Light-emitting device
A novel tandem structure for organic EL devices with a negative GSP_slope first layer addresses the issue of atmospheric exposure, ensuring high efficiency and reliability, suitable for high-definition displays.
Patent Information
- Application Number
- JP2024056145
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-15
AI Technical Summary
Organic EL devices are susceptible to deterioration when exposed to atmospheric components like water and oxygen, particularly affecting alkali metals or alkaline earth metals used in electron injection layers, which are essential for tandem structures, leading to reduced efficiency and reliability during photolithography processes.
A light-emitting device with a novel tandem structure is developed, utilizing a first layer with a negative GSP_slope to facilitate electron injection without an N-type CGL, thereby avoiding exposure to atmospheric components and maintaining efficiency and reliability.
The device maintains high efficiency and reliability by suppressing increases in drive voltage and preventing characteristic deterioration, suitable for high-definition display devices.
Smart Images

Figure 2024146902000001_ABST
Abstract
Description
[Technical field]
[0001] One aspect of the invention relates to a light emitting device.
[0002] Note that one embodiment of the present invention is not limited to the above technical field. Examples of the technical field of one embodiment of the present invention include a semiconductor device, a display device, a light-emitting device, a power storage device, a memory device, an electronic device, a lighting device, an input device (e.g., a touch sensor), an input / output device (e.g., a touch panel), a driving method thereof, or a manufacturing method thereof. [Background technology]
[0003] Display devices are being developed for various applications. For example, applications of large display devices include home television devices (also called televisions or television receivers), digital signage, and public information displays (PIDs), while applications of small display devices include smartphones and tablet terminals equipped with touch panels.
[0004] At the same time, display devices are also becoming higher in resolution. Devices that require high-resolution display devices include, for example, devices for virtual reality (VR), augmented reality (AR), substitutional reality (SR), and mixed reality (MR).
[0005] As a display element used in a display device, the development of a light-emitting device (also called a light-emitting element) is being actively promoted. A light-emitting device (also called an EL device or an EL element) utilizing the electroluminescence (hereinafter referred to as EL) phenomenon, particularly an organic EL device mainly using an organic compound, has characteristics such as being easily thin and lightweight, being capable of high-speed response to an input signal, and being capable of being driven by a DC constant voltage power source, and is therefore suitable for a display device.
[0006] In order to obtain a higher-definition light-emitting device using an organic EL device, research is being conducted on patterning the organic layer by photolithography using photoresist, etc., instead of deposition using a metal mask. By using photolithography, a high-definition display device with an EL layer spacing of several μm can be obtained (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Special Publication No. 2018-521459 [Patent Document 2] International Publication No. 2021 / 045178 Summary of the Invention [Problem to be solved by the invention]
[0008] It has long been known that the initial characteristics and reliability of the EL layer of an organic EL device are affected when it is exposed to atmospheric components such as water and oxygen, and so it has been common knowledge that it should be handled in a near-vacuum atmosphere. In particular, alkali metals or alkaline earth metals, or compounds of these, are used in the electron injection layer or the charge generation layer in the intermediate layer of a light-emitting device with a tandem structure, but these metals and compounds are highly reactive with water or oxygen, and when the surface of the EL layer is exposed to the atmosphere, they deteriorate in an instant and no longer function as an electron injection layer or charge generation layer.
[0009] However, in the process of processing by photolithography as described above, it is unavoidable to expose the surface of the EL layer to the air.
[0010] Here, 1,1'-pyridine-2,6-diyl-bis(1,3,4,6,7,8-hexahydro-2H-pyrimido[1,2-a]pyrimidine) (abbreviation: hpp2Py) is known as an organic compound that can be used in the electron injection layer instead of the above-mentioned alkali metals or alkaline earth metals or their compounds. Unlike alkali metals or alkaline earth metals or their compounds, hpp2Py is not easily deteriorated even when exposed to the atmosphere, so even if it is used in a light-emitting device that has been processed by a photolithography method that involves exposure to the atmosphere during the process, the light-emitting device is not easily deteriorated.
[0011] However, because electron injection is induced in hpp2Py upon contact with metals such as aluminum, it has been difficult to use it as an intermediate layer in a light-emitting device with a tandem structure due to concerns about metal contamination and light transparency.
[0012] Therefore, an object of one embodiment of the present invention is to provide a light-emitting device having a novel tandem structure. Alternatively, an object of another embodiment of the present invention is to provide a light-emitting device having a novel tandem structure with good efficiency. Alternatively, an object of one embodiment of the present invention is to provide a light-emitting device having a novel tandem structure with good reliability. Alternatively, an object of another embodiment of the present invention is to provide a light-emitting device having a novel tandem structure with good efficiency and reliability.
[0013] Alternatively, one embodiment of the present invention has an object to provide a light-emitting device having a novel tandem structure manufactured through a photolithography process. Alternatively, another embodiment of the present invention has an object to provide a light-emitting device having a novel tandem structure manufactured through a photolithography process and having good efficiency. Alternatively, one embodiment of the present invention has an object to provide a light-emitting device having a novel tandem structure manufactured through a photolithography process and having good reliability. Alternatively, another embodiment of the present invention has an object to provide a light-emitting device having a novel tandem structure manufactured through a photolithography process and having good light-emitting efficiency and reliability.
[0014] Alternatively, an object of one embodiment of the present invention is to provide a light-emitting device having a novel tandem structure that can be used in a high-definition display device. Alternatively, an object of another embodiment of the present invention is to provide a light-emitting device having a novel tandem structure that can be used in a high-definition display device and has good efficiency. Alternatively, an object of one embodiment of the present invention is to provide a light-emitting device having a novel tandem structure that can be used in a high-definition display device and has good reliability. Alternatively, an object of another embodiment of the present invention is to provide a light-emitting device having a novel tandem structure that can be used in a high-definition display device and has good emission efficiency and reliability.
[0015] Another object of another embodiment of the present invention is to provide a highly reliable display device. Another object of another embodiment of the present invention is to provide a high-definition display device. Another object of another embodiment of the present invention is to provide a high-definition and highly reliable display device.
[0016] Alternatively, it is an object of the present invention to provide a novel organic compound, a novel light-emitting device, a novel display device, a novel display module, and a novel electronic device.
[0017] Note that the description of these problems does not preclude the existence of other problems. One embodiment of the present invention does not necessarily have to solve all of these problems. Problems other than these can be extracted from the description of the specification, drawings, and claims. [Means for solving the problem]
[0018] One embodiment of the present invention is a light-emitting device having a first electrode, a second electrode opposite to the first electrode, a first light-emitting layer and a second light-emitting layer between the first electrode and the second electrode, and a first layer between the first light-emitting layer and the second light-emitting layer, wherein the GSP_slope (mV / nm) of the first layer has a positive / negative sign opposite to that of the GSP_slope (mV / nm) of the first light-emitting layer.
[0019] Alternatively, another embodiment of the present invention is a light-emitting device having a first electrode formed on a substrate, a second electrode opposing the first electrode, a first light-emitting layer and a second light-emitting layer between the first electrode and the second electrode, and a first layer between the first light-emitting layer and the second light-emitting layer, wherein the GSP_slope (mV / nm) of the first layer exhibits a negative value.
[0020] Alternatively, another embodiment of the present invention is a light-emitting device having a first electrode, a second electrode opposite to the first electrode, a first light-emitting layer and a second light-emitting layer between the first electrode and the second electrode, and an electron transport layer and a first layer between the first light-emitting layer and the second light-emitting layer, wherein the GSP_slope (mV / nm) of the first layer has an opposite positive / negative sign to that of the GSP_slope (mV / nm) of the electron transport layer.
[0021] Alternatively, another embodiment of the present invention is a light-emitting device having a first electrode formed on a substrate, a second electrode opposing the first electrode, a first light-emitting layer and a second light-emitting layer between the first electrode and the second electrode, and an electron transport layer and a first layer between the first light-emitting layer and the second light-emitting layer, wherein the GSP_slope (mV / nm) of the electron transport layer is positive and the GSP_slope (mV / nm) of the first layer is negative.
[0022] Alternatively, another embodiment of the present invention is a light-emitting device having a first electrode formed on a substrate, a second electrode opposing the first electrode, and a first light-emitting layer, an electron transport layer, an intermediate layer, and a second light-emitting layer between the first and second electrodes, in this order from the first electrode side, the intermediate layer having the first layer and the second layer in this order from the first electrode side, the electron transport layer and the first layer being in contact, and the GSP_slope (mV / nm) of the electron transport layer being positive and the GSP_slope (mV / nm) of the first layer being negative.
[0023] Another embodiment of the present invention is a light-emitting device having the above structure, in which the second layer is a layer that generates charges.
[0024] Another embodiment of the present invention is a light-emitting device having the above structure, in which the second layer contains an organic compound having a hole-transport property and a substance that exhibits an acceptor property for the organic compound having a hole-transport property.
[0025] Another embodiment of the present invention is a light-emitting device having the above structure, in which the substance that exhibits an acceptor property to the organic compound having a hole-transport property, which is included in the second layer, is an organic compound.
[0026] Another embodiment of the present invention is a light-emitting device having the above structure, in which the first layer has a function of blocking holes.
[0027] Another embodiment of the present invention is a light-emitting device having the above structure, in which the hole mobility of the first layer is lower than that of the electron-transport layer.
[0028] Alternatively, in the above structure, another embodiment of the present invention is a semiconductor device in which the hole mobility of the first layer is 1×10 -8 cm 2 / Vs or less.
[0029] Alternatively, in the above structure, another embodiment of the present invention is a semiconductor device in which the electron mobility at a square root of an electric field strength [V / cm] of the first layer is 1×10 -8 cm 2 / Vs or more.
[0030] Another embodiment of the present invention is a light-emitting device having the above structure, in which the first layer includes a first substance having any one of a pyrrolidine skeleton, a piperidine skeleton, and a hexahydropyrimidopyrimidine skeleton.
[0031] Another embodiment of the present invention is a light-emitting device having the above structure, in which the first layer includes a first substance and a second substance, the first substance being an organic compound having any one of a pyrrolidine skeleton, a piperidine skeleton, and a hexahydropyrimidopyrimidine skeleton, and the second substance being an organic compound having electron-transporting properties.
[0032] Another embodiment of the present invention is a light-emitting device having the above structure, in which the first substance is an organic compound having a 1,3,4,6,7,8-hexahydro-2H-pyrimido[1,2-a]pyrimidine skeleton.
[0033] Another embodiment of the present invention is a light-emitting device having the above structure, in which the GSP_slope (mV / nm) of the electron-transport layer and the GSP_slope (mV / nm) of the first layer differ by 20 (mV / nm) or more.
[0034] Alternatively, in the above structure, another embodiment of the present invention is a method for manufacturing a semiconductor device having a spin density of 1×10 17 spins / cm 3 A light emitting device comprising:
[0035] Another embodiment of the present invention is a light-emitting device having the above structure, in which the first electrode is electrically connected to the transistor.
[0036] Another embodiment of the present invention is a display module including the above-described light-emitting device and at least one of a connector and an integrated circuit.
[0037] Another embodiment of the present invention is an electronic device including any of the above light-emitting devices and at least one of a housing, a battery, a camera, a speaker, and a microphone.
[0038] In the above, GSP_slope (mV / nm) is a parameter expressed as V / d when the potential of the film surface is V (mV) and the film thickness is d (nm). Effect of the Invention
[0039] According to one embodiment of the present invention, a light-emitting device having a novel tandem structure can be provided. According to another embodiment of the present invention, a light-emitting device having a novel tandem structure with good efficiency can be provided. According to one embodiment of the present invention, a light-emitting device having a novel tandem structure with good reliability can be provided. According to another embodiment of the present invention, a light-emitting device having a novel tandem structure with good reliability and efficiency can be provided.
[0040] Alternatively, according to one embodiment of the present invention, a light-emitting device having a novel tandem structure manufactured through a photolithography process can be provided. Alternatively, according to another embodiment of the present invention, a light-emitting device having a novel tandem structure manufactured through a photolithography process and having good efficiency can be provided. Alternatively, according to one embodiment of the present invention, a light-emitting device having a novel tandem structure manufactured through a photolithography process and having good reliability can be provided. Alternatively, according to another embodiment of the present invention, a light-emitting device having a novel tandem structure manufactured through a photolithography process and having good reliability and light-emitting efficiency can be provided.
[0041] According to one embodiment of the present invention, a light-emitting device having a novel tandem structure that can be used in a high-definition display device can be provided. According to another embodiment of the present invention, a light-emitting device having a novel tandem structure that can be used in a high-definition display device and has good efficiency can be provided. According to one embodiment of the present invention, a light-emitting device having a novel tandem structure that can be used in a high-definition display device and has good reliability can be provided. According to another embodiment of the present invention, a light-emitting device having a novel tandem structure that can be used in a high-definition display device and has good efficiency and reliability can be provided.
[0042] According to one embodiment of the present invention, a display device with high resolution and high emission efficiency can be provided. According to one embodiment of the present invention, a display device with high resolution and good display performance can be provided. According to one embodiment of the present invention, a display device with good display quality and good display performance can be provided. According to one embodiment of the present invention, a display device with high resolution, high emission efficiency, and high reliability can be provided. According to one embodiment of the present invention, a display device with high resolution and good display performance and reliability can be provided. According to one embodiment of the present invention, a display device with good display quality, high display performance, and high reliability can be provided.
[0043] Alternatively, a novel display device, a novel display module, and a novel electronic device can be provided.
[0044] Note that the description of these effects does not preclude the existence of other effects. One embodiment of the present invention does not necessarily have all of these effects. Effects other than these can be extracted from the description in the specification, drawings, and claims. [Brief description of the drawings]
[0045] [Figure 1] 1(A) and 1(B) are diagrams illustrating a light-emitting device. [Diagram 2] 2(A) and 2(B) are diagrams showing a measuring device. [Diagram 3] FIG. 3 is a diagram showing the capacitance-voltage characteristics of element 10. As shown in FIG. [Figure 4] FIG. 4 is a diagram showing the capacitance-voltage characteristics of element 11. [Diagram 5] FIG. 5 shows the results of measurements performed using a measuring device. [Figure 6] FIG. 6 is a diagram illustrating a light emitting device. [Figure 7] FIG. 7 is a diagram illustrating a light emitting device. [Figure 8] 8(A) and 8(B) are a top view and a cross-sectional view of the display device. [Figure 9] 9A to 9E are cross-sectional views showing an example of a method for manufacturing a display device. [Figure 10] 10A to 10D are cross-sectional views showing an example of a method for manufacturing a display device. [Figure 11] 11A to 11D are cross-sectional views showing an example of a method for manufacturing a display device. [Figure 12] 12A to 12C are cross-sectional views showing an example of a method for manufacturing a display device. [Figure 13] 13A to 13C are cross-sectional views showing an example of a method for manufacturing a display device. [Figure 14] 14A to 14C are cross-sectional views showing an example of a method for manufacturing a display device. [Figure 15] 15(A) and 15(B) are perspective views showing configuration examples of a display module. [Figure 16] 16(A) and 16(B) are cross-sectional views showing configuration examples of a display device. [Figure 17] FIG. 17 is a perspective view showing a configuration example of a display device. [Figure 18] FIG. 18 is a cross-sectional view showing a configuration example of a display device. [Figure 19]FIG. 19 is a cross-sectional view showing a configuration example of a display device. [Figure 20] FIG. 20 is a cross-sectional view showing a configuration example of a display device. [Figure 21] 21A to 21D are diagrams illustrating examples of electronic devices. [Figure 22] 22A to 22F are diagrams showing examples of electronic devices. [Figure 23] 23A to 23G are diagrams showing examples of electronic devices. [Figure 24] FIG. 24 is a graph showing the luminance-current density characteristics of the light-emitting device 1. As shown in FIG. [Diagram 25] FIG. 25 is a diagram showing the luminance-voltage characteristics of the light-emitting device 1. As shown in FIG. [Figure 26] FIG. 26 is a graph showing the current efficiency-luminance characteristics of the light-emitting device 1. As shown in FIG. [Figure 27] FIG. 27 is a graph showing the current density-voltage characteristics of the light-emitting device 1. As shown in FIG. [Figure 28] FIG. 28 is a graph showing the electroluminescence spectrum of the light-emitting device 1. As shown in FIG. [Figure 29] FIG. 29 is a graph showing the change in luminance of the light-emitting device 1 with respect to the driving time when the device is driven at a constant current density of 50 mA / cm 2 . [Diagram 30] FIG. 30 is a diagram showing the capacitance-voltage characteristics of the measurement device. [Diagram 31] FIG. 31 is a graph showing the luminance-current density characteristics of the light-emitting device 2. As shown in FIG. [Diagram 32] FIG. 32 is a graph showing the current efficiency-luminance characteristics of the light-emitting device 2. As shown in FIG. [Diagram 33] FIG. 33 is a diagram showing the luminance-voltage characteristics of the light-emitting device 2. As shown in FIG. [Diagram 34] FIG. 34 is a graph showing the current density-voltage characteristics of the light-emitting device 2. As shown in FIG. [Diagram 35] FIG. 35 is a graph showing the electroluminescence spectrum of the light-emitting device 2. As shown in FIG. [Diagram 36]FIG. 36 is a graph showing the change in luminance of the light-emitting device 2 with respect to the driving time when the device is driven at a constant current density of 50 mA / cm 2 . [Figure 37] 37(A) and 37(B) are diagrams showing the capacitance-voltage characteristics of the measurement device L21 and the measurement device L22. [Figure 38] FIG. 38 is a diagram showing the capacitance-voltage characteristics of the measuring device 3. As shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0046] The embodiments will be described in detail with reference to the drawings. However, the present invention is not limited to the following description, and it will be easily understood by those skilled in the art that the modes and details of the present invention can be modified in various ways without departing from the spirit and scope of the present invention. Therefore, the present invention should not be interpreted as being limited to the description of the embodiments shown below.
[0047] In this specification, etc., a device fabricated using a metal mask or an FMM (fine metal mask, high-definition metal mask) may be referred to as a device with an MM (metal mask) structure. In addition, in this specification, etc., a device fabricated without using a metal mask or an FMM may be referred to as a device with an MML (metal maskless) structure.
[0048] (Embodiment 1) A tandem-type organic EL device has multiple light-emitting units, each of which has an emitting layer between electrodes, and an intermediate layer sandwiched between the light-emitting units. This intermediate layer includes a charge generation layer (CGL).
[0049] A CGL is a layer in which electrons and holes are generated by charge separation when a voltage is applied. Generally, a layer in which a material with hole transport properties and a material with acceptor properties for the hole transport properties are laminated or mixed (P-type CGL), and a layer in which a material with electron transport properties and a material with donor properties for the electron transport properties are laminated or mixed (N-type CGL) are used as a CGL.
[0050] In addition, it is preferable that the intermediate layer has both a P-type CGL and an N-type CGL, with the P-type CGL on the cathode side and the N-type CGL on the anode side, because this makes it easier to inject holes or electrons into each light-emitting unit and reduces the driving voltage. This is because holes generated in the P-type CGL are injected into the light-emitting unit in contact with the cathode side surface of the intermediate layer via the material having hole transport properties of the P-type CGL, and electrons generated in the N-type CGL are injected into the light-emitting unit in contact with the anode side surface of the intermediate layer via the material having electron transport properties of the N-type CGL, thereby lowering the carrier injection barrier.
[0051] The N-type CGL may be a single film of a material having donor properties. In this case, the material having donor properties separates charges between the material having electron transport properties in the light-emitting unit on the anode side, so that electrons can be considered to be injected into the light-emitting unit at the time of charge separation. Similarly, the P-type CGL may be a single film of a material having acceptor properties. In this case, the material having acceptor properties separates charges between the material having hole transport properties in the light-emitting unit on the cathode side, so that holes can be considered to be injected into the light-emitting unit at the time of charge separation.
[0052] Here, as one of the methods for forming an organic semiconductor film into a predetermined shape, a vacuum deposition method using a metal mask (mask deposition) is widely used. However, in recent years, as density and definition are becoming higher, mask deposition is approaching its limit for further finer definition due to various reasons such as problems with alignment accuracy and problems with the placement distance to the substrate. Therefore, it is expected that organic semiconductor devices with more dense patterns can be realized by processing the shape of the organic semiconductor film using a photolithography method. Furthermore, since photolithography is easier to make larger areas than mask deposition, research on processing organic semiconductor films using photolithography is being conducted.
[0053] However, in the process of processing by the above-mentioned photolithography method, it is necessary to expose the surface of the organic compound layer (specifically, the EL layer or the like) to be processed to the atmosphere.
[0054] It has long been known that the initial characteristics or reliability of the EL layer in an organic EL device can be affected when exposed to atmospheric components such as water or oxygen, and so it has been common knowledge that such devices should be handled in a near-vacuum atmosphere.
[0055] In particular, alkali metals or alkaline earth metals, or compounds thereof (hereinafter also referred to as Li compounds, etc.) are often used in the electron injection layer of light-emitting devices and in the N-type CGL in the intermediate layer used in light-emitting devices with a tandem structure, and therefore are significantly affected when exposed to atmospheric components such as water and oxygen. These Li compounds, etc. are highly reactive with water or oxygen, and deteriorate in an instant not only when they come into direct contact with the air, but also when the surface of the EL layer containing them is exposed to the air even if not directly, and they no longer function as an electron injection layer or N-type CGL.
[0056] As mentioned above, in the process of processing by photolithography, it is necessary to expose the surface of the EL layer to the air. For this reason, the electron injection properties of the electron injection layer using Li compounds and the N-type CGL are greatly reduced by the photolithography process. Since the electron injection layer can be formed after processing by photolithography, this deterioration in characteristics can be avoided, but in the case of a tandem light-emitting device, if the light-emitting layer located on the cathode side of the intermediate layer is processed by photolithography, the intermediate layer will inevitably be exposed to processing. For this reason, it has been difficult to process a tandem light-emitting device using an intermediate layer using Li compounds (i.e., an N-type CGL) by photolithography.
[0057] Since both N-type and P-type CGLs generate charges, it is possible to use an intermediate layer in which only the P-type CGL generates charges, without providing an N-type CGL, which is likely to deteriorate during the photolithography process. In this case, however, the electrons generated in the P-type CGL are difficult to inject into the light-emitting unit that contacts the anode side surface of the intermediate layer, resulting in a significant increase in driving voltage. This is because there is a large difference between the Lowest Unoccupied Molecular Orbital (LUMO) level of the acceptor material in the P-type CGL and the LUMO level of the electron-transporting material that constitutes the electron-transporting layer in the light-emitting unit on the anode side.
[0058] In this way, photolithographic processing of tandem light-emitting devices poses a dilemma: if an N-type CGL is used, the N-type CGL deteriorates during photolithographic processing, resulting in an increase in driving voltage; however, if an N-type CGL is not used for the intermediate layer, the driving voltage increases due to the difference in LUMO levels.
[0059] Here, the inventors have found that in the case of a so-called forward-stacked tandem light-emitting device in which the anode is formed first, by forming a layer with a negative gradient of the giant surface potential (GSP) instead of the N-type CGL in the intermediate layer, it is possible to obtain a tandem light-emitting device in which an increase in driving voltage is suppressed without using an N-type CGL.
[0060] GSP is a phenomenon that occurs due to spontaneous orientation polarization (SOP), which occurs when the orientation of the permanent dipole moment of a deposited film is biased in the film thickness direction.
[0061] The surface potential of a vapor-deposited film that exhibits such GSP changes at a constant rate with increasing film thickness without saturating. For example, the surface potential of a vapor-deposited film of tris(8-quinolinolato)aluminum (Alq3) with a film thickness of 560 nm is approximately 28 V. The electric field strength is 5×10 5 This is approximately the same as the electric field strength during operation of a typical organic thin-film device.
[0062] The slope of GSP (GSP_slope) is a parameter expressed as V / d (mV / nm) for a film whose GSP changes in proportion to the film thickness, where the potential of the film surface is V (mV) and the film thickness is d (nm). Note that if the surface potential increases with an increase in film thickness, the GSP_slope is positive, and if the surface potential decreases with an increase in film thickness, the GSP_slope is negative, and the above-mentioned Alq3 can be said to be a material with a positive GSP_slope. Note that in a layer with a negative GSP_slope (hereinafter also referred to as a negative layer), the substrate side has a high potential, and in a layer with a positive GSP_slope (hereinafter also referred to as a positive layer), the substrate side has a low potential.
[0063] As mentioned above, this GSP is a phenomenon caused by the SOP, which occurs when the orientation of the permanent dipole moment is biased in the film thickness direction. In other words, in a layer with a negative GSP_slope, a positive polarization charge is induced on the deposition start side (substrate side) and a negative polarization charge is induced on the deposition end side (second electrode side), and similarly, in a layer with a positive GSP_slope, a negative polarization charge is induced on the deposition start side (substrate side) and a positive polarization charge is induced on the deposition end side (second electrode side), and these are the origins of GSP.
[0064] In an organic semiconductor device having a laminated structure, the voltage for injecting electrons or holes into the EL layer is also significantly affected by the polarization charge. In one embodiment of the present invention, the polarization charge and the interface charge in the laminated film resulting from the polarization charge are utilized to reduce the driving voltage of a tandem light-emitting device.
[0065] Generally, most organic compounds have a positive GSP_slope, so for example, when a first layer is formed on a second layer, the signs of the GSP_slope of the first layer and the second layer are the same positive sign. In this case, the polarization charge in the first layer is offset by the polarization charge in the second layer that is the base of the first layer, and only the remaining charge becomes the interface charge (fixed charge). Therefore, the density of the interface charge that exists at the interface between the two different layers is lower than the density of the polarization charge.
[0066] On the other hand, in a light-emitting device according to one embodiment of the present invention, as shown in FIG. 1, a first layer 21 having a negative GSP_slope is formed instead of an N-type CGL. A general layer having a positive GSP_slope can be used as the second layer 22 serving as the base. As described above, in the first layer 21 having a negative GSP_slope, a positive polarization charge is induced near the interface of the first layer 21 on the substrate 1000 side, and a negative polarization charge is induced near the interface on the opposite side. In addition, in the second layer 22 having a positive GSP_slope, a negative polarization charge is induced near the interface of the substrate 1000 side, and a positive polarization charge is induced near the interface on the opposite side, so that a positive polarization charge appears at the interface of the second layer 22 on the first layer 21 side.
[0067] Therefore, in the light-emitting device according to one embodiment of the present invention, the polarization charges in the vicinity of the interface of the first layer 21 on the substrate 1000 side are not cancelled out, and remain as they are as the interface charge 50. Furthermore, the positive polarization charges in the vicinity of the interface of the second layer 22 on the first layer 21 side also become the interface charge 50. That is, when the first layer 21 having a negative GSP_slope is formed instead of the N-type CGL, positive fixed charges are present at a high charge density in the vicinity of the interface between the first layer 21 and the second layer 22 that serves as the base thereof.
[0068] In the light-emitting device according to one embodiment of the present invention, the high density positive interfacial charge 50 near the interface between the first layer 21 and the second layer 22 makes it possible to easily inject electrons generated in the P-type CGL 20 into the first layer 21. As a result, even without using an N-type CGL in the intermediate layer 513, it becomes possible to inject electrons generated in the P-type CGL 20 into the first light-emitting unit 501 on the anode 101 side without a significant increase in drive voltage, and a tandem light-emitting device in which an increase in drive voltage is suppressed even without using an N-type CGL can be obtained.
[0069] In the light-emitting device according to one embodiment of the present invention, since an N-type CGL is not used for the intermediate layer 513, Li compounds which are prone to degradation are not used. Therefore, even after photolithography, degradation of characteristics such as an increase in driving voltage does not occur, and it is possible to obtain a tandem light-emitting device that maintains good characteristics.
[0070] As described above, a tandem light-emitting device in which the first layer 21 having a negative GSP_slope is formed instead of the N-type CGL can be a tandem light-emitting device that suppresses deterioration of characteristics such as an increase in driving voltage even after photolithography and maintains good characteristics. In addition, in Fig. 1, 102 is a cathode, 502 is a second light-emitting unit, 113_1 is a light-emitting layer of the first light-emitting unit 501, 113_2 is a light-emitting layer of the second light-emitting unit 502, and 114_1 is an electron transport layer of the first light-emitting unit 501.
[0071] Here, a method for determining the GSP_slope of an organic compound will be described.
[0072] As mentioned above, GSP is a phenomenon caused by the SOP, which occurs when the orientation of the permanent dipole moment of the evaporated film is biased in the film thickness direction. The amount of change in GSP that changes in proportion to the film thickness is called GSP_slope (mV / nm). It is known that it appears as the slope when the surface potential of the evaporated film measured by Kelvin probe measurement is plotted in the film thickness direction, but when performing measurements using this method, the effects of the underlying film and the measurement environment must be taken into consideration. On the other hand, when two films with different SOPs are stacked, the interfacial charge density (mC / m 2 ) and the GSP_slope of one film, the GSP_slope of the other film can be estimated. The interface charge density can be obtained by performing CV measurements (IS measurements) using a device structure that accumulates charges in one of the two different laminated films.
[0073] When films with different SOPs (thin film 1 and thin film 2, where thin film 1 is located on the anode side and thin film 2 is located on the cathode side) are stacked and a current is passed through them, the following formula holds if the carriers are electrons.
[0074]
number
[0075]
number
[0076] In formula (1), σ if_e is the interfacial charge density, V i is the electron injection voltage, V bi is the threshold voltage, d1 is the thickness of thin film 1, and ε1 is the dielectric constant of thin film 1. V i , V bi can be estimated from the capacitance-voltage characteristics of the device. The dielectric constant is also expressed by the ordinary refractive index n o In this way, the V estimated from the capacitance-voltage characteristic can be calculated as i , Vbi Using the dielectric constant ε1 of thin film 1 calculated from the refractive index and the thickness d1 of thin film 1, the interface charge density σ if_e can be sought.
[0077] Next, in formula (2), P1 and P2 are the SOPs of thin film 1 and thin film 2, ε2 is the dielectric constant of thin film 2, and d2 is the thickness of thin film 2. Here, from the above formula (1), the interface charge density σ if_e Therefore, by using a material with a known GSP_slope as thin film 1, the GSP_slope of thin film 2 can be estimated.
[0078] Therefore, Alq3, which has a known GSP_slope of (48 (mV / nm)), was used as thin film 1, and elements 10 and 11 were fabricated as measurement elements. An example in which the GSP_slope of NBPhen was obtained for element 10 and that of mPPhen2P was obtained for element 11 is shown below.
[0079] The device structures of element 10 and element 11 are shown in the table below and in FIG. 2(A). The anode 701 was formed on a substrate 700, and the hole injection layer 702, the first electron transport layer 703, the second electron transport layer 704, the electron injection layer 705, and the cathode 706 were formed by vacuum deposition in this order from the anode 701 (substrate 700) side. When elements 10 and 11 were formed, the substrate temperature was room temperature, the film formation rate was 0.2 nm / s to 0.4 nm / s, and deposition was continued without stopping while each layer was formed. In elements 10 and 11, the first electron transport layer 703 corresponds to thin film 1, and the second electron transport layer 704 corresponds to thin film 2.
[0080] The capacitance-voltage characteristics of the elements 10 and 11 are shown in FIG. 3 and FIG.
[0081] [Table 1]
[0082] Table 2 shows the ordinary refractive index n o, Electron injection voltage V of element 10 (NBPhen) and element 11 (mPPhen2P) obtained from Figs. i , threshold voltage V bi , the interface charge density σ calculated from equation (1) if_e ,GSP_slope calculated from equation (2) is shown.
[0083] [Table 2]
[0084] In this way, the GSP_slope can be estimated by fabricating a device in which Alq3, whose GSP_slope is known, and an organic compound whose GSP_slope is to be determined are layered, and measuring the capacitance-voltage characteristics.
[0085] In the above description, a method for calculating the GSP_slope of an organic compound used in an electron transport layer in which the carrier is an electron has been described. However, when the carrier is a hole, the GSP_slope of the organic compound can be calculated in the same manner using the following formulas (3) and (4) by using a measuring element as shown in FIG. 2(B). In the measuring element shown in FIG. 2(B), an anode 801 is formed on a substrate 800, and a hole injection layer 802, a first hole transport layer 803, a second hole transport layer 804, an electron injection layer 805, and a cathode 806 are formed by vacuum deposition in this order from the anode 801 (substrate 800) side. In the following formulas (3) and (4), σ if_h is the interfacial charge density.
[0086]
number
[0087]
number
[0088] The "GSP_slope of a layer" can be calculated as the GSP_slope of the film of the material that constitutes the layer. In addition, if thin film 1 or thin film 2 contains multiple organic compounds, the GSP_slope of the organic compound that is primarily contained (e.g., the one that is contained most abundantly) can be considered as the "GSP_slope of the layer." Alternatively, if thin film 1 or thin film 2 contains multiple organic compounds, the GSP_slope and content of each organic compound can be calculated, and the weighted average (GSP_slope_ave) can be defined as the GSP_slope of the organic compounds that constitute the layer.
[0089] In this manner, GSP_slope can be calculated.
[0090] The materials that form the evaporated film with a negative GSP slope are tris(7-propyl-8-hydroxyquinolinato)aluminum(III) (abbreviation: Al(7-Prq)3), tris(2-phenylpyridinato-N,C 2’ ) Iridium (III) (abbreviation: [Ir(ppy)3]), 2,2-bis[4-(4,6-diphenyl-1,3,5-triazin-2-yl)phenyl]hexafluoropropane (abbreviation: 6F-2TRZ), 2,2-bis[(4-diphenylamino)phenyl]hexafluoropropane (abbreviation: 6F-2TPA), 2,2-bis[9H-carbazole-9-(4-phenyl)]hexafluoropropane (abbreviation: 6F-2Cz), 1-(9,9'-spirobi[9H-fluoren]-2-yl)-1,3,4,6,7,8-hexahydro-2H-pyrimido[1,2-a]pyrimidine (abbreviation: 2hppSF), etc. can be mentioned. The first layer preferably contains the above-mentioned substance as the first substance.
[0091] The first layer may be a layer in which the first substance is mixed with another substance.
[0092] In one embodiment of the present invention, when the hole mobility of the first layer having a negative GSP_slope is lower than that of the second layer serving as the underlayer, the hole mobility of the first layer at a square root of the electric field intensity [V / cm] of 600 is preferably 1×10 -8 cm 2 / Vs or less, and more preferably, when the first layer has a hole-blocking function, holes flowing from the anode are accumulated in the vicinity of the interface between the first layer and the second layer, which makes it easier to inject electrons from the P-type CGL into the first layer.
[0093] In this case, the first layer can reduce hole mobility or block holes by including a highly basic material with an acid dissociation constant of pKa8 or more. Therefore, it is preferable that the first layer includes a highly basic material with an acid dissociation constant of pKa8 or more. That is, it is preferable that the first layer includes a first substance and a highly basic material with an acid dissociation constant of pKa8 or more. In addition, when the GSP_slope of the evaporated film of a highly basic material with an acid dissociation constant of pKa8 or more is negative, the highly basic material with an acid dissociation constant of pKa8 or more can be said to be the first substance, and therefore, by including the highly basic material with an acid dissociation constant of pKa8 or more, the first layer can be regarded as including both the first substance and the highly basic material with an acid dissociation constant of pKa8 or more.
[0094] By including a highly basic material with an acid dissociation constant pKa of 8 or higher in the first layer, the first layer can block holes and efficiently accumulate holes near the interface with the second layer, resulting in a tandem-type light-emitting device with an even lower driving voltage.
[0095] The reason why a material with a large acid dissociation constant pKa blocks holes is because the material has a large dipole moment. This dipole moment interacts with holes, allowing the first layer containing a material with a large acid dissociation constant pKa to block holes.
[0096] Another reason why highly basic materials with a large acid dissociation constant pKa are highly nucleophilic is that they can greatly reduce the hole transport property of the first layer. Highly nucleophilic materials may react with molecules that have received holes and become cation radicals to generate new molecules or intermediate states. This reaction may consume holes, greatly reducing the hole transport property of the first layer.
[0097] The highly basic material having an acid dissociation constant pKa of 8 or more is preferably an organic compound having a basic skeleton, and the acid dissociation constant pKa of the basic skeleton is preferably an organic compound having an acid dissociation constant pKa of 10 or more, and more preferably an organic compound having an acid dissociation constant pKa of 12 or more.
[0098] For the acid dissociation constant pKa of the basic skeleton, the value of an organic compound in which a part of the skeleton is substituted with hydrogen can be used. In addition, the acid dissociation constant pKa of the basic skeleton can be used as an indicator of the acidity of an organic compound having a basic skeleton. In addition, for an organic compound having a plurality of basic skeletons, the acid dissociation constant pKa of the basic skeleton having the highest acid dissociation constant pKa can be used as an indicator of the acidity of the organic compound. It is preferable to use a value measured using water as a solvent for the acid dissociation constant pKa.
[0099] Alternatively, the acid dissociation constant pKa of an organic compound may be determined by the following calculation.
[0100] First, the initial molecular structure of each molecule serving as a calculation model is set to the most stable structure (singlet ground state) obtained from first-principles calculations.
[0101] For the above first-principles calculation, Jaguar, a quantum chemistry calculation software made by Schrodinger, is used, and the most stable structure in the singlet ground state is calculated using density functional theory (DFT). 6-31G** is used as the basis function, and B3LYP-D3 is used as the functional. For the structure to be subjected to the quantum chemistry calculation, conformational analysis is performed using Schrodinger's Maestro GUI with mixed torsional / low-mode sampling, and sampling is performed.
[0102] In the pKa calculation, one or more atoms of each molecule are designated as basic sites, and a Macro Model is used to search for the stable structure of the protonated molecule in water, and a conformational search is performed using the OPLS2005 force field, and the lowest energy conformer is used. Using the Jaguar pKa calculation module, the structure is optimized with B3LYP / 6-31G*, and then a single-point calculation is performed with cc-pVTZ(+), and the pKa value can be calculated using empirical corrections for functional groups. For molecules with one or more atoms designated as basic sites, the largest value among the results obtained is used as the pKa value.
[0103] As the highly basic material, an organic compound having a pyrrolidine skeleton, a piperidine skeleton, or a hexahydropyrimidopyrimidine skeleton is preferable. Also, an organic compound having a guanidine skeleton is preferable. Specifically, examples of the organic compound having a basic skeleton represented by the following structural formulas (120) to (123) can be given.
[0104] [ka]
[0105] The organic compound having an acid dissociation constant pKa of 8 or more is preferably an organic compound having a bicyclo ring structure having two or more nitrogen atoms in the ring and a heteroaromatic hydrocarbon ring having 2 to 30 carbon atoms in the ring or an aromatic hydrocarbon ring having 6 to 30 carbon atoms in the ring, more preferably an organic compound having a 1,3,4,6,7,8-hexahydro-2H-pyrimido[1,2-a]pyrimidine skeleton and a heteroaromatic hydrocarbon ring having 2 to 30 carbon atoms in the ring or an aromatic hydrocarbon ring having 6 to 30 carbon atoms in the ring. Note that an organic compound having a bicyclo ring structure having two or more nitrogen atoms in the ring and a heteroaromatic hydrocarbon ring having 2 to 30 carbon atoms in the ring, more preferably an organic compound having a 1,3,4,6,7,8-hexahydro-2H-pyrimido[1,2-a]pyrimidine skeleton and a heteroaromatic hydrocarbon ring having 2 to 30 carbon atoms in the ring, is more preferably an organic compound having a 1,3,4,6,7,8-hexahydro-2H-pyrimido[1,2-a]pyrimidine skeleton and a heteroaromatic hydrocarbon ring having 2 to 30 carbon atoms in the ring.
[0106] More specifically, the organic compound is preferably represented by the following general formula (G1).
[0107] [ka]
[0108] In the organic compound represented by the general formula (G1), X is a group represented by the following general formula (G1-1), and Y is a group represented by the following general formula (G1-2). 1 and R 2 each independently represents hydrogen or deuterium, h represents an integer of 1 to 6, and Ar represents a substituted or unsubstituted heteroaromatic hydrocarbon ring having 2 to 30 carbon atoms constituting a ring, or a substituted or unsubstituted aromatic hydrocarbon ring having 6 to 30 carbon atoms constituting a ring. Note that Ar is preferably a substituted or unsubstituted heteroaromatic hydrocarbon ring having 2 to 30 carbon atoms constituting a ring.
[0109] [ka]
[0110] In the above general formulae (G1-1) and (G1-2), R 3 ~R 6 each independently represents hydrogen or deuterium, m represents an integer of 0 to 4, n represents an integer of 1 to 5, and m+1≧n (m+1 is n or more). When m or n is 2 or more, a plurality of R 3 ~R 6 may be the same or different.
[0111] The organic compound represented by the above general formula (G1) is preferably any one of the following general formulas (G2-1) to (G2-6).
[0112] [ka]
[0113] However, R 11 ~R 26 each independently represents hydrogen or deuterium, h represents an integer of 1 to 6, and Ar is a substituted or unsubstituted heteroaromatic hydrocarbon ring having 2 to 30 carbon atoms constituting a ring, or a substituted or unsubstituted aromatic hydrocarbon ring having 6 to 30 carbon atoms constituting a ring. Note that Ar is preferably a substituted or unsubstituted heteroaromatic hydrocarbon ring having 2 to 30 carbon atoms constituting a ring.
[0114] In the above general formula (G1) and general formulas (G2-1) to (G2-6), specific examples of the heteroaromatic hydrocarbon ring having 2 to 30 carbon atoms constituting a substituted or unsubstituted ring represented by Ar or the aromatic hydrocarbon ring having 6 to 30 carbon atoms constituting a substituted or unsubstituted ring represented by Ar include a pyridine ring, a bipyridine ring, a pyrimidine ring, a bipyrimidine ring, a pyrazine ring, a bipyrazine ring, a triazine ring, a quinoline ring, an isoquinoline ring, a benzoquinoline ring, a phenanthroline ring, a quinoxaline ring, a benzoquinoxaline ring, a dibenzoquinoxaline ring, an azofluorene ring, a diazofluorene ring, a carbazole ring, a benzocarbazole ring, a dibenzocarbazo Examples of the ring include a dibenzofuran ring, a benzonaphthofuran ring, a dinaphthofuran ring, a dibenzothiophene ring, a benzonaphthothiophene ring, a dinaphthothiophene ring, a benzofuropyridine ring, a benzofuropyrimidine ring, a benzothiopyridine ring, a benzothiopyrimidine ring, a naphthofuropyridine ring, a naphthofuropyrimidine ring, a naphthothiopyridine ring, a naphthothiopyrimidine ring, an acridine ring, a xanthene ring, a phenothiazine ring, a phenoxazine ring, a phenazine ring, a triazole ring, an oxazole ring, an oxadiazole ring, a thiazole ring, a thiadiazole ring, an imidazole ring, a benzimidazole ring, a pyrazole ring, and a pyrrole ring. In the above general formula (G1) and general formulas (G2-1) to (G2-6), specific examples of the heteroaromatic hydrocarbon ring having 6 to 30 carbon atoms constituting the substituted or unsubstituted ring represented by Ar include a benzene ring, a naphthalene ring, a fluorene ring, a dimethylfluorene ring, a diphenylfluorene ring, a spirofluorene ring, an anthracene ring, a phenanthrene ring, a triphenylene ring, a pyrene ring, a tetracene ring, a chrysene ring, a benzo[a]anthracene ring, etc. Among these, any one of the following structural formulas (Ar-1) to (Ar-27) is preferable.
[0115] [ka]
[0116] It is preferable that the above Ar contains nitrogen as an atom constituting a ring, and the Ar is bonded to the skeleton in parentheses in the above general formula (G1) via a bond to the nitrogen or a bond to a carbon adjacent to the nitrogen.
[0117] Specific examples of the organic compounds represented by the above general formula (G1) and general formulas (G2-1) to (G2-6) include organic compounds represented by the following structural formulas (101) to (117), such as 1,1'-(9,9'-spirobi[9H-fluorene]-2,7-diyl)bis(1,3,4,6,7,8-hexahydro-2H-pyrimido[1,2-a]pyrimidine) (abbreviation: 2,7hpp2SF) (structural formula 108) and 1-(9,9'-spirobi[9H-fluorene]-2-yl)-1,3,4,6,7,8-hexahydro-2H-pyrimido[1,2-a]pyrimidine (abbreviation: 2hppSF) (structural formula 109).
[0118] [ka]
[0119] Such organic compounds are particularly suitable for use in light-emitting devices fabricated using a photolithography process, because they are stable, have little risk of metal contamination in the manufacturing line, unlike alkali metals or alkaline earth metals or their compounds, and are easy to deposit, etc. Of course, they are also suitable for light-emitting devices fabricated using a process that does not use photolithography.
[0120] In addition, it is preferable that the material having a strong basicity of pKa8 or more does not have an electron-transporting skeleton, from the viewpoint of suppressing recombination of the injected electrons and blocked holes on the material having a strong basicity of pKa8 or more.
[0121] Among them, 2hppSF is a material having a negative GSP_slope and a strong basicity of pKa 8 or more, and therefore can be said to be the first substance. By using 2hppSF, a layer having a negative GSP_slope can be obtained with one material, and at the same time, it is possible to block holes, which is preferable because it allows the provision of a light-emitting device with a low driving voltage.
[0122] Whether or not a layer made of a certain material blocks holes can be determined by fabricating an electronic device that allows only holes to flow (hereinafter referred to as a hole-only device) and measuring the relationship between current density and voltage. For example, when a target layer is sandwiched in a hole-only device such as that shown in Table 3, if a significantly low current density is obtained, the target layer can be determined to be a layer that blocks holes. Specifically, when the measurement device shown in Table 3 was measured, if the current density was 0.01 mA / cm at an applied voltage of 10 V, 2 Layer 3 can be considered a hole blocking layer if the following results are obtained:
[0123] [Table 3]
[0124] In Table 3, ITSO represents indium tin oxide containing silicon oxide, PCBBiF represents N-(biphenyl-4-yl)-N-[4-(9-phenyl-9H-carbazol-3-yl)phenyl]-9,9-dimethyl-9H-fluoren-2-amine, and OCHD-003 represents an electron acceptor material containing fluorine and has a molecular weight of 672.
[0125] Using such a device, it is advisable to compare the relationship between the current density and voltage when no layer 3 is formed and when a 10 nm thick target layer is formed on layer 3. When measurements are performed with a 10 nm thick target layer sandwiched between layer 3, the current density is 0.01 mA / cm at 10 V. 2 The following layers can be considered as hole blocking layers:
[0126] The results of measurements using such a device are shown in Figure 5. In Figure 5, the layer 3 of the hole-only device for the above measurement is made up of a single film of N-(biphenyl-4-yl)-N-[4-(9-phenyl-9H-carbazol-3-yl)phenyl]-9,9-dimethyl-9H-fluoren-2-amine (abbreviation: PCBBiF), a single film of 9-(2-naphthyl)-9'-phenyl-9H,9'H-3,3'-bicarbazole (abbreviation: βNCCP), a single film of 1-(2',7'-di-tert-butyl-9,9'-spirobi[9H-fluoren]-2-yl)-1,3,4,6,7,8-hexafluorophenyl These are the results for devices formed with a single film of sahydro-2H-pyrimido[1,2-a]pyrimidine (abbreviation: 2',7'tBu-2hppSF), a single film of 2,2'-(1,3-phenylene)bis(9-phenyl-1,10-phenanthroline) (abbreviation: mPPhen2P), a co-evaporated film of mPPhen2P:PCBBiF (1:1, weight ratio), a co-evaporated film of mPPhen2P:βNCCP (1:1, weight ratio), and a co-evaporated film of mPPhen2P:2',7'tBu-2hppSF (1:1, weight ratio).
[0127] From this figure, it can be said that the layers formed with PCBBiF, βNCCP, mPPhen2P, mPPhen2P:PCBBiF (1:1, weight ratio), and mPPhen2P:βNCCP (1:1, weight ratio) are layers that do not block holes, while the layer formed with mPPhen2P:2',7'tBu-hppSF (1:1, weight ratio) and the layer formed with 2',7'tBu-2hppSF are layers that block holes.
[0128] In addition, when the layer to be measured is a mixed layer of materials A and B, two devices were fabricated: a device (Device X) in which the mixed layer was placed as the measurement target layer of the hole-only device, and a device (Device Y) in which either material A or material B, whichever has the deeper highest occupied molecular orbital (HOMO) level, was placed as the measurement target layer in a single layer. 2 When the voltage in device X is shifted higher by 1 V or more in device X, the mixed layer can be said to be a hole-blocking layer.
[0129] In addition, the first layer preferably has an electron transport property in order to transport the injected electrons to the second layer. The electron mobility of the first layer is 1×10 -8 cm 2 / Vs or more. Therefore, the first layer preferably contains a material having electron transport properties. The material having electron transport properties is preferably a material having an electron transport skeleton. The electron transport skeleton is preferably a skeleton having a π-electron deficient heteroaromatic ring. The skeleton having a π-electron deficient heteroaromatic ring is preferably a skeleton containing at least one of a polyazole skeleton, a pyridine skeleton, a diazine skeleton, and a triazine skeleton in the ring. Specifically, a pyrimidine skeleton, a pyrazine skeleton, a pyridazine skeleton, a pyridine skeleton, a triazine skeleton, a benzofuropyrimidine skeleton, a benzothienopyrimidine skeleton, a benzofuropyrazine skeleton, a benzothienopyrazine skeleton, and the like are preferable. Among them, a pyrimidine skeleton, a pyrazine skeleton, a triazine skeleton, and a benzofuropyrimidine skeleton are preferable.
[0130] Examples of the material having an electron transport property include 2-(4-biphenylyl)-5-(4-tert-butylphenyl)-1,3,4-oxadiazole (abbreviation: PBD), 3-(4-biphenylyl)-4-phenyl-5-(4-tert-butylphenyl)-1,2,4-triazole (abbreviation: TAZ), 1,3-bis[5-(p-tert-butylphenyl)-1,3,4-oxadiazol-2-yl]benzene (abbreviation: OXD-7), 9-[4-(5-phenyl-1,3,4-oxadiazol-2-yl)phenyl]-9H-carbazole (abbreviation: CO11), 2,2',2''-(1,3,5-benzenetriyl)tris(1-phenyl-1H-benzimidazole) (abbreviation: TPBI), 2-[3-(dibenzothiophen-4-yl)phenyl]-1-phenyl-1H-benzimidazole (abbreviation: mDBTBIm-II), 4,4'-bis(5-methylbenzoxazol-2-yl)stilbene (abbreviation: BzOS), and other organic compounds with an azole skeleton, 3,5-bis[3-(9H-carbazol-9-yl)phenyl]pyridine (abbreviation: 35DCzPPy), 1,3,5-tri[3-(3 -pyridyl)phenyl]benzene (abbreviation: TmPyPB), bathophenanthroline (abbreviation: BPhen), bathocuproine (abbreviation: BCP), 2,9-di(naphthalen-2-yl)-4,7-diphenyl-1,10-phenanthroline (abbreviation: NBPhen), 2,2'-(1,3-phenylene)bis(9-phenyl-1,10-phenanthroline) (abbreviation: mPPhen2P), 2-[3-(2-triphenylenyl)phenyl]-1,10-phenanthroline (abbreviation: mTpPPhen), 2-phenyl-9-(2-triphenylenyl)-1,10- Organic compounds containing heteroaromatic rings with a pyridine skeleton, such as phenanthroline (abbreviation: Ph-TpPhen), 2-[4-(9-phenanthrenyl)-1-naphthalenyl]-1,10-phenanthroline (abbreviation: PnNPhen), and 2-[4-(2-triphenylenyl)phenyl]-1,10-phenanthroline (abbreviation: pTpPPhen), 2-[3-(dibenzothiophen-4-yl)phenyl]dibenzo[f,h]quinoxaline (abbreviation: 2mDBTPDBq-II), 2-[3-(3'-dibenzothiophen-4-yl)biphenyl]dibenzo[f,h]quinoxaline (abbreviation: 2mDBTBPDBq-II), 2-[3'-(9H-carbazol-9-yl)biphenyl-3-yl]dibenzo[f,h]quinoxaline (abbreviation: 2mCzBPDBq), 2-[4'-(9-phenyl-9H-carbazol-3-yl)-3,1'-biphenyl-1-yl]dibenzo[f,h]quinoxaline (abbreviation: 2mpPCBPDBq), 2-[4-(3,6-diphenyl-9H-carbazol-9-yl)phenyl]dibenzo[f,h]quinoxaline (abbreviation: 2CzPDBq-III), 7-[3-(dibenzothiophene 7mDBTPDBq-II), 6-[3-(dibenzothiophen-4-yl)phenyl]dibenzo[f,h]quinoxaline (abbreviation: 6mDBTPDBq-II), 9-[3'-(dibenzothiophen-4-yl)biphenyl-3-yl]naphtho[1',2':4,5]furo[2,3-b]pyrazine (abbreviation: 9mDBtBPNfpr), 9-[(3'-dibenzothiophen-4-yl)biphenyl-4-yl]naphtho[1',2':4,5]furo[2,3-b]pyrazine (abbreviation: 9pmDB tBPNfpr), 4,6-bis[3-(phenanthren-9-yl)phenyl]pyrimidine (abbreviation: 4,6mPnP2Pm), 4,6-bis[3-(4-dibenzothienyl)phenyl]pyrimidine (abbreviation: 4,6mDBTP2Pm-II), 4,6-bis[3-(9H-carbazol-9-yl)phenyl]pyrimidine (abbreviation: 4,6mCzP2Pm), 9,9'-[pyrimidine-4,6-diylbis(biphenyl-3,3'-diyl)]bis(9H-carbazole) (abbreviation: 4,6mCzBP2Pm), 8-(biphenyl-4-yl)-4-[3-( dibenzothiophen-4-yl)phenyl]-[1]benzofuro[3,2-d]pyrimidine (abbreviation: 8BP-4mDBtPBfpm), 3,8-bis[3-(dibenzothiophen-4-yl)phenyl]benzofuro[2,3-b]pyrazine (abbreviation: 3,8mDBtP2Bfpr), 4,8-bis[3-(dibenzothiophen-4-yl)phenyl]-[1]benzofuro[3,2-d]pyrimidine (abbreviation: 4,8mDBtP2Bfpm), 8-[3'-(dibenzothiophen-4-yl)(biphenyl-3-yl)]naphtho[1',2':4,5]furo[3,2-d]pyrimidine (abbreviation: 8mDBtBPNfpm), 8-[(2,2'-binaphthalene)-6-yl]-4-[3-(dibenzothiophene-4-yl)phenyl]-[1]benzofuro[3,2-d]pyrimidine (abbreviation: 8(βN2)-4mDBtPBfpm), 2,2'-(pyridine-2,6-diyl)bis(4-phenylbenzo[h]quinazoline) (abbreviation: 2,6(P-Bqn)2Py), 2,2'-(pyridine-2,6-diyl)bis{4-[4-(2-naphthyl)phenyl]-6-phenylpyrimidine} (abbreviation: 2,6(NP-PP m)2Py), 6-(biphenyl-3-yl)-4-[3,5-bis(9H-carbazol-9-yl)phenyl]-2-phenylpyrimidine (abbreviation: 6mBP-4Cz2PPm), 2,6-bis(4-naphthalen-1-ylphenyl)-4-[4-(3-pyridyl)phenyl]pyrimidine (abbreviation: 2,4NP-6PyPPm), 4-[3,5-bis(9H-carbazol-9-yl)phenyl]-2-phenyl-6-(biphenyl-4-yl)pyrimidine (abbreviation: 6BP-4Cz2PPm), 7-[4-(9-phenyl-9H-carbazol- organic compounds with a diazine skeleton such as 2-(biphenyl-4-yl)-4-phenyl-6-(9,9'-spirobi[9H-fluoren]-2-yl)-1,3,5-triazine (abbreviation: BP-SFTzn), 2-{3-[3-(benzo[b]naphtho[1,2-d]furan-8-yl)phenyl]phenyl}-4,6-diphenyl-1,3,5-triazine (abbreviation: mBnfBPTzn), 2-{3-[3-(benzo[b]naphtho[1,2-d]furan-8-yl)phenyl]phenyl}-4,6-diphenyl-1,3,5-triazine (abbreviation: mBnfBPTzn), mBnfBPTzn-02), 2-{4-[3-(N-phenyl-9H-carbazol-3-yl)-9H-carbazol-9-yl]phenyl}-4,6-diphenyl-1,3,5-triazine (abbreviation: PCCzPTzn), 9-[3-(4,6-diphenyl-1,3,5-triazin-2-yl)phenyl]-9'-phenyl-2,3'-bi-9H-carbazole (abbreviation: mPCCzPTzn-02), 2-[3'-(9,9-Dimethyl-9H-fluoren-2-yl)biphenyl-3-yl]-4,6-diphenyl-1,3,5-triazine (abbreviation: mFBPTzn), 5-[3-(4,6-diphenyl-1,3,5-triazin-2-yl)phenyl]-7,7-dimethyl-5H,7H-indeno[2,1-b]carbazole (abbreviation: mINc(II)PTzn), 2-{3-[3-(dibenzothio 2,4,6-tris[3'-(pyridin-3-yl)biphenyl-3-yl]-1,3,5-triazine (abbreviation: TmPPPyTz), 2-[3-(2,6-dimethyl-3-pyridinyl)-5-(9-phenanthrenyl)phenyl]-4,6-diphenyl-1,3,5-triazine (abbreviation: mDBtBPTzn), 2,4,6-tris[3'-(pyridin-3-yl)biphenyl-3-yl]-1,3,5-triazine (abbreviation: TmPPPyTz), 1,3,5-Triazine (abbreviation: mPn-mDMePyPTzn), 11-[4-(biphenyl-4-yl)-6-phenyl-1,3,5-triazin-2-yl]-11,12-dihydro-12-phenylindolo[2,3-a]carbazole (abbreviation: BP-Icz(II)Tzn), 2-[3'-(triphenylen-2-yl)biphenyl-3-yl]-4,6-diphenyl- 1,3,5-triazine (abbreviation: mTpBPTzn), 3-[9-(4,6-diphenyl-1,3,5-triazin-2-yl)-2-dibenzofuranyl]-9-phenyl-9H-carbazole (abbreviation: PCDBfTzn), 2-(biphenyl-3-yl)-4-phenyl-6-{8-[(1,1':4',1''-terphenyl)-4-yl]-1-dibenzofuranyl}-1,3,Examples of the organic compounds include organic compounds containing a heteroaromatic ring having a triazine skeleton such as 5-triazine (abbreviation: mBP-TPDBfTzn). In addition, organic compounds containing a heteroaromatic ring having a diazine skeleton (pyrimidine skeleton, pyrazine skeleton, pyridazine skeleton), organic compounds containing a heteroaromatic ring having a pyridine skeleton, and organic compounds containing a heteroaromatic ring having a triazine skeleton are preferable because they have good reliability. In particular, organic compounds containing a heteroaromatic ring having a diazine (pyrimidine or pyrazine) skeleton and organic compounds containing a heteroaromatic ring having a triazine skeleton have high electron transport properties and contribute to reducing the driving voltage. In addition, benzofuropyrimidine skeleton, benzothienopyrimidine skeleton, benzofuropyrazine skeleton, and benzothienopyrazine skeleton are preferable because they have good reliability.
[0131] In addition, as the material having electron transport properties, for example, metal complexes such as bis(10-hydroxybenzo[h]quinolinato)beryllium(II) (abbreviation: BeBq2), bis(2-methyl-8-quinolinolato)(4-phenylphenolato)aluminum(III) (abbreviation: BAlq), bis(8-quinolinolato)zinc(II) (abbreviation: Znq), bis[2-(2-benzoxazolyl)phenolato]zinc(II) (abbreviation: ZnPBO), bis[2-(2-benzothiazolyl)phenolato]zinc(II) (abbreviation: ZnBTZ) can be used. As the organic compound having a π-electron-deficient heteroaromatic ring skeleton, for example, an organic compound having a heteroaromatic ring with a polyazole skeleton, an organic compound having a heteroaromatic ring with a pyridine skeleton, an organic compound having a heteroaromatic ring with a diazine skeleton, and an organic compound having a heteroaromatic ring with a triazine skeleton can be mentioned.
[0132] Among them, organic compounds having a phenanthroline skeleton such as mTpPPhen, PnNPhen and mPPhen2P are preferred, and organic compounds having a phenanthroline dimer structure such as mPPhen2P are more preferred because of their excellent stability. In addition, materials having a pyridine skeleton or a phenanthroline skeleton have a high pKa, and therefore have a high hole blocking property, and are particularly preferred.
[0133] In addition, the LUMO level of the material having electron transport properties in the first layer is preferably −3.00 eV or more and −2.00 eV or less, since this lowers the barrier for electron injection into the light-emitting layer.
[0134] In addition, when the first layer contains both a material having electron transport properties and a material having strong basicity, it is preferable that the material having strong basicity does not have electron donating properties to the material having electron transport properties. Since the material having strong basicity does not have electron donating properties, it does not easily react with atmospheric components such as water and oxygen, and therefore the stability is improved. This makes it possible to fabricate an intermediate layer and a tandem-type light-emitting device that are more stable to atmospheric components such as water and oxygen. For this reason, it is preferable that the first layer has a small signal observed by electron spin resonance (ESR) or no signal is observed. For example, when the spin density due to a signal observed near a g value of 2.00 is 1×10 17 spins / cm 3 Less than or equal to 1×10 is preferred 16 spins / cm 3 Less than is more preferred.
[0135] The first layer is preferably thin, but if it is too thick the driving voltage increases, and if it is too thin the characteristics, particularly the reliability, deteriorate. Therefore, the thickness is preferably 2 nm to 13 nm, more preferably 5 nm to 10 nm.
[0136] Most organic compounds have a positive GSP_slope, but the first layer can be made to have a negative GSP_slope by mixing with the first substance, which is a material having a negative GSP_slope. In this case, the mixing ratio at which the first layer becomes a layer having a negative GSP_slope changes depending on the GSP_slope value of the first substance and the GSP_slope value of the material having electron transport properties, but the first layer can be made to have a negative GSP_slope by appropriately increasing the ratio of the first substance.
[0137] The first layer is formed on and in contact with the second layer. The second layer, which is the base of the first layer, is a layer located closer to the substrate than the first layer. That is, the first layer is formed after the second layer is formed. The second layer also plays a role in transporting electrons to the light-emitting layer, so it is preferable that the second layer is a layer having electron transport properties. Specifically, the second layer is preferably an electron transport layer of the light-emitting unit that is in contact with the anode side surface of the intermediate layer. The base layer may be the light-emitting layer or a hole-blocking layer.
[0138] The electron mobility of the second layer is 1×10 at a square root of the electric field strength [V / cm] of 600. -8 cm 2 / Vs or more. Therefore, the second layer preferably contains a material having electron transport properties. The material having electron transport properties is preferably a material having an electron transport skeleton. The electron transport skeleton is preferably a skeleton having a π-electron deficient heteroaromatic ring. The skeleton having a π-electron deficient heteroaromatic ring is preferably a skeleton including at least one of a polyazole skeleton, a pyridine skeleton, a diazine skeleton, and a triazine skeleton in the ring. Specifically, a pyrimidine skeleton, a pyrazine skeleton, a pyridazine skeleton, a pyridine skeleton, a triazine skeleton, a benzofuropyrimidine skeleton, a benzothienopyrimidine skeleton, a benzofuropyrazine skeleton, a benzothienopyrazine skeleton, and the like are preferable. Among them, a pyrimidine skeleton, a pyrazine skeleton, a triazine skeleton, and a benzofuropyrimidine skeleton are preferable. As a specific material, the same material as the material having electron transport properties exemplified as a material that can be used for the first layer can be used.
[0139] In addition, when the first layer has hole blocking properties, the second layer is preferably a bipolar layer, i.e., a layer with relatively high hole transport properties, since it is possible to provide a light-emitting device with a lower driving voltage by accumulating holes. For this reason, it is preferable that the HOMO level of the organic compound contained in the second layer is -5.90 eV or more and -5.00 eV or less, preferably -5.80 eV or more and -5.00 eV or less, more preferably -5.70 eV or more and -5.15 eV or less. In addition, since the second layer also needs good electron transport properties, it is preferable that the LUMO level of the organic compound contained in the second layer is -3.15 eV or more and -2.50 eV or less, preferably -3.00 eV or more and -2.70 eV or less.
[0140] The second layer may be a layer made of a single material or a layer made of a plurality of materials. When the second layer contains a plurality of organic compounds, it is preferable that the HOMO level of the organic compound having the highest HOMO level is within the range described above. When the second layer contains a plurality of organic compounds, it is preferable that the LUMO level of the organic compound having the lowest LUMO level is within the range described above. When the second layer is made of a plurality of organic compounds, it is preferable that at least one of them is an organic compound having electron transport properties and at least one of them is an organic compound having hole transport properties.
[0141] In addition, it is preferable that the organic compound having electron transport properties and the organic compound having hole transport properties are one organic compound, that is, it is more preferable that the second layer contains an organic compound having both electron transport properties and hole transport properties, because this makes it easier to obtain a light-emitting device with good characteristics.
[0142] The organic compound having electron transport properties or the organic compound having both electron transport properties and hole transport properties used in the second layer has an electron mobility of 1×10 -7 cm 2 / Vs or more, preferably 1×10 -6 cm 2In addition, a hole-transporting organic compound or an organic compound having both an electron-transporting property and a hole-transporting property has a hole mobility of 1×10 -7 cm 2 / Vs or more, preferably 1×10 -6 cm 2 A material having a hole mobility of .gtoreq..times ...
[0143] The second layer preferably contains an organic compound having an acid dissociation constant pKa of 4 or less and having electron transport properties.
[0144] In addition, the second layer preferably contains an organic compound having an electron transporting skeleton and an organic compound having a hole transporting skeleton. Note that the organic compound having the electron transporting skeleton and the organic compound having the hole transporting skeleton are preferably one organic compound. That is, it is more preferable that the second layer contains an organic compound having both an electron transporting skeleton and a hole transporting skeleton, because it is easier to obtain a light-emitting device with good characteristics.
[0145] The electron transporting skeleton is preferably a skeleton having a π-electron deficient heteroaromatic ring. The skeleton having a π-electron deficient heteroaromatic ring is preferably a skeleton containing at least one of a polyazole skeleton, a pyridine skeleton, a diazine skeleton, and a triazine skeleton in the ring. Specifically, a pyrimidine skeleton, a pyrazine skeleton, a pyridazine skeleton, a pyridine skeleton, a triazine skeleton, a benzofuropyrimidine skeleton, a benzothienopyrimidine skeleton, a benzofuropyrazine skeleton, a benzothienopyrazine skeleton, and the like are preferred. Among them, a pyrimidine skeleton, a pyrazine skeleton, a triazine skeleton, and a benzofuropyrimidine skeleton are preferred. In addition, the hole transporting skeleton is preferably a skeleton having a π-electron rich heteroaromatic ring. As the π-electron rich heteroaromatic ring, for example, a condensed aromatic ring containing at least one of a pyrrole skeleton, a furan skeleton, and a thiophene skeleton in the ring is preferred. Specifically, a carbazole skeleton, a dibenzothiophene skeleton, or a skeleton in which an aromatic ring or a heteroaromatic ring is further condensed to these is preferred. Among these, a carbazole skeleton, a biscarbazole skeleton, and an indolocarbazole skeleton are preferable, and an amine skeleton, particularly a triphenylamine skeleton, is also preferable.
[0146] As the organic compound constituting the second layer, an organic compound having both an electron transporting skeleton and a hole transporting skeleton as described above is preferable. Specific examples of the organic compound include 3,6-bis(diphenylamino)-9-[4-(4,6-diphenyl-1,3,5-triazin-2-yl)phenyl]-9H-carbazole (abbreviation: DACT-II), 2-{3-[3-(N-phenyl-9H-carbazol-3-yl)-9H-carbazol-9-yl]phenyl}dibenzo[f,h]quinoxaline (abbreviation: 2mPCCzPDBq), 9-[3-( 4,6-diphenyl-1,3,5-triazin-2-yl)phenyl]-9'-phenyl-2,3'-bi-9H-carbazole (abbreviation: mPCCzPTzn-02), 11-[4-(biphenyl-4-yl)-6-phenyl-1,3,5-triazin-2-yl]-11,12-dihydro-12-phenylindolo[2,3-a]carbazole (abbreviation: BP-Icz(II)Tzn), and the like.
[0147] The organic compound constituting the second layer preferably emits thermally activated delayed fluorescence (TADF) (has TADF properties). Organic compounds with TADF properties have a high HOMO level, a low LUMO level, and short excitation lifetimes for both singlets and triplets. Therefore, when recombination occurs in the second layer, the excited state can be quickly deactivated, and a highly reliable light-emitting device can be provided. Among the organic compounds preferable for constituting the second layer, DACT-II can be given as an organic compound that further has TADF properties.
[0148] In addition, when the second layer is composed of a plurality of materials, the material having electron transport properties is preferably a material having an electron transport skeleton. The electron transport skeleton is preferably a skeleton having a π-electron deficient heteroaromatic ring. As the skeleton having a π-electron deficient heteroaromatic ring, for example, a skeleton containing at least one of a polyazole skeleton, a pyridine skeleton, a diazine skeleton, and a triazine skeleton in the ring is preferable. Specifically, a pyrimidine skeleton, a pyrazine skeleton, a pyridazine skeleton, a pyridine skeleton, a triazine skeleton, a benzofuropyrimidine skeleton, a benzothienopyrimidine skeleton, a benzofuropyrazine skeleton, a benzothienopyrazine skeleton, and the like are preferable. Among them, a pyrimidine skeleton, a pyrazine skeleton, a triazine skeleton, and a benzofuropyrimidine skeleton are preferable. As a specific material, the same material having electron transport properties as exemplified as a material that can be used for the first layer can be used.
[0149] In addition, when the second layer is composed of a plurality of organic compounds, examples of the organic compound having a hole transporting property include N-(4-biphenyl)-6,N-diphenylbenzo[b]naphtho[1,2-d]furan-8-amine (abbreviation: BnfABP), N,N-bis(4-biphenyl)-6-phenylbenzo[b]naphtho[1,2-d]furan-8-amine (abbreviation: BBABnf), 4,4'-bis(6-phenylbenzo[b]naphtho[1,2-d]furan-8-yl)-4''-phenyltriphenylamine (abbreviation: BnfBB1BP), N,N -Bis(4-biphenyl)benzo[b]naphtho[1,2-d]furan-6-amine (abbreviation: BBABnf(6)), N,N-bis(4-biphenyl)benzo[b]naphtho[1,2-d]furan-8-amine (abbreviation: BBABnf(8)), N,N-bis(4-biphenyl)benzo[b]naphtho[2,3-d]furan-4-amine (abbreviation: BBABnf(II)(4)), N,N-bis[4-(dibenzofuran-4-yl)phenyl]-4-amino-p-terphenyl (abbreviation: DBfBB1TP), N-[4-(dibenzothiophene-4 -yl)phenyl]-N-phenyl-4-biphenylamine (abbreviation: ThBA1BP), 4-(2-naphthyl)-4',4''-diphenyltriphenylamine (abbreviation: BBAβNB), 4-[4-(2-naphthyl)phenyl]-4',4''-diphenyltriphenylamine (abbreviation: BBAβNBi), 4,4'-diphenyl-4''-(6;1'-binaphthyl-2-yl)triphenylamine (abbreviation: BBAαNβNB), 4,4'-diphenyl-4''-(7;1'-binaphthyl-2-yl)triphenylamine (abbreviation: BB AαNβNB-03), 4,4'-diphenyl-4''-(7-phenyl)naphthyl-2-yltriphenylamine (abbreviation: BBAPβNB-03), 4,4'-diphenyl-4''-(6;2'-binaphthyl-2-yl)triphenylamine (abbreviation: BBA(βN2)B), 4,4'-diphenyl-4''-(7;2'-binaphthyl-2-yl)triphenylamine (abbreviation: BBA(βN2)B-03), 4,4'-diphenyl-4''-(4;2'-binaphthyl-1-yl)triphenylamine (abbreviation: BBAβNαNB), 4,4'-Diphenyl-4''-(5;2'-binaphthyl-1-yl)triphenylamine (abbreviation: BBAβNαNB-02), 4-(4-biphenylyl)-4'-(2-naphthyl)-4''-phenyltriphenylamine (abbreviation: TPBiAβNB), 4-(3-biphenylyl)-4'-[4-(2-naphthyl)phenyl]-4''-phenyltriphenylamine (abbreviation: mTPBiAβNBi), 4-(4-biphenylyl)-4'-[4-(2-naphthyl)phenyl] 4,4'-diphenyl-4''-[4'-(carbazol-9-yl)biphenyl-4-yl]triphenylamine (abbreviation: YGTBi1BP), 4'-[4-(3-phenyl-9H-carbazol-9-yl)furan-4''-phenyltriphenylamine (abbreviation: TPBiAβNBi), 4-phenyl-4'-(1-naphthyl)triphenylamine (abbreviation: αNBA1BP), 4,4'-bis(1-naphthyl)triphenylamine (abbreviation: αNBB1BP), 4,4'-diphenyl-4''-[4'-(carbazol-9-yl)biphenyl-4-yl]triphenylamine (abbreviation: YGTBi1BP), 4'-[4-(3-phenyl-9H-carbazol-9-yl)furan-4''-phenyltriphenylamine (abbreviation: TPBiAβNBi), N-[4-(9-phenyl-9H-carbazol-3-yl)phenyl]-N-[4-(1-naphthyl)phenyl]-9,9'-spirobi[9H-fluorene]-2-amine (abbreviation: PCBNBSF), N,N- Bis(biphenyl-4-yl)-9,9'-spirobi[9H-fluorene]-2-amine (abbreviation: BBASF), N,N-bis(biphenyl-4-yl)-9,9'-spirobi[9H-fluorene]-4-amine (abbreviation: BBASF(4)), N-(biphenyl-2-yl)-N-(9,9-dimethyl-9H-fluoren-2-yl)-9,9'-spirobi[9H-fluorene]-4-amine (abbreviation: oFBiSF), N-(biphenyl-4-yl)-N-(9,9-Dimethyl-9H-fluoren-2-yl)dibenzofuran-4-amine (abbreviation: FrBiF), N-[4-(1-naphthyl)phenyl]-N-[3-(6-phenyldibenzofuran-4-yl)phenyl]-1-naphthylamine (abbreviation: mPDBfBNBN), 4-phenyl-4'-(9-phenylfluoren-9-yl)triphenylamine (abbreviation: BPAFLP), 4-phenyl-3'-(9-phenylfluoren-9-yl)triphenylamine (abbreviation: mBPAFLP), 4-phenyl-4'-[4-(9-phenylfluoren-9-yl)furan 4,4'-diphenyl-4''-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBA1BP), 4,4'-diphenyl-4''-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBBi1BP), 4-(1-naphthyl)-4'-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBANB), 4,4'-di(1-naphthyl)-4''-(9-phenyl-9H-carbazol-3-yl)triphenylamine PCBNBB, N-phenyl-N-[4-(9-phenyl-9H-carbazol-3-yl)phenyl]-9,9'-spirobi[9H-fluorene]-2-amine (PCBASF), N-(biphenyl-4-yl)-N-[4-(9-phenyl-9H-carbazol-3-yl)phenyl]-9,9-dimethyl-9H-fluorene-2-amine (PCBBiF), N,N-bis(9,9-dimethyl-9H-fluorene-2-yl)-9,9'-spirobi-9H-fluorene-4-amine, N,N-bis(9,9-dimethyl-9H- fluoren-2-yl)-9,9'-spirobi-9H-fluoren-3-amine, N,N-bis(9,9-dimethyl-9H-fluoren-2-yl)-9,9'-spirobi-9H-fluoren-2-amine, N,N-bis(9,9-dimethyl-9H-fluoren-2-yl)-9,9'-spirobi-9H-fluoren-1-amine, N,N'-di(p-tolyl)-N,N'-diphenyl-p-phenylenediamine (abbreviation: DTDPPA), 4,4'-bis[N-(4-diphenylaminophenyl)-N-phenylamino]biphenyl (abbreviation: DPAB), 4,Examples of the compound include 4'-bis(N-{4-[N'-(3-methylphenyl)-N'-phenylamino]phenyl}-N-phenylamino)biphenyl (abbreviation: DNTPD), 1,3,5-tris[N-(4-diphenylaminophenyl)-N-phenylamino]benzene (abbreviation: DPA3B), N-(9,9-diphenyl-9H-fluoren-2-yl)-N,9-diphenyl-9H-carbazol-3-amine (abbreviation: PCAFLP(2)), and N-(9,9-diphenyl-9H-fluoren-2-yl)-N,9-diphenyl-9H-carbazol-2-amine (abbreviation: PCAFLP(2)-02).
[0150] The second layer is preferably as thin as possible, and a thickness of 5 nm to 10 nm is preferable in order to fabricate a highly reliable light-emitting device.
[0151] The P-type CGL is preferably formed from a composite material containing a material having an electron accepting property and an organic compound having a hole transporting property.
[0152] In addition, it is preferable that the material having electron acceptability has electron acceptability for an organic compound having hole transportability. When the material having electron acceptability has electron acceptability, charge separation occurs in the P-type CGL, and the material can function as a charge generation layer, so that the material can function as a tandem intermediate layer. In addition, it is preferable that the P-type CGL exhibits a signal observed by electron spin resonance. For example, when the spin density resulting from a signal observed near a g value of 2.00 is 1×10 17 spins / cm 3 More preferably, 1×10 18 spins / cm 3 More preferably, 1×10 19 spins / cm 3 The above is even more preferable.
[0153] As the substance having acceptor properties, an organic compound having an electron-withdrawing group (such as a halogen group or a cyano group) can be used, and examples thereof include 7,7,8,8-tetracyano-2,3,5,6-tetrafluoroquinodimethane (abbreviation: F4-TCNQ), chloranil, 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene (abbreviation: HAT-CN), 1,3,4,5,7,8-hexafluorotetracyano-naphthoquinodimethane (abbreviation: F6-TCNNQ), 2-(7-dicyanomethylene-1,3,4,5,6,8,9,10-octafluoro-7H-pyren-2-ylidene)malononitrile, and the like. In particular, compounds in which an electron-withdrawing group is bonded to a condensed aromatic ring having multiple heteroatoms, such as HAT-CN, are thermally stable and preferred. Radialene derivatives having an electron-withdrawing group (especially a halogen group such as a fluoro group, a cyano group, etc.) [3] are preferred because they have a very high electron-accepting property, and specific examples thereof include α,α',α''-1,2,3-cyclopropane triylidene tris[4-cyano-2,3,5,6-tetrafluorobenzeneacetonitrile], α,α',α''-1,2,3-cyclopropane triylidene tris[2,6-dichloro-3,5-difluoro-4-(trifluoromethyl)benzeneacetonitrile], and α,α',α''-1,2,3-cyclopropane triylidene tris[2,3,4,5,6-pentafluorobenzeneacetonitrile]. As the substance having acceptor properties, in addition to the organic compounds described above, transition metal oxides such as molybdenum oxide, vanadium oxide, ruthenium oxide, tungsten oxide, and manganese oxide can be used.
[0154] As the organic compound having a hole transporting property used in the composite material, various organic compounds such as aromatic amine compounds, heteroaromatic compounds, aromatic hydrocarbons, and polymer compounds (oligomers, dendrimers, polymers, etc.) can be used. Note that the organic compound having a hole transporting property used in the composite material is preferably 1×10 -6 cm 2It is preferable that the organic compound has a hole mobility of 1000 nm or more / Vs. The organic compound having hole transport properties used in the composite material is preferably a compound having a condensed aromatic hydrocarbon ring or a π-electron-rich heteroaromatic ring. As the condensed aromatic hydrocarbon ring, an anthracene ring, a naphthalene ring, etc. are preferable. As the π-electron-rich heteroaromatic ring, a condensed aromatic ring containing at least one of a pyrrole skeleton, a furan skeleton, and a thiophene skeleton in the ring is preferable, and specifically, a carbazole ring, a dibenzothiophene ring, or a ring in which an aromatic ring or a heteroaromatic ring is further condensed to the above rings is preferable.
[0155] Such organic compounds having hole transport properties preferably have any of a carbazole skeleton, a dibenzofuran skeleton, a dibenzothiophene skeleton, and an anthracene skeleton. In particular, the organic compounds may be aromatic amines having a substituent containing a dibenzofuran ring or a dibenzothiophene ring, aromatic monoamines having a naphthalene ring, or aromatic monoamines in which a 9-fluorenyl group is bonded to the nitrogen of the amine via an arylene group. It is preferable that the organic compounds having hole transport properties are substances having an N,N-bis(4-biphenyl)amino group, because this allows the manufacture of a light-emitting device with a long life.
[0156] As the organic compound having the hole-transporting property as described above, specifically, when the second layer is composed of multiple types of organic compounds, the materials listed as materials that can be used as the organic compound having the hole-transporting property can be used in the same manner.
[0157] In addition, as a material having hole transport properties, other aromatic amine compounds such as N,N'-di(p-tolyl)-N,N'-diphenyl-p-phenylenediamine (abbreviation: DTDPPA), 4,4'-bis[N-(4-diphenylaminophenyl)-N-phenylamino]biphenyl (abbreviation: DPAB), 4,4'-bis(N-{4-[N'-(3-methylphenyl)-N'-phenylamino]phenyl}-N-phenylamino)biphenyl (abbreviation: DNTPD), and 1,3,5-tris[N-(4-diphenylaminophenyl)-N-phenylamino]benzene (abbreviation: DPA3B) can also be used.
[0158] It is preferable that a third layer is provided between the P-type CGL and the first layer. The third layer has at least an electron transporting property and has a function of preventing an interaction between the P-type CGL and the first layer and smoothly transferring electrons. The LUMO level of the substance having an electron transporting property contained in the third layer is preferably located between the LUMO level of the acceptor substance in the P-type CGL and the lowest LUMO level of the material contained in the first layer. The specific energy level of the LUMO level of the substance having an electron transporting property used in the third layer is -5.00 eV or more, preferably -4.30 eV or more, and -3.00 eV or less, preferably -3.25 eV or less. Therefore, it is preferable that the substance having an electron transporting property used in the third layer has a LUMO level of -5.00 eV or more and -3.00 eV or less, and more preferably has a LUMO level of -4.30 eV or more and -3.25 eV or less. By using a layer made of such a material for the third layer, the electron injection property can be improved, an increase in the driving voltage can be suppressed, and reliability can be improved, which is preferable.Examples of the substance having an electron transport property used in the third layer include diquinoxalino[2,3-a:2',3'-c]phenazine (abbreviation: HATNA), 2,3,8,9,14,15-hexafluorodiquinoxalino[2,3-a:2',3'-c]phenazine (abbreviation: HATNA-F6), perylene tetracarboxylic acid derivatives such as 3,4,9,10-perylene tetracarboxylic diimide (abbreviation: PTCDI) and 3,4,9,10-perylene tetracarboxyl-bis-benzimidazole (abbreviation: PTCBI), (C60-Ih)[5,6]fullerene (abbreviation: C60), (C70-D5h)[5,6] Organic compounds such as fullerene (abbreviation: C70) and phthalocyanine (abbreviation: HPc), copper phthalocyanine (abbreviation: CuPc), zinc phthalocyanine (abbreviation: ZnPc), cobalt phthalocyanine (abbreviation: CoPc), iron phthalocyanine (abbreviation: FePc), tin phthalocyanine (abbreviation: SnPc), tin oxide phthalocyanine (abbreviation: SnOPc), titanium oxide phthalocyanine (abbreviation: TiOPc), vanadium oxide phthalocyanine (abbreviation: VOPc), and other metal phthalocyanines having copper, zinc, cobalt, iron, chromium, nickel, vanadium, titanium, tin, and the like, and derivatives thereof can be used. In particular, phthalocyanine-based metal complexes such as CuPc or ZnPc or 2,3,8,9,14,15-hexafluorodiquinoxalino[2,3-a:2',3'-c]phenazine are preferred. Among these, CuPc and ZnPc are preferred because they are inexpensive and have good characteristics. Furthermore, ZnPc has a small diffusion coefficient for silicon, which reduces the risk of metal diffusion into the semiconductor affecting the semiconductor characteristics, making it particularly suitable for use in displays that use silicon semiconductors.
[0159] The thickness of the third layer is preferably 1 nm or more and 10 nm or less, and more preferably 2 nm or more and 5 nm or less.
[0160] A light-emitting device according to one embodiment of the present invention having the above-described structure can have high current efficiency and a suppressed increase in driving voltage.
[0161] Note that the light-emitting device of one embodiment of the present invention is particularly suitable for a light-emitting device that has undergone a photolithography process; however, even a light-emitting device manufactured without undergoing a photolithography process has high stability against the atmosphere, which improves yield and contributes to cost reduction because it is not necessary to control the atmosphere more strictly during the manufacturing process.
[0162] (Embodiment 2) In the embodiment 1, a structure of a forward stacking method (a manufacturing method in which stacking is performed from the anode) is mainly described. In the embodiment, a light-emitting device according to one embodiment of the present invention having a structure of a reverse stacking method (a manufacturing method in which stacking is performed from the cathode) will be described.
[0163] In the case of a reverse-stack light-emitting device, a cathode is formed on a substrate, and the stacking order is reversed from that in FIG. 1(A), so that the first layer 21 is formed and then the second layer 22 is formed as shown in FIG. 1(B). In this case, in order to have a high density of positive interface charges 50 at the interface between the first layer 21 and the second layer 22, the first layer 21 is preferably formed of a material that has a positive GSP_slope, and the second layer 22 is preferably formed of a material that has a negative GSP_slope. In this way, a tandem-type light-emitting device in which the increase in driving voltage is suppressed can be obtained even without making the first layer 21 an N-type CGL. Since the first layer 21 does not contain a Li compound or the like, the tandem-type light-emitting device can be a light-emitting device in which the increase in driving voltage is suppressed even after a photolithography process.
[0164] In this case, the second layer 22 can be made of any of the substances listed as materials having a negative GSP_slope in the embodiment 1. However, in order to further reduce the driving voltage by accumulating the holes injected from the anode 101 near the interface between the second layer 22 and the first layer 21, it is preferable that the second layer 22 has a hole transporting property, and therefore it is preferable that the second layer 22 does not contain a highly basic material having a pKa of 8 or more.
[0165] Since the second layer 22 needs to have a function of transporting electrons injected from the first layer 21 to the light-emitting layer 113_1 on the anode 101 side, it preferably has electron transport properties and preferably contains a material having electron transport properties. Since the second layer 22 preferably has hole transport properties as described above, it is preferably a material having both hole transport properties and electron transport properties and preferably contains a material having a skeleton with hole transport properties and a skeleton with electron transport properties. The second layer 22 may have both a material with electron transport properties and a material with hole transport properties.
[0166] On the other hand, since it is preferable that the first layer 21 has a hole blocking property, the first layer 21 preferably contains a highly basic material having a pKa of 8 or more.
[0167] (Embodiment 3) In this embodiment, a light-emitting device according to one embodiment of the present invention will be described in detail.
[0168] 6 is a schematic diagram of a light-emitting device according to one embodiment of the present invention. The light-emitting device has an anode 101 provided on a substrate 1000, and an organic compound layer 103 between the anode 101 and a cathode 102. As described in Embodiment 1, the organic compound layer 103 includes a plurality of light-emitting units (a first light-emitting unit 501 and a second light-emitting unit 502 in FIG. 6) and an intermediate layer 513.
[0169] The first light-emitting unit 501 has at least a light-emitting layer 113_1, and the second light-emitting unit 502 has at least a light-emitting layer 113_2. The light-emitting layer 113_1 and the light-emitting layer 113_2 are layers containing a light-emitting substance, and emit light when a voltage is applied between the anode 101 and the cathode 102.
[0170] 6, the first light-emitting unit 501 preferably has functional layers such as a hole injection layer 111, a hole transport layer 112_1, and an electron transport layer 114_1 in addition to the layers described above. In addition, functional layers other than the functional layers described above, such as a hole blocking layer, an electron blocking layer, and an exciton blocking layer, may be included. Conversely, any of the layers described above may not be provided.
[0171] 6, in addition to the layers described above, the second light-emitting unit 502 preferably has functional layers such as a hole transport layer 112_2, an electron transport layer 114_2, and an electron injection layer 115. In addition, the second light-emitting unit 502 may include functional layers other than the layers described above, such as a hole blocking layer, an electron blocking layer, and an exciton blocking layer. Conversely, any of the layers described above may not be provided.
[0172] Moreover, the intermediate layer 513 has at least the first layer 21 and the P-type CGL 20 from the anode 101 side, and may have a third layer 23 between the first layer 21 and the P-type CGL 20. The first layer 21 is a layer having a negative GSP_slope as described in the first embodiment. The first layer 21 may further have an organic compound having an electron transporting property and / or a material having a strong basicity of pKa8 or more. The P-type CGL 20 is a layer that generates charges by applying a voltage. The P-type CGL 20 is preferably a layer containing an organic compound having a hole transporting property and a substance having an acceptor property with respect to the organic compound. The third layer 23 is a layer provided to prevent an interaction between the first layer 21 and the P-type CGL 20 and to improve reliability.
[0173] The specific configurations of the first layer 21, the P-type CGL 20, and the third layer 23 have been described in detail in the first embodiment, and therefore will not be described again.
[0174] The anode 101 and the cathode 102 may be formed as a single layer structure or a laminated structure, and in the case of a laminated structure, a layer in contact with the organic compound layer 103 substantially functions as an anode or a cathode. In the case of an electrode having a laminated structure, there is no restriction on the work function of layers other than the layer in contact with the organic compound layer 103, and materials may be selected according to required characteristics such as resistance value, ease of processing, reflectance, translucency, and stability.
[0175] The anode 101 is preferably formed using a metal, alloy, conductive compound, or mixture thereof having a large work function (specifically, 4.0 eV or more). Specific examples include indium oxide-tin oxide (ITO), indium oxide-tin oxide containing silicon or silicon oxide (ITSO), indium oxide-zinc oxide, and indium oxide containing tungsten oxide and zinc oxide (IWZO). These conductive metal oxide films are usually formed by a sputtering method, but may also be formed by applying a sol-gel method or the like. As an example of a method for forming indium oxide-zinc oxide, a method for forming indium oxide-zinc oxide by a sputtering method using a target in which 1 to 20 wt % of zinc oxide is added to indium oxide may be used. Indium oxide containing tungsten oxide and zinc oxide (IWZO) can also be formed by sputtering using a target containing 0.5 to 5 wt% tungsten oxide and 0.1 to 1 wt% zinc oxide relative to indium oxide. Other materials used for the anode include, for example, gold (Au), platinum (Pt), nickel (Ni), tungsten (W), chromium (Cr), molybdenum (Mo), iron (Fe), cobalt (Co), copper (Cu), palladium (Pd), titanium (Ti), aluminum (Al), or nitrides of metal materials (for example, titanium nitride). A layer of these laminated materials may also be used as the anode. For example, a film laminated in the order of Al, Ti, and ITSO on Ti is preferable because it has a good reflectance, is highly efficient, and can achieve high resolution of several thousand ppi. Alternatively, graphene can also be used as the material used for the anode. In addition, by using a composite material capable of forming the hole injection layer 111 described later as a layer in contact with the anode (typically a hole injection layer), it becomes possible to select an electrode material regardless of the work function.
[0176] The hole injection layer 111 is provided in contact with the anode and has a function of facilitating injection of holes into the organic compound layer 103. The hole injection layer 111 can be formed of a phthalocyanine-based compound or complex compound such as phthalocyanine (abbreviation: HPc) or copper phthalocyanine (abbreviation: CuPc), an aromatic amine compound such as 4,4'-bis[N-(4-diphenylaminophenyl)-N-phenylamino]biphenyl (abbreviation: DPAB) or 4,4'-bis(N-{4-[N'-(3-methylphenyl)-N'-phenylamino]phenyl}-N-phenylamino)biphenyl (abbreviation: DNTPD), or a polymer such as poly(3,4-ethylenedioxythiophene) / (polystyrenesulfonic acid) (abbreviation: PEDOT / PSS).
[0177] The hole injection layer 111 may be formed of a substance having electron acceptor properties. As the substance having acceptor properties, an organic compound having an electron-withdrawing group (such as a halogen group or a cyano group) can be used, and examples of the substance include 7,7,8,8-tetracyano-2,3,5,6-tetrafluoroquinodimethane (abbreviation: F4-TCNQ), chloranil, 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene (abbreviation: HAT-CN), 1,3,4,5,7,8-hexafluorotetracyano-naphthoquinodimethane (abbreviation: F6-TCNNQ), 2-(7-dicyanomethylene-1,3,4,5,6,8,9,10-octafluoro-7H-pyren-2-ylidene)malononitrile, and the like. In particular, compounds in which an electron-withdrawing group is bonded to a condensed aromatic ring having multiple heteroatoms, such as HAT-CN, are thermally stable and preferred. Radialene derivatives having an electron-withdrawing group (especially a halogen group such as a fluoro group, a cyano group, etc.) [3] are preferred because they have a very high electron-accepting property, and specific examples thereof include α,α',α''-1,2,3-cyclopropane triylidene tris[4-cyano-2,3,5,6-tetrafluorobenzeneacetonitrile], α,α',α''-1,2,3-cyclopropane triylidene tris[2,6-dichloro-3,5-difluoro-4-(trifluoromethyl)benzeneacetonitrile], and α,α',α''-1,2,3-cyclopropane triylidene tris[2,3,4,5,6-pentafluorobenzeneacetonitrile]. As the substance having acceptor properties, in addition to the organic compounds described above, transition metal oxides such as molybdenum oxide, vanadium oxide, ruthenium oxide, tungsten oxide, and manganese oxide can be used.
[0178] The hole injection layer 111 is preferably formed of a composite material containing the above-mentioned material having an acceptor property and an organic compound having a hole transport property. The composite material may be the same as the composite material exemplified as a material capable of forming the P-type CGL in the embodiment 1.
[0179] By forming the hole injection layer 111, the hole injection property is improved, and a light emitting device with a low driving voltage can be obtained.
[0180] Among substances having acceptor properties, organic compounds having acceptor properties are easy to use because they can be easily evaporated and formed into a film.
[0181] The hole transport layer 112_1 and the hole transport layer 112_2 are formed by containing an organic compound having a hole transport property. -6 cm 2 It is preferable that the hole mobility is 1 / Vs or more.
[0182] Examples of the material having the hole transporting property include 4,4'-bis[N-(1-naphthyl)-N-phenylamino]biphenyl (abbreviation: NPB), N,N'-diphenyl-N,N'-bis(3-methylphenyl)-4,4'-diaminobiphenyl (abbreviation: TPD), N,N'-bis(9,9'-spirobi[9H-fluorene]-2-yl)-N,N'-diphenyl-4,4'-diaminobiphenyl (abbreviation: BSPB), 4-phenyl-4'-(9-phenylfluorene-9-yl)triphenylamine (abbreviation: BPAFLP), 4-phenyl-3'- (9-Phenylfluoren-9-yl)triphenylamine (abbreviation: mBPAFLP), 4-phenyl-4'-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBA1BP), 4,4'-diphenyl-4''-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBBi1BP), 4-(1-naphthyl)-4'-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBANB), 4,4'-di(1-naphthyl)-4''-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBANB), Compounds with aromatic amine skeletons such as 9,9-dimethyl-N-phenyl-N-[4-(9-phenyl-9H-carbazol-3-yl)phenyl]fluoren-2-amine (abbreviation: PCBAF), and N-phenyl-N-[4-(9-phenyl-9H-carbazol-3-yl)phenyl]-9,9'-spirobi[9H-fluorene]-2-amine (abbreviation: PCBASF), 1,3-bis(N-carbazolyl)benzene (abbreviation: mCP), 4,4'-di(N-carbazolyl)phenylamine (abbreviation: PCBNBB), 9,9-dimethyl-N-phenyl-N-[4-(9-phenyl-9H-carbazol-3-yl)phenyl]fluoren-2-amine (abbreviation: PCBAF), and 4,4'-di(N-carbazolyl)phenylamine (abbreviation: PCBASF) bazolyl)biphenyl (abbreviation: CBP), 3,6-bis(3,5-diphenylphenyl)-9-phenylcarbazole (abbreviation: CzTP), 9,9'-diphenyl-9H,9'H-3,3'-bicarbazole (abbreviation: PCCP), 9,9'-bis(biphenyl-4-yl)-3,3'-bi-9H-carbazole (abbreviation: BisBPCz), 9,9'-bis(biphenyl-3-yl)-3,3'-bi-9H-carbazole (abbreviation: BismBPCz), 9-(biphenyl-3-yl)-9'-(biphenyl-4-yl)-9H,9'H-3,3'-Bicarbazole (abbreviation: mBPCCBP), 9-(2-naphthyl)-9'-phenyl-9H,9'H-3,3'-bicarbazole (abbreviation: βNCCP), 9-(3-biphenyl)-9'-(2-naphthyl)-3,3'-bi-9H-carbazole (abbreviation: βNCCmBP), 9-(4-biphenyl)-9'-(2-naphthyl)-3,3'-bi-9H-carbazole (abbreviation: βNCCBP), 9,9'-di-2-naphthyl-3,3'-9H,9'H-bicarbazole (abbreviation: BisβNCz), 9-( 2-naphthyl)-9'-[1,1':4',1"-terphenyl]-3-yl-3,3'-9H,9'H-bicarbazole, 9-(2-naphthyl)-9'-[1,1':3',1"-terphenyl]-3-yl-3,3'-9H,9'H-bicarbazole, 9-(2-naphthyl)-9'-[1,1':3',1"-terphenyl]-5'-yl-3,3'-9H,9'H-bicarbazole, 9-(2-naphthyl)-9'-[1,1':4',1"-terphenyl]-4-yl-3,3'-9H,9'H- Bicarbazole, 9-(2-naphthyl)-9'-[1,1':3',1"-terphenyl]-4-yl-3,3'-9H,9'H-bicarbazole, 9-(2-naphthyl)-9'-(triphenylen-2-yl)-3,3'-9H,9'H-bicarbazole, 9-phenyl-9'-(triphenylen-2-yl)-3,3'-9H,9'H-bicarbazole (abbreviation: PCCzTp), 9,9'-bis(triphenylen-2-yl)-3,3'-9H,9'H-bicarbazole, 9-(4-biphenyl)- Compounds having a carbazole skeleton such as 9'-(triphenylen-2-yl)-3,3'-9H,9'H-bicarbazole, 9-(triphenylen-2-yl)-9'-[1,1':3',1”-terphenyl]-4-yl-3,3'-9H,9'H-bicarbazole, and 9-[4-(9-phenyl-9H-carbazol-3-yl)phenyl]phenanthrene (abbreviation: PCPPn), 4,4',4''-(benzene-1,3,5-triyl)tri(dibenzothiophene) (abbreviation: DBT3P-II), 2,Examples of the compounds include compounds having a thiophene skeleton such as 8-diphenyl-4-[4-(9-phenyl-9H-fluoren-9-yl)phenyl]dibenzothiophene (abbreviation: DBTFLP-III) and 4-[4-(9-phenyl-9H-fluoren-9-yl)phenyl]-6-phenyldibenzothiophene (abbreviation: DBTFLP-IV), and compounds having a furan skeleton such as 4,4',4''-(benzene-1,3,5-triyl)tri(dibenzofuran) (abbreviation: DBF3P-II) and 4-{3-[3-(9-phenyl-9H-fluoren-9-yl)phenyl]phenyl}dibenzofuran (abbreviation: mmDBFFLBi-II). Among the above, compounds having an aromatic amine skeleton and compounds having a carbazole skeleton are preferable because they have good reliability, high hole transportability, and contribute to reducing the driving voltage. Note that the substances exemplified as the materials having a hole transport property used for the composite material of the hole injection layer 111 can also be suitably used as materials for forming the hole transport layer 112_1 and the hole transport layer 112_2.
[0183] The light-emitting layer 113_1 and the light-emitting layer 113_2 are layers containing a light-emitting material, and preferably contain a light-emitting material and a host material. The light-emitting layer may contain other materials at the same time. Alternatively, the light-emitting layer may be a laminate of two layers having different compositions.
[0184] The luminescent material may be a fluorescent material, a phosphorescent material, a material exhibiting thermally activated delayed fluorescence (TADF), or any other luminescent material.
[0185] Examples of materials that can be used as the fluorescent substance in the light-emitting layer include the following: In addition, fluorescent substances other than these can also be used.
[0186] 5,6-bis[4-(10-phenyl-9-anthryl)phenyl]-2,2'-bipyridine (abbreviation: PAP2BPy), 5,6-bis[4'-(10-phenyl-9-anthryl)biphenyl-4-yl]-2,2'-bipyridine (abbreviation: PAPP2BPy), N,N'-diphenyl-N,N'-bis[4-(9-phenyl-9H-fluoren-9-yl)phenyl]pyrene-1,6-diamine (abbreviation: 1,6FLPAPrn), N,N'-bis(3-methylphenyl)-N,N'-bis[3-(9-phenyl-9H-fluoren-9-yl )phenyl]pyrene-1,6-diamine (abbreviation: 1,6mMemFLPAPrn), N,N'-bis[4-(9H-carbazol-9-yl)phenyl]-N,N'-diphenylstilbene-4,4'-diamine (abbreviation: YGA2S), 4-(9H-carbazol-9-yl)-4'-(10-phenyl-9-anthryl)triphenylamine (abbreviation: YGAPA), 4-(9H-carbazol-9-yl)-4'-(9,10-diphenyl-2-anthryl)triphenylamine (abbreviation: 2YGAPPA), N,9-diphenyl-N-[4-( 10-phenyl-9-anthryl)phenyl]-9H-carbazol-3-amine (abbreviation: PCAPA), perylene, 2,5,8,11-tetra-tert-butylperylene (abbreviation: TBP), 4-(10-phenyl-9-anthryl)-4'-(9-phenyl-9H-carbazol-3-yl)triphenylamine (abbreviation: PCBAPA), N,N''-(2-tert-butylanthracene-9,10-diyldi-4,1-phenylene)bis(N,N',N'-triphenyl-1,4-phenylenediamine) (abbreviation: DPABPA), N,9 -Diphenyl-N-[4-(9,10-diphenyl-2-anthryl)phenyl]-9H-carbazol-3-amine (abbreviation: 2PCAPPA), N-[4-(9,10-diphenyl-2-anthryl)phenyl]-N,N',N'-triphenyl-1,4-phenylenediamine (abbreviation: 2DPAPPA), N,N,N',N',N'',N'',N'''',N'''-octaphenyldibenzo[g,p]chrysene-2,7,10,15-tetraamine (abbreviation: DBC1), Coumarin 30, N-(9,10-diphenyl-2-anthryl)-N,9-Diphenyl-9H-carbazol-3-amine (abbreviation: 2PCAPA), N-[9,10-bis(biphenyl-2-yl)-2-anthryl]-N,9-diphenyl-9H-carbazol-3-amine (abbreviation: 2PCABPhA), N-(9,10-diphenyl-2-anthryl)-N,N',N'-triphenyl-1,4-phenylenediamine (abbreviation: 2DPAPA), N-[9,10-bis(biphenyl-2-yl)-2-anthryl]-N,N',N'-triphenyl-1,4-phenylenediamine (abbreviation: 2DPABPhA) , 9,10-bis(biphenyl-2-yl)-N-[4-(9H-carbazol-9-yl)phenyl]-N-phenylanthracen-2-amine (abbreviation: 2YGABPhA), N,N,9-triphenylanthracen-9-amine (abbreviation: DPhAPhA), Coumarin 545T, N,N'-diphenylquinacridone (abbreviation: DPQd), rubrene, 5,12-bis(biphenyl-4-yl)-6,11-diphenyltetracene (abbreviation: BPT), 2-(2-{2-[4-(dimethylamino)phenyl]ethenyl}-6-methyl-4H-pyrazol-2-yl)-1,1-diphenylquinacridone (abbreviation: DPQd), DCM1), 2-{2-methyl-6-[2-(2,3,6,7-tetrahydro-1H,5H-benzo[ij]quinolizin-9-yl)ethenyl]-4H-pyran-4-ylidene}propanedinitrile (DCM2), N,N,N',N'-tetrakis(4-methylphenyl)tetracene-5,11-diamine (p-mPhTD), 7,14-diphenyl-N,N,N',N'-tetrakis(4-methylphenyl)acenaphtho[1,2-a]fluoranthene-3,10-diamine (abbreviation Name: p-mPhAFD), 2-{2-isopropyl-6-[2-(1,1,7,7-tetramethyl-2,3,6,7-tetrahydro-1H,5H-benzo[ij]quinolizin-9-yl)ethenyl]-4H-pyran-4-ylidene}propanedinitrile (abbreviation: DCJTI), 2-{2-tert-butyl-6-[2-(1,1,7,7-tetramethyl-2,3,6,7-tetrahydro-1H,5H-benzo[ij]quinolizin-9-yl)ethenyl]-4H-pyran-4-ylidene}propanedinitrile (abbreviation: DCJTB),6-Bis{2-[4-(dimethylamino)phenyl]ethenyl}-4H-pyran-4-ylidene)propanedinitrile (abbreviation: BisDCM), 2-{2,6-bis[2-(8-methoxy-1,1,7,7-tetramethyl-2,3,6,7-tetrahydro-1H,5H-benzo[ij]quinolizin-9-yl)ethenyl]-4H-pyran-4-ylidene}propanedinitrile (abbreviation: BisDCJTM), N,N'-diphenyl-N,N'-(1,6-pyrene-diyl)bis[(6-phenylbenzo[b ]naphtho[1,2-d]furan)-8-amine] (abbreviation: 1,6BnfAPrn-03), 3,10-bis[N-(9-phenyl-9H-carbazol-2-yl)-N-phenylamino]naphtho[2,3-b;6,7-b']bisbenzofuran (abbreviation: 3,10PCA2Nbf(IV)-02), 3,10-bis[N-(dibenzofuran-3-yl)-N-phenylamino]naphtho[2,3-b;6,7-b']bisbenzofuran (abbreviation: 3,10FrA2Nbf(IV)-02), etc. In particular, condensed aromatic diamine compounds such as pyrene diamine compounds such as 1,6FLPAPrn, 1,6mMemFLPAPrn, and 1,6BnfAPrn-03 are preferred because they have high hole trapping properties and excellent luminous efficiency or reliability.
[0187] In addition, 5,9-diphenyl-5,9-diaza-13b-boranaphtho[3,2,1-de]anthracene (abbreviation: DABNA1), 9-(biphenyl-3-yl)-N,N,5,11-tetraphenyl-5H,9H-[1,4]benzazaborino[2,3,4-kl]phenazaborin-3-amine (abbreviation: DABNA2), 2,12-di(tert-butyl)-5,9-di(4-tert-butylphenyl)-N,N-diphenyl-5H,9H-[1,4]benzazaborino[2,3,4-kl]phenazaborin-7-amine (abbreviation: DABNA3), Amine (abbreviation: DPhA-tBu4DABNA), 2,12-di(tert-butyl)-N,N,5,9-tetra(4-tert-butylphenyl)-5H,9H-[1,4]benzazaborino[2,3,4-kl]phenazaborine-7-amine (abbreviation: tBuDPhA-tBu4DABNA), 2,12-di(tert-butyl)-5,9-di(4-tert-butylphenyl)-7-methyl-5H,9H-[1,4]benzazaborino[2,3,4-kl]phenazaborine (abbreviation: Me-tBu4DABNA), N 7 ,N 7 ,N 13 ,N 13 Condensed heteroaromatic compounds containing nitrogen and boron, such as 5,9,11,15-octaphenyl-5H,9H,11H,15H-[1,4]benzazaborino[2,3,4-kl][1,4]benzazaborino[4',3',2':4,5][1,4]benzazaborino[3,2-b]phenazaborine-7,13-diamine (abbreviation: ν-DABNA) and 2-(4-tert-butylphenyl)benz[5,6]indolo[3,2,1-jk]benzo[b]carbazole (abbreviation: tBuPBibc), in particular compounds having a diaza-boranaphtho-anthracene skeleton, can be suitably used because they have a narrow emission spectrum and can emit blue light with good color purity.
[0188] In addition to these, 9,10,11-tris[3,6-bis(1,1-dimethylethyl)-9H-carbazolyl-9-yl]-2,5,15,18-tetrakis(1,1-dimethylethyl)indolo[3,2,1-de]indolo[3',2',1':8,1][1,4]benzazaborino[2,3,4-kl]phenazaborine (abbreviation: BBCz-G), 9,11-bis[3,6-bis(1,1-dimethylethyl)-9H-carbazolyl-9-yl]-2,5,15,18-tetrakis(1,1-dimethylethyl)indolo[3,2,1-de]indolo[3',2',1':8,1][1,4]benzazaborino[2,3,4-kl]phenazaborine (abbreviation: BBCz-Y) and the like can be preferably used.
[0189] When a phosphorescent material is used as the light-emitting material in the light-emitting layer, examples of materials that can be used include the following.
[0190] Organometallic iridium compounds with a 4H-triazole skeleton, such as tris{2-[5-(2-methylphenyl)-4-(2,6-dimethylphenyl)-4H-1,2,4-triazol-3-yl-κN2]phenyl-κC}iridium(III) (abbreviation: [Ir(mpptz-dmp)3]) and tris(5-methyl-3,4-diphenyl-4H-1,2,4-triazolato)iridium(III) (abbreviation: [Ir(Mptz)3]). complexes, organometallic iridium complexes with 1H-triazole skeletons such as tris[3-methyl-1-(2-methylphenyl)-5-phenyl-1H-1,2,4-triazolato]iridium(III) (abbreviation: [Ir(Mptz1-mp)3]), tris(1-methyl-5-phenyl-3-propyl-1H-1,2,4-triazolato)iridium(III) (abbreviation: [Ir(Prptz1-Me)3]), fac-tris[1-( 2,6-diisopropylphenyl)-2-phenyl-1H-imidazole]iridium(III) (abbreviation: [Ir(iPrpim)3]), tris[3-(2,6-dimethylphenyl)-7-methylimidazo[1,2-f]phenanthridinato]iridium(III) (abbreviation: [Ir(dmpimpt-Me)3]), tris(2-{1-[2,6-bis(1-methylethyl)phenyl]-1H-imidazol-2-yl-κN3} organometallic iridium complexes with an imidazole skeleton, such as tris[(6-tert-butyl-3-phenyl-2H-imidazo[4,5-b]pyrazin-1-yl-κC2)phenyl-κC]iridium(III) (abbreviation: [Ir(cb)3]), and organometallic complexes with a benzimidazolidene skeleton, such as bis[2-(4',6'-difluorophenyl)pyridinato-N,C 2’ ]iridium(III) tetrakis(1-pyrazolyl)borate (abbreviation: FIr6), bis[2-(4',6'-difluorophenyl)pyridinato-N,C 2’ ]iridium(III) picolinate (abbreviation: FIrpic), bis{2-[3',5'-bis(trifluoromethyl)phenyl]pyridinato-N,C 2’}Iridium(III) picolinate (abbreviation: [Ir(CF3ppy)2(pic)]), bis[2-(4',6'-difluorophenyl)pyridinato-N,C 2’ ] Organometallic iridium complexes with phenylpyridine derivatives having electron-withdrawing groups as ligands, such as iridium(III) acetylacetonate (abbreviated as FIracac), are examples of such compounds that exhibit blue phosphorescence and have a peak emission wavelength in the range of 450 nm to 520 nm.
[0191] In addition, tris(4-methyl-6-phenylpyrimidinato)iridium(III) (abbreviation: [Ir(mppm)3]), tris(4-t-butyl-6-phenylpyrimidinato)iridium(III) (abbreviation: [Ir(tBuppm)3]), (acetylacetonato)bis(6-methyl-4-phenylpyrimidinato)iridium(III) (abbreviation: [Ir(mppm)2(acac)]), (acetylacetonato)bis(6-tert-butyl-4-phenylpyrimidinato)iridium(III) (abbreviation: [Ir(tBuppm)2(acac)]), (acetylacetonato)bis[6-(2-norbornyl)-4-phenylpyrimidinato]iridium(III) (abbreviation: [Ir(nbppm)2(acac)]), (acetylacetonato)bis[5-methyl-6- Organometallic iridium complexes having a pyrimidine skeleton, such as (2-methylphenyl)-4-phenylpyrimidinato]iridium(III) (abbreviation: [Ir(mpmppm)2(acac)]) and (acetylacetonato)bis(4,6-diphenylpyrimidinato)iridium(III) (abbreviation: [Ir(dppm)2(acac)]); organometallic iridium complexes having a pyrazine skeleton, such as (acetylacetonato)bis(3,5-dimethyl-2-phenylpyrazinato)iridium(III) (abbreviation: [Ir(mppr-Me)2(acac)]) and (acetylacetonato)bis(5-isopropyl-3-methyl-2-phenylpyrazinato)iridium(III) (abbreviation: [Ir(mppr-iPr)2(acac)]); 2’) Iridium(III) (abbreviation: [Ir(ppy)3]), bis(2-phenylpyridinato-N,C 2’ )iridium(III) acetylacetonate (abbreviation: [Ir(ppy)2(acac)]), bis(benzo[h]quinolinato)iridium(III) acetylacetonate (abbreviation: [Ir(bzq)2(acac)]), tris(benzo[h]quinolinato)iridium(III) (abbreviation: [Ir(bzq)3]), tris(2-phenylquinolinato-N,C 2’ ) Iridium(III) (abbreviation: [Ir(pq)3]), bis(2-phenylquinolinato-N,C 2’)iridium(III) acetylacetonate (abbreviation: [Ir(pq)2(acac)]), [2-d3-methyl-8-(2-pyridinyl-κN)benzofuro[2,3-b]pyridine-κC]bis[2-(5-d3-methyl-2-pyridinyl-κN2)phenyl-κC]iridium(III) (abbreviation: Ir(5mppy-d3)2(mbfpypy-d3)), [2-d3- Methyl-(2-pyridinyl-κN)benzofuro[2,3-b]pyridine-κC]bis[2-(2-pyridinyl-κN)phenyl-κC]iridium(III) (abbreviation: [Ir(ppy)2(mbfpypy-d3)]), [2-(4-d3-methyl-5-phenyl-2-pyridinyl-κN2)phenyl-κC]bis[2-(5-d3-methyl-2-pyridinyl-κN2)phenyl In addition to organometallic iridium complexes having a pyridine skeleton such as [2-methyl-(2-pyridinyl-κN)benzofuro[2,3-b]pyridine-κC]bis[2-(2-pyridinyl-κN)phenyl-κC]iridium(III) (abbreviation: [Ir(ppy)2(mbfpypy)]), [2-(4-methyl-5-phenyl-2-pyridinyl-κN)phenyl-κC]bis[2-(2-pyridinyl-κN)phenyl-κC]iridium (abbreviation: [Ir(ppy)2(mdppy)]), rare earth metal complexes such as tris(acetylacetonato)(monophenanthroline)terbium(III) (abbreviation: [Tb(acac)3(Phen)]) can be mentioned. These are compounds that mainly exhibit green phosphorescence and have emission peaks in the wavelength range of 500 nm to 600 nm. Note that organometallic iridium complexes having a pyrimidine skeleton are particularly preferred because they are remarkably excellent in reliability and luminous efficiency.
[0192] In addition, organometallic iridium complexes having a pyrimidine skeleton, such as (diisobutyrylmethanato)bis[4,6-bis(3-methylphenyl)pyrimidinato]iridium(III) (abbreviation: [Ir(5mdppm)2(dibm)]), bis[4,6-bis(3-methylphenyl)pyrimidinato](dipivaloylmethanato)iridium(III) (abbreviation: [Ir(5mdppm)2(dpm)]), and bis[4,6-di(naphthalen-1-yl)pyrimidinato](dipivaloylmethanato)iridium(III) (abbreviation: [Ir(d1npm)2(dpm)]); Organometallic iridium complexes with a pyrazine skeleton, such as (acetylacetonato)bis(2,3,5-triphenylpyrazinate)iridium(III) (abbreviation: [Ir(tppr)2(acac)]), bis(2,3,5-triphenylpyrazinate)(dipivaloylmethanato)iridium(III) (abbreviation: [Ir(tppr)2(dpm)]), and (acetylacetonato)bis[2,3-bis(4-fluorophenyl)quinoxalinato]iridium(III) (abbreviation: [Ir(Fdpq)2(acac)]), tris(1-phenylisoquinolinato-N,C 2’ ) Iridium(III) (abbreviation: [Ir(piq)3]), bis(1-phenylisoquinolinato-N,C 2’Organometallic iridium compounds with pyridine skeletons such as (3,7-diethyl-4,6-nonanedionato-κO4,κO6)bis[2,4-dimethyl-6-[7-(1-methylethyl)-1-isoquinolinyl-κN]phenyl-κC]iridium(III) and (3,7-diethyl-4,6-nonanedionato-κO4,κO6)bis[2,4-dimethyl-6-[5-(1-methylethyl)-2-quinolinyl-κN]phenyl-κC]iridium(III). In addition to iridium complexes, platinum complexes such as 2,3,7,8,12,13,17,18-octaethyl-21H,23H-porphyrin platinum(II) (abbreviation: PtOEP), tris(1,3-diphenyl-1,3-propanedionato)(monophenanthroline)europium(III) (abbreviation: [Eu(DBM)3(Phen)]), tris[1-(2-thenoyl)-3,3,3-trifluoroacetonato](monophenanthroline)europium(III) (abbreviation: [Eu(TTA)3(Phen)]) are examples of rare earth metal complexes. These are compounds that exhibit red phosphorescence and have a peak emission in the wavelength range from 600 nm to 700 nm. In addition, organometallic iridium complexes with a pyrazine skeleton can emit red light with good chromaticity.
[0193] In addition to the above-mentioned phosphorescent compounds, known phosphorescent compounds may be selected and used.
[0194] TADF materials include fullerene and its derivatives, acridine and its derivatives, eosin derivatives, etc. Also included are metal-containing porphyrins including magnesium (Mg), zinc (Zn), cadmium (Cd), tin (Sn), platinum (Pt), indium (In), palladium (Pd), etc. Examples of the metal-containing porphyrin include protoporphyrin-tin fluoride complex (SnF2(Proto IX)), mesoporphyrin-tin fluoride complex (SnF2(Meso IX)), hematoporphyrin-tin fluoride complex (SnF2(Hemato IX)), coproporphyrin tetramethyl ester-tin fluoride complex (SnF2(Copro III-4Me)), octaethylporphyrin-tin fluoride complex (SnF2(OEP)), etioporphyrin-tin fluoride complex (SnF2(Etio I)), and octaethylporphyrin-platinum chloride complex (PtCl2OEP), which are shown in the following structural formulas.
[0195] [ka]
[0196] In addition, 2-(biphenyl-4-yl)-4,6-bis(12-phenylindolo[2,3-a]carbazol-11-yl)-1,3,5-triazine (abbreviation: PIC-TRZ), 9-(4,6-diphenyl-1,3,5-triazin-2-yl)-9'-phenyl-9H,9'H-3,3'-bicarbazole (abbreviation: PCCzTzn), 2-{4-[3-(N-phenyl-9H-carbazol-3-yl)-9H-carbazol-9-yl]phenyl}-4,6-diphenyl-1,3,5-triazine (abbreviation: PCCzPTzn), 2-[4-(10H-phenoxazin-10-yl)phenyl]-4,6-diphenyl-1,3,5-triazine (abbreviation: PCCzPTzn), Heterocyclic compounds having one or both of a π-electron rich heteroaromatic ring and a π-electron deficient heteroaromatic ring, such as 3-[4-(5-phenyl-5,10-dihydrophenazin-10-yl)phenyl]-4,5-diphenyl-1,2,4-triazole (abbreviation: PPZ-3TPT), 3-(9,9-dimethyl-9H-acridin-10-yl)-9H-xanthen-9-one (abbreviation: ACRXTN), bis[4-(9,9-dimethyl-9,10-dihydroacridine)phenyl]sulfone (abbreviation: DMAC-DPS), and 10-phenyl-10H,10'H-spiro[acridin-9,9'-anthracene]-10'-one (abbreviation: ACRSA), can also be used. The heterocyclic compound has a π-electron rich heteroaromatic ring and a π-electron deficient heteroaromatic ring, and therefore has high electron transport and hole transport properties, and is therefore preferred. Among the skeletons having a π-electron deficient heteroaromatic ring, the pyridine skeleton, the diazine skeleton (pyrimidine skeleton, pyrazine skeleton, pyridazine skeleton), and the triazine skeleton are preferred because they are stable and reliable. In particular, the benzofuropyrimidine skeleton, the benzothienopyrimidine skeleton, the benzofuropyrazine skeleton, and the benzothienopyrazine skeleton are preferred because they have high acceptor properties and good reliability. In addition, among the skeletons having a π-electron rich heteroaromatic ring, the acridine skeleton, the phenoxazine skeleton, the phenothiazine skeleton, the furan skeleton, the thiophene skeleton, and the pyrrole skeleton are preferred because they are stable and reliable.In addition, the furan skeleton is preferably a dibenzofuran skeleton, and the thiophene skeleton is preferably a dibenzothiophene skeleton. In addition, the pyrrole skeleton is particularly preferably an indole skeleton, a carbazole skeleton, an indolocarbazole skeleton, a bicarbazole skeleton, or a 3-(9-phenyl-9H-carbazol-3-yl)-9H-carbazole skeleton. In addition, a substance in which a π-electron-rich heteroaromatic ring and a π-electron-deficient heteroaromatic ring are directly bonded is particularly preferable because the electron donating property of the π-electron-rich heteroaromatic ring and the electron accepting property of the π-electron-deficient heteroaromatic ring are both strong, and the energy difference between the S1 level and the T1 level is small, so that thermally activated delayed fluorescence can be efficiently obtained. In addition, an aromatic ring to which an electron-withdrawing group such as a cyano group is bonded may be used instead of the π-electron-deficient heteroaromatic ring. In addition, an aromatic amine skeleton, a phenazine skeleton, or the like can be used as the π-electron-rich skeleton. In addition, examples of the π-electron-deficient skeleton that can be used include a xanthene skeleton, a thioxanthene dioxide skeleton, an oxadiazole skeleton, a triazole skeleton, an imidazole skeleton, an anthraquinone skeleton, a boron-containing skeleton such as phenylborane or boranthrene, an aromatic ring having a nitrile group or a cyano group such as benzonitrile or cyanobenzene, a heteroaromatic ring, a carbonyl skeleton such as benzophenone, a phosphine oxide skeleton, a sulfone skeleton, etc. In this way, a π-electron-deficient skeleton and a π-electron-rich skeleton can be used in place of at least one of a π-electron-deficient heteroaromatic ring and a π-electron-rich heteroaromatic ring.
[0197] [ka]
[0198] TADF materials are materials that have a small difference between the S1 and T1 levels and have the function of converting triplet excitation energy to singlet excitation energy by reverse intersystem crossing. Therefore, triplet excitation energy can be upconverted to singlet excitation energy by a small amount of thermal energy (reverse intersystem crossing), and singlet excitation states can be generated efficiently. In addition, triplet excitation energy can be converted into light emission.
[0199] In addition, exciplexes (also called exciplexes), which form an excited state with two types of substances, have an extremely small difference between the S1 level and the T1 level and function as TADF materials that can convert triplet excitation energy into singlet excitation energy.
[0200] As an index of the T1 level, a phosphorescence spectrum observed at low temperatures (for example, 77 K to 10 K) may be used. For a TADF material, when a tangent line is drawn at the base of the short wavelength side of the fluorescence spectrum, and the energy of the wavelength of the extrapolated line is taken as the S1 level, and a tangent line is drawn at the base of the short wavelength side of the phosphorescence spectrum, and the energy of the wavelength of the extrapolated line is taken as the T1 level, the difference between S1 and T1 is preferably 0.3 eV or less, and more preferably 0.2 eV or less.
[0201] In addition, when a TADF material is used as a light-emitting material, the S1 level of the host material is preferably higher than the S1 level of the TADF material, and the T1 level of the host material is preferably higher than the T1 level of the TADF material.
[0202] As the host material of the light-emitting layer, various carrier transporting materials such as a material having an electron transporting property and / or a material having a hole transporting property, or the above-mentioned TADF material can be used.
[0203] As the material having hole transport properties, an organic compound having an amine skeleton, a π-electron-rich heteroaromatic ring skeleton, etc. is preferable. As the π-electron-rich heteroaromatic ring, a condensed aromatic ring containing at least one of an acridine skeleton, a phenoxazine skeleton, a phenothiazine skeleton, a furan skeleton, a thiophene skeleton, and a pyrrole skeleton in the ring is preferable, and specifically, a carbazole ring, a dibenzothiophene ring, or a ring in which an aromatic ring or a heteroaromatic ring is further condensed to the above is preferable.
[0204] Such organic compounds having hole transport properties preferably have any of a carbazole skeleton, a dibenzofuran skeleton, a dibenzothiophene skeleton, and an anthracene skeleton. In particular, the organic compounds may be aromatic amines having a substituent containing a dibenzofuran ring or a dibenzothiophene ring, aromatic monoamines having a naphthalene ring, or aromatic monoamines in which a 9-fluorenyl group is bonded to the nitrogen of the amine via an arylene group. It is preferable that the organic compounds having hole transport properties are substances having an N,N-bis(4-biphenyl)amino group, because this allows the manufacture of a light-emitting device with a long life.
[0205] Specifically, such organic compounds include the organic compounds cited as examples of materials having hole transport properties in the hole transport layer. Among them, compounds having an aromatic amine skeleton or a carbazole skeleton are preferable because they have good reliability, high hole transport properties, and contribute to reducing the driving voltage. In addition, it is preferable to use a compound having a bicarbazole skeleton and an aromatic hydrocarbon group, especially a naphthyl group, such as βNCCP, because it is possible to obtain a light-emitting device with good reliability. Note that the naphthyl group is preferably bonded to the nitrogen at the 9th position of at least one of the two carbazole skeletons.
[0206] As the material having electron transport properties, for example, a metal complex or an organic compound having a π-electron-deficient heteroaromatic ring is preferable. As the metal complex, bis(10-hydroxybenzo[h]quinolinato)beryllium(II) (abbreviation: BeBq2), bis(2-methyl-8-quinolinolato)(4-phenylphenolato)aluminum(III) (abbreviation: BAlq), bis(8-quinolinolato)zinc(II) (abbreviation: Znq), bis[2-(2-benzoxazolyl)phenolato]zinc(II) (abbreviation: ZnPBO), bis[2-(2-benzothiazolyl)phenolato]zinc(II) (abbreviation: ZnBTZ) and the like can be mentioned. Examples of organic compounds having a π-electron-deficient heteroaromatic ring skeleton include organic compounds containing a heteroaromatic ring having a polyazole skeleton, organic compounds containing a heteroaromatic ring having a pyridine skeleton, organic compounds containing a heteroaromatic ring having a diazine skeleton, and organic compounds containing a heteroaromatic ring having a triazine skeleton.
[0207] Among organic compounds having a π-electron-deficient heteroaromatic ring skeleton, organic compounds having a heteroaromatic ring with a diazine skeleton (pyrimidine skeleton, pyrazine skeleton, pyridazine skeleton), organic compounds having a heteroaromatic ring with a pyridine skeleton, and organic compounds having a heteroaromatic ring with a triazine skeleton are preferable because of their good reliability. In particular, organic compounds having a heteroaromatic ring with a diazine (pyrimidine or pyrazine) skeleton and organic compounds having a heteroaromatic ring with a triazine skeleton have high electron transport properties and contribute to reducing the driving voltage. In addition, benzofuropyrimidine skeleton, benzothienopyrimidine skeleton, benzofuropyrazine skeleton, and benzothienopyrazine skeleton are preferable because of their high acceptor properties and good reliability.
[0208] Specifically, as the material having an electron transporting property, it is possible to use the materials exemplified as the material having an electron transporting property that can be used for the first layer.
[0209] As a TADF material that can be used as a host material, the same TADF materials listed above can be used. When a TADF material is used as a host material, the triplet excitation energy generated in the TADF material is converted to singlet excitation energy by reverse intersystem crossing, and the energy is then transferred to the light-emitting material, thereby increasing the light-emitting efficiency of the light-emitting device. In this case, the TADF material functions as an energy donor, and the light-emitting material functions as an energy acceptor.
[0210] This is very effective when the luminescent material is a fluorescent luminescent material. In this case, in order to obtain high luminous efficiency, the S1 level of the TADF material is preferably higher than the S1 level of the fluorescent luminescent material. In addition, the T1 level of the TADF material is preferably higher than the S1 level of the fluorescent luminescent material. Therefore, the T1 level of the TADF material is preferably higher than the T1 level of the fluorescent luminescent material.
[0211] It is also preferable to use a TADF material that emits light that overlaps with the wavelength of the lowest energy absorption band of the fluorescent material, because this allows for smooth transfer of excitation energy from the TADF material to the fluorescent material, resulting in efficient emission.
[0212] In addition, in order to efficiently generate singlet excitation energy from triplet excitation energy by reverse intersystem crossing, it is preferable that carrier recombination occurs in the TADF material. In addition, it is preferable that the triplet excitation energy generated in the TADF material does not transfer to the triplet excitation energy of the fluorescent material. For this purpose, it is preferable that the fluorescent material has a protective group around the luminophore (skeleton causing light emission) of the fluorescent material. As the protective group, a substituent having no π bond is preferable, and a saturated hydrocarbon is preferable, specifically, an alkyl group having 3 to 10 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 10 carbon atoms, and a trialkylsilyl group having 3 to 10 carbon atoms are mentioned, and it is more preferable that there are a plurality of protective groups. Since a substituent having no π bond has poor function of transporting carriers, the distance between the TADF material and the luminophore of the fluorescent material can be increased without affecting carrier transport or carrier recombination. Here, the luminophore refers to an atomic group (skeleton) causing light emission in the fluorescent material. The luminophore preferably has a skeleton having a π bond, preferably contains an aromatic ring, and preferably has a condensed aromatic ring or a condensed heteroaromatic ring. Examples of such luminophore include a phenanthrene skeleton, a stilbene skeleton, an acridone skeleton, a phenoxazine skeleton, a phenothiazine skeleton, a naphthalene skeleton, an anthracene skeleton, a fluorene skeleton, a chrysene skeleton, a triphenylene skeleton, a tetracene skeleton, a pyrene skeleton, a perylene skeleton, a coumarin skeleton, a quinacridone skeleton, and a naphthobisbenzofuran skeleton. In particular, fluorescent substances having a naphthalene skeleton, an anthracene skeleton, a fluorene skeleton, a chrysene skeleton, a triphenylene skeleton, a tetracene skeleton, a pyrene skeleton, a perylene skeleton, a coumarin skeleton, a quinacridone skeleton, and a naphthobisbenzofuran skeleton are preferred because they have a high fluorescence quantum yield.
[0213] When a fluorescent emitting material is used as the emitting material, a material having an anthracene skeleton is suitable as the host material. When a material having an anthracene skeleton is used as the host material of the fluorescent emitting material, it is possible to realize an emitting layer having both good luminous efficiency and durability. As a material having an anthracene skeleton to be used as the host material, a material having a diphenylanthracene skeleton, particularly a 9,10-diphenylanthracene skeleton, is preferable because it is chemically stable. In addition, when the host material has a carbazole skeleton, it is preferable because the hole injection and transport properties are improved, but when it contains a benzocarbazole skeleton in which a benzene ring is further condensed to carbazole, the HOMO level is about 0.1 eV shallower than the carbazole skeleton, making it easier for holes to enter, which is more preferable. In particular, when the host material contains a dibenzocarbazole skeleton, it is preferable because the HOMO level is about 0.1 eV shallower than the carbazole skeleton, making it easier for holes to enter, and it also has excellent hole transport properties and high heat resistance. Therefore, a more preferable host material is a substance having both a 9,10-diphenylanthracene skeleton and a carbazole skeleton (or a benzocarbazole skeleton or a dibenzocarbazole skeleton). From the viewpoint of the hole injection / transport property, a benzofluorene skeleton or a dibenzofluorene skeleton may be used instead of the carbazole skeleton.Examples of such substances include 9-phenyl-3-[4-(10-phenyl-9-anthryl)phenyl]-9H-carbazole (abbreviation: PCzPA), 3-[4-(1-naphthyl)phenyl]-9-phenyl-9H-carbazole (abbreviation: PCPN), 9-[4-(10-phenyl-9-anthracenyl)phenyl]-9H-carbazole (abbreviation: CzPA), 7-[4-(10-phenyl-9-anthryl)phenyl]-7H-dibenzo[c,g]carbazole (abbreviation: cgDBCzPA), 6-[3-(9,10-diphenyl-2-anthryl)phenyl]benzo[b]naphtho[1,2-d]furan (abbreviation: 2mBnfPPA), 9-phenyl-10-[4-(9-phenyl-9H-fluoren-9-yl)biphenyl-4'- 9-(1-naphthyl)-10-[4-(2-naphthyl)phenyl]anthracene (abbreviation: αN-βNPAnth), 9-(1-naphthyl)-10-(2-naphthyl)anthracene (abbreviation: α,βADN), 2-(10-phenylanthracen-9-yl)dibenzofuran, 2-(10-phenyl-9-anthracenyl)benzo Zo[b]naphtho[2,3-d]furan (abbreviation: Bnf(II)PhA), 9-(2-naphthyl)-10-[3-(2-naphthyl)phenyl]anthracene (abbreviation: βN-mβNPAnth), 1-{4-[10-(biphenyl-4-yl)-9-anthracenyl]phenyl}-2-ethyl-1H-benzimidazole (abbreviation: EtBImPBPhA), etc. In particular, CzPA, cgDBCzPA, 2mBnfPPA, and PCzPA are preferred choices because they show very good properties.
[0214] The host material may be a mixture of a plurality of substances, and when a mixture of host materials is used, it is preferable to mix a material having an electron transporting property with a material having a hole transporting property. By mixing a material having an electron transporting property with a material having a hole transporting property, the transporting property of the light-emitting layer 113 can be easily adjusted, and the recombination region can be easily controlled. The weight ratio of the content of the material having a hole transporting property to the material having an electron transporting property is preferably 1:19 to 19:1 (material having a hole transporting property:material having an electron transporting property).
[0215] A phosphorescent material can be used as a part of the mixed material. The phosphorescent material can be used as an energy donor that provides excitation energy to a fluorescent material when the fluorescent material is used as a light-emitting material.
[0216] In addition, these mixed materials may form an exciplex. It is preferable to select a combination that forms an exciplex that emits light that overlaps with the wavelength of the lowest energy absorption band of the light-emitting material, because this makes energy transfer smooth and allows efficient light emission. In addition, the use of this structure is preferable because the driving voltage is reduced.
[0217] At least one of the materials forming the exciplex may be a phosphorescent material, which allows the triplet excitation energy to be efficiently converted into singlet excitation energy by reverse intersystem crossing.
[0218] As a combination of materials that efficiently form an exciplex, it is preferable that the HOMO level of the material having hole transport properties is equal to or higher than the HOMO level of the material having electron transport properties. It is also preferable that the LUMO level of the material having hole transport properties is equal to or higher than the LUMO level of the material having electron transport properties. The LUMO level and HOMO level of the material can be derived from the electrochemical properties (reduction potential and oxidation potential) of the material measured by cyclic voltammetry (CV) measurement.
[0219] The formation of an exciplex can be confirmed, for example, by comparing the emission spectrum of a material having hole transport properties, the emission spectrum of a material having electron transport properties, and the emission spectrum of a mixed film obtained by mixing these materials, and observing the phenomenon that the emission spectrum of the mixed film shifts to a longer wavelength than the emission spectrum of each material (or has a new peak on the longer wavelength side). Alternatively, the formation of an exciplex can be confirmed by comparing the transient photoluminescence (PL) of a material having hole transport properties, the transient PL of a material having electron transport properties, and the transient PL of a mixed film obtained by mixing these materials, and observing the difference in transient response, such as the transient PL lifetime of the mixed film having a longer lifetime component than the transient PL lifetime of each material, or the proportion of delayed components becoming larger. The above-mentioned transient PL may also be read as transient electroluminescence (EL). That is, the formation of an exciplex can also be confirmed by comparing the transient EL of a material having hole transport properties, the transient EL of a material having electron transport properties, and the transient EL of a mixed film obtained by mixing these materials, and observing the difference in transient response.
[0220] The electron transport layer 114_1 is the second layer 22, and has been described in detail in the first embodiment, so that a repeated description will be omitted.
[0221] The electron transport layer 114_2 is a layer containing a substance having an electron transport property. The material having an electron transport property is a material having an electron mobility of 1×10 -7 cm 2 / Vs or more, preferably 1×10 -6 cm 2 A substance having an electron mobility of 100 / Vs or more is preferable. Note that, other substances can be used as long as they have a higher transportability of electrons than holes. Note that, as the organic compound, an organic compound having a π-electron-deficient heteroaromatic ring is preferable. As the organic compound having a π-electron-deficient heteroaromatic ring, for example, it is preferable to use one or more of an organic compound having a heteroaromatic ring with a polyazole skeleton, an organic compound having a heteroaromatic ring with a pyridine skeleton, an organic compound having a heteroaromatic ring with a diazine skeleton, and an organic compound having a heteroaromatic ring with a triazine skeleton.
[0222] As the organic compound having electron transport properties that can be used in the electron transport layer 114_2, the organic compound that can be used as the organic compound having electron transport properties in the light emitting layer 113_1 and the light emitting layer 113_2 can be used in the same way. Among them, organic compounds containing a heteroaromatic ring having a diazine skeleton, organic compounds containing a heteroaromatic ring having a pyridine skeleton, and organic compounds containing a heteroaromatic ring having a triazine skeleton are preferable because they have good reliability. In particular, organic compounds containing a heteroaromatic ring having a diazine (pyrimidine or pyrazine) skeleton and organic compounds containing a heteroaromatic ring having a triazine skeleton have high electron transport properties and contribute to reducing the driving voltage. Among them, organic compounds having a phenanthroline skeleton such as mTpPPhen, PnNPhen, and mPPhen2P are preferable, and organic compounds having a phenanthroline dimer structure such as mPPhen2P are more preferable because they have excellent stability.
[0223] The electron transport layer 114_1 and the electron transport layer 114_2 may have a laminated structure. When the electron transport layer 114_1 has a laminated structure, the layer in contact with the first layer 21 becomes the second layer 22 and has the structure shown in the embodiment 1. The layer on the light-emitting layer 113_1 side may be formed using the material described as the material capable of forming the electron transport layer 114_2. When the electron transport layer 114_1 and the electron transport layer 114_2 have a laminated structure, the layer in contact with the light-emitting layer 113_1 and the light-emitting layer 113_2 may function as a hole blocking layer. When the electron transport layer in contact with the light-emitting layer is made to function as a hole blocking layer, it is preferable to use a material whose HOMO level is deeper than the HOMO level of the material contained in the light-emitting layer by 0.5 eV or more.
[0224] Between the electron transport layer 114_2 and the cathode 102, a layer containing an alkali metal or an alkaline earth metal, or a compound thereof, such as lithium oxide (Li2O), lithium fluoride (LiF), cesium fluoride (CsF), calcium fluoride (CaF2), or 8-hydroxyquinolinato-lithium (abbreviation: Liq), may be provided as the electron injection layer 115. The electron injection layer 115 may be a layer made of a substance having an electron transport property containing an alkali metal or an alkaline earth metal, or a compound thereof, or an electride may be used. For example, an electride may be a substance in which electrons are added to a mixed oxide of calcium and aluminum at a high concentration. In addition, the organic compounds listed as organic compounds having a strong basicity in the first embodiment may also be used.
[0225] The electron-injecting layer 115 may use any of the above substances alone, or may contain any of the above substances in a layer made of a substance having an electron-transporting property.
[0226] Note that a layer containing a fluoride of the alkali metal or alkaline earth metal in a substance having an electron transporting property (preferably an organic compound having a bipyridine skeleton) at a concentration at which the fluoride is in a microcrystalline state or higher (50 wt % or higher) can be used as the electron injection layer 115. Since this layer has a low refractive index, it is possible to provide a light-emitting device with better external quantum efficiency.
[0227] The cathode 102 may have a laminated structure, and in that case, the layer in contact with the organic compound layer 103 substantially functions as the cathode. As a material for forming the cathode, a metal, an alloy, an electrically conductive compound, a mixture thereof, or the like having a small work function (specifically, 3.8 eV or less) can be used. Specific examples of such cathode materials include alkali metals such as lithium (Li) or cesium (Cs), elements belonging to Group 1 or Group 2 of the periodic table such as magnesium (Mg), calcium (Ca), and strontium (Sr), and alloys (MgAg, AlLi) and compounds (lithium fluoride (LiF), cesium fluoride (CsF), calcium fluoride (CaF2), etc.) containing these, rare earth metals such as europium (Eu), ytterbium (Yb), and alloys containing these, etc. However, by providing the electron injection layer 115 or a thin film of the above-mentioned material having a small work function between the cathode 102 and the electron transport layer, various conductive materials such as Al, Ag, ITO, indium oxide-tin oxide containing silicon or silicon oxide can be used as the cathode regardless of the magnitude of the work function.
[0228] When the cathode 102 is made of a material transparent to visible light, the light-emitting device can emit light from the cathode 102 side, and when the anode 101 is made of a material transparent to visible light, the light-emitting device can emit light from the anode 101 side.
[0229] These conductive materials can be formed into a film by a dry method such as a vacuum deposition method or a sputtering method, an inkjet method, a spin coating method, etc. Also, they may be formed by a wet method using a sol-gel method, or may be formed by a wet method using a paste of a metal material.
[0230] In addition, various methods can be used for forming the organic compound layer 103, regardless of whether it is a dry method or a wet method. For example, a vacuum deposition method, a gravure printing method, an offset printing method, a screen printing method, an inkjet method, a spin coating method, or the like may be used.
[0231] Moreover, the above-mentioned electrodes or layers may be formed using different film formation methods.
[0232] 6, a light-emitting device having two light-emitting units has been described, but the present invention can be applied to a light-emitting device having three or more light-emitting units stacked together. As in the light-emitting device according to the present embodiment, by disposing a plurality of light-emitting units between a pair of electrodes and separating them with an intermediate layer 513, it is possible to realize an element that can emit light with high luminance while keeping the current density low and has a long life. In addition, it is possible to realize a light-emitting device that can be driven at a low voltage and consumes low power.
[0233] In addition, by making the emission colors of the respective light-emitting units different, it is possible to obtain light emission of a desired color from the light-emitting device as a whole. For example, in a light-emitting device having two light-emitting units, it is possible to obtain a light-emitting device that emits white light as a whole by obtaining red and green emission colors from the first light-emitting unit and blue emission color from the second light-emitting unit.
[0234] Each layer and electrode, such as the organic compound layer 103, the first light-emitting unit 501, the second light-emitting unit 502, and the intermediate layer 513, can be formed by using, for example, a deposition method (including a vacuum deposition method), a droplet discharge method (also called an ink-jet method), a coating method, a gravure printing method, etc. They may also include a low molecular weight material, a medium molecular weight material (including an oligomer and a dendrimer), or a polymer material.
[0235] FIG. 7 shows two adjacent tandem-type light-emitting elements (light-emitting device 130c, light-emitting device 130d) fabricated by photolithography.
[0236] The light-emitting device 130c has an organic compound layer 103c between an anode 101c and a cathode 102 on a substrate 1000. The organic compound layer 103c has a structure in which a first light-emitting unit 501c and a second light-emitting unit 502c are laminated with an intermediate layer 513c sandwiched therebetween. Although an example in which two light-emitting units are laminated is shown in FIG. 7, a structure in which three or more light-emitting units are laminated may also be used. The first light-emitting unit 501c has a hole injection layer 111c, a hole transport layer 112c_1, a light-emitting layer 113c_1, and an electron transport layer 114c_1 (second layer 22c). The intermediate layer 513c has a P-type CGL 20c, a third layer 23c, and a first layer 21c. The third layer 23c may or may not be present. The second light-emitting unit 502c includes a hole-transporting layer 112c_2, a light-emitting layer 113c_2, an electron-transporting layer 114c_2, and an electron-injecting layer 115.
[0237] The light-emitting device 130d has an organic compound layer 103d between an anode 101d and a cathode 102 on a substrate 1000. The organic compound layer 103d has a structure in which a first light-emitting unit 501d and a second light-emitting unit 502d are laminated with an intermediate layer 513d sandwiched therebetween. Although an example in which two light-emitting units are laminated is shown in FIG. 7, a structure in which three or more light-emitting units are laminated may also be used. The first light-emitting unit 501d has a hole injection layer 111d, a hole transport layer 112d_1, a light-emitting layer 113d_1, and an electron transport layer 114d_1 (second layer 22d). The intermediate layer 513d has a P-type CGL 20d, a third layer 23d, and a first layer 21d. The third layer 23d may or may not be present. The second light-emitting unit 502d includes a hole-transporting layer 112d_2, a light-emitting layer 113d_2, an electron-transporting layer 114d_2, and an electron-injecting layer 115.
[0238] In light emitting device 130c and light emitting device 130d, intermediate layer 513c and intermediate layer 513d, and second layer 22c and second layer 22d preferably have the configurations as described in the first embodiment.
[0239] It is preferable that the electron injection layer 115 and the cathode 102 are a continuous layer shared by the light-emitting device 130c and the light-emitting device 130d. The organic compound layer 103c and the organic compound layer 103d other than the electron injection layer 115 are processed by photolithography after the electron transport layer 114c_2 and the electron transport layer 114d_2 are formed, respectively, and are therefore independent of each other. The end (outline) of the organic compound layer 103c other than the electron injection layer 115 is processed by photolithography, so that it roughly coincides with the direction perpendicular to the substrate. The end (outline) of the organic compound layer 103d other than the electron injection layer 115 is processed by photolithography, so that it roughly coincides with the direction perpendicular to the substrate.
[0240] In addition, since the organic compound layer 103c and the organic compound layer 103d are processed by photolithography, a gap d exists between the organic compound layer 103c and the organic compound layer 103d. In addition, since the organic compound layer is processed by photolithography, the distance between the anode 101c and the anode 101d can be made smaller than that in the case of performing mask deposition, and can be set to 2 μm or more and 5 μm or less.
[0241] (Embodiment 4) In this embodiment, a mode in which a light-emitting device of one embodiment of the present invention is used as a display element of a display device will be described.
[0242] As shown in FIGS. 8A and 8B, a plurality of light emitting devices 130 are formed on an insulating layer 175 to constitute a display device.
[0243] The display device has a pixel portion 177 in which a plurality of pixels 178 are arranged in a matrix. The pixel 178 has a sub-pixel 110R, a sub-pixel 110G, and a sub-pixel 110B.
[0244] In this specification and the like, when describing matters common to, for example, the subpixels 110R, 110G, and 110B, they may be referred to as subpixels 110. When describing matters common to other components distinguished by alphabets, they may be described using symbols without the alphabets.
[0245] The sub-pixel 110R emits red light, the sub-pixel 110G emits green light, and the sub-pixel 110B emits blue light. This allows an image to be displayed in the pixel section 177. In the present embodiment, sub-pixels of three colors, red (R), green (G), and blue (B), are described as an example, but combinations of sub-pixels of other colors may be used. The number of sub-pixels is not limited to three, and may be four or more. Examples of the four sub-pixels include sub-pixels of four colors, R, G, B, and white (W), sub-pixels of four colors, R, G, B, and yellow (Y), and sub-pixels of R, G, B, and infrared (IR).
[0246] In this specification and the like, the row direction may be referred to as the X direction, and the column direction may be referred to as the Y direction. The X direction and the Y direction intersect, for example, perpendicularly.
[0247] 8A shows an example in which subpixels of different colors are arranged side by side in the X direction, and subpixels of the same color are arranged side by side in the Y direction. Note that subpixels of different colors may be arranged side by side in the Y direction, and subpixels of the same color may be arranged side by side in the X direction.
[0248] A connection portion 140 and a region 141 may be provided outside the pixel portion 177. The region 141 is provided between the pixel portion 177 and the connection portion 140. The region 141 is provided with an organic compound layer 103. In addition, the connection portion 140 is provided with a conductive layer 151C.
[0249] 8A shows an example in which the region 141 and the connection portion 140 are located on the right side of the pixel portion 177, but the positions of the region 141 and the connection portion 140 are not particularly limited. The region 141 and the connection portion 140 may be singular or plural.
[0250] Fig. 8(B) is an example of a cross-sectional view between dashed line A1-A2 in Fig. 8(A). As shown in Fig. 8(B), the display device has an insulating layer 171, a conductive layer 172 on the insulating layer 171, an insulating layer 173 on the insulating layer 171 and on the conductive layer 172, an insulating layer 174 on the insulating layer 173, and an insulating layer 175 on the insulating layer 174. The insulating layer 171 is provided on a substrate (not shown). An opening reaching the conductive layer 172 is provided in the insulating layer 175, the insulating layer 174, and the insulating layer 173, and a plug 176 is provided to fill the opening.
[0251] In the pixel section 177, the light emitting device 130 is provided on the insulating layer 175 and the plug 176. A protective layer 131 is provided so as to cover the light emitting device 130. The substrate 120 is bonded onto the protective layer 131 by a resin layer 122. In addition, an inorganic insulating layer 125 and an insulating layer 127 on the inorganic insulating layer 125 are preferably provided between adjacent light emitting devices 130.
[0252] 8B shows multiple cross sections of the inorganic insulating layer 125 and the insulating layer 127, it is preferable that the inorganic insulating layer 125 and the insulating layer 127 are connected to one another when the display device is viewed from above. In other words, it is preferable that the inorganic insulating layer 125 and the insulating layer 127 are insulating layers having an opening over the first electrode.
[0253] In FIG. 8B, the light emitting device 130 includes a light emitting device 130R, a light emitting device 130G, and a light emitting device 130B. The light emitting device 130R, the light emitting device 130G, and the light emitting device 130B emit light of different colors. For example, the light emitting device 130R can emit red light, the light emitting device 130G can emit green light, and the light emitting device 130B can emit blue light. The light emitting device 130R, the light emitting device 130G, or the light emitting device 130B may emit other visible light or infrared light.
[0254] The display device of one embodiment of the present invention can be, for example, a top emission type that emits light in a direction opposite to a substrate on which a light-emitting device is formed. Note that the display device of one embodiment of the present invention may be a bottom emission type.
[0255] The light-emitting device 130R has the configuration shown in the first to third embodiments. The light-emitting device 130R has an anode 101R (pixel electrode) composed of a conductive layer 151R and a conductive layer 152R, a first EL layer 104R on the anode 101R, a second EL layer 105 on the first EL layer 104R, and a cathode 102 (common electrode) on the second EL layer 105. The second EL layer 105 is preferably located closer to the cathode 102 (common electrode) than the light-emitting layer closest to the cathode, and is preferably a hole blocking layer, a second electron transport layer, an electron injection layer, or a laminate of these. In the light-emitting device 130R, the layer formed by combining the first EL layer 104R and the second EL layer 105 becomes an organic compound layer 103R, which corresponds to the organic compound layer 103 in the first to third embodiments.
[0256] The light-emitting device 130G has the configuration shown in the first to third embodiments. The light-emitting device 130G has an anode 101G (pixel electrode) composed of a conductive layer 151G and a conductive layer 152G, a first EL layer 104G on the anode 101G, a second EL layer 105 on the first EL layer 104G, and a cathode 102 (common electrode) on the second EL layer 105. The second EL layer 105 is preferably located closer to the cathode 102 (common electrode) than the light-emitting layer closest to the cathode, and is preferably a hole blocking layer, a second electron transport layer, an electron injection layer, or a laminate of these. In the light-emitting device 130G, the layer formed by combining the first EL layer 104G and the second EL layer 105 is an organic compound layer 103G, which corresponds to the organic compound layer 103 in the first to third embodiments.
[0257] The light-emitting device 130B has the configuration shown in the first to third embodiments. It has an anode 101B (pixel electrode) consisting of a conductive layer 151B and a conductive layer 152B, a first EL layer 104B on the anode 101B, a second EL layer 105 on the first EL layer 104B, and a cathode 102 (common electrode) on the second EL layer 105. The second EL layer 105 is preferably located closer to the cathode 102 (common electrode) than the light-emitting layer closest to the cathode, and is preferably a hole blocking layer, a second electron transport layer, an electron injection layer, or a laminate of these. In the light-emitting device 130B, the layer formed by combining the first EL layer 104B and the second EL layer 105 becomes an organic compound layer 103B, which corresponds to the organic compound layer 103 in the first to third embodiments.
[0258] One of a pixel electrode (first electrode) and a common electrode (second electrode) of a light-emitting device functions as an anode, and the other functions as a cathode. In this embodiment, unless otherwise specified, the pixel electrode functions as an anode, and the common electrode functions as a cathode.
[0259] The first EL layer 104R, the first EL layer 104G, and the first EL layer 104B are independent in an island shape, or for each luminescent color. It is preferable that the first EL layer 104R, the first EL layer 104G, and the first EL layer 104B do not overlap each other. By providing the first EL layer 104 in an island shape for each light-emitting device 130, it is possible to suppress leakage current between adjacent light-emitting devices 130 even in a high-definition display device. This makes it possible to prevent crosstalk and realize a display device with extremely high contrast. In particular, it is possible to realize a display device with high current efficiency at low luminance.
[0260] The island-shaped first EL layer 104 can be formed by forming an EL film and processing the EL film by photolithography. Since the light-emitting device according to one embodiment of the present invention does not use a Li compound or the like in the intermediate layer, a light-emitting device with good characteristics can be obtained even when the light-emitting device is processed by photolithography.
[0261] The first EL layer 104 is preferably provided so as to cover the upper surface and side surfaces of the anode 101 (pixel electrode) of the light-emitting device 130. This makes it easier to increase the aperture ratio of the display device compared to a configuration in which the end of the first EL layer 104 is located inside the end of the pixel electrode. In addition, covering the side surfaces of the pixel electrode of the light-emitting device 130 with the first EL layer 104 can prevent the pixel electrode and the cathode 102 from coming into contact with each other, thereby preventing short circuits in the light-emitting device 130.
[0262] In the display device of one embodiment of the present invention, the anode 101 (pixel electrode) of the light-emitting device preferably has a stacked structure. For example, in the example shown in FIG. 8B, the anode 101 of the light-emitting device 130 has a stacked structure of a conductive layer 151 provided on the insulating layer 171 side and a conductive layer 152 provided on the organic compound layer side.
[0263] For example, a metal material can be used as the conductive layer 151. Specifically, metals such as aluminum (Al), titanium (Ti), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), gallium (Ga), zinc (Zn), indium (In), tin (Sn), molybdenum (Mo), tantalum (Ta), tungsten (W), palladium (Pd), gold (Au), platinum (Pt), silver (Ag), yttrium (Y), neodymium (Nd), and alloys containing appropriate combinations of these metals can also be used.
[0264] The conductive layer 152 can be made of an oxide containing one or more selected from indium, tin, zinc, gallium, titanium, aluminum, and silicon. For example, it is preferable to use a conductive oxide containing one or more of indium oxide, indium tin oxide, indium zinc oxide, zinc oxide, zinc oxide containing gallium, titanium oxide, indium zinc oxide containing gallium, indium zinc oxide containing aluminum, indium tin oxide containing silicon, and indium zinc oxide containing silicon. In particular, indium tin oxide containing silicon has a large work function, for example, a work function of 4.0 eV or more, and therefore can be suitably used for the conductive layer 152.
[0265] The conductive layer 151 may have a stacked structure of multiple layers having different materials, and the conductive layer 152 may have a stacked structure of multiple layers having different materials. In this case, the conductive layer 151 may have a layer using a material that can be used for the conductive layer 152, such as a conductive oxide, or the conductive layer 152 may have a layer using a material that can be used for the conductive layer 151, such as a metal material. For example, when the conductive layer 151 has a stacked structure of two or more layers, a layer in contact with the conductive layer 152 can be a layer using a material that can be used for the conductive layer 152.
[0266] Note that the conductive layer 151 preferably has a tapered end. Specifically, the conductive layer 151 preferably has a tapered end with a taper angle of less than 90°. In this case, the conductive layer 152 provided along the side surface of the conductive layer 151 also has a tapered end. By making the side surface of the conductive layer 152 tapered, the coverage of the first EL layer 104 provided along the side surface of the conductive layer 152 can be improved.
[0267] In the display device of one embodiment of the present invention, the light-emitting device 130 has the structure described in any of Embodiments 1 to 3, and thus the display device can have favorable characteristics in which an increase in driving voltage is suppressed.
[0268] Next, an example of a method for manufacturing a display device having the structure shown in FIG. 8A will be described with reference to FIGS.
[0269] [Production method example 1] The thin films (insulating films, semiconductor films, conductive films, etc.) that make up the display device can be formed using a sputtering method, a chemical vapor deposition (CVD) method, a vacuum deposition method, a pulsed laser deposition (PLD) method, an atomic layer deposition (ALD) method, or the like.
[0270] Furthermore, the thin films (insulating films, semiconductor films, conductive films, etc.) constituting the display device can be formed by wet film formation methods such as spin coating, dipping, spray coating, inkjet, dispensing, screen printing, offset printing, doctor knife method, slit coating, roll coating, curtain coating, or knife coating.
[0271] Furthermore, when processing the thin films that constitute the display device, they can be processed using, for example, a photolithography method.
[0272] In the photolithography method, the light used for exposure may be, for example, i-line (wavelength 365 nm), g-line (wavelength 436 nm), h-line (wavelength 405 nm), or a mixture of these. In addition, ultraviolet light, KrF laser light, ArF laser light, etc. may also be used. Exposure may also be performed by immersion exposure technology. Extreme ultraviolet (EUV) light or X-rays may also be used as the light used for exposure. An electron beam may also be used instead of the light used for exposure.
[0273] The thin film can be etched by dry etching, wet etching, sandblasting, or the like.
[0274] 9(A), an insulating layer 171 is formed on a substrate (not shown). Then, a conductive layer 172 and a conductive layer 179 are formed on the insulating layer 171, and an insulating layer 173 is formed on the insulating layer 171 so as to cover the conductive layer 172 and the conductive layer 179. Then, an insulating layer 174 is formed on the insulating layer 173, and an insulating layer 175 is formed on the insulating layer 174.
[0275] The substrate may be a substrate having at least a heat resistance sufficient to withstand a subsequent heat treatment, such as a glass substrate, a quartz substrate, a sapphire substrate, a ceramic substrate, an organic resin substrate, a single crystal semiconductor substrate made of silicon, silicon carbide, or the like, a polycrystalline semiconductor substrate, a compound semiconductor substrate made of silicon germanium, or the like, or an SOI substrate.
[0276] 9A, an opening reaching the conductive layer 172 is formed in the insulating layer 175, the insulating layer 174, and the insulating layer 173. Then, a plug 176 is formed to fill the opening.
[0277] 9A, a conductive film 151f, which will later become the conductive layers 151R, 151G, 151B, and 151C, is formed on the plugs 176 and the insulating layer 175. The conductive film 151f can be made of, for example, a metal material.
[0278] 9A, a resist mask 191 is formed over the conductive film 151f. The resist mask 191 can be formed by applying a photosensitive material (photoresist) and then performing exposure and development.
[0279] 9B, for example, the conductive film 151f is removed from a region that does not overlap with the resist mask 191. In this way, the conductive layer 151 is formed.
[0280] 9C, the resist mask 191 is removed. The resist mask 191 can be removed by ashing using oxygen plasma, for example.
[0281] Next, as shown in FIG. 9(D), insulating film 156f, which will later become insulating layer 156R, insulating layer 156G, insulating layer 156B, and insulating layer 156C, is formed on conductive layer 151R, conductive layer 151G, conductive layer 151B, conductive layer 151C, and insulating layer 175.
[0282] The insulating film 156f can be an inorganic insulating film such as an insulating oxide film, a nitride insulating film, an oxynitride insulating film, or a nitride oxide insulating film, for example, a silicon oxynitride film.
[0283] Subsequently, as shown in FIG. 9(E), the insulating film 156f is processed to form an insulating layer 156R, an insulating layer 156G, an insulating layer 156B, and an insulating layer 156C.
[0284] Next, as shown in FIG. 10(A), a conductive film 152f is formed on the conductive layer 151R, the conductive layer 151G, the conductive layer 151B, the conductive layer 151C, the insulating layer 156R, the insulating layer 156G, the insulating layer 156B, the insulating layer 156C, and the insulating layer 175.
[0285] The conductive film 152f may be, for example, a conductive oxide, or may be a multilayer film.
[0286] Subsequently, as shown in FIG. 10B, the conductive film 152f is processed to form a conductive layer 152R, a conductive layer 152G, a conductive layer 152B, and a conductive layer 152C.
[0287] 10(C), the organic compound film 103Rf is formed on the conductive layer 152R, the conductive layer 152G, the conductive layer 152B, and the insulating layer 175. Note that, as shown in FIG. 10(C), the organic compound film 103Rf is not formed on the conductive layer 152C.
[0288] Subsequently, as shown in FIG. 10(C), a sacrificial film 158Rf and a mask film 159Rf are formed.
[0289] By providing the sacrificial film 158Rf on the organic compound film 103Rf, damage to the organic compound film 103Rf during the manufacturing process of the display device can be reduced, and the reliability of the light-emitting device can be improved.
[0290] The sacrificial film 158Rf is made of a film having high resistance to the processing conditions of the organic compound film 103Rf, specifically, a film having a high etching selectivity with respect to the organic compound film 103Rf. The mask film 159Rf is made of a film having a high etching selectivity with respect to the sacrificial film 158Rf.
[0291] The sacrificial film 158Rf and the mask film 159Rf are formed at a temperature lower than the heat-resistant temperature of the organic compound film 103Rf. The substrate temperature when forming the sacrificial film 158Rf and the mask film 159Rf is typically 100° C. or higher and 200° C. or lower, preferably 100° C. or higher and 150° C. or lower, and more preferably 100° C. or higher and 120° C. or lower.
[0292] The sacrificial film 158Rf and the mask film 159Rf are preferably made of a film that can be removed by wet etching or dry etching.
[0293] In addition, the sacrificial film 158Rf formed on and in contact with the organic compound film 103Rf is preferably formed using a formation method that causes less damage to the organic compound film 103Rf than the mask film 159Rf. For example, the ALD method or the vacuum deposition method is more preferable than the sputtering method.
[0294] The sacrificial film 158Rf and the mask film 159Rf may each be made of one or more of a metal film, an alloy film, a metal oxide film, a semiconductor film, an organic insulating film, and an inorganic insulating film, for example.
[0295] The sacrificial film 158Rf and the mask film 159Rf may be made of, for example, a metal material such as gold, silver, platinum, magnesium, nickel, tungsten, chromium, molybdenum, iron, cobalt, copper, palladium, titanium, aluminum, yttrium, zirconium, or tantalum, or an alloy material containing the metal material. In particular, it is preferable to use a low melting point material such as aluminum or silver. It is preferable to use a metal material capable of blocking ultraviolet rays for one or both of the sacrificial film 158Rf and the mask film 159Rf, since it is possible to suppress irradiation of ultraviolet rays during pattern exposure to the organic compound film 103Rf, and thus to suppress deterioration of the organic compound film 103Rf.
[0296] Furthermore, for the sacrificial film 158Rf and the mask film 159Rf, metal oxides such as In-Ga-Zn oxide, indium oxide, In-Zn oxide, In-Sn oxide, indium titanium oxide (In-Ti oxide), indium tin zinc oxide (In-Sn-Zn oxide), indium titanium zinc oxide (In-Ti-Zn oxide), indium gallium tin zinc oxide (In-Ga-Sn-Zn oxide), and indium tin oxide containing silicon can be used.
[0297] In addition, in the above metal oxide, an element M (M is one or more elements selected from aluminum, silicon, boron, yttrium, copper, vanadium, beryllium, titanium, iron, nickel, germanium, zirconium, molybdenum, lanthanum, cerium, neodymium, hafnium, tantalum, tungsten, and magnesium) may be used instead of gallium.
[0298] For the sacrificial film 158Rf and the mask film 159Rf, it is preferable to use a semiconductor material such as silicon or germanium because it has a high affinity with the semiconductor manufacturing process, or a compound containing the above semiconductor material may be used.
[0299] Moreover, various inorganic insulating films can be used as the sacrificial film 158Rf and the mask film 159Rf, respectively. In particular, an oxide insulating film is preferable because it has higher adhesion to the organic compound film 103Rf than a nitride insulating film.
[0300] 10(C), a resist mask 190R is formed. The resist mask 190R can be formed by applying a photosensitive material (photoresist) and then performing exposure and development.
[0301] The resist mask 190R is provided in a position overlapping with the conductive layer 152R. The resist mask 190R is preferably provided also in a position overlapping with the conductive layer 152C, which can prevent the conductive layer 152C from being damaged during the manufacturing process of the display device.
[0302] 10(D), a resist mask 190R is used to remove a portion of the mask film 159Rf to form a mask layer 159R. The mask layer 159R remains on the conductive layer 152R and the conductive layer 152C. The resist mask 190R is then removed. The mask layer 159R is then used as a mask (also called a hard mask) to remove a portion of the sacrificial film 158Rf to form a sacrificial layer 158R.
[0303] By using the wet etching method, damage to the organic compound film 103Rf during processing of the sacrificial film 158Rf and the mask film 159Rf can be reduced compared to the case of using the dry etching method. When using the wet etching method, it is preferable to use an acid aqueous solution such as a developing solution, an alkaline aqueous solution such as a tetramethylammonium hydroxide (TMAH) aqueous solution, a chemical solution using dilute hydrofluoric acid, oxalic acid, phosphoric acid, acetic acid, nitric acid, or a mixture of these.
[0304] Furthermore, when dry etching is used in processing the sacrificial film 158Rf, deterioration of the organic compound film 103Rf can be suppressed by not using an oxygen-containing gas as an etching gas.
[0305] The resist mask 190R can be removed in the same manner as the resist mask 191.
[0306] 10(D), the organic compound film 103Rf is processed to form the organic compound layer 103R. For example, the mask layer 159R and the sacrificial layer 158R are used as a hard mask to remove a part of the organic compound film 103Rf to form the organic compound layer 103R.
[0307] 10D, a laminated structure of the organic compound layer 103R, the sacrificial layer 158R, and the mask layer 159R remains on the conductive layer 152R. Also, the conductive layer 152G and the conductive layer 152B are exposed.
[0308] The organic compound film 103Rf is preferably processed by anisotropic etching, particularly anisotropic dry etching, or wet etching may be used.
[0309] When dry etching is used, deterioration of the organic compound film 103Rf can be suppressed by not using an oxygen-containing gas as an etching gas.
[0310] Moreover, a gas containing oxygen may be used as the etching gas. When the etching gas contains oxygen, the etching speed can be increased. Therefore, etching can be performed under low power conditions while maintaining a sufficiently high etching speed. This makes it possible to suppress damage to the organic compound film 103Rf. Furthermore, problems such as adhesion of reaction products generated during etching can be suppressed.
[0311] When using a dry etching method, it is preferable to use a gas containing one or more of H2, CF4, C4F8, SF6, CHF3, Cl2, H2O, BCl3, or a group 18 element such as He or Ar as an etching gas. Alternatively, it is preferable to use a gas containing one or more of these elements and oxygen as an etching gas. Alternatively, oxygen gas may be used as an etching gas.
[0312] Subsequently, as shown in FIG. 11(A), an organic compound film 103Gf which will later become the organic compound layer 103G is formed.
[0313] The organic compound film 103Gf can be formed by the same method as that used for forming the organic compound film 103Rf, and can have the same configuration as the organic compound film 103Rf.
[0314] 11(A), a sacrificial film 158Gf and a mask film 159Gf are formed in this order. Then, a resist mask 190G is formed. The material and the forming method of the sacrificial film 158Gf and the mask film 159Gf are the same as those applicable to the sacrificial film 158Rf and the mask film 159Rf. The material and the forming method of the resist mask 190G are the same as those applicable to the resist mask 190R.
[0315] The resist mask 190G is provided in a position overlapping with the conductive layer 152G.
[0316] Then, as shown in FIG. 11B, a part of the mask film 159Gf is removed using a resist mask 190G to form a mask layer 159G. The mask layer 159G remains on the conductive layer 152G. Then, the resist mask 190G is removed. Then, a part of the sacrificial film 158Gf is removed using the mask layer 159G as a mask to form a sacrificial layer 158G. Then, the organic compound film 103Gf is processed to form an organic compound layer 103G. Thereby, as shown in FIG. 11B, a laminated structure of the organic compound layer 103G, the sacrificial layer 158G, and the mask layer 159G remains on the conductive layer 152G. Also, the mask layer 159R and the conductive layer 152B are exposed.
[0317] Subsequently, as shown in FIG. 11(C), an organic compound film 103Bf is formed.
[0318] The organic compound film 103Bf can be formed by the same method as that used for forming the organic compound film 103Rf, and can have the same structure as the organic compound film 103Rf.
[0319] 11(C), a sacrificial film 158Bf and a mask film 159Bf are formed in this order. Then, a resist mask 190B is formed. The material and the forming method of the sacrificial film 158Bf and the mask film 159Bf are the same as those applicable to the sacrificial film 158Rf and the mask film 159Rf. The material and the forming method of the resist mask 190B are the same as those applicable to the resist mask 190R.
[0320] The resist mask 190B is provided in a position overlapping with the conductive layer 152B.
[0321] 11(D), a part of the mask film 159Bf is removed using a resist mask 190B to form a mask layer 159B. The mask layer 159B remains on the conductive layer 152B. Then, the resist mask 190B is removed. Then, a part of the sacrificial film 158Bf is removed using the mask layer 159B as a mask to form a sacrificial layer 158B. Then, the organic compound film 103Bf is processed to form an organic compound layer 103B. For example, a part of the organic compound film 103Bf is removed using the mask layer 159B and the sacrificial layer 158B as a hard mask to form the organic compound layer 103B.
[0322] 11D, a laminated structure of the organic compound layer 103B, the sacrificial layer 158B, and the mask layer 159B remains on the conductive layer 152B. Also, the mask layers 159R and 159G are exposed.
[0323] It is preferable that the side surfaces of the organic compound layer 103R, the organic compound layer 103G, and the organic compound layer 103B are perpendicular or approximately perpendicular to the surface on which they are formed. For example, it is preferable that the angle between the surface on which they are formed and these side surfaces is 60 degrees or more and 90 degrees or less.
[0324] As described above, the distance between two adjacent ones of the organic compound layer 103R, the organic compound layer 103G, and the organic compound layer 103B formed by photolithography can be narrowed to 8 μm or less, 5 μm or less, 3 μm or less, 2 μm or less, or 1 μm or less. Here, the distance can be defined, for example, as the distance between two adjacent opposing ends of the organic compound layer 103R, the organic compound layer 103G, and the organic compound layer 103B. In this way, by narrowing the distance between the island-shaped organic compound layers, a display device having high definition and a large aperture ratio can be provided. In addition, the distance between the first electrodes between adjacent light-emitting devices can also be narrowed, and can be, for example, 10 μm or less, 8 μm or less, 5 μm or less, 3 μm or less, or 2 μm or less. Note that the distance between the first electrodes between adjacent light-emitting devices is preferably 2 μm or more and 5 μm or less.
[0325] Next, as shown in FIG. 12(A), it is preferable to remove the mask layers 159R, 159G, and 159B.
[0326] The mask layer removal process can be performed using the same method as the mask layer processing process. In particular, by using a wet etching method, damage to the organic compound layer 103 during removal of the mask layer can be reduced compared to the case of using a dry etching method.
[0327] The mask layer may also be removed by dissolving it in a polar solvent such as water or alcohol, such as ethyl alcohol, methyl alcohol, isopropyl alcohol (IPA), or glycerin.
[0328] After removing the mask layer, a drying treatment may be performed to remove water adsorbed on the surface. For example, a heat treatment can be performed in an inert gas atmosphere or a reduced pressure atmosphere. The heat treatment can be performed at a substrate temperature of 50° C. to 200° C., preferably 60° C. to 150° C., and more preferably 70° C. to 120° C. A reduced pressure atmosphere is preferable because it allows drying at a lower temperature.
[0329] Subsequently, as shown in FIG. 12(B), an inorganic insulating film 125f is formed.
[0330] Subsequently, as shown in FIG. 12(C), an insulating film 127f, which will later become the insulating layer 127, is formed on the inorganic insulating film 125f.
[0331] The substrate temperature when forming the inorganic insulating film 125f and the insulating film 127f is preferably 60°C or more, 80°C or more, 100°C or more, or 120°C or more, and 200°C or less, 180°C or less, 160°C or less, 150°C or less, or 140°C or less.
[0332] As the inorganic insulating film 125f, it is preferable to form an insulating film having a thickness of 3 nm or more, 5 nm or more, or 10 nm or more and 200 nm or less, 150 nm or less, 100 nm or less, or 50 nm or less within the above substrate temperature range.
[0333] The inorganic insulating film 125f is preferably formed by, for example, the ALD method. By using the ALD method, damage during film formation can be reduced, and a film with high coverage can be formed, which is preferable. As the inorganic insulating film 125f, for example, an aluminum oxide film is preferably formed by the ALD method.
[0334] The insulating film 127f is preferably formed by using the above-mentioned wet film formation method. The insulating film 127f is preferably formed by using a photosensitive material, for example, by spin coating, and more specifically, is preferably formed by using a photosensitive resin composition containing an acrylic resin.
[0335] Subsequently, exposure is performed to expose a part of the insulating film 127f to visible light or ultraviolet light. The insulating layer 127 is formed in a region sandwiched between any two of the conductive layers 152R, 152G, and 152B, and around the conductive layer 152C.
[0336] The width of the insulating layer 127 to be formed later can be controlled by the exposed region of the insulating film 127f. In this embodiment, the insulating layer 127 is processed so as to have a portion overlapping with the upper surface of the conductive layer 151.
[0337] The light used for exposure preferably contains i-line (wavelength 365 nm), and may contain at least one of g-line (wavelength 436 nm) and h-line (wavelength 405 nm).
[0338] Subsequently, as shown in FIG. 13(A), development is performed to remove the exposed area of the insulating film 127f, thereby forming an insulating layer 127a.
[0339] 13(B), an etching process is performed using the insulating layer 127a as a mask to remove a part of the inorganic insulating film 125f and to thin the thickness of the sacrificial layers 158R, 158G, and 158B. As a result, the inorganic insulating layer 125 is formed under the insulating layer 127a. In addition, the surfaces of the thin parts of the sacrificial layers 158R, 158G, and 158B are exposed. In the following, the etching process using the insulating layer 127a as a mask may be referred to as the first etching process.
[0340] The first etching process can be performed by dry etching or wet etching. Note that, when the inorganic insulating film 125f is formed using the same material as the sacrificial layers 158R, 158G, and 158B, the first etching process can be performed at once, which is preferable.
[0341] When dry etching is performed, it is preferable to use a chlorine-based gas. As the chlorine-based gas, Cl2, BCl3, SiCl4, CCl4, etc. can be used alone or in a mixture of two or more gases. In addition, oxygen gas, hydrogen gas, helium gas, argon gas, etc. can be appropriately added alone or in a mixture of two or more gases to the chlorine-based gas. By using dry etching, the thin film regions of the sacrificial layer 158R, the sacrificial layer 158G, and the sacrificial layer 158B can be formed with good in-plane uniformity.
[0342] As the dry etching apparatus, a dry etching apparatus having a high density plasma source can be used. As the dry etching apparatus having a high density plasma source, for example, an inductively coupled plasma (ICP) etching apparatus can be used. Alternatively, a capacitively coupled plasma (CCP) etching apparatus having parallel plate electrodes can be used.
[0343] In addition, it is preferable to perform the first etching process by wet etching. By using the wet etching method, damage to the organic compound layer 103R, the organic compound layer 103G, and the organic compound layer 103B can be reduced compared to the case of using the dry etching method. For example, the wet etching can be performed using an alkaline solution. For example, a TMAH aqueous solution, which is an alkaline solution, can be used for wet etching of an aluminum oxide film. Also, an acid solution containing fluoride can be used. In this case, the wet etching can be performed by the paddle method. Note that, when the inorganic insulating film 125f is formed using the same material as the sacrificial layer 158R, the sacrificial layer 158G, and the sacrificial layer 158B, the above-mentioned etching process can be performed at once, which is preferable.
[0344] In the first etching process, the sacrificial layers 158R, 158G, and 158B are not completely removed, and the etching process is stopped when the film thickness becomes thin. In this way, by leaving the corresponding sacrificial layers 158R, 158G, and 158B on the organic compound layers 103R, 103G, and 103B, it is possible to prevent the organic compound layers 103R, 103G, and 103B from being damaged in the subsequent process.
[0345] Next, the entire substrate is exposed to light, and it is preferable to irradiate the insulating layer 127a with visible light or ultraviolet light. The energy density of the exposure is 0 mJ / cm 2 Larger, 800mJ / cm 2 It is preferable to set the concentration to 0 mJ / cm or less. 2 Larger than 500mJ / cm 2 It is more preferable to set the following. By performing such exposure after development, the transparency of the insulating layer 127a can be improved in some cases. In addition, the substrate temperature required for a heat treatment for transforming the insulating layer 127a into a tapered shape in a later step can be reduced in some cases.
[0346] Here, the presence of a barrier insulating layer against oxygen (e.g., an aluminum oxide film, etc.) as the sacrificial layer 158R, the sacrificial layer 158G, and the sacrificial layer 158B can reduce the diffusion of oxygen into the organic compound layer 103R, the organic compound layer 103G, and the organic compound layer 103B.
[0347] Next, heat treatment (also referred to as post-baking) is performed. By performing heat treatment, the insulating layer 127a can be transformed into the insulating layer 127 having tapered sides (FIG. 13C). The heat treatment is performed at a temperature lower than the heat resistance temperature of the organic compound layer. The heat treatment can be performed at a substrate temperature of 50° C. to 200° C., preferably 60° C. to 150° C., more preferably 70° C. to 130° C. The heating atmosphere may be an air atmosphere or an inert gas atmosphere. The heating atmosphere may be an atmospheric pressure atmosphere or a reduced pressure atmosphere. This can improve the adhesion between the insulating layer 127 and the inorganic insulating layer 125 and also improve the corrosion resistance of the insulating layer 127.
[0348] In the first etching process, the sacrificial layers 158R, 158G, and 158B are not completely removed, and the sacrificial layers 158R, 158G, and 158B are left in a state where the film thickness is reduced, so that the organic compound layers 103R, 103G, and 103B can be prevented from being damaged and deteriorated in the heat treatment, thereby improving the reliability of the light-emitting device.
[0349] 14(A), an etching process is performed using the insulating layer 127 as a mask to remove parts of the sacrificial layer 158R, the sacrificial layer 158G, and the sacrificial layer 158B. As a result, openings are formed in the sacrificial layer 158R, the sacrificial layer 158G, and the sacrificial layer 158B, respectively, and the upper surfaces of the organic compound layer 103R, the organic compound layer 103G, the organic compound layer 103B, and the conductive layer 152C are exposed. Note that, hereinafter, this etching process may be referred to as a second etching process.
[0350] An end portion of the inorganic insulating layer 125 is covered with an insulating layer 127. Also, Fig. 14(A) shows an example in which a part of the end portion of the sacrificial layer 158G (specifically, the tapered portion formed by the first etching process) is covered with the insulating layer 127, and the tapered portion formed by the second etching process is exposed.
[0351] The second etching process is performed by wet etching. By using the wet etching method, damage to the organic compound layer 103R, the organic compound layer 103G, and the organic compound layer 103B can be reduced compared to the case of using the dry etching method. The wet etching can be performed using, for example, an alkaline solution or an acidic solution. It is preferable to use an aqueous solution so that the organic compound layer 103 does not dissolve.
[0352] 14(B), a common electrode 155 is formed on the organic compound layer 103R, the organic compound layer 103G, the organic compound layer 103B, the conductive layer 152C, and the insulating layer 127. The common electrode 155 can be formed by a method such as a sputtering method or a vacuum deposition method. At this time, as shown in FIG. 8(B), the organic compound layer 103 may be formed as a laminated structure of the first EL layer 104 and the second EL layer 105, and the common electrode 155 may be formed thereon.
[0353] 14(C), the protective layer 131 is formed on the common electrode 155. The protective layer 131 can be formed by a method such as a vacuum deposition method, a sputtering method, a CVD method, or an ALD method.
[0354] Then, the substrate 120 is attached over the protective layer 131 using the resin layer 122, so that a display device can be manufactured. As described above, in a manufacturing method of a display device according to one embodiment of the present invention, the insulating layer 156 is provided so as to have a region overlapping with a side surface of the conductive layer 151, and the conductive layer 152 is formed so as to cover the conductive layer 151 and the insulating layer 156. This can increase the yield of the display device and suppress the occurrence of defects.
[0355] As described above, in the manufacturing method of the display device according to one embodiment of the present invention, the island-shaped organic compound layer 103R, the island-shaped organic compound layer 103G, and the island-shaped organic compound layer 103B are formed by forming a film on one surface and then processing it, instead of using a fine metal mask, so that the island-shaped layers can be formed with a uniform thickness. As a result, a high-definition display device or a display device with a high aperture ratio can be realized. Even if the definition or aperture ratio is high and the distance between the subpixels is extremely short, the organic compound layer 103R, the organic compound layer 103G, and the organic compound layer 103B can be prevented from contacting each other in adjacent subpixels. Therefore, leakage current can be prevented from occurring between the subpixels. As a result, crosstalk can be prevented, and a display device with extremely high contrast can be realized. Even in a display device including a tandem light-emitting device manufactured by a photolithography method, a display device with good characteristics can be provided.
[0356] (Embodiment 5) In this embodiment, a display device according to one embodiment of the present invention will be described.
[0357] The display device of the present embodiment can be a high-definition display device. Therefore, the display device of the present embodiment can be used for, for example, a display unit of a wristwatch-type or bracelet-type information terminal (wearable device), a VR device such as a head-mounted display (HMD), and a head-mounted wearable device such as a glasses-type AR device.
[0358] The display device of the present embodiment can be a high-resolution display device or a large-sized display device. Therefore, the display device of the present embodiment can be used in electronic devices having relatively large screens, such as television devices, desktop or notebook personal computers, computer monitors, digital signage, and large game machines such as pachinko machines, as well as in the display units of digital cameras, digital video cameras, digital photo frames, mobile phones, portable game machines, personal digital assistants, and sound reproducing devices.
[0359] [Display module] 15(A) shows a perspective view of a display module 280. The display module 280 has a display device 100A and an FPC 290. Note that the display device included in the display module 280 is not limited to the display device 100A, and may be either a display device 100B or a display device 100E described later.
[0360] The display module 280 has a substrate 291 and a substrate 292. The display module 280 has a display unit 281. The display unit 281 is a region that displays an image in the display module 280, and is a region where light from each pixel provided in a pixel unit 284 described later can be viewed.
[0361] 15(B) shows a perspective view that typically illustrates the configuration on the substrate 291 side. A circuit portion 282, a pixel circuit portion 283 on the circuit portion 282, and a pixel portion 284 on the pixel circuit portion 283 are stacked on the substrate 291. A terminal portion 285 for connecting to an FPC 290 is provided in a portion of the substrate 291 that does not overlap with the pixel portion 284. The terminal portion 285 and the circuit portion 282 are electrically connected by a wiring portion 286 that is composed of a plurality of wirings.
[0362] The pixel section 284 has a plurality of pixels 284a arranged periodically. An enlarged view of one pixel 284a is shown on the right side of Fig. 15(B). The various configurations described in the previous embodiment can be applied to the pixel 284a. Fig. 15(B) shows an example in which the pixel 284a has the same configuration as the pixel 178 shown in Fig. 8(A) and Fig. 8(B).
[0363] The pixel circuit section 283 has a plurality of pixel circuits 283a that are periodically arranged.
[0364] One pixel circuit 283a is a circuit that controls the driving of a plurality of elements included in one pixel 284a.
[0365] The circuit portion 282 includes a circuit for driving each pixel circuit 283a of the pixel circuit portion 283. For example, it is preferable that the circuit portion 282 includes one or both of a gate line driver circuit and a source line driver circuit. In addition, the circuit portion 282 may include at least one of an arithmetic circuit, a memory circuit, a power supply circuit, and the like.
[0366] The FPC 290 functions as wiring for supplying a video signal, a power supply potential, or the like from the outside to the circuit portion 282. In addition, an IC (integrated circuit) may be mounted on the FPC 290.
[0367] Since the display module 280 can be configured such that one or both of the pixel circuit portion 283 and the circuit portion 282 are stacked below the pixel portion 284, the aperture ratio (effective display area ratio) of the display portion 281 can be made extremely high.
[0368] Such a display module 280 has extremely high resolution and can be suitably used in VR devices such as HMDs or glasses-type AR devices. For example, even in a configuration in which the display unit of the display module 280 is viewed through a lens, the display module 280 has an extremely high resolution display unit 281, so that pixels are not visible even when the display unit is enlarged with a lens, and a highly immersive display can be performed. In addition, the display module 280 is not limited to this and can be suitably used in electronic devices having a relatively small display unit.
[0369] [Display device 100A] The display device 100A shown in FIG. 16A includes a substrate 301, a light emitting device 130R, a light emitting device 130G, a light emitting device 130B, a capacitor 240, and a transistor 310.
[0370] The substrate 301 corresponds to the substrate 291 in FIGS. 15A and 15B. The transistor 310 is a transistor having a channel formation region in the substrate 301. For example, a semiconductor substrate such as a single crystal silicon substrate can be used as the substrate 301. The transistor 310 includes a part of the substrate 301, a conductive layer 311, a low-resistance region 312, an insulating layer 313, and an insulating layer 314. The conductive layer 311 functions as a gate electrode. The insulating layer 313 is located between the substrate 301 and the conductive layer 311 and functions as a gate insulating layer. The low-resistance region 312 is a region in which the substrate 301 is doped with impurities and functions as a source or drain. The insulating layer 314 is provided to cover a side surface of the conductive layer 311.
[0371] In addition, an element isolation layer 315 is provided between two adjacent transistors 310 so as to be embedded in the substrate 301 .
[0372] In addition, an insulating layer 261 is provided to cover the transistor 310 , and a capacitor 240 is provided on the insulating layer 261 .
[0373] Capacitor 240 has conductive layer 241, conductive layer 245, and insulating layer 243 located therebetween. Conductive layer 241 functions as one electrode of capacitor 240, conductive layer 245 functions as the other electrode of capacitor 240, and insulating layer 243 functions as a dielectric of capacitor 240.
[0374] The conductive layer 241 is provided over the insulating layer 261 and is embedded in the insulating layer 254. The conductive layer 241 is electrically connected to one of the source and the drain of the transistor 310 by a plug 271 embedded in the insulating layer 261. The insulating layer 243 is provided to cover the conductive layer 241. The conductive layer 245 is provided in a region overlapping with the conductive layer 241 with the insulating layer 243 interposed therebetween.
[0375] An insulating layer 255 is provided covering the capacitor 240, an insulating layer 174 is provided on the insulating layer 255, and an insulating layer 175 is provided on the insulating layer 174. Light-emitting device 130R, light-emitting device 130G, and light-emitting device 130B are provided on the insulating layer 175. An insulator is provided in the region between adjacent light-emitting devices.
[0376] An insulating layer 156R is provided so as to have a region overlapping with a side surface of the conductive layer 151R, an insulating layer 156G is provided so as to have a region overlapping with a side surface of the conductive layer 151G, and an insulating layer 156B is provided so as to have a region overlapping with a side surface of the conductive layer 151B. A conductive layer 152R is provided so as to cover the conductive layer 151R and the insulating layer 156R, a conductive layer 152G is provided so as to cover the conductive layer 151G and the insulating layer 156G, and a conductive layer 152B is provided so as to cover the conductive layer 151B and the insulating layer 156B. A sacrificial layer 158R is located on the organic compound layer 103R, a sacrificial layer 158G is located on the organic compound layer 103G, and a sacrificial layer 158B is located on the organic compound layer 103B.
[0377] The conductive layer 151R, the conductive layer 151G, and the conductive layer 151B are electrically connected to one of the source or the drain of the transistor 310 via an insulating layer 243, an insulating layer 255, an insulating layer 174, a plug 256 embedded in the insulating layer 175, a conductive layer 241 embedded in the insulating layer 254, and a plug 271 embedded in the insulating layer 261. Various conductive materials can be used for the plug.
[0378] Further, a protective layer 131 is provided on the light emitting devices 130R, 130G, and 130B. The substrate 120 is bonded onto the protective layer 131 with a resin layer 122. For details of the components from the light emitting devices 130 to the substrate 120, refer to the fourth embodiment. The substrate 120 corresponds to the substrate 292 in FIG. 15(A).
[0379] Fig. 16(B) is a modified example of the display device 100A shown in Fig. 16(A). The display device shown in Fig. 16(B) has a colored layer 132R, a colored layer 132G, and a colored layer 132B, and the light-emitting device 130 has an area overlapping one of the colored layer 132R, the colored layer 132G, and the colored layer 132B. In the display device shown in Fig. 16(B), the light-emitting device 130 can emit, for example, white light. Also, for example, the colored layer 132R can transmit red light, the colored layer 132G can transmit green light, and the colored layer 132B can transmit blue light.
[0380] [Display device 100B] FIG. 17 shows a perspective view of the display device 100B.
[0381] The display device 100B has a configuration in which a substrate 352 and a substrate 351 are bonded together. In Fig. 17, the substrate 352 is indicated by a dashed line.
[0382] The display device 100B has a pixel unit 177, a connection unit 140, a circuit 356, wiring 355, etc. Fig. 17 shows an example in which an IC 354 and an FPC 353 are mounted on the display device 100B. Therefore, the configuration shown in Fig. 17 can also be called a display module having the display device 100B, an IC, and an FPC. Here, a display device having a connector such as an FPC attached to a substrate, or a display device having an IC mounted on the substrate, is called a display module.
[0383] The connection section 140 is provided outside the pixel section 177. There may be one or more connection sections 140. The connection section 140 electrically connects the common electrode of the light emitting device and the conductive layer, and can supply a potential to the common electrode.
[0384] The circuit 356 can be, for example, a scanning line driver circuit.
[0385] The wiring 355 has a function of supplying signals and power to the pixel portion 177 and the circuit 356. The signals and power are input to the wiring 355 from the outside via the FPC 353 or from the IC 354.
[0386] 17 shows an example in which an IC 354 is provided on a substrate 351 by a chip on glass (COG) method or a chip on film (COF) method. For example, an IC having a scanning line driver circuit or a signal line driver circuit can be used as the IC 354. Note that the display device 100B and the display module may not include an IC. Also, the IC may be mounted on an FPC by a COF method, for example.
[0387] [Display device 100C] FIG. 18 shows an example of a cross section of the display device 100C, which is obtained by cutting a part of a region including the FPC 372, a part of the pixel section 177, a part of the connection section 140, and a part of a region including the end portion.
[0388] The display device 100C shown in Figure 18 has, between a substrate 351 and a substrate 352, a transistor 201, a transistor 205, a light-emitting device 130R that emits red light, a light-emitting device 130G that emits green light, and a light-emitting device 130B that emits blue light, etc.
[0389] For details of the light emitting devices 130R, 130G, and 130B, refer to the first to fourth embodiments.
[0390] Light-emitting device 130R has conductive layer 224R, conductive layer 151R on conductive layer 224R, and conductive layer 152R on conductive layer 151R. Light-emitting device 130G has conductive layer 224G, conductive layer 151G on conductive layer 224G, and conductive layer 152G on conductive layer 151G. Light-emitting device 130B has conductive layer 224B, conductive layer 151B on conductive layer 224B, and conductive layer 152B on conductive layer 151B.
[0391] The conductive layer 224R is connected to the conductive layer 222b of the transistor 205 through an opening provided in the insulating layer 214. An end of the conductive layer 151R is located outside an end of the conductive layer 224R. An insulating layer 156R is provided to have a region in contact with a side surface of the conductive layer 151R, and a conductive layer 152R is provided to cover the conductive layer 151R and the insulating layer 156R.
[0392] Conductive layer 224G, conductive layer 151G, conductive layer 152G, and insulating layer 156G in light-emitting device 130G, and conductive layer 224B, conductive layer 151B, conductive layer 152B, and insulating layer 156B in light-emitting device 130B are similar to conductive layer 224R, conductive layer 151R, conductive layer 152R, and insulating layer 156R in light-emitting device 130R, and therefore detailed description thereof will be omitted.
[0393] Recesses are formed in the conductive layers 224R, 224G, and 224B so as to cover the openings provided in the insulating layer 214. The layer 128 is embedded in the recesses.
[0394] The layer 128 has a function of planarizing the recesses of the conductive layer 224R, the conductive layer 224G, and the conductive layer 224B. The conductive layer 151R, the conductive layer 151G, and the conductive layer 151B, which are electrically connected to the conductive layer 224R, the conductive layer 224G, and the conductive layer 224B, are provided on the conductive layer 224R, the conductive layer 224G, and the conductive layer 224B, and the layer 128. Therefore, the regions overlapping with the recesses of the conductive layer 224R, the conductive layer 224G, and the conductive layer 224B can also be used as light-emitting regions, and the aperture ratio of the pixel can be increased.
[0395] The layer 128 may be an insulating layer or a conductive layer. Various inorganic insulating materials, organic insulating materials, and conductive materials can be appropriately used for the layer 128. In particular, the layer 128 is preferably formed using an insulating material, and more preferably formed using an organic insulating material. For example, the organic insulating material that can be used for the insulating layer 127 described above can be used for the layer 128.
[0396] A protective layer 131 is provided on the light emitting device 130R, the light emitting device 130G, and the light emitting device 130B. The protective layer 131 and the substrate 352 are bonded via an adhesive layer 142. The substrate 352 is provided with a light shielding layer 157. A solid sealing structure, a hollow sealing structure, or the like can be applied to seal the light emitting device 130. In FIG. 18, the space between the substrate 352 and the substrate 351 is filled with the adhesive layer 142, and a solid sealing structure is applied. Alternatively, the space may be filled with an inert gas (nitrogen, argon, or the like), and a hollow sealing structure may be applied. In this case, the adhesive layer 142 may be provided so as not to overlap with the light emitting device. The space may also be filled with a resin different from the adhesive layer 142 provided in a frame shape.
[0397] 18 shows an example in which the connection portion 140 has a conductive layer 224C obtained by processing the same conductive film as the conductive layers 224R, 224G, and 224B, a conductive layer 151C obtained by processing the same conductive film as the conductive layers 151R, 151G, and 151B, and a conductive layer 152C obtained by processing the same conductive film as the conductive layers 152R, 152G, and 152B. Also, FIG. 18 shows an example in which an insulating layer 156C is provided so as to have an area overlapping with a side surface of the conductive layer 151C.
[0398] The display device 100B is a top emission type. Light emitted by the light emitting device is emitted to the substrate 352 side. The substrate 352 is preferably made of a material that is highly transparent to visible light. When the light emitting element emits infrared or near infrared light, it is preferably made of a material that is highly transparent to the infrared light. The pixel electrode contains a material that reflects visible light, and the counter electrode (common electrode 155) contains a material that transmits visible light.
[0399] An insulating layer 211, an insulating layer 213, an insulating layer 215, and an insulating layer 214 are provided over a substrate 351 in this order. A part of the insulating layer 211 functions as a gate insulating layer for each transistor. A part of the insulating layer 213 functions as a gate insulating layer for each transistor. The insulating layer 215 is provided to cover the transistors. The insulating layer 214 is provided to cover the transistors and functions as a planarizing layer. Note that the number of gate insulating layers and the number of insulating layers covering the transistors are not limited, and each may be a single layer or two or more layers.
[0400] Each of the insulating layers 211, 213, and 215 is preferably an inorganic insulating film.
[0401] The insulating layer 214, which functions as a planarizing layer, is preferably an organic insulating layer.
[0402] The transistor 201 and the transistor 205 each have a conductive layer 221 functioning as a gate, an insulating layer 211 functioning as a gate insulating layer, a conductive layer 222a and a conductive layer 222b functioning as a source and a drain, a semiconductor layer 231, an insulating layer 213 functioning as a gate insulating layer, and a conductive layer 223 functioning as a gate.
[0403] A connection portion 204 is provided in a region of the substrate 351 where the substrate 352 does not overlap. In the connection portion 204, a source electrode or a drain electrode of the transistor 201 is electrically connected to the FPC 372 through a conductive layer 166 and a connection layer 242. The conductive layer 166 is an example of a laminated structure of a conductive film obtained by processing the same conductive film as the conductive layers 224R, 224G, and 224B, a conductive film obtained by processing the same conductive film as the conductive layers 151R, 151G, and 151B, and a conductive film obtained by processing the same conductive film as the conductive layers 152R, 152G, and 152B. On the upper surface of the connection portion 204, the conductive layer 166 is exposed. This allows the connection portion 204 and the FPC 353 to be electrically connected through the connection layer 242.
[0404] It is preferable to provide a light-shielding layer 157 on the surface of the substrate 352 facing the substrate 351. The light-shielding layer 157 can be provided between adjacent light-emitting devices, at the connection portion 140, etc. In addition, various optical members can be disposed on the outer side of the substrate 352.
[0405] The materials usable for the substrate 120 can be used for the substrate 351 and the substrate 352, respectively.
[0406] The adhesive layer 142 may be made of a material that can be used for the resin layer 122 .
[0407] The connection layer 242 may be an anisotropic conductive film (ACF), an anisotropic conductive paste (ACP), or the like.
[0408] [Display device 100D] A display device 100D shown in FIG. 19 differs from the display device 100C shown in FIG. 18 mainly in that the display device 100D is a bottom-emission type display device.
[0409] Light emitted by the light emitting device is emitted to the side of the substrate 351. It is preferable that a material having high transparency to visible light is used for the substrate 351. On the other hand, the light transmissivity of a material used for the substrate 352 does not matter.
[0410] It is preferable to form a light-shielding layer between the substrate 351 and the transistor 201 and between the substrate 351 and the transistor 205. Fig. 19 shows an example in which the light-shielding layer 117 is provided over the substrate 351, the insulating layer 153 is provided over the light-shielding layer, and the transistors 201, 205, and the like are provided over the insulating layer 153.
[0411] Light emitting device 130R includes a conductive layer 112R, a conductive layer 126R on conductive layer 112R, and a conductive layer 129R on conductive layer 126R.
[0412] Light emitting device 130B has conductive layer 112B, conductive layer 126B on conductive layer 112B, and conductive layer 129B on conductive layer 126B.
[0413] The conductive layers 112R, 112B, 126R, 126B, 129R, and 129B are made of a material that is highly transparent to visible light. The common electrode 155 is preferably made of a material that reflects visible light.
[0414] Although the light emitting device 130G is not shown in FIG. 19, the light emitting device 130G is also provided.
[0415] In addition, in FIG. 19 and other figures, an example is shown in which the upper surface of layer 128 has a flat portion, but the shape of layer 128 is not particularly limited.
[0416] [Display device 100E] The display device 100E shown in FIG. 20 is a modification of the display device 100C shown in FIG. 18, and differs from the display device 100C mainly in that the display device 100E has colored layers 132R, 132G, and 132B.
[0417] In the display device 100E, the light emitting device 130 has an area overlapping one of the colored layer 132R, the colored layer 132G, and the colored layer 132B. The colored layer 132R, the colored layer 132G, and the colored layer 132B can be provided on the surface of the substrate 352 facing the substrate 351. An end of the colored layer 132R, an end of the colored layer 132G, and an end of the colored layer 132B can overlap the light blocking layer 157.
[0418] In the display device 100E, the light emitting device 130 can emit, for example, white light. For example, the colored layer 132R can transmit red light, the colored layer 132G can transmit green light, and the colored layer 132B can transmit blue light. The display device 100E may be configured such that the colored layers 132R, 132G, and 132B are provided between the protective layer 131 and the adhesive layer 142.
[0419] 18 and 20 and the like show an example in which the upper surface of the layer 128 has a flat portion, but the shape of the layer 128 is not particularly limited.
[0420] This embodiment mode can be combined with other embodiment modes or examples as appropriate. In addition, in the case where a plurality of configuration examples are shown in one embodiment mode in this specification, the configuration examples can be combined as appropriate.
[0421] (Embodiment 6) In this embodiment, an electronic device according to one embodiment of the present invention will be described.
[0422] The electronic devices of this embodiment include the display device of one embodiment of the present invention in a display portion. The display device of one embodiment of the present invention has high display performance and can easily achieve high definition and high resolution. Therefore, the display device of one embodiment of the present invention can be used in the display portion of various electronic devices.
[0423] Examples of electronic devices include electronic devices with relatively large screens, such as television devices, desktop or notebook personal computers, computer monitors, digital signage, large game machines such as pachinko machines, as well as digital cameras, digital video cameras, digital photo frames, mobile phones, portable game machines, personal digital assistants, and audio playback devices.
[0424] In particular, the display device of one embodiment of the present invention can be suitably used in electronic devices having a relatively small display area because it can increase the resolution. Examples of such electronic devices include wristwatch-type and bracelet-type information terminals (wearable devices), and head-mounted wearable devices such as VR devices, glasses-type AR devices, and MR devices.
[0425] The electronic device of this embodiment may have a sensor (including a function of measuring force, displacement, position, speed, acceleration, angular velocity, rotation speed, distance, light, liquid, magnetism, temperature, chemical substances, sound, time, hardness, electric field, current, voltage, power, radiation, flow rate, humidity, gradient, vibration, odor, or infrared rays).
[0426] An example of a wearable device that can be worn on the head will be described with reference to FIGS. 21(A) to 21(D).
[0427] Electronic device 700A shown in FIG. 21(A) and electronic device 700B shown in FIG. 21(B) each have a pair of display panels 751, a pair of housings 721, a communication unit (not shown), a pair of mounting units 723, a control unit (not shown), an imaging unit (not shown), a pair of optical members 753, a frame 757, and a pair of nose pads 758.
[0428] The display device of one embodiment of the present invention can be applied to the display panel 751. Thus, the electronic device can be highly reliable.
[0429] Each of the electronic device 700A and the electronic device 700B can project an image displayed on the display panel 751 onto a display area 756 of the optical member 753. Since the optical member 753 has translucency, a user can see the image displayed in the display area superimposed on a transmitted image visually recognized through the optical member 753.
[0430] The electronic device 700A and the electronic device 700B may be provided with a camera capable of capturing an image of the front as an imaging unit. In addition, the electronic device 700A and the electronic device 700B may each be provided with an acceleration sensor such as a gyro sensor, thereby detecting the orientation of the user's head and displaying an image corresponding to the orientation in the display area 756.
[0431] The communication unit has a wireless communication device and can supply, for example, a video signal through the wireless communication device. Note that instead of or in addition to the wireless communication device, a connector to which a cable through which a video signal and a power supply potential can be connected may be provided.
[0432] Furthermore, the electronic device 700A and the electronic device 700B are provided with a battery, which can be charged wirelessly and / or wired.
[0433] The housing 721 may be provided with a touch sensor module.
[0434] As the touch sensor module, various touch sensors can be applied. For example, various types of sensors can be adopted, such as a capacitance type, a resistive film type, an infrared type, an electromagnetic induction type, a surface acoustic wave type, or an optical type. In particular, it is preferable to apply a capacitance type or an optical type sensor to the touch sensor module.
[0435] Electronic device 800A shown in Figure 21 (C) and electronic device 800B shown in Figure 21 (D) each have a pair of display units 820, a housing 821, a communication unit 822, a pair of mounting units 823, a control unit 824, a pair of imaging units 825, and a pair of lenses 832.
[0436] The display device of one embodiment of the present invention can be applied to the display portion 820. Thus, the electronic device can be made highly reliable.
[0437] Display unit 820 is provided inside housing 821 at a position that can be viewed through lens 832. Also, by displaying different images on the pair of display units 820, it is possible to perform three-dimensional display using parallax.
[0438] It is preferable that electronic device 800A and electronic device 800B each have a mechanism capable of adjusting the left-right positions of lens 832 and display unit 820 so that they are optimally positioned according to the position of the user's eyes.
[0439] The mounting portion 823 allows the user to mount the electronic device 800A or the electronic device 800B on the head.
[0440] The imaging unit 825 has a function of acquiring external information. Data acquired by the imaging unit 825 can be output to the display unit 820. An image sensor can be used for the imaging unit 825. In addition, multiple cameras may be provided so as to be compatible with multiple angles of view, such as telephoto and wide angle.
[0441] The electronic device 800A may have a vibration mechanism that functions as a bone conduction earphone.
[0442] The electronic device 800A and the electronic device 800B may each have an input terminal. The input terminal can be connected to a cable for supplying a video signal from a video output device or the like and power for charging a battery provided in the electronic device.
[0443] The electronic device of one embodiment of the present invention may have a function of wireless communication with the earphone 750.
[0444] 21B includes an earphone unit 727. A part of a wiring connecting the earphone unit 727 and a control unit may be disposed inside the housing 721 or the attachment unit 723.
[0445] 21D includes an earphone unit 827. For example, the earphone unit 827 and the control unit 824 may be configured to be connected to each other by wire.
[0446] As described above, as electronic devices according to one embodiment of the present invention, both glasses-type devices (such as the electronic device 700A and the electronic device 700B) and goggles-type devices (such as the electronic device 800A and the electronic device 800B) are suitable.
[0447] An electronic device 6500 shown in FIG. 22A is a portable information terminal that can be used as a smartphone.
[0448] The electronic device 6500 includes a housing 6501, a display portion 6502, a power button 6503, a button 6504, a speaker 6505, a microphone 6506, a camera 6507, and a light source 6508. The display portion 6502 has a touch panel function.
[0449] The display device of one embodiment of the present invention can be applied to the display portion 6502. Therefore, the electronic device can be highly reliable.
[0450] FIG. 22B is a schematic cross-sectional view including the end portion of the housing 6501 on the microphone 6506 side.
[0451] A light-transmitting protective member 6510 is provided on the display surface side of the housing 6501, and a display panel 6511, optical members 6512, a touch sensor panel 6513, a printed circuit board 6517, a battery 6518, etc. are arranged in the space surrounded by the housing 6501 and the protective member 6510.
[0452] A display panel 6511, an optical member 6512, and a touch sensor panel 6513 are fixed to the protective member 6510 by an adhesive layer (not shown).
[0453] In an area outside the display unit 6502, a part of the display panel 6511 is folded back, and the folded back part is connected to an FPC 6515. An IC 6516 is mounted on the FPC 6515. The FPC 6515 is connected to a terminal provided on a printed circuit board 6517.
[0454] The display device of one embodiment of the present invention can be applied to the display panel 6511. Therefore, an extremely lightweight electronic device can be realized. In addition, since the display panel 6511 is extremely thin, a large-capacity battery 6518 can be mounted thereon while keeping the thickness of the electronic device small. In addition, by folding back a part of the display panel 6511 and arranging a connection portion with the FPC 6515 on the back side of the pixel portion, an electronic device with a narrow frame can be realized.
[0455] 22C shows an example of a television set. In a television set 7100, a display portion 7000 is incorporated in a housing 7171. Here, the housing 7171 is supported by a stand 7173.
[0456] The display device of one embodiment of the present invention can be applied to the display portion 7000. Therefore, the electronic device can be provided with high reliability.
[0457] A television set 7100 shown in FIG. 22C can be operated using an operation switch provided in a housing 7171 and a remote control unit 7151 provided separately.
[0458] 22D shows an example of a laptop personal computer 7200. The laptop personal computer 7200 includes a housing 7211, a keyboard 7212, a pointing device 7213, and an external connection port 7214. A display portion 7000 is incorporated in the housing 7211.
[0459] The display device of one embodiment of the present invention can be applied to the display portion 7000. Therefore, the electronic device can be provided with high reliability.
[0460] 22(E) and 22(F) show an example of digital signage.
[0461] 22E includes a housing 7301, a display portion 7000, and a speaker 7303. The digital signage 7300 may further include an LED lamp, an operation key (including a power switch or an operation switch), a connection terminal, various sensors, a microphone, and the like.
[0462] 22F shows a digital signage 7400 attached to a cylindrical pillar 7401. The digital signage 7400 has a display unit 7000 provided along the curved surface of the pillar 7401.
[0463] 22E and 22F, the display device of one embodiment of the present invention can be applied to the display portion 7000. Therefore, the electronic device can have high reliability.
[0464] The larger the display unit 7000, the more information can be provided at one time. Also, the larger the display unit 7000, the more easily it catches people's attention, which can increase the advertising effect of, for example, advertisements.
[0465] Furthermore, as shown in FIG. 22(E) and FIG. 22(F), it is preferable that the digital signage 7300 or the digital signage 7400 can be linked via wireless communication with an information terminal 7311 or an information terminal 7411 such as a smartphone carried by a user.
[0466] The electronic devices shown in Figures 23(A) to 23(G) have a housing 9000, a display unit 9001, a speaker 9003, operation keys 9005 (including a power switch or an operation switch), a connection terminal 9006, a sensor 9007 (including a function of measuring force, displacement, position, speed, acceleration, angular velocity, rotation speed, distance, light, liquid, magnetism, temperature, chemical substances, sound, time, hardness, electric field, current, voltage, power, radiation, flow rate, humidity, gradient, vibration, odor or infrared rays), a microphone 9008, etc.
[0467] 23(A) to 23(G) have various functions, such as a function of displaying various information (still images, videos, text images, etc.) on a display unit, a touch panel function, a function of displaying a calendar, date, time, etc., a function of controlling processing by various software (programs), a wireless communication function, a function of reading and processing a program or data recorded in a recording medium, etc.
[0468] The electronic devices shown in FIGS. 23A to 23G will be described in detail below.
[0469] FIG. 23A is a perspective view showing a mobile information terminal 9171. The mobile information terminal 9171 can be used as, for example, a smartphone. Note that the mobile information terminal 9171 may be provided with a speaker 9003, a connection terminal 9006, a sensor 9007, or the like. The mobile information terminal 9171 can display text and image information on a plurality of surfaces thereof. FIG. 23A shows an example in which three icons 9050 are displayed. Information 9051 shown in a dashed rectangle can also be displayed on another surface of the display unit 9001. Examples of the information 9051 include notification of incoming e-mail, SNS, phone call, etc., the title of the e-mail or SNS, the sender's name, the date and time, the remaining battery level, radio wave intensity, and the like. Alternatively, the icon 9050, etc. may be displayed at the position where the information 9051 is displayed.
[0470] 23B is a perspective view of a mobile information terminal 9172. The mobile information terminal 9172 has a function of displaying information on three or more surfaces of the display unit 9001. Here, an example is shown in which information 9052, information 9053, and information 9054 are displayed on different surfaces. For example, a user can check information 9053 displayed in a position that can be observed from above the mobile information terminal 9172 while the mobile information terminal 9172 is stored in a breast pocket of a garment.
[0471] 23C is a perspective view of a tablet terminal 9173. The tablet terminal 9173 is capable of executing various applications such as mobile phone, e-mail, text browsing and creation, music playback, Internet communication, computer games, etc. The tablet terminal 9173 has a display unit 9001, a camera 9002, a microphone 9008, and a speaker 9003 on the front side of a housing 9000, operation keys 9005 as operation buttons on the left side of the housing 9000, and a connection terminal 9006 on the bottom.
[0472] 23D is a perspective view showing a wristwatch-type mobile information terminal 9200. The mobile information terminal 9200 can be used as, for example, a smart watch (registered trademark). The display surface of the display unit 9001 is curved, and display can be performed along the curved display surface. The mobile information terminal 9200 can also perform hands-free conversation by communicating with, for example, a headset capable of wireless communication. The mobile information terminal 9200 can also perform data transmission and charging with another information terminal through a connection terminal 9006. Note that charging may be performed by wireless power supply.
[0473] 23(E) to 23(G) are perspective views showing a foldable mobile information terminal 9201. FIG. 23(E) is a perspective view of the mobile information terminal 9201 in an unfolded state, FIG. 23(G) is a perspective view of the mobile information terminal 9201 in a folded state, and FIG. 23(F) is a perspective view of a state in the middle of changing from one of FIG. 23(E) and FIG. 23(G) to the other. The mobile information terminal 9201 has excellent portability in a folded state, and has excellent viewability of the display due to a seamless wide display area in an unfolded state. A display portion 9001 of the mobile information terminal 9201 is supported by three housings 9000 connected by a hinge 9055. For example, the display portion 9001 can be bent with a curvature radius of 0.1 mm or more and 150 mm or less.
[0474] This embodiment mode can be combined with other embodiment modes or examples as appropriate. In addition, in the case where a plurality of configuration examples are shown in one embodiment mode in this specification, the configuration examples can be combined as appropriate. EXAMPLES
[0475] In this example, a detailed manufacturing method and characteristics of a light-emitting device 1 according to one embodiment of the present invention will be described. The structural formulae of main compounds used in this example are shown below.
[0476] [ka]
[0477] (Method of fabricating light-emitting device 1) First, on a glass substrate, a 100 nm thick silver-palladium-copper alloy (APC: Ag-Pd-Cu) was laminated as a reflective electrode and a 100 nm thick indium tin oxide containing silicon oxide (ITSO) was laminated as a transparent electrode by sputtering. This laminated film was patterned by photolithography to form an anode 101. The transparent electrode functions as an anode and is also called the first electrode together with the reflective electrode.
[0478] Next, as a pretreatment for forming a light-emitting device on the substrate, the substrate surface was washed with water, baked at 200° C. for 1 hour, and then subjected to UV ozone treatment for 370 seconds.
[0479] After that, about 1 × 10 -4 The substrate was introduced into a vacuum deposition apparatus whose inside had been reduced in pressure to 10 Pa, and vacuum baking was carried out at 170° C. for 60 minutes in a heating chamber in the vacuum deposition apparatus, and then the substrate was allowed to cool for about 30 minutes.
[0480] Next, the substrate was fixed to a holder installed in a vacuum deposition apparatus so that the surface on which the anode 101 was formed was facing downward, and N-(biphenyl-4-yl)-N-[4-(9-phenyl-9H-carbazol-3-yl)phenyl]-9,9-dimethyl-9H-fluoren-2-amine (abbreviation: PCBBiF) represented by the above structural formula (i) and an electron acceptor material (OCHD-003) containing fluorine and having a molecular weight of 672 were co-deposited by a deposition method to a thickness of 10 nm on the inorganic insulating film and the anode 101 in a weight ratio of 1:0.03 (=PCBBiF:OCHD-003) to form a hole injection layer 111.
[0481] On the hole injection layer 111, PCBBiF was deposited to a thickness of 60 nm to form a first hole transport layer.
[0482] Subsequently, 8-(1,1':4',1''-terphenyl-3-yl)-4-[3-(dibenzothiophen-4-yl)phenyl]-[1]benzofuro[3,2-d]pyrimidine (abbreviation: 8mpTP-4mDBtPBfpm) represented by the above structural formula (ii), 9-(2-naphthyl)-9'-phenyl-9H,9'H-3,3'-bicarbazole (abbreviation: βNCCP) represented by the above structural formula (iii), and [2-d A first light-emitting layer was formed by co-evaporating 40 nm of 8mpTP-4mDBtPBfpm:βNCCP:Ir(5mppy-d3)2(mbfpypy-d3) and 3-methyl-8-(2-pyridinyl-κN)benzofuro[2,3-b]pyridine-κC]bis[2-(5-d3-methyl-2-pyridinyl-κN2)phenyl-κC]iridium(III) (abbreviation: Ir(5mppy-d3)2(mbfpypy-d3)) in a weight ratio of 0.5:0.5:0.1 (=8mpTP-4mDBtPBfpm:βNCCP:Ir(5mppy-d3)2(mbfpypy-d3)).
[0483] After that, 3,6-bis(diphenylamino)-9-[4-(4,6-diphenyl-1,3,5-triazin-2-yl)phenyl]-9H-carbazole (abbreviation: DACT-II) represented by the above structural formula (v) was evaporated to a thickness of 10 nm to form a first electron transport layer.
[0484] After the formation of the first electron transport layer, 2,2'-(1,3-phenylene)bis(9-phenyl-1,10-phenanthroline) (abbreviation: mPPhen2P) represented by the above structural formula (vi) and 1-(9,9'-spirobi[9H-fluorene]-2-yl)-1,3,4,6,7,8-hexahydro-2H-pyrimido[1,2-a]pyrimidine (abbreviation: 2hppSF) represented by the above structural formula (vii) were co-deposited to a thickness of 5 nm so as to give a weight ratio of 1:1 (=mPPhen2P:2hppSF), copper phthalocyanine (abbreviation: CuPc) represented by the above structural formula (viii) was deposited to a thickness of 2 nm, and further PCBBiF and OCHD-003 were co-deposited to a thickness of 10 nm so as to give a weight ratio of 1:0.15 (=PCBBiF:OCHD-003) to form an intermediate layer.
[0485] On the intermediate layer, PCBBiF was evaporated to a thickness of 55 nm to form a second hole transport layer.
[0486] A second light-emitting layer was formed on the second hole-transporting layer by co-evaporation of 8mpTP-4mDBtPBfpm, βNCCP, and Ir(5mppy-d3)2(mbfpypy-d3) to a thickness of 40 nm in a weight ratio of 0.5:0.5:0.1 (=8mpTP-4mDBtPBfpm:βNCCP:Ir(5mppy-d3)2(mbfpypy-d3)).
[0487] Thereafter, 2-{3-[3-(N-phenyl-9H-carbazol-3-yl)-9H-carbazol-9-yl]phenyl}dibenzo[f,h]quinoxaline (abbreviation: 2mPCCzPDBq) represented by the above structural formula (ix) was evaporated to a thickness of 20 nm, and further mPPhen2P was evaporated to a thickness of 20 nm to form a second electron transport layer.
[0488] Next, processing was performed using photolithography. The sample was removed from the vacuum deposition apparatus and exposed to the atmosphere. Then, using trimethylaluminum (TMA) as a precursor and water vapor as an oxidizing agent, aluminum oxide was deposited to a thickness of 30 nm by the ALD method to form the first sacrificial layer.
[0489] A composite oxide (IGZO) containing indium, gallium, zinc, and oxygen was deposited by sputtering on the first sacrificial layer to a thickness of 50 nm to form a second sacrificial layer.
[0490] A photoresist was formed on the second sacrificial layer, and the second sacrificial layer was processed by lithography so that a slit having a width of 3 μm was formed at a position 3.5 μm away from the anode 101 .
[0491] Specifically, the second sacrificial layer was processed using an etching gas containing CF4, O2, and He with the resist as a mask, and then the resist was removed using a solution containing tetramethylammonium hydroxide (abbreviation: TMAH).
[0492] Next, the first sacrificial layer was processed using an etching gas containing fluoroform (CHF3) and helium (He) at a flow rate ratio of CHF3:He = 1:9, with the second sacrificial layer as a hard mask. After this, the second electron transport layer, the second light-emitting layer, the second hole transport layer, the intermediate layer, the first electron transport layer, the first light-emitting layer, the first hole transport layer, and the hole injection layer were processed using an etching gas containing oxygen (O2).
[0493] After processing, the second sacrificial layer was removed using an etching gas containing CF4, O2, and He, and the first sacrificial layer was removed using a basic chemical solution to expose the second electron transport layer.
[0494] The sample with the second electron transport layer exposed was then washed with 1×10 -4 The sample was introduced into a vacuum deposition apparatus whose inside had been reduced in pressure to about Pa, and vacuum-baked at 110° C. for 1 hour in the heating chamber of the vacuum deposition apparatus. After that, the sample was left to cool for about 30 minutes.
[0495] Next, lithium fluoride and ytterbium were evaporated at a weight ratio of 2:1 (=LiF:Yb) to a thickness of 1.5 nm to form the electron injection layer 115, and then silver (Ag) and magnesium (Mg) were co-evaporated at a volume ratio of 1:0.1 and a film thickness of 15 nm to form the cathode 102 (second electrode). In addition, 4,4',4''-(benzene-1,3,5-triyl)tri(dibenzothiophene) (abbreviation: DBT3P-II) represented by the above structural formula (x) was deposited at a thickness of 70 nm on the cathode 102 as a cap layer to improve the light extraction efficiency.
[0496] Next, in a glove box with a nitrogen atmosphere, the light-emitting device was sealed with a glass substrate to prevent it from being exposed to the atmosphere (a UV-curable sealant was applied around the device, UV was irradiated only onto the sealant without irradiating the light-emitting device, and a heat treatment was performed at 80°C under atmospheric pressure for 1 hour), forming light-emitting device 1. The element structure of light-emitting device 1 is shown in the table below.
[0497] [Table 4]
[0498] Thus, in the light-emitting device 1, an organic compound having a HOMO level of -5.9 eV or more and -5.0 eV or less is used in the first electron transport layer. In addition, the first layer having mPPhen2P:2hppSF=1:1 is formed in the intermediate layer, and this film is a film that blocks holes. In addition, 2hppSF is an organic compound having an acid dissociation constant pKa of 13.95 and a strong basicity of pKa8 or more. In addition, mPPhen2P, which is a material having electron transport properties and a LUMO level of -3.0 eV or more and -2.0 eV or less, is used in the first layer.
[0499] Here, we measured the electron spin resonance spectrum of a thin film co-deposited on a quartz substrate with mPPhen2P and 2hppSF in a weight ratio of 1:1 (=mPPhen2P:2hppSF) to a thickness of 50 nm. No signal was observed near the g value of 2.00, and the spin density was 8 × 10 16 spins / cm 3 It was found that the electron spin resonance spectrum was less than 100 nm. The measurement of the electron spin resonance spectrum by the ESR method was performed using an electron spin resonance measuring device E500 type (manufactured by Bruker). The above measurement was performed at room temperature with a resonance frequency of 9.56 GHz, output of 1 mW, modulation magnetic field of 50 mT, modulation width of 0.5 mT, time constant of 0.04 s, and sweep time of 1 min. From this, it can be said that 2hppSF does not exhibit electron donating properties to mPPhen2P.
[0500] The P-type CGL is a layer containing PCBBiF, an organic compound with hole transport properties, and OCHD-003, which exhibits electron acceptor properties, and is a charge generation layer that separates charges when a voltage is applied.
[0501] Here, PCBBiF and OCHD-003 were co-deposited on a quartz substrate in a weight ratio of 1:0.1 (PCBBiF:OCHD-003) to a thickness of 100 nm. The electron spin resonance spectrum of the thin film was measured at room temperature. A signal was observed at a g value of approximately 2.00, and the spin density was 5×10 19 spins / cm 3 From this, it was found that the layer exhibits electron accepting properties for OCHD-003 and PCBBiF, and the layer containing PCBBiF and OCHD-003 functions as a charge generating layer.
[0502] The luminance-current density characteristics of the light-emitting device 1 are shown in Fig. 24, the luminance-voltage characteristics in Fig. 25, the current efficiency-luminance characteristics in Fig. 26, the current density-voltage characteristics in Fig. 27, and the electroluminescence spectrum in Fig. 28. 2 The main characteristics in the vicinity are shown in Table 5. The luminance, CIE chromaticity, and electroluminescence spectrum were measured using a spectroradiometer (SR-UL1R, manufactured by Topcon Corporation) at room temperature.
[0503] [Table 5]
[0504] It can be seen from Fig. 28 (spectrum) that the light-emitting device 1 emits green light originating from Ir(5mppy-d3)2(mbfpypy-d3). In addition, it can be seen from Fig. 26 (current efficiency) that the light-emitting device 1 functions as a tandem-type light-emitting device.
[0505] Furthermore, from Figure 25 (brightness-voltage characteristics), it was found that the light-emitting device 1, although a tandem-type light-emitting device fabricated via a photolithography process, exhibited a driving voltage similar to that of a light-emitting device fabricated via a vacuum integrated process.
[0506] In addition, the current density of the light-emitting device 1 was 50 mA / cm 2The change in luminance versus drive time during constant current drive was measured and the results are shown in Fig. 29. Fig. 29 shows that light-emitting device 1 is a light-emitting device with good reliability.
[0507] In this manner, by using the configuration of the present invention, it is possible to provide a light-emitting device having excellent characteristics, such as high luminous efficiency and low driving voltage.
[0508] Next, the results of determining the GSP_slope of the first layer are shown. The GSP_slope of the first layer was determined by fabricating a measurement device as shown in the table below. Note that the film thicknesses in Table 4 and the film thicknesses of the anode, hole injection layer, electron injection layer, and cathode in the table below are design film thicknesses. On the other hand, the film thicknesses of electron transport layer 1 and electron transport layer 2 in the table below require accurate values to calculate the GSP_slope, so the values listed are those measured using a spectroscopic ellipsometer (M-2000U manufactured by J.A. Woollam Japan).
[0509] [Table 6]
[0510] The structural formulas of the main organic compounds used in the measurement device are shown below.
[0511] [ka]
[0512] For the measurement device, the substrate temperature was room temperature, and the deposition rate was 0.2 nm / s to 0.4 nm / s, and deposition was performed without stopping deposition while forming one layer. In the measurement device, electron transport layer 1 corresponds to thin film 1, and electron transport layer 2 corresponds to thin film 2, and electron transport layer 2 is formed of the same material as the first layer in light-emitting device 1. The capacitance-voltage characteristics of the measurement device are shown in Figure 30. The GSP_slope of Alq3 is known (48 (mV / nm)).
[0513] Table 7 shows the ordinary refractive index n o , the electron injection voltage V of the measurement device obtained from Figure 30 i , threshold voltage V bi , the interface charge density σ calculated from the formula (1) shown in the first embodiment if_e , and GSP_slope calculated from equation (2).
[0514] [Table 7]
[0515] In this way, it was found that the first layer used in the intermediate layer in the light-emitting device 1 was a layer having a negative GSP_slope. As a result, the light-emitting device 1, which is a light-emitting device according to one embodiment of the present invention, was able to be a light-emitting device with good characteristics in which an increase in driving voltage was suppressed even after a photolithography process. EXAMPLES
[0516] In this example, a detailed manufacturing method and characteristics of a light-emitting device 2 according to one embodiment of the present invention will be described. The structural formulae of main compounds used in this example are shown below.
[0517] [ka]
[0518] (Method of manufacturing light-emitting device 2) First, on a glass substrate, 100 nm of silver was laminated as a reflective electrode and 10 nm of indium tin oxide containing silicon oxide (ITSO) was laminated as a transparent electrode by sputtering from the substrate side. This laminated film was patterned by photolithography to form an anode 101. The transparent electrode functions as an anode and is also called the first electrode together with the reflective electrode.
[0519] Next, as a pretreatment for forming a light-emitting device on the substrate, the substrate surface was washed with water and baked at 200° C. for 1 hour.
[0520] After that, about 1 × 10 -4 The substrate was introduced into a vacuum deposition apparatus whose inside had been reduced in pressure to 1 Pa, and vacuum baking was carried out at 170° C. for 30 minutes in a heating chamber in the vacuum deposition apparatus, and the substrate was then allowed to cool for approximately 30 minutes.
[0521] Next, the substrate was fixed to a holder installed in a vacuum deposition apparatus so that the surface on which the anode 101 was formed was facing downward, and N-(biphenyl-4-yl)-N-[4-(9-phenyl-9H-carbazol-3-yl)phenyl]-9,9-dimethyl-9H-fluoren-2-amine (abbreviation: PCBBiF) represented by the above structural formula (i) and an electron acceptor material (OCHD-003) containing fluorine and having a molecular weight of 672 were co-deposited by a deposition method to a thickness of 10 nm on the inorganic insulating film and the anode 101 in a weight ratio of 1:0.03 (=PCBBiF:OCHD-003) to form a hole injection layer 111.
[0522] On the hole injection layer 111, PCBBiF was deposited to a thickness of 20 nm to form a first hole transport layer.
[0523] Subsequently, 8-(1,1':4',1''-terphenyl-3-yl)-4-[3-(dibenzothiophen-4-yl)phenyl]-[1]benzofuro[3,2-d]pyrimidine (abbreviation: 8mpTP-4mDBtPBfpm) represented by the above structural formula (ii), 9-(2-naphthyl)-9'-phenyl-9H,9'H-3,3'-bicarbazole (abbreviation: βNCCP) represented by the above structural formula (iii), and [2-d A first light-emitting layer was formed by co-evaporating 40 nm of 8mpTP-4mDBtPBfpm:βNCCP:Ir(5mppy-d3)2(mbfpypy-d3) and 3-methyl-8-(2-pyridinyl-κN)benzofuro[2,3-b]pyridine-κC]bis[2-(5-d3-methyl-2-pyridinyl-κN2)phenyl-κC]iridium(III) (abbreviation: Ir(5mppy-d3)2(mbfpypy-d3)) in a weight ratio of 0.5:0.5:0.1 (=8mpTP-4mDBtPBfpm:βNCCP:Ir(5mppy-d3)2(mbfpypy-d3)).
[0524] After that, 2-{3-[3-(N-phenyl-9H-carbazol-3-yl)-9H-carbazol-9-yl]phenyl}dibenzo[f,h]quinoxaline (abbreviation: 2mPCCzPDBq) represented by the above structural formula (ix) was evaporated to a thickness of 10 nm to form a first electron transport layer.
[0525] After the formation of the first electron transport layer, 2,2'-(1,3-phenylene)bis(9-phenyl-1,10-phenanthroline) (abbreviation: mPPhen2P) represented by the above structural formula (vi) and 1-(9,9'-spirobi[9H-fluorene]-2-yl)-1,3,4,6,7,8-hexahydro-2H-pyrimido[1,2-a]pyrimidine (abbreviation: 2hppSF) represented by the above structural formula (vii) were co-deposited to a thickness of 5 nm so as to give a weight ratio of 1:1 (=mPPhen2P:2hppSF), copper phthalocyanine (abbreviation: CuPc) represented by the above structural formula (viii) was deposited to a thickness of 2 nm, and further PCBBiF and OCHD-003 were co-deposited to a thickness of 10 nm so as to give a weight ratio of 1:0.15 (=PCBBiF:OCHD-003) to form an intermediate layer.
[0526] On the intermediate layer, PCBBiF was evaporated to a thickness of 65 nm to form a second hole transport layer.
[0527] A second light-emitting layer was formed on the second hole-transporting layer by co-evaporation of 8mpTP-4mDBtPBfpm, βNCCP, and Ir(5mppy-d3)2(mbfpypy-d3) to a thickness of 40 nm in a weight ratio of 0.5:0.5:0.1 (=8mpTP-4mDBtPBfpm:βNCCP:Ir(5mppy-d3)2(mbfpypy-d3)).
[0528] Thereafter, 2mPCCzPDBq was evaporated to a thickness of 20 nm, and mPPhen2P was evaporated to a thickness of 20 nm to form a second electron transport layer.
[0529] Next, lithium fluoride and ytterbium were evaporated at a weight ratio of 2:1 (=LiF:Yb) to a thickness of 1.5 nm to form the electron injection layer 115, and then silver (Ag) and magnesium (Mg) were co-evaporated at a volume ratio of 1:0.1 and a film thickness of 15 nm to form the cathode 102 (second electrode). In addition, 4,4',4''-(benzene-1,3,5-triyl)tri(dibenzothiophene) (abbreviation: DBT3P-II) represented by the above structural formula (x) was deposited at a thickness of 70 nm on the cathode 102 as a cap layer to improve the light extraction efficiency.
[0530] Next, in a glove box with a nitrogen atmosphere, the light-emitting device was sealed with a glass substrate to prevent it from being exposed to the atmosphere (a UV-curable sealant was applied around the device, UV was irradiated only onto the sealant without irradiating the light-emitting device, and a heat treatment was performed at 80°C under atmospheric pressure for 1 hour), forming light-emitting device 2. The element structure of light-emitting device 2 is shown in the table below.
[0531] [Table 8]
[0532] Thus, in the light-emitting device 2, an organic compound having a HOMO level of -5.9 eV or more and -5.0 eV or less is used in the first electron transport layer. In addition, a first layer having mPPhen2P:2hppSF=1:1 is formed in the intermediate layer, and this film is a film that blocks holes. In addition, 2hppSF is an organic compound having an acid dissociation constant pKa of 13.95 and a strong basicity of pKa8 or more. In addition, mPPhen2P, which is a material having electron transport properties and a LUMO level of -3.0 eV or more and -2.0 eV or less, is used in the first layer.
[0533] Here, we measured the electron spin resonance spectrum of a thin film co-deposited on a quartz substrate with mPPhen2P and 2hppSF in a weight ratio of 1:1 (=mPPhen2P:2hppSF) to a thickness of 50 nm. No signal was observed near the g value of 2.00, and the spin density was 8 × 1016 spins / cm 3 It was found that the electron spin resonance spectrum was less than 100 nm. The measurement of the electron spin resonance spectrum by the ESR method was performed using an electron spin resonance measuring device E500 type (manufactured by Bruker). The above measurement was performed at room temperature with a resonance frequency of 9.56 GHz, output of 1 mW, modulation magnetic field of 50 mT, modulation width of 0.5 mT, time constant of 0.04 s, and sweep time of 1 min. From this, it can be said that 2hppSF does not exhibit electron donating properties to mPPhen2P.
[0534] The P-type CGL is a layer containing PCBBiF, an organic compound with hole transport properties, and OCHD-003, which exhibits electron acceptor properties, and is a charge generation layer that separates charges when a voltage is applied.
[0535] Here, PCBBiF and OCHD-003 were co-deposited on a quartz substrate in a weight ratio of 1:0.1 (PCBBiF:OCHD-003) to a thickness of 100 nm. The electron spin resonance spectrum of the thin film was measured at room temperature. A signal was observed at a g value of approximately 2.00, and the spin density was 5×10 19 spins / cm 3 From this, it was found that the layer exhibits electron accepting properties for OCHD-003 and PCBBiF, and the layer containing PCBBiF and OCHD-003 functions as a charge generating layer.
[0536] The luminance-current density characteristic of the light-emitting device 2 is shown in FIG. 31, the current efficiency-luminance characteristic is shown in FIG. 32, the luminance-voltage characteristic is shown in FIG. 33, the current density-voltage characteristic is shown in FIG. 34, and the electroluminescence spectrum is shown in FIG. 35. 2 The main characteristics in the vicinity are shown in Table 9. The luminance, CIE chromaticity, and electroluminescence spectrum were measured at room temperature using a spectroradiometer (SR-UL1R, manufactured by Topcon Corporation).
[0537] [Table 9]
[0538] It can be seen from Fig. 35 (spectrum) that the light-emitting device 2 emits green light originating from Ir(5mppy-d3)2(mbfpypy-d3). In addition, it can be seen from Fig. 32 (current efficiency) that the light-emitting device 2 functions as a tandem-type light-emitting device.
[0539] The current density of the light-emitting device 2 was 50 mA / cm 2 The change in luminance versus drive time during constant current drive was measured and the results are shown in Fig. 36. Fig. 36 shows that light-emitting device 2 is a light-emitting device with good reliability.
[0540] In this manner, by using the configuration of the present invention, it is possible to provide a light-emitting device having excellent characteristics such as high luminous efficiency, low driving voltage, and long life.
[0541] Next, the results of determining the GSP_slope of the first layer are shown. The GSP_slope of the first layer was determined by fabricating a measurement device as shown in the table below. Note that the film thicknesses in Table 8 and the film thicknesses of the anode, hole injection layer, electron injection layer, and cathode in the table below (Table 10) are design film thicknesses. On the other hand, the film thicknesses of electron transport layer 1 and electron transport layer 2 in the table below require accurate values to calculate the GSP_slope, so the values shown are those measured using a spectroscopic ellipsometer (M-2000U manufactured by J.A. Woollam Japan).
[0542] [Table 10]
[0543] The structural formulas of the main organic compounds used in the measurement device are shown below.
[0544] [ka]
[0545] For the measurement device, the substrate temperature was room temperature, and the deposition rate was 0.2 nm / s to 0.4 nm / s, and deposition was performed without stopping deposition while forming one layer. In the measurement device, electron transport layer 1 corresponds to thin film 1, and electron transport layer 2 corresponds to thin film 2, and electron transport layer 2 is formed of the same material as the first layer in light-emitting device 1. The capacitance-voltage characteristics of the measurement device are shown in Figure 30. The GSP_slope of Alq3 is known (48 (mV / nm)).
[0546] Table 11 shows the ordinary refractive index n o , the electron injection voltage V of the measurement device obtained from Figure 37 i , threshold voltage V bi , the interface charge density σ calculated from the formula (1) shown in the first embodiment if_e , and GSP_slope calculated from equation (2).
[0547] [Table 11]
[0548] Thus, it was found that the first layer used in the intermediate layer in the light-emitting device 2 was a layer having a negative GSP_slope. As a result, the light-emitting device 2, which is a light-emitting device according to one embodiment of the present invention, can be a light-emitting device with good characteristics and a low driving voltage. In addition, since Li is not used as the first layer of the intermediate layer, the light-emitting device having the configuration of the present invention can be a light-emitting device with good characteristics in which an increase in driving voltage is suppressed even after a photolithography process.
[0549] Next, the results of determining the GSP_slope of the second layer (first electron transport layer) in light-emitting device 2 are shown. The GSP_slope of the second layer (first electron transport layer) was determined by fabricating a measurement device as shown in the table below. Note that the film thicknesses of the anode, hole injection layer, thin film 1, and cathode in Table 12 are design film thicknesses. Meanwhile, the film thickness of thin film 2 in the table below is the value measured using a spectroscopic ellipsometer (M-2000U manufactured by J.A. Woollam Japan) because an accurate value is required to calculate the GSP_slope.
[0550] [Table 12]
[0551] The structural formulas of the main organic compounds used in the measuring device L21 and the measuring device L22 are shown below.
[0552] [ka]
[0553] For the measurement devices L21 and L22, the substrate temperature was room temperature, the deposition rate was 0.2 nm / s to 0.4 nm / s, and deposition was performed without stopping deposition while forming one layer. For the measurement devices L21 and L22, the thin film 1 was formed of the same material as the second layer (first electron transport layer) in the light-emitting device 2, and the thin film 2 was formed of Alq3. The carriers in the measurement devices L21 and L22 were holes, and the carriers were accumulated in the thin film 2. The formulas for calculating GSP_slope were the formulas (3) and (4) shown in the first embodiment.
[0554] The capacitance-voltage characteristics of the measurement device L21 and the measurement device L22 are shown in Figure 37(A) and Figure 37(B). Note that the GSP_slope of Alq3 is known (48 (mV / nm)).
[0555] Table 13 shows the ordinary refractive index no , the electron injection voltage V of the measurement device obtained from Figure 37 i , threshold voltage V bi , the interface charge density σ calculated from the formula (3) shown in the first embodiment if_h , and GSP_slope calculated from equation (4).
[0556] [Table 13]
[0557] Thus, it was found that the second layer (first electron transport layer) in the light-emitting device 2 had a positive GSP_slope of 12.4 mV / nm, and that the GSP_slope of the first layer was opposite in sign to that of the first layer. In addition, the difference between the GSP_slope of the first layer and that of the second layer was 20 mV / nm or more.
[0558] As a result, the light-emitting device 2, which is a light-emitting device according to one embodiment of the present invention, can be a light-emitting device with low driving voltage and good characteristics. In addition, since Li is not used for the first layer of the intermediate layer, the light-emitting device having the configuration of the present invention can be a light-emitting device with good characteristics in which an increase in driving voltage is suppressed even after a photolithography process.
[0559] The results of determining the GSP_slope of the first light-emitting layer in light-emitting device 2 are also shown. The GSP_slope of the first light-emitting layer was determined by fabricating measurement device 3 as shown in the table below. Note that the film thicknesses of the reflective electrode, anode, hole injection layer, electron injection layer, cathode and cap layer in Table 14 are design film thicknesses. Meanwhile, the film thicknesses of thin film 1 and thin film 2 in the table below are values measured using a spectroscopic ellipsometer (M-2000U manufactured by J.A. Woollam Japan).
[0560] [Table 14]
[0561] The structural formulae of the main organic compounds used in the measuring device 3 are shown below.
[0562] [ka]
[0563] The measurement device 3 had a substrate temperature of room temperature and a deposition rate of 0.2 nm / s to 0.4 nm / s except for thin film 2. Thin film 2 was deposited by co-evaporation using three deposition sources, with deposition rates of 0.05 nm / s for 8mpTP-4mDBtPBfpm and βNCCP, and 0.01 nm / s for Ir(5mppy-d3)2(mbfpypy-d3). Deposition was continued without stopping deposition between the formation of each layer.
[0564] In the measuring device 3, the thin film 2 was formed with the same material and at the same deposition rate as the first light-emitting layer in the light-emitting device 2, and the thin film 1 was formed of 4,4'-bis[N-(1-naphthyl)-N-phenylamino]biphenyl (abbreviation: NPB). The carriers in this measuring device were holes, and the structure was such that the carriers were accumulated in the thin film 2. The formulas for calculating GSP_slope were the formulas (3) and (4) shown in the first embodiment.
[0565] The capacitance-voltage characteristics of the measurement device 3 are shown in Fig. 38. The GSP_slope of the NPB is known (5.5 (mV / nm)).
[0566] Table 15 shows the ordinary refractive index n2 of thin film 2. o , the electron injection voltage V of the measurement device 3 obtained from FIG. i , threshold voltage V bi , the interface charge density σ calculated from the formula (3) shown in the first embodiment if_h , and GSP_slope calculated from equation (4).
[0567] [Table 15]
[0568] Thus, it was found that the first light-emitting layer in the light-emitting device 2 had a positive GSP_slope of 51.3 mV / nm, and the positive and negative GSP_slope of the first layer was opposite to that of the first layer. In addition, the difference between the GSP_slope of the first layer and that of the first light-emitting layer was 20 mV / nm or more.
[0569] As a result, the light-emitting device 2, which is a light-emitting device according to one embodiment of the present invention, can be a light-emitting device with low driving voltage and good characteristics. In addition, since Li is not used for the first layer of the intermediate layer, the light-emitting device having the configuration of the present invention can be a light-emitting device with good characteristics in which an increase in driving voltage is suppressed even after a photolithography process. [Explanation of symbols]
[0570] 20 P type CGL 20c P type CGL 20d P type CGL 21 First Layer 21c First Layer 21d First Layer 22 Second Layer 22c Second Layer 22d Second Layer 50 interfacial charge 100 display device 100A display device 100B display device 100C display device 100E display unit 100D display device 101c anode 101d anode 101B Anode 101G anode 101R Anode 101 Anode 102 Cathode 103c Organic compound layer 103d Organic compound layer 103B Organic compound layer 103Bf Organic compound film 103G organic compound layer 103Gf organic compound film 103R Organic compound layer 103Rf Organic compound film 103 Organic compound layer 104 First EL layer 104R First EL layer 104G 1st EL layer 104B First EL layer 105 Second EL layer 110B subpixel 110G subpixel 110R subpixel 110 subpixels 111 Hole injection layer 111c Hole injection layer 111d Hole injection layer 112 Hole transport layer 112_1 Hole transport layer 112_2 Hole transport layer 112c_1 Hole transport layer 112c_2 Hole transport layer 112d_1 Hole transport layer 112d_2 Hole transport layer 112R conductive layer 112B Conductive layer 113 Light-emitting layer 113_1 Emitting layer 113_2 Emitting layer 113c_1 Emitting layer 113c_2 Emitting layer 113d_1 Light-emitting layer 113d_2 Emitting layer 114 Electron transport layer 114_1 Electron transport layer 114c_1 Electron transport layer 114c_2 Electron transport layer 114d_1 Electron transport layer 114d_2 Electron transport layer 115 Electron injection layer 117 Light blocking layer 120 Substrate 122 Resin layer 125f Inorganic insulating film 125 Inorganic insulating layer 126R conductive layer 126B Conductive layer 127a Insulating layer 127f Insulating film 127 Insulating Layer 128 layers 129R conductive layer 129B Conductive layer 130B Light Emitting Device 130c Light Emitting Device 130d Light-emitting device 130G Light Emitting Device 130R Light Emitting Device 130 Light Emitting Devices 131 Protective layer 132B Colored layer 132G colored layer 132R colored layer 140 Connection 141 areas 142 Adhesive layer 151B Conductive layer 151C conductive layer 151f Conductive film 151G conductive layer 151R conductive layer 151 Conductive layer 152B Conductive layer 152C conductive layer 152f Conductive film 152G Conductive layer 152R Conductive layer 152 Conductive layer 153 Insulating Layer 155 Common electrode 156B Insulating layer 156C Insulating layer 156f Insulating film 156G Insulation layer 156R Insulation layer 156 Insulating Layer 157 Light blocking layer 158B Sacrificial Layer 158Bf sacrificial film 158G Sacrificial Layer 158Gf sacrificial film 158R Sacrificial layer 158Rf Sacrificial film 159B Mask layer 159Bf Mask membrane 159G Mask layer 159Gf Mask Film 159R Mask layer 159Rf Mask Film 166 Conductive Layer 171 Insulating Layer 172 Conductive Layer 173 Insulating Layer 174 Insulating Layer 175 Insulating Layer 176 Plug 177 Pixel section 178 pixels 179 Conductive Layer 190B Resist mask 190G Resist Mask 190R Resist Mask 191 Resist Mask 201 Transistor 204 Connection 205 Transistor 211 Insulating layer 213 Insulating Layer 214 Insulating layer 215 Insulating Layer 221 Conductive Layer 222a conductive layer 222b Conductive layer 223 Conductive Layer 224B Conductive layer 224C conductive layer 224G conductive layer 224R conductive layer 231 Semiconductor Layer 240 capacity 241 Conductive Layer 242 Connection Layer 243 Insulating Layer 245 Conductive Layer 254 Insulating layer 255 Insulation Layer 256 Plug 261 Insulating Layer 271 Plug 280 Display Module 281 Display section 282 Circuit section 283a Pixel circuit 283 Pixel circuit section 284a pixels 284 Pixel section 285 Terminal section 286 Wiring section 290 FPC 291 Substrate 292 Substrate 301 Substrate 310 Transistor 311 Conductive layer 312 Low resistance region 313 Insulating Layer 314 Insulating layer 315 Element isolation layer 351 Substrate 352 Substrate 353 FPC 354 IC 355 Wiring 356 circuits 372 FPC 501 First Light Emitting Unit 501c First light emitting unit 501d First Light Emitting Unit 502 Second Light Emitting Unit 502c Second light emitting unit 502d Second Light Emitting Unit 513 Middle Class 513c middle tier 513d middle class 700 Substrates 701 Anode 702 Hole injection layer 703 First electron transport layer 704 Second electron transport layer 705 Electron injection layer 706 Cathode 700A electronic equipment 700B Electronic equipment 721 Case 723 Mounting Part 727 Earphones 750 Earphones 751 Display Panel 753 Optical Components 756 Display area 757 Frames 758 Nose pad 800 boards 800A electronic equipment 800B Electronic equipment 801 Anode 802 Hole injection layer 803 First hole transport layer 804 Second hole transport layer 805 Electron injection layer 806 Cathode 820 Display section 821 Case 822 Communications Department 823 Mounting part 824 Control Unit 825 Imaging unit 827 Earphones 832 Lens 6500 Electronic equipment 6501 Case 6502 Display section 6503 Power button 6504 Button 6505 Speaker 6506 Microphone 6507 Camera 6508 Light source 6510 Protective materials 6511 Display Panel 6512 Optical components 6513 Touch Sensor Panel 6515 FPC 6516 IC 6517 Printed Circuit Board 6518 Battery 7000 Display 7100 Television equipment 7151 Remote control device 7171 Case 7173 Stand 7200 Notebook Personal Computer 7211 Case 7212 Keyboard 7213 Pointing Device 7214 External connection port 7300 Digital Signage 7301 Case 7303 Speaker 7311 Information terminal 7400 Digital Signage 7401 Pillar 7411 Information terminal 9000 Chassis 9001 Display section 9002 Camera 9003 Speaker 9005 Operation key 9006 Connection terminal 9007 Sensor 9008 Microphone 9050 Icon 9051 Information 9052 Information 9053 Information 9054 Information 9055 Hinge 9171 Mobile Information Terminal 9172 Mobile Information Terminal 9173 Tablet PC 9200 Mobile Information Terminal 9201 Mobile information terminals
Claims
1. A first electrode; a second electrode facing the first electrode; a first light-emitting layer and a second light-emitting layer between the first electrode and the second electrode; a first layer between the first light-emitting layer and the second light-emitting layer; A light-emitting device in which the GSP_slope (mV / nm) of the first layer is a value with an opposite sign to the GSP_slope (mV / nm) of the first light-emitting layer (where GSP_slope (mV / nm) is a parameter expressed as V / d when the potential of the surface of the film is V (mV) and the film thickness is d (nm).)
2. A first electrode formed on a substrate; a second electrode facing the first electrode; a first light-emitting layer and a second light-emitting layer between the first electrode and the second electrode; a first layer between the first light-emitting layer and the second light-emitting layer; A light-emitting device in which the GSP_slope (mV / nm) of the first layer exhibits a negative value. (Note that GSP_slope (mV / nm) is a parameter expressed as V / d when the potential of the surface of the film is V (mV) and the film thickness is d (nm).)
3. A first electrode; a second electrode facing the first electrode; a first light-emitting layer and a second light-emitting layer between the first electrode and the second electrode; an electron transport layer and a first layer between the first light-emitting layer and the second light-emitting layer; A light-emitting device in which the GSP_slope (mV / nm) of the first layer is a value with a positive / negative sign opposite to that of the GSP_slope (mV / nm) of the electron transport layer (wherein GSP_slope (mV / nm) is a parameter expressed as V / d when the potential of the surface of the film is V (mV) and the film thickness is d (nm).
4. A first electrode formed on a substrate; a second electrode facing the first electrode; a first light-emitting layer and a second light-emitting layer between the first electrode and the second electrode; an electron transport layer and a first layer between the first light-emitting layer and the second light-emitting layer; The GSP_slope (mV / nm) of the electron transport layer is a positive value, A light-emitting device in which the GSP_slope (mV / nm) of the first layer exhibits a negative value. (Note that GSP_slope (mV / nm) is a parameter expressed as V / d when the potential of the surface of the film is V (mV) and the film thickness is d (nm).)
5. A first electrode formed on a substrate; a second electrode facing the first electrode; a first light-emitting layer, an electron transport layer, an intermediate layer, and a second light-emitting layer are disposed between the first electrode and the second electrode in this order from the first electrode side; the intermediate layer has a first layer and a second layer in this order from the first electrode side, the electron transport layer and the first layer are in contact with each other; The GSP_slope (mV / nm) of the electron transport layer is a positive value, A light-emitting device in which the GSP_slope (mV / nm) of the first layer exhibits a negative value. (Note that GSP_slope (mV / nm) is a parameter expressed as V / d when the potential of the surface of the film is V (mV) and the film thickness is d (nm).)
6. In claim 5, The second layer is a charge generating layer.
7. In any one of claims 1 to 6, The first layer has a hole blocking function.
8. In any one of claims 1 to 6, The hole mobility of the first layer when the square root of the electric field intensity [V / cm] is 600 is 1×10 -8 cm 2 / Vs or less.
9. In any one of claims 1 to 6, A light-emitting device, wherein the first layer includes a first material having any one of a pyrrolidine skeleton, a piperidine skeleton, and a hexahydropyrimidopyrimidine skeleton.
10. In any one of claims 1 to 6, the first layer having a first material and a second material; the first substance is an organic compound having any one of a pyrrolidine skeleton, a piperidine skeleton, and a hexahydropyrimidopyrimidine skeleton, The second substance is an organic compound having an electron transporting property.
11. In any one of claims 3 to 6, A light-emitting device, wherein the difference between a GSP_slope (mV / nm) value of the electron transport layer and a GSP_slope (mV / nm) value of the first layer is 20 (mV / nm) or more.
12. In any one of claims 1 to 6, The spin density of the first layer is 1×10 17 spins / cm 3 2. A light emitting device, comprising:
Citation Information
Patent Citations
Method for high-resolution patterning of an organic layer
JP2018521459A
Organic thin film and method for producing organic thin film, organic electroluminescent element, display device, lighting device, organic thin film solar cell, photoelectric conversion element, thin film transistor, coating composition and material for organic electroluminescent elements
WO2021045178A1