Fluorine-silicon composite modified hyperbranched waterborne polyurethane emulsion as well as preparation method and application thereof
The fluorosilic composite modified superspin is prepared by using polyadipate-1,4-butanediol ester, bihydroxyl-terminated polysiloxane and fluorine-containing monomers in aqueous polyurethanes, combined with high-speed shear emulsification method. The aqueous polyurethane emulsion solves the problem of insufficient mechanical properties and corrosion resistance of water-based polyurethane emulsions in the prior art, and achieves the improvement of high mechanical properties, hydrophobicity and corrosion resistance.
Patent Information
- Application Number
- CN202411130676.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-16
AI Technical Summary
The existing fluorosilic composite modified water-based polyurethane emulsions have shortcomings in mechanical properties, hydrophobic properties and corrosion resistance, and it is difficult to meet the needs of high mechanical properties and high corrosion resistance at the same time.
Polyadipate-1,4-butanediol ester and bihydroxyl-terminated polysiloxane are used as soft segments of aqueous polyurethane, diisocyanate and hydrophilic chain extender form hard segments, and fluorine-containing monomers are used as sealing. The end agent was combined with high-speed shear emulsion method to prepare fluorosilicone composite modified hyperbranched aqueous polyurethane emulsion.
A water-based polyurethane film with excellent mechanical properties, hydrophobicity, resistance to natural environment and chemical media corrosion was obtained, which significantly improved the dispersion of the emulsion and colloidal stability, reduced production costs, and reduced the amount of organic solvent use.
Smart Images

Figure CN119019637A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyurethane emulsion synthesis, and in particular to a fluorine-silicon composite modified hyperbranched waterborne polyurethane emulsion and a preparation method and application thereof. Background Art
[0002] The information disclosed in the background of the invention is only intended to enhance the understanding of the overall background of the invention and should not be necessarily regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Waterborne polyurethane is a new type of polyurethane product that uses water instead of traditional organic solvents as a dispersion medium. With its advantages of being green, environmentally friendly, safe and having good film-forming properties, it is gradually replacing traditional organic solvent-based polyurethanes in daily life. However, the chain segments of waterborne polyurethanes are mostly linear structures and contain abundant hydrophilic groups, which makes the mechanical properties, hydrophobic properties and corrosion resistance of waterborne polyurethane films inferior to those of traditional organic solvent-based polyurethanes.
[0004] The fluorine-silicon composite modified waterborne polyurethane emulsions reported in the prior art generally have poor emulsion adhesion performance, and it is difficult to simultaneously meet the high mechanical properties and high corrosion resistance of the latex film after the emulsion is formed into a film. Therefore, it is an urgent problem to provide a fluorine-silicon composite modified waterborne polyurethane emulsion with strong adhesion, strong mechanical properties and high corrosion resistance by regulating the types and contents of fluorine-containing alcohols and polysiloxanes. Summary of the invention
[0005] In view of this, the present invention provides a fluorine-silicon composite modified hyperbranched waterborne polyurethane emulsion and a preparation method and application thereof. The fluorine-silicon composite modified hyperbranched waterborne polyurethane emulsion provided by the present invention not only has excellent dispersibility and colloidal stability, but also exhibits extremely strong adhesion performance. The waterborne polyurethane film prepared using the emulsion not only exhibits excellent mechanical properties, but also exhibits excellent hydrophobicity and resistance to natural environment corrosion and chemical medium corrosion.
[0006] In a first aspect, the present invention provides a method for preparing a fluorine-silicon composite modified hyperbranched aqueous polyurethane emulsion, comprising the following steps:
[0007] In an inert atmosphere, poly(1,4-butylene adipate), dihydroxy-terminated polysiloxane and diisocyanate are reacted under the action of a catalyst to obtain a prepolymer; a hydrophilic chain extender is added to the prepolymer to react, a small molecule diol chain extender and a cross-linking agent are added to react, a fluorine-containing end-capping agent is added to react, and finally a neutralizing agent is added to react to obtain a polymer product; water is added to the polymer product, high-speed shear emulsification is performed, and rotary evaporation is performed until no solvent drips to obtain the polymer product;
[0008] Wherein, the addition amount of the dihydroxy-terminated polysiloxane is 4-6wt% of the total mass of the raw materials of the polymerization product.
[0009] Preferably, the number average molecular weight of the poly(1,4-butylene adipate) is 1500-2500 Da; the molecular weight of the dihydroxy-terminated polysiloxane is 1000-3000 Da, and the viscosity is 600-1000 mPa·s.
[0010] Preferably, the mass ratio of the poly(1,4-butylene adipate), diisocyanate, catalyst, hydrophilic chain extender, small molecule diol chain extender, cross-linking agent, fluorine-containing end-capping agent and neutralizing agent is (43-47): (28-34): (0.01-0.02): (3-6): (2.5-4): (0.8-1.5): (5-7): (3-4).
[0011] Preferably, the diisocyanate is selected from one or more of isophorone diisocyanate, 4,4-diisocyanate dicyclohexylmethane or toluene diisocyanate.
[0012] Preferably, the catalyst is selected from one or more of dibutyltin dilaurate, monobutyltin oxide, dibutyltin oxide, and dibutyltin diacetate.
[0013] Preferably, the hydrophilic chain extender is selected from one or more of dimethylolpropionic acid, dimethylolbutanoic acid, and 3,4-dihydroxyphenylpropionic acid.
[0014] Preferably, the hydrophilic chain extender is first dissolved in an organic solvent and then added to the prepolymer; the organic solvent is selected from one or more of acetone, methyl ethyl ketone, ethyl acetate, tetrahydrofuran or methyl formate; the dosage ratio of the hydrophilic chain extender to the organic solvent is (2-4) g: 10 mL.
[0015] Preferably, the cross-linking agent is selected from one or more of trimethylolpropane, glycerol, pentaerythritol or butanethritol.
[0016] Preferably, the small molecule diol chain extender is selected from one or more of 1,4-butanediol, ethylene glycol, diethylene glycol, pentanediol, 1,2-propylene glycol, 1,3-propylene glycol, dipropylene glycol or 1,6-hexanediol.
[0017] Preferably, the fluorine-containing end-capping agent is selected from one or more of 1H,1H,2H,2H-perfluoro-1-octanol, hexafluoroisopropanol, 2,2,3,3,4,4,5,5-octafluoro-1-pentanol or 1H,1H,2H,2H-perfluoro-1-decanol.
[0018] Preferably, the neutralizing agent is one or more of trimethylamine, triethylamine, tributylamine and triethanolamine.
[0019] Preferably, the diisocyanate is isophorone diisocyanate; the catalyst is dibutyltin dilaurate; the hydrophilic chain extender is dimethylolpropionic acid; the cross-linking agent is trimethylolpropane; the small molecule diol chain extender is selected from 1,4-butanediol; and the fluorine-containing end-capping agent is 1H,1H,2H,2H-perfluoro-1-octanol.
[0020] Preferably, the inert atmosphere is selected from one or more of nitrogen, argon, helium or neon.
[0021] Preferably, in the step of reacting under the action of a catalyst to obtain a prepolymer, the reaction temperature is 70-90°C and the reaction time is 80-110 min; in the step of reacting after adding a hydrophilic chain extender, the reaction temperature is 70-90°C and the reaction time is 110-140 min; in the step of adding a small molecule diol chain extender and a cross-linking agent to react, the reaction temperature is 70-90°C and the reaction time is 80-110 min; 110-140 min; in the step of adding a fluorine-containing end-capping agent to react, the reaction temperature is 70-90°C and the reaction time is 110-140 min; in the step of reacting to obtain a polymer product, the reaction temperature is 40-50°C and the reaction time is 50-70 min.
[0022] Preferably, in the step of adding water to the polymerization product, the mass ratio of the polymerization product to water is 3:(6-8).
[0023] Preferably, the rotation speed of the high-speed shear emulsification is 8000-12000 r / min, and the time of the high-speed shear emulsification is 8-15 min.
[0024] Preferably, the temperature of the rotary evaporation is 45-55°C.
[0025] In a second aspect, the present invention provides a fluorine-silicon composite modified hyperbranched aqueous polyurethane emulsion prepared by the above preparation method.
[0026] In a third aspect, the present invention provides the use of the above-mentioned fluorosilicone composite modified hyperbranched aqueous polyurethane emulsion as a water-resistant coating or a water-resistant adhesive.
[0027] Compared with the prior art, the present invention has achieved the following beneficial effects:
[0028] (1) The present invention uses poly(1,4-butylene adipate) and dihydroxy-terminated polysiloxane as the soft segment of the waterborne polyurethane, uses the chain segment formed by diisocyanate, hydrophilic chain extender and small molecule diol chain extender as the hard segment, and uses a hydrophobic fluorine-containing monomer as a capping agent. After polymerization, a fluorine-silicon composite modified hyperbranched waterborne polyurethane emulsion is prepared by a high-speed shear emulsification method. The preparation method of the present invention greatly reduces the amount of organic solvent used, while ensuring product performance, greatly reduces the production cost and the harm of reactants to human health and the natural environment, and the entire production process of the product does not involve high temperature and high pressure reactions, the production plan is scientific and reasonable, and the production process is safe and reliable;
[0029] (2) The fluorosilicone composite modified hyperbranched aqueous polyurethane emulsion obtained by the preparation method of the present invention has excellent dispersibility and colloidal stability, and also exhibits extremely strong adhesion performance. The aqueous polyurethane latex film prepared using the aqueous polyurethane emulsion not only exhibits excellent mechanical properties but also exhibits excellent hydrophobicity and resistance to natural environmental corrosion and chemical media (including acids, alkalis and salts) corrosion, and is expected to greatly expand its application in the fields of water-resistant coatings and water-resistant adhesives. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The drawings constituting part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their description are used to explain the present invention and do not constitute an improper limitation of the present invention. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative work.
[0031] Figure 1 is a schematic diagram of the structural formula of the polymer product in Example 1 of the present invention;
[0032] Figure 2 It is the infrared spectra of the aqueous polyurethane emulsions of Example 1 and Comparative Examples 1 to 5 of the present invention;
[0033] Figure 3 This is a picture showing the anti-graffiti performance of the waterborne polyurethane latex film of Example 1 of the present invention;
[0034] Figure 4 This is a picture showing the adhesion performance of the FSiWPU5 emulsion of Example 1 of the present invention. DETAILED DESCRIPTION
[0035] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0036] The present invention provides a method for preparing a fluorine-silicon composite modified hyperbranched waterborne polyurethane emulsion, comprising the following steps:
[0037] In an inert atmosphere, poly(1,4-butylene adipate), dihydroxy-terminated polysiloxane and diisocyanate are reacted under the action of a catalyst to obtain a prepolymer; a hydrophilic chain extender is added to the prepolymer to react, a small molecule diol chain extender and a cross-linking agent are added to react, a fluorine-containing end-capping agent is added to react, and finally a neutralizing agent is added to react to obtain a polymer product; water is added to the polymer product, high-speed shear emulsification is performed, and rotary evaporation is performed until no solvent drips to obtain the polymer product;
[0038] Wherein, the addition amount of the dihydroxy-terminated polysiloxane is 4-6wt% of the total mass of the raw materials of the polymerization product.
[0039] The present invention adopts a stepwise polymerization method to synthesize a polymer product, which can maintain a small emulsion particle size, ensure the stability of the emulsion while ensuring the excellent performance of the waterborne polyurethane coating or film. The present invention introduces a dihydroxyl-terminated polysiloxane and a fluorine-containing end-capping agent to modify the waterborne polyurethane, and the obtained emulsion exhibits high emulsion stability and high adhesion, and the latex film prepared therefrom has high strength, high toughness, high water resistance, high chemical corrosion resistance and excellent anti-graffiti performance.
[0040] The invention finds that the addition amount of dihydroxy-terminated polysiloxane has a significant influence on the finally obtained fluorosilicone composite modified hyperbranched waterborne polyurethane emulsion, and the addition of an appropriate amount of dihydroxy-terminated polysiloxane can greatly improve the adhesion of the emulsion, and can improve the strength, toughness, hydrophobicity and chemical corrosion resistance of the latex film; while the addition of too much dihydroxy-terminated polysiloxane will have an adverse effect on various properties, and even the performance in terms of strength, hydrophobicity, chemical corrosion resistance and the like will be worse than that of the emulsion without the addition of dihydroxy-terminated polysiloxane, so the invention limits the addition amount of dihydroxy-terminated polysiloxane to 4-6wt% of the total mass of the raw materials of the polymerization product, and more preferably 5wt%.
[0041] It should be noted that the "total mass of raw materials of the polymerization product" here refers to the total mass of poly(1,4-butylene adipate), dihydroxy-terminated polysiloxane, diisocyanate, catalyst, hydrophilic chain extender, small molecule diol chain extender, cross-linking agent, fluorine-containing end-capping agent and neutralizer.
[0042] In the present invention, the number average molecular weight of the poly(1,4-butylene adipate) is 1500-2500 Da; the molecular weight of the dihydroxy-terminated polysiloxane is 1000-3000 Da, and the viscosity is 600-1000 mPa·s.
[0043] In the present invention, the mass ratio of the poly(1,4-butylene adipate), diisocyanate, catalyst, hydrophilic chain extender, small molecule diol chain extender, crosslinking agent, fluorine-containing end-capping agent and neutralizing agent is (43-47): (28-34): (0.01-0.02): (3-6): (2.5-4): (0.8-1.5): (5-7): (3-4).
[0044] In the present invention, the diisocyanate is selected from one or more of isophorone diisocyanate, 4,4-diisocyanate dicyclohexylmethane or toluene diisocyanate, and is more preferably isophorone diisocyanate.
[0045] In the present invention, the catalyst is selected from one or more of dibutyltin dilaurate, monobutyltin oxide, dibutyltin oxide, and dibutyltin diacetate, and more preferably dibutyltin dilaurate.
[0046] In the present invention, the hydrophilic chain extender is selected from one or more of dimethylol propionic acid, dimethylol butyric acid, 1,2-propylene glycol-3-sodium sulfonate, N-methyl-N,N-di(2-hydroxyethyl)betaine or 1,4-butanediol-2-sodium sulfonate, more preferably dimethylol propionic acid.
[0047] In the present invention, since the hydrophilic chain extender is usually solid, the hydrophilic chain extender is first dissolved in an organic solvent and then added to the prepolymer; the organic solvent is selected from one or more of acetone, methyl ethyl ketone, ethyl acetate, tetrahydrofuran or methyl formate, more preferably acetone. The amount ratio of the hydrophilic chain extender to the organic solvent is (2-4) g: 10 mL. The boiling point of the organic solvent selected in the present invention is lower than that of water, and it can be removed in the subsequent rotary evaporation process. In the process of the reaction of the present invention, an organic solvent can be appropriately added to the system according to the viscosity to maintain the appropriate viscosity of the system. The present invention does not impose any special restrictions on the amount of addition and the addition steps, and the method of adding organic solvents to control the viscosity commonly used in the art can be used.
[0048] In the present invention, the crosslinking agent is selected from one or more of trimethylolpropane, propylene glycol, pentaerythritol or butanethritol, and is more preferably trimethylolpropane, which has a lower melting point and is in a molten state at the polymerization reaction temperature, which is conducive to the reaction.
[0049] In the present invention, the small molecule diol chain extender is selected from one or more of 1,4-butanediol, ethylene glycol, diethylene glycol, pentanediol, 1,2-propylene glycol, 1,3-propylene glycol, dipropylene glycol or 1,6-hexanediol, more preferably 1,4-butanediol.
[0050] In the present invention, the fluorine-containing end-capping agent is selected from one or more of 1H,1H,2H,2H-perfluoro-1-octanol, hexafluoroisopropanol, 2,2,3,3,4,4,5,5-octafluoro-1-pentanol or 1H,1H,2H,2H-perfluoro-1-decanol, more preferably 1H,1H,2H,2H-perfluoro-1-octanol.
[0051] In the present invention, the neutralizing agent is one or more of trimethylamine, triethylamine, tributylamine and triethanolamine, more preferably triethylamine.
[0052] In the present invention, the inert atmosphere is selected from one or more of nitrogen, argon, helium or neon, preferably nitrogen.
[0053] In the present invention, in the step of reacting under the action of a catalyst to obtain a prepolymer, the reaction temperature is 70-90°C and the reaction time is 80-110 min; in the step of reacting after adding a hydrophilic chain extender, the reaction temperature is 70-90°C and the reaction time is 110-140 min; in the step of adding a small molecule diol chain extender and a cross-linking agent to react, the reaction temperature is 70-90°C and the reaction time is 80-110 min; 110-140 min; in the step of adding a fluorine-containing end-capping agent to react, the reaction temperature is 70-90°C and the reaction time is 110-140 min; in the step of reacting to obtain a polymer product, the reaction temperature is 40-50°C and the reaction time is 50-70 min.
[0054] In the present invention, in the step of adding water to the polymerization product, the mass ratio of the polymerization product to water is 3:(6-8).
[0055] In the present invention, the rotation speed of the high-speed shear emulsification is 8000-12000 r / min, and the time of the high-speed shear emulsification is 8-15 min.
[0056] In the present invention, the temperature of the rotary evaporation is 45-55° C. The purpose of the rotary evaporation is to remove the organic solvent added to the system, and those skilled in the art can determine the temperature of the rotary evaporation according to the boiling point of the selected organic solvent.
[0057] The present invention also provides a fluorine-silicon composite modified hyperbranched waterborne polyurethane emulsion prepared by the above preparation method. The fluorine-silicon composite modified hyperbranched waterborne polyurethane emulsion prepared by the present invention has extremely strong adhesion and colloidal stability, and the latex film obtained therefrom has high strength, high toughness, high chemical resistance, high hydrophobicity and high anti-graffiti performance.
[0058] The present invention also provides the use of the fluorine-silicon composite modified hyperbranched aqueous polyurethane emulsion as a water-resistant coating or a water-resistant adhesive.
[0059] The technical solution of the present invention is further described below in conjunction with specific examples. In the following examples, the number average molecular weight of poly(1,4-butylene adipate) (PBA) is 2000 Da, the molecular weight of dihydroxy-terminated polysiloxane (PDMS) is 2000 Da, and the viscosity is 800 mPa·s.
[0060] Example 1
[0061] This embodiment provides a method for preparing a fluorine-silicon composite modified hyperbranched waterborne polyurethane emulsion, wherein the mass fraction of the dihydroxy-terminated polysiloxane in the raw material is 5wt%.
[0062] In a four-necked flask equipped with a thermometer, a mechanical stirring rod, a spherical condenser and a nitrogen inlet, nitrogen was introduced for 20 minutes to ensure that the flask was in a nitrogen atmosphere. After the temperature of the oil bath pot rose to 80°C, 27.0g of poly(1,4-butylene adipate) (PBA), 3.0g of dihydroxy-terminated polysiloxane (PDMS), 18.54g of isophorone diisocyanate (IPDI), and 0.01g of dibutyltin dilaurate (DBTDL) were added, and the reaction was continued at 80°C for 90min to obtain a prepolymer, and then 2.67g of dihydroxymethylpropionic acid (DMPA) and 10mL of acetone were added, and the reaction was continued at 80°C for 120min, and then 1.90g of 1,4-butanediol (BDO) and 0.59g of trimethylolpropane (TMP) were added, and the reaction was continued at 80°C for 90min, and then 3.56g of 1H,1H,2H,2H-perfluoro-1-octanol, continue to react at 80°C for 120min, measure the -NCO of the system by di-n-butylamine method, when the theoretical requirement is reached, reduce the system temperature to 45°C, add 2.02g triethylamine, react at 45°C for 60min to obtain the polymerization product, and use about 35mL acetone in the whole synthesis process. The structural formula of the polymerization product in this embodiment is shown in the figure Figure 1 shown.
[0063] Then, 50.00 g of the polymer product was transferred to a beaker, 116.67 g of deionized water was added, and the product was emulsified at room temperature for 10 minutes using a high-speed shear emulsifier at a speed of 9000 r / min. The emulsified product was then rotary evaporated at 50° C. using a rotary evaporator until no solvent was dripped to obtain a water-based polyurethane emulsion, which was recorded as FSiWPU5 and had an R value (ratio of isocyanate group to hydroxyl group) of 1.3.
[0064] Example 2
[0065] This embodiment provides a method for preparing a fluorine-silicon composite modified hyperbranched waterborne polyurethane emulsion.
[0066] In a four-necked flask equipped with a thermometer, a mechanical stirring rod, a spherical condenser and a nitrogen inlet, nitrogen was introduced for 20 minutes to ensure that the flask was in a nitrogen atmosphere. After the temperature of the oil bath pot rose to 80°C, 27.0g of poly(1,4-butylene adipate) (PBA), 3.0g of dihydroxy-terminated polysiloxane (PDMS), 18.54g of toluene diisocyanate (TDI), and 0.01g of dibutyltin dilaurate (DBTDL) were added, and the reaction was continued at 80°C for 90min to obtain a prepolymer, and then 2.67g of dihydroxymethylbutyric acid (DMBA, dissolved in 10mL of acetone) was added, and the reaction was continued at 80°C for 120min, and then 1.90g of 1,4-butanediol (BDO) and 0.59g of propylene glycol were added, and the reaction was continued at 80°C for 90min, and then 3.56g of 2,2,3,3,4,4,5,5-octafluoro-1-pentanol was reacted at 80°C for 120 min. The -NCO of the system was measured by the di-n-butylamine method. When the theoretical requirement was met, the system temperature was lowered to 45°C, 2.02 g of triethylamine was added, and the reaction was carried out at 45°C for 60 min to obtain a polymerization product. About 35 mL of acetone was used in the whole synthesis process.
[0067] Then, 50.00 g of the polymer product was transferred to a beaker, 116.67 g of deionized water was added, and the product was emulsified for 10 min at room temperature using a high-speed shear emulsifier. The emulsified product was then evaporated at 50° C. using a rotary evaporator until no solvent was dripped to obtain an aqueous polyurethane emulsion.
[0068] Example 3
[0069] This embodiment provides a method for preparing a fluorine-silicon composite modified hyperbranched waterborne polyurethane emulsion.
[0070] In a four-necked flask equipped with a thermometer, a mechanical stirring rod, a spherical condenser and a nitrogen inlet, nitrogen was introduced for 20 minutes to ensure that the flask was in a nitrogen atmosphere. After the oil bath temperature was raised to 80°C, 27.0 g of poly(1,4-butylene adipate) (PBA), 3.0 g of dihydroxy-terminated polysiloxane (PDMS), and 18.2 g of 4,4-diisocyanate dicyclohexylmethane (HMDI) and 0.01g dibutyltin oxide (DBTO) were reacted at 80°C for 90min to obtain a prepolymer, and then 3.2g dihydroxymethylpropionic acid (DMPA, dissolved in 15mL acetone) was added, and the reaction was continued at 80°C for 120min, and then 1.80g ethylene glycol and 0.5g trimethylolpropane (TMP) were added, and the reaction was continued at 80°C for 90min, and then 3.56g hexafluoroisopropanol was added, and the reaction was continued at 80°C for 120min. The -NCO of the system was measured by the di-n-butylamine method. When the theoretical requirement was met, the system temperature was lowered to 45°C, 2.02g triethanolamine was added, and the reaction was continued at 45°C for 60min to obtain a polymerization product. About 40mL acetone was used in the whole synthesis process.
[0071] Then, 50.00 g of the polymer product was transferred to a beaker, 116.67 g of deionized water was added, and the product was emulsified for 10 min at room temperature using a high-speed shear emulsifier. The emulsified product was then evaporated at 50° C. using a rotary evaporator until no solvent was dripped to obtain an aqueous polyurethane emulsion.
[0072] Comparative Example 1
[0073] The difference between this comparative example and Example 1 is that no bishydroxy-terminated polysiloxane is added to the raw materials of this comparative example, and the missing amount is supplemented by poly(1,4-butylene adipate); the specific difference is that 30.0g of poly(1,4-butylene adipate) (PBA) and 0g of bishydroxy-terminated polysiloxane (PDMS) are added to this comparative example, and the obtained fluorine-modified hyperbranched aqueous polyurethane emulsion is recorded as FWPU, and the R value is 1.3.
[0074] Comparative Example 2
[0075] Compared with Example 1, the difference between this comparative example and Example 1 is that the mass fraction of the dihydroxy-terminated polysiloxane in the raw material of this comparative example is 10wt%. The specific difference is that 24.0g of poly(1,4-butylene adipate) (PBA) and 6.0g of dihydroxy-terminated polysiloxane (PDMS) are added to this comparative example, and the obtained fluorosilicone composite modified hyperbranched aqueous polyurethane emulsion is recorded as FSiWPU10, and the R value is 1.3.
[0076] Comparative Example 3
[0077] Compared with Example 1, the difference between this comparative example and Example 1 is that the mass fraction of the dihydroxy-terminated polysiloxane in the raw materials of this comparative example is 15wt%. The specific difference is that 21.0g of poly(1,4-butylene adipate) (PBA) and 9.0g of dihydroxy-terminated polysiloxane (PDMS) are added to this comparative example, and the obtained fluorosilicone composite modified hyperbranched aqueous polyurethane emulsion is recorded as FSiWPU15, and the R value is 1.3.
[0078] Comparative Example 4
[0079] Compared with Example 1, the difference between this comparative example and Example 1 is that the mass fraction of the dihydroxy-terminated polysiloxane in the raw material of this comparative example is 20wt%. The specific difference is that 18.0g of poly(1,4-butylene adipate) (PBA) and 12.0g of dihydroxy-terminated polysiloxane (PDMS) are added to this comparative example, and the obtained fluorosilicone composite modified hyperbranched aqueous polyurethane emulsion is recorded as FSiWPU20, and the R value is 1.3.
[0080] Comparative Example 5
[0081] The difference between this comparative example and Example 1 is that the raw materials of this comparative example do not contain 1H, 1H, 2H, 2H-perfluoro-1-octanol. The specific preparation method is as follows:
[0082] In a four-necked flask equipped with a thermometer, a mechanical stirring rod, a spherical condenser and a nitrogen inlet, nitrogen was introduced for 20 minutes to ensure that the flask was in a nitrogen atmosphere. After the temperature of the oil bath pot rose to 80°C, 27.0g of poly(1,4-butylene adipate) (PBA), 3.0g of dihydroxy-terminated polysiloxane (PDMS), 16.71g of isophorone diisocyanate (IPDI), and 0.01g of dibutyltin dilaurate (DBTDL) were added, and the reaction was continued at 80°C for 90min to obtain a prepolymer, and then 2.39g of dihydroxymethylpropionic acid (DMPA, dissolved in 35mL of acetone) was added, and the reaction was continued at 80°C for 120min, and then 1.70g of 1,4-Butanediol (BDO) and 0.53g trimethylolpropane (TMP) were reacted at 80°C for 90min, and the -NCO of the system was measured by the di-n-butylamine method. When the theoretical requirement was met, the system temperature was lowered to 45°C, 1.81g triethylamine was added, and the reaction was continued at 45°C for 60min to obtain a polymerization product.
[0083] Then, 50.00 g of the polymer product was transferred to a beaker, 116.67 g of deionized water was added, and the product was emulsified for 10 min at room temperature using a high-speed shear emulsifier. The emulsified product was then evaporated at 50° C. using a rotary evaporator until no solvent was dripped to obtain a water-based polyurethane emulsion, which was recorded as SiWPU5 and had an R value of 1.3.
[0084] Test example
[0085] 1. After drying, the aqueous polyurethane emulsions of Example 1 and Comparative Examples 1 to 5 were subjected to infrared spectroscopy measurement:
[0086] The infrared spectra of each sample are shown in Figure 2 As shown, at 2270cm -1 There is no vibration absorption peak on the left and right, indicating that the -NCO group has reacted completely; 3357cm -1 The -NH stretching vibration absorption peak is at 2923-2850cm -1 The CH symmetric and asymmetric absorption peaks corresponding to the CH2 group; 1723cm -1 The C=O stretching vibration absorption peak is at 1161cm -1 The asymmetric stretching vibration absorption peak of COC is at 1243cm -1 CF stretching vibration peak at 1099cm -1 The characteristic absorption peak of Si-O-Si is 801cm -1 The characteristic absorption peak of Si-CH3 is at . The typical absorption peak of waterborne polyurethane appears in the infrared spectrum, which can prove that the waterborne polyurethane is successfully prepared and that the polysiloxane and fluorocarbon groups have been successfully introduced into the system.
[0087] 2. Physical property determination of aqueous polyurethane emulsions of Example 1 and Comparative Examples 1 to 5:
[0088] The test results are shown in Table 1. The fluorosilicone water-based polyurethane emulsions were placed in a centrifuge tube and centrifuged at 3500r / min for 15 minutes without stratification, indicating that they all had excellent colloidal stability. After being placed for six months, no precipitation or demulsification occurred, indicating that they all had long-term stability. The adhesion of the water-based polyurethane did not change with the change of the polysiloxane content, and all had good adhesion properties. Due to the flexibility of polysiloxane itself, the pencil hardness of the film decreased to a certain extent after adding polysiloxane.
[0089] Table 1 Physical properties of waterborne polyurethane emulsion
[0090]
[0091] Note: In Table 1, the centrifugal stability determination method is: centrifuge the emulsion sample in a centrifuge at a speed of 3500r / min for 15min. If no stratification occurs, it means that it can exist stably; the adhesion is in accordance with the national standard GB / T9286-1998 "Paints and varnishes-cross-cut test of paint films"; the pencil hardness is in accordance with the national standard GB / T6739-1996 "Pencil determination method for coating film hardness".
[0092] 3. Particle size distribution and PDI determination of aqueous polyurethane emulsions of Example 1 and Comparative Examples 1 to 5:
[0093] Take 50 μl of waterborne polyurethane emulsion sample, add deionized water to dilute to 8 ml, and then use dynamic light scattering nanoparticle size analyzer to test the emulsion particle size distribution and polymer dispersion index (PDI), the test temperature is 25 ° C, and the average value is obtained by three measurements. The test results are shown in Table 2.
[0094] Table 2 Average particle size and PDI of waterborne polyurethane emulsion
[0095]
[0096] As can be seen from Table 2, when the percentage of other monomers such as fluorinated alcohol in the fixed system remains unchanged, the content of polysiloxane is increased from 0wt% to 10wt%, and the particle size of the emulsion increases from 38.58nm to 55.85nm, which has little effect on the size of the latex particles. However, when the content of polysiloxane continues to increase, the particle size of the emulsion increases sharply with the increase of the percentage of polysiloxane. When the amount of polysiloxane added is 15wt%, the particle size of the emulsion reaches 88.30nm. This is because after polysiloxane is embedded in the main chain of waterborne polyurethane as a hydrophobic monomer, the ratio of hydrophilic segment and hydrophobic segment in the waterborne polyurethane segment will be changed, and the Si-O-Si main chain in polysiloxane is covered by the hydrophobic methyl side chain, so during emulsification, the hydrophobic polysiloxane curls inside the latex particles, while the hydrophilic group is wrapped around the latex particles. Therefore, with the increase of the content of hydrophobic polysiloxane, the particle size becomes larger and unevenly distributed.
[0097] 4. Determination of hydrophobic properties of aqueous polyurethane emulsions and surface elements of latex films of Example 1 and Comparative Examples 1 to 5:
[0098] Weigh a certain amount of fluorosilicone waterborne polyurethane emulsion, pour it into a polytetrafluoroethylene mold, dry it at room temperature for 48 hours, and then dry it in an oven at 60℃ for 24 hours to obtain a waterborne polyurethane film; weigh a certain amount of fluorosilicone waterborne polyurethane emulsion, evenly coat it on a tinplate, dry it at room temperature for 48 hours, and then dry it in an oven at 60℃ for 24 hours, and the waterborne polyurethane will form a film on the tinplate and adhere tightly to the tinplate. After forming a film on the tinplate, the contact angle is tested by the sessile drop method to characterize its hydrophobic properties; after forming a film in a polytetrafluoroethylene mold, a waterborne polyurethane film is obtained, and a 2cm*2cm waterborne polyurethane film is cut from it, and it is soaked in deionized water for 24 hours and then taken out, and its water absorption rate is calculated, and the results are shown in Table 3; after forming a film in a polytetrafluoroethylene mold, a waterborne polyurethane film is obtained, and a 0.5cm*0.5cm sample is cut from the film, and the surface composition of the film is analyzed by X-ray photoelectron spectroscopy (XPS), and the results are shown in Table 4.
[0099] Table 3 Contact angle and water absorption of polyurethane latex film
[0100]
[0101] Table 4 Percentage of elements on the film surface (unit: %)
[0102]
[0103] It can be seen from Tables 3 and 4 that the water resistance of the film increases first and then decreases with the increase of the polysiloxane content. When polysiloxane is not introduced into the waterborne polyurethane segment, the contact angle of the film is 104.44° and the water absorption rate is 5.60%; when the percentage of other monomers such as fluorinated alcohol in the fixed system remains unchanged, the content of polysiloxane is increased from 0wt% to 5wt%, the contact angle of the film increases to 113.56°, the water absorption rate decreases to 5.55%, and the water resistance of the film is improved to a certain extent; however, when the content of polysiloxane continues to increase, the water resistance of the film decreases with the increase of the percentage of polysiloxane. When the addition amount of polysiloxane is 20wt%, the contact angle of the film reaches 94.91° and the water absorption rate increases to 8.21%. In order to explain this phenomenon, XPS test was carried out on fluorosilicone waterborne polyurethane film to clarify the elemental composition of the film surface (Table 4). It was found that the migration behavior of fluorine and silicon elements to the film surface during the emulsion film formation process was not a cooperative relationship but a competitive relationship. The polysiloxane embedded in the main chain would hinder the migration efficiency of the terminal carbon fluoride group. When the polysiloxane content increased from 0wt% to 5wt%, although the fluorine content on the film surface decreased slightly, the migration of silicon elements to the surface could make up for the fluorine gap. Therefore, the contact angle of the film surface did not decrease but increased slightly, and the water resistance of the film was improved. However, when the polysiloxane content continued to increase, the fluorine content on the film surface dropped sharply, and the silicon content continued to increase and reached saturation. In addition, the ability of polysiloxane to reduce surface energy was lower than that of carbon fluoride groups. Therefore, the contact angle and water absorption rate of the film decreased and increased respectively with the continued increase of polysiloxane content, and the water resistance of the film decreased.
[0104] 5. Determination of mechanical properties of the aqueous polyurethane latex films of Example 1 and Comparative Examples 1 to 5:
[0105] The mechanical properties of polyurethane latex film were tested according to GB / T16777-2008 standard. A certain amount of fluorosilicone water-based polyurethane emulsion was weighed and poured into a polytetrafluoroethylene mold. After drying at room temperature for 48 hours, it was dried in an oven at 60°C for 24 hours to obtain a water-based polyurethane film. A dumbbell-shaped specimen was cut from the film with a dumbbell-shaped cutter, and its mechanical properties, including tensile stress and elongation at break, were tested with a universal material testing machine at a tensile rate of 50 mm / min. The test results are shown in Table 5.
[0106] Table 5 Determination of mechanical properties of polyurethane latex film
[0107]
[0108] It can be seen from Table 5 that when the percentage of other monomers such as fluorinated alcohol in the fixed system remains unchanged, with the increase of polysiloxane content, the tensile strength of the film first increases and then decreases. When the percentage of polysiloxane is 5wt%, the maximum tensile strength of the film is 62.82MPa, the elongation at break is 757.75%, and the toughness is 211.43MJ / m 3 , showing the best mechanical properties, this is because in the process of film formation of waterborne polyurethane emulsion, the hard segment composed of isocyanate and chain extender and the soft segment composed of polyol have a tendency to separate spontaneously in thermodynamics due to the different polarity and molecular motion deformation ability of the chain segments, forming a special aggregation structure, namely microphase separation. The addition of polysiloxane enhances the microphase separation of the film and improves the directional movement of the microphase segment in the film under the action of external force during the stretching process, thereby improving the tensile strength of the film. When the percentage of polysiloxane is greater than 5wt%, the mechanical properties show a downward trend, this is because too much polysiloxane leads to too strong microphase separation, which leads to a decrease in the interaction force between the soft and hard segments, so that the mechanical properties of the film are reduced.
[0109] 6. Determination of thermal stability of the aqueous polyurethane latex films of Example 1 and Comparative Examples 1 to 5:
[0110] Weigh a certain amount of fluorosilicone waterborne polyurethane emulsion, pour it into a polytetrafluoroethylene mold, dry it at room temperature for 48 hours, and then dry it in an oven at 60°C for 24 hours to obtain a waterborne polyurethane film. Cut 5-10 mg of the sample and heat it from 25°C to 600°C at a heating rate of 20°C / min in a nitrogen atmosphere using a high-precision thermogravimetric analyzer. The test results are shown in Table 6.
[0111] Table 6 Thermal stability of waterborne polyurethane latex films
[0112]
[0113] Note: In Table 6, T 10% Refers to the temperature at which weight loss reaches 10%, T 50% Refers to the temperature at which weight loss reaches 50%, T 90% Refers to the temperature at which weight loss reaches 90%.
[0114] As shown in Table 6, the thermal stability of waterborne polyurethane film can be analyzed from two stages. The first stage is around 250℃-400℃, which is mainly the decomposition of the urethane bonds with poor thermal stability in the chain segment; the second stage is around 400℃-600℃, which is mainly the decomposition of the soft segment macromolecular polyol. It can be seen that with the increase of polysiloxane content, the thermal stability of waterborne polyurethane film increases significantly in the second decomposition stage. This is because the high bond energy and high ionization tendency of Si-O bonds allow the polysiloxane chain segment to absorb more heat and enhance the thermal stability of the chain segment.
[0115] 7. Natural environment resistance and chemical resistance of the aqueous polyurethane latex films of Example 1 and Comparative Examples 1 to 5
[0116] Weigh a certain amount of fluorosilicone water-based polyurethane emulsion and evenly coat it on the tinplate. Dry it at room temperature for 48 hours and then dry it in an oven at 60°C for 24 hours. The water-based polyurethane forms a film on the tinplate and adheres tightly to it. After the film is formed on the tinplate, the tinplate is placed outdoors to experience the influence of the natural environment to test its anti-corrosion and natural environment resistance. The test results are shown in Table 7.
[0117] Table 7 Natural environment resistance of waterborne polyurethane latex film
[0118]
[0119] From the above test results, it can be seen that after 42 days of treatment, the film did not show any bubbling or falling off, and had a good anti-corrosion effect on the coated substrate, indicating that the prepared fluorosilicone water-based polyurethane has excellent resistance to natural environmental corrosion and can be used in metal corrosion protection.
[0120] Weigh a certain amount of fluorosilicone waterborne polyurethane emulsion, evenly coat it on the tinplate, dry it at room temperature for 48 hours, and then dry it in an oven at 60°C for 24 hours. The waterborne polyurethane forms a film on the tinplate and adheres tightly to it. After forming a film on the tinplate, immerse the tinplate in 5% sulfuric acid solution (Table 8), 5% sodium chloride solution (Table 9), and 5% sodium bicarbonate solution (Table 10) to test its chemical environment resistance.
[0121] Table 8 Acid resistance of waterborne polyurethane latex film
[0122]
[0123]
[0124] Table 9 Salt resistance of waterborne polyurethane latex film
[0125]
[0126] Table 10 Alkali resistance of waterborne polyurethane latex film
[0127]
[0128]
[0129] It can be seen from Tables 8 to 10 that when the polysiloxane content is 5wt% (Example 1), after immersion in 5% sulfuric acid or 5% sodium chloride solution for 30 days, the latex film did not show any bubbling or falling off, indicating that it has excellent resistance to acid and salt chemical environments; after immersion in 5% sodium bicarbonate solution for 20 days, the latex film did not show any bubbling or falling off, indicating that it has excellent resistance to alkali chemical environments.
[0130] 8. Determination of anti-graffiti performance of the waterborne polyurethane latex film of Example 1:
[0131] Weigh a certain amount of FSiWPU5 emulsion of Example 1, evenly apply it on a wooden board, dry it at room temperature for 48 hours, and then dry it in an oven at 60°C for 24 hours. The water-based polyurethane forms a film on the wooden board to form an antifouling coating. The droplet flow behavior of two different liquids (orange juice and dyed water) dripping onto the inclined antifouling coating was tested to study the liquid oleophobicity and antifouling properties of the coating. An anti-graffiti test was performed using a water-based pen. The coating was completely marked and completely dried for one minute in a well-ventilated environment. After that, the mark was wiped with a dry paper towel and photos were taken to record the appearance before and after erasure.
[0132] The test results are as follows Figure 3 As shown, it can be seen that orange juice and water can slide off the coating easily without leaving any traces, while when they slide off ordinary wooden boards or wooden boards coated with ordinary wood varnish, obvious water stains will be left. This comparison shows that the prepared FSiWPU5 coating has excellent anti-fouling properties and can effectively protect wooden boards. In addition, anti-graffiti ability is also an important criterion for judging the anti-fouling performance of coatings. In this study, the anti-graffiti performance of coatings was judged by observing the shrinkage behavior of water-based marker pen handwriting. The pictures shown compare the shrinkage behavior of water-based marker pen handwriting on different substrates. It can be seen that the handwriting did not shrink on the wooden board and the varnished wooden board. On the contrary, since the surface of the FSiWPU5 coating contains rich low-surface-energy fluorine and silicon elements, the handwriting of the marker pen on the wooden board coated with the FSiWPU5 coating shows a very obvious shrinkage behavior, and the handwriting can be easily wiped off with thin paper without leaving obvious visible traces, which means that the coating has excellent anti-graffiti performance.
[0133] 9. Determination of adhesion properties of aqueous polyurethane emulsions of Example 1 and Comparative Examples 1 to 2:
[0134] Two tinplate sheets or wooden boards were adhered together using the aqueous polyurethane emulsions of Example 1 and Comparative Examples 1-2, with an adhesion area of 2.5 cm 2 After the emulsion dries, test the adhesion performance of the emulsion. The test process and results are as follows: Figure 4 As shown in Table 11.
[0135] Table 11 Adhesion properties of waterborne polyurethane emulsion
[0136]
[0137] After 20 microliters of the emulsion was dripped as an adhesive, an object weighing 25.7 kg could be successfully lifted after the emulsion of Example 1 dried, indicating that the emulsion has extremely strong adhesion properties. In addition, after the tinplate sheet after adhesion was soaked in water for 7 days and then taken out, it was still able to easily lift a weight of 25.7 kg, proving that the emulsion has extremely strong water-resistant adhesion when used as an adhesive. Compared with the other samples, the FSiWPU5 emulsion of Example 1 showed the best adhesion properties on both tinplate and wood boards. This unexpected performance greatly expanded the application of waterborne polyurethane in adhesives, especially water-resistant adhesives.
[0138] In summary, when the polysiloxane content is 5wt%, the particle size of the fluorosilicone waterborne polyurethane emulsion is small, it can exist stably for a long time, and the emulsion has unexpected adhesion properties; the tensile strength of the film formed after the emulsion is dried increases, and the mechanical properties are improved; the contact angle of the film increases while the water absorption rate decreases, and the hydrophobic property is improved; the thermal stability of the film increases in the range of 400℃ to 500℃; the film has excellent resistance to natural environmental corrosion and chemical media (including acid, alkali and salt) corrosion. Comprehensive consideration shows that when the polysiloxane content is 5wt%, the comprehensive performance of the fluorosilicone waterborne polyurethane system is optimal.
[0139] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a fluorine-silicon composite modified hyperbranched aqueous polyurethane emulsion, It is characterized in that The steps include: In an inert atmosphere, poly(1,4-butylene adipate), dihydroxy-terminated polysiloxane and diisocyanate are reacted under the action of a catalyst to obtain a prepolymer; a hydrophilic chain extender is added to the prepolymer to react, a small molecule diol chain extender and a cross-linking agent are added to react, a fluorine-containing end-capping agent is added to react, and finally a neutralizing agent is added to react to obtain a polymer product; Add water to the polymer product, emulsify it at high speed shearing, and rotary evaporate until no solvent drips to obtain the product; Wherein, the addition amount of the dihydroxy-terminated polysiloxane is 4-6wt% of the total mass of the raw materials of the polymerization product.
2. The preparation method according to claim 1, It is characterized in that The number average molecular weight of the poly(1,4-butylene adipate) is 1500-2500Da; the molecular weight of the dihydroxy-terminated polysiloxane is 1000-3000Da, and the viscosity is 600-1000mPa·s.
3. The preparation method according to claim 2, Features The mass ratio of the poly(1,4-butylene adipate), diisocyanate, catalyst, hydrophilic chain extender, small molecule diol chain extender, crosslinking agent, fluorine-containing end-capping agent and neutralizing agent is (43-47): (28-34): (0.01-0.02): (3-6): (2.5-4): (0.8-1.5): (5-7): (3-4).
4. The preparation method according to claim 2, It is characterized in that The diisocyanate is selected from one or more of isophorone diisocyanate, 4,4-diisocyanate dicyclohexylmethane or toluene diisocyanate; The catalyst is selected from one or more of dibutyltin dilaurate, monobutyltin oxide, dibutyltin oxide, and dibutyltin diacetate; The hydrophilic chain extender is selected from one or more of dimethylol propionic acid, dimethylol butyric acid, 1,2-propylene glycol-3-sodium sulfonate, N-methyl-N,N-di(2-hydroxyethyl)betaine or 1,4-butanediol-2-sodium sulfonate.
5. The preparation method according to claim 1, It is characterized in that The hydrophilic chain extender is first dissolved in an organic solvent and then added to the prepolymer; the organic solvent is selected from one or more of acetone, methyl ethyl ketone, ethyl acetate, butyl acetate, dimethyl sulfoxide, tetrahydrofuran or methyl formate; the dosage ratio of the hydrophilic chain extender to the organic solvent is (2-4) g: 10 mL.
6. The preparation method according to claim 5, It is characterized in that The cross-linking agent is selected from one or more of trimethylolpropane, glycerol, pentaerythritol or butanethritol; The small molecule diol chain extender is selected from one or more of 1,4-butanediol, ethylene glycol, diethylene glycol, pentanediol, 1,2-propylene glycol, 1,3-propylene glycol, dipropylene glycol or 1,6-hexanediol; The fluorine-containing end-capping agent is selected from one or more of 1H,1H,2H,2H-perfluoro-1-octanol, hexafluoroisopropanol, 2,2,3,3,4,4,5,5-octafluoro-1-pentanol or 1H,1H,2H,2H-perfluoro-1-decanol; The neutralizing agent is one or more of trimethylamine, triethylamine, tributylamine and triethanolamine.
7. The preparation method according to claim 4, It is characterized in that The inert atmosphere is selected from one or more of nitrogen, argon, helium or neon; in the step of reacting under the action of a catalyst to obtain a prepolymer, the reaction temperature is 70-90°C and the reaction time is 80-110 min; in the step of reacting after adding a hydrophilic chain extender, the reaction temperature is 70-90°C and the reaction time is 110-140 min; in the step of adding a small molecule diol chain extender and a cross-linking agent to react, the reaction temperature is 70-90°C and the reaction time is 80-110 min; 110-140 min; in the step of adding a fluorine-containing end-capping agent to react, the reaction temperature is 70-90°C and the reaction time is 110-140 min; in the step of reacting to obtain a polymer product, the reaction temperature is 40-50°C and the reaction time is 50-70 min.
8. The preparation method according to claim 1, It is characterized in that In the step of adding water to the polymerization product, the mass ratio of the polymerization product to water is 3:(6-8); the rotation speed of the high-speed shear emulsification is 8000-12000 r / min, and the time of the high-speed shear emulsification is 8-15 min; the temperature of the rotary evaporation is 45-55°C.
9. The fluorine-silicon composite modified hyperbranched waterborne polyurethane emulsion prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the fluorine-silicon composite modified hyperbranched aqueous polyurethane emulsion as claimed in claim 9 as a water-resistant coating or a water-resistant adhesive.
Citation Information
Patent Citations
Water-based polyurethane emulsion used for waterproof paint and preparation method thereof
CN109265647A
Low-fluoride-silicon waterborne polyurethane emulsion and elastic film product thereof
CN109824849A
Fluorine-containing waterborne polyurethane as well as preparation method and application thereof
CN117362579A
Waterborne polyurethane with high mechanical strength and high elongation at break and preparation method thereof
CN117866170A
Manufacturing method of water based polyurethane adhesive composition with excellent adhesion
KR101784727B1
Cited By
Washing-free digital dyeing adhesive with disperse dye one-way loading function and preparation method of washing-free digital dyeing adhesive
CN119775526A
A waterless digital dyeing adhesive with a function of unidirectional loading of disperse dyes and a preparation method thereof
CN119775526B