Explosion-proof member
The thermally responsive adhesive layer in the explosion-proof member addresses pressure-related malfunctions in sealed battery packs by detaching upon temperature rise, ensuring safety through controlled gas discharge.
Patent Information
- Application Number
- JP2023061233
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-05
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional explosion-proof valves in sealed battery packs malfunction due to pressure fluctuations during normal operation, leading to potential safety risks.
An explosion-proof member with a thermally responsive adhesive layer that detaches upon temperature increase, allowing gas discharge without relying on pressure changes.
Ensures the safety of sealed battery packs by preventing malfunctions and deformation or rupture due to temperature-induced pressure increases, effectively managing thermal runaway scenarios.
Smart Images

Figure 2024148256000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an explosion-proof member. [Background technology]
[0002] Sealed battery packs containing batteries or capacitors inside a sealed housing are widely used. In such sealed battery packs, gas may be generated inside the housing due to a chemical reaction of the electrolyte. It is known that when gas is generated inside the housing, the internal pressure of the housing increases, causing the housing to deform or burst. For this reason, a technology for blocking a gas exhaust hole provided in the housing with an explosion-proof valve has been conventionally adopted for sealed battery packs. In the explosion-proof valve, when the internal pressure of the housing reaches a predetermined value, the valve opens or the thin film valve breaks. This allows gas to be discharged from inside the housing, thereby avoiding deformation or bursting of the housing. For example, Patent Document 1 discloses an explosion-proof valve structure in which a gas exhaust hole in a sealing plate of a sealed electrochemical device is blocked by an explosion-proof valve body, and when the internal pressure of the device increases, the explosion-proof valve body breaks to discharge gas. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-072051 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, because conventional explosion-proof valves are triggered by an increase in the internal pressure of the casing, they can malfunction due to fluctuations in the pressure difference between the inside and outside of the casing during normal operation.
[0005] Therefore, an object of the present invention is to provide a new explosion-proof member suitable for ensuring the safety of a sealed battery pack. [Means for solving the problem]
[0006] As a result of extensive research, the present inventors have found that the above object can be achieved by using a temperature rise in the housing that accompanies a temperature rise inside the housing as a trigger.
[0007] The present invention relates to An explosion-proof member suitable for being fixed to a housing in a state of covering an opening of the housing, a film that prevents a foreign object from entering the housing through the opening in the above-described arrangement; and a pressure-sensitive adhesive layer; The first surface of the adhesive layer is connected to the membrane at a peripheral portion of the membrane or to a base member connected to the membrane at the peripheral portion; a second surface of the adhesive layer facing the opposite side to the first surface is fixed to the housing so as to surround the opening in the arrangement; The adhesive layer has a thermal responsiveness that reduces the adhesive strength by heating. Explosion-proof materials, to provide. Effect of the Invention
[0008] According to the present invention, it is possible to provide a new explosion-proof member suitable for ensuring the safety of a sealed battery pack. [Brief description of the drawings]
[0009] [Figure 1A] FIG. 1A is a cross-sectional view that illustrates an example of an explosion-proof member according to a first embodiment. [Figure 1B] FIG. 1B is a perspective view that illustrates the explosion-proof member of FIG. 1A. [Diagram 2] FIG. 2 is a cross-sectional view showing an example of a state in which the explosion-proof member of FIG. 1A is fixed to a housing in a state in which the explosion-proof member covers an opening of the housing. [Figure 3A] FIG. 3A is a cross-sectional view that illustrates a first modified example of the explosion-proof member of the first embodiment. [Figure 3B] FIG. 3B is a perspective view that illustrates the explosion-proof member of FIG. 3A. [Figure 4]FIG. 4 is a cross-sectional view showing an example of a state in which the explosion-proof member of FIG. 3A is fixed to the housing in a state in which the explosion-proof member covers the opening of the housing. [Figure 5A] FIG. 5A is a cross-sectional view that illustrates a second modified example of the explosion-proof member of the first embodiment. [Figure 5B] FIG. 5B is a perspective view that illustrates the explosion-proof member of FIG. 5A. [Figure 6] FIG. 6 is a cross-sectional view showing an example of a state in which the explosion-proof member of FIG. 5A is fixed to the housing in a state in which the explosion-proof member covers the opening of the housing. [Figure 7A] FIG. 7A is a cross-sectional view that illustrates an example of an explosion-proof member according to the second embodiment. [Figure 7B] FIG. 7B is an exploded perspective view showing a schematic diagram of the explosion-proof member of FIG. 7A. [Figure 8] FIG. 8 is a cross-sectional view showing an example of a state in which the explosion-proof member of FIG. 7A is fixed to the housing in a state in which the explosion-proof member covers the opening of the housing. [Figure 9] FIG. 9 is a schematic side view for explaining the peel test. [Figure 10] FIG. 10 is a schematic side view for explaining the peel adhesion test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The explosion-proof member according to the first aspect of the present invention is An explosion-proof member suitable for being fixed to a housing in a state of covering an opening of the housing, a film that prevents a foreign object from entering the housing through the opening in the above-described arrangement; and a pressure-sensitive adhesive layer; The first surface of the adhesive layer is connected to the membrane at a peripheral portion of the membrane or to a base member connected to the membrane at the peripheral portion; a second surface of the adhesive layer facing the opposite side to the first surface is fixed to the housing so as to surround the opening in the arrangement; The adhesive layer has a thermal responsiveness such that the adhesive strength is reduced by heating.
[0011] In a second aspect of the present invention, for example, in the explosion-proof component according to the first aspect, the adhesive layer has the thermal responsiveness in at least one selected from the group consisting of i) the first surface, ii) the second surface, and iii) an inner surface included in the adhesive layer and in contact with a substrate.
[0012] In a third aspect of the present invention, for example, in the explosion-proof component according to the first or second aspect, the adhesive layer substantially loses its adhesive force in an atmosphere at 160° C. due to the thermal responsiveness.
[0013] In a fourth aspect of the present invention, for example, in the explosion-proof component according to the third aspect, the peel time of the pressure-sensitive adhesive layer at 160° C. determined by the following peel test is 60 seconds or less. <Peel test> A sample body in which the single-sided adhesive tape having the adhesive layer is directly attached to an aluminum test plate is placed on the heating surface of a hot plate so that the adhesive layer is in contact with the heating surface of the hot plate. At this time, the horizontal position of the upper surface of the aluminum test plate is defined as the reference position. The heating surface is heated from 100°C to 180°C, and when the upper surface of the aluminum test plate exceeds the reference position, The time is the peel time at that temperature.
[0014] In a fifth aspect of the present invention, for example, in the explosion-proof component according to any one of the first to fourth aspects, the initial adhesive strength of the adhesive layer to an aluminum test plate, as determined by the following peel adhesion test, is 0.5 N / 20 mm or more. <Peel adhesion test> The single-sided adhesive tape having the adhesive layer is subjected to a "180° peel adhesion test against stainless steel test plate" as defined in JIS Z0237:2009. However, the aluminum test plate is used instead of the stainless steel test plate. The measured peel adhesion is regarded as the initial adhesive strength.
[0015] In a sixth aspect of the present invention, for example, in the explosion-proof member according to any one of the first to fifth aspects, the pressure-sensitive adhesive layer contains a thermal blowing agent.
[0016] In a seventh aspect of the present invention, for example, in the explosion-proof member according to the second aspect, the adhesive layer is a) a single layer, b) a single-sided adhesive tape including the base material and an adhesive part, or c) a double-sided adhesive tape including the base material, and a first adhesive part and a second adhesive part that sandwich the base material.
[0017] In an eighth aspect of the present invention, for example, an explosion-proof component according to any one of the first to seventh aspects comprises the base member and a cover member that is perpendicular to the surface of the membrane and covers the surface of the membrane when observed along a direction from the outside to the inside of the housing in the arrangement, is spaced apart from the surface of the membrane, and is connected to the base member.
[0018] In a ninth aspect of the present invention, for example, in the explosion-proof component according to any one of the first to eighth aspects, the film is a gas-permeable film, and the gas-permeable film has a gas-permeable portion surrounded by the peripheral portion.
[0019] In a tenth aspect of the present invention, for example, in the explosion-proof component according to any one of the first to ninth aspects, the air permeability in the thickness direction of the film is expressed as a Frazier number measured in accordance with the air permeability measurement method A (Fragile type method) defined in JIS L1096:2010, and is 0.001 cm 3 / (cm 2 sec) and 18.8 cm 3 / (cm 2 · seconds) or less.
[0020] In an eleventh aspect of the present invention, for example, in the explosion-proof component according to any one of the first to tenth aspects, the film is a porous film or a non-porous film.
[0021] In a twelfth aspect of the present invention, for example, the explosion-proof member according to any one of the first to eleventh aspects includes a release liner bonded to the second surface of the pressure-sensitive adhesive layer.
[0022] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. The present invention is not limited to the following embodiment.
[0023] [Explosion-proof materials] The explosion-proof member of this embodiment is suitable for the arrangement P in which the explosion-proof member is fixed to the housing 70 in a state in which the opening 71 of the housing is covered. The explosion-proof member includes a film 1 that suppresses the intrusion of foreign matter into the inside 72 of the housing 70 through the opening 71 in the arrangement P, and a pressure-sensitive adhesive layer 2. A first surface 2a of the pressure-sensitive adhesive layer 2 is connected to the film 1 at the peripheral portion 11 of the film 1, or is connected to a base member 3 that is connected to the film 1 at the peripheral portion 11 of the film 1. A second surface 2b of the pressure-sensitive adhesive layer 2 facing the opposite side to the first surface 2a of the pressure-sensitive adhesive layer 2 is fixed to the housing 70 so as to surround the opening 71 in the arrangement P. The pressure-sensitive adhesive layer 2 has a thermal responsiveness that reduces the pressure-sensitive adhesive force when heated. In this specification, "thermal responsiveness" refers to a property in which the pressure-sensitive adhesive force is reduced when heated. More specifically, this refers to a property that exhibits sufficient tackiness and adhesion in a room temperature environment, but decreases when heated to, for example, 80° C. or higher, or even 100° C. or higher. The foreign matter to be inhibited by the film 1 is, for example, solid matter such as dust and dirt. However, the foreign matter may include liquids such as water and oil in addition to solid matter.
[0024] The explosion-proof member of the present embodiment has such a structure that, when the temperature of the inside 72 of the housing 70 rises, the adhesive strength of the adhesive layer 2 is reduced, and at least a part including the film 1, or the whole of the member, can be automatically detached (naturally peeled off) from the adherend (e.g., the housing 70). Detachment of the film 1 of the explosion-proof member allows, for example, gas generated in the inside 72 of the housing 70 to be discharged from the opening 71. Thus, unlike conventional explosion-proof valves that are triggered by an increase in the internal pressure of the housing 70, the explosion-proof member of the present embodiment is triggered by a temperature increase in the housing 70 associated with a temperature increase in the inside 72 of the housing 70, and therefore, malfunction due to fluctuations in the internal and external pressure difference due to fluctuations in the internal pressure of the housing 70 during normal operation, etc., is avoided.
[0025] In addition, in a sealed battery pack, the battery may go into thermal runaway due to a rise in temperature inside the housing caused by overcharging or the like. When the battery goes into thermal runaway, the temperature inside the housing may rise suddenly, leading to a fire, or the internal pressure of the housing may rise with the sudden rise in temperature inside the housing, resulting in deformation or explosion of the housing. The sudden rise in temperature inside the housing due to thermal runaway of the battery occurs before the internal pressure of the housing rises. Therefore, conventional explosion-proof valves cannot fully avoid these dangers. However, according to the explosion-proof member of this embodiment, even if the battery goes into thermal runaway due to a rise in temperature inside 72 of the housing 70, the film 1 of the explosion-proof member can be detached without waiting for an excessive rise in the internal pressure of the housing 70.
[0026] In the following, as a first embodiment, an explosion-proof member 10 in which a first surface 2a of the adhesive layer 2 is connected to a membrane 1 at a peripheral portion 11 of the membrane 1 will be described. As a second embodiment, an explosion-proof member 40 in which a first surface 2a of the adhesive layer 2 is connected to a base member 3 which is connected to the membrane 1 at a peripheral portion 11 of the membrane 1 will be described.
[0027] First Embodiment An example of an explosion-proof member of the first embodiment is shown in Figures 1A to 1B. The explosion-proof member 10 shown in Figures 1A to 1B is an explosion-proof member suitable for arrangement P in which the explosion-proof member 10 is fixed to the housing 70 while covering the opening 71 of the housing 70. The explosion-proof member 10 includes a film 1 that prevents foreign matter from entering the interior 72 of the housing 70 through the opening 71 in arrangement P, and a pressure-sensitive adhesive layer 2.
[0028] 2 is a cross-sectional view showing an example of a state in which the explosion-proof member 10 is fixed to the housing 70 while covering the opening 71 of the housing 70. That is, the explosion-proof member 10 shown in FIG.
[0029] The adhesive layer 2 has a first surface 2a in contact with the membrane 1 and a second surface 2b facing the opposite side to the first surface 2a. In this embodiment, the first surface 2a of the adhesive layer 2 is connected to the membrane 1 so as to be along the peripheral portion 11 of the membrane 1. The second surface 2b of the adhesive layer 2 is fixed to the housing 70 so as to surround the opening 71 in the arrangement P.
[0030] In the example shown in Figs. 1A to 1B, the adhesive layer 2 is a single layer. In this embodiment, the adhesive layer 2 may be a) a single layer, b) a single-sided adhesive tape including a substrate and an adhesive part, or c) a double-sided adhesive tape including a substrate and a first adhesive part and a second adhesive part sandwiching the substrate. That is, in the adhesive layer 2, the substrate is provided by any selection, and may be present or absent. The adhesive layers 2 of b) and c) will be described in Modifications 1 and 2 below.
[0031] When the adhesive layer 2 is a single layer, the adhesive layer 2 may have thermal responsiveness on at least one selected from the group consisting of the first surface 2a and the second surface 2b. For example, when the first surface 2a of the adhesive layer 2 has thermal responsiveness, when the temperature of the housing 70 rises with the temperature rise of the inside 72 of the housing 70, the adhesive force on the first surface 2a decreases, and the film 1 of the explosion-proof member 10 can be automatically detached from the adherend. For example, when the second surface 2b of the adhesive layer 2 has thermal responsiveness, when the temperature of the housing 70 rises with the temperature rise of the inside 72 of the housing 70, the adhesive force on the second surface 2b decreases, and the film 1 of the explosion-proof member 10 can be automatically detached from the adherend.
[0032] Due to the thermal responsiveness, the adhesive layer 2 may substantially lose its adhesive strength in an atmosphere of 160° C. In this specification, "substantially loses its adhesive strength in an atmosphere of N° C." means a state in which the adhesive strength of the adhesive layer 2 is reduced in an atmosphere of N° C., and the film 1 of the explosion-proof member 10 can automatically detach from the adherend. "A state in which the film 1 of the explosion-proof member 10 can automatically detach from the adherend" means, for example, a state in which the film 1 of the explosion-proof member 10 can fall off from the adherend by its own weight.
[0033] Due to the thermal responsiveness, the adhesive layer 2 may substantially lose its adhesive strength in an atmosphere of 140°C, may substantially lose its adhesive strength in an atmosphere of 130°C, may substantially lose its adhesive strength in an atmosphere of 120°C, may substantially lose its adhesive strength in an atmosphere of 100°C, and may further substantially lose its adhesive strength in an atmosphere of 90°C.
[0034] In the explosion-proof component 10, the peel time T of the adhesive layer 2 at 160° C. was determined by the following peel test. 160 The time T 160 The peeling time T may be 40 seconds or less, or even 30 seconds or less. 160 The lower limit of the peeling time T 160 The lower limit may be, for example, 5 seconds.
[0035] <Peel test> FIG. 9 is a schematic side view for explaining a peel test. First, a single-sided adhesive tape 2 having an adhesive layer 2 is t By directly attaching the sample body SB to the aluminum test plate 81, 1 Next, the sample body SB is placed on the heating surface 90s of the hot plate 90 so that the adhesive layer 2 is in contact with the heating surface 90s. 1 At this time, the horizontal position of the upper surface 81s of the aluminum test plate 81 is set to the reference position h 0 Next, the heating surface 90s is heated from 100° C. to 180° C., and the upper surface 81s of the aluminum test plate 81 is brought to the reference position h 0 The time that exceeds this limit is defined as the peeling time T N (See FIG. 7B.)
[0036] Sample body SB 1 The single-sided adhesive tape 2 can be produced by the following method. A polyethylene terephthalate (PET) film having a thickness of 38 μm is used as the substrate 22. A 35 μm thick adhesive part is formed on the substrate 22, and the single-sided adhesive tape 2 t One-sided adhesive tape 2 tCut the single-sided adhesive tape 2 into a size of 20 mm in width and 40 mm in length. t is directly attached to an aluminum test plate 81 having a thickness of 0.5 mm, a width of 40 mm, and a length of 125 mm. In this way, the sample body SB 1 is obtained.
[0037] The above peel test is suitable for the pressure-sensitive adhesive layer 2 that expands upon heating and exhibits peelability, and a different peel test may be used depending on the type of thermal responsiveness.
[0038] According to the study by the present inventors, the peeling time T N and peeling time T for the iron test plate N is the peeling time T N For example, the peel time T 160 but When the peel time is 9 seconds, the peel time T 160 and peeling time T for the iron test plate 160 can be on the order of 10 seconds.
[0039] In the explosion-proof member 10, the peel time T of the adhesive layer 2 at 90° C. obtained by the above peel test 90 In the present embodiment, T 90 If ≦60 seconds is satisfied, T 160 The peeling time T ≦60 (seconds) is satisfied. This is because the adhesive layer 2 that substantially loses its adhesive force in an atmosphere at 90° C. necessarily substantially loses its adhesive force in an atmosphere at a higher temperature of 160° C. 90 The peeling time T may be 40 seconds or less, or even 30 seconds or less. 90 The lower limit of the peeling time T 90 The lower limit may be, for example, 5 seconds.
[0040] In the explosion-proof member 10, the initial adhesive strength F of the adhesive layer 2 to an aluminum test plate was determined by the following peel adhesion test. 0 may be 0.5N / 20mm or more.
[0041] <Peel adhesion test> FIG. 10 is a schematic side view for explaining the peel adhesion test. First, a single-sided adhesive tape 2 cut to a size of 20 mm in width and 140 mm in length was t Prepare two pieces of single-sided adhesive tape. t The single-sided adhesive tape 2 was then attached to the aluminum test plate 82 so that the adhesive layer 2 was in contact with the aluminum test plate 82. t Place the JIS A manual roller with a mass of 2 kg specified in Z0237:2009 is moved back and forth once, and the single-sided adhesive tape 2 t and an aluminum test plate 82 are joined to form a sample body SB 2 Then, the bonded sample body SB 2 The resulting sample body SB is left in a 25°C environment for 20 to 40 minutes to stabilize the bond. 2 The adhesive strength was measured by setting the adhesive strength on a tensile tester equipped with a thermostatic chamber (Shimadzu Corporation, product name "Shimadzu Autograph AG-120kN") and carrying out the "180° peel adhesion test against stainless steel test plate" as specified in JIS Z0237:2009. However, an aluminum test plate (thickness 0.5 mm, width 40 mm, length 125 mm) was used instead of the stainless steel test plate. The measured peel adhesion force was expressed as the initial adhesive strength F 0 (N / 20 mm). Specifically, one end of an aluminum test plate 82 is fixed to the upper chuck 91 of the tensile tester, and one end of the single-sided adhesive tape 2 is fixed to the upper chuck 91 of the tensile tester. t One end of the single-sided adhesive tape 2 is folded back 180° and fixed to the lower chuck 92 of the tensile testing device. t Sample body SB 2 A 180° peel test is carried out by peeling the sample from the SB in the length direction. 2The load when the aluminum test plate 82 is peeled off from the tape is measured, and the maximum load (the maximum load excluding the peak top at the beginning of the measurement) is calculated. The maximum load is divided by the tape width to obtain the adhesive strength F. 0 (N / 20mm).
[0042] According to the study by the present inventors, the adhesive strength F of the adhesive layer 2 to a stainless steel test plate 0 and adhesive strength F to iron test plate 0 is the adhesive strength F to the aluminum test plate 0 For example, the initial adhesive strength F of the adhesive layer 2 to an aluminum test plate may be larger than 0 When the adhesive strength F to the stainless steel test plate is 3.0N / 20mm, 0 and adhesive strength F to iron test plate 0 is greater than 3.0N / 20m and may be 5.0N / 20m or greater.
[0043] In the explosion-proof member 10, the adhesive strength F 0 The adhesive strength F may be 2.0 N / 20 mm or more, 2.5 N / 20 mm or more, or 3 N / 20 mm or more. 0 There is no particular upper limit for the adhesive strength F 0 The upper limit may be, for example, 40N / 20mm or 30N / 20mm.
[0044] [Adhesive layer] The adhesive layer 2 has a thermal responsiveness that reduces the adhesive strength by heating. With such a structure, when the temperature of the housing 70 increases with the temperature of the inside 72 of the housing 70, the adhesive strength of the adhesive layer 2 decreases. The adhesive strength of the adhesive layer 2 is reduced, and the film 1 of the explosion-proof member 10 can automatically detach from the adherend. By the detachment of the film 1 of the explosion-proof member 10, for example, gas generated inside the housing 70 72 can be discharged from the opening 71.
[0045] In this specification, "adhesive" means "adhesion" or "bonding." For example, "adhesive layer" means "adhesive layer" or "adhesive layer." "Adhesive strength" means "adhesive strength" or "adhesive strength."
[0046] In this specification, "adhesion" (pressure-sensitive adhesive), as defined by JIS, is a type of adhesion, a temporary adhesion, and refers to the property of being able to adhere by applying only a slight pressure. In addition, because it has cohesive force and elasticity, it is a property that while it adheres strongly, it can also be peeled off from a hard, smooth surface. An adhesive is a soft solid and does not change state like an adhesive. An adhesive wets the adherend in its original state and resists peeling, so when adherends are attached to each other, it can instantly exert adhesive strength that can withstand practical use. In other words, an adhesive has both the properties of a liquid (fluidity) that wets the adherend and the properties of a solid (cohesive force) that resist peeling. Since an adhesive is a soft solid, the contact area with the adherend gradually increases by applying pressure or taking time. And because it can maintain this softness for a long time, it has the property of being able to be peeled off when desired.
[0047] In this specification, "adhesive" refers to the property of bonding the surfaces of the same or different solids together to form a single unit, as defined by the JIS. An adhesive is a fluid liquid when bonding adherends together, wetting and blending with the adherends. It then turns into a solid through heating or chemical reaction, firmly binding the adherends at their interfaces and exerting a force that resists peeling. In other words, an adhesive wets as a liquid and bonds as a solid.
[0048] The adhesive layer 2 may be, for example, a heat-expandable adhesive layer made of a material that expands due to heat, a heat-shrinkable adhesive layer made of a material that shrinks due to heat, a heat-meltable adhesive layer made of a material that melts due to heat, a heat-sublimable adhesive layer made of a material that sublimes due to heat, or a thermally decomposable adhesive layer made of a material that decomposes due to heat.
[0049] In terms of being able to more effectively exert the effects of the present invention, the adhesive layer 2 is preferably a pressure-sensitive adhesive layer, and more preferably a thermally expandable pressure-sensitive adhesive layer.
[0050] The adhesive layer 2 may contain a thermal blowing agent. The adhesive layer 2 may be provided with thermal responsiveness by the thermal blowing agent.
[0051] The thermal blowing agent typically contains thermally expandable microspheres. When the adhesive layer 2 contains a thermal blowing agent, after the explosion-proof component 10 is fixed to the adherend, the thermally expandable microspheres contained in the thermal blowing agent are foamed and / or expanded by heating, thereby reducing the adhesive area between the adhesive layer 2 and the adherend. This causes a decrease in the adhesive strength of the adhesive layer 2, allowing the film 1 of the explosion-proof component 10 to be automatically detached.
[0052] (thermal expandable microspheres) The heat-expandable microspheres are not particularly limited and may be appropriately selected from known heat-expandable microspheres, which may be used alone or in combination of two or more. Examples of heat-expandable microspheres include low-boiling liquids such as propane, propylene, butene, normal butane, isobutane, isopentane, neopentane, normal pentane, normal hexane, isohexane, heptane, octane, petroleum ether, methane halides, and tetraalkylsilanes, and Microspheres can be used in which a substance that easily gasifies and expands when heated, such as azodicarbonamide that decomposes thermally into a gas, is encapsulated in an elastic shell-forming substance.
[0053] The shell-forming substance is, for example, a polymer of a radically polymerizable monomer. Examples of the monomer include nitrile monomers such as acrylonitrile, methacrylonitrile, α-chloroacrylonitrile, α-ethoxyacrylonitrile, and fumaronitrile; carboxylic acid monomers such as acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, and citraconic acid; vinylidene chloride; vinyl acetate; (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, and β-carboxyethyl acrylate; styrene monomers such as styrene, α-methylstyrene, and chlorostyrene; amide monomers such as acrylamide, substituted acrylamide, methacrylamide, and substituted methacrylamide; and mixtures thereof. The shell-forming material is composed of a heat-fusible material or a material that breaks down due to thermal expansion.
[0054] The shell-forming material may be a copolymer of one or more substances. Examples of the copolymer include vinylidene chloride-methyl methacrylate-acrylonitrile copolymer, methyl methacrylate-acrylonitrile-methacrylonitrile copolymer, methyl methacrylate-acrylonitrile copolymer, acrylonitrile-methacrylonitrile-itaconic acid copolymer, etc. The heat-expandable microspheres can be produced by a conventional method such as a coacervation method or an interfacial polymerization method.
[0055] As the heat-expandable microspheres, for example, commercially available products such as Matsumoto Microspheres (F-36, F-50, FN-100SS) manufactured by Matsumoto Yushi Seiyaku Co., Ltd. can be used.
[0056] Heat-expandable microspheres other than those mentioned above can also be used. Examples of such heat-expandable microspheres include various inorganic and organic foaming agents. Representative examples of inorganic foaming agents include ammonium carbonate, ammonium hydrogen carbonate, sodium hydrogen carbonate, ammonium nitrite, sodium borohydride, and various azides. Representative examples of organic blowing agents include water; fluorinated alkane-based compounds such as trichloromonofluoromethane and dichloromonofluoromethane; azo compounds such as azobisisobutyronitrile, azodicarbonamide and barium azodicarboxylate; hydrazine compounds such as paratoluenesulfonylhydrazide, diphenylsulfone-3,3'-disulfonylhydrazide, 4,4'-oxybis(benzenesulfonylhydrazide) and allylbis(sulfonylhydrazide); semicarbazide compounds such as p-toluylenesulfonylsemicarbazide and 4,4'-oxybis(benzenesulfonylsemicarbazide); triazole compounds such as 5-morpholyl-1,2,3,4-thiatriazole; and N-nitroso compounds such as N,N'-dinitrosopentamethylenetetramine and N,N'-dimethyl-N,N'-dinitrosoterephthalamide.
[0057] From the viewpoint of efficiently reducing the adhesive strength of the adhesive layer 2 by heating, the heat-expandable microspheres preferably have an appropriate strength such that they do not burst until the volume expansion rate reaches 5 times or more, more preferably 7 times or more, and particularly preferably 10 times or more. The blending amount of the heat-expandable microspheres can be appropriately set depending on the expansion ratio and / or the reduction in adhesive strength of the adhesive layer 2. The blending amount of the heat-expandable microspheres is, for example, 1 to 150 parts by weight, preferably 10 to 130 parts by weight, and more preferably 25 to 100 parts by weight, based on 100 parts by weight of the base polymer forming the adhesive layer 2.
[0058] The adhesive layer 2 further contains an adhesive having adhesive properties. From the viewpoint of a balance between an appropriate adhesive strength before heating and an adhesive strength after heating, the adhesive is preferably a pressure-sensitive adhesive. More preferred is a pressure-sensitive adhesive based on a polymer having a dynamic modulus of elasticity in the range of 5 kPa to 1 MPa at 25 to 150° C. The pressure-sensitive adhesive will be described in detail below.
[0059] (Adhesive) The adhesive is preferably one that does not restrict the foaming and / or expansion of the heat-expandable microspheres when heated as much as possible. Examples of such adhesives include known adhesives such as acrylic adhesives, rubber adhesives, vinyl alkyl ether adhesives, silicone adhesives, polyester adhesives, polyamide adhesives, urethane adhesives, styrene-diene block copolymer adhesives, creep property-improved adhesives obtained by blending these adhesives with a heat-meltable resin having a melting point of about 200° C. or less, and radiation-curable adhesives. The adhesives may be used alone or in combination of two or more kinds (see, for example, JP-A-56-61468 and JP-A-63-17981).
[0060] As the adhesive, an acrylic adhesive or a rubber adhesive can be suitably used, and an acrylic adhesive can be particularly suitably used. Examples of the acrylic adhesive include an acrylic adhesive having an acrylic polymer (homopolymer or copolymer) using one or more (meth)acrylic acid alkyl esters as a monomer component as a base polymer. Examples of the (meth)acrylic acid alkyl esters in such acrylic adhesives include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, and nonyl (meth)acrylate. Examples of the (meth)acrylic acid alkyl ester include isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate, which have a linear or branched alkyl group with 1 to 20 carbon atoms in the alkyl group. In this specification, "(meth)acrylic" means "acrylic" and / or "methacrylic". Among these, (meth)acrylic acid alkyl esters with an alkyl group with 4 to 18 carbon atoms are more preferred. The content of the (meth)acrylic acid alkyl ester is preferably 50 to 100% by weight, and more preferably 70 to 100% by weight, based on the total amount (100% by weight) of monomer components constituting the acrylic pressure-sensitive adhesive.
[0061] The acrylic polymer may contain units corresponding to other monomer components copolymerizable with the (meth)acrylic acid alkyl ester, if necessary, for the purpose of modifying the cohesive strength, heat resistance, crosslinkability, etc. Examples of such monomer components include carboxyl group-containing monomers such as acrylic acid, methacrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid; acid anhydride monomers such as maleic anhydride and itaconic anhydride; hydroxyl group-containing monomers such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, hydroxyhexyl (meth)acrylate, hydroxyoctyl (meth)acrylate, hydroxydecyl (meth)acrylate, hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl methacrylate; sulfonic acid group-containing monomers such as styrene sulfonic acid, allyl sulfonic acid, 2-(meth)acrylamido-2-methylpropanesulfonic acid, (meth)acrylamidopropanesulfonic acid, sulfopropyl (meth)acrylate, and (meth)acryloyloxynaphthalenesulfonic acid; (meth)acrylamide, N,N-dimethyl(meth)acrylamide, and N-butyl(meth)acryl. (N-substituted) amide monomers such as amide, N-methylol (meth)acrylamide, and N-methylolpropane (meth)acrylamide; (meth)acrylic acid aminoalkyl monomers such as aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, and t-butylaminoethyl (meth)acrylate; (meth)acrylic acid alkoxyalkyl monomers such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate; N-cyclohexylmaleimide, N-isopropylmaleimide maleimide monomers such as N-laurylmaleimide and N-phenylmaleimide; itaconimide monomers such as N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-cyclohexylitaconimide and N-laurylitaconimide; itaconimide monomers such as N-(meth)acryloyloxymethylenesuccinimide, N-(meth)acryloyl-6-oxyhexamethylenesuccinimide, N-(meth)acryloyl-8-oxyoctadecyloxymethylenesuccinimide, N-(meth)acrylo ... succinimide-based monomers such as tamethylene succinimide; vinyl acetate, vinyl propionate, N-vinylpyrrolidone, methylvinylpyrrolidone, vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, vinylmorpholine, N-vinyl carboxylic acid amides, styrene, α-methylstyrene, N-vinylcaprolactam, and other vinyl monomers; cyanoacrylate monomers such as acrylonitrile and methacrylonitrile; epoxy group-containing acrylic resin monomers such as glycidyl (meth)acrylate; glycol-based acrylic ester monomers such as polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, methoxyethylene glycol (meth)acrylate, and methoxypolypropylene glycol (meth)acrylate; acrylic ester monomers having a heterocycle, a halogen atom, a silicon atom, or the like, such as tetrahydrofurfuryl (meth)acrylate, fluorine (meth)acrylate, and silicone (meth)acrylate;Examples of the monomer component include polyfunctional monomers such as hexanediol di(meth)acrylate, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, epoxy acrylate, polyester acrylate, and urethane acrylate; olefin monomers such as isoprene, butadiene, and isobutylene; and vinyl ether monomers such as vinyl ether. These monomer components can be used alone or in combination. From the viewpoint of improving cohesive strength and crosslinking properties, the monomer component is preferably a hydroxyl group-containing monomer or a carboxyl group-containing monomer, and more preferably hydroxyethyl (meth)acrylate or acrylic acid. The content of the hydroxyl group-containing monomer is preferably less than 10% by weight, more preferably 8% by weight or less, and particularly preferably 5% by weight or less, based on the total amount (100% by weight) of the monomer components constituting the acrylic polymer. The content of the carboxyl group-containing monomer is preferably less than 20% by weight, more preferably 5% by weight or less, based on the total amount (100% by weight) of the monomer components constituting the acrylic pressure-sensitive adhesive.
[0062] Rubber-based adhesives include natural rubber and various synthetic rubbers, such as polyisoprene rubber, styrene-butadiene (SB) rubber, styrene-isoprene (SI) rubber, styrene-isoprene-styrene block copolymer (SIS) rubber, styrene-butadiene-styrene block copolymer (SBS) rubber, styrene-ethylene-butylene-styrene block copolymer (SEBS) rubber, styrene-ethylene-propylene-styrene block copolymer (SEPS) rubber, styrene-ethylene-propylene block copolymer (SEP) rubber, reclaimed rubber, butyl rubber, and polyisobutylene; and rubber-based adhesives using modified equivalents of these as the base polymer.
[0063] In addition, the adhesive contains a crosslinking agent, a tackifying resin, a pigment, a dye, a filler, an anti-aging agent, a conductive agent, etc. The toner may contain additives such as antistatic agents, ultraviolet absorbers, light stabilizers, release regulators, softeners, surfactants, flame retardants, and antioxidants.
[0064] Examples of the crosslinking agent include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, melamine-based crosslinking agents, peroxide-based crosslinking agents, as well as urea-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, carbodiimide-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, amine-based crosslinking agents, etc. As the crosslinking agent, isocyanate-based crosslinking agents and epoxy-based crosslinking agents can be preferably used.
[0065] Examples of isocyanate crosslinking agents include lower aliphatic polyisocyanates such as butylene diisocyanate and hexamethylene diisocyanate; alicyclic isocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate, and isophorone diisocyanate; aromatic isocyanates such as 2,4-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, and xylylene diisocyanate; and isocyanate adducts such as trimethylolpropane / tolylene diisocyanate trimer adduct (manufactured by Nippon Polyurethane Industry Co., Ltd., Coronate L), trimethylolpropane / hexamethylene diisocyanate trimer adduct (manufactured by Nippon Polyurethane Industry Co., Ltd., Coronate HL), and isocyanurate of hexamethylene diisocyanate (manufactured by Nippon Polyurethane Industry Co., Ltd., Coronate HX). These compounds may be used alone or in combination of two or more. The amount of the isocyanate crosslinking agent may be appropriately set depending on the adhesive strength required for the adhesive, and is, for example, 0.1 to 20 parts by weight, preferably 0.5 to 10 parts by weight, per 100 parts by weight of the base polymer constituting the adhesive.
[0066] Examples of epoxy crosslinking agents include N,N,N',N'-tetraglycidyl-m-xylylenediamine, diglycidylaniline, 1,3-bis(N,N-glycidylaminomethyl)cyclohexane (Tetrad C, manufactured by Mitsubishi Gas Chemical Co., Ltd.), 1,6-hexanediol diglycidyl ether (Epolites 1600, manufactured by Kyoeisha Chemical Co., Ltd.), neopentyl glycol diglycidyl ether (Epolites 1500NP, manufactured by Kyoeisha Chemical Co., Ltd.), ethylene glycol diglycidyl ether (Epolites 40E, manufactured by Kyoeisha Chemical Co., Ltd.), propylene glycol diglycidyl ether (Epolites 70P, manufactured by Kyoeisha Chemical Co., Ltd.), polyethylene glycol diglycidyl ether (Epiol E-400, manufactured by Nippon Oil & Fats Co., Ltd.), polypropylene glycol diglycidyl ether (Epiol E-400, manufactured by Nippon Oil & Fats Co., Ltd.), Examples of the epoxy resins include epoxy resins having two or more epoxy groups in the molecule, such as Epiol P-200, sorbitol polyglycidyl ether (Nagase Chemtex Corporation, Denacol EX-611), glycerol polyglycidyl ether (Nagase Chemtex Corporation, Denacol EX-314), pentaerythritol polyglycidyl ether, polyglycerol polyglycidyl ether (Nagase Chemtex Corporation, Denacol EX-512), sorbitan polyglycidyl ether, trimethylolpropane polyglycidyl ether, adipic acid diglycidyl ester, o-phthalic acid diglycidyl ester, triglycidyl-tris(2-hydroxyethyl)isocyanurate, resorcinol diglycidyl ether, and bisphenol-S-diglycidyl ether. These crosslinking agents may be used alone or in combination of two or more. The amount of the epoxy crosslinking agent may be appropriately set according to the adhesive strength required for the adhesive. The amount of the epoxy crosslinking agent added is, for example, 0.01 to 10 parts by weight, and preferably 0.03 to 5 parts by weight, relative to 100 parts by weight of the base polymer constituting the pressure-sensitive adhesive.
[0067] The plasticizer is not particularly limited, and for example, trimellitic acid ester plasticizers, pyromellitic acid ester plasticizers, polyester plasticizers, adipic acid plasticizers, etc. can be used, and trimellitic acid ester plasticizers and pyromellitic acid ester plasticizers can be preferably used. The plasticizers can be used alone or in combination of two or more kinds. Examples of the mellitic acid ester plasticizer include trimellitic acid trialkyl esters such as tri(n-octyl) trimellitate, tri(2-ethylhexyl) trimellitate, triisooctyl trimellitate, triisononyl trimellitate, and triisodecyl trimellitate. Examples of the pyromellitic acid ester plasticizer include pyromellitic acid tetraalkyl esters such as tetra(n-octyl) pyromellitate and tetra(2-ethylhexyl) pyromellitate. The amount of the plasticizer to be added can be appropriately set depending on the purpose. The amount of the plasticizer to be added is, for example, 1 to 20 parts by weight, preferably 1 to 5 parts by weight, based on 100 parts by weight of the base polymer constituting the adhesive.
[0068] When selecting a tackifier resin, it is necessary to select one that is highly compatible with the adhesive, not one that is poorly compatible with the adhesive. When a tackifier resin that is poorly compatible with the adhesive is blended, not only a compatible portion in which the adhesive and the tackifier resin are compatible with each other, but also an incompatible portion in which the adhesive and the tackifier resin are separated from each other is formed in the adhesive. That is, a domain of the tackifier resin with a high glass transition temperature (Tg) is locally formed on the surface of the adhesive, and a surface with partially low adhesive strength is formed. Therefore, on a surface where the domain portion of the tackifier resin with low adhesive strength is exposed, the micro-components of the workpiece are bonded to the surface of the adhesive layer by weak adhesive strength, and are easily peeled off by vibration during processing such as dicing. This tendency becomes more pronounced, especially as the workpiece becomes smaller after cutting, because the domain portion of the tackifier resin becomes larger relative to the size of the workpiece. For this reason, even if adhesive strength is improved by simply increasing the amount of tackifier resin, if the tackifier resin is not compatible with the adhesive, the adhesive strength is a physical property that can be considered the average value of the entire adhesive surface, and therefore chipping caused by variations in the in-plane physical properties when the adhesive layer surface is viewed microscopically cannot be eliminated.
[0069] As the tackifier resin, rosin resins derived from rosin, terpene resins derived from terpenes such as pinene, aliphatic hydrocarbon resins derived from petroleum fractions, aromatic hydrocarbon resins, etc. can be used. Tackifier resins such as terpene phenolic resins and rosin phenolic resins, which are copolymerized with phenolic groups such as rosin phenol and terpene phenol, are preferred. The molecular structure of rosin phenol, especially terpene phenol, is not three-dimensionally crowded, and the hydroxyl group of the phenolic group and the ester group in the acrylic adhesive tend to interact with each other, improving compatibility. Specific examples of tackifier resins that can be used include terpene phenolic resins such as YS Polystar S145 manufactured by Yasuhara Chemical Co., Ltd. and Tamanor 901 manufactured by Arakawa Chemical Co., Ltd. As the rosin phenolic resin, Sumilight Resin PR-12603 manufactured by Sumitomo Bakelite Co., Ltd. can be used. On the other hand, in the case of rosin ester resins, compatibility is expected due to intermolecular interactions between the ester groups contained in the structure and the ester groups in the acrylic adhesive, but since the composition of rosin ester resins has an alicyclic structure, it is sterically crowded compared to terpene phenol resins, etc., and the influence of interactions due to functional groups is low. In addition, hydroxyl value, acid value, etc. can be used as an index of compatibility between adhesives and resins. In resins with high hydroxyl groups, interaction between the hydroxyl groups and the ester groups in the acrylic adhesive is expected, and in resins with high acid values, the proportion of carboxyl groups in the structure is high, and they can have intermolecular interactions with the ester groups in the acrylic adhesive, resulting in improved compatibility. Even in rosin ester resins with a sterically crowded structure, if the acid value or hydroxyl value is high, the probability of intermolecular interactions with the ester groups in the acrylic adhesive increases, and compatibility is improved. For example, Super Ester A115, a rosin ester resin manufactured by Arakawa Chemical Co., Ltd., can be used. The hydroxyl value at which improved compatibility is expected is 45 or more, more preferably 70 or more, and the acid value is 15 or more, more preferably 40 or more. The amount of the tackifier resin is, for example, 5 to 100 parts by weight, preferably 10 to 50 parts by weight, per 100 parts by weight of the base polymer constituting the adhesive.
[0070] [film] The membrane 1 may be a breathable membrane. When the membrane 1 is a breathable membrane, the membrane 1 is surrounded by a peripheral portion 11. It also has a ventilation portion 12. When the film 1 is a ventilation film, the explosion-proof component 10 can be endowed with an internal pressure adjusting function.
[0071] The air permeability in the thickness direction of the membrane 1 is expressed as the Frazier number measured in accordance with the air permeability measurement method A (Fragile type method) specified in JIS L1096:2010, and is expressed as a value of 0.001 cm 3 / (cm 2 sec) and 18.8 cm 3 / (cm 2 10 seconds) or less.
[0072] The lower limit of the air permeability in the thickness direction of the membrane 1 is 0.01 cm 3 / (cm 2 · seconds) may be as small as 0.1cm 3 / (cm 2 · seconds) may be further increased by 0.2 cm 3 / (cm 2 sec).
[0073] The membrane 1 may be a porous membrane or a non-porous membrane. When the membrane 1 is a porous membrane, the membrane 1 can function as a gas permeable membrane.
[0074] As the membrane 1, a woven fabric, nonwoven fabric, mesh or net made of resin or metal, or a resin porous membrane can be used. For example, the membrane 1 may have a structure in which a resin porous membrane and a breathable reinforcing layer are laminated. The reinforcing layer can improve the strength of the membrane 1. The resin porous membrane is, for example, a fluororesin porous body and a polyolefin porous body that can be manufactured by a known stretching method or extraction method. The fluororesin is, for example, polytetrafluoroethylene (PTEF), polychlorotrifluoroethylene, tetrafluoroethylene-hexafluoropropylene copolymer, tetrafluoroethylene-perfluoroalkylvinylether copolymer, and tetrafluoroethylene-ethylene copolymer. Monomers constituting polyolefin are, for example, ethylene, propylene, and 4-methylpentene-1,1 butene, and polyolefins that are homopolymers or copolymers of these monomers can be used for the membrane 1. A nanofiber film porous body using polyacrylonitrile, nylon, or polylactic acid may be used for the membrane 1. When the explosion-proof member 10 is to have an internal pressure adjusting function, it is preferable to use a PTFE porous body for the membrane 1, which can ensure breathability with a small area and has a high ability to prevent foreign matter from entering the inside 72 of the housing 70. The average pore size of the PTFE porous body is preferably 0.01 μm or more and 10 μm or less. The reinforcing layer is, for example, a woven fabric, a nonwoven fabric, a mesh, a net, a sponge, a foam, or a porous body made of a resin or a metal. The resin porous membrane and the reinforcing layer can be laminated by a method such as adhesive lamination, heat lamination, heat welding, ultrasonic welding, or adhesion with an adhesive.
[0075] The membrane 1 may be subjected to a liquid-repellent treatment. The liquid-repellent treatment can be performed by applying a liquid-repellent agent containing a substance with low surface tension to the membrane 1 and drying the coating film formed by the application. The liquid-repellent agent contains, for example, a polymer having a perfluoroalkyl group as the above-mentioned substance. The liquid-repellent agent can be applied by, for example, an air spray method, an electrostatic spray method, a dip coating method, a spin coating method, a roll coating method, a curtain flow coating method, an impregnation method, or the like.
[0076] The thickness of the film 1 is 1 to 1000 μm, preferably 3 to 600 μm.
[0077] The thickness of the adhesive layer 2 is 3 to 300 μm, preferably 5 to 150 μm, and more preferably 10 to 100 μm. With such a structure, the adhesive layer 2 can exhibit a function of providing a large adhesive area by conforming to the surface shape of the adherend, and a function of promoting the formation of a wavy structure by the three-dimensional structural change of the adhesive layer 2.
[0078] As shown in FIGS. 1A and 1B, the explosion-proof member 10 may include a release liner 5 bonded to the second surface 2b of the adhesive layer 2. With such a structure, the adhesive force of the adhesive layer 2 can be protected until the explosion-proof member 10 is fixed to the housing 70. The release liner 5 is peeled off when the adhesive layer 2 is used. The release liner 5 may be removed as necessary. It is installed in the facility and may or may not be present.
[0079] [Release liner] The release liner 5 may have release surfaces on both sides or only one side (single side).
[0080] As the release liner 5, known or conventional release paper and the like can be used. Specifically, as the release liner 5, for example, a substrate having a release agent layer such as a plastic film or paper surface-treated with a release agent such as a silicone-based, long-chain alkyl-based, fluorine-based, or molybdenum sulfide-based release agent; a low-adhesion substrate made of a fluorine-based polymer such as polytetrafluoroethylene, polychlorotrifluoroethylene, polyvinyl fluoride, polyvinylidene fluoride, a tetrafluoroethylene-hexafluoropropylene copolymer, or a chlorofluoroethylene-vinylidene fluoride copolymer; a low-adhesion substrate made of a non-polar polymer such as an olefin resin (for example, polyethylene, polypropylene, etc.); etc. can be used. In a substrate having a release agent layer, the surface of the release agent layer is the release surface, and in a low-adhesion substrate, the surface of the low-adhesion substrate is the release surface. The release liner 5 can be formed by a known or conventional method. In addition, the thickness of the release liner 5 is not particularly limited.
[0081] 1A to 1B, the explosion-proof member 10 has a disk shape. However, the shape of the explosion-proof member 10 is not limited to the example shown in Fig. 1A to 1B. The shape of the explosion-proof member 10 may be, for example, a rectangular shape or a polygonal shape.
[0082] The housing 70 to which the explosion-proof member 10 is fixed may be made of, for example, resin, metal, or a composite material thereof. The housing 70 may be made of metal. Examples of metal include stainless steel, aluminum, and iron. The housing 70 may be made of resin. Examples of resin include polybutylene terephthalate (PBT), polypropylene (PP), and polyamide (PA).
[0083] <Variation 1> 3A to 3B show a first modified example of the explosion-proof member of the first embodiment. The explosion-proof member 20 shown in Figs. 3A to 3B has the same configuration as the explosion-proof member 10 described above, except that the adhesive layer 2 is a single-sided adhesive tape including a substrate 22 and an adhesive portion 21. Therefore, in the following, the same elements of the explosion-proof member 20 as those of the explosion-proof member 10 are denoted by the same reference numerals, and description thereof will be omitted.
[0084] 4 is a cross-sectional view showing an example of a state in which the explosion-proof member 20 is fixed to the housing 70 while covering the opening 71 of the housing 70. That is, the explosion-proof member 20 shown in FIG.
[0085] In Modification 1, a first surface 22a of a substrate 22, which corresponds to a first surface 2a of the adhesive layer 2, is connected to the membrane 1 so as to be aligned with a peripheral portion 11 of the membrane 1. As shown in Fig. 4, a second surface 21b of the adhesive portion 21, which corresponds to a second surface 2b of the adhesive layer 2, is fixed to a housing 70 so as to surround an opening 71 in the arrangement P.
[0086] When the adhesive layer 2 is a single-sided adhesive tape, the adhesive layer 2 may have thermal responsiveness in at least one selected from the group consisting of the first surface 21a of the adhesive portion 21 and the second surface 21b of the adhesive portion 21. For example, when the first surface 21a of the adhesive portion 21 has thermal responsiveness, when the temperature of the housing 70 rises with the rise in the temperature of the inside 72 of the housing 70, the adhesive strength of the first surface 21a of the adhesive portion 21 decreases, which enables the film 1 of the explosion-proof member 20 to automatically detach from the adherend. For example, when the second surface 21b of the adhesive portion 21 has thermal responsiveness, when the temperature of the housing 70 rises with the rise in the temperature of the inside 72 of the housing 70, the adhesive strength of the first surface 21a of the adhesive portion 21 decreases, which enables the film 1 of the explosion-proof member 20 to automatically detach from the adherend. When the temperature rises, the adhesive strength of the second surface 21b decreases, and the film 1 of the explosion-proof member 20 can automatically detach from the adherend.
[0087] In the explosion-proof member 20, the adhesive / tacky part 21 may contain a thermal foaming agent. The adhesive / tacky part 21 may be provided with thermal responsiveness by the thermal foaming agent.
[0088] The substrate 22 can be used as a support for the single-sided adhesive tape. As the substrate 22, for example, a thin material such as a plastic substrate such as a plastic film or sheet, a nonwoven fabric, a metal foil, paper, cloth, a rubber substrate such as a rubber sheet, a foam such as a foam sheet, or a laminate thereof (particularly, a laminate of a plastic substrate and another substrate, a laminate of plastic films, etc.) can be used. As the substrate 22, a plastic substrate such as a plastic film or sheet can be preferably used.
[0089] Examples of plastic substrates include polyester films such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), and polybutylene terephthalate (PBT), olefin resins containing α-olefin as a monomer component, such as polyethylene (PE), polypropylene (PP), ethylene-propylene copolymer, and ethylene-vinyl acetate copolymer (EVA), amide resins such as polyamide (nylon) and fully aromatic polyamide (aramid), polyimide (PI) films, polyvinyl chloride (PVC) films, polyphenylene sulfide (PPS) films, fluorine films, and polyether ether ketone (PEEK) films. These materials can be used alone or in combination of two or more.
[0090] Examples of polyethylene terephthalate (PET) films that can be used include Lumirror manufactured by Toray Industries, Teijin Tetron Film and Melinex manufactured by Teijin DuPont Films, and Diafoil manufactured by Mitsubishi Plastics. Examples of polyethylene naphthalate (PEN) films that can be used include Teonex manufactured by Teijin DuPont Films. Examples of polyimide (PI) films that can be used include Kapton manufactured by Toray DuPont, Apical manufactured by Kaneka, and Upilex manufactured by Ube Industries. Examples of polypropylene (PP) films that can be used include Torayfan manufactured by Toray Industries, Suntox manufactured by Suntox, and Pylen Film manufactured by Toyobo. Examples of polyvinyl chloride (PVC) films that can be used include Artron manufactured by Mitsubishi Plastics, and Achilles Type C+ manufactured by Achilles. Examples of polyethylene (PE) films that can be used include NSO manufactured by Okura Kogyo. Examples of polyphenylene sulfide (PPS) films that can be used include Torelina manufactured by Toray Industries. Examples of the fluorine film that can be used include Toyoflon manufactured by Toray Industries, Inc. and Tedlar Film manufactured by DuPont Co., Ltd. When a plastic base material is used as the base material 22, the deformability such as elongation rate may be controlled by a stretching treatment or the like.
[0091] As the nonwoven fabric, a nonwoven fabric made of a heat-resistant natural fiber can be preferably used, and in particular, a nonwoven fabric containing Manila hemp can be preferably used. As the synthetic resin nonwoven fabric, for example, a polypropylene resin nonwoven fabric, a polyethylene resin nonwoven fabric, an ester resin nonwoven fabric, etc. can be mentioned.
[0092] The metal foil is not particularly limited, and in addition to common metal foils such as copper foil, stainless steel foil, and aluminum foil, foils made of various materials such as thick silver foil, iron foil, and alloys of nickel and chromium can be used.
[0093] The paper is not particularly limited, but generally, Japanese paper, craft paper, glassine paper, fine paper, synthetic paper, topcoat paper, etc. can be used.
[0094] The thickness of the substrate 22 can be appropriately set depending on the strength, flexibility, purpose of use, etc. The thickness is, for example, but not limited to, 1 to 1000 μm, preferably 1 to 500 μm, more preferably 3 to 300 μm, and particularly preferably 5 to 250 μm. The substrate 22 may have a single layer form or a laminate form.
[0095] The substrate 22 may be attached to the film 1 by an adhesive (not shown) via the first surface 22a of the substrate 22. As the adhesive, for example, an adhesive based on the resin used for the pressure-sensitive adhesive can be used.
[0096] <Variation 2> 5A to 5B show a second modified example of the explosion-proof member of the first embodiment. The explosion-proof member 30 shown in Figs. 5A to 5B has the same configuration as the explosion-proof member 10 described above, except that the adhesive layer 2 is a double-sided adhesive tape including a substrate 22, and a first adhesive portion 211 and a second adhesive portion 212 that sandwich the substrate 22. Therefore, in the following, the same elements of the explosion-proof member 30 as those of the explosion-proof member 10 are denoted by the same reference numerals, and description thereof will be omitted.
[0097] 6 is a cross-sectional view showing an example of a state in which the explosion-proof member 30 is fixed to the housing 70 while covering the opening 71 of the housing 70. That is, the explosion-proof member 30 shown in FIG.
[0098] In the second modification, a first surface 212a of the second adhesive portion 212, which corresponds to the first surface 2a of the adhesive layer 2, is connected to the membrane 1 so as to be aligned with the peripheral portion 11 of the membrane 1. As shown in Fig. 6, a second surface 211b of the first adhesive portion 211, which corresponds to the first surface 21a of the adhesive portion 21, is fixed to the housing 70 so as to surround the opening 71 in the arrangement P.
[0099] 5A to 5B, the adhesive layer 2 is a double-sided adhesive tape including a substrate 22, and a first adhesive portion 211 and a second adhesive portion 212 that sandwich the substrate 22. The adhesive layer 2 is bonded to the film 1 via the second adhesive 212.
[0100] When the adhesive layer 2 is a double-sided adhesive tape, the adhesive layer 2 may have thermal responsiveness in at least one selected from the group consisting of the first surface 211a of the first adhesive portion 211, the second surface 211b of the first adhesive portion 211, the first surface 212a of the second adhesive portion 212, and the second surface 212b of the second adhesive portion 212. For example, when the second surface 211b of the first adhesive portion 211 has thermal responsiveness, when the temperature of the housing 70 increases with the temperature increase of the inside 72 of the housing 70, a decrease in the adhesive force occurs in the second surface 211b of the first adhesive portion 211, and the film 1 of the explosion-proof member 30 can be automatically detached from the adherend. For example, if the second surface 212b of the second adhesive portion 212 has thermal responsiveness, when the temperature of the housing 70 rises in conjunction with an increase in the temperature of the interior 72 of the housing 70, the adhesive force of the second surface 212b of the second adhesive portion 212 decreases, making it possible for the membrane 1 of the explosion-proof member 30 to automatically detach from the adherend.
[0101] In the explosion-proof member 30, at least one selected from the group consisting of the first adhesive portion 211 and the second adhesive portion 212 may contain a thermal blowing agent. The thermal blowing agent may impart thermal responsiveness to at least one selected from the group consisting of the first adhesive portion 211 and the second adhesive portion 212.
[0102] The material constituting the base material 22 may be the same as the material described in the first modification.
[0103] [Manufacturing methods for explosion-proof components] The above-mentioned explosion-proof members 10, 20, and 30 can be produced, for example, by the following method.
[0104] The explosion-proof member 10 can be produced, for example, by preparing a coating liquid containing an adhesive and heat-expandable microspheres as a thermal foaming agent, using a solvent as necessary, applying the coating liquid onto the film 1, and drying it. The explosion-proof member 10 can also be produced by applying the coating liquid onto a release paper to form a pressure-sensitive adhesive layer 2, and then transferring the pressure-sensitive adhesive layer 2 to the film 1.
[0105] The explosion-proof member 20 can be produced, for example, by applying the above-mentioned coating liquid onto a substrate 22 to form a single-sided adhesive tape including the substrate 22 and an adhesive portion 21, and then bonding the single-sided adhesive tape to a membrane 1 with an adhesive or bonding agent.
[0106] The explosion-proof member 30 can be produced, for example, by applying the above-mentioned coating liquid to the top and bottom of the substrate 22, forming a double-sided adhesive tape including the substrate 22 and a first adhesive portion 211 and a second adhesive portion 212 that sandwich the substrate 22, and then bonding the double-sided adhesive tape to the membrane 1 via the second adhesive portion 212.
[0107] The membrane 1 can be produced, for example, by the following method. The method described below is an example in which the membrane 1 is a PTE porous membrane.
[0108] (Preparation of PTFE porous membrane) First, a mixture of PTFE fine powder and a liquid lubricant is formed into a sheet extending in a predetermined direction in an unsintered state by at least one of an extrusion method and a rolling method to obtain a sheet-like compact.
[0109] The PTFE fine powder is not particularly limited, and various commercially available powders can be used, such as Polyflon F104 (manufactured by Daikin Industries, Ltd.), Fluon CD-123 (manufactured by Asahi Glass Co., Ltd.), and Teflon (registered trademark) 6J (manufactured by Mitsui-DuPont Fluorochemicals Co., Ltd.).
[0110] The liquid lubricant is not particularly limited as long as it can wet the PTFE fine powder and can be removed by evaporation, extraction, or other methods. For example, liquid paraffin, naphtha, toluene, and xylene, which are hydrocarbons, can be mentioned, as well as alcohols, ketones, esters, and fluorine-based solvents. A mixture of two or more of these may also be used. The amount of lubricant added varies depending on the molding method for the sheet-shaped molded product, but is usually about 5 to 50 parts by weight per 100 parts by weight of the PTFE fine powder.
[0111] As an example of a method for forming a mixture of PTFE fine powder and a liquid lubricant into a sheet extending in a predetermined direction, the PTFE fine powder to which the liquid lubricant has been added is compressed in a cylinder, extruded with a ram extruder to form a sheet, and then rolled to an appropriate thickness (usually 50 to 500 μm) with a pair of rolls.
[0112] Thereafter, the sheet-form compact containing the liquid lubricant is pre-stretched in the width direction perpendicular to the longitudinal direction of the sheet-form compact at a temperature at which the liquid lubricant does not evaporate, usually at room temperature. The stretching ratio at this time is preferably 1.5 to 20 times. The pre-stretching may be performed in a bath filled with the liquid lubricant.
[0113] After the preliminary stretching, the liquid lubricant is removed from the sheet-form body by a heating method or an extraction method, and the sheet-form body is dried.
[0114] Next, the sheet-like molded product from which the liquid lubricant has been removed is stretched in the longitudinal direction (the above-mentioned predetermined direction) at a temperature equal to or higher than the melting point of PTFE. The stretching ratio at this time is preferably 40 to 200 times. If the stretching ratio is lower than 40 times, the fibrils observed in the finally obtained PTFE porous membrane may become large. This is because the length becomes shorter and the average pore size becomes smaller, making it difficult to obtain high breathability. Also, if the stretching ratio is too high, the sheet-shaped molded product breaks and a PTFE porous membrane cannot be obtained. A more preferable stretching ratio is 60 to 160 times.
[0115] Thereafter, the sheet-like molded product stretched in the longitudinal direction is stretched in the transverse direction, usually at 40 to 400° C. The stretching ratio at this time is preferably 3 to 40. The temperature during stretching is more preferably 100 to 300° C. in order to obtain high breathability and prevent breakage during stretching.
[0116] From an industrial perspective, it is preferable to have fewer steps, but the above-mentioned longitudinal and transverse stretching may be carried out in multiple steps. In addition, as long as the longitudinal stretching is carried out first, the order or combination of the subsequent longitudinal or transverse stretching steps is not particularly limited. The above steps provide a PTFE porous membrane.
[0117] <Second embodiment> An example of an explosion-proof member of the second embodiment is shown in Figures 7A to 7B. The explosion-proof member 40 shown in Figures 7A to 7B is an explosion-proof member suitable for arrangement P in which the explosion-proof member 40 is fixed to the housing 70 while covering the opening 71 of the housing 70. In the explosion-proof member 40, the first surface 2a of the adhesive layer 2 is connected to the base member 3 connected to the film 1 at the peripheral portion 11 of the film 1. In the following, the same elements of the explosion-proof member 40 as those of the explosion-proof member 10 are denoted by the same reference numerals, and the description thereof may be omitted.
[0118] 8 is a cross-sectional view showing an example of a state in which the explosion-proof member 40 is fixed to the housing 70 while covering the opening 71 of the housing 70. That is, the explosion-proof member 40 shown in FIG.
[0119] The adhesive layer 2 has a thermal responsiveness that reduces its adhesive strength when heated. With this structure, when the temperature of the housing 70 rises with an increase in temperature of the inside 72 of the housing 70, the adhesive strength of the adhesive layer 2 decreases, and the film 1 of the explosion-proof member 40 can automatically detach from the adherend. When the film 1 of the explosion-proof member 40 detaches, for example, gas generated in the inside 72 of the housing 70 can be discharged from the opening 71.
[0120] The explosion-proof member 40 includes a base member 3. As shown in Figures 7A to 7B, a through hole 31 is formed in the center of the base member 3. The membrane 1 is disposed on the base member 3 so as to cover the through hole 31.
[0121] The explosion-proof member 40 further includes a cover member 4 that protects the membrane 1. The cover member 4 is disposed on the base member 3 so as to cover the membrane 1. The cover member 4 is perpendicular to the surface of the membrane 1, and when observed along a direction from the outside 73 toward the inside 72 of the housing 70 in the arrangement P, the cover member 4 covers the surface of the membrane 1 and is spaced apart from the surface of the membrane 1, and is connected to the base member 3. The cover member 4 prevents the membrane 1 from being damaged by foreign objects flying from the outside 73.
[0122] 7A and 7B, a plurality of openings 41 may be provided on the side surface of the cover member 4. With such a structure, foreign matter that has entered the interior 72 of the cover member 4 can be discharged through the openings 41.
[0123] The membrane 1 may be bonded to the base member 3. The membrane 1 may be bonded to the base member 3 by various welding methods such as thermal welding, ultrasonic welding, laser welding, etc. The membrane 1 may be disposed on the base member 3 by insert molding the membrane 1 together with the base member 3.
[0124] The base member 3 and the cover member 4 are made of, for example, resin. These members made of resin have good moldability. These members can be molded by injection molding, compression molding, powder molding, etc. The base member 3 and the cover member 4 can be formed by a known molding method such as injection molding. Since mass productivity can be improved, the base member 3 and the cover member 4 are preferably formed by injection molding. The resin constituting the base member 3 and the cover member 4 is typically a thermoplastic resin. Examples of the thermoplastic resin include polyamide (PA) such as nylon, polybutylene terephthalate (PBT), polyethylene terephthalate (PET), polyphenylene sulfide (PPS), polycarbonate (PC), polypropylene (PP), and polyphenylene ether (PPE). The resin constituting the base member 3 and the cover member 4 may contain additives such as pigments such as carbon black and titanium white; reinforcing fillers such as glass particles and glass fibers; and water repellent materials. The surfaces of the above-mentioned members may be subjected to a liquid repellent treatment. The liquid repellent treatment can be performed by the method described above as the liquid repellent treatment method for the film 1, an electrodeposition coating method, or film formation by plasma polymerization.
[0125] The cover member 4 may be joined to the base member 3 at the periphery of the base member 3. The cover member 4 can be joined to the base member 3 by various welding methods such as thermal welding, ultrasonic welding, and laser welding.
[0126] The adhesive layer 2 of the explosion-proof member 40 may have the structure described in Modification 1 and Modification 2 of the first embodiment. That is, the adhesive layer 2 of the explosion-proof member 40 may be a) a single layer, b) a single-sided adhesive tape including a substrate and an adhesive portion, or c) a double-sided adhesive tape including a substrate and a first adhesive portion and a second adhesive portion that sandwich the substrate.
[0127] 7A to 7B, the explosion-proof member 40 has a substantially disk shape. However, the shape of the explosion-proof member 40 is not limited to the example shown in Figures 7A to 7B. The shape of the explosion-proof member 40 may be, for example, a rectangular shape or a polygonal shape.
[0128] The above-described embodiments may be mutually applied unless technically inconsistent. Furthermore, the above-described embodiments and modifications may be combined with each other unless technically inconsistent. EXAMPLES
[0129] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the examples shown below.
[0130] The air permeability in the thickness direction of the film prepared in this example was evaluated by the above-mentioned method. 0 and peel time T at N°C N was evaluated by the method described above.
[0131] [Preparation of membrane] (membrane a) 100 parts by weight of PTFE fine powder (Polyflon F-104, Daikin Industries, Ltd.) was mixed with 20 parts by weight of liquid lubricant (n-dodecane, Japan Energy Corporation), compressed into a cylinder, and extruded with a ram extruder to obtain a sheet-like molded body stretched in a predetermined direction. This sheet-like molded body containing the liquid lubricant was passed between metal rolling rolls and rolled to a thickness of 300 μm. Next, the sheet-like molded body was heated to 150 ° C. to remove the liquid lubricant, and the sheet-like molded body was dried. This sheet-like molded body was stretched at 370 ° C. in the longitudinal direction by 4 times to obtain a PTFE porous membrane. The PTFE porous membrane thus obtained was named membrane a. The thickness of membrane a was 250 μm. The air permeability in the thickness direction of membrane a was 0.2 cm 3 / (cm 2 -seconds).
[0132] (membrane b) A PTFE porous membrane was obtained in the same manner as for membrane a, except that the stretching ratio in the longitudinal direction was doubled. The PTFE porous membrane thus obtained was named membrane b. The thickness of membrane b was 280 μm. The air permeability in the thickness direction of membrane b was 0.001 cm 3 / (cm 2 -seconds).
[0133] (membrane c) A PTFE porous membrane was obtained in the same manner as for membrane a, except that the stretching ratio in the longitudinal direction was 20 times. The PTFE porous membrane thus obtained was named membrane c. The thickness of membrane c was 200 μm. The air permeability in the thickness direction of membrane c was 15.4 cm 3 / (cm 2 -seconds).
[0134] (membrane d) A PET film (Toray Industries, Lumirror #38-S10) was used as film d. The thickness of film d was 38 μm. The air permeability of film d in the thickness direction was 0 cm 3 / (cm 2 -seconds).
[0135] (membrane e) The reinforcing layer was laminated at 200°C so as to sandwich the membrane c, thereby preparing a laminate consisting of the reinforcing layer, membrane c, and reinforcing layer. The laminate thus obtained was named membrane e. A nonwoven fabric (Acstar H1020-8T, manufactured by Toray Industries, Inc.) was used as the reinforcing layer. The reinforcing layer had a thickness of 100 μm. The membrane e had a thickness of 400 μm. The air permeability in the thickness direction of membrane e was 10.8 cm 3 / (cm 2 -seconds).
[0136] [Preparation of adhesive layer] (Single-sided adhesive tape A) A toluene solution was prepared by blending 100 parts by weight of an acrylic copolymer (ethyl acrylate: 2-ethylhexyl acrylate: hydroxyethyl acrylate: methyl methacrylate = 70 parts by weight: 30 parts by weight: 5 parts by weight: 6 parts by weight), 2 parts by weight of an isocyanate crosslinking agent (Coronate L, manufactured by Nippon Polyurethane Industry Co., Ltd.), 30 parts by weight of a terpene phenol tackifier resin (Yasuhara Chemical Co., Ltd., YS Polystar S145, hydroxyl value 100 mg KOH / g, acid value 2 mg KOH / g), and 35 parts by weight of thermally expandable microspheres (Matsumoto Yushi Seiyaku Co., Ltd., Matsumoto Microsphere: F-30). The toluene solution was applied to a PET film (Toray Industries, Inc., Lumirror #38-S10) as a substrate so that the thickness after drying was 35 μm, and an adhesive layer (single-sided adhesive tape) including a substrate and an adhesive portion was prepared. The single-sided adhesive tape obtained in this manner was designated as single-sided adhesive tape A. The thickness of the substrate was 38 μm, and the thickness of the adhesive portion was 35 μm.
[0137] (Single-sided adhesive tape B1) A pressure-sensitive adhesive layer (single-sided adhesive tape) was obtained in the same manner as for single-sided adhesive tape A, except that thermally expandable microspheres (Matsumoto Microsphere: F-50, manufactured by Matsumoto Yushi Pharmaceutical Co., Ltd.) were used. The single-sided adhesive tape thus obtained was designated as single-sided adhesive tape B1. The thickness of the substrate was 38 μm, and the thickness of the adhesive portion was 35 μm.
[0138] (Single-sided adhesive tape B2) An adhesive layer (single-sided adhesive tape) was obtained in the same manner as in single-sided adhesive tape A, except that heat-expandable microspheres (Matsumoto Microsphere: F-50, manufactured by Matsumoto Yushi Pharmaceutical Co., Ltd.) were used and the amount of isocyanate-based crosslinking agent (Coronate L, manufactured by Nippon Polyurethane Industry Co., Ltd.) was 1 part by weight. The single-sided adhesive tape thus obtained was designated single-sided adhesive tape B2. The thickness of the substrate was 38 μm, and the thickness of the adhesive portion was 35 μm.
[0139] (Single-sided adhesive tape C) Thermally expandable microspheres: Matsumoto Microsphere: FN-100SS, manufactured by Matsumoto Yushi Pharmaceutical Co., Ltd. A pressure-sensitive adhesive layer (single-sided adhesive tape) was obtained in the same manner as in single-sided adhesive tape A, except that 100 μm thick was used. The single-sided adhesive tape thus obtained was designated single-sided adhesive tape C. The thickness of the substrate was 38 μm, and the thickness of the adhesive portion was 35 μm.
[0140] [Example 1] A single-sided adhesive tape A was bonded to one main surface of the film a so that the substrate was in contact with the film a. The member thus obtained was the explosion-proof member of Example 1. A double-sided adhesive tape (manufactured by Nitto Denko Corporation, No. 5000NS) was used for bonding. For the explosion-proof member of Example 1, the initial adhesive strength F of the adhesive layer was 0 and the peel time T of the adhesive layer at N°C N However, in Example 1, a stainless steel test plate (SUS304, surface finish BA, thickness 0.5 mm, width 40 mm, length 125 mm) was used instead of the aluminum test plate in the peel test. In the peel adhesion test, a stainless steel test plate (SUS304, surface finish BA, thickness 0.5 mm, width 40 mm, length 125 mm) was used instead of the aluminum test plate. The results are shown in Table 1.
[0141] [Example 2] The explosion-proof member of Example 2 was the same as the explosion-proof member of Example 1. For the explosion-proof member of Example 2, the initial adhesive strength F 0 and the peel time T of the adhesive layer at N°C N In Example 2, however, an aluminum test plate (thickness 0.5 mm, width 40 mm, length 125 mm) was used in the peel test as described above. An aluminum test plate (thickness 0.5 mm, width 40 mm, length 125 mm) was used in the peel adhesion test as described above. The results are shown in Table 1.
[0142] [Example 3] The explosion-proof member of Example 3 was the same as the explosion-proof member of Example 1. For the explosion-proof member of Example 3, the initial adhesive strength F 0 and the peel time T of the adhesive layer at N°C NHowever, in Example 3, an iron test plate (thickness 0.5 mm, width 40 mm, length 125 mm) was used instead of the aluminum test plate in the peel test. In the peel adhesion test, an iron test plate (thickness 0.5 mm, width 40 mm, length 125 mm) was used instead of the aluminum test plate. The results are shown in Table 1.
[0143] [Example 4] A single-sided adhesive tape B1 was bonded to one main surface of the film a so that the substrate was in contact with the film a. The member thus obtained was the explosion-proof member of Example 4. A double-sided adhesive tape (manufactured by Nitto Denko Corporation, No. 5000NS) was used for bonding. For the explosion-proof member of Example 4, the initial adhesive strength F of the adhesive layer was 0 and the peel time T of the adhesive layer at N°C N However, in Example 4, in the peel test and the peel adhesion test, a stainless steel test plate was used instead of the aluminum test plate as in Example 1. The results are shown in Table 1.
[0144] [Example 5] The explosion-proof member of Example 5 was the same as the explosion-proof member of Example 4. For the explosion-proof member of Example 5, the initial adhesive strength F 0 and the peel time T of the adhesive layer at N°C N However, in Example 5, an aluminum test plate was used in the peel test and the peel adhesion test, as in Example 2. The results are shown in Table 1.
[0145] [Example 6] The explosion-proof member of Example 6 was the same as the explosion-proof member of Example 4. For the explosion-proof member of Example 6, the initial adhesive strength F 0 and the peel time T of the adhesive layer at N°C N However, in Example 6, an iron test plate was used instead of the aluminum test plate in the peel test and the peel adhesion test, as in Example 3. The results are shown in Table 1.
[0146] [Example 7] A single-sided adhesive tape B2 was bonded to one main surface of the film a so that the substrate was in contact with the film a. The member thus obtained was the explosion-proof member of Example 7. A double-sided adhesive tape (manufactured by Nitto Denko Corporation, No. 5000NS) was used for bonding. For the explosion-proof member of Example 7, the initial adhesive strength F of the adhesive layer was 0 and the peel time T of the adhesive layer at N°C N However, in Example 7, an aluminum test plate was used in the peel test and the peel adhesion test, as in Example 2. The results are shown in Table 1.
[0147] [Example 8] A single-sided adhesive tape C was bonded to one main surface of the film a so that the substrate was in contact with the film a. The member thus obtained was the explosion-proof member of Example 8. For bonding, a double-sided adhesive tape (manufactured by Nitto Denko Corporation, No. 5000NS) was used. For the explosion-proof member of Example 8, the initial adhesive strength F of the adhesive layer was 0 and the peel time T of the adhesive layer at N°C N However, in Example 8, in the peel test and the peel adhesion test, a stainless steel test plate was used instead of the aluminum test plate as in Example 1. The results are shown in Table 1.
[0148] [Example 9] The explosion-proof member of Example 9 was the same as the explosion-proof member of Example 8. For the explosion-proof member of Example 9, the initial adhesive strength F 0 and the peel time T of the adhesive layer at N°C N However, in Example 9, an aluminum test plate was used in the peel test and the peel adhesion test, as in Example 2. The results are shown in Table 1.
[0149] [Example 10] The explosion-proof member of Example 10 was the same as the explosion-proof member of Example 8. For the explosion-proof member of Example 10, the initial adhesive strength F of the pressure-sensitive adhesive layer was 0 and the peel time T of the adhesive layer at N°C NHowever, in Example 10, in the peel test and the peel adhesion test, an iron test plate was used instead of the aluminum test plate as in Example 3. The results are shown in Table 1.
[0150] [Example 11] The single-sided adhesive tape A was bonded to one main surface of the film b so that the substrate was in contact with the film b. The member thus obtained was the explosion-proof member of Example 11. For bonding, a double-sided adhesive tape (manufactured by Nitto Denko Corporation, No. 5000NS) was used. For the explosion-proof member of Example 11, the initial adhesive strength F of the adhesive layer was 0 and the peel time T of the adhesive layer at N°C N However, in Example 11, in the peel test and the peel adhesion test, a stainless steel test plate was used instead of the aluminum test plate as in Example 1. The results are shown in Table 1.
[0151] [Example 12] The single-sided adhesive tape A was bonded to one main surface of the film c so that the substrate was in contact with the film c. The member thus obtained was the explosion-proof member of Example 12. For bonding, a double-sided adhesive tape (manufactured by Nitto Denko Corporation, No. 5000NS) was used. For the explosion-proof member of Example 12, the initial adhesive strength F of the adhesive layer was 0 and the peel time T of the adhesive layer at N°C N However, in Example 12, in the peel test and the peel adhesion test, a stainless steel test plate was used instead of the aluminum test plate as in Example 1. The results are shown in Table 1.
[0152] [Example 13] A single-sided adhesive tape A was bonded to one main surface of the film d so that the substrate was in contact with the film d. The member thus obtained was used as the explosion-proof member of Example 13. For bonding, a double-sided adhesive tape (manufactured by Nitto Denko Corporation, No. 5000NS) was used. For the explosion-proof member of Example 13, the adhesive layer Initial adhesive strength F 0 and the peel time T of the adhesive layer at N°C NHowever, in Example 13, in the peel test and the peel adhesion test, a stainless steel test plate was used instead of the aluminum test plate as in Example 1. The results are shown in Table 1.
[0153] [Example 14] A single-sided adhesive tape A was bonded to one main surface of the film e so that the substrate was in contact with the film e. The member thus obtained was the explosion-proof member of Example 14. A double-sided adhesive tape (manufactured by Nitto Denko Corporation, No. 5000NS) was used for bonding. For the explosion-proof member of Example 14, the initial adhesive strength F of the adhesive layer was 0 and the peel time T of the adhesive layer at N°C N However, in Example 14, in the peel test and the peel adhesion test, a stainless steel test plate was used instead of the aluminum test plate as in Example 1. The results are shown in Table 1.
[0154] [Comparative Example 1] A double-sided adhesive tape (Nitto Denko Corporation, No. 5000NS) was attached to one of the main surfaces of the film a to obtain a member, which was used as the explosion-proof member of Comparative Example 1. That is, in Comparative Example 1, a single-sided adhesive tape was not used, and the film a was directly bonded to the test plate by the double-sided adhesive tape. For the explosion-proof member of Comparative Example 1, the initial adhesive strength F of the adhesive part of the double-sided adhesive tape was 0 and the peel time T of the adhesive part at N°C N However, in Comparative Example 1, in the peel test and the peel adhesion test, a stainless steel test plate was used instead of the aluminum test plate as in Example 1. The results are shown in Table 1.
[0155] [Comparative Example 2] The explosion-proof member of Comparative Example 2 was the same as the explosion-proof member of Comparative Example 1. For the explosion-proof member of Comparative Example 2, the initial adhesive strength F 0 and the peel time T of the adhesive part at N°C N However, in Comparative Example 2, an aluminum test plate was used in the peel test and the peel adhesion test, as in Example 2. The results are shown in Table 1.
[0156] [Comparative Example 3] The explosion-proof member of Comparative Example 3 was the same as the explosion-proof member of Comparative Example 1. For the explosion-proof member of Comparative Example 3, the initial adhesive strength F 0 and the peel time T of the adhesive part at N°C N However, in Comparative Example 3, an iron test plate was used in the peel test and the peel adhesion test instead of the aluminum test plate, as in Example 3. The results are shown in Table 1.
[0157] [Table 1]
[0158] Peel time T N and the peeling time T N As can be seen from the comparison, the explosion-proof members of Examples 1 to 14 exhibited superior thermal response to the explosion-proof members of Comparative Examples 1 to 3. Specifically, the explosion-proof members of Comparative Examples 1 to 3 had a peeling time T 60 was longer than 120 seconds, whereas the explosion-proof members of Examples 1 to 13 had a peeling time T 60 From the results shown in Table 1, the explosion-proof members of Examples 1 to 13 had a high viscosity due to their thermal response. It is understood that the adhesive layer had substantially lost its adhesive power in an atmosphere at 160°C.
[0159] For example, as can be seen from the comparison of Examples 1 to 3, the peel time T N and peeling time T for the iron test plate N is the peeling time T N For example, the peel time T 160 The peeling time for the stainless steel test plate was 9 seconds (Example 2), whereas the peeling time for the stainless steel test plate was 10 seconds (Example 3). 160 is 10 seconds (Example 1), and the peel time T 160 The time was 10 seconds (Example 3).
[0160] On the other hand, for example, as can be seen from the comparison of Examples 1 to 3, the adhesive strength F of the adhesive layer to the stainless steel test plate 0 and adhesive strength F to iron test plate 0 is the adhesive strength F to the aluminum test plate 0 For example, the initial adhesive strength F 0 The adhesive strength F of the adhesive to the stainless steel test plate was 1.0 N / 20 mm (Example 2). 0 The adhesive strength F to the iron test plate was 1.3 N / 20 mm (Example 1). 0 The force was 1.2 N / 20 mm (Example 3). [Industrial Applicability]
[0161] The technology of the present invention can be applied to a sealed battery pack in which a battery or a capacitor is housed inside a sealed housing. [Explanation of symbols]
[0162] 10, 20, 30, 40 Explosion-proof materials 1 membrane 1a Front page 1b Second side 11 Periphery 12 Ventilation section 2 Adhesive layer 2a Front page 2b Second side 21 Adhesive Section 21a Front page 21b Second side 211 First Adhesive Division 211a Front page 211b Second side 212 Second adhesive section 212a Front page 212b Second side 22 Base material 22a 1st page 22b 2nd side 3 Base material 31 Through hole 4 Cover member 41 Opening 5 Release Liner 70 Case 71 Aperture 72 Internal 73 External
Claims
1. An explosion-proof member suitable for being fixed to a housing in a state of covering an opening of the housing, a film that prevents foreign matter from entering the housing through the opening in the arrangement; and a pressure-sensitive adhesive layer; a first surface of the pressure-sensitive adhesive layer is connected to the membrane at a peripheral portion of the membrane or to a base member connected to the membrane at the peripheral portion; a second surface of the adhesive layer facing the opposite side to the first surface is fixed to the housing so as to surround the opening in the arrangement; the adhesive layer has a thermal responsiveness that reduces adhesive strength when heated. Explosion-proof materials.
2. the pressure-sensitive adhesive layer has the thermoresponsiveness in at least one selected from the group consisting of i) the first surface, ii) the second surface, and iii) an inner surface included in the pressure-sensitive adhesive layer and in contact with a substrate; The explosion-proof member according to claim 1.
3. Due to the thermal responsiveness, the adhesive layer substantially loses its adhesive strength in an atmosphere of 160°C. The explosion-proof member according to claim 1.
4. the peel time of the pressure-sensitive adhesive layer at 160°C determined by the following peel test is 60 seconds or less; The explosion-proof member according to claim 3. <Peel test> A sample body in which the single-sided adhesive tape having the adhesive layer is directly attached to an aluminum test plate is placed on the heating surface of a hot plate so that the adhesive layer is in contact with the heating surface. At this time, the horizontal position of the upper surface of the aluminum test plate is defined as the reference position. The heating surface is heated from 100°C to 180°C, and the time when the upper surface of the aluminum test plate passes the reference position is defined as the peel time at that temperature.
5. the initial adhesive strength of the adhesive layer to an aluminum test plate, as determined by the following peel adhesion test, is 0.5 N / 20 mm or more; The explosion-proof member according to claim 1. <Peel adhesion test> The single-sided adhesive tape having the adhesive layer is subjected to the "180° peel adhesion test against stainless steel test plate" specified in JIS Z0237:2009. However, the aluminum test plate is used instead of the stainless steel test plate. The measured peel adhesion is defined as the initial adhesive strength.
6. The pressure-sensitive adhesive layer contains a thermal blowing agent. The explosion-proof member according to claim 1.
7. the pressure-sensitive adhesive layer is a) a single layer, b) a single-sided pressure-sensitive adhesive tape including the substrate and a pressure-sensitive adhesive portion, or c) a double-sided pressure-sensitive adhesive tape including the substrate and a first pressure-sensitive adhesive portion and a second pressure-sensitive adhesive portion that sandwich the substrate. The explosion-proof member according to claim 2.
8. the base member; perpendicular to the surface of the membrane and from the exterior of the housing to the interior in the arrangement a cover member that covers the surface of the film when observed along the direction, is spaced from the surface of the film, and is connected to the base member; The explosion-proof member according to claim 1.
9. The membrane is a breathable membrane, The breathable membrane has a breathable portion surrounded by the peripheral portion. The explosion-proof member according to claim 1.
10. The air permeability in the thickness direction of the film is expressed as a Frazier number measured in accordance with the air permeability measurement method A (Fragile type method) specified in JIS L1096:2010, and is 0.001 cm 3 / (cm 2 ・seconds) and 18.8 cm 3 / (cm 2 seconds) or less, The explosion-proof member according to claim 1.
11. The membrane is a porous membrane or a non-porous membrane. The explosion-proof member according to claim 1.
12. a release liner bonded to the second surface of the pressure-sensitive adhesive layer; The explosion-proof member according to claim 1.
Citation Information
Patent Citations
Explosion proof valve structure of closed electrochemical device
JP2020072051A
Cited By
Knitted component and method of manufacturing the same
US12297569B2
Battery pack and device including same
WO2026141852A1