Method for producing granules

By spraying latex and a coagulant solution, adding an emulsifier, and heat-treating polymer fine particles, the method enhances the bulk specific gravity of polymer powder and granules, overcoming the limitations of conventional production methods.

JP2024146504AInactive Publication Date: 2024-10-15KANEKA CORP

Patent Information

Application Number
JP2023059454
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional methods for producing polymer powder and granules are inadequate in terms of bulk specific gravity, necessitating a need for improved manufacturing techniques to enhance this property.

Method used

A method involving the spraying of latex containing polymer fine particles and a coagulant solution, followed by a contact step, emulsifier addition, and heat treatment to achieve a concentration of polymer fine particles between 3% to 50% and emulsifier X between 0.002% to 0.045%, resulting in the formation of aggregates with high bulk specific gravity.

Benefits of technology

The method produces powder and granules with significantly increased bulk specific gravity, addressing the limitations of existing technologies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146504000001
    Figure 2024146504000001
Patent Text Reader

Abstract

To provide a method for producing granules that enables the formation of high bulk-density granules.SOLUTION: A method for producing granules includes: a step for contacting droplets of latex of fine polymer particles with droplets of a coagulant solution; and a heating step for heating a suspension containing specific amounts of the fine polymer particle aggregates and the coagulant.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing powder or granular material. [Background technology]

[0002] Powders of polymer fine particles are used as resin modifiers such as impact resistance modifiers, etc. As a method for producing such powders, a method has been proposed in which a latex of polymer fine particles is coagulated to form an aggregate, and the aggregate is then dried (for example, Patent Documents 1 to 3). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2000-026526 A [Patent Document 2] JP 2001-302802 A [Patent Document 3] International Publication WO2006 / 070590 Summary of the Invention [Problem to be solved by the invention]

[0004] However, the above-mentioned conventional techniques are not sufficient in terms of the bulk density of powder or granules, and there is room for further improvement.

[0005] One embodiment of the present invention has been made in consideration of the above problems, and an object of the present invention is to provide a new method for producing powder or granular material that can provide powder or granular material having a high bulk density. [Means for solving the problem]

[0006] The present inventors conducted extensive research to solve the above problems and have now completed the present invention.

[0007] That is, one embodiment of the present invention includes the following configuration. [1] A method for producing powder or granular material, comprising: a contacting step of spraying and / or dropping latex containing polymer fine particles from a first nozzle, and further spraying and / or dropping a coagulant solution containing a coagulant from a second nozzle, thereby bringing the droplets of the latex into contact with droplets of the coagulant solution; and a heat treatment step of heat treating a suspension containing aggregates of the polymer fine particles obtained in the contacting step, wherein in the heat treatment step, a concentration of the polymer fine particles in 100% by weight of the suspension is 3% by weight to 50% by weight. [2] A method for producing powder or granular material, comprising: a contacting step of spraying and / or dropping latex containing polymer fine particles from a first nozzle, and further spraying and / or dropping a coagulant solution containing a coagulant from a second nozzle, thereby bringing droplets of the latex into contact with droplets of the coagulant solution; an emulsifier adding step of adding an emulsifier X to a suspension containing aggregates of the polymer fine particles obtained in the contacting step; and a heat treatment step of heat treating the suspension obtained in the emulsifier adding step, wherein the amount of the emulsifier X in 100% by weight of the suspension in the heat treatment step is 0.002% by weight to 0.045% by weight. [3] The method for producing powder or granular material according to [2], wherein the emulsifier X is at least one selected from the group consisting of sulfur-based emulsifiers, phosphorus-based emulsifiers, sarcosine acid-based emulsifiers, and carboxylic acid-based emulsifiers. [4] The method for producing a powder or granular material according to any one of [1] to [3], wherein the polymer fine particles have an elastomer and a graft portion grafted to the elastomer. [5] The method for producing powder or granular material according to [4], wherein the elastic body contains at least one type selected from the group consisting of diene-based rubbers, (meth)acrylate-based rubbers, and organosiloxane-based rubbers. [6] The method for producing a powder or granular material according to [4] or [5], wherein the graft portion contains one or more structural units selected from the group consisting of an aromatic vinyl unit, a vinyl cyan unit, and a (meth)acrylate unit. [7] The method for producing a powder or granular material according to any one of [1] to [6], further comprising, after the heat treatment step, a recovery step of recovering the agglomerates from the suspension, and a drying step of drying the recovered agglomerates. Effect of the Invention

[0008] According to one aspect of the present invention, a novel method for producing powder or granular material can be provided, which can provide powder or granular material having a high bulk density. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] An embodiment of the present invention will be described below, but the present invention is not limited thereto. The present invention is not limited to each configuration described below, and various modifications are possible within the scope of the claims. In addition, embodiments or examples obtained by appropriately combining the technical means disclosed in different embodiments or examples are also included in the technical scope of the present invention. Furthermore, new technical features can be formed by combining the technical means disclosed in each embodiment. All academic documents and patent documents described in this specification are incorporated herein by reference. In addition, unless otherwise specified in this specification, "A to B" representing a numerical range means "A or more (including A and greater than A) and B or less (including B and smaller than B)".

[0010] In this specification, a "structural unit derived from an X monomer" contained in a polymer, copolymer, or resin may be referred to as an "X unit".

[0011] 1. Technical Concept of the Present Invention As a method for producing aggregates and powder particles of polymer fine particles from latex containing polymer fine particles (hereinafter sometimes referred to as latex), techniques such as those in Patent Documents 1 to 3 are known. Patent Document 3 discloses a method for producing coagulated latex particles from a polymer latex containing a water-soluble polymer compound, in which the polymer latex is sprayed or dropped into a gas phase containing an inorganic salt and / or an acid in an aerosol state, and the polymer latex droplets are dropped or poured into an aqueous phase.

[0012] However, in the conventional technology, there was room for further improvement in terms of the bulk density of powders and granules. The present inventors conducted intensive research in order to provide powders and granules with a high bulk density. As a result, the present inventors independently obtained the following new finding: in a production method in which droplets of latex of polymer microparticles are brought into contact with droplets of a coagulant solution to form aggregates of polymer microparticles, by heat-treating a suspension containing polymer microparticles at a specific concentration, it is surprisingly possible to obtain powders and granules with a high bulk density. The reason for this is unclear, but is presumed to be as follows: If the amount of polymer microparticle agglomerates in the suspension is small, the agglomerates will fuse together during heat treatment, resulting in coarse particles and a low bulk density. However, if the amount of agglomerates is large, the agglomerates can be prevented from fusing together and becoming coarse particles during heat treatment, resulting in a powder with a high bulk density. However, one embodiment of the present invention is not limited to such a speculation.

[0013] Furthermore, as a result of extensive research, the inventors have independently obtained the following new finding: in a production method in which droplets of latex of polymer microparticles are brought into contact with droplets of a coagulant solution to form aggregates of polymer microparticles, by further adding a specific amount of emulsifier to a suspension containing the aggregates and then heat-treating the resulting suspension, it is surprisingly possible to obtain powder particles with a high bulk density. The reason for this is unclear, but is presumed to be as follows: By adding an emulsifier to the suspension, it is possible to prevent the agglomerates from fusing together and becoming coarse particles during heat treatment, and therefore a powder having a high bulk density can be obtained. However, one embodiment of the present invention is not limited to such a speculation.

[0014] 2. Manufacturing method of powder and granular material A method for producing powder or granular material according to one embodiment of the present invention includes a contact step of spraying and / or dropping latex containing polymer fine particles from a first nozzle, and further spraying and / or dropping a coagulant solution containing a coagulant from a second nozzle to bring the droplets of the latex into contact with the droplets of the coagulant solution, and a heat treatment step of heat treating the suspension containing aggregates of the polymer fine particles obtained in the contact step, in which the concentration of the polymer fine particles in 100% by weight of the suspension in the heat treatment step is 3% by weight to 50% by weight. Such a production method may be referred to as a "first production method".

[0015] In this specification, a "latex of polymer microparticles" may be simply referred to as a "latex", an "aggregate of polymer microparticles" may be simply referred to as an "aggregate", and a "powder of polymer microparticles" may be simply referred to as a "powder".

[0016] The first manufacturing method has the above-mentioned configuration, and therefore has the advantage of being able to provide powder or granular material with a large bulk density.

[0017] Another embodiment of the method for producing powder or granular material according to the present invention includes a contact step of contacting droplets of the latex and droplets of the coagulant solution by spraying and / or dropping latex containing polymer fine particles from a first nozzle and further spraying and / or dropping a coagulant solution containing a coagulant from a second nozzle, an emulsifier addition step of adding emulsifier X to the suspension containing aggregates of the polymer fine particles obtained in the contact step, and a heat treatment step of heat treating the suspension obtained in the emulsifier addition step, in which the amount of the emulsifier X is 0.002% by weight to 0.045% by weight in 100% by weight of the suspension. Such a production method may be referred to as a "second production method".

[0018] The second manufacturing method has the above-mentioned configuration, and therefore has the advantage of being able to provide powder or granular material with a high bulk density.

[0019] The first and second manufacturing methods may be collectively referred to as the "manufacturing methods of the present disclosure."

[0020] Below, the raw materials (components) used in the production method of the present disclosure will be described in detail, and then each step of the production method of the present disclosure will be described.

[0021] (2-1.Latex) In this specification, the term "latex" refers to a solution that includes a solvent and polymer fine particles, and in which the polymer fine particles are dispersed in the solvent. The solvent for latex is not particularly limited, but may be water, for example. Latex in which the solvent is water is sometimes called "aqueous latex." In the solvent for latex, the polymer fine particles are preferably dispersed in the form of primary particles.

[0022] The concentration (amount) of the polymer microparticles in the latex is not particularly limited, but is preferably 10% to 55% by weight, more preferably 20% to 50% by weight, even more preferably 30% to 50% by weight, and particularly preferably 30% to 40% by weight, based on 100% by weight of the latex. When the concentration of the polymer microparticles in the latex is within the above range, the resulting aggregate can provide a powder having a better bulk density. The concentration of the polymer microparticles in the latex can be adjusted by appropriately changing the amount of the solvent (e.g., water) used in the production process of the polymer microparticles and the amount of the monomer used.

[0023] The concentration of polymer particles in latex can be calculated, for example, by the following method: 0.5 g of latex is placed in a hot air convection dryer at 120°C for 3 hours to evaporate the water, the weight W(g) of the residue (solid content) after drying is measured, the obtained value (W(g)) is divided by the weight of the latex before drying, 0.5 g, and the obtained value is multiplied by 100. By such an operation, the "concentration of solid content in latex" can be calculated. The residue after drying latex, i.e., the solid content, mainly contains polymer particles, but may also contain components other than polymer particles. On the other hand, the amount of components in latex that can become solid content other than polymer particles is extremely small. Therefore, the "concentration of solid content in latex" calculated by the above-mentioned method can be regarded as the "concentration of polymer particles in latex".

[0024] The latex containing polymer fine particles can be produced by a known method, for example, an emulsion polymerization method of polymer fine particles, or a method of suspending polymer fine particles and an emulsifier in a solvent, etc. The emulsion polymerization method of polymer fine particles will be described in detail in the section (2-3. Production method of polymer fine particles) below.

[0025] (2-2. Polymer microparticles) The polymer microparticles are not particularly limited in other aspects as long as they are microparticles obtained by polymerization. The polymer microparticles may be (a) made of only one type of polymer (first polymer), or (b) made of two or more types of polymers having a second polymer covering the first polymer. In addition, these polymers may have a graft portion.

[0026] In addition to the first polymer and the second polymer covering it, the polymer microparticles may further contain other components such as other commonly used processing aids. When the polymer microparticles contain two or more types of polymers, the polymer microparticles may have a layer structure (multilayer structure), for example, each of the multiple polymers contained in the polymer microparticles may form each layer. When the polymer microparticles contain two or more types of polymers, each polymer (for example, each of the first polymer and the second polymer) may have a single-layer structure, a multilayer structure, or a combination of a single-layer structure and a multilayer structure. When the polymer microparticles contain the first polymer and the second polymer, it is preferable that the second polymer is present so as to cover at least a part of the first polymer, in other words, it is preferable that the second polymer is present outside the first polymer in the polymer microparticles. In this case, it is preferable that the first polymer and the second polymer are not chemically bonded to each other.

[0027] The polymer microparticles preferably have an elastomer and a graft portion grafted to the elastomer. A polymer having an elastomer and a graft portion grafted to the elastomer may also be called a "rubber-containing graft copolymer". That is, the polymer microparticles are preferably rubber-containing graft copolymers. When the polymer microparticles are rubber-containing graft copolymers, the polymer microparticles have the advantage of being able to exhibit suitable behavior in the manufacturing method of the present disclosure. Hereinafter, an embodiment of the present invention will be described taking the case where the polymer microparticles are rubber-containing graft copolymers as an example.

[0028] (Elastic body) The elastic body preferably contains one or more selected from the group consisting of diene rubber, (meth)acrylate rubber, and organosiloxane rubber. The elastic body may contain natural rubber in addition to the above-mentioned rubber. The elastic body may also be called an elastic portion or rubber particles.

[0029] The case where the elastomer contains a diene rubber (case A) will be described. In case A, the obtained resin composition can provide a molded article or cured product having excellent toughness and impact resistance. A molded article or cured product having excellent toughness and / or impact resistance can also be said to be a molded article or cured product having excellent durability.

[0030] The diene rubber is an elastomer containing, as a constituent unit, a constituent unit derived from a diene monomer. The diene monomer can also be called a conjugated diene monomer. In case A, the diene rubber may contain, in 100% by weight of the constituent units, 50 to 100% by weight of constituent units derived from diene monomers and 0 to 50% by weight of constituent units derived from vinyl monomers other than diene monomers copolymerizable with the diene monomers. In case A, the diene rubber may contain, as a constituent unit, a constituent unit derived from a (meth)acrylate monomer in an amount less than the constituent units derived from the diene monomers.

[0031] Examples of the diene monomer include 1,3-butadiene, isoprene (2-methyl-1,3-butadiene), 2-chloro-1,3-butadiene, etc. These diene monomers may be used alone or in combination of two or more.

[0032] Examples of vinyl monomers other than diene monomers that can be copolymerized with diene monomers (hereinafter, also referred to as vinyl monomer A) include vinyl arenes such as styrene, α-methylstyrene, monochlorostyrene, and dichlorostyrene; vinyl carboxylic acids such as acrylic acid and methacrylic acid; vinyl cyanides such as acrylonitrile and methacrylonitrile; vinyl halides such as vinyl chloride, vinyl bromide, and chloroprene; vinyl acetate; alkenes such as ethylene, propylene, butylene, and isobutylene; and polyfunctional monomers such as diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, and divinylbenzene. The above-mentioned vinyl monomer A may be used alone or in combination of two or more kinds. Among the above-mentioned vinyl monomers A, styrene is particularly preferred. In the diene rubber in case A, the constituent unit derived from the vinyl monomer A is an optional component. In case A, the diene rubber may be composed only of structural units derived from diene monomers.

[0033] In case A, the diene rubber is preferably butadiene rubber (also called polybutadiene rubber) consisting of structural units derived from 1,3-butadiene, or butadiene-styrene rubber (also called polystyrene-butadiene) which is a copolymer of 1,3-butadiene and styrene, and butadiene rubber is more preferable. According to the above configuration, the desired effect of the polymer microparticles containing the diene rubber can be more effectively exhibited. In addition, butadiene-styrene rubber is more preferable in that the transparency of the obtained molded body or cured product can be increased by adjusting the refractive index.

[0034] In one embodiment of the present invention, the elastomer preferably contains 30% by weight or more of diene rubber, more preferably 40% by weight or more, more preferably 50% by weight or more, more preferably 60% by weight or more, more preferably 70% by weight or more, preferably 80% by weight or more, even more preferably 90% by weight or more, particularly preferably 95% by weight or more, and most preferably 100% by weight. In other words, it is most preferable that the elastomer is composed only of diene rubber.

[0035] In one embodiment of the present invention, the elastomer contains butadiene rubber and / or butadiene-styrene rubber, and in 100% by weight of the elastomer, the total of butadiene rubber and butadiene-styrene rubber is preferably 30% by weight or more, more preferably 40% by weight or more, more preferably 50% by weight or more, more preferably 60% by weight or more, more preferably 70% by weight or more, more preferably 80% by weight or more, even more preferably 90% by weight or more, particularly preferably 95% by weight or more, and most preferably 100% by weight. In other words, the elastomer is most preferably composed of only butadiene rubber, only butadiene-styrene rubber, or only butadiene rubber and butadiene-styrene rubber.

[0036] The case where the elastomer contains a (meth)acrylate rubber (Case B) will be described. In Case B, a wide range of polymer designs for the elastomer are possible by combining a variety of monomers.

[0037] The (meth)acrylate rubber is an elastomer containing, as a structural unit, a structural unit derived from a (meth)acrylate monomer. In case B, the (meth)acrylate rubber may contain, in 100% by weight of structural units, 50 to 100% by weight of structural units derived from a (meth)acrylate monomer, and 0 to 50% by weight of structural units derived from a vinyl monomer other than the (meth)acrylate monomer that is copolymerizable with the (meth)acrylate monomer. In case B, the (meth)acrylate rubber may contain, as a structural unit, a structural unit derived from a diene monomer in an amount less than the structural unit derived from the (meth)acrylate monomer.

[0038] Examples of the (meth)acrylate monomer include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, dodecyl (meth)acrylate, stearyl (meth)acrylate, and behenyl (meth)acrylate; aromatic ring-containing (meth)acrylates such as phenoxyethyl (meth)acrylate and benzyl (meth)acrylate; 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and the like. Examples of the monomers include hydroxyalkyl (meth)acrylates such as acrylate; glycidyl (meth)acrylates such as glycidyl (meth)acrylate and glycidyl alkyl (meth)acrylate; alkoxyalkyl (meth)acrylates; allyl alkyl (meth)acrylates such as allyl (meth)acrylate and allyl alkyl (meth)acrylate; and polyfunctional (meth)acrylates such as monoethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, and tetraethylene glycol di(meth)acrylate. These (meth)acrylate monomers may be used alone or in combination of two or more. Among these (meth)acrylate monomers, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate are preferred, and methyl (meth)acrylate and butyl (meth)acrylate are more preferred.

[0039] In case B, the (meth)acrylate rubber is preferably one or more selected from the group consisting of methyl (meth)acrylate rubber, ethyl (meth)acrylate rubber, butyl (meth)acrylate rubber, and 2-ethylhexyl (meth)acrylate rubber, more preferably one or more selected from the group consisting of methyl (meth)acrylate rubber and butyl (meth)acrylate rubber, even more preferably one or more selected from the group consisting of butyl (meth)acrylate rubber, and particularly preferably butyl acrylate. The methyl (meth)acrylate rubber is a rubber containing 50% or more by weight of methyl (meth)acrylate units in 100% by weight of rubber, the ethyl (meth)acrylate rubber is a rubber containing 50% or more by weight of ethyl (meth)acrylate units in 100% by weight of rubber, the butyl (meth)acrylate rubber is a rubber containing 50% or more by weight of butyl (meth)acrylate units in 100% by weight of rubber, the butyl acrylate rubber is a rubber containing 50% or more by weight of butyl acrylate units in 100% by weight of rubber, and the 2-ethylhexyl (meth)acrylate rubber is a rubber containing 50% or more by weight of 2-ethylhexyl (meth)acrylate units in 100% by weight of rubber. According to this configuration, the glass transition temperature (Tg) of the elastomer is lowered, so that polymer microparticles and resin compositions with low Tg can be obtained. As a result, (i) the resulting resin composition can provide a molded article or cured product having excellent toughness, and (ii) the viscosity of the resin composition can be reduced.

[0040] In one embodiment of the present invention, the elastomer preferably contains 30% by weight or more of (meth)acrylate rubber, more preferably 40% by weight or more, more preferably 50% by weight or more, more preferably 60% by weight or more, more preferably 70% by weight or more, more preferably 80% by weight or more, even more preferably 90% by weight or more, particularly preferably 95% by weight or more, and most preferably 100% by weight. In other words, the elastomer is most preferably composed only of (meth)acrylate rubber. This configuration has the advantage of being able to provide a molded or cured product with a good balance of physical properties such as color tone, tensile strength, impact resistance, dispersibility, and compatibility. Specifically, depending on the type of resin (matrix resin) into which the powder particles are to be blended, when the elastomer contains 60% by weight or more of a (meth)acrylate-based rubber out of 100% by weight of the elastomer, compared with when the elastomer contains a large amount (e.g., 60% by weight or more out of 100% by weight of the elastomer) of diene-based rubber (e.g., polybutadiene rubber), the resulting resin composition or a molded or cured product obtained from the resin composition has the advantage of being better in color, tensile strength, impact resistance, dispersibility and / or compatibility.

[0041] In one embodiment of the present invention, the elastomer preferably contains 30% by weight or more of butyl (meth)acrylate rubber, more preferably 40% by weight or more, more preferably 50% by weight or more, more preferably 60% by weight or more, more preferably 70% by weight or more, more preferably 80% by weight or more, even more preferably 90% by weight or more, particularly preferably 95% by weight or more, and most preferably 100% by weight. In other words, the elastomer is most preferably composed of only butyl (meth)acrylate rubber. This configuration has the advantage of being able to provide a molded or cured product with a good balance of physical properties such as color tone, tensile strength, impact resistance, dispersibility, and compatibility. Specifically, depending on the type of resin (matrix resin) into which the powder particles are to be blended, when the elastomer contains 60% by weight or more of butyl (meth)acrylate rubber out of 100% by weight of the elastomer, compared with when the elastomer contains a large amount (e.g., 60% by weight or more out of 100% by weight of the elastomer) of diene rubber (e.g., polybutadiene rubber), the resulting resin composition or a molded or cured product obtained from the resin composition has the advantage of being better in color, tensile strength, impact resistance, dispersibility and / or compatibility.

[0042] Examples of vinyl monomers other than (meth)acrylate monomers copolymerizable with (meth)acrylate monomers (hereinafter also referred to as vinyl monomer B) include the monomers listed in the vinyl monomer A. Only one type of vinyl monomer B may be used, or two or more types may be used in combination. Among the vinyl monomers B, styrene is particularly preferred. In the (meth)acrylate rubber in case B, the constituent unit derived from the vinyl monomer B is an optional component. In case B, the (meth)acrylate rubber may be composed only of constituent units derived from (meth)acrylate monomers.

[0043] The case where the elastomer contains an organosiloxane-based rubber (Case C) will be described below. In Case C, the resulting resin composition can provide a molded article or cured product having sufficient heat resistance and excellent impact resistance at low temperatures.

[0044] Examples of organosiloxane rubbers include (i) organosiloxane polymers composed of alkyl or aryl disubstituted silyloxy units, such as dimethylsilyloxy, diethylsilyloxy, methylphenylsilyloxy, diphenylsilyloxy, and dimethylsilyloxy-diphenylsilyloxy, and (ii) organosiloxane polymers composed of alkyl or aryl monosubstituted silyloxy units, such as organohydrogensilyloxy in which a portion of the alkyl in the side chain is replaced with a hydrogen atom. These organosiloxane polymers may be used alone or in combination of two or more.

[0045] In this specification, a polymer composed of dimethylsilyloxy units is referred to as dimethylsilyloxy rubber, a polymer composed of methylphenylsilyloxy units is referred to as methylphenylsilyloxy rubber, and a polymer composed of dimethylsilyloxy units and diphenylsilyloxy units is referred to as dimethylsilyloxy-diphenylsilyloxy rubber. In case C, the organosiloxane rubber is preferably one or more selected from the group consisting of dimethylsilyloxy rubber, methylphenylsilyloxy rubber, and dimethylsilyloxy-diphenylsilyloxy rubber, since (i) the resin composition containing the obtained powdery material can provide a molded product or cured product having excellent heat resistance, and (ii) dimethylsilyloxy rubber is more preferable, since it is easily available and economical.

[0046] In one embodiment of the present invention, the elastomer preferably contains 30% by weight or more of organosiloxane rubber, more preferably 40% by weight or more, more preferably 50% by weight or more, more preferably 60% by weight or more, more preferably 70% by weight or more, more preferably 80% by weight or more, even more preferably 90% by weight or more, particularly preferably 95% by weight or more, and most preferably 100% by weight. In other words, it is most preferable that the elastomer is composed only of organosiloxane rubber. According to the above-mentioned configuration, the obtained resin composition can provide a molded body or cured product having excellent heat resistance.

[0047] In one embodiment of the present invention, the elastomer is preferably one or more selected from the group consisting of butadiene rubber, butadiene-styrene rubber, butadiene-(meth)acrylate rubber, ethyl (meth)acrylate rubber, butyl (meth)acrylate rubber, 2-ethylhexyl (meth)acrylate rubber, dimethylsilyloxy rubber, methylphenylsilyloxy rubber, and dimethylsilyloxy-diphenylsilyloxy rubber, and more preferably one or more selected from the group consisting of butadiene rubber, butadiene-styrene rubber, butyl (meth)acrylate rubber, and dimethylsilyloxy rubber.

[0048] (Elastomeric bridge structure) From the viewpoint of maintaining the dispersion stability of the polymer microparticles in the thermosetting resin, it is preferable that a crosslinked structure is introduced into the elastomer. A commonly used method can be adopted as a method for introducing a crosslinked structure into the elastomer, and examples thereof include the following methods. That is, in the production of the elastomer, a method is exemplified in which a crosslinkable monomer such as a multifunctional monomer and / or a mercapto group-containing compound is mixed with a monomer capable of constituting the elastomer, and then polymerized. In this specification, the production of a polymer such as an elastomer is also referred to as polymerizing a polymer.

[0049] Methods for introducing a crosslinked structure into an organosiloxane rubber include the following: (A) a method of using a polyfunctional alkoxysilane compound in combination with other materials when polymerizing an organosiloxane rubber; (B) a method of introducing reactive groups (e.g., (i) a mercapto group and (ii) a reactive vinyl group, etc.) into an organosiloxane rubber, and then adding (i) an organic peroxide or (ii) a polymerizable vinyl monomer, etc., to the resulting reaction product to cause a radical reaction; and (C) a method of mixing a crosslinkable monomer such as a polyfunctional monomer and / or a mercapto group-containing compound with other materials when polymerizing an organosiloxane rubber, and then polymerizing the rubber.

[0050] A polyfunctional monomer can be said to be a monomer having two or more radically polymerizable reactive groups in the same molecule. The radically polymerizable reactive group is preferably a carbon-carbon double bond. Examples of polyfunctional monomers include (meth)acrylates having ethylenically unsaturated double bonds, such as allyl alkyl (meth)acrylates and allyloxy alkyl (meth)acrylates, and do not include butadiene. Examples of monomers having two (meth)acrylic groups include ethylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate, butane diol di(meth)acrylate, hexane diol di(meth)acrylate, cyclohexane dimethanol di(meth)acrylate, and polyethylene glycol di(meth)acrylates. Examples of the polyethylene glycol di(meth)acrylates include triethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, and polyethylene glycol (600) di(meth)acrylate. Examples of monomers having three (meth)acrylic groups include alkoxylated trimethylolpropane tri(meth)acrylates, glycerol propoxy tri(meth)acrylate, pentaerythritol tri(meth)acrylate, and tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate. Examples of the alkoxylated trimethylolpropane tri(meth)acrylates include trimethylolpropane tri(meth)acrylate and trimethylolpropane triethoxy tri(meth)acrylate. Further, examples of monomers having four (meth)acrylic groups include pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, etc. Further, examples of monomers having five (meth)acrylic groups include dipentaerythritol penta(meth)acrylate, etc. Further, examples of monomers having six (meth)acrylic groups include ditrimethylolpropane hexa(meth)acrylate, etc.Polyfunctional monomers also include diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, divinylbenzene, and the like.

[0051] Among the above-mentioned polyfunctional monomers, polyfunctional monomers that can be preferably used for introducing a crosslinked structure into the elastomer include allyl methacrylate, ethylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate (e.g., 1,3-butylene glycol dimethacrylate, etc.), butanediol di(meth)acrylate, hexanediol di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate, and polyethylene glycol di(meth)acrylates. These polyfunctional monomers may be used alone or in combination of two or more.

[0052] (Volume average particle size of elastic body) The volume average particle diameter of the elastic body is preferably 0.03 μm to 50.00 μm, more preferably 0.05 μm to 10.00 μm, more preferably 0.08 μm to 2.00 μm, even more preferably 0.10 μm to 1.00 μm, even more preferably 0.10 μm to 0.80 μm, and particularly preferably 0.10 μm to 0.50 μm. When the volume average particle diameter of the elastic body is (i) 0.03 μm or more, an elastic body having a desired volume average particle diameter can be stably obtained, and (ii) when it is 50.00 μm or less, the heat resistance and impact resistance of the obtained molded body or cured product become good. The volume average particle diameter of the elastic body can be measured using a dynamic light scattering type particle size distribution measuring device or the like, using an aqueous latex containing the elastic body as a sample. The method for measuring the volume average particle diameter of the elastic body will be described in detail in the following examples.

[0053] (Ratio of elastic body) The proportion of the elastomer in the polymer microparticles is preferably 40 to 97% by weight, more preferably 60 to 95% by weight, and even more preferably 70 to 93% by weight, based on 100% by weight of the entire polymer microparticles. When the proportion of the elastomer is (i) 40% by weight or more, the resulting resin composition can provide a molded article or cured product having excellent toughness and impact resistance, and (ii) when the proportion is 97% by weight or less, the polymer microparticles do not easily aggregate, so that the resin composition does not become highly viscous, and as a result, the resulting resin composition can be easy to handle.

[0054] In one embodiment of the present invention, the "elastic body" of the polymer microparticles may consist of only one type of elastomer having the same composition of constitutional units.

[0055] (Graft part) The graft moiety preferably contains one or more structural units selected from the group consisting of aromatic vinyl units, vinylcyan units, and (meth)acrylate units. The graft moiety having such a structure can play various roles. The "various roles" include, for example, (i) improving the compatibility between the polymer microparticles and the matrix resin, (ii) improving the dispersibility of the polymer microparticles in the matrix resin, and (iii) enabling the polymer microparticles to be dispersed in the form of primary particles in a resin composition containing a matrix resin and polymer microparticles (hereinafter also simply referred to as "resin composition"), or in a molded product or cured product thereof.

[0056] Specific examples of monomers from which the aromatic vinyl units are derived include styrene, α-methylstyrene, p-methylstyrene, and divinylbenzene.

[0057] Specific examples of monomers from which vinylcyan units are derived include acrylonitrile and methacrylonitrile.

[0058] Specific examples of monomers from which (meth)acrylate units are derived include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, hydroxyethyl (meth)acrylate, and hydroxybutyl (meth)acrylate, etc. In this specification, (meth)acrylate refers to acrylate and / or methacrylate.

[0059] The one or more monomers selected from the group consisting of the aromatic vinyl monomer, the vinyl cyan monomer, and the (meth)acrylate monomer may be used alone or in combination of two or more.

[0060] The graft portion preferably contains 10 to 95% by weight of aromatic vinyl units, vinylcyan units and (meth)acrylate units in total, based on 100% by weight of the graft portion, more preferably 30 to 92% by weight, even more preferably 50 to 90% by weight, particularly preferably 60 to 87% by weight, and most preferably 70 to 85% by weight.

[0061] The graft portion preferably contains, as a constituent unit, a constituent unit derived from a monomer having a reactive group. The monomer having a reactive group is preferably a monomer having one or more reactive groups selected from the group consisting of an epoxy group, an oxetane group, a hydroxyl group, an amino group, an imide group, a carboxylic acid group, a carboxylic anhydride group, a cyclic ester, a cyclic amide, a benzoxazine group, and a cyanate ester group, more preferably a monomer having one or more reactive groups selected from the group consisting of an epoxy group, a hydroxyl group, and a carboxylic acid group, and most preferably a monomer having an epoxy group. According to the above configuration, the graft portion of the polymer fine particles can be chemically bonded to the matrix resin in the resin composition. This allows the polymer fine particles to be maintained in a good dispersion state without agglomerating in the resin composition or in a molded or cured product thereof.

[0062] Specific examples of monomers having an epoxy group include glycidyl group-containing vinyl monomers such as glycidyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, and allyl glycidyl ether.

[0063] Specific examples of monomers having a hydroxyl group include, for example, (i) hydroxy linear alkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate (particularly, hydroxy linear C1-6 alkyl (meth)acrylates); (ii) caprolactone-modified hydroxy (meth)acrylates; (iii) hydroxy branched alkyl (meth)acrylates such as α-(hydroxymethyl)methyl acrylate and α-(hydroxymethyl)ethyl acrylate; and (iv) hydroxyl group-containing (meth)acrylates such as mono(meth)acrylates of polyester diols (particularly saturated polyester diols) obtained from divalent carboxylic acids (such as phthalic acid) and dihydric alcohols (such as propylene glycol).

[0064] Specific examples of the monomer having a carboxylic acid group include monocarboxylic acids such as acrylic acid, methacrylic acid, and crotonic acid, and dicarboxylic acids such as maleic acid, fumaric acid, and itaconic acid. As the monomer having a carboxylic acid group, the above-mentioned monocarboxylic acids are preferably used.

[0065] The above-mentioned monomers having a reactive group may be used alone or in combination of two or more kinds.

[0066] The graft portion preferably contains 0.5% by weight to 90.0% by weight of a structural unit derived from a monomer having a reactive group, more preferably 1.0% by weight to 50.0% by weight, even more preferably 2.0% by weight to 35.0% by weight, and particularly preferably 3.0% by weight to 20.0% by weight, based on 100% by weight of the graft portion. When the graft portion contains (i) 0.5% by weight or more of a structural unit derived from a monomer having a reactive group, the resulting resin composition can provide a molded article or cured product having sufficient impact resistance, and (ii) when the graft portion contains 90.0% by weight or less, the resulting resin composition can provide a molded article or cured product having sufficient impact resistance, and has the advantage of having good storage stability of the resin composition.

[0067] The structural unit derived from a monomer having a reactive group is preferably contained in the graft portion, and more preferably contained only in the graft portion.

[0068] The graft portion may contain a structural unit derived from a polyfunctional monomer as a structural unit. When the graft portion contains a structural unit derived from a polyfunctional monomer, it has the following advantages: (i) swelling of the polymer fine particles in the resin composition can be prevented, (ii) the viscosity of the resin composition is reduced, so that the handleability of the resin composition tends to be improved, and (iii) the dispersibility of the polymer fine particles in the matrix resin is improved.

[0069] When the graft portion does not contain a structural unit derived from a polyfunctional monomer, the resulting resin composition can provide a molded article or cured product that is more excellent in toughness and impact resistance, compared to when the graft portion contains a structural unit derived from a polyfunctional monomer.

[0070] Specific examples of the polyfunctional monomer are the same as those explained in the section (Elastomer) above, so the explanation therefor is incorporated by reference and will not be repeated here.

[0071] Among the polyfunctional monomers, polyfunctional monomers that can be preferably used for polymerization of the graft portion include allyl methacrylate, ethylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate, and polyethylene glycol di(meth)acrylates. These polyfunctional monomers may be used alone or in combination of two or more.

[0072] The graft portion preferably contains 1 to 20% by weight, and more preferably 5 to 15% by weight, of structural units derived from polyfunctional monomers, based on 100% by weight of the graft portion.

[0073] In the polymerization of the graft portion, the above-mentioned monomers may be used alone or in combination of two or more. The graft portion may contain, as a constituent unit, a constituent unit derived from another monomer in addition to the constituent unit derived from the above-mentioned monomer.

[0074] In one embodiment of the present invention, the graft portion may be composed of only one type of graft portion having structural units of the same composition. In one embodiment of the present invention, the graft portion may be composed of multiple types of graft portions each having a structural unit of a different composition.

[0075] The graft portion may cover at least a portion of the elastic body, or may cover the entire elastic body. A portion of the graft portion may penetrate into the inside of the elastic body. It is preferable that at least a portion of the graft portion covers at least a portion of the elastic body. In other words, it is preferable that at least a portion of the graft portion is present on the outermost side of the polymer microparticle.

[0076] The polymer microparticles may form a layer structure. For example, one embodiment of the present invention is one in which the elastomer forms the innermost layer (also referred to as a core layer) and a layer of the graft portion is formed as the outermost layer (also referred to as a shell layer) on the outside of the elastomer. A structure in which the elastomer forms the core layer and the graft portion forms the shell layer can also be called a core-shell structure. In one embodiment of the present invention, the polymer microparticles may have a core-shell structure.

[0077] (Surface crosslinked polymer) The rubber-containing graft copolymer preferably further has a surface cross-linked polymer in addition to the elastomer and the graft portion grafted to the elastomer. In other words, the polymer microparticle preferably further has a surface cross-linked polymer in addition to the elastomer and the graft portion grafted to the elastomer. Hereinafter, an embodiment of the present invention will be described taking as an example a case where the polymer microparticle (e.g., rubber-containing graft copolymer) further has a surface cross-linked polymer. In this case, (i) the blocking resistance can be improved in the production of the polymer microparticles, and (ii) the dispersibility of the polymer microparticles in the thermosetting resin becomes better. The reasons for this are not particularly limited, but can be assumed as follows: By covering at least a part of the elastomer with the surface cross-linked polymer, the exposure of the elastomer part of the polymer microparticles is reduced, and as a result, the elastomers are less likely to stick to each other, and the dispersibility of the polymer microparticles is improved.

[0078] When the polymer microparticles have a surface-crosslinked polymer, they can also have the following effects: (i) the effect of reducing the viscosity of the resin composition, (ii) the effect of increasing the crosslink density in the elastomer, and (iii) the effect of increasing the graft efficiency of the grafted portion. The crosslink density in the elastomer refers to the degree of the number of crosslinked structures in the entire elastomer.

[0079] The surface cross-linked polymer is composed of a polymer containing, as structural units, 30 to 100% by weight of structural units derived from polyfunctional monomers and 0 to 70% by weight of structural units derived from other vinyl monomers, totaling 100% by weight.

[0080] The polyfunctional monomer that can be used for the polymerization of the surface cross-linked polymer includes the same monomer as the polyfunctional monomer described above. Among these polyfunctional monomers, the polyfunctional monomer that can be preferably used for the polymerization of the surface cross-linked polymer includes allyl methacrylate, ethylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate (e.g., 1,3-butylene glycol dimethacrylate, etc.), butanediol di(meth)acrylate, hexanediol di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate, and polyethylene glycol di(meth)acrylates. These polyfunctional monomers may be used alone or in combination of two or more.

[0081] The polymer microparticles may contain a surface cross-linked polymer polymerized independently of the polymerization of the rubber-containing graft copolymer, or may contain a surface cross-linked polymer polymerized together with the rubber-containing graft copolymer. The polymer microparticles may be a multi-stage polymer obtained by multi-stage polymerization of an elastomer, a surface cross-linked polymer, and a graft portion in this order. In any of these embodiments, the surface cross-linked polymer can cover at least a part of the elastomer.

[0082] The surface cross-linked polymer can be regarded as a part of the elastomer. In other words, the surface cross-linked polymer can be regarded as a part of the rubber-containing graft copolymer, and can also be called a surface cross-linked polymerization part. When the polymer microparticles contain a surface cross-linked polymer, the graft part may be (i) grafted to an elastomer other than the surface cross-linked polymer, (ii) grafted to a surface cross-linked polymer, or (iii) grafted to both an elastomer other than the surface cross-linked polymer and a surface cross-linked polymer. When the polymer microparticles contain a surface cross-linked polymer, the volume average particle diameter of the elastomer mentioned above refers to the volume average particle diameter of the elastomer containing the surface cross-linked polymer.

[0083] The case where the polymer microparticle is a multi-stage polymer obtained by multi-stage polymerization of an elastomer, a surface cross-linked polymer, and a graft portion in this order (case D) will be described. In case D, the surface cross-linked polymer may cover a part of the elastomer, or may cover the whole of the elastomer. In case D, a part of the surface cross-linked polymer may penetrate into the inside of the elastomer. In case D, the graft portion may cover a part of the surface cross-linked polymer, or may cover the whole of the surface cross-linked polymer. In case D, a part of the graft portion may penetrate into the inside of the surface cross-linked polymer. In case D, the elastomer, the surface cross-linked polymer, and the graft portion may have a layer structure. For example, an embodiment in which the elastomer is the innermost layer (core layer), a layer of the surface cross-linked polymer exists outside the elastomer as an intermediate layer, and a layer of the graft portion exists outside the surface cross-linked polymer as an outermost layer (shell layer) is also one embodiment of the present invention.

[0084] (Volume average particle size of polymer particles (Mv)) The volume average particle diameter (Mv) of the polymer microparticles is preferably 0.03 μm to 50.00 μm, more preferably 0.05 μm to 10.00 μm, more preferably 0.08 μm to 2.00 μm, even more preferably 0.10 μm to 1.00 μm, even more preferably 0.10 μm to 0.80 μm, and particularly preferably 0.10 μm to 0.50 μm, since a resin composition having a desired viscosity and high stability can be obtained. When the volume average particle diameter (Mv) of the polymer microparticles is within the above range, there is also an advantage that the dispersibility of the polymer microparticles in the matrix resin is improved. In this specification, the "volume average particle diameter (Mv) of the polymer microparticles" refers to the volume average particle diameter of the primary particles of the polymer microparticles, unless otherwise specified. The volume average particle diameter of the polymer microparticles can be measured using a dynamic light scattering particle size distribution measuring device or the like, using an aqueous latex containing the polymer microparticles as a sample.

[0085] (2-3. Method for producing polymer microparticles) An example of a method for producing polymer microparticles will be described below, taking as an example a case where the polymer microparticles are a rubber-containing graft copolymer having an elastomer and a graft portion grafted to the elastomer. The polymer microparticles can be produced, for example, by polymerizing an elastomer, and then graft polymerizing a polymer constituting the graft portion to the elastomer in the presence of the elastomer.

[0086] The polymer microparticles can be produced by known methods, such as emulsion polymerization, suspension polymerization, and microsuspension polymerization. Specifically, the polymerization of the elastomer in the polymer microparticles and the polymerization of the graft portion (graft polymerization) can be carried out by known methods, such as emulsion polymerization, suspension polymerization, and microsuspension polymerization. Among these, the emulsion polymerization method is particularly preferred as a method for producing polymer microparticles. By producing polymer microparticles by emulsion polymerization, latex (e.g., aqueous latex) containing polymer microparticles can be obtained. In this specification, the latex obtained by emulsion polymerization may be referred to as "emulsion-polymerized latex". The emulsion polymerization method has the advantages of (i) easy composition design of polymer microparticles, (ii) easy industrial production of polymer microparticles, and (iii) easy production of latex suitable for use in the production method of the present disclosure.

[0087] When emulsion polymerization is employed as a method for producing polymer fine particles, a known emulsifier (dispersant) can be used as the emulsifier (dispersant) for producing the polymer fine particles.

[0088] Specific examples of emulsifiers that can be used in the method for producing polymer microparticles are the same as those explained in the section (2-5. Emulsifier X) below, so the explanation therefor is incorporated by reference and will not be repeated here.

[0089] In the method for producing polymer microparticles, the emulsifier is preferably one or more selected from the group consisting of sulfur-based emulsifiers, phosphorus-based emulsifiers, sarcosinic acid-based emulsifiers, and carboxylic acid-based emulsifiers, more preferably one or more selected from the group consisting of sodium dodecylbenzenesulfonate, sodium polyoxyethylene lauryl ether phosphate, sodium N-lauroyl sarcosinate, alkyl ether carboxylate, and sodium palmitate, further preferably one or more selected from the group consisting of sodium dodecylbenzenesulfonate, sodium polyoxyethylene lauryl ether phosphate, and sodium N-lauroyl sarcosinate, and particularly preferably sodium N-lauroyl sarcosinate. This configuration has the advantages of high emulsifying power and improved quality of the resulting powder or granule.

[0090] When a polyfunctional monomer is used in the polymerization of the elastomer or the graft portion for the purpose of introducing a crosslinked structure into the elastomer or the graft portion, a known chain transfer agent can be used in a known amount range. By using the chain transfer agent, the molecular weight and / or degree of crosslinking of the obtained elastomer or the graft portion can be easily adjusted.

[0091] In the production of the polymer microparticles, in addition to the above-mentioned components, a surfactant may be further used. The type and amount of the surfactant used are within the known ranges.

[0092] In the production of polymer microparticles, the polymerization conditions such as polymerization temperature, pressure, and deoxidation may be appropriately set within known numerical ranges.

[0093] A latex containing polymer fine particles can be obtained by the above-mentioned method for producing polymer fine particles. That is, the description in the section (Method for producing polymer fine particles) can be used as a description regarding the method for producing latex.

[0094] (2-4. Coagulant solution) The term "coagulant solution" used in the manufacturing method of the present disclosure refers to a liquid coagulant, and a solution containing a solvent and a coagulant. In this specification, the coagulant solution according to one embodiment of the present disclosure (the coagulant solution used in the manufacturing method of the present disclosure) may be referred to as the "present coagulant solution." In the present coagulant solution, the coagulant may be dispersed or dissolved in the solvent.

[0095] In this specification, a liquid coagulant refers to a liquid substance that functions as a coagulant (i.e., a substance in which the solute itself is liquid without being dissolved or dispersed in a solvent). When using a liquid substance as a coagulant, the substance (coagulant) may be used after being dissolved or dispersed in a solvent to form a solution, or the substance (coagulant) may be used (sprayed) as a coagulant solution without being dissolved or dispersed in a solvent. In other words, the "coagulant solution" in the manufacturing method disclosed herein also includes the liquid substance itself that functions as a coagulant.

[0096] When a solution containing a solvent and a coagulant is used as the coagulant solution, the solvent for the coagulant solution is not particularly limited, but may be, for example, water.

[0097] The coagulant contained in the coagulant solution may be any substance that has the property of coagulating and coagulating polymer particles in a solution containing latex and additives. Examples of the coagulant include (i) inorganic acids (salts) and / or organic acids (salts) and (ii) polymer coagulants. One of these coagulants may be used alone, or two or more may be used in combination. In this specification, inorganic acids (salts) mean "inorganic acids and their salts," and organic acids (salts) mean "organic acids and their salts."

[0098] The coagulant solution is preferably an aqueous solution containing one or more substances selected from the group consisting of monovalent inorganic acids, salts of monovalent inorganic acids, divalent inorganic acids, salts of divalent inorganic acids, trivalent inorganic acids, salts of trivalent inorganic acids, etc. as coagulants. Examples of monovalent inorganic acids include (a) halogen acids such as chloric acid, bromic acid, and iodic acid, and (b) nitric acid, etc. Examples of divalent inorganic acids include sulfuric acid, etc. Examples of trivalent inorganic acids include phosphoric acid, etc. Examples of cationic elements or molecules that can form salts with these inorganic acids include alkali metals, alkaline earth metals, transition metals (especially iron and zinc), metals of Group 13 such as aluminum, and ammonium, etc.

[0099] The coagulant solution preferably contains, as a coagulant, one or more substances selected from the group consisting of monovalent organic acids, monovalent organic acid salts, divalent organic acids, divalent organic acid salts, etc. Examples of monovalent organic acids include formic acid, acetic acid, etc. Examples of monovalent organic acid salts include salts of formic acid, acetic acid, etc. with alkali metals, etc. Examples of divalent organic acids include oxalic acid, malic acid, maleic acid, malonic acid, tartaric acid, etc. Examples of divalent organic acid salts include salts of acetic acid, formic acid, etc. with alkaline earth metals, etc.

[0100] (i) Specific examples of inorganic acids (salts) and / or organic acids (salts) include: (a) Alkali metal halides, such as sodium chloride, potassium chloride, lithium chloride, sodium bromide, potassium bromide, lithium bromide, potassium iodide, and sodium iodide; alkali metal sulfides, such as potassium sulfate, sodium sulfate, and ammonium sulfate; ammonium chloride; alkali metal nitrates, such as sodium nitrate, potassium nitrate, and other inorganic salts, such as calcium chloride, ferrous sulfate, magnesium sulfate, zinc sulfate, copper sulfate, barium chloride, ferrous chloride, ferric chloride, magnesium chloride, ferric sulfate, aluminum sulfate, potassium alum, and iron alum; (b) Inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid, and phosphoric acid; (c) organic acids such as acetic acid, formic acid, and the like; and (d) Organic acid salts such as sodium acetate, calcium acetate, sodium formate, calcium formate, and the like, and salts of these organic acids;

[0101] The polymer coagulant is not particularly limited as long as it is a polymer compound having a hydrophilic group and a hydrophobic group. Examples of the polymer coagulant include anionic polymer coagulants, cationic polymer coagulants, and nonionic polymer coagulants. Among these, cationic polymer coagulants are preferred because they have the advantage of neutralizing the charge of the polymer particles.

[0102] The cationic polymer coagulant is preferably a polymer coagulant having a cationic group in the molecule, that is, a polymer coagulant that exhibits cationicity when dissolved in water. Specific examples of cationic polymer coagulants include polyamines, polydicyandiamides, cationic starch, cationic poly(meth)acrylamide, water-soluble aniline resins, polythiourea, polyethyleneimine, quaternary ammonium salts, polyvinylpyridines, chitosan, etc.

[0103] As the coagulant, among those mentioned above, (a) an aqueous solution of a monovalent or divalent inorganic acid salt such as sodium chloride, potassium chloride, sodium sulfate, ammonium chloride, calcium chloride, magnesium chloride, magnesium sulfate, or barium chloride, or (b) an aqueous solution of a monovalent or divalent inorganic acid such as hydrochloric acid or sulfuric acid, can be preferably used, since it can provide a powder or grain having a higher bulk density and a smaller amount of fine powder.

[0104] The concentration (amount) of the coagulant in the coagulant solution is not particularly limited, but for example, in the total amount of the coagulant solution (100% by weight), it is preferably 0.1% by weight to 45.0% by weight, more preferably 5.0% by weight to 40.0% by weight, even more preferably 10.0% by weight to 40.0% by weight, even more preferably 20.0% by weight to 40.0% by weight, and particularly preferably 30.0% by weight to 40.0% by weight. According to this configuration, the coagulant is more likely to exert its coagulation action on the polymer fine particles, and the amount of coagulant used in the second contact step can be reduced. As a result, there is an advantage that the production cost of the aggregate and powder can be reduced, and the amount of impurities derived from the coagulant contained in the obtained aggregate and powder can be reduced.

[0105] When the coagulant is a substance in a solid (e.g., powder) state, the concentration (wt%) of the coagulant in the coagulant solution can be calculated, for example, by the following method: 0.5 g of the coagulant solution is placed in a hot air convection dryer at a temperature higher than the boiling point of the solvent (e.g., the boiling point of the solvent + 20°C) for 3 hours to evaporate the solvent. Then, the weight (g) of the residue (solid content) after drying is measured. Next, the obtained value is divided by the weight of the coagulant solution before drying, 0.5 g, and the obtained value is further multiplied by 100. In addition, when the coagulant is in a liquid state, the concentration of the coagulant in the coagulant solution can also be measured by performing fractional distillation.

[0106] The coagulant solution can be obtained, for example, by mixing a solid (e.g., powder) substance that functions as a coagulant with a solvent. When mixing multiple types of coagulants, each coagulant may be (a) mixed with the solvent all at once, or (b) mixed individually. In addition, a commercially available coagulant that is dissolved or dispersed in a solvent in advance may be (a) used as it is as a coagulant solution, or (b) further mixed with a solvent before use.

[0107] (2-5. Emulsifier X) In the second production method, an emulsifier is added to the suspension in an emulsifier addition step. The "emulsifier used in the emulsifier addition step" may be referred to as "emulsifier X" in this specification to distinguish it from the "emulsifier used in the production of polymer microparticles (emulsion polymerization)".

[0108] The emulsifier X is not particularly limited, but examples thereof include anionic emulsifiers, nonionic emulsifiers, polyvinyl alcohol, alkyl-substituted cellulose, polyvinylpyrrolidone, polyacrylic acid derivatives, etc. Examples of the anionic emulsifier include sulfur-based emulsifiers, phosphorus-based emulsifiers, sarcosinic acid-based emulsifiers, and carboxylic acid-based emulsifiers. Examples of the sulfur-based emulsifier include sodium dodecylbenzenesulfonate (abbreviation: SDBS). Examples of the phosphorus-based emulsifier include sodium polyoxyethylene lauryl ether phosphate. Examples of the sarcosinic acid-based emulsifier include sodium N-lauroyl sarcosinate. Examples of the carboxylic acid-based emulsifier include alkyl ether carboxylate and sodium palmitate.

[0109] In the second manufacturing method, the emulsifier X is preferably one or more selected from the group consisting of sulfur-based emulsifiers, phosphorus-based emulsifiers, sarcosinic acid-based emulsifiers, and carboxylic acid-based emulsifiers, more preferably one or more selected from the group consisting of sodium dodecylbenzenesulfonate, sodium polyoxyethylene lauryl ether phosphate, sodium N-lauroyl sarcosinate, alkyl ether carboxylate, and sodium palmitate, further preferably one or more selected from the group consisting of sodium dodecylbenzenesulfonate, sodium polyoxyethylene lauryl ether phosphate, sodium N-lauroyl sarcosinate, alkyl ether carboxylate, and sodium palmitate, and particularly preferably sodium N-lauroyl sarcosinate. This configuration has the advantages of high emulsifying power and improved quality of the resulting powder or granule.

[0110] The emulsifier X may be the same as or different from the emulsifier used in the production of polymer fine particles (emulsion polymerization).

[0111] (2-6.Device) The apparatus used in the manufacturing method of the present disclosure (hereinafter, sometimes referred to as manufacturing apparatus or apparatus) is not particularly limited, but may be an apparatus equipped with a container having a substantially vertical inner wall. The container preferably includes a gas phase region. In this specification, the vertically extending inner wall of the container may be referred to as a "side wall". The container preferably includes a first nozzle on the upper part (top) or side wall surface of the container for spraying and / or dropping latex, for example, into the gas phase, and a second nozzle on the upper part (top) or side wall surface of the container for spraying and / or dropping a coagulant solution containing a coagulant, for example, into the gas phase.

[0112] The shape of the container is not particularly limited, but is preferably cylindrical. When the container is cylindrical, the diameter thereof is preferably, for example, 30 cm to 500 cm.

[0113] The container may have a receiving tank having a liquid phase region at the bottom. The case where the container has a gas phase region and is provided with a receiving tank having a liquid phase region (hereinafter also referred to as "Case E") will be described.

[0114] In case E, the aggregates generated in the gas phase may fall in the gas phase and drop into the liquid phase of the receiving tank. In other words, in case E, the aggregates of polymer fine particles generated in the gas phase are collected in the liquid phase. More specifically, in case E, the combined droplets formed after the latex droplets and the coagulant solution droplets come into contact with each other in the gas phase may contain aggregates of polymer fine particles, and the droplets may fall in the gas phase and enter the liquid phase. Therefore, in case E, after the start of the contacting step, the liquid phase may contain uncoagulated polymer fine particles, aggregates of polymer fine particles, components other than the polymer fine particles contained in the latex (including the solvent of the latex), the coagulant, and components other than the coagulant contained in the coagulant solution (including the solvent of the coagulant solution).

[0115] In case E, when the container has a receiving tank having a liquid phase region, the height from the top of the container to the liquid level of the liquid phase in the receiving tank at the bottom is preferably 50 cm to 10 m, more preferably 1 m to 5 m, and further preferably 2 m to 3 m, from the viewpoint of appropriately progressing coagulation of polymer fine particles in the latex in the gas phase.

[0116] In case E, the liquid phase is not particularly limited, but may be, for example, water or water (aqueous solution) containing a coagulant. The liquid phase may be a coagulant solution. In other words, the liquid phase may contain a coagulant.

[0117] In case E, the coagulant that the liquid phase may contain is preferably a coagulant contained in the coagulant solution sprayed and / or dropped from the second nozzle. In case E, the coagulant that the liquid phase may contain may be a different type of coagulant from the coagulant contained in the coagulant solution sprayed and / or dropped from the second nozzle.

[0118] In case E, the concentration (amount) of the coagulant in the liquid phase is not particularly limited, but may be, for example, lower than the concentration (amount) of the coagulant in the coagulant solution sprayed and / or dropped from the second nozzle. This configuration has the advantage of reducing the amount of remaining impurities contained in the aggregate.

[0119] In case E, the concentration (amount) of the coagulant in the liquid phase is, for example, preferably 0.01% by weight to 10.00% by weight, more preferably 0.05% by weight to 5.00% by weight, even more preferably 0.10% by weight to 3.00% by weight, even more preferably 0.25% by weight to 2.00% by weight, and particularly preferably 0.50% by weight to 1.50% by weight. The higher the concentration (amount) of the coagulant in the liquid phase, the more it is possible to promote the coagulation of the dropped aggregates that are not sufficiently coagulated. The lower the concentration (amount) of the coagulant in the liquid phase, the more advantageous it is to prevent the aggregates from fusing together and becoming coarse.

[0120] The container may be connected, as necessary, to a recovery device for recovering the resulting agglomerates from the container, a drying device for drying the recovered agglomerates to obtain powder or granular material, and a temperature control device for adjusting the temperature inside the container or the temperature of each solution and liquid phase sprayed and / or dropped into the container.

[0121] (2-7. Contact process) The manufacturing method of the present disclosure includes a contacting step of spraying and / or dropping latex containing polymer fine particles from a first nozzle, and further spraying and / or dropping a coagulant solution containing a coagulant from a second nozzle, thereby contacting the latex droplets with the coagulant solution droplets. In a preferred embodiment of the contacting step, the container includes a gas phase region, and the latex containing polymer fine particles is sprayed and / or dropped into the gas phase from the first nozzle, and further sprayed and / or dropped into the gas phase with the coagulant solution containing a coagulant from the second nozzle. This allows the latex droplets and the coagulant solution droplets to come into contact with each other in the gas phase of the container. The latex droplets and the coagulant solution droplets that have come into contact with each other may be integrated (unified). Therefore, the contacting step can be said to be (a) a step of integrating (unifying) droplets of latex and droplets of coagulant solution, (b) a step of obtaining droplets containing latex and coagulant solution, and (c) a step of preparing droplets containing latex and coagulant solution. Moreover, the droplets containing latex and coagulant solution obtained in the contacting step can be said to be "droplets of latex and coagulant solution integrated together" or "droplets of a solution containing polymer fine particles derived from latex and a coagulant derived from the coagulant solution."

[0122] In the contact step, the polymer microparticles may be coagulated in droplets formed by the integration of the latex and the coagulant solution. When the latex containing the polymer microparticles is sprayed and / or dropped into the gas phase from the first nozzle, and the coagulant solution containing the coagulant is further sprayed and / or dropped into the gas phase from the second nozzle, the aggregates of the polymer microparticles may be generated in the gas phase. Therefore, the contact step can be said to be a step of coagulating the polymer microparticles, or a step of preparing the aggregates of the polymer microparticles.

[0123] In this specification, "spraying" a liquid (e.g., latex and coagulant solution) means spraying (spraying in mist) the liquid in a state where the liquid is compressed, ultrasonically treated, or otherwise formed into droplets (microdroplets) having a diameter smaller than the diameter of the nozzle outlet (hole) through which the liquid is sprayed. In this specification, "dripping" a liquid (e.g., latex and coagulant solution) means spraying the liquid as droplets having a diameter similar to the diameter of the nozzle outlet (hole) through which the liquid is sprayed, without any particular treatment. Note that when spraying a liquid using a two-fluid nozzle, even if the liquid itself to be sprayed is not pressurized, the liquid is considered to be "sprayed" when a substance other than the liquid (e.g., gas) is sprayed simultaneously in a pressurized state to spray the liquid in the form of microdroplets.

[0124] In the contact step, when the latex is sprayed, the direction of spraying is not particularly limited and may be vertical, horizontal or oblique. In the contact step, when the latex is dropped, the latex is usually dropped in a vertical direction, but is not limited thereto. In the contact step, it is preferable to spray and / or drop the latex in a vertical direction, since this has the advantage that the aggregates can be efficiently collected.

[0125] In the contact step, when the coagulant solution is sprayed, the direction of spraying is not particularly limited and may be vertical, horizontal or oblique. In the contact step, when the coagulant solution is dropped, the coagulant solution is usually dropped in a vertical direction, but is not limited thereto. In the contact step, it is preferable to spray the coagulant solution in a horizontal direction, since this has the advantage of efficiently bringing the droplets of latex and the droplets of the coagulant solution into contact with each other.

[0126] In this specification, the term "vertical direction" refers to the "weight direction." The "vertical direction" can also be referred to as the "vertical downward direction."

[0127] In one embodiment of the present invention, when a liquid (e.g., latex and coagulant solution) is "sprayed and / or dropped in a vertical direction," it is not necessary to spray and / or drop the liquid in a completely vertical direction. For example, the liquid may be sprayed and / or dropped in a direction inclined within a range of 15°, 10°, or 5° with respect to the vertical direction. That is, "sprayed and / or dropped in a vertical direction" in this specification is a concept including the aspect of spraying and / or dropping at an angle to the vertical direction. In this specification, the direction in which the liquid (e.g., latex and coagulant solution) is sprayed and / or dropped can be said to be the direction in which the nozzle of the nozzle that sprays or drops the liquid faces. In other words, the direction in which the liquid is sprayed or dropped can be adjusted by adjusting the direction in which the nozzle of the nozzle that sprays or drops the liquid faces.

[0128] In this specification, the term "horizontal direction" refers to a direction perpendicular to the vertical direction. The "horizontal direction" can also be said to be a direction perpendicular to the weight direction.

[0129] In one embodiment of the present invention, when a liquid (e.g., latex, an additive solution, or a coagulant solution) is "sprayed (or dripped) in a horizontal direction," the liquid does not necessarily have to be sprayed (or dripped) in a completely horizontal direction, and may be sprayed (or dripped) in a direction tilted within a range of 15°, 10°, or 5° from the horizontal direction as a reference. In other words, "sprayed (or dripped) in a horizontal direction" in this specification includes a mode in which the liquid is sprayed (or dripped) at an angle relative to the horizontal direction in this manner.

[0130] The first nozzle used in the contact step will be described. The first nozzle is not particularly limited as long as it can spray and / or drop the latex, but is preferably a pressure nozzle, a two-fluid nozzle, an ultrasonic nozzle, a high-frequency device, or a dropping nozzle. Among them, the first nozzle is more preferably a pressure nozzle, and even more preferably a swirl-flow type pressure nozzle (swirl-flow type nozzle), because it can easily spray droplets having a volume average droplet diameter of 200 μm to 400 μm and a sharp particle size distribution, and is economically superior among nozzles capable of spraying such droplets.

[0131] The diameter of the first nozzle is not particularly limited, but is preferably 0.01 mm to 2.00 mm, more preferably 0.05 mm to 1.50 mm, and even more preferably 0.10 mm to 1.00 mm. When the diameter is 2.00 mm or less, there is no risk that the droplets of the sprayed and / or dropped latex become excessively large, and the polymer fine particles in the droplets containing the latex and the coagulant solution obtained in the contact step can be sufficiently aggregated, and as a result, a powder with a high bulk density can be obtained. In addition, when the diameter is 0.01 mm or more, the possibility of the nozzle being blocked during the spraying or dropping of the latex can be reduced, and the aggregates can be stably produced.

[0132] The spray pressure of the first nozzle is, for example, 0.5 kg / cm 2 ~30.0kg / cm 2 and preferably 1.0 kg / cm 2 ~10.0kg / cm 2 It is more preferable that the spray pressure of the first nozzle is 0.5 kg / cm. 2 If the spray pressure of the first nozzle is 30.0 kg / cm or more, the droplets of the sprayed latex do not become excessively large, and the polymer fine particles in the droplets containing the latex and the coagulant solution obtained in the contacting step can be sufficiently aggregated, so that a powder having a high bulk density can be obtained. 2 If the amount is equal to or less than this, there is no risk that the droplets of the sprayed latex will become excessively small, and the amount of fine powder in the resulting powder or granule can be reduced.

[0133] The first nozzle is preferably located at or near the top of the vessel.

[0134] In this specification, the vertical distance between the center of the outlet of the first nozzle and the bottom surface of the container is referred to as the "vertical distance between the first nozzle and the bottom surface." In this specification, the "vertical distance between the center of the outlet of the first nozzle and the bottom surface of the container" refers to the "distance between the center of the outlet of the first nozzle and the liquid level of the liquid phase" when the container is provided with a receiving tank having a liquid phase area, and refers to the "distance between the center of the outlet of the first nozzle and the bottom surface of the bottom of the container" when the container is not provided with a receiving tank having a liquid phase area. In addition, when there are multiple first nozzles, the shortest (closest) value among the vertical distances between the center of the outlet of each first nozzle and the bottom surface of the container is referred to as the vertical distance between the first nozzle and the bottom surface.

[0135] In order to ensure a sufficient solidification time and provide powder having better powder properties, the vertical distance between the first nozzle and the bottom surface is preferably 100 cm or more, more preferably 150 cm or more, and particularly preferably 200 cm or more. In order to prevent the device from becoming excessively large, the upper limit of the vertical distance between the first nozzle and the bottom surface is preferably 300 cm or less.

[0136] The tip angle of the spray cone of the latex sprayed and / or dropped from the first nozzle is not particularly limited, but is preferably 5° to 140°, and more preferably 30° to 90°. When the angle of the spray cone of the latex is in the above range, (i) aggregates can be produced efficiently, and (ii) excessive enlargement of the device used for producing the aggregates can be suppressed. Furthermore, (iii) by setting the tip angle of the spray cone to 5° or more, it is possible to suppress the coalescence of the sprayed and / or dropped latex droplets, and (iv) by setting the tip angle of the spray cone to 140° or less, it is possible to suppress the adhesion of the sprayed and / or dropped latex droplets to the wall surface of the device for producing the aggregates, and since it is not necessary to enlarge the device to prevent the adhesion of the latex droplets to the wall surface, the device can be made smaller. In this specification, the term "spray cone" refers to an aggregate of droplets of the liquid sprayed and / or dropped from the nozzle outlet, observed when the liquid is sprayed and / or dropped. The shape of the spray cone of the latex is not particularly limited, and may be, for example, a fan shape, a cone shape, or a hollow cone shape.

[0137] The number of the first nozzles is not particularly limited and may be one or more than one. When two or more nozzles are used as the first nozzles, (a) each nozzle may only spray latex, (b) each nozzle may only drip latex, or (c) at least one nozzle may spray latex while at least another nozzle drips latex.

[0138] The second nozzle used in the contact step will be described. The second nozzle is not particularly limited as long as it can spray the coagulant solution, but is preferably a pressure nozzle (one-fluid nozzle), a two-fluid nozzle, an ultrasonic nozzle or a high-frequency device, and more preferably a pressure nozzle (one-fluid nozzle) or a two-fluid nozzle. When a pressure nozzle (one-fluid nozzle) or a two-fluid nozzle is used as the second nozzle, it is possible to spray the coagulant solution with fine droplets (in the form of a spray), and it is possible to efficiently contact the droplets of the latex with the droplets of the coagulant solution.

[0139] The diameter of the second nozzle is not particularly limited, but is preferably 0.01 mm to 2.00 mm, more preferably 0.05 mm to 1.50 mm, and even more preferably 0.10 mm to 1.00 mm. If the diameter is 2.00 mm or less, there is no risk that the droplets of the sprayed coagulant solution will become excessively large, and the polymer fine particles in the droplets containing the latex and the coagulant solution can be sufficiently aggregated, resulting in a powder with a high bulk density. In addition, if the diameter is 0.01 mm or more, the possibility of the nozzle being blocked during spraying of the coagulant solution can be reduced, and the aggregates can be stably produced.

[0140] The spray pressure of the second nozzle is, for example, 0.5 kg / cm 2 ~100.0kg / cm 2 and preferably 1.0 kg / cm 2 ~50.0kg / cm 2 It is more preferable that the spray pressure of the second nozzle is 0.5 kg / cm. 2 If the spray pressure of the second nozzle is 100.0 kg / cm or more, the droplets of the coagulant solution sprayed are not excessively large, and the droplets of the latex and the droplets of the coagulant solution can be efficiently contacted with each other. As a result, a powder having a high bulk density can be obtained. In addition, if the spray pressure of the second nozzle is 100.0 kg / cm or more, the droplets of the latex and the droplets of the coagulant solution can be efficiently contacted with each other. 2 If the amount is less than this, the droplets of the coagulant solution do not scatter excessively, can be efficiently brought into contact with the droplets containing latex and the coagulant solution, and adhesion of the coagulant solution to the container wall surface can be reduced.

[0141] The second nozzle is preferably installed on the inner wall surface (or near the inner wall surface) of the container.

[0142] In this specification, the vertical distance between the center of the outlet of the second nozzle and the bottom surface of the container is referred to as the "vertical distance between the second nozzle and the bottom surface." In this specification, the "vertical distance between the center of the outlet of the second nozzle and the bottom surface of the container" refers to the "distance between the center of the outlet of the second nozzle and the liquid level of the liquid phase" when the container is equipped with a receiving tank having a liquid phase area, and refers to the "distance between the center of the outlet of the second nozzle and the bottom surface of the bottom of the container" when the container is not equipped with a receiving tank having a liquid phase area. In addition, when there are multiple second nozzles, the shortest (closest) value among the vertical distances between the center of the outlet of each second nozzle and the bottom surface of the container is regarded as the vertical distance between the second nozzle and the bottom surface.

[0143] In order to ensure a sufficient solidification time and provide powder with better powder properties, the vertical distance between the second nozzle and the bottom surface is preferably 50 cm or more, and more preferably 60 cm or more. The vertical distance between the second nozzle and the bottom surface may be 70 cm or more, 80 cm or more, 90 cm or more, or 100 cm or more. In order to prevent the device from becoming excessively large, the upper limit of the vertical distance between the second nozzle and the bottom surface is preferably 280 cm or less, and more preferably 250 cm or less.

[0144] The vertical distance between the first nozzle and the second nozzle is not particularly limited. Since the second nozzle can efficiently bring the latex droplets and the coagulant solution droplets into contact with each other, the vertical distance between the first nozzle and the second nozzle is preferably 3 cm to 50 cm, more preferably 5 cm to 40 cm, further preferably 7 cm to 30 cm, and particularly preferably 10 cm to 25 cm.

[0145] The horizontal distance between the first nozzle and the second nozzle is not particularly limited. From the viewpoint of (a) efficiently contacting the droplets of latex with the droplets of the coagulant solution and (b) preventing the device from becoming excessively large, the horizontal distance between the first nozzle and the second nozzle is preferably 50 cm or less, and may be 30 cm or less.

[0146] In this specification, the "vertical distance between the first nozzle and the second nozzle" and the "horizontal distance between the first nozzle and the second nozzle" are values ​​measured by the following method: (1) drawing a vertical line passing through the center of the outlet (hole) of the first nozzle (first line); (2) drawing a horizontal line (perpendicular to the vertical direction) passing through the center of the outlet (hole) of the second nozzle (second line); (3) the vertical distance between the intersection of the first line and the second line and the center of the outlet of the first nozzle is defined as the "vertical distance between the first nozzle and the second nozzle", and the horizontal distance between the intersection of the first line and the second line and the center of the outlet of the second nozzle is defined as the "horizontal distance between the first nozzle and the second nozzle". In addition, when there are multiple nozzles to be compared in distance (for example, when there are multiple first nozzles and multiple second nozzles), the shortest (closest) value among the distances between nozzles of different types is determined to be the distance between the nozzles.

[0147] When the first nozzle and the second nozzle are both located at or near the top of the vessel, the horizontal distance between the first nozzle and the second nozzle can be zero. do.

[0148] The tip angle of the spray cone of the coagulant solution sprayed from the second nozzle is not particularly limited, but is preferably 5° to 140°, and more preferably 30° to 90°. When the angle of the spray cone of the coagulant solution is in the above range, (i) the droplets containing the latex and the additive solution can be efficiently brought into contact with the droplets of the coagulant solution, so that the aggregates can be efficiently produced, and (ii) the excessive increase in size of the device used for producing the aggregates can be suppressed. Furthermore, (iii) in particular, by setting the tip angle of the spray cone to 5° or more, it is also possible to suppress the droplets of the sprayed coagulant solution from coalescing with each other. In addition, the shape of the spray cone of the coagulant solution is not particularly limited, and may be, for example, a fan shape, a cone shape, or a hollow cone shape.

[0149] The number of the second nozzles is not particularly limited, and may be one, or may be two or more.

[0150] The volume average droplet diameter of the droplets of latex sprayed and / or dropped in the contact step is preferably 50 μm to 5 mm, more preferably 100 μm to 800 μm, further preferably 150 μm to 600 μm, and particularly preferably 200 μm to 400 μm. If the volume average droplet diameter of the droplets of latex sprayed and / or dropped is 50 μm or more, the amount of fine powder in the resulting powder or granule can be reduced. If the volume average droplet diameter of the droplets of latex sprayed and / or dropped is 5 mm or less, the polymer fine particles in the droplets containing the latex and coagulant solution obtained in the contact step can be sufficiently aggregated, and as a result, a powder or granule with a high bulk density can be obtained.

[0151] The volume average droplet diameter of the droplets of the coagulant solution sprayed in the contact step is preferably 0.01 μm to 500.00 μm, more preferably 0.05 μm to 100.00 μm, and even more preferably 0.10 μm to 50.00 μm. According to the above configuration, the droplets of latex and the droplets of the coagulant solution can be efficiently contacted with each other, and the polymer fine particles in the droplets containing the latex and the coagulant solution can be sufficiently aggregated. As a result, there is an advantage that a powder having a high bulk density can be obtained.

[0152] The volume average droplet diameter of the latex droplets and the coagulant solution droplets can be measured, for example, by a laser diffraction type spray droplet diameter measuring device.

[0153] In the contact step, the amount of the coagulant to be brought into contact with the droplets of latex can be appropriately adjusted depending on the type (composition) of the polymer fine particles, the type of the coagulant, the concentration of the polymer fine particles in the latex, and the concentration of the coagulant in the coagulant solution. In this specification, the "amount of the coagulant to be brought into contact with the droplets of latex" refers to the amount of the coagulant in the coagulant solution sprayed per unit time relative to the total amount of the polymer fine particles in the latex sprayed and / or dropped per unit time in the contact step. Since there are advantages that (a) the generation of unagglomerated polymer fine particles can be prevented, more aggregates of the polymer fine particles can be obtained, and (b) the amount of coagulant-derived impurities contained in the obtained aggregates and powder can be reduced, the amount of the coagulant to be brought into contact with the droplets of latex is preferably 1 to 30 parts by weight, more preferably 2 to 20 parts by weight, and even more preferably 3 to 15 parts by weight, relative to the total amount of the polymer fine particles in the latex sprayed and / or dropped per unit time (100 parts by weight). In addition, the "amount of coagulant to be brought into contact with the Lalatex droplets" in the contacting step can be adjusted by appropriately changing the concentration of the coagulant in the coagulant solution, the amount of coagulant solution sprayed per unit time, etc.

[0154] The temperature of the latex when subjected to the contact step (immediately before spraying and / or dropping) is not particularly limited. The temperature of the latex when subjected to the contact step is, for example, preferably 1°C to 100°C, more preferably 1°C or higher and less than 100°C, more preferably 5°C to 80°C, even more preferably 10°C to 70°C, even more preferably 15°C to 50°C, and particularly preferably 20°C to 30°C. When the temperature of the latex when subjected to the contact step is within the above range, there is an advantage that the stability of the latex can be ensured.

[0155] The temperature of the coagulant solution when subjected to the contact step (immediately before spraying and / or dropping) is not particularly limited. The temperature of the coagulant solution when subjected to the contact step is, for example, preferably 1°C to 100°C, more preferably 1°C or more and less than 100°C, more preferably 5°C to 80°C, even more preferably 10°C to 70°C, even more preferably 15°C to 50°C, and particularly preferably 20°C to 30°C. The temperature of the coagulant solution when subjected to the contact step may be the same as or different from the temperature of the latex when subjected to the contact step. When the temperature of the coagulant solution when subjected to the contact step is within the above range, there are advantages such as (a) the advantage that the precipitation of the coagulant in the coagulant solution can be suppressed, and (b) the advantage that the evaporation of the solvent of the coagulant solution can be suppressed, and the concentration of the coagulant solution can be kept constant.

[0156] The temperature in the container in the contact step is not particularly limited, but is preferably 1°C to 100°C, more preferably 1°C or more and less than 100°C, more preferably 5°C to 90°C, more preferably 10°C to 85°C, more preferably 20°C to 80°C, more preferably 30°C to 75°C, even more preferably 40°C to 70°C, and particularly preferably 50°C to 70°C. When the temperature in the container in the contact step is within the above range, the polymer fine particles in the droplets containing the latex and the coagulant solution can be sufficiently aggregated, and as a result, a powder having a high bulk density can be obtained. The temperature in the container in the contact step can be controlled, for example, by feeding water vapor into the container. When the container has a gas phase region, the "temperature in the container" can also be called the "temperature of the gas phase".

[0157] In the manufacturing method of the present disclosure, in the contact step, water may be allowed to flow down along the inner wall surface of the container. This can prevent the sprayed and / or dripped latex and coagulant solution, and the generated aggregates, from adhering to the inner wall surface of the container. The amount of water (flowing water) allowed to flow down along the inner wall surface is not particularly limited, but is preferably 10 parts by weight to 10,000 parts by weight per 100 parts by weight of polymer fine particles in the latex. When the amount of water allowed to flow down along the inner wall surface of the container is within the above range, the latex and coagulant solution, and the generated aggregates can be prevented from adhering to the inner wall surface of the container, and there is no risk of the load of wastewater treatment becoming excessively high. The temperature of the water allowed to flow down along the inner wall surface is preferably 0°C to 100°C, more preferably 10°C to 90°C, from the viewpoint of simplifying the flowing down operation.

[0158] In the contact step, aggregates of polymer fine particles are generated, and a suspension containing the aggregates can be obtained. The form of the suspension is not particularly limited, and the following methods can be used: (1A) The latex and the coagulant solution sprayed and / or dropped in the contact step contain a solvent (e.g., water). Therefore, a mixture containing the aggregates, the coagulant, the solvent in the latex, and the solvent in the coagulant solution can be obtained, for example, at the bottom of the container. The mixture can be made into a suspension; (2A) As mentioned above, the vessel may include a receiving tank having a region of a liquid phase. In this case (i.e., in case E), the aggregates formed in the gas phase, together with the droplets containing the aggregates, descend through the gas phase and enter (fall into) the liquid phase provided at the bottom of the vessel. This results in a suspension containing the liquid phase, the aggregates, the coagulant, the solvent in the latex, and the solvent in the coagulant solution. Therefore, in case E, the contacting step can also be said to be a step of preparing a suspension; (3A) In the contact step, when water is allowed to flow down along the inner wall surface of the container, a mixture containing the aggregates, the coagulant, the solvent in the latex, the solvent in the coagulant solution, and the flowing water can be obtained, for example, at the bottom of the container. The mixture can be made into a suspension; (4A) In the case of case E, when water is allowed to flow down along the inner wall surface of the container, a mixture containing the liquid phase, the aggregates, the coagulant, the solvent in the latex, the solvent in the coagulant solution, and the flowing water can be obtained, for example, at the bottom of the container. The mixture can be made into a suspension; (5A) The mixture obtained in (1A) above or the mixed liquid obtained in (3A) or (4A) above may be removed from the container and added to another container containing a liquid phase to obtain a mixture or a mixed liquid consisting of the mixed liquid and a liquid phase, and the mixed liquid may be made into a suspension; (6A) A separate container containing a liquid phase may be connected to the container. The case where a separate container containing a liquid phase is connected to the container (hereinafter also referred to as "Case F") will be described. In Case F, the mixture obtained in (1A) above or the mixed liquid obtained in (3A) or (4A) above may be transferred from the container to a separate container containing a liquid phase to obtain a mixture or a mixed liquid consisting of the mixed liquid and the liquid phase, and the mixed liquid may be made into a suspension. In addition, in Case F and when water is made to flow down along the inner wall surface of the container, the mixed liquid containing the aggregates, the solvent in the latex, the solvent in the coagulant solution, and the flowing water may be transferred from the container to a separate container containing a liquid phase by the flowing water, and a mixture or a mixed liquid consisting of the mixed liquid and the liquid phase may be obtained, and the mixed liquid may be made into a suspension.

[0159] In any of the above cases, the suspension may contain uncoagulated polymer microparticles, aggregates of polymer microparticles, components other than the polymer microparticles contained in the latex (including the solvent for the latex), a coagulant, and components other than the coagulant contained in the coagulant solution (including the solvent for the coagulant solution).

[0160] In any of the above cases, the concentration of the polymer fine particles in the suspension can be appropriately adjusted by adding a solvent such as water to the obtained suspension.

[0161] In the above (2A), (4A) to (6A), the temperature of the liquid phase is not particularly limited, but is, for example, preferably 1° C. to 100° C., more preferably 5° C. to 90° C., more preferably 10° C. to 85° C., more preferably 20° C. to 80° C., more preferably 30° C. to 75° C., even more preferably 40° C. to 70° C., and particularly preferably 50° C. to 70° C. This step has the advantage that insufficiently coagulated aggregates can be sufficiently coagulated, and as a result, a powder or granular material with a high bulk density can be obtained.

[0162] (2-8. Emulsifier addition process) The second production method includes an emulsifier addition step, which can be said to be a step of preparing a suspension containing at least aggregates of polymer fine particles and emulsifier X. In the second production method, the emulsifier addition step is carried out after the contact step and before the heat treatment step.

[0163] In the first production method, an emulsifier addition step may be carried out. When the emulsifier addition step is carried out in the first production method, the emulsifier addition step is preferably carried out after the contact step and before the heat treatment step.

[0164] In the emulsifier addition step, emulsifier X itself may be added to the suspension, or emulsifier X may be mixed with any solvent such as water, and the resulting mixture (emulsifier X solution) may then be added to the suspension.

[0165] In the emulsifier adding step, it is preferable to add the emulsifier to the suspension and then stir the resulting suspension. Alternatively, it is preferable to add the emulsifier to the stirred suspension in the emulsifier adding step. According to these configurations, the emulsifier can be uniformly or approximately uniformly dispersed in the suspension.

[0166] In the emulsifier addition step, it is preferable to add emulsifier X to the suspension so that the amount of emulsifier X in the suspension obtained through the emulsifier addition step is 0.002% by weight to 0.045% by weight in 100% by weight of the suspension. The "suspension obtained through the emulsifier addition step" can also be called (i) the "suspension to be heat-treated" in the heat treatment step of the second production method, and (ii) when the emulsifier addition step is performed in the first production method, it can also be called the "suspension to be heat-treated" in the heat treatment step of the first production method.

[0167] In the emulsifier addition step, when emulsifier X is mixed with any solvent such as water and the resulting mixture (emulsifier X solution) is added to the suspension, the temperature of the emulsifier X solution is not particularly limited. The temperature of the emulsifier X solution is, for example, preferably 1°C to 100°C, more preferably 1°C or higher and less than 100°C, more preferably 5°C to 80°C, even more preferably 10°C to 70°C, even more preferably 15°C to 50°C, and particularly preferably 20°C to 30°C. This configuration has the advantage that the solvent is less likely to evaporate and the concentration of emulsifier X in the mixture is stable.

[0168] The temperature of the suspension in the emulsifier addition step is not particularly limited, but for example, it is preferably 1°C to 100°C, more preferably 1°C or higher and less than 100°C, more preferably 5°C to 90°C, more preferably 10°C to 85°C, more preferably 20°C to 80°C, more preferably 30°C to 75°C, even more preferably 40°C to 70°C, and particularly preferably 50°C to 70°C. When the temperature of the suspension in the emulsifier addition step is within the above range, there is an advantage that the emulsifier X is sufficiently dispersed in the suspension and fusion of the coagulated body can be prevented. The temperature of the suspension in the emulsifier addition step can be controlled, for example, by supplying water vapor to the suspension.

[0169] (2-9. Heat treatment process) The manufacturing method of the present disclosure includes a heat treatment step of heat-treating the suspension after the contact step, which causes the agglomerates to compact and become more dense, thereby obtaining a powder with a higher bulk density.

[0170] When the first manufacturing method does not include an emulsifier addition step, the heat treatment step is carried out after the contact step. When the first manufacturing method does not include an emulsifier addition step, the heat treatment step is a step of heat treating the suspension containing aggregates of polymer microparticles obtained in the contact step. When the first manufacturing method includes an emulsifier addition step, the heat treatment step is carried out after the emulsifier addition step. When the first manufacturing method includes an emulsifier addition step, the heat treatment step is a step of heat treating the suspension obtained in the emulsifier addition step. In the second manufacturing method, the heat treatment step is carried out after the emulsifier addition step. The heat treatment step in the second manufacturing method is a step of heat treating the suspension obtained in the emulsifier addition step.

[0171] In the first manufacturing method, in the heat treatment step, the concentration of the polymer microparticles in 100% by weight of the suspension is 3% by weight to 50% by weight. In the heat treatment step of the first manufacturing method, the concentration of the polymer microparticles in 100% by weight of the suspension is preferably 5% by weight or more, more preferably 8% by weight or more, more preferably 10% by weight or more, more preferably 13% by weight or more, more preferably 15% by weight or more, more preferably 18% by weight or more, more preferably 20% by weight or more, even more preferably 23% by weight or more, and particularly preferably 25% by weight or more. The higher the concentration of the polymer microparticles in the suspension, the higher the bulk density of the powdered granules that can be obtained. In the heat treatment step of the first manufacturing method, the concentration of the polymer microparticles in 100% by weight of the suspension is preferably 45% by weight or less, more preferably 40% by weight or less, even more preferably 35% by weight or less, and particularly preferably 30% by weight or less. The higher the concentration of the polymer microparticles in the suspension, the more uniform the heat treatment can be performed on the whole, and the coarse graining of the aggregates due to the heat treatment can be prevented.

[0172] In the second production method, the concentration of the polymer fine particles in 100% by weight of the suspension in the heat treatment step is not particularly limited. In the heat treatment step of the second manufacturing method, for example, the concentration of the polymer microparticles may be 0.10% by weight or more and less than 10.00% by weight. In the heat treatment step of the second manufacturing method, the concentration of the polymer microparticles in 100% by weight of the suspension is preferably 0.50% by weight or more, more preferably 1.00% by weight or more, preferably 2.00% by weight or more, more preferably 3.00% by weight or more, even more preferably 5.00% by weight or more, and particularly preferably 8.00% by weight or more. The higher the concentration of the polymer microparticles in the suspension, the more advantageous it is that a powder with a large bulk density can be obtained with a smaller amount of emulsifier. In the heat treatment step of the second manufacturing method, the concentration of the polymer microparticles may be the same as the concentration of the polymer microparticles in the suspension in the heat treatment step of the first manufacturing method.

[0173] In the second manufacturing method, in the heat treatment step, the amount of emulsifier X in 100% by weight of the suspension is 0.002% by weight to 0.045% by weight. In the heat treatment step of the second manufacturing method, the amount of emulsifier X in 100% by weight of the suspension is particularly preferably 0.003% by weight or more. The greater the amount of emulsifier X in the suspension, the more advantageous it is that the more the fusion of aggregates during heat treatment can be prevented. In the heat treatment step of the second manufacturing method, the amount of emulsifier X in 100% by weight of the suspension is preferably 0.040% by weight or less, more preferably 0.035% by weight or less, more preferably 0.030% by weight or less, even more preferably 0.025% by weight or less, and particularly preferably 0.020% by weight or less. The smaller the amount of emulsifier X in the suspension, the more advantageous it is that the amount of emulsifier remaining in the powder or granule is reduced, and the quality of the powder or granule is improved.

[0174] In the heat treatment step, the method for heat treating the suspension is not particularly limited, but may be, for example, a method in which high-temperature (for example, 130° C.) water vapor is fed into the suspension.

[0175] In the heat treatment step, the suspension in the container may be heat-treated in the container after the contact step, or the suspension in the container may be removed from the container and heat-treated in a separate container.

[0176] In the heat treatment step, the temperature of the suspension (heat treatment temperature) is not particularly limited, but is preferably 60° C. to 130° C., more preferably 65° C. to 125° C., more preferably 70° C. to 120° C., more preferably 75° C. to 115° C., more preferably 80° C. to 110° C., even more preferably 85° C. to 105° C., and particularly preferably 90° C. to 100° C. This configuration has the advantages of allowing the aggregate to be sufficiently heat-treated and simplifying the equipment.

[0177] In the heat treatment step, the time for heat treating the suspension is not particularly limited, but is preferably 30 seconds or more, more preferably 1 minute or more, even more preferably 2 minutes or more, and particularly preferably 3 minutes or more. According to this configuration, the suspension can be heat treated sufficiently, so that the aggregates are sufficiently densified, and as a result, a powder having a smaller bulk density can be obtained. Note that, since the longer the heat treatment time, the more energy is consumed, so from the viewpoint of energy saving and low fuel consumption, the upper limit of the heat treatment time can be appropriately set, and for example, it is preferable that it is 15 minutes or less.

[0178] It is preferable that the manufacturing method according to the present disclosure further includes, after the heat treatment step, a recovery step of recovering the agglomerates from the suspension, and a drying step of drying the recovered agglomerates.

[0179] (2-10. Recovery process) The recovery step is a step of recovering the aggregates from the suspension, or the recovery step can be said to be a step of separating the aggregates from the suspension.

[0180] The method for separating the aggregates from the suspension (separation method) is not particularly limited, and for example, centrifugal dehydration, static separation, filtration dehydration (e.g., suction filtration), squeeze dehydration, or water evaporation can be applied. In addition, the equipment for carrying out the above-mentioned various separation methods can be appropriately selected according to the desired separation method. For example, a screw press, a roller press, a belt screen, a vibrating sieve, a multi-plate vibrating filter, a suction filter, a vacuum dehydrator, a pressurized dehydrator, a belt press, a centrifugal dehydrator, etc. can be used.

[0181] When a solution containing a coagulant is used as the aqueous phase of the receiving tank, the coagulant solution in the second contact step may drop into the receiving tank and mix with the solution containing the coagulant, causing the concentration of the coagulant in the solution containing the coagulant to change unintentionally. For example, if the concentration of the coagulant in the solution containing the coagulant in the aqueous phase is lower than the concentration of the coagulant in the coagulant solution used in the second contact step, the concentration of the coagulant in the solution containing the coagulant in the aqueous phase increases. Therefore, it is preferable to control the concentration of the coagulant in the solution containing the coagulant in the recovery step within a desired range. The method of control is not particularly limited, but for example, when the first contact step and the second contact step are performed while performing a flow-down operation, the flow-down water can be allowed to flow into the receiving tank to control the concentration of the coagulant in the solution containing the coagulant within a desired range.

[0182] The temperature of the solution containing the coagulant in the receiving tank in the recovery step is not particularly limited, but from the viewpoint of preventing the aggregates from fusing together and more sufficiently coagulating insufficiently coagulated aggregates, the temperature is, for example, preferably 20°C to 100°C, more preferably 40°C to 100°C, and even more preferably 60°C to 100°C.

[0183] (2-11. Drying process) The drying process is a process for drying the agglomerates (or the suspension dispersion containing the agglomerates) recovered in the recovery process. By drying the agglomerates, moisture originating from the latex, coagulant solution, liquid phase, etc. contained in the agglomerates is removed, and it can also be said that the drying process is a process for promoting fusion between polymer microparticles within the agglomerates.

[0184] In the drying step, the method for drying the aggregate is not particularly limited, and any known method can be used. For example, the aggregate may be dried by subjecting the aggregate to a heat treatment.

[0185] When drying the aggregate by heat treatment, the heat treatment temperature is not particularly limited, but is, for example, preferably 60° C. to 120° C., more preferably 60° C. to 100° C., and even more preferably 65° C. to 95° C. The heat treatment time is, for example, preferably 1 minute to 60 minutes, and more preferably 5 minutes to 30 minutes.

[0186] [4. Powder] The powder obtained by the manufacturing method of the present disclosure is also one embodiment of the present invention. The "powder according to one embodiment of the present invention" may be referred to as the "present powder". The present powder has an advantage that a good dispersion state of polymer microparticles can be achieved in a resin composition obtained by blending a matrix resin with the present powder, or in a molded or cured product thereof. In this specification, the "powder (powder of polymer microparticles)" may be an aggregate of primary particles of polymer microparticles, in other words, secondary particles of polymer microparticles.

[0187] The present powder has the advantage of having a high bulk density. The present powder has a bulk density of 0.36 g / cm 3 It is preferable that the content is 0.37 g / cm or more. 3 More preferably, it is 0.38 g / cm or more. 3 More preferably, it is 0.39 g / cm or more. 3 More preferably, it is 0.40 g / cm or more. 3It is particularly preferable that the bulk density of the powder or granule is 0.36 g / cm or more. The higher the bulk density of the powder or granule, the more densely the polymer fine particles are aggregated in the powder or granule. 3 A powder or granule having the above-mentioned bulk density can be said to have a sufficiently high bulk density. Such a powder or granule having a sufficiently high bulk density has an advantage that it can be packed densely into a transport tank, a bag, etc., and therefore transportation costs can be reduced. The upper limit of the bulk density of the powder or granule is not particularly limited, but it is preferably, for example, 1.0 g / cm. 3 It can be the following: EXAMPLES

[0188] Hereinafter, one embodiment of the present invention will be described in more detail with reference to examples and comparative examples, but the present invention is not limited thereto. One embodiment of the present invention can be practiced with appropriate modifications within the scope of the above or below-described purpose, and all such modifications are included in the technical scope of the present invention.

[0189] [Measurement method] First, the methods for evaluating the aggregates and powder produced in the Production Examples, and the methods for evaluating the resin compositions and aqueous liquids recovered in the Examples and Comparative Examples will be described.

[0190] (Measurement of volume average particle size) The volume average particle diameter (Mv) of the polymer particles dispersed in the latex was measured using Nanotrac WaveII-EX150 (manufactured by Microtrackbell Co., Ltd.). The latex diluted with deionized water was used as the measurement sample. The measurement was performed by inputting the refractive index of water and the polymer particles obtained in each production example, adjusting the sample concentration so that the measurement time was 120 seconds and the loading index was within the range of 1 to 10.

[0191] (Measurement of bulk density of powders and granules) The bulk density of the resulting powder was measured using a bulk density measuring device (JIS K-6720 model, manufactured by Kuramochi Scientific Instruments Manufacturing Co., Ltd.).

[0192] [Production Example 1] <Latex manufacturing> (Polymerization of the first elastic body) A mixture having the following composition was charged into a glass reactor, and the temperature inside the glass reactor was raised to 80° C. while stirring in a nitrogen stream: Mixture composition: (parts by weight) Ion-exchanged water 220 Boric acid 0.3 Sodium carbonate 0.03 Sodium N-lauroyl sarcosinate 0.09 Sodium formaldehyde sulfoxylate 0.09 Disodium ethylenediaminetetraacetate 0.006 Ferrous sulfate heptahydrate 0.002.

[0193] Then, a mixture of a first monomer component consisting of 25 parts by weight of methyl methacrylate and 0.1 parts by weight of allyl methacrylate, 0.1 parts by weight of t-dodecyl mercaptan as a chain transfer agent, and 0.1 parts by weight of t-butyl hydroperoxide (BHPO) as a polymerization initiator was prepared. Next, 25% by weight of the mixture (100% by weight) prepared was charged into the glass reactor at once, and polymerization was carried out for 45 minutes.

[0194] Next, the remaining 75% by weight of the mixture was continuously added to the glass reactor over 1 hour. After the continuous addition was completed, the glass reactor was kept at 80°C for another 2 hours to complete the polymerization, and a latex of an elastomer (the first elastomer, which can also be said to be the innermost layer elastomer) was obtained. During the temperature maintenance (2 hours at 80°C) after the addition of the mixture, 0.2 parts by weight of sodium N-lauroyl sarcosinate was added to the glass reactor. The average particle size of the obtained first elastomer was 0.16 μm, and the polymerization conversion rate (amount of polymerization product / amount of monomer charged) was 98%.

[0195] (Polymerization of the second elastic body) The glass reactor used in the polymerization of the first elastomer was used as it was for the polymerization of the second elastomer. First, the inside of the glass reactor containing the latex of the first elastomer was kept at 80°C in a nitrogen stream. After 0.1 parts by weight of potassium persulfate was added to the latex, a second monomer mixture consisting of 41 parts by weight of butyl acrylate (n-butyl acrylate), 9 parts by weight of styrene, and 1 part by weight of allyl methacrylate was continuously added for 5 hours. During the continuous addition, potassium oleate was added to the latex in three separate additions, totaling 0.1 parts by weight. After the continuous addition of the second monomer mixture was completed, 0.05 parts by weight of potassium persulfate was further added to the reaction system to complete the polymerization. The temperature inside the glass reactor was kept at 80°C for another 2 hours to obtain a latex of an elastomer (an elastomer consisting only of butyl acrylate rubber) formed by further polymerizing the first elastomer with the second elastomer. The volume average particle size of the resulting elastic body was 0.23 μm, and the polymerization conversion rate was 99%.

[0196] (Polymerization of grafted portion) The glass reactor used in the polymerization of the second elastomer was used as it was for the polymerization of the graft portion. First, the inside of the glass reactor containing the latex of the elastomer was kept at 80°C. After 0.02 parts by weight of potassium persulfate was added to the latex, a graft monomer mixture consisting of 24 parts by weight of methyl methacrylate, 1 part by weight of butyl acrylate (n-butyl acrylate), and 0.1 parts by weight of t-dodecyl mercaptan was continuously added over 1 hour. After the addition of the graft monomer mixture was completed, the temperature inside the glass reactor was kept at 80°C for another 1 hour to obtain a latex (aqueous latex) of a rubber-containing graft copolymer (polymer fine particles) having an elastomer and a graft portion grafted to the elastomer. The volume average particle diameter of the obtained polymer fine particles was 0.25 μm, and the polymerization conversion rate was 99%. The amount (concentration) of the solid content (polymer fine particles) in 100% by weight of the obtained latex was 35% by weight.

[0197] Example 1 <Production of aggregates and granules> (contact process) The amount of latex in Production Example 1 shown in Table 1 was adjusted to 25° C. The latex was sprayed at a pressure of 3.7 kg / cm from a first nozzle (a swirl-type nozzle (diameter 0.6 mm), which is a type of pressure nozzle) provided at the top of a column (1 m above the liquid level in the bottom receiving tank) of a cylindrical vessel (having a gas phase region) with a diameter of 80 cm and a height of 100 cm. 2 The latex was sprayed vertically downward into the gas phase as droplets with a volume average droplet diameter of 200 μm. The shape of the spray cone of the sprayed latex was conical, and the tip angle was 70° to 90°. The temperature inside the vessel was adjusted to 60°C.

[0198] At the same time, a coagulant solution (aqueous solution of calcium chloride; the concentration of calcium chloride in 100% by weight of the aqueous calcium chloride solution is 35% by weight, and the temperature is 25°C) was mixed with air and sprayed horizontally into the gas phase from a second nozzle (two-fluid nozzle (0.5 mm diameter)) installed on the inner wall of the container so as to be located 20 cm horizontally and 20 cm vertically below the first nozzle. The volume average droplet diameter of the coagulant solution was 0.1 μm to 30.0 μm. The amount of the coagulant solution sprayed was 5 parts by weight per unit time per 100 parts by weight of the solid content (polymer fine particles) of the latex sprayed per unit time. The specific amount of the coagulant solution sprayed is shown in Table 1. The spray pressure of the second nozzle (coagulant solution) was 4.0 kg / cm 2 The shape of the spray cone of the sprayed coagulant solution was a hollow cone, and the tip angle was 70° to 90°. By this operation, the droplets of latex falling in the gas phase were brought into contact with the droplets of the coagulant solution sprayed into the gas phase, and an aggregate was obtained.

[0199] The aggregates that had descended in the gas phase were dropped at the bottom of the container into 35 kg of an aqueous calcium chloride solution (receiving tank liquid) in a receiving tank. The calcium chloride concentration in the 100% by weight aqueous calcium chloride solution was 1% by weight, and the aqueous calcium chloride solution had been heated to 60°C by supplying water vapor. This contact step yielded a suspension containing aggregates of polymer microparticles. The amount (concentration) of polymer microparticles in the 100% by weight suspension thus obtained was as shown in Table 1.

[0200] After the contact step, water vapor was fed into the suspension in the receiving tank, and the suspension was heat-treated at 95°C for 5 minutes (heat treatment step). Thereafter, the suspension was recovered, and the recovered suspension was subjected to suction filtration for 20 minutes to obtain a dehydrated aggregate (recovery step). Next, the obtained aggregate was dried at 60°C for 1 hour or more using a dryer to obtain a powder (drying step). The bulk density of the obtained powder was measured. The results are shown in Table 1.

[0201] (Examples 2 and 3 and Comparative Example 1) A powder was produced by carrying out the contacting step, heat treatment step, recovery step and drying step in the same manner as in Example 1, except that the spray amounts of latex and coagulant solution in the contacting step were changed as shown in Table 1. The measurement results of bulk density are shown in Table 1.

[0202] Example 4 (Emulsifier addition process) After the entire amount of latex was sprayed (i.e., after the contact step), sodium N-lauroyl sarcosinate was added as an emulsifier to the suspension in the receiving tank. The amount of sodium N-lauroyl sarcosinate added was such that the amount of sodium N-lauroyl sarcosinate in 100% by weight of the suspension obtained after the emulsifier addition step was the amount (wt%) shown in Table 1.

[0203] After the emulsifier addition step, steam was fed into the suspension in the receiving tank, and the suspension was heat-treated at 95°C for 5 minutes (heat treatment step). The suspension was then recovered (recovery step). The recovered suspension was then subjected to suction filtration for 20 minutes to obtain a dehydrated aggregate. The obtained aggregate was then washed with 2000 parts by weight of water at 70°C. The washed aggregate was then subjected to suction filtration again for 20 minutes to obtain a dehydrated aggregate. The obtained aggregate was then dried at 60°C for 1 hour or more using a dryer to obtain a powder (drying step). The bulk density of the obtained powder was measured. The results are shown in Table 1.

[0204] (Example 5, Comparative Examples 2 and 3) A powder was produced by carrying out the emulsifier adding step, contacting step, heat treatment step, recovery step and drying step in the same manner as in Example 4, except that the amount of emulsifier sodium N-lauroyl sarcosinate added in the emulsifier adding step was changed to the amount shown in Table 1. The measurement results of the bulk density are shown in Table 1.

[0205] [Table 1] [Industrial Applicability]

[0206] According to one embodiment of the present invention, a powder of polymer fine particles having a large bulk density can be produced. Therefore, the production method according to one embodiment of the present invention can be suitably used as one step in the production of a modifier for thermoplastic resin.

Claims

1. a contacting step of spraying and / or dropping latex containing polymer fine particles from a first nozzle, and further spraying and / or dropping a coagulant solution containing a coagulant from a second nozzle, thereby bringing droplets of the latex into contact with droplets of the coagulant solution; a heat treatment step of heat-treating the suspension containing the aggregates of the polymer fine particles obtained in the contact step, In the heat treatment step, the concentration of the polymer fine particles is 3% by weight to 50% by weight in 100% by weight of the suspension.

2. a contacting step of spraying and / or dropping latex containing polymer fine particles from a first nozzle, and further spraying and / or dropping a coagulant solution containing a coagulant from a second nozzle, thereby bringing droplets of the latex into contact with droplets of the coagulant solution; an emulsifier adding step of adding an emulsifier X to the suspension containing the aggregates of the polymer fine particles obtained in the contacting step; A heat treatment step of heat-treating the suspension obtained in the emulsifier addition step, In the heat treatment step, the amount of the emulsifier X is 0.002% by weight to 0.045% by weight based on 100% by weight of the suspension.

3. 3. The method for producing powder or granular material according to claim 2, wherein the emulsifier X is at least one selected from the group consisting of sulfur-based emulsifiers, phosphorus-based emulsifiers, sarcosinic acid-based emulsifiers, and carboxylic acid-based emulsifiers.

4. The method for producing granular material according to claim 1 , wherein the polymer fine particles have an elastomer and a graft portion graft-bonded to the elastomer.

5. 5. The method for producing powder or granular material according to claim 4, wherein the elastic body comprises at least one rubber selected from the group consisting of diene-based rubber, (meth)acrylate-based rubber, and organosiloxane-based rubber.

6. The method for producing powder or granular material according to claim 4, wherein the graft portion contains one or more structural units selected from the group consisting of an aromatic vinyl unit, a vinylcyan unit, and a (meth)acrylate unit.

7. a recovery step of recovering the aggregates from the suspension after the heat treatment step; The method for producing powder or granular material according to any one of claims 1 to 6, further comprising a drying step of drying the recovered agglomerate.

Citation Information

Patent Citations

  • Production of polymer latex

    JP2000026526A

  • Method of producing granular polymer

    JP2001302802A

  • Process for producing aggregated latex particle

    WO2006070590A1

Cited By

  • Method for manufacturing powders and granules

    JP2026120436A

  • Method for manufacturing powders and granules

    JP2026120437A