Packaging container, packaging container with contents, method of shutting off moisture, and method of manufacturing packaging container

A packaging container with a supercritical nitrogen-derived sea-island structure enhances water vapor barrier properties without increasing thickness or material use, addressing environmental concerns and extending product shelf life.

JP2024147196APending Publication Date: 2024-10-16TOPPAN HOLDINGS INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023060055
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-03
Publication Date
2024-10-16

AI Technical Summary

Technical Problem

Existing packaging containers for granular refreshing products face challenges in improving water vapor barrier properties without increasing environmental impact, as methods like increasing wall thickness or laminating barrier films lead to higher resin use and reduced recyclability.

Method used

A packaging container design featuring a sea-island structure with closed cells derived from supercritical nitrogen, forming a labyrinth effect and permeation resistance, which enhances water vapor barrier properties without increasing thickness or using additional materials.

Benefits of technology

The design improves water vapor barrier properties while minimizing environmental load by reducing resin use and maintaining structural integrity, thus extending product shelf life and reducing material waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024147196000001_ABST
    Figure 2024147196000001_ABST
Patent Text Reader

Abstract

To provide a packaging container allowed to enhance the water-vapor barrier properties while suppressing the increase of the burden on environment, a packaging container with contents, and methods of shutting off moisture and methods of manufacturing a packaging container.SOLUTION: A resin packaging container 1 comprises a bottom member 2 and a lid member 3 that forms an accommodation space S with the bottom member 2 by being fitted with the bottom member 2. At least one of the bottom member 2 and the lid member 3 has a bubble region R where the aggregate density of independent bubbles having an inner diameter equal to or greater than 10 μm becomes 10 count / mm2 or more.SELECTED DRAWING: Figure 6
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a packaging container, a packaging container containing a content, a moisture blocking method, and a method for manufacturing a packaging container. [Background technology]

[0002] Conventionally, resin packaging containers for dispensing granular cooling materials and the like have been known (e.g., Patent Documents 1 and 2). These are card-shaped cases in which a tray-shaped bottom member and a lid member fit together, and a hinge cap molded integrally with the bottom member can be opened and closed. These have the characteristics of a small number of parts, low cost, excellent portability, and high pressure resistance. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 3657351 [Patent Document 2] Patent No. 3953581 Summary of the Invention [Problem to be solved by the invention]

[0004] Incidentally, the deterioration rate of foods such as cooling granules can be slowed down by suppressing moisture absorption. Therefore, the expiration date can be extended by improving the water vapor barrier property of the packaging container. Possible means for improving the water vapor barrier property of the packaging container include a method of increasing the thickness of the packaging container and a method of laminating a barrier film on the packaging container.

[0005] However, when the thickness of the packaging container is increased, the amount of resin used increases, which causes a problem of a large environmental load.In addition, when a barrier film is laminated on a packaging container, the number of materials used for the packaging container increases, which reduces recyclability, which causes a problem of a large environmental load.

[0006] Therefore, an object of the present invention is to provide a packaging container, a packaging container containing contents, a moisture blocking method, and a method for manufacturing a packaging container that can enhance water vapor barrier properties while suppressing an increase in environmental load. [Means for solving the problem]

[0007] The present invention provides at least the following [1] to

[12] .

[0008] [1] A method for manufacturing a thermoplastic resin composition comprising: a first member; and a second member that is fitted to the first member to form a storage space between the first member and the second member; wherein at least one of the first member and the second member has an inner diameter of 10 μm or more and a density of closed bubbles of 10 bubbles / mm 2 A resin packaging container having an air bubble region of at least 100%.

[0009] In this packaging container, the contents can be stored in the storage space formed between the first member and the second member. At least one of the first member and the second member has a density of closed bubbles having an inner diameter of 10 μm or more of 10 bubbles / mm 2 In other words, the bubble region has 10 independent bubbles with an inner diameter of 10 μm or more at a rate of 10 bubbles / mm 2 They exist at a density of 100 μm or more. Therefore, in the bubble region, the resin and the closed bubbles form an island structure, which is thought to create a maze effect that complicates the path of water vapor passing through the resin. In addition, in the bubble region, the water vapor permeability coefficient differs between the resin and the closed bubbles, so the boundary between the resin and the closed bubbles is thought to act as a resistance to water vapor permeation. It is thought that such a maze effect and permeation resistance make it difficult for water vapor to permeate, so the water vapor barrier property can be improved without increasing the thickness of the packaging container or laminating a barrier film on the packaging container. Therefore, the water vapor barrier property can be improved while suppressing an increase in the environmental load.

[0010] [2] The packaging container according to [1], wherein at least one of the first member and the second member has a flat thin-walled portion having a thickness of 0.7 mm or less, and the thin-walled portion has the bubble region. In this packaging container, since at least one of the first member and the second member has a flat thin-walled portion having a thickness of 0.7 mm or less, the amount of resin used in the packaging container can be reduced, and the increase in environmental load can be further suppressed. Moreover, since the thin-walled portion has a bubble region, the water vapor barrier property can be improved even in the thin-walled portion.

[0011] [3] The packaging container according to [1] or [2], wherein the closed bubbles are derived from nitrogen in a supercritical state. In this packaging container, since the closed bubbles are derived from nitrogen in a supercritical state, the packaging container is easily foamed during production, and the inner diameter of the closed bubbles formed by the foaming is about 10 μm or more and 70 μm or less. Such fine closed bubbles give the resin a complex and fine three-dimensional structure, so that the rigidity and shape stability of the packaging container are increased even if the packaging container is thin. This makes it possible to suppress a decrease in the water vapor barrier property due to the bending of the packaging container.

[0012] [4] The packaging container according to any one of [1] to [3], wherein the first member has a bottom plate portion, a side plate portion rising from the periphery of the bottom plate portion and fitting into the second member, an opening formed in the side plate portion, and a hinge cap for opening and closing the opening. In this packaging container, the first member has a bottom plate portion, a side plate portion rising from the periphery of the bottom plate portion and fitting into the second member, an opening formed in the side plate portion, and a hinge cap for opening and closing the opening, so that the contents can be contained airtightly by closing the hinge cap, and the contained contents can be removed by opening the hinge cap.

[0013] [5] The packaging container according to [4], wherein the side plate portion has the bubble region and is discontinuous in the direction along the periphery of the bottom plate portion due to the opening. In this packaging container, since the side plate portion is discontinuous in the direction along the periphery of the bottom plate portion due to the opening, the side plate portion is easily deflected near the opening. If the side plate portion deflects near the opening, a gap is generated between the hinge cap and the side plate portion, and water vapor may enter through the gap. However, since the side plate portion has a bubble region, the resin in the side plate portion has a complex three-dimensional structure due to the closed bubbles, and the rigidity and shape stability of the side plate portion are increased. In particular, when the closed bubbles are derived from nitrogen in a supercritical state, the rigidity and shape stability of the side plate portion are further increased. Therefore, it is possible to suppress the deterioration of the water vapor barrier property caused by the deflection of the side plate portion.

[0014] [6] Water vapor permeability is 1.60g / mm 2 The packaging container according to any one of [1] to [5], wherein the water vapor transmission rate is 1.60 g / mm 2 / day or less, moisture absorption of the contents can be suppressed.

[0015] [7] A content-containing packaging container comprising the packaging container according to any one of [1] to [6] and a content accommodated in the packaging container. Since the content-containing packaging container comprises the packaging container described above, it is possible to enhance water vapor barrier properties while suppressing an increase in environmental load.

[0016] [8] A moisture blocking method comprising the steps of: storing contents in the packaging container according to any one of [1] to [6]; and retaining the contents in the packaging container. In this moisture blocking method, the contents are stored in the packaging container and retained, so that it is possible to enhance the water vapor barrier property while suppressing an increase in the environmental load.

[0017] [9] A method for producing the packaging container according to any one of [1] to [6], comprising: (A) a step of mixing a resin material and a supercritical fluid to prepare a molten resin composition; (B) a step of injecting the molten resin composition into a cavity of a mold; and (C) after the step (B), mixing at least a part of the supercritical fluid into a molten resin composition having an inner diameter of 10 μm or more and a population density of 10 particles / mm. 2 and a step of foaming the foam to form the above-mentioned closed cells.

[0018] In this method for producing a packaging container, a molten resin composition in which a resin material and a supercritical fluid are mixed is injected into a cavity of a mold, and at least a part of the supercritical fluid is mixed into a molten resin having an inner diameter of 10 μm or more and a population density of 10 particles / mm 2 Since the foam is expanded to form the above-mentioned closed cells, a packaging container can be produced that can enhance the water vapor barrier property while suppressing an increase in the environmental load.

[0019]

[10] The method for producing a packaging container according to [9], wherein the supercritical fluid is nitrogen in a supercritical state. In this method for producing a packaging container, since the supercritical fluid is nitrogen in a supercritical state, a packaging container having high rigidity and shape stability can be produced even if it has a thin wall thickness.

[0020]

[11] The method for producing a packaging container according to

[10] , wherein the mass of the nitrogen as the supercritical fluid in the molten resin composition is 0.5 to 1.0 parts by mass when the mass of the resin material in the molten resin composition is 100 parts by mass. This amount is a quantity in which at least a part of the supercritical fluid is mixed with a molten resin having an inner diameter of 10 μm or more and a population density of 10 particles / mm 2 This is suitable for foaming to form the above-mentioned closed cells. Effect of the Invention

[0021] According to the present invention, it is possible to improve the water vapor barrier property while suppressing an increase in the environmental load. [Brief description of the drawings]

[0022] [Figure 1]FIG. 1 is a perspective view of a packaging container according to one embodiment of the present invention. [Diagram 2] FIG. 4 is a plan view of the bottom member as viewed from the inner surface side. [Diagram 3] 3A is an end view taken along line IIIA-IIIA in FIG. 2, and FIG. 3B is a cross-sectional view taken along line IIIB-IIIB in FIG. [Figure 4] FIG. 4 is a plan view of the cover member as viewed from the inner surface side. [Diagram 5] 4. (A) is an end view taken along line VA-VA in FIG. 4. (B) is a cross-sectional view taken along line VB-VB in FIG. [Figure 6] FIG. 2 is an end view showing the vicinity of a side surface of the packaging container. [Figure 7] FIG. 2 is a schematic cross-sectional view of a bottom member and a cover member. [Figure 8] 3 is a plan view of the bottom member corresponding to FIG. 2, showing measurement positions for evaluating the water vapor permeability of the bottom member. FIG. [Figure 9] 13 is a graph showing the results of moisture proof evaluation of the entire packaging container. [Figure 10] 1 is a graph showing measured values ​​of water vapor transmission rate of a base member. [Figure 11] 1 is a graph showing measured values ​​of water vapor transmission rate after 6 hours. [Figure 12] 1 is a graph showing measured water vapor transmission rates after 12 hours. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] A preferred embodiment of the present invention will be described in detail below with reference to the drawings. In each drawing, the same or corresponding parts are given the same reference numerals, and duplicated explanations will be omitted. In this specification, a numerical range indicated using "~" indicates a range including the numerical values ​​before and after "~" as the minimum and maximum values, respectively. The packaging container of this embodiment is a card-shaped case with a hinged cap for putting contents such as granular cooling materials into the case and dispensing them in small portions.

[0024] <Packaging container> As shown in Figs. 1 to 6, the packaging container 1 of this embodiment is a resin container, and is formed by fitting together a tray-shaped bottom member 2, which is a first member, and a tray-shaped lid member 3, which is a second member. In the packaging container 1, a storage space S for storing contents is formed between the bottom member 2 and the lid member 3. The packaging container 1 is substantially rectangular (here, a rectangle with rounded corners) in a plan view, and has an opening 5 on one long side. The outer shape of the packaging container 1 may be substantially polygonal, substantially square, substantially circular, substantially elliptical, or other irregular shapes. Examples of irregular shapes include a shape in which the center is curved or bent and narrowed (also called a Daruma shape, a snowman shape, a gourd shape, etc.). A hinge cap 22 is integrally formed with the bottom member 2 via a thin, bendable hinge 21, which allows the opening 5 to be closed. The cap that closes the opening 5 may be a cap without a hinge. In this specification, the direction in which the bottom member 2 and the cover member 3 are fitted together is referred to as the "thickness direction", and any direction perpendicular thereto is referred to as the "width direction".

[0025] The packaging container 1 may have any size. The following two sizes are given as examples of the size:

[0026] Dimension A type: The length of the long side of the rounded rectangle may be 55 mm or more and 100 mm or less, 60 mm or more and 90 mm or less, or 70 mm or more and 85 mm or less. The length of the short side of the rounded rectangle may be 30 mm or more and 70 mm or less, 40 mm or more and 60 mm or less, or 45 mm or more and 55 mm or less. The thickness of the packaging container 1 in the thickness direction may be 5 mm or more and 9 mm or less, or 6 mm or more and 8 mm or less.

[0027] Dimension B type: The length of the long side of the rounded rectangle may be 60 mm or more and 120 mm or less, 70 mm or more and 110 mm or less, or 80 mm or more and 100 mm or less. The length of the short side of the rounded rectangle may be 30 mm or more and 70 mm or less, 40 mm or more and 60 mm or less, or 50 mm or more and 55 mm or less. The thickness of the packaging container 1 in the thickness direction may be 9 mm or more and 13 mm or less, or 10 mm or more and 12 mm or less.

[0028] In addition to the above-mentioned dimension A type and dimension B type, the length in the width direction of the packaging container 1 may be 30 mm or more and 150 mm or less, or 50 mm or more and 120 mm or less. The thickness in the thickness direction of the packaging container 1 may be 5 mm or more and 90 mm or less, or 5 mm or more and 40 mm or less, or 5 mm or more and 20 mm or less.

[0029] The bottom member 2 and the cover member 3 are also substantially rectangular (rounded rectangle), but the portion forming the opening 5 is a recess recessed inward into the rectangle. The bottom member 2 and the cover member 3 each have a bottom plate portion 23, 33 that extends in the width direction, and a side plate portion 24, 34 that rises and extends in the thickness direction from the periphery of the bottom plate portion 23, 33. The bottom plate portion 23, 33 and the side plate portion 24, 34 are flat thin-walled portions having a thickness of 0.7 mm or less. The side plate portion 24, 34 is continuous along the periphery of the bottom plate portion 23, 33 except for the portion that becomes the opening 5 of the packaging container 1. In other words, the side plate portion 24, 34 is cut out by the opening 5, and is discontinuous in the direction along the periphery of the bottom plate portion 23, 33 by the opening 5.

[0030] On the inner surface of the bottom plate portion 23 of the bottom member 2, cylindrical bosses 25 (25a, 25b, 25c, 25d, 25e) are formed at a total of five locations: four locations near each of the four rounded corners, and a location along the long side on the side where the opening 5 is located that is closer to the opening 5 side than the center of the long side. The bosses 25 protrude vertically from the bottom plate portion 23, and each is formed at a position separated from the side plate portion 24 in the width direction.

[0031] For example, as shown in Fig. 3(B), boss 25d is a hollow cylinder protruding in the thickness direction, and the hollow portion is partitioned by a partition wall (a wall forming the cylinder) to form a boss hole. The depth of the boss hole is equal to the height of boss 25d. This structure is common to all bosses 25.

[0032] A support pillar 27 is formed in the center of the inner surface of the bottom plate portion 23 of the bottom member 2. The support pillar 27 protrudes vertically from the bottom plate portion 23. The support pillar 27 does not contribute to the fitting of the bottom member 2 and the lid member 3. The top of the support pillar 27 may or may not be in contact with the bottom plate portion 33 of the lid member 3. When a load is applied in the thickness direction of the packaging container 1, the top of the support pillar 27 can abut against the bottom plate portion 33 of the lid member 3 to resist the load.

[0033] Among the rounded corners of the bottom plate portion 23, a guide rib 28 for guiding the contents to the opening 5 is provided near the rounded corner closest to the opening 5. The guide rib 28 is a plate-shaped wall protruding vertically from the bottom plate portion 23 and is integrated with the boss 25a. The guide rib 28 extends linearly from the boss 25a so as to form a part of a tangent to a circle when the cylindrical shape of the boss 25a is viewed from its axial direction, and extends to a position where it does not contact the side plate portion 24 forming the short side of the packaging container 1. The distance between the guide rib 28 and the side plate portion 24 may be the same as the distance between the boss 25 and the side plate portion 24. In this composite of the integrated boss 25a and the guide rib 28, the boss 25a contributes to the fitting of the bottom member 2 and the cover member 3, and the guide rib 28 does not contribute to the fitting of the bottom member 2 and the cover member 3.

[0034] On the other hand, on its inner surface, the bottom plate portion 33 of the cover member 3 has pins 35 (35a, 35b, 35c, 35d, 35e) formed at positions corresponding to each of the bosses 25 (25a, 25b, 25c, 25d, 25e) formed on the bottom plate portion 23 of the bottom member 2.

[0035] For example, as shown in Fig. 5(B), pin 35d is a hollow cylinder protruding in the thickness direction, and is partitioned by partition walls (walls forming the cylinder) to give it a rod-like shape as a whole. The outer diameter of the cylinder is approximately the same as the inner diameter of boss 25d, and is designed to fit into the boss hole. This structure is common to all pins 35.

[0036] Guides 39 are formed on the inner surface of the bottom plate 33 of the lid member 3 at positions along the side plate 34. The guides 39 are formed in eight positions in total: two along the long side having the opening 5, three along the other long side, one on one of the short sides closer to the opening 5, and two on the other short side. Each guide 39 is formed by rising vertically from the bottom plate 23, and each is located slightly away from the side plate 34. In the packaging container 1, the guides are located near the inside of the stepped portion 24a of the bottom member 2 to prevent the fitting state from shifting excessively (see FIG. 6).

[0037] The bottom member 2 has thin-walled recesses 26 in its bottom plate portion 23, where the thickness is reduced. The thin-walled recesses 26 are formed in three rows in a rectangular shape in a plan view extending in the long side direction. The cover member 3 also has thin-walled recesses 36 formed in a similar manner in its bottom plate portion 33. These thin-walled recesses 26, 36 correspond to reduced thickness portions for suppressing the occurrence of warpage in injection molding, which will be described later.

[0038] The total area of ​​the thin-walled recesses 26 in the bottom plate portion 23 and the total area of ​​the thin-walled recesses 36 in the bottom plate portion 33 may be 10% to 80%, 15% to 70%, or 20% to 60%, with the area of ​​the inner surfaces of the bottom member 2 and the lid member 3 of the bottom plate portions 23, 33 that extend in the width direction (the total area of ​​the thin-walled recess portions and the non-thin-walled recess portions) being 100%.

[0039] As shown in Fig. 3, the side plate portion 24 of the bottom member 2 has a step at its end, and is divided into a raised step portion 24a and a lowered step portion 24b along the inner peripheral surface. From the viewpoint of improving the airtightness of the packaging container 1, it is preferable that the step is provided on the entire outer periphery except for the opening 5. At least one of the raised step portion 24a and the lowered step portion 24b abuts against the side plate portion 34 of the lid member 3 when the bottom member 2 and the lid member 3 are fitted together, thereby playing a role in sealing the bottom member 2 and the lid member 3. Here, the tip of the raised step portion 24a is located between the side plate portion 34 of the lid member 3 and the guide 39, as shown in Fig. 6.

[0040] In the packaging container 1, the bottom member 2 and the lid member 3 are fitted together by fitting the boss 25 and the pin 35 together, and the shape is fixed. As shown in FIG. 6, the side plate portion 24 of the bottom member 2 and the side plate portion 34 of the lid member 3 form the side surface of the packaging container 1. Here, the distance L between the inner surface of the bottom plate portion 23 of the bottom member 2 and the inner surface of the bottom plate portion 33 of the lid member 3 must be greater than the thickness of the contents to be filled. For example, in the above-mentioned "dimension A type", the distance L may be 5.0 mm to 6.0 mm, or 5.2 mm to 5.8 mm. In the above-mentioned "dimension B type", the distance L may be 7.0 mm to 9.0 mm, or 7.5 mm to 8.5 mm.

[0041] The height of each part will be described. The height of the boss 25 and the pin 35 may be 30% to 100%, 40% to 90%, or 50% to 80% of the distance L. However, since the boss 25 and the pin 35 need to fit together, the sum of their heights needs to be greater than the distance L.

[0042] The height of guide 39 may be 5% to 40%, 10% to 35%, or 20% to 30% of distance L. The height of guide 39 may be 1.0 mm to 2.0 mm, or 1.3 mm to 1.7 mm.

[0043] The thickness of each part will be described. The thickness T1 of the part (flat part) of the bottom plate part 23, 33 other than the thin recessed part 26, 36 is 0.70 mm or less. This thickness T1 may be 0.65 mm or less, 0.60 mm or less, 0.55 mm or less, 0.50 mm or less, 0.45 mm or less, 0.40 mm or less, or 0.35 mm or less. The specific range of the thickness T1 may be 0.50 mm to 0.70 mm, 0.55 mm to 0.65 mm, or 0.58 mm to 0.63 mm. The thickness T2 of the thin recessed part 26, 36 may be 0.50 mm or less, 0.45 mm or less, 0.40 mm or less, or 0.35 mm or less. A specific range of the thickness T2 may be 0.35 mm to 0.55 mm, 0.40 mm to 0.53 mm, or 0.44 mm to 0.52 mm. As for the thickness ratio, the thickness T2 in the thin recesses 26, 36 is 80% or less, or may be 75% or less, or may be 70% or less of the thickness T1 of the portion other than the thin recesses 26, 36. When T1 and T2 are values ​​that satisfy these numerical ranges, the occurrence of a phenomenon in which the resin material does not reach the flow end of the cavity (hereinafter referred to as "short shot") is easily suppressed.

[0044] The thickness T2 of the thin recesses 26, 36 may be 40% or more, 50% or more, or 60% or more of the thickness T1 of the portion other than the thin recesses 26, 36. Alternatively, the thickness T2 of the thin recesses 26, 36 may be 70% to 80%, 71% to 79%, or 72% to 78% of the thickness T1 of the portion other than the thin recesses 26, 36.

[0045] The thickness T4 (FIG. 3(A)) of the side plate portion 24, 34 may be the same as the thickness T1 of the portion of the bottom plate portion 23, 33 that is not the thin recessed portion 26, 36, except for the portion where the stepped portion 24a is formed. Alternatively, the thickness T4 of the side plate portion 24, 34 may be 110% to 180%, or 130% to 150%, of the thickness T1 of the bottom plate portion 23, 33, taking into consideration the formation of the stepped portion 24a. Alternatively, the thickness T4 of the side plate portion 24, 34 may be 250% to 350%, or 270% to 300% of the thickness T1 of the bottom plate portion 23, 33, taking into consideration the formation of the stepped portion 24a. The specific range of the thickness T4 may be 1.50 mm to 2.00 mm, 1.60 mm to 1.90 mm, or 1.65 mm to 1.80 mm.

[0046] In boss 25d, the thickness T3 of the partition wall separating the inside and outside of the boss hole may be 0.60 mm to 1.00 mm, 0.60 mm to 0.90 mm, 0.80 mm to 0.90 mm, or 0.60 mm to 0.80 mm. The thickness T3 of the partition wall may be 90% to 150%, 100% to 140%, or 110% to 130% of the thickness T1 of the portion of bottom plate portion 23 other than thin recess 26. This value is the same for bosses 25 other than boss 25d.

[0047] The thickness of the guide rib 28 is the same as the thickness T3 of the partition wall of the boss 25d. Alternatively, the thickness of the guide rib 28 may be different from the thickness T3 of the partition wall of the boss 25d. In either case, it is preferable that the thickness of the guide rib 28 does not become an obstacle when the cover member 3 and the bottom member 2 are fitted together.

[0048] The resin constituting the bottom member 2 and the cover member 3 is preferably a thermoplastic resin, and in particular, a polypropylene resin or a polyethylene resin. The resin constituting the bottom member 2 and the cover member 3 may contain a polypropylene resin or a polyethylene resin, and a resin other than the polypropylene resin and the polyethylene resin.

[0049] When the packaging container 1 is formed by injection molding, the melt flow rate of the thermoplastic resin is preferably 15 g / 10 min or more, more preferably 20 to 40 g / 10 min, and even more preferably 25 to 36 g / 10 min. When this value is 15 g / 10 min or more, the occurrence of short shots in injection molding tends to be easily suppressed, while when it is 40 g / 10 min or less, a molded product with excellent drop resistance tends to be produced. This melt flow rate may be 50 g / 10 min or less. The melt flow rate (MFR) here means a value measured under conditions of a temperature of 230° C. and a load of 2.16 kg in accordance with the method described in JIS K7210-1:2014.

[0050] The lid member 3 and the bottom member 2 are fitted together to form the packaging container 1. When fitting, as explained with reference to Figures 3(B) and 5(B), the outer peripheral surfaces of the pins 35c, 35d come into contact with the inner peripheral surfaces of the bosses 25c, 25d, generating friction to allow the fitting to occur. At the same time, the stepped portion 24a of the side plate portion 24 enters the inside of the side plate portion 34, and the bottom member 2 and the lid member 3 are closed.

[0051] 7, at least one of the bottom member 2 and the cover member 3 has a bubble region R. In the present embodiment, as an example, both the bottom member 2 and the cover member 3 have a bubble region R, and all of the bottom plate portion 23, the side plate portion 24, and the boss 25 of the bottom member 2, and all of the bottom plate portion 33, the side plate portion 34, and the pin 35 of the cover member 3 have a bubble region R. The bubble region R is a region in which the density of closed bubbles B having an inner diameter of 10 μm or more is 10 bubbles / mm 2 In other words, the bubble region R is a region where the number of independent bubbles B having an inner diameter of 10 μm or more is 10 / mm 2 The area where the density of the independent bubbles B having an inner diameter of 10 μm or more is 10 pieces / mm 2 Any region not exceeding this size is not the bubble region R of this embodiment. Also, in the bubble region R, microbubbles having an inner diameter of less than 10 μm may be present.

[0052] "Closed cells" refers to spaces that exist in a molded product and in which gas is trapped. Each of the closed cells B exists as a space that is independent of the others. The closed cells B are, for example, bubbles that originate from the manufacturing method described below, and specifically, bubbles that are formed by foaming a supercritical fluid. Examples of supercritical fluids include nitrogen (N2) in a supercritical state and carbon dioxide (CO2) in a supercritical state.

[0053] The "inner diameter" refers to the diameter of the circumscribing circle when the closed cell B is optically observed, and can be measured using an optical microscope.

[0054] The "collection density of closed cells" means the number of closed cells B per unit area. In counting the number of closed cells B, an area of ​​0.2 mm square may be observed using an optical microscope (KH7000, manufactured by HiROX) and the number of closed cells B whose cross sections are located on the cross section of the molded article may be counted, or if the resin is transparent, the number of closed cells B up to a depth observable by cross-sectional observation may be counted.

[0055] The gas constituting the closed bubbles B is preferably nitrogen or carbon dioxide used in the manufacturing method described below. When the bottom member 2 and the cover member 3 contain the closed bubbles B, the curing shrinkage of the resin after manufacturing is suppressed, and the occurrence of warping is also suppressed.

[0056] The bottom member 2 and the lid member 3 may have a bubble region R and surface layers L1 and L2 located on the inner surface 1a and the outer surface 1b of the packaging container 1 so as to sandwich the bubble region R. The surface 1a is the surface on the side of the storage space S of the packaging container 1, and the surface 1b is the surface on the opposite side of the storage space S of the packaging container 1. The bubble region R is a layer that is not exposed to the surface 1a and the surface 1b of the packaging container 1. The surface layers L1 and L2 are layers that do not have the bubble region R and are exposed to the surface 1a and the surface 1b of the packaging container 1. The surface layer L1 is a layer that forms the surface 1a of the packaging container 1, and the surface layer L2 is a layer that forms the surface 1b of the packaging container 1. The bubble region R and the surface layers L1 and L2 are integrally formed, and no physical boundary such as an interface is formed between them. As described below, it is believed that water vapor is less likely to permeate through the bubble region R due to the labyrinth effect and permeation resistance of the closed bubbles B, and in view of this belief, it is preferable that as many closed bubbles B as possible are present in the bubble region R. However, if the bubble region R is located on the surface 1a and the surface 1b of the packaging container 1, the appearance of the packaging container 1 is likely to deteriorate. For this reason, by providing the surface layers L1 and L2 on either side of the bubble region R, deterioration of the appearance of the packaging container 1 can be suppressed.

[0057] The inner diameter of the closed bubbles B in the bubble region R is less than the wall thickness of the packaging container 1, for example, less than 0.7 mm. When the surface layer L1 and the surface layer L2 are provided, the inner diameter of the closed bubbles B is less than the thickness of the bubble region R sandwiched between the surface layer L1 and the surface layer L2. The inner diameter of the closed bubbles B in the bubble region R may be, for example, 10 μm to 1000 μm, 15 μm to 800 μm, 15 μm to 500 μm, or 15 μm to 200 μm. When the closed bubbles B are derived from nitrogen in a supercritical state, the inner diameter of the closed bubbles B in the bubble region R is, for example, 10 μm to 150 μm, or 10 μm to 100 μm, or 10 μm to 50 μm. When the closed bubbles B are derived from carbon dioxide in a supercritical state, the inner diameter of the closed bubbles B in the bubble region R is, for example, 40 μm or more and 1000 μm or less, or 50 μm or more and 500 μm or less, or 50 μm or more and 180 μm or less.

[0058] The density of the independent bubbles B having an inner diameter of 10 μm or more in the bubble region R is, for example, 10 bubbles / mm 2 More than 800 pieces / mm 2 It may be less than 10 pieces / mm 2 More than 500 pieces / mm 2 It may be less than 20 pieces / mm 2 More than 500 pieces / mm 2 It may be the following.

[0059] The water vapor permeability of the packaging container 1 is, for example, 1.60 g / mm 2 / day or less, 1.55g / mm 2 / day or less, or 1.40g / mm 2 / day.

[0060] "Water vapor permeability" refers to the water vapor permeability measured using a water vapor permeability measuring device when the change in the measurement result falls below a certain level. Measurements of water vapor permeability are performed at 1.5 hour intervals from the start of measurement, and when the "change rate" from the measurement value at the previous measurement point is within ±10% for three or more consecutive measurement points, the average value of the first three points is regarded as the water vapor permeability.

[0061] The "rate of change" is expressed as "[(measurement result from the immediately preceding measurement)-(measurement result from the current measurement)] / (measurement result from the immediately preceding measurement)".

[0062] Since gas (water vapor) is originally taken into the resin, it takes a certain amount of time for this gas (water vapor) to be completely replaced by carrier gas during measurement. In other words, the water vapor permeability value changes over time from the start of measurement due to the influence of the gas (water vapor) originally taken into the resin. Therefore, in order to eliminate the influence of the gas (water vapor) originally taken into the resin, the water vapor permeability is measured not at a specific point in time, but at the measurement result when the change falls below a certain level (the average value of the measurement results at multiple points in time).

[0063] The water vapor permeability of the packaging container 1 is measured with the hinge cap 22 closed. The water vapor permeability of the packaging container 1 is measured, for example, by using a MOCON water vapor permeability measuring device (PERMATRAN-W 3 / 34, manufactured by AMETEK MOCON) with the bottom plate portions 23, 33 as the measurement object.

[0064] <Method of shielding against moisture> A moisture blocking method will now be described. The moisture blocking method of this embodiment includes a step of storing contents in the above-mentioned packaging container 1, and a step of retaining the contents in the packaging container 1. In the step of storing the contents in the packaging container 1, the hinge cap 22 is opened, and the contents are placed in the storage space S through the opening 5. In the step of retaining the contents in the packaging container 1, the hinge cap 22 is closed with the contents stored in the storage space S, and the packaging container 1 is kept airtight. As a result, the packaging container 1 blocks water, and it is possible to suppress moisture absorption by the contents.

[0065] <Manufacturing method of packaging containers> The method for producing the packaging container according to the present embodiment includes the following steps.

[0066] (A) A step of mixing a resin material with a supercritical fluid to prepare a molten resin composition. (B) A step of injecting a molten resin composition into a cavity of a mold. (C) After the above step (B), a step of foaming the supercritical fluid. (D) A step of recovering the molded product from the mold. (E) A step of fitting the bottom member and the cover member together.

[0067] A series of steps from step (A) to step (D) can be carried out, for example, using a MuCell injection molding machine ("MuCell" is a registered trademark of Trexel Co. Ltd.) (see, for example, Japanese Patent No. 6085729 and Japanese Patent No. 6430684).

[0068] [(A) Process] First, a resin material and a supercritical fluid are mixed to prepare a molten resin composition. The above-mentioned thermoplastic resins can be used as the resin material. 0.5 to 2.5 parts by mass of the supercritical fluid is added to 100 parts by mass of the resin material. Nitrogen or carbon dioxide in a supercritical state is used as the supercritical fluid.

[0069] When using nitrogen in a supercritical state as the supercritical fluid, 0.5 to 1.0 parts by mass of the supercritical fluid is added to 100 parts by mass of the resin material. When the amount of supercritical fluid is 0.5 parts by mass or more, foaming caused by nitrogen in a supercritical state can be promoted. On the other hand, when the amount of supercritical fluid is 1.0 part by mass or less, the dwell pressure in step (C) can be set relatively low, which tends to suppress post-blistering.

[0070] When carbon dioxide in a supercritical state is used as the supercritical fluid, 0.8 to 2.5 parts by mass of the supercritical fluid are added per 100 parts by mass of the resin material. When the amount of the supercritical fluid is 0.8 parts by mass or more, the viscosity of the molten resin composition is reduced by the addition of carbon dioxide, and the occurrence of short shots can be suppressed. In addition, foaming caused by carbon dioxide in a supercritical state can be promoted. On the other hand, when the amount of the supercritical fluid is 2.5 parts by mass or less, the dwell pressure in step (C) can be set relatively low, and there is a tendency that post-blistering can be suppressed.

[0071] The temperature of the molten resin composition (screw cylinder temperature) may be set according to the melting point or MFR of the resin material. When a polypropylene resin is used, this temperature is preferably about 210 to 230°C. When a polyethylene resin is used, this temperature is preferably about 220 to 240°C. When this temperature is equal to or higher than the lower limit, the resin easily flows in the cavity, while when the temperature is equal to or lower than the upper limit, the resin tends to be prevented from burning.

[0072] The molten resin composition may contain components other than the resin material and the supercritical fluid, that is, the molten resin composition may further contain, for example, a filler, a colorant, a slip agent, an antistatic agent, etc., as necessary.

[0073] [(B) Process] A mold corresponding to the shapes of the bottom member 2 and the lid member 3 of the packaging container 1 to be manufactured is prepared. Then, the molten resin composition prepared in the step (A) is injected into the cavity through the gate of the mold. The injection speed is preferably 60 mm / sec or more, more preferably 200 mm / sec or more, and even more preferably 250 mm / sec or more. By making the injection speed 60 mm / sec or more, it is easy to make the resin reach the flow end, and the occurrence of short shots tends to be suppressed. The upper limit of the injection speed is, for example, 350 mm / sec.

[0074] Even if the distance from the cavity gate to the farthest flow end (hereinafter referred to as "maximum flow length") is 60 mm or more, it is preferable that the molten resin composition reaches the flow end. The maximum flow length may be, for example, 70 mm or more or 80 mm or more. The upper limit of the maximum flow length is, for example, 120 mm. From the viewpoint of suppressing the occurrence of short shots, it is preferable that the relationship between the maximum flow length ML and the thickness T2 of the thin-walled recess to be molded satisfies the following relationship. 100≦ML / T2≦300

[0075] [(C) Process] After the step (B), at least a part of the supercritical fluid is immersed in a granular material having an inner diameter of 10 μm or more and a collection density of 10 particles / mm 2 The foam is expanded to form the above-mentioned closed cells B.

[0076] When the supercritical fluid is nitrogen in a supercritical state, in order to foam at least a part of the supercritical fluid in this way, for example, the cavity is held at a pressure of 15 to 85 MPa and cooled. When this pressure is 15 MPa or more, it is possible to suppress the occurrence of short shots while promoting the foaming of nitrogen in a supercritical state, while when it is 85 MPa or less, it tends to be possible to suppress the occurrence of after-swelling while promoting the foaming of nitrogen in a supercritical state. This value is preferably 25 to 80 MPa, and more preferably 30 to 75 MPa. The pressure holding time may be determined while taking into account the gate sealing time, and may be, for example, 0.1 to 1.5 seconds.

[0077] When the supercritical fluid is carbon dioxide in a supercritical state, in order to foam at least a part of the supercritical fluid in this way, for example, the cavity is kept under a pressure condition of 15 to 100 MPa and cooled. When this pressure is 15 MPa or more, it is possible to suppress the occurrence of short shots while promoting the foaming of carbon dioxide in a supercritical state, while when it is 100 MPa or less, it tends to be possible to suppress the occurrence of after-swelling while promoting the foaming of carbon dioxide in a supercritical state. This value is preferably 30 to 95 MPa, and more preferably 40 to 90 MPa. The pressure-holding time may be determined while taking into account the gate seal time, and may be, for example, 0.1 to 1.5 seconds.

[0078] From the viewpoint of producing a thin-walled portion, it is preferable not to carry out a process called "core-back" for reducing the pressure inside the cavity. Core-back is a process in which the movable part of the mold is moved to expand the volume of the cavity before the molten resin composition filled in the cavity finishes solidifying (see Japanese Patent No. 6085729).

[0079] [(D) Process] The molded product is removed from the mold when the temperature of the molded product (bottom member 2 or lid member 3) in the mold falls to about 30 to 60° C. In this embodiment, pressure dwell is performed in step (C) and the above-mentioned "core back" is not performed, so that large voids that can be confirmed visually are not formed in the molded product of this embodiment.

[0080] [(E) Process] The bottom member 2, which is the molded product recovered from the metal mold, is fitted to the cover member 3. In this way, the packaging container 1 is obtained.

[0081] As described above, in the packaging container 1 according to this embodiment, the contents can be stored in the storage space S formed between the bottom member 2 and the lid member 3. At least one of the bottom member 2 and the lid member 3 has a density of closed bubbles B having an inner diameter of 10 μm or more of 10 bubbles / mm 2That is, in the bubble region R, the number of independent bubbles B having an inner diameter of 10 μm or more is 10 / mm 2 The closed bubbles B are present at a density of 100 to 1500 nm. Therefore, in the bubble region R, the resin and the closed bubbles B form an island structure, which is thought to create a maze effect that complicates the path of water vapor passing through the resin. In addition, in the bubble region R, the resin and the closed bubbles B have different water vapor permeability coefficients, so the boundaries between the resin and the closed bubbles B may act as a resistance to water vapor permeation. It is thought that such a maze effect and resistance to permeation make it difficult for water vapor to permeate, so that the water vapor barrier property can be improved without increasing the thickness of the packaging container 1 or laminating a barrier film on the packaging container 1. Therefore, the water vapor barrier property can be improved while suppressing an increase in the environmental load.

[0082] In addition, in this packaging container 1, at least one of the bottom member 2 and the lid member 3 has flat bottom plate portions 23, 33 and side plate portions 24, 34 with a thickness of 0.7 mm or less, so that it is possible to reduce the amount of resin used in the packaging container 1 and further suppress an increase in the environmental load. Moreover, because the bottom plate portions 23, 33 and the side plate portions 24, 34 have air bubble regions R, it is possible to improve the water vapor barrier property in the bottom plate portions 23, 33 and the side plate portions 24, 34 as well.

[0083] In addition, this packaging container 1 has surface layers L1, L2 that are located on the inner surface 1a of the packaging container 1 and the outer surface 1b of the packaging container 1, sandwiching the air bubble region R, and do not have the air bubble region R, thereby improving the water vapor barrier properties while suppressing the occurrence of poor appearance of the packaging container 1.

[0084] Furthermore, in this packaging container 1, when the closed bubbles B are derived from nitrogen in a supercritical state, they are more likely to foam during the manufacturing of the packaging container 1, and the inner diameter of the closed bubbles B formed by the foaming is approximately 10 μm or more and 70 μm or less. Such fine closed bubbles B give the resin a complex and fine three-dimensional structure, so that the rigidity and shape stability of the packaging container 1 are increased even if the thickness of the packaging container 1 is thin. This makes it possible to suppress a decrease in the water vapor barrier property that accompanies bending of the packaging container 1.

[0085] Furthermore, in this packaging container 1, the bottom member 2 has a bottom plate portion 23, a side plate portion 24 that rises from the periphery of the bottom plate portion 23 and is fitted into the lid member 3, an opening 5 formed in the side plate portion 24, and a hinge cap 22 that opens and closes the opening 5, so that the contents can be contained airtight by closing the hinge cap 22, and the contained contents can be removed by opening the hinge cap 22.

[0086] In addition, in this packaging container 1, the side plate portions 24, 34 are discontinuous in the direction along the periphery of the bottom plate portions 23, 33 due to the opening 5, so that the side plate portions 24, 34 are easily deflected near the opening 5. If the side plate portions 24, 34 deflect near the opening 5, a gap is generated between the hinge cap 22 and the side plate portions 24, 34, and water vapor may enter through the gap. However, since the side plate portions 24, 34 have the bubble region R, the resin in the side plate portions 24, 34 has a complex three-dimensional structure due to the closed bubbles B, so that the rigidity and shape stability of the side plate portions 24, 34 are improved. In particular, when the closed bubbles B are derived from nitrogen in a supercritical state, the rigidity and shape stability of the side plate portions 24, 34 are further improved. Therefore, it is possible to suppress the deterioration of the water vapor barrier property caused by the deflection of the side plate portions 24, 34.

[0087] In addition, the packaging container 1 has a water vapor permeability of 1.60 g / mm 2 / day or less, moisture absorption of the contents can be suppressed.

[0088] The content-containing packaging container according to this embodiment includes the above-described packaging container 1, and therefore can improve the water vapor barrier property while suppressing an increase in the environmental load.

[0089] In the moisture blocking method according to the present embodiment, the contents are contained and held in the packaging container 1 described above, so that it is possible to enhance the water vapor barrier property while suppressing an increase in the environmental load.

[0090] In the method for producing a packaging container according to the present embodiment, a molten resin composition in which a resin material and a supercritical fluid are mixed is injected into a cavity of a mold, and at least a part of the supercritical fluid is mixed into a molten resin having an inner diameter of 10 μm or more and a population density of 10 particles / mm 2 Since the foaming is carried out so as to produce the above-mentioned closed cells, it is possible to manufacture a packaging container 1 that can enhance the water vapor barrier property while suppressing an increase in the environmental load.

[0091] Furthermore, in this method for producing a packaging container, by using nitrogen in a supercritical state as the supercritical fluid, a packaging container 1 having high rigidity and shape stability can be produced even if it has a thin wall thickness.

[0092] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to the above-described embodiments. EXAMPLES

[0093] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0094] (Resin material) Resin: Polypropylene (Sunallomer Co., Ltd., random copolymer "PM931V", MFR: 25g / 10min, white colorant blended at a ratio of 100:5)

[0095] (Structure of Molded Body) A bottom member 2 with a hinge cap shown in Fig. 2 and a lid member 3 shown in Fig. 3 were molded. The gate position was set to a position closer to the hinge cap in the long side direction of the bottom member, and also closer to the hinge cap in the short side direction of the bottom member. The designed maximum flow length (L), i.e., the linear distance from the gate to the furthest point of the molded body, was designed to be 83 mm. The lid member 3 was also set to a similar position.

[0096] (Evaluation of moisture resistance of entire packaging container) The molded bottom and cover members were fitted together with 12 g of silica gel placed inside. This was left to stand for 24 hours in an environment with a temperature of 30°C and a humidity of 80%. After that, the weight of the silica gel was measured to determine the weight increase rate.

[0097] (Observation of foaming state) The side plate and the pin of the molded lid member were each observed under a microscope (manufactured by HiROX, product name "KH7000") at a magnification of 140 times to check the number and size of the closed bubbles.

[0098] (Evaluation of water vapor permeability of base material) The molded lid member was set in a MOCON water vapor transmission rate measuring device (PERMATRAN-W 3 / 34, manufactured by AMETEK MOCON), and the water vapor transmission rate from the outside (opposite the storage space) to the inside (storage space side) of the bottom plate was measured after 6 and 12 hours under an environment of 40°C temperature and 90% humidity. The water vapor transmission rate measurement area M was a circular area with a diameter of 2.5 cm as shown in Figure 8. In the measurement of water vapor transmission rate, the water vapor transmission rate was measured at 1.5 hour intervals from the start of the measurement, and when the rate of change from the measurement value at the previous measurement point was within ±10% at three or more consecutive measurement points, the average value of the measurements at the first three points was taken as the water vapor transmission rate.

[0099] <Example 1> A molten resin composition was prepared by adding 0.80 parts by mass of supercritical nitrogen to 100 parts by mass of resin. Using this molten resin composition, a bottom member and a cover member were injection molded under the conditions shown in Table 1 and the design values ​​shown in Table 2. The flat portion is the portion of the bottom plate that is not a thin-walled recess.

[0100] The number and size of closed bubbles were measured for the side plate and pin of the molded lid member. The thickness of the flat surface and thin recess of each of the molded bottom member and lid member were also measured. The moisture resistance of the entire packaging container and the water vapor transmission rate of the bottom member were also evaluated. In the evaluation of the water vapor transmission rate of the bottom member, the average value of the measurements at three points after 4.5 hours, 6 hours, and 7.5 hours was taken as the water vapor transmission rate, and the water vapor transmission rate was 1.53 g / mm 2 / day. Table 3 shows the occurrence of closed bubbles, Table 4 shows the results of the water vapor permeability evaluation of the bottom member, and Figure 9 shows the results of the moisture proofing evaluation of the entire packaging container. The collection density of closed bubbles was an estimated value converted from the number of closed bubbles observed in a specified observation area. Note that in the evaluation of the water vapor permeability of the bottom member, data from the previous measurement point where the rate of change from the measurement value at the previous measurement point is within ±10% is not necessary, but for reference, the measured values ​​of the water vapor permeability of the bottom member are shown in Figures 10 to 12.

[0101] <Example 2> A molten resin composition was prepared by adding 1.50 parts by mass of supercritical carbon dioxide to 100 parts by mass of resin. Using this molten resin composition, injection molding of a bottom member and a cover member was performed under the conditions shown in Table 1 and the design values ​​shown in Table 2.

[0102] The number and size of closed bubbles were measured for the side plate and pin of the molded lid member. The thickness of the flat surface and thin recess of each of the molded bottom member and lid member were also measured. The moisture resistance of the entire packaging container and the water vapor transmission rate of the bottom member were also evaluated. In the evaluation of the water vapor transmission rate of the bottom member, the average value of the measurements taken at three points after 9 hours, 10.5 hours, and 12 hours was taken as the water vapor transmission rate, and the water vapor transmission rate was 1.22 g / mm 2 / day. Table 3 shows the occurrence of closed bubbles, Table 4 shows the results of the water vapor permeability evaluation of the bottom member, and Figure 9 shows the results of the moisture proofing evaluation of the entire packaging container. The collection density of closed bubbles was an estimated value converted from the number of closed bubbles observed in a specified observation area. Note that in the evaluation of the water vapor permeability of the bottom member, data from the previous measurement point where the rate of change from the measurement value at the previous measurement point is within ±10% is not necessary, but for reference, the measured values ​​of the water vapor permeability of the bottom member are shown in Figures 10 to 12.

[0103] <Comparative Example 1> The bottom member and the cover member were injection molded under the conditions shown in Table 1 and with the design values ​​shown in Table 2 using simply molten resin without adding any gas in a supercritical state.

[0104] The number and size of the closed bubbles were measured for the side plate and pin of the molded lid member. In addition, the moisture resistance of the entire packaging container and the water vapor permeability of the bottom member were evaluated. In the evaluation of the water vapor permeability of the bottom member, the average value of the measurements at three points after 4.5 hours, 6 hours, and 7.5 hours was taken as the water vapor permeability, and the water vapor permeability value was 1.72 g / mm 2 / day. The results of the water vapor permeability evaluation of the bottom member are shown in Table 4. The results of the moisture proofing evaluation of the entire packaging container are shown in Figure 9. Note that in the evaluation of the water vapor permeability of the bottom member, data before the rate of change from the measured value at the previous measurement point falls within ±10% is not required, but for reference, the measured values ​​of the water vapor permeability of the bottom member are shown in Figures 10 to 12.

[0105] [Table 1]

[0106] [Table 2]

[0107] [Table 3]

[0108] [Table 4]

[0109] From the results shown in Fig. 9, it can be seen that the packaging containers of Examples 1 and 2 have high water vapor barrier properties because the moisture resistance evaluation of the entire packaging container is higher than that of the packaging container of Comparative Example 1. Furthermore, the closed cells of Example 1 have a smaller inner diameter than the closed cells of Example 2, and the moisture resistance evaluation of the entire packaging container of Example 1 is higher than that of the packaging container of Example 2. This is thought to be because the closed cells derived from supercritical nitrogen have a smaller inner diameter than the closed cells derived from supercritical carbon dioxide, and therefore the packaging container of Example 1 has higher rigidity and shape stability than the packaging container of Example 2, and the decrease in water vapor barrier property due to bending of the packaging container is suppressed.

[0110] From the results shown in Table 4, it is apparent that the bottom members of Examples 1 and 2 have lower water vapor permeability than the bottom member of Comparative Example 1, and therefore have high water vapor barrier properties. [Industrial Applicability]

[0111] The present invention can be utilized as a packaging container for containing and dispensing small amounts of contents such as granular cooling materials. [Explanation of symbols]

[0112] 1...packaging container, 1a...surface, 1b...surface, 2...bottom member, 3...lid member, 5...opening, 21...hinge, 22...hinge cap, 23...bottom plate portion, 24...side plate portion, 24a...raised portion, 24b...lowered portion, 25 (25a, 25b, 25c, 25d, 25e)...boss, 26...thin-walled recess, 27...support, 28...guide rib, 33...bottom plate portion, 34...side plate portion, 35 (35a, 35b, 35c, 35d, 35e)...pin, 36...thin-walled recess, 39...guide, B...closed bubble, L1...surface layer, L2...surface layer, M...measurement area, R...bubble area, S...containment space.

Claims

1. A first member; a second member that is fitted into the first member to form an accommodation space between the first member and the second member, At least one of the first member and the second member has a density of closed bubbles having an inner diameter of 10 μm or more of 10 bubbles / mm 2 or more. Plastic packaging container.

2. At least one of the first member and the second member has a flat thin-wall portion having a thickness of 0.7 mm or less, The thin wall portion has the bubble region. The packaging container according to claim 1.

3. The closed bubbles are derived from nitrogen in a supercritical state. The packaging container according to claim 1.

4. The first member has a bottom plate portion, a side plate portion rising from a peripheral edge of the bottom plate portion and fitted to the second member, an opening portion formed in the side plate portion, and a hinge cap for opening and closing the opening portion. The packaging container according to claim 1.

5. The side plate portion has the bubble region and is discontinuous in a direction along a periphery of the bottom plate portion by the opening. The packaging container according to claim 4.

6. Water vapor permeability is 1.60g / mm 2 / day or less, The packaging container according to claim 1.

7. A packaging container according to any one of claims 1 to 6, and a content contained in the packaging container. Packaging container with contents.

8. A step of placing contents in the packaging container according to any one of claims 1 to 6; and retaining the contents within the packaging container. A method of shielding against moisture.

9. A method for producing the packaging container according to any one of claims 1 to 6, comprising the steps of: (A) mixing a resin material and a supercritical fluid to prepare a molten resin composition; (B) injecting the molten resin composition into a cavity of a mold; (C) After the step (B), at least a part of the supercritical fluid is immersed in a granular material having an inner diameter of 10 μm or more and a population density of 10 particles / mm 2 and a step of foaming the foam to form the above-mentioned closed cells. A method for manufacturing packaging containers.

10. The supercritical fluid is nitrogen in a supercritical state. A method for producing the packaging container according to claim 9.

11. When the mass of the resin material in the molten resin composition is 100 parts by mass, the mass of the nitrogen as the supercritical fluid in the molten resin composition is 0.5 to 1.0 parts by mass. The method for producing the packaging container according to claim 10.

Citation Information

Patent Citations

  • Card case with hinge cap

    JP3657351B2

  • case with hinge cap

    JP3953581B2