Tin oxide-containing dispersion, method for manufacturing the same, film formation coating liquid and method for manufacturing base material with film

A dispersion liquid with sintered tin oxide secondary particles and a specific dispersant balances conductivity and transparency in conductive films by optimizing particle size and dispersant use, addressing grain boundary resistance issues.

JP2024146605AActive Publication Date: 2024-10-15JGC CATALYSTS & CHEMICALS LTD

Patent Information

Application Number
JP2023059608
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

Existing conductive films face challenges in achieving both high transparency and conductivity due to issues with grain boundary resistance, which is influenced by particle size and the presence of dispersants in the coating solution.

Method used

A dispersion liquid containing sintered tin oxide secondary particles with an average diameter of 170 to 700 nm, a dispersant with a sulfo or sulfonyl group, and an organic solvent, along with a binder, is used to form a coating film that balances conductivity and transparency by minimizing grain boundary resistance.

Benefits of technology

The solution results in a film with high conductivity and transparency, achieved by optimizing particle size and dispersant usage to reduce grain boundary resistance and maintain dispersibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146605000001
    Figure 2024146605000001
Patent Text Reader

Abstract

To provide a dispersion and a coating liquid, capable of forming a coating film that achieves both conductivity and transparency.SOLUTION: A dispersion includes: secondary particles obtained by sintering tin oxide-containing particles; a dispersant having a sulfonic group or a sulfonyl group and having a carbon number of 6 or more; and an organic solvent. The average particle size of the secondary particles is 170-700 nm; and 1.0×1015 or more and less than 1.0×1017 sulfonic groups or sulfonyl groups per 1 nm2 of the surface area of the secondary particles are included in the dispersion.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a conductive tin oxide-containing dispersion, and a coating liquid for film formation and a film-coated substrate prepared using the dispersion. [Background technology]

[0002] Conventionally, the formation of conductive films from coating solutions using dispersions containing conductive particles has been studied. Such conductive films are used as antistatic films for displays of personal computers, car navigation systems, touch panels, etc. Preventing the film from becoming charged can prevent the adhesion of dirt and other debris.

[0003] The properties required for an antistatic film are, of course, high conductivity (low electrical resistivity), but high transparency is also required to ensure visibility on displays, etc. To achieve high transparency, it is important that the particles are dispersed in the solvent and coating film without agglomerating.

[0004] Patent Document 1 discloses a coating liquid containing tin-containing metal oxide particles, which are aggregates of primary particles having an average particle size of 1 to 50 nm, a dispersant, and a solvent. The particles contained in this coating liquid have a small secondary particle size of 2 to 100 nm, so that a film made of the coating liquid using this dispersion has high transparency.

[0005] Patent Document 2 discloses a composition for forming an antistatic film, which contains inorganic oxide particles having sulfonic acid groups on the surface and a matrix forming component, in order to obtain a transparent coating excellent in antistatic performance, haze, transparency, strength, scratch resistance, hardness, etc. Since the inorganic oxide particles have sulfonic acid groups on the surface, the film containing these particles has high conductivity. In addition, since the particle diameter is small at 5 to 50 nm, the transparency is excellent.

[0006] Generally, factors that cause electrical resistance in a conductive film using a conductive filler include resistance within the filler (bulk resistance) and resistance at the interface between the fillers (grain boundary resistance). Bulk resistance varies greatly depending on the filler material, and grain boundary resistance increases as the number of particle interfaces in the path through which electricity flows (conductive path) increases. In addition, the presence of a dispersant that has penetrated into the grain boundaries further increases the grain boundary resistance. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2015-511575 A [Patent Document 2] JP 2007-106936 A Summary of the Invention [Problem to be solved by the invention]

[0008] The coating solution containing the tin-containing metal oxide particles described in the cited document 1 shows high transparency when formed into a coating film, but because the average particle size is small, adding the amount of particles necessary to make the coating film have the desired electrical conductivity results in a large number of particles in the film. As a result, the number of contact points between particles increases, increasing the grain boundary resistance, and the resistance of the film increases. If the secondary particle size is increased to reduce the grain boundary resistance in the coating film, the specific surface area of ​​the secondary particles decreases, and a large amount of dispersant that cannot be adsorbed on the secondary particle surface is present in the dispersion or coating solution. When formed into a coating film, the dispersant penetrates between the particles, increasing the grain boundary resistance, and the electrical conductivity of the film decreases.

[0009] The particles described in the cited document 2 have a small particle diameter of 5 to 50 nm, and therefore can provide a film with excellent transparency. However, because the specific surface area is large, a large amount of dispersant is required to stably disperse the particles in a dispersion liquid, and when a large amount of dispersant is used, the dispersants chemically bond with each other, resulting in a thick layer of dispersant covering the particle surface, which tends to increase grain boundary resistance when formed into a coating film.

[0010] Therefore, an object of the present invention is to provide a dispersion and a coating liquid capable of forming a coating film having both electrical conductivity and transparency. [Means for solving the problem]

[0011] The dispersion of this embodiment is a dispersion containing secondary particles formed by sintering tin oxide-containing particles (hereinafter referred to as tin oxide-containing secondary particles), a dispersant having a sulfo group or a sulfonyl group, and an organic solvent. The average particle size of the secondary particles is 170 to 700 nm, the dispersant has 6 or more carbon atoms, and the sulfo group or the sulfonyl group in the dispersant is 100% or more. The surface area of ​​the tin oxide secondary particles is 1 nm 2 For 1.0×10 15 pcs or more 1.0×10 17 A film obtained from a coating solution containing a dispersion of such a composition exhibits high electrical conductivity and is also highly transparent.

[0012] The method for producing the dispersion includes a step of mixing a tin oxide-containing powder, a dispersant, and an organic solvent to prepare a suspension (mixing step), and a step of dispersing the suspension to prepare a dispersion of tin oxide-containing secondary particles (dispersing step). In the dispersing step, the average particle size of the tin oxide-containing secondary particles is adjusted to 170 to 700 nm. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The dispersion of the present invention contains secondary particles formed by sintering tin oxide-containing particles, a dispersant having a sulfo group or a sulfonyl group and a carbon number of 6 or more, and an organic solvent. The average particle size of the secondary particles is 170 to 700 nm, and the surface area of ​​the secondary particles is 1 nm 2 1.0×10 15 pcs or more 1.0×10 17 Fewer than one sulfo or sulfonyl group is contained in the dispersion.

[0014] By using tin oxide-containing secondary particles with an average particle size of 170 to 700 nm, a film with high transparency and good electrical conductivity can be obtained. If the average particle size is less than 200 nm, a highly transparent dispersion is obtained, but the electrical conductivity is low. On the other hand, if the average particle size exceeds 700 nm, the electrical conductivity is improved, but the transparency is reduced.

[0015] The crystallite diameter of the tin oxide-containing particles is preferably 5 to 15 nm. When the crystallite diameter is 5 nm or more, the crystallinity of the tin oxide particles is high, so that the conductivity of the particles themselves is high, and the conductivity of the resulting film is high. When the crystallite diameter is 15 nm or less, the transparency of the particles themselves is high, and the transparency of the resulting film is also high. In other words, when the crystallite diameter is in the above range, the film formed from the coating liquid using the dispersion liquid containing the tin oxide-containing particles has both transparency and conductivity.

[0016] [Tin oxide-containing particles (primary particles)] The average particle size of the tin oxide-containing particles is preferably 20 to 40 nm. When the primary particle size is within the above range, the secondary particles formed by sintering these particles also have high transparency when formed into a coating film. In other words, when the primary particle size is 170 to 700 nm, light is scattered when passing through the coating film, and transparency is reduced. On the other hand, the particles of the present invention are secondary particles formed by sintering particles having a small average particle size as described above, so that when formed into a film, scattering of light passing through the coating film is suppressed compared to a film containing particles simply having a particle size within the above range, and as a result, a conductive film with high transparency is obtained.

[0017] As the tin oxide-containing powder, for example, a tin oxide-containing powder manufactured by a method described in Japanese Patent Application Laid-Open No. 6-76636 or Japanese Patent Application No. 62-51008 can be used. In addition, as a method for preparing a tin oxide-containing powder, a method of neutralizing a tin ion solution and a method of adding a solution of tin chloride dissolved in heated water to perform hydrolysis can be mentioned. The neutralization method will be explained below. After ionizing tin oxide by adding an acid, the ions are neutralized using a base. This results in a precipitate of tin oxide. This is dried and fired to obtain a tin oxide-containing powder. During neutralization, antimony trioxide is also ionized and can be neutralized (co-precipitated) together with the tin ions. Co-precipitation allows antimony to be doped into the tin oxide-containing powder. Doping 2 to 12 mass % of antimony with respect to the total amount of tin oxide particles to be prepared increases the conductivity of the tin oxide particles.

[0018] [Dispersant] In the present invention, the dispersant refers to a surfactant, a coupling agent, etc. A surfactant is specifically a substance having a hydrophilic part and a hydrophobic part in one molecule. A coupling agent is a metal alkoxide having an organic functional group and an alkoxy group in one molecule.

[0019] The dispersant used in the dispersion of the present invention contains a sulfo group or a sulfonyl group. Although the details are unclear, it is thought that the dispersant has these functional groups, which form an extremely thin hydration layer on the particle surface, making it easier for electricity to flow. This makes it possible to suppress an increase in grain boundary resistance between particles in the film when it is made into a film, resulting in a transparent and highly conductive film.

[0020] The dispersant used in the present invention includes a surfactant such as decane sulfonic acid, and a titanate coupling agent having a sulfo group or a sulfonyl group in the organic chain.

[0021] The dispersant has a sulfo group or a sulfonyl group in the molecule, and the surface area of ​​the secondary particles is 1 nm 2 For 1.0×10 15 pcs or more 1.0×10 17When the content is within this range, the tin oxide particles can be uniformly dispersed in the dispersion to have a size within the above-mentioned range of secondary particle diameter, while suppressing an increase in grain boundary resistance when the tin oxide particles are formed into a film. On the other hand, when the dispersant is added in an amount greater than the above-mentioned range, the molecular chains of the dispersant adsorbed on the surfaces of the tin oxide-containing secondary particles become entangled with each other, causing the particles to aggregate, resulting in a decrease in dispersibility, a dispersion with a particle diameter smaller than the above-mentioned range of secondary particle diameter is obtained, and when the film is formed, the conductivity decreases due to the large amount of dispersant contained between the particles.

[0022] Here, the surface area of ​​the particle is calculated by the formula "4πr 2 " (π is the constant of the circumference of a circle, and r is the volume average particle diameter measured by the centrifugal sedimentation method divided by 2).

[0023] The carbon number of the dispersant is 6 or more. If it is less than 6, the molecular chain is too short to function as a dispersant, and the particles aggregate in the dispersion, resulting in a decrease in the transparency of the film when made into a film. A preferred carbon number is 6 to 18. With a carbon number in this range, it is possible to achieve both the dispersibility of the particles in the dispersion and the electrical conductivity and transparency of the film when made into a film.

[0024] [Organic solvents] The organic solvent used here may be any solvent that can be removed by a drying process or the like after application and can dissolve the dispersant. Examples of the organic solvent include alcohol, glycol, glycol ethers, ketones, and aromatic hydrocarbons. Specific examples include isopropyl alcohol, butanol, methyl ethyl ketone (MEK), toluene, methyl isobutyl ketone (MIBK), and cyclohexanone.

[0025] [Other ingredients] Other components may be added to the coating solution using the dispersion of the present invention as necessary. For example, when a film is formed using a coating solution containing silica particles, the film has high conductivity and low haze. This is believed to be because the tin oxide particles are present along the periphery of the silica particles, which makes it easier to form a conductive path. In addition, when the coating solution contains silica particles, the film surface becomes slippery, so when used on the outermost surface, it has the effect of improving scratch resistance and is easy to prevent the films from sticking to each other when the substrates are stacked. Therefore, the substrate with the film is easy to handle.

[0026] <Coating solution> A coating liquid is prepared by adding a binder to the above-mentioned tin oxide-containing secondary particle dispersion liquid. Even if a binder is added to this dispersion liquid, the tin oxide-containing secondary particles are unlikely to aggregate. Even if they aggregate, they are redispersed by irradiating the coating liquid with ultrasonic waves.

[0027] The redispersion of the tin oxide particles is promoted by adding an additional dispersant as described above before the ultrasonic irradiation. The type of the dispersant may be the same as or different from the dispersant already contained in the dispersion liquid.

[0028] [Binder] The binder may be any binder that can be dissolved in an organic solvent and can form a conductive film. For example, it may be a thermoplastic resin, a thermosetting resin, an ultraviolet-curing resin, etc. A mixture of multiple types of binders may be used.

[0029] [Organic solvent for coating liquid] If necessary, an organic solvent may be added to the coating liquid for the purpose of adjusting the concentration to form a film, suppressing the drying speed, and adjusting the viscosity and surface tension. The organic solvent to be added may be the same type as the organic solvent derived from the dispersion liquid or a different type, as long as it can dissolve the dispersant and the binder.

[0030] A substrate with a film can be manufactured by applying the above-mentioned coating liquid onto a substrate and drying it. The substrate may be any substrate that can form a uniform liquid film and can withstand the drying temperature. Coating methods include bar coater method, dip method, spray method, spinner method, roll coating method, gravure coating method, slit coating method, and pressure coating method. The average film thickness can be appropriately selected depending on the application. If the average film thickness is 50 nm or more, it is easy to suppress sudden voltage changes caused by static electricity. The average film thickness is preferably 80 nm or more. If the average film thickness is 1000 nm or less, transparency is high. The average film thickness is preferably 300 nm or less.

[0031] <Method of producing coating liquid> The method for producing the coating liquid will be described below.

[0032] First, a tin oxide-containing powder precursor is calcined to prepare a tin oxide-containing powder [first step]. Next, in the presence of a dispersant having a sulfo group or a sulfonyl group and an organic solvent, the tin oxide-containing powder is dispersed so that the average particle size is 170 nm to 700 nm to prepare a tin oxide-containing secondary particle dispersion [second step]. After that, a binder is added to prepare a coating liquid [third step].

[0033] 《First step》 The tin oxide powder precursor is calcined to obtain a tin oxide-containing powder. The calcination temperature is preferably 400° C. to 700° C. At this calcination temperature, the crystallinity of the tin oxide-containing particles is improved.

[0034] 《Second step》 A tin oxide-containing powder, a dispersant, and an organic solvent are mixed to prepare a suspension of the tin oxide-containing powder. Here, a dispersant having a sulfo group or a sulfonyl group is mixed as the dispersant. If such a dispersant is used, the dispersed tin oxide secondary particles are easily dispersed in an organic solvent without re-aggregation. It is preferable to mix and dissolve the dispersant in an organic solvent to prepare a dispersant solution, and then mix the tin oxide-containing powder and the dispersant solution. With this method, the dispersant is uniformly applied to the surface of the tin oxide-containing secondary particles in the dispersion step. The tin oxide-containing secondary particles are dispersed so that the average particle diameter is 170 to 700 nm. When the average particle diameter of the tin oxide-containing secondary particles is 170 nm or more, high conductivity is obtained when the particles are made into a film. On the other hand, when the average particle diameter of the tin oxide particles is 700 nm or less, the transparency of the film is reduced.

[0035] The tin oxide-containing powder can be pulverized using a media mill such as a bead mill, a high-speed stirrer, a high-pressure homogenizer, an ultrasonic homogenizer, a wet grinding machine such as a jet mill. In particular, the use of a bead mill makes it easy to disperse the tin oxide-containing powder in the suspension. When a bead mill is used, the dispersion time, peripheral speed, and bead packing rate must be appropriately adjusted depending on the size and shape of the bead mill used. The bead diameter is appropriately adjusted depending on the peripheral speed. When the beads used are glass or zirconia, they are easy to obtain. When the beads used are inorganic oxides such as zirconia or alumina, the energy given to the tin oxide-containing powder is high, so that the tin oxide-containing powder is easily dispersed. After dispersion, the dispersion liquid can be filtered using a stainless steel wire mesh or the like to remove coarse particles. EXAMPLES

[0036] [Example 1] The preparation methods of the dispersion liquid and the coating liquid are specifically described below. The preparation conditions of the dispersion liquid and the coating liquid in other examples and comparative examples are also shown in Table 1.

[0037] <Preparation of tin oxide-containing powder> First, a tin oxide-containing powder was prepared as follows. 153 g of potassium stannate was dissolved in 343 g of water. 9.3 g of tartar emetic was added and dissolved therein. This was added together with nitric acid to warm water at 50° C. over 12 hours so as to maintain the pH at 8.5. This resulted in a tin oxide powder precursor aqueous dispersion. The tin oxide powder precursor was filtered out from the tin oxide powder precursor aqueous dispersion and washed. Thereafter, the tin oxide powder was dried at 100° C. for 5 hours and further calcined at 550° C. for 3 hours to obtain a tin oxide-containing powder. The crystallite size of the obtained particles was 10.4 nm.

[0038] The crystallite size was measured using Rigaku's RINT (registered trademark) 1400 (X-ray structure analyzer) for tin oxide-containing powder. The diffraction peak pattern was analyzed using PDXL, and the crystallite size of the particles was calculated from the half-width of the diffraction peak using Scherrer's formula (D = K x λ / (β x cosθ)). D is the crystallite size (nm), K is the Scherrer constant, λ is the wavelength of the X-ray (nm), β is the spread of the diffraction line width (rad), and θ is the Bragg angle (rad).

[0039] <Preparation of tin oxide-containing secondary particle dispersion> Next, the tin oxide-containing powder, the dispersant, and the organic solvent were mixed to prepare a suspension. 1.7 g of dioctyl sulfosuccinate sodium salt (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., active ingredient 96%) was mixed as a dispersant, and 74.5 g of cyclohexanone (manufactured by Hayashi Pure Chemical Industries, Ltd.) was mixed as an organic solvent. This was stirred for 10 minutes to prepare a dispersant solution. 76.2 g of this dispersant solution was mixed with 45.7 g of tin oxide-containing powder in a 500 mL glass beaker to prepare a suspension.

[0040] 230 g of glass beads BZ-06 (manufactured by AS ONE Corporation, bead diameter 0.5 mmφ) was added to 121.9 g of the suspension. Tin oxide-containing secondary particles were prepared by dispersing the tin oxide-containing powder in the suspension using a batch-type bead mill Easy Nano RMBII type. Dispersion was continued until the average particle diameter of the tin oxide-containing secondary particles reached 190 nm (average particle diameter of the tin oxide particles listed in Table 1) (in other examples and comparative examples, dispersion was continued until the average particle diameter of the tin oxide-containing secondary particles reached the average particle diameter listed in Table 1). The peripheral speed of the bead mill was 12 m / s. Glass beads were separated from the suspension using a stainless steel wire mesh with a mesh size of 44 μm. Cyclohexanone was added to this to prepare a tin oxide-containing secondary particle dispersion (solid concentration 35.0 mass%).

[0041] The average particle size of the tin oxide-containing secondary particles was measured by diluting the dispersion liquid with an organic solvent to a solid concentration of 0.3%, and using a centrifugal sedimentation size measuring device BI-DCP (manufactured by Brookhaven Instruments Corporation).

[0042] <Preparation of coating solution> 15.0 g of vinyl chloride-vinyl acetate copolymer resin (Solvine C (registered trademark) manufactured by Nissin Chemical Industry Co., Ltd.) was dissolved as a binder in 85.0 g of cyclohexanone to prepare a binder solution. 16.7 g of this binder solution was added to 21.4 g of tin oxide-containing secondary particle dispersion liquid during stirring to prepare a coating solution precursor. After stirring this coating solution precursor for 5 minutes, 6.9 g of cyclohexanone and propylene glycol monomethyl ether (manufactured by Hayashi Pure Chemical Industries Co., Ltd.) were added. After stirring for 60 minutes, ultrasonic waves were irradiated for 60 seconds using an ultrasonic disperser (Horne type 5281 manufactured by Kaijo Co., Ltd.) and filtered using a stainless steel wire mesh to prepare a coating solution.

[0043] 《Coating》 This coating solution was applied onto a polyester film (Cosmoshine (registered trademark) A4360 manufactured by Toyobo Co., Ltd.) by a bar coater method. The coating solution was dried for 20 minutes under conditions of 25°C and 50 RH% to obtain a film-coated substrate. The surface resistance and optical properties of this film-coated substrate were measured as follows. The measurement results of other examples and comparative examples are also shown in Table 1.

[0044] <Evaluation> (1)Surface resistance The surface resistance of the film was measured using a surface resistance measuring device (Hirester UX MCP-HT800 manufactured by Nitto Seiko Analytech Co., Ltd.).

[0045] (2) Optical properties The haze of the film-coated substrate was measured using a haze meter (HZ-V3 manufactured by Suga Test Instruments Co., Ltd.).

[0046] [Example 2] <Preparation of tin oxide-containing secondary particle dispersion> The tin oxide-containing powder prepared in the same manner as in Example 1 was mixed with 74.5 g of MEK (manufactured by Hayashi Pure Chemical Industries, Ltd.) as an organic solvent used to prepare the dispersant solution, and 2.0 g of PLENACT (registered trademark) KR-9SA (manufactured by Ajinomoto Fine-Techno Co., Ltd., active ingredient 80%) as a dispersant. The mixture was stirred for 10 minutes to prepare a dispersant solution. A suspension was prepared by mixing 76.5 g of the dispersant solution and 45.7 g of the tin oxide-containing powder in a 500 mL glass beaker.

[0047] Next, 230 g of glass beads BZ-06 were added to 122.2 g of the suspension, and tin oxide particles were prepared in the same manner as in Example 1, except that the glass beads were dispersed until the average particle diameter of the tin oxide particles reached 380 nm. The glass beads were separated from the suspension using a stainless steel wire mesh with a mesh size of 44 μm. MEK was added thereto to prepare a tin oxide-containing secondary particle dispersion (solid concentration 35.0 mass%).

[0048] <Preparation of coating solution> 30.0 g of acrylic resin (Kuraray Co., Ltd.'s Kuralyte (registered trademark) LA2270) was dissolved as a binder in 70.0 g of MEK to prepare a binder solution. 13.88 g of this binder solution was added to 27.0 g of the dispersion solution being stirred, and the mixture was stirred for 5 minutes. 3.75 g of silica sol (solvent: MIBK, SiO2 concentration: 37%, average particle size measured by SEM: 140 nm) surface-treated with 3-methacryloxypropyltrimethoxysilane was added as silica particles to the tin oxide-containing secondary particle dispersion to prepare a coating solution precursor. After stirring this coating solution precursor for 5 minutes, 0.15 g of Plysurf (registered trademark) A212C (Dai-ichi Kogyo Seiyaku Co., Ltd.) was added as an additional dispersant. This dispersion solution was stirred for 5 minutes. 5.22 g of the above mixed solvent was added to the dispersion solution. Further, after stirring for 60 minutes, ultrasonic waves were applied for 60 seconds using an ultrasonic disperser (Kaijo Horn type 5281), and the dispersion was filtered using a stainless steel wire mesh to prepare a coating liquid. In the same manner as in Example 1, a coating liquid and a film-coated substrate were obtained, except that the coating liquid was prepared by filtering the dispersion using a stainless steel wire mesh.

[0049] [Example 3] A dispersion liquid, a coating liquid and a film-coated substrate were obtained in the same manner as in Example 1, except that the dispersion was continued until the average particle diameter reached 670 nm.

[0050] [Example 4] A dispersion liquid, a coating liquid and a film-coated substrate were obtained in the same manner as in Example 2, except that the dispersion was continued until the average particle diameter reached 280 nm.

[0051] [Example 5] A dispersion, a coating liquid and a film-coated substrate were obtained in the same manner as in Example 1, except that 5.0 g of dioctyl sulfosuccinate sodium salt was added to 125.2 g of the suspension during dispersion, and dispersion was continued until the average particle size reached 280 nm.

[0052] [Comparative Example 1] During dispersion, dispersion was continued until the average particle size reached 130 nm. Except for this, a dispersion liquid, a coating liquid, and a film-coated substrate were obtained in the same manner as in Example 2.

[0053] [Comparative Example 2] During dispersion, 1.6 g of a phosphate ester-based anionic surfactant, Plysurf A212C, was added as a dispersant to 121.8 g of the suspension, and dispersion was continued until the average particle size reached 230 nm. Except for this, a dispersion liquid, a coating liquid, and a film-coated substrate were obtained in the same manner as in Example 1.

[0054] [Comparative Example 3] During dispersion, 4.8 g of PLENACT TTS was added as a dispersant to 125.0 g of the suspension, and dispersion was continued until the average particle size reached 530 nm. In the same manner as in Example 1, a dispersion liquid, a coating liquid, and a film-coated substrate were obtained.

[0055] [Comparative Example 4] A dispersion liquid, a coating liquid and a film-coated substrate were obtained in the same manner as in Example 2, except that 1.7 g of PLENACT 38S was added as a dispersant to 119.9 g of the suspension during dispersion, and dispersion was continued until the average particle size reached 630 nm.

[0056] [Comparative Example 5] A dispersion, a coating liquid and a film-coated substrate were obtained in the same manner as in Example 2, except that 8.3 g of dioctyl sodium sulfosuccinate was added to 128.5 g of the suspension and dispersion was continued until the average particle size reached 310 nm.

[0057] [Comparative Example 6] An attempt was made to prepare a dispersion in the same manner as in Example 1, except that the dispersant was changed to 1.7 g of methanesulfonic acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.); however, the dispersion thickened and could not be carried on to the subsequent steps.

[0058] [Table 1]

Claims

1. A dispersion liquid containing secondary particles formed by sintering tin oxide-containing particles, a dispersant having a sulfo group or a sulfonyl group, and an organic solvent, The average particle size of the secondary particles is 170 to 700 nm, The dispersant has 6 or more carbon atoms, In the dispersion, the sulfo group or sulfonyl group in the dispersant is 2 1.0 x 10 15 1.0×10 pieces or more 17 The dispersion liquid is characterized in that the number of particles contained is less than one.

2. 2. The dispersion according to claim 1, wherein the crystallite size of the tin oxide-containing particles is 5 to 15 nm.

3. 3. The dispersion according to claim 1, having a solids concentration of 5 to 40%.

4. A coating liquid comprising the dispersion according to claim 1 and a binder.

5. A method for producing a film-coated substrate, comprising forming a film on a substrate by using the coating liquid according to claim 4.

6. A first step of calcining a tin oxide-containing powder precursor to obtain a tin oxide-containing powder; a second step of dispersing the tin oxide-containing powder in a solution containing a dispersant having a sulfo group or a sulfonyl group and an organic solvent to obtain a tin oxide-containing secondary particle dispersion, A method for producing a tin oxide-containing dispersion, comprising adjusting the average particle size of the tin oxide-containing secondary particles to 170 to 700 nm in the second step.

Citation Information

Patent Citations

  • Transparent electrically conductive coating agent for plasticized flexible polyvinyl chloride

    JP1988066267A

  • Treatment of transparent powder having conductivity

    JP1988151619A

  • Composition for forming ultraviolet ray- and heat ray-shielding transparent layer, and transparent layer and use of the same

    JP2008231367A

  • Dispersion for forming heat ray shielding film

    JP2011012112A

  • Composition for forming antimony-doped tin oxide conductive film and antimony-doped tin oxide conductive film

    JP2017054623A

Cited By

  • Hydrogen gas detection device and control program

    JP2026154366A