulant.
[0121] The coagulant that the liquid phase may contain is preferably a coagulant contained in the coagulant solution sprayed and / or dropped from the second sprayer. The coagulant that the liquid phase may contain may be a different type of coagulant from the coagulant contained in the coagulant solution sprayed and / or dropped from the second sprayer.
[0122] The concentration (amount) of the coagulant in the liquid phase is not particularly limited, but is preferably lower than the concentration (amount) of the coagulant in the coagulant solution sprayed and / or dropped from the second sprayer. This configuration has the advantage of reducing the amount of remaining impurities contained in the aggregate.
[0123] The concentration (amount) of the coagulant in the liquid phase is, for example, preferably 0.01% by weight to 5.00% by weight, more preferably 0.05% by weight to 4.00% by weight, even more preferably 0.10% by weight to 3.00% by weight, even more preferably 0.25% by weight to 2.00% by weight, and particularly preferably 0.50% by weight to 1.50% by weight, based on the total amount of the liquid phase (100% by weight). This configuration has the advantage of being able to reduce the amount of residual impurities contained in the aggregate.
[0124] In the first manufacturing method, a case where the container is provided with a receiving tank having a liquid phase region (hereinafter also referred to as "Case E") will be described. In Case E, as described above, the aggregates generated in the gas phase drop in the gas phase and enter the liquid phase. More specifically, in Case E, the combined droplets formed after the latex droplets and the coagulant solution droplets come into contact with each other in the gas phase may contain aggregates of polymer fine particles, and the droplets drop in the gas phase and enter the liquid phase. Therefore, in Case E, after the start of the contact step, the liquid phase may contain uncoagulated polymer fine particles, aggregates of polymer fine particles, components other than the polymer fine particles contained in the latex (including the solvent of the latex), the coagulant, and components other than the coagulant contained in the coagulant solution (including the solvent of the coagulant solution).
[0125] (2-9. Contact process) The present production method includes a spraying step of spraying and / or dropping a latex containing fine polymer particles from a first sprayer. In the spraying step, it is preferable to spray and / or drop the latex from the first sprayer into a gas phase.
[0126] In this specification, "spraying" a liquid (e.g., latex and coagulant solution) means spraying (spraying in mist) the liquid in a state where the liquid is compressed, ultrasonically treated, or otherwise formed into droplets (microdroplets) smaller than the diameter of the nozzle (hole) of a sprayer (e.g., a sprayer nozzle) that sprays the liquid. In this specification, "dripping" a liquid (e.g., latex and coagulant solution) means spraying the liquid as droplets having a diameter similar to the diameter of the nozzle (hole) of a sprayer that sprays the liquid without any particular treatment. Note that when spraying a liquid using a two-fluid nozzle, even if the liquid itself to be sprayed is not pressurized, the liquid is considered to be "sprayed" when a substance other than the liquid (e.g., a gas) is sprayed simultaneously in a pressurized state to spray the liquid in the form of microdroplets.
[0127] In the contact step, when the latex is sprayed, the direction of spraying is not particularly limited and may be vertical, horizontal or oblique. In the contact step, when the latex is dropped, the latex is usually dropped in a vertical direction, but is not limited thereto. In the contact step, it is preferable to spray and / or drop the latex in a vertical direction, since this has the advantage that the aggregates can be easily collected.
[0128] In this specification, the term "vertical direction" refers to the "weight direction." The "vertical direction" can also be referred to as the "vertical downward direction."
[0129] In one embodiment of the present invention, when liquid (e.g., latex and coagulant solution) is "sprayed and / or dropped in a vertical direction", it is not necessary to spray and / or drop the liquid in a completely vertical direction. For example, the liquid may be sprayed and / or dropped in a direction inclined within a range of 15°, 10°, or 5° with respect to the vertical direction. That is, "sprayed and / or dropped in a vertical direction" in this specification is a concept including the aspect of spraying and / or dropping at an angle to the vertical direction. In this specification, the direction in which the liquid (e.g., latex and coagulant solution) is sprayed and / or dropped can be said to be the direction in which the nozzle of the sprayer that sprays or drops the liquid faces. In other words, the direction in which the liquid is sprayed or dropped can be adjusted by adjusting the direction in which the nozzle of the sprayer that sprays or drops the liquid faces.
[0130] In this specification, the term "horizontal direction" refers to a direction perpendicular to the vertical direction. The "horizontal direction" can also be said to be a direction perpendicular to the weight direction.
[0131] In one embodiment of the present invention, when a liquid (e.g., latex, an additive solution, or a coagulant solution) is "sprayed (or dripped) in a horizontal direction," the liquid does not necessarily have to be sprayed (or dripped) in a completely horizontal direction, and may be sprayed (or dripped) in a direction tilted within a range of 15°, 10°, or 5° from the horizontal direction as a reference. In other words, "sprayed (or dripped) in a horizontal direction" in this specification includes a mode in which the liquid is sprayed (or dripped) at an angle relative to the horizontal direction in this manner.
[0132] In the first manufacturing method, in the contact step, a coagulant solution containing a coagulant is further sprayed and / or dropped from a second sprayer. In the first manufacturing method, it is preferable to spray and / or drop the coagulant solution from the second sprayer into the gas phase. In the first manufacturing method, latex containing polymer fine particles is sprayed and / or dropped from a first sprayer in the gas phase of the container, and further, a coagulant solution containing a coagulant is sprayed and / or dropped from a second sprayer, so that the droplets of the latex and the droplets of the coagulant solution can be brought into contact with each other in the gas phase. The droplets of latex and the droplets of the coagulant solution that have come into contact with each other in the gas phase can be integrated (united).
[0133] In the contact step of the first manufacturing method, in addition to spraying and / or dropping latex into the gas phase, a coagulant solution is further sprayed and / or dropped into the gas phase. Therefore, the contact step in the first manufacturing method can be said to be (a) a step of integrating (unifying) droplets of latex and droplets of coagulant solution in the gas phase, (b) a step of obtaining droplets containing latex and coagulant solution, or (c) a step of preparing droplets containing latex and coagulant solution in the gas phase. In the first manufacturing method, the droplets containing latex and coagulant solution obtained in the contact step can be said to be "droplets of latex and coagulant solution integrated together" or "droplets of a solution containing polymer fine particles derived from latex and a coagulant derived from the coagulant solution".
[0134] In the contact step in the first production method, the polymer microparticles may be coagulated in droplets formed by combining the latex and the coagulant solution in the gas phase. In the contact step in the first production method, aggregates of the polymer microparticles may be generated in the gas phase. Therefore, the contact step in the first production method can be said to be a step of coagulating the polymer microparticles, or a step of preparing aggregates of the polymer microparticles.
[0135] Also, in the first manufacturing method, in case E, as described above, the aggregates generated in the gas phase fall through the gas phase together with the droplets containing the aggregates, and enter (fall into) the liquid phase provided at the bottom of the container. As a result, in case E, a suspension containing the liquid phase, the aggregates of polymer microparticles, and the coagulant is obtained. Therefore, in case E, the contact step can also be said to be a step of preparing a suspension.
[0136] In the contact step of the first production method, when the coagulant solution is sprayed, the direction of spraying is not particularly limited and may be vertical, horizontal or oblique. In the contact step, when the coagulant solution is dropped, the coagulant solution is usually dropped in a vertical direction, but is not limited thereto. In the contact step, it is preferable to spray the coagulant solution in a horizontal direction, since this has the advantage of efficiently contacting the coagulant droplets with the latex droplets.
[0137] The first sprayer used in the contact step is not particularly limited as long as it can spray and / or drop the latex. The first sprayer is preferably equipped with a nozzle (a device equipped with a nozzle), and is preferably, for example, a pressure nozzle, a two-fluid nozzle, an ultrasonic nozzle, a high-frequency device, or a drop nozzle. In particular, in the first production method, the first sprayer is preferably equipped with a nozzle. On the other hand, in the second production method, the first sprayer may be a device capable of spraying a liquid by rotation, such as an atomizer.
[0138] The first atomizer is preferably located at the top of the container.
[0139] The number of the first sprayers is not particularly limited and may be one or more than one. When two or more nozzles are used as the first sprayers, (a) each nozzle may only spray latex, (b) each nozzle may only drip latex, or (c) at least one nozzle may spray latex while at least another nozzle drips latex.
[0140] In the first manufacturing method, since droplets having a volume average droplet diameter of 200 μm to 400 μm and a sharp particle size distribution can be easily sprayed and the method is economically superior among nozzles capable of spraying such droplets, the first sprayer is preferably equipped with a nozzle, more preferably a pressurized nozzle, and even more preferably a swirl-type pressurized nozzle (swirl-type nozzle).
[0141] In the present manufacturing method, when the first sprayer is equipped with a nozzle, the orifice diameter of the nozzle is not particularly limited. The orifice diameter of the nozzle is preferably 2.3 mm to 6.0 mm, more preferably 3.0 mm to 5.8 mm, further preferably 4.0 mm to 5.5 mm, and particularly preferably 4.4 mm to 5.4 mm. When the orifice diameter of the nozzle is 2.3 mm or more, there is an advantage that nozzle clogging can be suppressed. When the orifice diameter of the nozzle is 6.0 mm or less, there is an advantage that a powder having a relatively narrow particle size distribution can be obtained.
[0142] In the present manufacturing method, when the first sprayer is equipped with a nozzle, the minimum foreign matter passing diameter of the nozzle is not particularly limited. The minimum foreign matter passing diameter of the nozzle is preferably 2.3 mm to 6.0 mm, more preferably 2.3 mm to 5.5 mm, even more preferably 2.3 mm to 5.0 mm, and particularly preferably 2.3 mm to 4.5 mm. When the minimum foreign matter passing diameter of the nozzle is 2.3 mm or more, there is an advantage that nozzle clogging can be suppressed. When the minimum foreign matter passing diameter of the nozzle is 6.0 mm or less, there is an advantage that a powder having a relatively narrow particle size distribution can be obtained. In this specification, the "minimum foreign matter passing diameter of the nozzle" refers to the narrowest diameter of the solution flow path in the nozzle.
[0143] In the first manufacturing method, the spray pressure of the first sprayer is, for example, 0.5 kg / cm 2 ~30.0kg / cm 2 and preferably 1.0 kg / cm 2 ~10.0kg / cm 2In the first manufacturing method, it is more preferable that the spray pressure of the first sprayer is 0.5 kg / cm. 2 If the spray pressure of the first sprayer is 30.0 kg / cm or more, the droplets of the sprayed latex do not become excessively large, and the polymer fine particles in the droplets containing the latex and the coagulant solution obtained in the contact step can be sufficiently aggregated, so that a powder having a high bulk density can be obtained. 2 If the amount is equal to or less than this, there is no risk that the droplets of the sprayed latex will become excessively small, and the amount of fine powder in the resulting powder or granule can be reduced.
[0144] In the first production method, the tip angle of the spray cone of the latex sprayed and / or dropped from the first sprayer is not particularly limited, but is preferably 5° to 140°, and more preferably 30° to 90°. In the first production method, when the angle of the spray cone of the latex is in the above range, (i) aggregates can be produced efficiently, and (ii) excessive enlargement of the apparatus used for producing the aggregates can be suppressed. Furthermore, (iii) by setting the tip angle of the spray cone to 5° or more, it is possible to suppress the coalescence of the sprayed and / or dropped droplets of latex, and (iv) by setting the tip angle of the spray cone to 140° or less, it is possible to suppress the adhesion of the sprayed and / or dropped droplets of latex to the wall surface of the apparatus for producing the aggregates, and since it is not necessary to enlarge the apparatus in order to prevent the adhesion of the latex droplets to the wall surface, the apparatus can be made smaller. In this specification, the term "spray cone" refers to a collection of droplets of a liquid sprayed and / or dropped from the outlet of a sprayer, which is observed when the liquid is sprayed and / or dropped from the nozzle of the sprayer. In the first production method, the shape of the spray cone of the latex is not particularly limited, and may be, for example, a fan shape, a cone shape, or a hollow cone shape.
[0145] In the first production method, the volume average droplet diameter of the latex droplets sprayed and / or dropped in the contact step is preferably 50 μm to 5 mm, more preferably 100 μm to 800 μm, even more preferably 150 μm to 600 μm, and particularly preferably 200 μm to 400 μm. In the first production method, if the volume average droplet diameter of the latex droplets sprayed and / or dropped is 50 μm or more, the amount of fine powder in the obtained powder or granule can be reduced. In addition, in the first production method, if the volume average droplet diameter of the latex droplets sprayed and / or dropped is 5 mm or less, the polymer fine particles in the droplets containing the latex and coagulant solution obtained in the contact step can be sufficiently aggregated, and as a result, a powder or granule with a high bulk density can be obtained.
[0146] Hereinafter, a case where a device equipped with a nozzle is used as the first sprayer in the second manufacturing method (hereinafter also referred to as "Case G") will be described.
[0147] In case G, the shape of the spray cone of the latex is not particularly limited, but since a sufficient residence time for drying can be ensured, the shape of the spray cone of the latex is more preferably a fan shape, a cone shape, or a hollow cone shape, and particularly preferably a hollow cone shape.
[0148] In case G, the diameter of the nozzle of the first sprayer is not particularly limited, but is preferably 2.3 mm to 6.0 mm, more preferably 2.5 mm to 5.8 mm, and even more preferably 2.7 mm to 5.5 mm. When the diameter of the nozzle is 6.0 mm or less, it is advantageous that a powder having a relatively narrow particle size distribution can be obtained. In addition, when the diameter of the nozzle is 2.3 mm or more, it is advantageous that nozzle clogging can be suppressed.
[0149] In case G, the spray pressure of the first sprayer is, for example, 0.5 kg / cm 2 ~30.0kg / cm 2 and preferably 1.0 kg / cm 2 ~10.0kg / cm2 In case G, the spray pressure of the first sprayer is 0.5 kg / cm 2 In the case where the spray pressure of the first sprayer is 30.0 kg / cm or more, there is an advantage that the sprayed droplets of latex do not become excessively large, and a sufficient residence time for drying in the device can be secured. 2 When the ratio is equal to or less than 1, there is no risk that the droplets of the sprayed latex will become excessively small, and there is an advantage that the amount of fine powder in the resulting powder or granule can be reduced.
[0150] In case G, the tip angle of the spray cone of the latex sprayed and / or dropped from the first sprayer is not particularly limited, but is preferably 5° to 160°, and more preferably 30° to 150°. In case G, when the tip angle of the spray cone is 5° or more, it has an advantage that the sprayed and / or dropped droplets of latex can be prevented from coalescing with each other. In case G, when the tip angle of the spray cone is 160° or less, it has an advantage that the sprayed and / or dropped droplets of latex can be prevented from adhering to the wall surface of the apparatus for producing the dried product, and since there is no need to enlarge the apparatus in order to prevent the latex droplets from adhering to the wall surface, the apparatus can be made smaller.
[0151] In the contact step in case G, the volume average droplet diameter of the sprayed and / or dropped latex droplets is preferably 50 μm to 5 mm, more preferably 100 μm to 800 μm, further preferably 150 μm to 600 μm, and particularly preferably 200 μm to 400 μm. In the contact step in case G, when the volume average droplet diameter of the sprayed and / or dropped latex droplets is 50 μm or more, there is an advantage that the amount of fine powder in the obtained powder or granule can be reduced. In addition, in the contact step in case G, when the volume average droplet diameter of the sprayed and / or dropped latex droplets is 5 mm or less, there is an advantage that the size of the apparatus can be suppressed.
[0152] Hereinafter, a case where an atomizer is used as the first sprayer in the second manufacturing method (hereinafter also referred to as "Case H") will be described.
[0153] In Case H, the spray angle of the sprayed and / or dropped latex is not particularly limited, but is preferably 90° to 180°, and more preferably 100° to 180°. In Case H, when the spray angle is 90° or more, there is an advantage that the droplets of the sprayed and / or dropped latex can be prevented from coalescing. In Case H, when the spray angle is 180° or less, there is an advantage that the residence time required for drying can be sufficiently secured.
[0154] In case H, the rotation speed of the rotating disk of the atomizer is not particularly limited, but is preferably 1000 rpm to 20000 rpm, and more preferably 3000 rpm to 18000 rpm. In case H, when the rotation speed is 1000 rpm or more, it is advantageous that the sprayed and / or dropped latex droplets can be prevented from becoming excessively enlarged, and therefore the residence time required for drying can be sufficiently secured. In case H, when the rotation speed is 20000 rpm or less, it is advantageous that the sprayed and / or dropped latex droplets can be prevented from becoming excessively fine, and therefore the amount of fine powder of the obtained powder or granule can be reduced.
[0155] In the contact step in Case H, the volume average droplet diameter of the sprayed and / or dropped latex droplets is preferably 50 μm to 5 mm, more preferably 100 μm to 800 μm, further preferably 150 μm to 600 μm, and particularly preferably 200 μm to 400 μm. In the contact step in Case H, when the volume average droplet diameter of the sprayed and / or dropped latex droplets is 50 μm or more, there is an advantage that the amount of fine powder in the obtained powder or granule can be reduced. In addition, in the contact step in Case H, when the volume average droplet diameter of the sprayed and / or dropped latex droplets is 5 mm or less, there is an advantage that the size of the apparatus can be suppressed.
[0156] In this specification, the vertical distance between the center of the nozzle of the first sprayer and the liquid level of the liquid phase at the bottom of the container is referred to as the "vertical distance between the first sprayer and the liquid phase." When there are multiple first sprayers, the shortest (closest) value among the vertical distances between the center of the nozzle of each first sprayer and the liquid level of the liquid phase at the bottom of the container is referred to as the vertical distance between the first sprayer and the liquid phase.
[0157] In the first production method, the vertical distance between the first sprayer and the liquid phase is preferably 100 cm or more, more preferably 150 cm or more, and particularly preferably 200 cm or more, because a sufficient solidification time can be ensured and a powder having better powder properties can be provided. From the viewpoint of preventing the device from becoming excessively large, the upper limit of the vertical distance between the first sprayer and the liquid phase is preferably 300 cm or less.
[0158] In the second manufacturing method, the vertical distance between the first sprayer and the liquid phase is preferably 100 cm or more, more preferably 150 cm or more, and particularly preferably 200 cm or more. This configuration has the advantage of ensuring sufficient drying time to remove moisture from the droplets. In addition, in the second manufacturing method, from the viewpoint of preventing the device from becoming excessively large, the upper limit of the vertical distance between the first sprayer and the liquid phase is preferably 500 cm or less.
[0159] The second sprayer used in the contact step of the first production method will be described. The second sprayer is not particularly limited as long as it can spray the coagulant solution, but is preferably a pressure nozzle (one-fluid nozzle), a two-fluid nozzle, an ultrasonic nozzle or a high-frequency device, and more preferably a pressure nozzle (one-fluid nozzle) or a two-fluid nozzle. When a pressure nozzle (one-fluid nozzle) or a two-fluid nozzle is used as the second sprayer, it is possible to spray the coagulant solution with fine droplets (in the form of aerosol) into the gas phase, and it is possible to efficiently contact the droplets of latex with the droplets of the coagulant solution.
[0160] The diameter of the second sprayer is not particularly limited, but is preferably 0.01 mm to 2.00 mm, more preferably 0.05 mm to 1.50 mm, and even more preferably 0.10 mm to 1.00 mm. If the diameter is 2.00 mm or less, there is no risk that the droplets of the sprayed coagulant solution will become excessively large, and the polymer fine particles in the droplets containing the latex and the coagulant solution can be sufficiently aggregated, resulting in a powder with a high bulk density. In addition, if the diameter is 0.01 mm or more, the possibility of the nozzle being blocked during spraying of the coagulant solution can be reduced, and the aggregates can be stably produced.
[0161] The spray pressure of the second sprayer is, for example, preferably 0.5 kg / cm2 to 100.0 kg / cm2, more preferably 1.0 kg / cm2 to 50.0 kg / cm2. If the spray pressure of the second sprayer is 0.5 kg / cm2 or more, there is no risk that the droplets of the sprayed coagulant solution will become excessively large, and the droplets of latex and the droplets of the coagulant solution can be efficiently contacted. As a result, a powder with a high bulk density can be obtained. Also, if the spray pressure of the second sprayer is 100.0 kg / cm2 or less, the droplets of the coagulant solution do not scatter excessively, and can be efficiently contacted with the droplets containing latex and the coagulant solution, and adhesion of the coagulant solution to the wall surface of the container can be reduced.
[0162] The second sprayer is preferably installed on (or near) the side wall of the container.
[0163] In this specification, the vertical distance between the center of the nozzle of the second sprayer and the liquid level of the liquid phase at the bottom of the container is referred to as the "vertical distance between the second sprayer and the liquid phase." When there are multiple second sprayers, the shortest (closest) value among the vertical distances between the center of the nozzle of each second sprayer and the liquid level of the liquid phase at the bottom of the container is referred to as the vertical distance between the second sprayer and the liquid phase.
[0164] In order to ensure a sufficient solidification time and provide a powder having superior powder characteristics, the vertical distance between the second sprayer and the liquid phase is preferably 50 cm or more, and more preferably 60 cm or more. The vertical distance between the second sprayer and the liquid phase may be 70 cm or more, 80 cm or more, 90 cm or more, or 100 cm or more. In order to prevent the device from becoming excessively large, the upper limit of the vertical distance between the second sprayer and the liquid phase is preferably 280 cm or less, and more preferably 250 cm or less.
[0165] In the first manufacturing method, the vertical distance between the first sprayer and the second sprayer is not particularly limited. Since the latex droplets and the coagulant solution droplets can be efficiently contacted with each other, the vertical distance between the first sprayer and the second sprayer is preferably 5 cm to 50 cm, more preferably 10 cm to 40 cm, even more preferably 15 cm to 35 cm, more preferably 15 cm to 30 cm, and particularly preferably 15 cm to 25 cm.
[0166] In the first manufacturing method, the horizontal distance between the first sprayer and the second sprayer is not particularly limited. From the viewpoint of (a) efficiently contacting the latex droplets with the coagulant solution droplets and (b) preventing the device from becoming excessively large, the horizontal distance between the first sprayer and the second sprayer in the first manufacturing method is preferably 50 cm or less, and may be 30 cm or less.
[0167] In this specification, the "vertical distance between the first sprayer and the second sprayer" and the "horizontal distance between the first sprayer and the second sprayer" are values measured by the following method: (1) draw a vertical line passing through the center of the nozzle (hole) of the first sprayer (first line); (2) draw a horizontal line (perpendicular to the vertical direction) passing through the center of the nozzle (hole) of the second sprayer (second line); (3) The vertical distance between the intersection of the first line and the second line and the center of the nozzle of the first sprayer is defined as the "vertical distance between the first sprayer and the second sprayer", and the horizontal distance between the intersection of the first line and the second line and the center of the nozzle of the second sprayer is defined as the "horizontal distance between the first sprayer and the second sprayer". In addition, when there are multiple outlets to be compared in distance (for example, when there are multiple first sprayers and multiple second sprayers), the shortest (closest) value among the distances between sprayers of different types is determined to be the distance between the sprayers.
[0168] In the first manufacturing method, when the first sprayer and the second sprayer are both installed at or near the top of the container, the horizontal distance between the first sprayer and the second sprayer can be 0.
[0169] In the first manufacturing method, the tip angle of the spray cone of the coagulant solution sprayed from the second sprayer is not particularly limited, but is preferably 5° to 140°, and more preferably 30° to 90°. In the first manufacturing method, when the angle of the spray cone of the coagulant solution is in the above range, (i) the droplets containing the latex and the additive solution can be efficiently contacted with the droplets of the coagulant solution, so that the aggregates can be efficiently manufactured, and (ii) the excessive size of the device used for manufacturing the aggregates can be suppressed. Furthermore, in the first manufacturing method, (iii) in particular, by setting the tip angle of the spray cone to 5° or more, it is also possible to suppress the droplets of the sprayed coagulant solution from coalescing with each other. In addition, in the first manufacturing method, the shape of the spray cone of the coagulant solution is not particularly limited, and may be, for example, a fan shape, a cone shape, or a hollow cone shape.
[0170] In the first production method, the number of the second sprayers is not particularly limited, and may be one, or two or more.
[0171] In the first manufacturing method, the volume average droplet diameter of the droplets of the coagulant solution sprayed in the contact step is preferably 0.01 μm to 500.00 μm, more preferably 0.05 μm to 100.00 μm, and even more preferably 0.10 μm to 50.00 μm. According to the above configuration, the droplets of latex and the droplets of the coagulant solution can be efficiently contacted with each other, and the polymer fine particles in the droplets containing the latex and the coagulant solution can be sufficiently aggregated. As a result, there is an advantage that a powder having a high bulk density can be obtained.
[0172] The volume average droplet diameter of the latex droplets and the coagulant solution droplets can be measured, for example, by a laser diffraction type spray droplet diameter measuring device.
[0173] In the contact step of the first production method, the amount of coagulant to be brought into contact with the droplets of latex can be appropriately adjusted depending on the type (composition) of the polymer fine particles, the type of coagulant, the concentration of the polymer fine particles in the latex, and the concentration of the coagulant in the coagulant solution, etc. In this specification, the "amount of coagulant to be brought into contact with the droplets of latex" means the amount of coagulant in the coagulant solution sprayed per unit time relative to the total amount of the polymer fine particles in the latex sprayed and / or dropped per unit time in the contact step. Since there are advantages that (a) the generation of unagglomerated polymer fine particles can be prevented, more aggregates of polymer fine particles can be obtained, and (b) the amount of coagulant-derived impurities contained in the obtained aggregates and powder can be reduced, in the first production method, the amount of coagulant to be contacted with the droplets of latex is preferably 1 to 30 parts by weight, more preferably 2 to 20 parts by weight, and even more preferably 3 to 15 parts by weight, relative to 100 parts by weight of the total amount of polymer fine particles in the latex sprayed and / or dropped per unit time. Note that the "amount of coagulant to be contacted with the droplets of latex" in the contact step can be adjusted by appropriately changing the concentration of the coagulant in the coagulant solution, the amount of the coagulant solution sprayed per unit time, etc.
[0174] In the first production method, the temperature of the latex when subjected to the contact step (immediately before spraying and / or dropping) is not particularly limited. The temperature of the latex when subjected to the contact step is, for example, preferably 1°C to 100°C, more preferably 1°C or higher and less than 100°C, more preferably 5°C to 80°C, even more preferably 10°C to 70°C, even more preferably 15°C to 50°C, and particularly preferably 20°C to 30°C. In the first production method, when the temperature of the latex when subjected to the contact step is within the above range, there is an advantage that the stability of the latex can be ensured.
[0175] In the second production method, the temperature of the latex when it is subjected to the contact step (immediately before spraying and / or dropping) is not particularly limited. The temperature of the latex when it is subjected to the contact step is, for example, preferably 1°C to 100°C, more preferably 1°C or more and less than 100°C, more preferably 5°C to 80°C, even more preferably 10°C to 70°C, even more preferably 15°C to 50°C, and particularly preferably 20°C to 30°C. In the second production method, when the temperature of the latex when it is subjected to the contact step is within the above range, there is an advantage that the stability of the latex can be ensured.
[0176] In the first manufacturing method, the temperature of the coagulant solution when it is subjected to the contact step (immediately before spraying and / or dropping) is not particularly limited. In the first manufacturing method, the temperature of the coagulant solution when it is subjected to the contact step is, for example, preferably 1°C to 100°C, more preferably 1°C or more and less than 100°C, more preferably 5°C to 80°C, even more preferably 10°C to 70°C, even more preferably 15°C to 50°C, and particularly preferably 20°C to 30°C. In addition, in the first manufacturing method, the temperature of the coagulant solution when it is subjected to the contact step may be the same as or different from the temperature of the latex when it is subjected to the contact step. In the first manufacturing method, when the temperature of the coagulant solution when it is subjected to the contact step is within the above range, there are advantages such as (a) the advantage that the precipitation of the coagulant in the coagulant solution can be suppressed, and (b) the advantage that the evaporation of the solvent of the coagulant solution can be suppressed, and the concentration of the coagulant solution can be kept constant.
[0177] In the first production method, the temperature inside the container (the temperature of the gas phase region) in the contact step is not particularly limited, but for example, it is preferably 1°C to 100°C, more preferably 1°C or higher and less than 100°C, more preferably 10°C to 95°C, more preferably 20°C to 95°C, more preferably 30°C to 90°C, more preferably 40°C to 90°C, more preferably 50°C to 85°C, even more preferably 60°C to 85°C, even more preferably 70°C to 85°C, and particularly preferably 75°C to 85°C. In the first production method, when the temperature in the container in the contact step is within the above range, the polymer fine particles in the droplets containing the latex and the coagulant solution can be sufficiently aggregated, and as a result, a powder having a high bulk density can be obtained. In the first production method, the temperature in the container in the contact step can be controlled, for example, by supplying water vapor into the container.
[0178] In the second production method, the temperature inside the container in the contact step (temperature of the gas phase region) is not particularly limited, but is, for example, preferably 100° C. to 200° C., more preferably 100° C. to 190° C., even more preferably 100° C. to 180° C., even more preferably 100° C. to 170° C., and particularly preferably 100° C. to 160° C. In the second production method, when the temperature inside the container in the contact step is within the above range, there is an advantage that the water in the droplets can be evaporated.
[0179] In the first manufacturing method, in the contact step, water may be allowed to flow down along the side wall surface of the container. This can prevent the latex and coagulant solution sprayed and / or dropped into the gas phase, and the aggregates formed in the gas phase, from adhering to the side wall surface of the container. In the first manufacturing method, the amount of water (flowing water) allowed to flow down along the side wall surface is not particularly limited, but is preferably 10 parts by weight to 10,000 parts by weight per 100 parts by weight of polymer fine particles in the latex. In the first manufacturing method, when the amount of water allowed to flow down along the side wall surface of the container is within the above range, it can prevent the latex and coagulant solution, and the aggregates formed in the gas phase from adhering to the side wall surface of the container, and there is no risk of the load of wastewater treatment becoming excessively high. In the first manufacturing method, the temperature of the water allowed to flow down along the side wall surface is preferably 0°C to 100°C, more preferably 10°C to 90°C, from the viewpoint of simplifying the flowing down operation.
[0180] In the first production method, when water is made to flow down along the side wall surface of the container in the contact step, the aggregates obtained in the gas phase may be transferred to another container together with the flowing water. After being transferred to the other container in this way, the heat treatment step described below may be carried out in the other container using a suspension containing the aggregates.
[0181] In case E, the concentration (amount) of the coagulant in the liquid phase provided at the bottom of the container is preferably 0.01% by weight to 5.00% by weight in the total amount of the liquid phase (100% by weight). In case E, in the contact step, droplets of the latex produced in the gas phase and the coagulant solution combined together fall in the gas phase and enter the liquid phase. In case E, (i) droplets of latex and droplets of the coagulant solution that did not come into contact in the gas phase in the contact step, and (ii) sprayed washing water also enter the liquid phase. In case E, if the concentration (amount) of the coagulant in the coagulant solution is higher (concentrated) than the concentration (amount) of the coagulant in the liquid phase, the concentration (amount) of the coagulant in the liquid phase increases as the contact step progresses. In case E, if water is made to flow down along the inner wall surface of the container in the contact step, it is possible to adjust the concentration (amount) of the coagulant in the liquid phase during the contact step by adjusting the amount of water.
[0182] In case E, the temperature of the liquid phase in the contact step is not particularly limited, but is preferably 1°C to 100°C, more preferably 5°C to 90°C, more preferably 10°C to 85°C, more preferably 20°C to 80°C, more preferably 30°C to 75°C, even more preferably 40°C to 70°C, and particularly preferably 50°C to 70°C. The lower the temperature of the liquid phase, the slower the reaction rate of the aggregation of the polymer microparticles, and the higher the temperature of the liquid phase, the faster the reaction rate of the aggregation of the polymer microparticles. In addition, the lower the temperature of the liquid phase, the smaller the amount of energy consumed. Therefore, the temperature of the liquid phase may be appropriately set from the viewpoint of the reaction rate and the energy consumed.
[0183] (Spraying interruption-cleaning-spraying restart process) In the present production method, a spray interruption-washing-spray resumption process is carried out in the contacting process. The spray interruption-washing-spray resumption process is a process of interrupting the spraying and / or dripping of latex from the first sprayer, spraying washing water from the first sprayer at a pressure of 0.05 MPa to 50.00 MPa, and resuming the spraying and / or dripping of latex from the first sprayer.
[0184] In the contact step, the spray interruption-cleaning-spray resumption steps are preferably carried out within 75 minutes from the start of the spraying step, more preferably within 70 minutes from the start of the spraying step, more preferably within 65 minutes from the start of the spraying step, more preferably within 60 minutes from the start of the spraying step, more preferably within 55 minutes from the start of the spraying step, even more preferably within 50 minutes from the start of the spraying step, and particularly preferably within 45 minutes from the start of the spraying step. This configuration has the advantage that the spray outlet of the sprayer can be cleaned before it becomes clogged.
[0185] In the spray interruption-washing-spray resumption steps, the spraying time of the washing water is preferably 5 seconds or more, more preferably 6 seconds or more, more preferably 7 seconds or more, more preferably 8 seconds or more, even more preferably 9 seconds or more, and particularly preferably 10 seconds or more. According to this configuration, (i) the first production method has an advantage that the obtained suspension is not excessively diluted, and (ii) the second production method has an advantage that the evaporation of the solvent from the latex droplets proceeds efficiently and there is no risk of the obtained powder or granule being excessively wetted.
[0186] In the spray interruption-washing-spray resumption process, the spray pressure of the washing water is preferably 0.05 MPa to 50.00 MPa, more preferably 0.05 MPa to 10.00 MPa, more preferably 0.10 MPa to 10.00 MPa, even more preferably 0.10 MPa to 5.00 MPa, and particularly preferably 1.00 MPa to 3.00 MPa. This configuration has the advantage that scale near and / or inside the nozzle can be vigorously removed.
[0187] In the contact step, the spray interruption-washing-spray restart steps may be repeated multiple times. That is, after restarting the spraying and / or dripping of latex from the first sprayer, the spraying and / or dripping of latex from the first sprayer may be interrupted, washing water may be sprayed from the first sprayer at a pressure of 0.05 MPa to 50.00 MPa, and the spraying and / or dripping of latex from the first sprayer may be restarted. By carrying out the spray interruption-washing-spray restart steps, it becomes unnecessary to interrupt the powder / granular material production method (contact step) to wash the nozzle used for spraying latex, or the frequency of interruption is reduced, and the contact step can be carried out for a longer period of time than before. After repeating the spray interruption-washing-spray restart steps multiple times, the spraying and / or dripping of latex from the first sprayer is terminated, thereby completing the contact step.
[0188] In the contact step, when the spraying interruption-cleaning-spraying restart step is performed multiple times, the second or subsequent spraying interruption-cleaning-spraying restart step is preferably performed within 75 minutes, more preferably within 70 minutes, more preferably within 65 minutes, more preferably within 60 minutes, more preferably within 55 minutes, even more preferably within 50 minutes, and particularly preferably within 45 minutes from the restart of spraying and / or dripping of latex from the first sprayer. This configuration has the advantage that the sprayer outlet can be cleaned before it becomes clogged.
[0189] (2-11. Heat treatment process) The first manufacturing method preferably further includes a heat treatment step of heat-treating the suspension containing the liquid phase, the aggregates of the polymer microparticles, and the coagulant after the contact step. The heat treatment step can be said to be a step of heat-treating the suspension obtained through the contact step. In the first manufacturing method, by heat-treating the suspension, the surfaces of the polymer microparticles are partially melted to form dense aggregates. As a result, a powder with a higher bulk density can be obtained.
[0190] In the first production method, the suspension can be said to be a liquid phase after the start of the contact step. Therefore, in the first production method, the suspension can contain uncoagulated polymer fine particles, aggregates of polymer fine particles, components other than the polymer fine particles contained in the latex (including the solvent of the latex), washing water, the coagulant, and components other than the coagulant contained in the coagulant solution (including the solvent of the coagulant solution).
[0191] In the heat treatment step, the amount of polymer microparticles in the suspension is not particularly limited. In the heat treatment step, the amount of polymer microparticles in 100% by weight of the suspension is, for example, preferably 0.1% by weight or more, more preferably 0.3% by weight or more, more preferably 0.5% by weight or more, more preferably 0.8% by weight or more, more preferably 1.0% by weight or more, more preferably 3.0% by weight or more, even more preferably 5.0% by weight or more, and particularly preferably 8.0% by weight or more. In the heat treatment step, the larger the amount of polymer microparticles in the suspension, the higher the bulk density of the powder or granules can be obtained. In the heat treatment step, the amount of polymer microparticles in 100% by weight of the suspension is, for example, preferably 45% by weight or less, more preferably 40% by weight or less, even more preferably 35% by weight or less, even more preferably 30% by weight or less, and particularly preferably 25% by weight or less. In the heat treatment step, the smaller the amount of polymer microparticles in the suspension, the less likely coarse particles are to be generated.
[0192] In the heat treatment step, the amount of coagulant in the suspension is not particularly limited. In the heat treatment step, the amount of polymer fine particles in 100% by weight of the suspension is, for example, preferably 0.01% by weight or more, more preferably 0.03% by weight or more, more preferably 0.05% by weight or more, more preferably 0.08% by weight or more, more preferably 0.10% by weight or more, more preferably 0.30% by weight or more, more preferably 0.50% by weight or more, more preferably 0.80% by weight or more, more preferably 1.00% by weight or more, even more preferably 1.10% by weight or more, and particularly preferably 1.20% by weight or more. In the heat treatment step, the more the amount of coagulant in the suspension, the stronger the coagulation force, and the less the amount of resin leaking into the wastewater. In the heat treatment step, the amount of the coagulant in 100% by weight of the suspension is, for example, preferably 10.0% by weight or less, more preferably 8.0% by weight or less, even more preferably 6.0% by weight or less, even more preferably 4.0% by weight or less, and particularly preferably 2.0% by weight or less. In the heat treatment step, the smaller the amount of coagulant in the suspension, the more advantageous it is that remaining impurities in the aggregate can be removed with a smaller amount of washing water.
[0193] In the heat treatment step, the total amount of the polymer fine particles and the coagulant in the suspension is not particularly limited. In the heat treatment step, the total amount of the polymer fine particles and the coagulant in 100% by weight of the suspension is preferably 0.2% by weight or more, more preferably 0.5% by weight or more, more preferably 0.8% by weight or more, more preferably 1.0% by weight or more, more preferably 3.0% by weight or more, more preferably 5.0% by weight or more, even more preferably 8.0% by weight or more, and particularly preferably 10.0% by weight or more. The larger the total amount, the higher the bulk density of the powder or granules can be obtained. In the heat treatment step of the first manufacturing method, the total amount of the polymer fine particles and the coagulant in 100% by weight of the suspension is preferably 45% by weight or less, more preferably 40% by weight or less, even more preferably 35% by weight or less, and particularly preferably 30% by weight or less. The smaller the total amount, the more advantageous it is that the remaining impurities in the aggregate can be removed with a small amount of washing water.
[0194] In the heat treatment step, the method for heat treating the suspension is not particularly limited, but may be, for example, a method in which high-temperature (for example, 130° C.) water vapor is fed into the suspension.
[0195] In the heat treatment step, the suspension in the container may be heat-treated in the container after the contact step, or the suspension in the container may be removed from the container and heat-treated in a separate container.
[0196] In the heat treatment step, the temperature of the suspension (heat treatment temperature) is not particularly limited, but is preferably 60° C. to 130° C., more preferably 65° C. to 125° C., more preferably 70° C. to 120° C., more preferably 75° C. to 115° C., more preferably 80° C. to 110° C., even more preferably 85° C. to 105° C., and particularly preferably 90° C. to 100° C. This configuration has the advantage of being able to form dense aggregates.
[0197] In the heat treatment step, the time for which the suspension is heat treated is not particularly limited, but is preferably 30 seconds to 15 minutes, more preferably 1 minute to 12 minutes, even more preferably 2 minutes to 10 minutes, and particularly preferably 3 minutes to 8 minutes. This configuration has the advantage of being able to form dense aggregates.
[0198] When carrying out the heat treatment, it is preferable to suppress the aggregation between aggregates (aggregation between powder particles) during heating and (after) drying. Therefore, it is preferable to add 0.5 to 3.0 parts by weight of hard non-elastic polymer latex (based on solid content) to 100 parts by weight of aggregate (based on solid content) before heat treatment. The hard non-elastic polymer latex may be added to the aggregate before heat treatment, for example, it may be added to the aggregate recovered in the recovery step before heat treatment and mixed, or it may be added (contained) in the liquid phase in the contact step, so that it is substantially added to the aggregate in the contact step. By heat treating the aggregate to which the hard non-elastic polymer latex has been added under the above-mentioned heat treatment conditions, a powder particle in which aggregation between powder particles is suppressed can be obtained.
[0199] As the hard non-elastic polymer, for example, a polymer obtained by polymerizing a monomer capable of forming a rubber elastomer such as butadiene in a small amount (for example, 30% by weight or less, preferably 20% by weight or less, more preferably 10% by weight or less, particularly 0% by weight of the entire polymer) other than this monomer can be used. Examples of monomers that do not form rubber elastomers include (1) alkyl (meth)acrylates having an alkyl group with 10 or less carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate, (2) vinyl arenes such as styrene, α-methylstyrene, monochlorostyrene, and dichlorostyrene, and vinyl cyanides such as acrylonitrile, and (3) polyfunctional monomers such as 1,3-butylene glycol di(meth)acrylate, allyl (meth)acrylate, diallyl phthalate, triallyl cyanurate, monoethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, divinylbenzene, and glycidyl (meth)acrylate. These monomers may be used alone or in appropriate combination.
[0200] (2-12. Recovery process) The first production method preferably further comprises (i) a recovery step of recovering the aggregates from the suspension obtained after the contact step, or (ii) a recovery step of recovering the aggregates from the heat-treated suspension after the heat treatment step. The recovery step can also be said to be a step of separating the aggregates from the suspension.
[0201] In the first production method, the method for separating the aggregates from the suspension (separation method) is not particularly limited, and for example, centrifugal dehydration, static separation, filtration dehydration (e.g., suction filtration), squeeze dehydration, or water evaporation can be applied. In addition, in the first production method, the equipment for carrying out the various separation methods can be appropriately selected according to the desired separation method. For example, in the first production method, a screw press, a roller press, a belt screen, a vibrating sieve, a multi-plate vibrating filter, a suction filter, a vacuum dehydrator, a pressurized dehydrator, a belt press, a centrifugal dehydrator, etc. can be used.
[0202] (2-13. Drying process) The first production method preferably further comprises (i) a drying step of heat-treating the suspension obtained after the contact step and drying the aggregates in the suspension, (ii) a drying step of further heat-treating the heat-treated suspension after the heat-treatment step and drying the aggregates in the suspension, or (iii) a drying step of drying the recovered aggregates after the recovery step. The drying step can also be said to be a step of drying the aggregates to remove moisture derived from the latex, coagulant solution, and liquid phase contained in the aggregates and to promote fusion between polymer fine particles in the aggregates by drying the aggregates.
[0203] In the drying step, the method for drying the aggregate is not particularly limited, and any known method can be used. For example, the aggregate may be dried by subjecting the aggregate to a heat treatment.
[0204] When the aggregate is dried by heat treatment in the drying step, the heat treatment temperature is not particularly limited, but is, for example, preferably 60° C. to 120° C., more preferably 60° C. to 100° C., and even more preferably 65° C. to 95° C. In addition, in the drying step, the heat treatment time is, for example, preferably 1 minute to 60 minutes, and more preferably 5 minutes to 30 minutes.
[0205] In the second manufacturing method, since the temperature in the container is within the above-mentioned range in the contact step, it is possible to evaporate the solvent from the droplets of latex produced by spraying. This allows aggregates of polymer microparticles to be produced in the contact step, and the resulting aggregates can be dried. As a result, in the second manufacturing method, a powder of polymer microparticles can be obtained by the contact step.
[0206] [4. Powder] The powder obtained by this manufacturing method is also one embodiment of the present invention. The "powder according to one embodiment of the present invention" may be referred to as the "present powder". The present powder has an advantage that a good dispersion state of polymer microparticles can be achieved in a resin composition obtained by blending the present powder with a matrix resin, or in a molded or cured product thereof. In this specification, the "powder (powder of polymer microparticles)" may be an aggregate of primary particles of polymer microparticles, in other words, secondary particles of polymer microparticles.
[0207] The powder or granule has an advantage of having a narrow particle size distribution. In this specification, the particle size distribution of the powder or granule is the difference between D90 and D10 of the powder or granule divided by D50. The method for measuring D10, D50 and D90 of the powder or granule will be described in detail in the examples described later.
[0208] The particle size distribution width of the present powder or granule is preferably 3.0 or less, more preferably 2.8 or less, more preferably 2.5 or less, more preferably 2.3 or less, more preferably 2.0 or less, more preferably 1.8 or less, even more preferably 1.5 or less, and particularly preferably 1.3 or less. The smaller the particle size distribution width of the powder or granule, the smaller the amount of fine powder in the powder or granule. The smaller the amount of fine powder in the powder or granule, the less dusting, the better the workability, and the higher the packing rate during packaging, which has the advantage of lowering transportation costs. The lower limit of the particle size distribution width of the present powder or granule is not particularly limited, but may be, for example, 0.1 or more. EXAMPLES
[0209] Hereinafter, one embodiment of the present invention will be described in more detail with reference to examples and comparative examples, but the present invention is not limited thereto. One embodiment of the present invention can be practiced with appropriate modifications within the scope of the above or below-described purpose, and all such modifications are included in the technical scope of the present invention.
[0210] [Measurement method] First, the methods for evaluating the polymer fine particles produced in the Production Examples and the methods for evaluating the powder particles produced in the Examples and Comparative Examples will be described.
[0211] <Evaluation of whether continuous operation is possible> The feasibility of continuous operation was evaluated based on the change in the flow rate of the latex sprayed from the first sprayer.
[0212] If the change in the latex flow rate was within ±10% from the start of spraying (start of the contact process), continuous operation was judged to be "possible." If the change in the latex flow rate was more than ±10% from the start of spraying (start of the contact process), continuous operation was judged to be "not possible" and marked as "no."
[0213] <D of powder and granules 10 , D 50 and D. 90 Measurements > Powder D 10 , D 50 and D. 90 was measured using a laser diffraction / scattering type particle size distribution analyzer LA-950 (HORIBA). In particular, a surfactant aqueous solution was obtained by adding 0.05 g of sodium dodecyl sulfate, a surfactant, as a dispersant to 20 mL of ion-exchanged water. Then, 0.2 g of the powder or granule to be measured was added to the above surfactant aqueous solution, and the powder or granule was dispersed in the surfactant aqueous solution to obtain a dispersion for measurement. The prepared dispersion was introduced into the above laser diffraction / scattering type particle size distribution analyzer, and the particle size distribution of the powder or granule was measured. The D of the powder or granule was measured. 10 is the particle size that corresponds to 10% of the maximum particle size in the cumulative particle size distribution based on volume, and D 50 is the particle size that corresponds to 50% of the maximum particle size in the cumulative particle size distribution based on volume, and D of powder 90 is the particle size that corresponds to 90% of the maximum particle size in the cumulative particle size distribution based on volume. The particle size distribution width of the powder or granular material was calculated from the following formula: Particle size distribution width=(D 90 -D 10 ) / D 50 .
[0214] [Production Example 1] <Latex manufacturing> (Polymerization of the first elastic body) A mixture having the following composition was charged into a glass reactor, and the temperature inside the glass reactor was raised to 80° C. while stirring in a nitrogen stream: Mixture composition: (parts by weight) Ion-exchanged water 220 Boric acid 0.3 Sodium carbonate 0.03 Sodium N-lauroyl sarcosinate 0.09 Sodium formaldehyde sulfoxylate 0.09 Disodium ethylenediaminetetraacetate 0.006 Ferrous sulfate heptahydrate 0.002.
[0215] Then, a mixture of a first monomer component consisting of 25 parts by weight of methyl methacrylate and 0.1 parts by weight of allyl methacrylate, 0.1 parts by weight of t-dodecyl mercaptan as a chain transfer agent, and 0.1 parts by weight of t-butyl hydroperoxide (BHPO) as a polymerization initiator was prepared. Next, 25% by weight of the mixture (100% by weight) prepared was charged into the glass reactor at once, and polymerization was carried out for 45 minutes.
[0216] Next, the remaining 75% by weight of the mixture was continuously added to the glass reactor over 1 hour. After the continuous addition was completed, the glass reactor was kept at 80°C for another 2 hours to complete the polymerization, and a latex of an elastomer (the first elastomer, which can also be said to be the innermost layer elastomer) was obtained. During the temperature maintenance (2 hours at 80°C) after the addition of the mixture, 0.2 parts by weight of sodium N-lauroyl sarcosinate was added to the glass reactor. The average particle size of the obtained first elastomer was 0.16 μm, and the polymerization conversion rate (amount of polymerization product / amount of monomer charged) was 98%.
[0217] (Polymerization of the second elastic body) The glass reactor used in the polymerization of the first elastomer was used as it was for the polymerization of the second elastomer. First, the inside of the glass reactor containing the latex of the first elastomer was kept at 80°C in a nitrogen stream. After 0.1 parts by weight of potassium persulfate was added to the latex, a second monomer mixture consisting of 41 parts by weight of butyl acrylate (n-butyl acrylate), 9 parts by weight of styrene, and 1 part by weight of allyl methacrylate was continuously added for 5 hours. During the continuous addition, potassium oleate was added to the latex in three separate additions, totaling 0.1 parts by weight. After the continuous addition of the second monomer mixture was completed, 0.05 parts by weight of potassium persulfate was further added to the reaction system to complete the polymerization. The temperature inside the glass reactor was kept at 80°C for another 2 hours to obtain a latex of an elastomer (an elastomer consisting only of butyl acrylate rubber) formed by further polymerizing the first elastomer with the second elastomer. The volume average particle size of the obtained elastic body was 0.23 μm, and the polymerization conversion rate was 99%.
[0218] (Polymerization of grafted portion) The glass reactor used in the polymerization of the second elastomer was used as it was for the polymerization of the graft portion. First, the inside of the glass reactor containing the latex of the elastomer was kept at 80°C. After 0.02 parts by weight of potassium persulfate was added to the latex, a graft monomer mixture consisting of 24 parts by weight of methyl methacrylate, 1 part by weight of butyl acrylate (n-butyl acrylate), and 0.1 parts by weight of t-dodecyl mercaptan was continuously added over 1 hour. After the addition of the graft monomer mixture was completed, the temperature inside the glass reactor was kept at 80°C for another 1 hour to obtain a latex (aqueous latex) of a rubber-containing graft copolymer (polymer fine particles) having an elastomer and a graft portion grafted to the elastomer. The volume average particle diameter of the obtained polymer fine particles was 0.25 μm, and the polymerization conversion rate was 99%. The amount (concentration) of the solid content (polymer fine particles) in 100% by weight of the obtained latex was 35% by weight.
[0219] (Preparation of Hard Non-Elastomeric Polymer Latex (P-1)) 200 parts by weight of deionized water, 0.3 parts by weight of sodium oleate, 0.002 parts by weight of ferrous sulfate (FeSO4·7H2O), 0.005 parts by weight of EDTA·2Na salt, and 0.2 parts by weight of sodium formaldehyde sulfoxylate were added to a 100L polymerization vessel (pressure-resistant reaction vessel with stirrer). The temperature inside the vessel was raised to 70°C while stirring. After that, a monomer mixture consisting of 45 parts by weight of methyl methacrylate, 45 parts by weight of styrene, 10 parts by weight of 1,3-butylene glycol dimethacrylate, and 0.3 parts by weight of cumene hydroperoxide was continuously added to the contents of the polymerization vessel over a period of 7 hours. During this time, 0.3 parts by weight of sodium oleate was added at the 2nd, 4th, and 6th hours after the start of the continuous addition. After the continuous addition of the monomer mixture was completed, the contents were stirred for an additional 2 hours to obtain a hard non-elastic polymer latex (P-1). The polymerization conversion was 99%.
[0220] Example 1 (contact process) 1000 g of latex (containing 350 g of polymer fine particles) of Production Example 1 was adjusted to 25°C. A cylindrical container with a vertical side wall was used as the container. The diameter of the container was 80 cm. The container had a liquid phase at the bottom to receive the aggregates generated in the gas phase. The vertical height from the top of the container to the liquid level of the liquid phase was 100 cm. As the first sprayer, a swirling cone nozzle, which is a type of pressurized nozzle, with a nozzle diameter of 4.9 mm (minimum foreign object passing diameter of 2.3 mm) was used. The first sprayer was provided at the upper part (top) of the container. The vertical distance between the first sprayer and the liquid phase was 100 cm. Steam was blown into the gas phase of the container to set the temperature inside the container to 80°C. In an atmosphere of 80°C, the latex containing polymer fine particles was sprayed vertically downward using the first sprayer. The spray pressure of the latex was 3.7 kg / cm 2 The volume average droplet diameter of the sprayed latex was 200 μm. The shape of the spray cone of the sprayed latex was a full cone, and the tip angle was 50° to 60°.
[0221] At the same time as spraying the latex, a coagulant solution (aqueous solution of calcium chloride; the concentration of calcium chloride in 100% by weight of the aqueous calcium chloride solution is 35% by weight, and the temperature is 25°C) was mixed with air and sprayed horizontally by a second sprayer. The spray pressure of the coagulant solution was 4.0 kg / cm. 2 The volume average droplet diameter of the sprayed coagulant solution was 0.10 μm to 30.00 μm. The shape of the spray cone of the sprayed coagulant solution was a hollow cone, and the tip angle was 70° to 90°. Here, a two-fluid nozzle with a nozzle diameter of 0.5 mm was used as the second sprayer. The second sprayer was installed on the side wall of the container at a position lower than the first sprayer so as to spray the coagulant solution horizontally. The horizontal distance between the first sprayer and the second sprayer was 20 cm, and the vertical distance between the first sprayer and the second sprayer was 10 cm. The amount of the coagulant solution sprayed was such that the amount of the coagulant (calcium chloride) sprayed per unit time was 5 to 10 parts by weight per 100 parts by weight of the polymer fine particles in the latex sprayed per unit time.
[0222] (Spraying interruption-cleaning-spraying restart process) After carrying out the above-mentioned contact step for 40 minutes, the spraying of latex from the first sprayer was interrupted, washing water was sprayed from the first sprayer at a pressure of 2 MPa for 10 seconds, and the spraying of latex from the first sprayer was resumed. The spraying of latex after resumption was continued for 40 minutes. By this operation, the droplets of latex descending in the gas phase were brought into contact with the droplets of the coagulant solution sprayed into the gas phase, and an aggregate was obtained.
[0223] The aggregates that had descended in the gas phase were dropped into 35 kg of an aqueous calcium chloride solution (liquid phase) at the bottom of the container. The calcium chloride concentration in the 100% by weight aqueous calcium chloride solution, which is the liquid phase, was 1% by weight. The aqueous calcium chloride solution, which is the liquid phase, was heated to 80°C by supplying water vapor. The aqueous calcium chloride solution, which is the liquid phase, contained 1 part by weight of hard non-elastic polymer latex (P-1) per 100 parts by weight of polymer microparticles in order to prevent fusion between the polymer microparticles. This contact step resulted in a suspension containing aggregates of polymer microparticles. The amount (concentration) of polymer microparticles in the 100% by weight suspension thus obtained was 10.7% by weight.
[0224] After the contact step, water vapor was blown into the suspension, and the suspension was heat-treated at 95°C for 5 minutes (heat treatment step). Thereafter, aggregates were collected from the suspension (collection step), and then the obtained aggregates were dried (drying step) to obtain powder or granules. The particle size distribution of the obtained powder or granules was measured. The results are shown in Table 1.
[0225] Example 2 Regarding the spray interruption-washing-spray resumption process, after the contact step was carried out for 40 minutes, the spraying of latex from the first sprayer was interrupted, washing water was sprayed from the first sprayer at a pressure of 2 MPa for 20 seconds, and the spraying of latex from the first sprayer was resumed again for 40 minutes, and washing water was sprayed from the first sprayer at a pressure of 2 MPa for 20 seconds. Except for this, a powder was obtained in the same manner as in Example 1. The particle size distribution of the obtained powder was measured. The results are shown in Table 1.
[0226] Example 3 Regarding the spray interruption-washing-spray resumption process, after the contact step was carried out for 40 minutes, the spraying of latex from the first sprayer was interrupted, washing water was sprayed from the first sprayer at a pressure of 2 MPa for 5 seconds, and the spraying of latex from the first sprayer was resumed again for 40 minutes, and washing water was sprayed from the first sprayer at a pressure of 2 MPa for 5 seconds. Except for this, a powder was obtained in the same manner as in Example 1. The particle size distribution of the obtained powder was measured. The results are shown in Table 1.
[0227] Comparative Example 1 The contact step was carried out continuously for 80 minutes without performing the steps of interrupting spraying, washing and restarting spraying. Except for this, a powder was obtained in the same manner as in Example 1. The particle size distribution of the obtained powder was measured. The results are shown in Table 1.
[0228] It can be said that the first production method was carried out in Examples 1 to 3. The washing water used in Examples 1 to 3 was ion-exchanged water.
[0229] [Table 1] [Industrial Applicability]
[0230] The method for producing powder or granular material according to one embodiment of the present invention can be carried out continuously. Therefore, the method for producing powder or granular material can be efficiently provided. Therefore, the method for producing powder or granular material according to one embodiment of the present invention can be suitably used as one step in the production of a modifier for thermoplastic resin.
Claims
1. A method for producing a powder of polymer fine particles, comprising the steps of: The method includes a spraying step of spraying and / or dropping the latex containing the polymer fine particles from a first sprayer, A method for producing powder or granular material, comprising the steps of interrupting spraying, washing and restarting spraying in the spraying step: Here, the spraying interruption-washing-spraying resumption process is a process of interrupting spraying and / or dripping of the latex from the first sprayer, spraying washing water from the first sprayer at a pressure of 0.05 MPa to 50.00 MPa, and resuming spraying and / or dripping of the latex from the first sprayer.
2. 2. The method for producing powder or granular material according to claim 1, wherein the first sprayer has a nozzle, and an orifice diameter of the nozzle is 2.3 mm to 6.0 mm.
3. 2. The method for producing powder or granular material according to claim 1, wherein in the spraying step, the spraying interruption-cleaning-spraying restart steps are carried out within 50 minutes from the start of the spraying step.
4. 2. The method for producing powder or granular material according to claim 1, wherein in the spraying step, the spraying time of the cleaning water is 10 seconds or more.
5. The method for producing granular material according to claim 1 , wherein the polymer fine particles have an elastomer and a graft portion graft-bonded to the elastomer.
6. 6. The method for producing powder or granular material according to claim 5, wherein the elastic body comprises at least one rubber selected from the group consisting of diene-based rubber, (meth)acrylate-based rubber, and organosiloxane-based rubber.
7. 6. The method for producing powder or granular material according to claim 5, wherein the graft portion contains one or more structural units selected from the group consisting of an aromatic vinyl unit, a vinylcyan unit, and a (meth)acrylate unit.
8. 8. The method for producing a powder or granular material according to any one of claims 1 to 7, wherein in the spraying step, a coagulant solution containing a coagulant is further sprayed and / or dropped from a second sprayer to bring the droplets of the latex into contact with the droplets of the coagulant solution in a gas phase.
9. The method for producing powder or granular material according to claim 8 , wherein in the spraying step, the coagulant solution is sprayed in a horizontal direction.
10. 8. The method for producing powder or granular material according to claim 1, wherein in the spraying step, agglomerates of the polymer fine particles are generated by evaporating a solvent from droplets of the latex produced by spraying.
Citation Information
Patent Citations
Method for preventing clogging of nozzle for coating
JP2000279857A
Method and device for cleaning liquid discharge head and fine particle production apparatus