Reinforced film-coated floor and preparation method thereof

By setting up a layered reinforced structure inside the base material of the wood-plastic floor and using prefabricated wear-resistant layers, and directly printing the pattern layer with printing technology, the problems of wood grain simulation and cost are solved, and high compressive strength and high elasticity are achieved Modulus flooring products reduce production costs and improve laying efficiency.

CN119041650AInactive Publication Date: 2024-11-29ANHUI SENTAI WPC TECH FLOOR CO LTD

Patent Information

Application Number
CN202411144653.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The wood grain simulation degree of existing wood plastic floors is not high, the production cost is high, and the compressive strength and elastic modulus are insufficient, making it difficult to meet the user's experience needs.

Method used

A layered reinforced structure is used to replace the UV resin coating with a prefabricated wear-resistant layer, and a pattern layer is directly printed on the carrier through printing technology to improve the adhesive strength between the pattern layer and the wear-resistant layer and reduce production cost.

Benefits of technology

Realize realistic flooring products with high compressive strength and large elastic modulus, reduce production costs, improve laying efficiency and material utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119041650A_ABST
    Figure CN119041650A_ABST
Patent Text Reader

Abstract

The invention relates to a reinforced film-coated floor. Belongs to the technical field of wood-plastic floors. The invention relates to a reinforced film-coated floor, which comprises a base material with a layered reinforcing structure inside; the wear-resistant layer at least covers the upper surface of the base material and plays a role in protecting the floor; the pattern layer is arranged between the base material and the wear-resistant layer and plays a role in decorating the floor; and the adhesive layer is arranged between the pattern layer and the wear-resistant layer, plays a role of elastic connection, and is provided with repeated carbamate chain segments. According to the invention, the prefabricated wear-resistant layer is adhered to the surface of the shell, so that the use amount of the UV light-cured resin is reduced, and the production cost is reduced; the layered reinforcement is arranged in the base material, so that the compressive strength and the elastic modulus of the floor are improved, the span can be increased when the floor is laid, the use amount of keels is reduced, the laying cost is reduced, and the laying efficiency is improved; meanwhile, the thermal shrinkage rate of the floor is also reduced; a balance layer is not needed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a film-covered floor, in particular to an enhanced film-covered floor and a preparation method thereof, belonging to the technical field of film-covered floors. Background Art

[0002] Wood plastic flooring is usually made by first extruding the wood plastic mixed raw materials from a mold through an extruder to form a base board, and then using a pattern roller to carve the wood texture on the base board. However, the wood texture pattern formed in this way is not only relatively simple, but also not realistic enough.

[0003] In order to improve the simulation degree of wood grain, targeted research and development has also been carried out in this field. For example, the Chinese invention patent application with publication number CN102294812A discloses a polystyrene imitation wood profile, which solves the appearance defect problem of plastic flooring itself to a certain extent. It is to put the surface material and the core material into the auxiliary extruder and the main extruder respectively, and co-extrude them into a mold so that the surface material is coated on the core material. The surface material is high-impact polystyrene and contains a rhytometric masterbatch that has good compatibility with high-impact polystyrene but different fluidity and dispersibility. The core material is a polystyrene micro-foam board. The surface of the co-extruded profile is embossed to produce a three-dimensional effect or other effects. This method uses base color masterbatches and rhytometric masterbatches of different colors. The base color masterbatch has good fluidity and is dispersed in the polystyrene material during the processing to form a base color; the rhytometric masterbatch has a low melt index and poor dispersibility. It cannot be evenly dispersed during the processing, and forms wood grain or other patterns as the material is extruded. However, the dispersion process of the flow color masterbatch is relatively random and difficult to control, and the base color and the flow color are prone to blending and color bleeding in adjacent areas. The imitation wood texture of the above co-extruded floor is quite different from the wood texture, and ordinary users can easily distinguish the above floor from solid wood flooring in appearance.

[0004] 3D printing technology can improve the simulation degree of wood grain. The patent document with publication number CN109653465A discloses a production method of PVC decorative board with 3D effect, which includes: coating UV primer on the surface of PVC board substrate; irradiation curing; coating UV white paint; irradiation curing; printing patterns with flatbed inkjet printer to obtain semi-finished products; coating UV wear-resistant paint; irradiation curing; printing concave-convex effect layer with flatbed inkjet printer; irradiation curing; coating UV topcoat; irradiation curing. However, the production of this floor relies on expensive production lines and requires coating of a large amount of UV resin, and the material cost is also difficult to reduce.

[0005] In addition, floors installed through keels usually require a higher elastic modulus, otherwise the floor will bend during use, which will greatly affect people's experience. Summary of the invention

[0006] The present invention aims to solve the above technical problems and provide a reinforced film-covered floor. The floor of the present invention has relatively low production cost, realistic wood grain, high compressive strength and large elastic modulus.

[0007] The technical solution of the present invention to solve the above problems is as follows: An enhanced film-covered floor comprising - A substrate having a hard thermoplastic shell on the outside and a foamed plastic filled inside, with a layered reinforcement structure between the thermoplastic shell and the foamed plastic; - a wear-resistant layer, covering at least the upper surface of the substrate, and protecting the floor; - a pattern layer, which is arranged between the substrate and the wear-resistant layer and serves to decorate the floor; - an adhesive layer, disposed between the pattern layer and the wear-resistant layer, having repeated urethane segments.

[0008] The main idea of ​​the above technical solution of the present invention is: 1. Improving the mechanical strength of the substrate by arranging a layered reinforcement structure inside the substrate; 2. Pasting a prefabricated wear-resistant layer on the substrate to replace the UV resin coating in the prior art, thereby significantly reducing the production cost.

[0009] As a preferred embodiment of the above technical solution, the pattern layer uses the substrate as a carrier and is printed on the decorative surface of the substrate; a primer layer is also provided between the pattern layer and the decorative surface of the substrate.

[0010] As another preferred embodiment of the above technical solution, the pattern layer uses a PVC white film as a carrier and is printed on the surface of the PVC white film; the PVC white film is connected to the substrate via a second adhesive layer.

[0011] In the above technical solution of the present invention, the pattern is directly printed on the carrier by using printing technology; compared with the thermal transfer technology, the adhesive strength between the pattern layer and the wear-resistant layer is effectively improved.

[0012] During the research and development process, the inventor used thermal transfer technology to transfer the pattern to the carrier film, because thermal transfer technology is more mature and has lower requirements for equipment. In order to improve the effect of thermal transfer, it is necessary to coat the carrier film with adhesive. However, when removing the transfer film, the transfer film is very difficult to remove, and even defective products may appear because the transfer film is not completely removed. However, if the curing time is controlled within 10 hours, the transfer film can be easily removed; but doing so brings a new problem. The adhesive strength between the transfer pattern and the carrier film will be significantly reduced. The inventor analyzed that this is because when the transfer film is removed, the initial adhesion of the adhesive layer between the transfer pattern and the carrier film is destroyed. For this reason, the inventor abandoned the transfer solution and adopted direct printing.

[0013] The products of the above two schemes are slightly different in structure. The main difference is that when making a pattern layer on a substrate, a primer is coated on the substrate to improve the bonding strength between the pattern and the substrate. Since the primer is located under the pattern layer, the primer can be a colored paint, such as adding a small amount of titanium dioxide to make the background color white, thereby covering the substrate and eliminating the base color difference caused by different batches.

[0014] The second solution is to set the pattern on the surface of the PVC white film through a flatbed inkjet printer to produce a color film with a realistic pattern; then apply adhesive on the pattern surface or wear-resistant layer of the color film to fit the pattern layer to the wear-resistant layer; finally, apply a second adhesive layer on the back surface or substrate of the color film to fit the pattern layer to the substrate.

[0015] The same thing about the two is that a UV protective layer can be further provided on the pattern layer, which can protect the pattern and make the pattern layer and the wear-resistant layer fit more firmly.

[0016] In addition, there is another situation where the pattern layer is set on the wear-resistant layer. In this solution, the primer can also be applied on the wear-resistant layer first to improve the bonding strength between the pattern and the wear-resistant layer; but in this case, since the primer is located on the upper surface of the pattern layer in the finished product, the primer can only be a transparent paint, otherwise the pattern layer will be covered; of course, it is not ruled out that the primer is deliberately made translucent to change the visual effect and make the pattern layer looming. After the pattern is printed, a UV protective layer can be further set on the pattern layer to make the pattern layer fit more firmly with the substrate.

[0017] As a preferred embodiment of the above technical solution, the substrate comprises a foam core formed of foam plastic, a thermoplastic shell, and a layered reinforcement formed of a reinforced fiber mesh cloth impregnated with a thermosetting resin and arranged between the foam core and the thermoplastic shell.

[0018] As a preferred embodiment of the above technical solution, the foaming core is a foamed product of polymerized olefins / olefin derivatives.

[0019] In the above technical solution of the present invention, the polymerized olefin may be polyethylene or polypropylene, and the polymerized olefin derivative may be polyvinyl chloride or polystyrene.

[0020] The polyolefin foamed product of the present invention is prepared by first preparing a master batch with polyolefin as the base resin and plant fiber powder and / or mineral powder as the filler; then the master batch is input into an extruder, a foaming agent is added (or a foaming agent is not added and then prepared by a physical foaming process), and then a processing aid is mixed in, and then extruded through a melt foaming die. Since the substrate of the present invention also includes a layered reinforcement and a shell, the preparation process of the foam core can also be combined with other processes. The foamed product of a polymerized olefin derivative is prepared by preparing a polymerized olefin derivative such as polyvinyl chloride as the base resin, and the process principle is the same.

[0021] As a preferred embodiment of the above technical solution, the layered reinforcement is formed by glass fiber mesh cloth impregnated with ABS resin.

[0022] As a preferred embodiment of the above technical solution, the base resin of the shell is polymerized olefin / olefin derivative.

[0023] As a further preferred embodiment of the above technical solution, the polymerized olefin derivative is polyvinyl chloride.

[0024] As a preferred embodiment of the above technical solution, the wear-resistant layer is a prefabricated PMMA film.

[0025] When PMMA is selected, PMMA not only has good mechanical properties, such as wear resistance and surface hardness, but also has good performance in isolating ultraviolet rays in natural light, and the products made are less likely to fade.

[0026] Another object of the present invention is to provide a method for preparing the above-mentioned floor.

[0027] A method for preparing an enhanced film-covered floor comprises the following steps: S1. providing a base material and a prefabricated wear-resistant layer; S2, applying a cleaning agent on the surface of the substrate to treat the lubricating wax on the surface of the substrate, and then performing a corona treatment; S3, applying a primer layer on the surface of the substrate, and printing a pattern on the primer layer using an industrial printer to form a decorative layer; S4, performing corona treatment on the wear-resistant layer, and controlling the dyne value to be above 50; S5, applying polyurethane hot melt adhesive on the decorative layer, or applying polyurethane hot melt adhesive on the back surface of the wear-resistant layer, and then hot-pressing the substrate and the wear-resistant layer; S6. Maintain health for more than 36 hours.

[0028] As a preferred embodiment of the above technical solution, the cleaning agent is dichloromethane.

[0029] Another object of the present invention is to provide another method for preparing the above floor.

[0030] A method for preparing an enhanced film-covered floor comprises the following steps: S1. providing a base material and a prefabricated wear-resistant layer; S2, applying a cleaning agent on the surface of the substrate to treat the lubricating wax on the surface of the substrate, and then performing a corona treatment; S3, providing a carrier film, and performing corona treatment on both sides of the carrier film, and controlling the dyne value to be above 46; S4, printing a pattern on the carrier film using an industrial printer to form a decorative layer; S5, applying polyurethane hot melt adhesive on the substrate, or applying polyurethane hot melt adhesive on the back surface of the decorative layer, and then hot pressing the decorative layer and the substrate; S6, health care for more than 16 hours; S7, corona treatment is performed on the wear-resistant layer, and the dyne value is controlled to be above 50; S8, applying polyurethane hot melt adhesive on the decorative layer, or applying polyurethane hot melt adhesive on the back surface of the wear-resistant layer, and then hot-pressing the substrate and the wear-resistant layer; S9. Maintain health for more than 36 hours.

[0031] As a preferred embodiment of the above technical solution, the cleaning agent is dichloromethane.

[0032] As a preferred embodiment of the above technical solution, the carrier film is a PVC white film.

[0033] During the research and development process, the inventors found that the second adhesive layer always cracked. At first, the inventors polished and corona treated the substrate, and the problem was significantly improved, but the cracking problem still occurred from time to time and could not be completely eliminated. Analysis showed that it was caused by oil leakage from the thermoplastic shell of the substrate. The so-called oil leakage refers to the fact that in the production process of the substrate, in order to facilitate molding and extrusion, some processing aids, such as polyethylene wax, stearate, etc., are often added to the material. These substances will slowly precipitate from the thermoplastic shell over time and gradually enrich at the interface between the thermoplastic shell and the second adhesive layer; because these substances have poor adhesion, when an enriched phase is formed, it is easy to cause local cracking of the second adhesive layer. In the above technical solution of the present invention, dichloromethane is first sprayed on the surface of the substrate, and then wiped clean with cloth or paper, etc., which can effectively remove the processing aid-rich phase that is difficult to detect with the naked eye; then the thermoplastic shell is polished and corona treated, and the polishing is to increase the surface roughness and provide more microscopic contact area; corona is an electric shock treatment that locally breaks the chemical bonds of the plastic molecules and produces carbonyl, hydroxyl and other highly polar groups, which make the surface of the object have higher adhesion and adhesion; thereby improving the adhesive strength between the PVC white film and the substrate, ensuring that the second adhesive layer does not crack.

[0034] As a preferred embodiment of the above technical solution, the substrate is prepared by the following method comprising the following steps: 1) The matrix resin is squeezed into the main channel of the mold through the main extruder to form a pressure-maintaining core; 2) Feeding the layered reinforcement into the reinforcement material channel of the mold; 3) Feed the shell resin into the co-extrusion flow channel of the co-extrusion die through the auxiliary extruder; extrude the shell resin from the co-extrusion flow channel to form a shell with a frame-shaped cross-section; 4) The pressure-retaining core, the layered reinforcement and the shell are extruded from respective independent flow channels to form a mold blank; at the same time, the mold blank is passed into a shaping die, and the pressure-retaining core is foamed in the shell constrained by the inner wall of the shaping die to fill the shell, and at the same time, the mold blank is compounded and cooled in the shaping die to obtain the substrate.

[0035] Regarding the question of how to implant the layered reinforcements; this is difficult for those skilled in the art, because it is generally understood that in order to fuse the layered reinforcements with the foamed core, the reinforcement material channel must be connected to the main channel, so that the glass fiber reinforcement layer can be integrated into the foamed layer. The problem with this is that there is a lot of pressure inside the main channel. Once the reinforcement material channel is connected to the main channel, the pressure will be released in the reverse direction along the reinforcement material channel, and the material in the main channel will naturally be squeezed into the reinforcement material channel, and even further foamed, thereby blocking the reinforcement material channel, making it difficult to continue to input the layered reinforcements, forcing production to be interrupted; generally speaking, the mold needs to be disassembled and the reinforcement material channel needs to be cleaned within a very short production cycle. In addition, due to the early pressure relief, some areas foam in advance, which also makes it difficult to control the quality of the foamed core.

[0036] In the above technical scheme of the present invention, the above problems are solved by changing the production method and modifying the mold. It is mainly manifested in the following aspects: in the mold, 1. The main channel is designed to maintain pressure in the entire mold; 2. The reinforcing material channel, the co-extrusion channel and the main channel are independent of each other, and they are merged at the port of the mold discharge plate; 3. A shaping die is installed at the mold outlet; in terms of method, 1. Abandon the previous idea of ​​forming a composite sheet from the mold outlet; 2. Abandon the previous idea of ​​the shell material covering the formed foaming core, use a prefabricated shell, use the foaming core to be foamed to fill the formed shell, and insert the layered reinforcement before filling. Specifically for the present invention, the filling is not to continuously transport the filling material into the shell, but to achieve it by the automatic foaming and expansion of the pressure-maintaining core after it comes out of the pressure-maintaining main channel; therefore, after the mold blank is extruded from the mold, it needs to enter the shaping die immediately, and the shaping die is used to constrain the shell, so that the pressure-maintaining core is foamed in the shell constrained by the inner wall of the shaping die, and the shell is filled. At the same time, the shaping mold can also be placed in a water tank to improve the cooling and shaping effect of the shaping mold.

[0037] Another object of the present invention is to provide a co-extrusion mold for preparing the above floor.

[0038] The co-extrusion die is provided with a main channel, a reinforcing material channel and a co-extrusion channel; the main channel, the reinforcing material channel and the co-extrusion channel are independent of each other in the die and converge at the outlet of the co-extrusion die; The reinforcing material channel comprises a first channel and a second channel distributed on both sides of the main channel, the first channel has a first straight-line discharge port, and the second channel has a second straight-line discharge port; The discharge port of the co-extrusion channel is a rectangular ring structure and is sleeved around the discharge port of the main channel, and the first discharge port is arranged between the upper frame of the discharge port of the main channel and the upper frame of the co-extrusion channel outlet, and the second discharge port is arranged between the lower frame of the discharge port of the main channel and the lower frame of the co-extrusion channel outlet.

[0039] In summary, the present invention has the following beneficial effects: 1. The present invention improves the compressive strength and elastic modulus of the floor by arranging a layered reinforcement inside the substrate, which can increase the span when laying the floor, reduce the amount of keels, reduce the laying cost, and improve the laying efficiency; 2. The present invention reduces the thermal shrinkage of the floor by arranging a layered reinforcement inside the substrate; no balancing layer is required; 3. The present invention reduces the amount of UV light-curing resin used by pasting a prefabricated wear-resistant layer on the shell surface, thereby reducing production costs; 4. The wear-resistant layer of the present invention is made of PMMA material, which has the advantages of high hardness, wear resistance and yellowing resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 It is a schematic diagram of the product structure; Figure 2 is a schematic diagram of the surface structure of Example 1; Figure 3 is a schematic diagram of the surface structure of Example 2; In the figure, 1-substrate, 2-decorative layer, 3-wear-resistant layer; 11- foam core, 12- reinforcement, 13- thermoplastic shell; 21-carrier layer, 22-pattern layer; 201 - adhesive layer, 202 - second adhesive layer. DETAILED DESCRIPTION

[0041] The present invention is further explained below in conjunction with the accompanying drawings.

[0042] This specific implementation is only an explanation of the present invention, not a limitation of the present invention. Any changes made by those skilled in the art after reading the description of the present invention, as long as they are within the scope of the claims, will be protected by the patent law.

[0043] Embodiment 1 like Figure 1~2As shown, a reinforced laminate floor comprises a substrate 1, a decorative layer 2 and a prefabricated wear-resistant layer 3 arranged in sequence; an adhesive layer 201 is arranged between the decorative layer 2 and the wear-resistant layer 3; and a second adhesive layer 202 is arranged between the decorative layer 2 and the substrate 1. The decorative layer 2 is formed by a pattern layer 22 arranged on a carrier layer 21.

[0044] The substrate 1 is resin-based, such as Figure 1 As shown, it includes a foam core 11 , a layered reinforcement 12 and a thermoplastic shell 13 . The shell covers the foam core 11 , and the layered reinforcement 12 is arranged between the foam core 11 and the thermoplastic shell 13 .

[0045] Specifically, the foam core 11 is a PVC foam product with a density of about 0.8 g / m³.

[0046] The layered reinforcement 12 is a glass fiber mesh impregnated with ABS.

[0047] The shell is non-foamed or low-foamed PVC.

[0048] In this embodiment, the carrier layer 21 is a prefabricated white PVC film.

[0049] The preparation method of the above-mentioned film-coated floor is as follows: S1. Provide a substrate and a prefabricated wear-resistant layer, wherein the wear-resistant layer is made of PMMA thin sheet with a thickness of about 0.5 mm; S2, applying dichloromethane to the surface of the substrate to treat the surface of the substrate, and then wiping it clean with a cleaning cloth; S3, provide a PVC white film, with corona on both sides, and the dyne value of the corona reaches 46; S4. Printing a pattern on the PVC white film by a flatbed inkjet printer, and curing the pattern layer to produce a PVC color film with a pattern layer; the pattern layer is formed by curing the water-based color paste, and the amount used is about 30mL / ㎡; S5, applying polyurethane hot melt adhesive to the non-printing surface of the PVC color film, and then hot-pressing the decorative layer and the substrate; S6, health care for 16 hours; S7, performing corona treatment on the wear-resistant layer, wherein the dyne value of the corona reaches 50; S8, applying polyurethane hot melt adhesive on the corona surface of the wear-resistant layer, and then hot-pressing the substrate and the wear-resistant layer; S9. Maintain health for 36 hours.

[0050] The substrate 1 is prepared by the following method: 1) The matrix resin is squeezed into the main channel of the mold through the main extruder to form a pressure-maintaining core; 2) Feeding the layered reinforcement into the reinforcement material channel of the mold; 3) Feed the shell resin into the co-extrusion flow channel of the co-extrusion die through the auxiliary extruder; extrude the shell resin from the co-extrusion flow channel to form a shell with a frame-shaped cross-section; 4) The pressure-retaining core, the layered reinforcement and the shell are extruded from respective independent flow channels to form a mold blank; at the same time, the mold blank is passed into a shaping die, and the pressure-retaining core is foamed in the shell constrained by the inner wall of the shaping die to fill the shell, and at the same time, the mold blank is compounded and cooled in the shaping die to obtain the substrate.

[0051] Embodiment 2 like Figure 1 and 3 As shown, a reinforced laminate floor comprises a substrate 1, a decorative layer 2 and a prefabricated wear-resistant layer 3; wherein an adhesive layer 201 is provided between the pattern layer 2 and the wear-resistant layer 3.

[0052] The substrate 1 is resin-based, such as Figure 1 As shown, it includes a foam core 11, a layered reinforcement 12 and a thermoplastic shell 13. The shell covers the foam core 11, and the layered reinforcement 12 is arranged between the foam core 11 and the shell 13.

[0053] Specifically, the foam core 11 is a PVC foam product with a density of about 0.8 g / m³.

[0054] The layered reinforcement 12 is a glass fiber mesh impregnated with ABS.

[0055] The shell is non-foamed or low-foamed PVC.

[0056] In this embodiment, the carrier layer 21 is a primer layer disposed on the substrate 1 .

[0057] The preparation method of the above-mentioned film-coated floor is as follows: S1. Provide a substrate and a prefabricated wear-resistant layer, wherein the wear-resistant layer is made of PMMA thin sheet with a thickness of about 0.5 mm; S2, applying dichloromethane to the surface of the substrate to treat the surface of the substrate, wiping it clean with a cleaning cloth, and then performing corona treatment; S3, applying a primer layer on the surface of the substrate and curing it by irradiation; the primer formula is: 75% acrylate, 3.5% photoinitiator 184, 1.5% photoinitiator TPO, 10.0% diluent hydroxyethyl acrylate, 10% titanium dioxide; the dosage is 10g / ㎡; S4. Use an industrial printer to print a pattern on the primer layer to form a pattern layer, and solidify the pattern layer; the pattern layer is formed by solidifying the water-based color paste, and the amount used is about 30mL / ㎡; S5, performing corona treatment on the wear-resistant layer, and controlling the dyne value to be above 50; S6, applying polyurethane hot melt adhesive to the corona surface of the wear-resistant layer, and then hot-pressing the substrate and the wear-resistant layer together; S7. Maintain health for 36 hours.

[0058] Comparative Example 1 According to patent document CN 110670839B, a foamed floor with wood texture is produced.

[0059] The products of Example 1, Example 2 and Comparative Example 1 were tested in accordance with the relevant contents of BS EN 15534-1-2014+A1-2017 to measure their bending failure load, bending strength, bending elastic modulus and thermal shrinkage. The results are shown in the following table.

[0060] The following abrasion resistance test and immersion peeling test were performed on Examples 1 and 2.

[0061] The wear test is carried out according to EN 660-2 and the mass loss per 100 revolutions is calculated.

[0062] The immersion peeling test is carried out in accordance with GB / T 17657-2013.

[0063] The wear test results are shown in the following table: The results of the immersion stripping test are shown in the following table: Dip stripping / mm Example 1 0mm Example 2 0mm

Claims

1. A reinforced film-covered floor, characterized in that: include - a substrate (1) having a hard thermoplastic shell on the outside and a foamed plastic filled inside, with a layered reinforcement structure between the thermoplastic shell and the foamed plastic; - a decorative layer (2), covering the substrate, comprising a carrier layer (21) and a pattern layer (22) arranged on the carrier layer; - a wear-resistant layer (3), covering the decorative layer and playing a protective role; - an adhesive layer (201), arranged between the decorative layer and the wear-resistant layer, and having repeated urethane segments.

2. The enhanced film-covered floor according to claim 1, characterized in that: The carrier layer (21) is a primer layer provided based on the substrate.

3. The enhanced film-covered floor according to claim 1, characterized in that: The carrier layer (21) is a prefabricated carrier film, and the carrier film is connected to the substrate (1) via a second adhesive layer (202).

4. The enhanced film-covered floor according to claim 1, characterized in that: The substrate comprises a foam core (11) formed of foam plastic, a thermoplastic shell (13), and a layered reinforcement (12) formed of a reinforced fiber mesh cloth impregnated with a thermosetting resin and arranged between the foam core (11) and the thermoplastic shell (13).

5. The enhanced film-covered floor according to claim 4, characterized in that: The foam core (11) is a foamed product of polymerized olefins / olefin derivatives.

6. The enhanced film-covered floor according to claim 4, characterized in that: The layered reinforcement (12) is formed by glass fiber mesh cloth impregnated with ABS resin.

7. The enhanced film-covered floor according to claim 4, characterized in that: The base resin of the shell (13) is polymerized olefin / olefin derivative.

8. The enhanced film-covered floor according to claim 7, characterized in that: The polymerized olefin derivative is polyvinyl chloride.

9. The method for preparing the enhanced film-covered floor according to claim 2, comprising the following steps: S1, providing a substrate (1) and a prefabricated wear-resistant layer (3); S2, applying a cleaning agent to the surface of the substrate (1) to treat the lubricating wax on the surface of the substrate, and then performing a corona treatment; S3, applying a primer layer on the surface of the substrate (1), and printing a pattern on the primer layer using an industrial printer to form a decorative layer (2); S4, performing corona treatment on the wear-resistant layer (3), and controlling the dyne value to be above 50; S5, applying polyurethane hot melt adhesive on the decorative layer (2), or applying polyurethane hot melt adhesive on the back surface of the wear-resistant layer (3), and then hot pressing the substrate (1) and the wear-resistant layer (3); S6. Maintain health for more than 36 hours.

10. The method for preparing the enhanced film-covered floor according to claim 3, comprising the following steps: S1, providing a substrate (1) and a prefabricated wear-resistant layer (3); S2, applying a cleaning agent to the surface of the substrate (1) to treat the lubricating wax on the surface of the substrate, and then performing a corona treatment; S3, providing a carrier film, and performing corona treatment on both sides of the carrier film, and controlling the dyne value to be above 46; S4, using an industrial printer to print a pattern on the carrier film to form a decorative layer (2); S5, applying polyurethane hot melt adhesive on the substrate (1), or applying polyurethane hot melt adhesive on the back surface of the decorative layer (2), and then hot pressing the decorative layer (2) and the substrate (1); S6, health care for more than 16 hours; S7, performing corona treatment on the wear-resistant layer (3), and controlling the dyne value to be above 50; S8, applying polyurethane hot melt adhesive on the decorative layer (2), or applying polyurethane hot melt adhesive on the back surface of the wear-resistant layer (3), and then hot pressing the substrate (1) and the wear-resistant layer (3); S9. Maintain health for more than 36 hours.

Citation Information

Patent Citations

  • Novel highly wear-resistant and anti-skid polyvinyl chloride (PVC) floor and preparation technology thereof

    CN107345442A

  • Plate with transfer pattern decorative layer and preparation method thereof

    CN112238656A

  • Reinforced wood texture floor as well as preparation method and mold thereof

    CN115027116A

  • Wood-plastic fence printing plate

    CN117246017A

  • Composite film and preparation method thereof, and preparation method of film pasting plate

    CN118003732A

Cited By

  • Polyolefin-based LVT floor and preparation method thereof

    CN121024282A

  • Outdoor paving floor and preparation method thereof

    CN122358838A

  • Preparation method for reinforced film-coated floor

    WO2026040891A1

  • Manufacturing method for joining assembly, joining assembly, and composite floor

    WO2026148717A1