Square silicon substrate and manufacturing method therefor

The manufacturing of square silicon substrates with controlled thickness and low roughness through mechanical polishing addresses inefficiencies in existing technologies, enabling high-yield semiconductor production and cost-effective use of peripheral areas.

JP2024148284APending Publication Date: 2024-10-18MITSUBISHI MATERIALS CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023061295
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-05
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing silicon substrates for semiconductor chips and solar panels face issues such as non-uniform thickness, roughness, and inefficiency in utilizing peripheral areas, leading to challenges in forming fine wiring patterns and increased manufacturing costs.

Method used

A method for manufacturing a square silicon substrate with controlled thickness variation (TTV ≤ 100.0 μm) and low roughness (Ra ≤ 2.0 nm) using mechanical polishing without chemical etching, ensuring the entire surface is usable for circuit formation, including the periphery.

Benefits of technology

The method enables the production of high-yield semiconductor chips with reduced costs and improved flatness, allowing for fine wiring patterns and efficient use of the entire substrate surface, while maintaining structural integrity and preventing cracking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148284000001_ABST
    Figure 2024148284000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method for a square silicon substrate.SOLUTION: There is provided a manufacturing method for a square silicon substrate, the square silicon substrate having a first surface for forming a circuit and a second surface positioned opposite to the first surface. The manufacturing method includes: a slicing step of slicing a silicon ingot to form a square plate-shaped member; a grinding step of grinding both surfaces of the plate-shaped member; and a polishing step of mechanically polishing one surface of the plate-shaped member, which has been subjected to the grinding step, to form a square silicon substrate having a first surface. Chemical etching is not performed during the grinding step, during the polishing step, and between the grinding step and the polishing step, and the square silicon substrate is formed to have a thickness of 0.5 mm or more and 2.0 mm or less. Moreover, in the square silicon substrate, a TTV in the first surface is 100.0 μm or less, and the maximum peak height Rp of the first surface is 100.0 nm or less. In the polishing step, a finishing slurry composed of finishing abrasive grains and a liquid having a hydrogen ion exponent of 7.0 or more and 9.0 or less is used.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention is a silicon substrate for semiconductor use. [Background technology]

[0002] Silicon substrates formed by slicing a silicon ingot have conventionally been used as semiconductor substrates. Silicon substrates for manufacturing multiple semiconductor chips are made of single crystal silicon and have a round outer shape, while silicon substrates for solar panels are mainly made of polycrystalline silicon and have a square outer shape. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 5401683 [Patent Document 2] JP 2017-208571 A [Patent Document 3] JP 2015-6990 A [Patent Document 4] JP 2006-202831 A [Non-patent literature]

[0004] [Non-Patent Document 1] Issued in July 2002, by the Japan Electronics and Information Technology Industries Association, JEITA EM-3602 "Standard Specifications for Dimensional Standards of Silicon Mirror Wafers" Summary of the Invention [Problem to be solved by the invention]

[0005] Incidentally, a method for manufacturing a silicon substrate made of single crystal silicon for manufacturing semiconductor chips is disclosed in Patent Document 1, but as shown in Non-Patent Document 1, the silicon substrate for semiconductor chips is formed in a round shape using a silicon ingot, and the peripheral area is excluded and the inner area is used for circuit formation, so there is an unused area. It is desirable to utilize the silicon substrate including the peripheral area. In the manufacture of large rectangular silicon substrates, polishing the surface can result in only the corners being scraped off, which can cause thickness variations within the surface. In addition, as a method for manufacturing silicon substrates, chemical etching is performed on a plate-shaped member formed by slicing a silicon ingot (Patent Documents 2, 3, and 4), but when chemical etching using an acid solution is performed on a round or square plate-shaped member made of polycrystalline silicon, grain boundaries may be preferentially removed, or only the grain boundaries may not be removed, which may result in a rough etched surface. In addition, with chemical etching, the removal rate differs depending on the crystal plane orientation of the plate-shaped member, which may result in a rough surface.

[0006] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide a square silicon substrate and a method for manufacturing the same. [Means for solving the problem]

[0007] The square silicon substrate of the present invention has a thickness of 0.5 mm or more and 2.0 mm or less, a total thickness variation (hereinafter referred to as TTV) in a first surface for forming a circuit is 100.0 μm or less, and further, a maximum peak height Rp of the first surface is 100.0 nm or less.

[0008] The term "square" means that, when the square silicon substrate is viewed from above, four corners are arranged on the periphery, forming a rectangular outline. Note that the square shape also includes a case where one or more of the four corners are cut out to form a notch. In a rectangular silicon substrate, the variation in the overall thickness, including the peripheral portion, is small, and the first surface for circuit generation has a small roughness and high flatness, so that the entire first surface can be used for circuit formation. The dimensions of the rectangular silicon substrate are not limited, but it is formed into a rectangular shape with a side length of 300 mm or more, for example. If the thickness of the square silicon substrate is thinner than 0.5 mm, it will warp, and if it is thicker than 2.0 mm, it will become too heavy and difficult to transport. If the TTV is greater than 100.0 μm, it becomes impossible to form a fine wiring pattern with a line width of 2 μm on the first surface. If the maximum peak height Rp of the first surface is greater than 100.0 nm, it also becomes difficult to form a fine wiring pattern.

[0009] The rectangular silicon substrate of the present invention is made of polycrystalline silicon, and preferably made of columnar crystal silicon.

[0010] Since silicon substrates have reduced thickness variation and roughness, even those made of polycrystalline silicon have the advantage that they can be used for semiconductor chips. Furthermore, when made of columnar crystal silicon, the bending strength is greater than when made of single crystal silicon or polycrystalline silicon (excluding columnar crystal silicon), making it possible to prevent cracks.

[0011] In the square silicon substrate of the present invention, the TTV is preferably determined by the area (S1 [mm 2 ]) (TTV / S1) is 1.00×10 ―6 [mm -1 ]below.

[0012] This value (TTV / S1) is considered as the flatness relative to the area of ​​the square silicon substrate, and the value (TTV / S1) is 1.00×10 ―6 [mm -1 ] or less, the deviation in the thickness direction during the exposure process for forming wiring is small, making it possible to form fine wiring. ―6 [mm -1If the thickness of the wiring is larger than 100 nm, the thickness direction deviation increases during the exposure process for forming the wiring, which makes it difficult to form fine wiring, which is undesirable.

[0013] In the square silicon substrate of the present invention, the first surface preferably has an arithmetic mean roughness Ra of 2.0 nm or less.

[0014] By setting the arithmetic mean roughness Ra to 2.0 nm or less, a fine wiring pattern can be formed. If the arithmetic mean roughness Ra is greater than 2.0 nm, it becomes difficult to form a fine wiring pattern.

[0015] The method for manufacturing a square silicon substrate of the present invention is a method for manufacturing a square silicon substrate having a first surface for forming a circuit and a second surface opposite to the first surface, and includes a slicing step of slicing a silicon ingot to form a square plate-shaped member, a grinding step of grinding both surfaces of the plate-shaped member, and a polishing step of mechanically polishing one surface of the plate-shaped member that has been subjected to the grinding step to form the square silicon substrate having the first surface, and is characterized in that chemical etching is not performed during the grinding step, the polishing step, and between the grinding step and the polishing step, and the square silicon substrate is formed to a thickness of 0.5 mm to 2.0 mm.

[0016] "Mechanical polishing" refers to the process of removing irregularities and other imperfections by scraping the surface to be polished with abrasive grains, etc., without involving any chemical action that would dissolve or alter the surface. "Mechanical polishing" does not include "mechanochemical polishing", which is mechanical but also involves chemical polishing. In the method for manufacturing a silicon substrate of the present invention, one side of a plate-shaped member that has been subjected to a grinding process is mechanically polished to form a first surface without performing chemical etching using an acid solution, so that the first surface is formed with small variations in thickness and is flat with small roughness over its entire area.

[0017] In the method for producing a silicon substrate of the present invention, preferably, in the polishing step, a finishing slurry consisting of finishing abrasive grains and a liquid having a hydrogen ion exponent [pH] of 7.0 to 9.0 is used. In the polishing step, the finishing abrasive grains used are those that do not cause chemical reaction, and for this reason, the liquid used is preferably pure water.

[0018] By performing mechanical polishing without performing chemical etching with an acid solution, the amount of etching does not vary at different locations on the plate-shaped member, and the entire first surface can be polished approximately uniformly. Effect of the Invention

[0019] According to the present invention, it is possible to manufacture a large rectangular substrate with small overall thickness variation and good flatness of the circuit formation surface. Although the application is not limited, when used in the manufacture of semiconductor chips, the number of chips that can be obtained can be increased, and the manufacturing cost and the unit price of the chip can be reduced. [Brief description of the drawings]

[0020] [Figure 1] FIG. 2A is a plan view of a square silicon substrate according to an embodiment of the present invention, and FIG. 2B is a partially enlarged cross-sectional view of the square silicon substrate taken along line A1-A1 in FIG. [Diagram 2] FIG. 11 is a plan view showing a modified example of a square silicon substrate according to an embodiment of the present invention. [Diagram 3] 1A to 1C are diagrams illustrating a manufacturing process of a square silicon substrate according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, a square silicon substrate 1 according to an embodiment of the present invention will be described with reference to the drawings. As shown in FIG. 1(a), the rectangular silicon substrate 1 has a pair of first edges 11 extending in a straight line parallel to each other and a pair of second edges 12 extending in a straight line parallel to each other and disposed at right angles to the first edges 11, and the peripheral edge is formed into a rectangle when viewed in a plan view. The lengths L11, L12 of the first edges 11 and the second edges 12 are not limited, but are, for example, 300 mm or more and 900 mm or less. The lengths L11, L12 of the first edges 11 and the second edges 12 are preferably 500 mm or more and 900 mm or less. In the rectangular silicon substrate 1, the four points where the first edges 11 and the second edges 12 are connected are referred to as corners 13. As shown in FIG. 1( b ), the square silicon substrate 1 has a first surface 110 for forming a circuit thereon, and a second surface 120 located opposite to the first surface 110 . Furthermore, the square silicon substrate 1 is made of single crystal or polycrystalline silicon, and preferably, among the polycrystalline silicon, columnar crystal silicon obtained by crystal growth in one direction is also used. When the square silicon substrate 1 is made of columnar crystal silicon, the square silicon substrate 1 is formed such that the first surface 110 and the second surface 120 intersect with the crystal growth direction. In the first edge portion 11 and the second edge portion 12 which form the peripheral portion of the square silicon substrate 1, as shown in FIG. 1(b), a first edge 141 is formed by the first surface 110 and the outer peripheral end face 130, and a second edge 142 is formed by the second surface 120 and the outer peripheral end face 130. The thickness t1 of the square silicon substrate 1 is, for example, 0.5 mm or more and 2.0 mm or less. The thickness t1 is determined by measuring the thicknesses of the central measurement point P1 and the four corner measurement points P2 to P5 using a micrometer or a three-dimensional measuring machine, and calculating the average value of these. In FIG. 1, the five measurement points are represented by circles. The central measurement point P1 is the point where one imaginary line connecting the diagonally arranged corners on the outline in a plan view intersects with the other imaginary line. The corner measurement points P2 to P5 are points around each corner, each 10 mm inward from the first edge 11 and the second edge 12.

[0022] The square silicon substrate 1 has a high flatness with a small roughness over the entire first surface 110, including the peripheral portion of the square silicon substrate 1. Specifically, the first surface 110 has an arithmetic mean roughness Ra of, for example, 2.1 nm or less, and preferably 2.0 nm or less. The first surface 110 also has a maximum peak height Rp of, for example, 100.0 nm or less, and preferably 50.0 nm or less.

[0023] The square silicon substrate 1 is formed with small variations in thickness, and its total thickness variation (TTV) is, for example, 100.0 μm or less, preferably 70.0 μm or less, and more preferably 40.0 μm or less. Here, TTV is the difference (tmax-tmin) between the maximum thickness tmax of the square silicon substrate 1 and the minimum thickness tmin of the square silicon substrate 1. The second surface 120 of the square silicon substrate 1 is fixed to the mounting surface of a measuring table by a suction device or the like, and this mounting surface is used as a reference surface. The maximum thickness tmax is the maximum thickness (dimension) of the square silicon substrate 1 from the reference surface, and the minimum thickness tmin is the minimum thickness (dimension) of the square silicon substrate 1 from the reference surface. Both the maximum thickness tmax and the minimum thickness tmin are for the entire first surface 110 including the peripheral portion of the square silicon substrate 1. In FIG. 1(b), the measuring table 200 is represented by a dashed line, and the state in which the second surface 120 of the square silicon substrate 1 is fixed to the mounting surface 210 of the table 200 is shown.

[0024] Furthermore, in the square silicon substrate 1, the TTV is defined as the area S of the first surface 110. 2 Divided by (unit: mm ―1 :TTV / S1) is considered as the flatness relative to the area of ​​the square silicon substrate 1, and is, for example, 1.00×10 ―6 mm ―1 or less, preferably 0.50×10 ―6 mm ―1 More preferably, it is 0.20×10 or less. ―6 mm ―1 The following is the result.

[0025] The square silicon substrate 1 may have a position specifying portion formed on a part of the periphery as a reference for specifying two-dimensional position information within a surface, for example, as a mark serving as an origin. For example, in the rectangular silicon substrate 1A shown in FIG. 2, one corner 13 is cut out and formed as a notch 15 so that the shape of one corner is different from the shapes of the other three corners. The notch 15 has a dimension L21 of 1.0 mm or more and 20.0 mm or less along a first direction in which the first edge 11 extends, and a dimension L22 of 1.0 mm or more and 20.0 mm or less along a second direction in which the second edge 12 extends (perpendicular to the first direction), and is sufficiently short compared to the first edge 11 and the second edge 12 of the rectangular silicon substrate 1A. In this case, the rectangular silicon substrate 1A also has a substantially rectangular outer shape when viewed from the first surface 110 side. The notch 15 is not limited to a shape extending linearly in a plan view viewed from the first surface 11 side, and may be formed in an arc shape or the like. The notch 15 may be formed as a so-called notch obtained by cutting out a part of an edge extending linearly. The position identifying portion can also be used to identify the directionality of the square silicon substrate 1A. In this way, a square silicon substrate 1 with corners intentionally cut off is also within the scope of the technical concept of the present invention.

[0026] (Method of manufacturing square silicon substrate 1) The manufacturing method of the square silicon substrate 1 includes a slicing step of slicing a silicon ingot to form a plate-shaped member, a grinding step of grinding both sides of the plate-shaped member, and a polishing step of polishing one side of the plate-shaped member after the grinding step, as shown in Fig. 3. Hereinafter, one side of the plate-shaped member is referred to as a first processed surface, and the other side opposite to the first processed surface is referred to as a second processed surface.

[0027] (Slicing process) In the slicing process, a band saw or a wire saw with diamond abrasive grains is used to cut a single crystal or polycrystalline silicon ingot into a plate-like member having a thickness of, for example, 1.0 mm to 2.2 mm. The silicon ingot may be rectangular or cylindrical. The prismatic silicon ingot may be, for example, 300 mm to 1200 mm in length, 300 mm to 1200 mm in width, and 10 mm to 300 mm in height (thickness). The plate-like member is formed so that its outer shape in plan view from the first processing surface side is square or rectangular. Columnar crystal silicon ingots are produced by injecting molten silicon into a mold having a rectangular or circular horizontal cross section, and then cooling the mold from below, causing the silicon to solidify in one direction from bottom to top in the mold, thereby forming a prismatic or cylindrical silicon ingot, and the surface is ground and polished to form the columnar crystal silicon ingot into the desired rectangular parallelepiped. Furthermore, when a silicon ingot with columnar crystals is used, the silicon ingot is sliced ​​so that a first processed surface of the plate-shaped member and a second processed surface positioned opposite to the first processed surface intersect with the crystal growth direction. The cylindrical silicon ingot may be, for example, one having a diameter of φ400 mm or more and φ1200 mm or less and a height (thickness) of 10 mm or more and 300 mm or less. When a cylindrical silicon ingot is used, the plate-like member is formed so that its outer shape in a plan view from the first processing surface side is circular. For example, a silicon ingot with a diameter of 450 mm or more is made of polycrystal. A cylindrical ingot with large vertical and horizontal dimensions is also made of polycrystal.

[0028] (Grinding process) In the grinding process, the first and second processed surfaces are ground and roughly polished. Note that no chamfering is performed on the peripheral portions of the plate-shaped member between the slicing process and the grinding process, so both the first and second processed surfaces are cross sections formed in the slicing process. In the grinding process, a coarser polishing is performed, as a pretreatment for the polishing process, using, for example, a lapping machine, compared to the polishing in the polishing process. Hereinafter, the lapping process performed on the first and second processed surfaces using the lapping machine will be referred to as the lapping process. In a lapping machine, a plate-like member is held by a carrier, and lapping slurry is placed between the rotating lapping plate and the surface to be polished, thereby performing polishing. The lapping slurry is composed of lapping abrasive grains and lapping liquid, and the pH of the lapping slurry is 7.0 to 9.0. The lapping abrasive grains are made of SiC or Al2O3. The lapping liquid may be, for example, pure water, an anionic surfactant such as sodium laurate, a cationic surfactant such as dodecylamine hydrochloride, a nonionic surfactant such as polyethylene glycol mono-4-nonylphenyl ether, or a polyhydric alcohol such as glycol. In the lapping machine, the first processing surface side and the second processing surface side of the plate-like member protruding from the carrier are polished so that the thickness of the plate-like member after the lapping process is close to the thickness of the carrier. During the lapping process, the thickness of the plate-like member protruding from the carrier is preferably 0.1 mm or more and 0.5 mm or less, so that the polishing can be suitably performed on the entire first processing surface and the second processing surface. If the thickness of the plate-like member protruding from the carrier exceeds 0.5 mm, the edges of the first processing surface and the second processing surface may be damaged, and if the thickness of the plate-like member protruding from the carrier is thinner than 0.1 mm, the carrier is scraped and deformed, which may cause the plate-like member to come off. The arithmetic mean roughness Ra of the first machined surface and the second machined surface of the plate-like member after the lapping step is set to, for example, 1.0 μm or less. The thickness of the plate-like member after the lapping step is set to, for example, 1.0 mm or more and 2.2 mm or less. Furthermore, as a grinding step for reducing the roughness of the first and second surfaces of the plate-shaped member before the polishing step, instead of the lapping step, a surface grinding machine may be used to perform surface grinding of the plate-shaped member. In the surface grinding machine, unevenness of the first and second processed surfaces of the plate-shaped member may be removed by a grinding wheel provided on a rotating grinding machine. A grinding wheel is fixed to the grinding machine, and this grinding wheel is also made of SiC or Al2O3. The arithmetic mean roughness Ra of the first and second processed surfaces of the plate-shaped member after the grinding step is, for example, 1.0 μm or less.

[0029] (Polishing process) In the polishing process, the first processed surface that has been subjected to the grinding process is mechanically finished by a polishing device. Note that, since no chemical etching is performed between the grinding process and the polishing process to remove irregularities on the first processed surface of the plate-shaped member, the first processed surface that is surface-treated in the polishing process is a lapping processed surface. The polishing device holds a plate-like member with a carrier and applies finishing slurry between a rotating pad and the surface to be polished, thereby performing polishing. The finishing slurry is composed of finishing abrasive grains and a finishing liquid, and the hydrogen ion exponent (pH) of the finishing slurry is 7.0 or more and 9.0 or less. The finishing abrasive grains are composed of SiO2, and the finishing liquid can be, for example, pure water, anionic surfactants such as sodium laurate, cationic surfactants such as dodecylamine hydrochloride, nonionic surfactants such as polyethylene glycol mono-4-nonylphenyl ether, polyhydric alcohols such as glycol, and preferably pure water is used. In the polishing device, the first processing surface side of the plate-like member protruding from the carrier is polished so that the thickness of the plate-like member after the polishing process is close to the thickness of the carrier. During the polishing process, the thickness of the plate-like member protruding from the carrier is preferably 0.1 mm to 0.5 mm, which allows the entire first processing surface to be suitably polished. If the thickness of the plate-like member protruding from the carrier exceeds 0.5 mm, the edge of the first processing surface may be damaged, and if the thickness of the plate-like member protruding from the carrier is less than 0.1 mm, the carrier may be scraped and deformed, which may cause the plate-like member to come off. After the polishing process, the arithmetic mean roughness Ra of the first processed surface is set to, for example, 2.0 nm or less, the maximum peak height Rp of the first processed surface is set to, for example, 100.0 nm or less, the thickness t1 is set to, for example, 0.5 mm or more and 2.0 mm or less, the TTV is set to, for example, 100.0 μm or less, and further, the value (TTV / S1) obtained by dividing the TTV by the area S1 of the first processed surface is set to, for example, 1.00×10 ―6 mm ―1 To the following: Through this polishing process, the first processed surface is formed into a mirror-finished first surface 110, and the silicon substrate is completed.

[0030] In the silicon substrate of this embodiment, unevenness on the surface of the plate-like member is removed without chemical etching in the grinding step, the polishing step, and between the grinding step and the polishing step, so that the variation in the overall thickness including the peripheral portion is small, and the first surface 110 for circuit generation has small roughness and high flatness, so that the entire area of ​​the first surface 110 including the peripheral portion can be used for circuit formation. Therefore, the silicon substrate of this embodiment can be subjected to a process for forming a wiring pattern, including the peripheral portion. Compared to a round silicon substrate in which processes such as forming wiring patterns are performed in the area inside the peripheral edge without utilizing the peripheral edge, the silicon substrate of this embodiment can increase the number of semiconductor chips, etc., from which it is possible to reduce manufacturing costs and unit prices of products. If the thickness of the square silicon substrate is thinner than 0.5 mm, it will warp, and if it is thicker than 2.0 mm, it will become too heavy and difficult to transport. If the TTV is greater than 100.0 μm, it is not possible to form a fine wiring pattern with a line width of 2 μm on the first surface. If the maximum peak height Rp of the first surface 110 is greater than 100.0 nm, it is also difficult to form a fine wiring pattern. In particular, in a conventional polycrystalline silicon substrate that has been subjected to chemical etching, the grain boundaries are preferentially removed or remain, which can result in a large TTV and maximum peak height Rp. However, even when the rectangular silicon substrate 1 is made of polycrystalline silicon, the first surface 110 is formed so that the TTV and maximum peak height Rp of the first surface 110 are small, thereby enabling good circuit formation.

[0031] When the silicon substrate is made of columnar crystal silicon, the bending strength of the substrate is greater than when it is made of single crystal or non-columnar polycrystal, and cracking can be prevented.

[0032] Furthermore, the value (TTV / S1) is 1.00×10 ―6 [mm -1 If the value (TTV / S1) is 1.00×10 or less, the deviation in the thickness direction during the exposure process for forming wiring is small, making it possible to form fine wiring. ―6 [mm-1 If the thickness of the wiring is larger than 100 nm, the thickness direction deviation increases during the exposure process for forming the wiring, which makes it difficult to form fine wiring, which is undesirable.

[0033] By setting the arithmetic mean roughness Ra to 2.0 nm or less, a fine wiring pattern can be formed. If the arithmetic mean roughness Ra is greater than 2.0 nm, it becomes difficult to form a fine wiring pattern. In particular, in a conventional polycrystalline silicon substrate that has been subjected to chemical etching, the grain boundaries are preferentially removed or remain, which can result in a large arithmetic mean roughness Ra. However, even when the square silicon substrate 1 is made of polycrystalline silicon, the first surface 110 is formed so as to have a small arithmetic mean roughness Ra, thereby enabling good circuit formation.

[0034] Conventionally, when a plate-shaped member is chemically etched, the amount of etching by the acid solution may differ at different locations on the plate-shaped member. However, in the method for manufacturing a square silicon substrate of the present embodiment, the entire surface can be polished almost uniformly.

[0035] The present invention can be practiced without being limited to the above-described description and illustrated examples. Although the silicon substrate has a side length of 300 mm or more as an example, the present invention can also be applied to the manufacture of silicon substrates with sides of less than 300 mm.

[0036] In addition, although the uses of the square silicon substrate are not limited, for example, when it is used as a substrate for an interposer, the square silicon substrate itself is formed thin, so that the thickness of the entire packaged chip can be reduced. The silicon substrate of this embodiment can also be used as a substrate for a solar panel.

[0037] (Directional Identification) When a rectangular silicon substrate has a chamfered portion on a part of its periphery, the orientation of the rectangular silicon substrate can be identified. Another example of a configuration for identifying the orientation is one in which the entire periphery of the rectangular silicon substrate is chamfered and a part of the periphery is provided that protrudes when viewed in a plane. EXAMPLES

[0038] A number of silicon substrates with different outer shapes and thicknesses were manufactured, and the outer shape, thickness, thickness variation, and first surface roughness were evaluated.

[0039] The method for manufacturing a silicon substrate includes a slicing step of slicing a silicon ingot to form a plate-shaped member, a grinding step of grinding both sides (first and second processed surfaces) of the sliced ​​plate-shaped member, and a polishing step of polishing the first processed surface of the plate-shaped member after the grinding step. Note that in the method for manufacturing a silicon substrate, a beveling step of chamfering the periphery of the sliced ​​plate-shaped member is not performed between the slicing step and the grinding step, and an etching step of chemically etching both sides (first and second processed surfaces) of the plate-shaped member is not performed between the grinding step and the polishing step.

[0040] (Grinding process) The grinding step was carried out using either a lapping machine or a surface grinding machine. The lapping machine held the plate-like member with a carrier, and performed lapping by putting a lapping slurry between the rotating lapping plate and the surface to be polished. The lapping slurry is composed of lapping abrasive grains and lapping liquid. The lapping abrasive grains are made of SiC or Al2O3. The lapping liquid is made of pure water, and may contain an anionic surfactant such as sodium laurate, a cationic surfactant such as dodecylamine hydrochloride, a nonionic surfactant such as polyethylene glycol mono-4-nonylphenyl ether, or a polyhydric alcohol such as glycol. A grinding wheel is fixed to the grinding machine and is made of the same material as the lapping abrasive grains. In the surface grinding machine, irregularities on the first and second processed surfaces of the plate-shaped member are removed by a grinding wheel attached to the rotating grinding machine. The grinding wheel attached to the grinding machine is made of SiC or Al2O3.

[0041] (Polishing process) In the polishing step, the first processed surface of the plate-shaped member that had been subjected to the grinding step was mechanically polished with a polishing device to be finished into a mirror surface. In the polishing device, with the plate-like member held by the carrier, a finishing slurry was placed between the rotating pad and the surface to be polished, and the first processed surface was polished. The finishing slurry is composed of finishing abrasive grains and finishing liquid. The finishing abrasive grains are made of SiO2, and the finishing slurry is made of pure water, and may contain an anionic surfactant such as sodium laurate, a cationic surfactant such as dodecylamine hydrochloride, a nonionic surfactant such as polyethylene glycol mono-4-nonylphenyl ether, and a polyhydric alcohol such as glycol.

[0042] Among the samples manufactured by the silicon substrate manufacturing method, samples 1 to 21 were made using rectangular silicon ingots. Of these, sample 17 is made of single crystal silicon, sample 12 is made of polycrystal (excluding columnar crystals), and the others are made of columnar crystal silicon. In addition, in the silicon substrate of columnar crystal silicon, the first and second surfaces are formed so as to intersect with the growth direction of the columnar crystals. Samples 1 to 21 have a square or rectangular outer shape when viewed in plan from the first surface side. Sample 22 uses a cylindrical silicon ingot, and has a circular outer shape when viewed from above from the first surface side. Among the manufacturing methods described above, the polishing step was omitted, and a square silicon substrate was manufactured by the slicing step and the grinding step to obtain Sample 23. In addition, the manufacturing method includes a slicing process, a grinding process, an etching process in which the first processed surface is chemically etched after the grinding process, and a polishing process in which the etched surface is polished after the etching process. This produces a square silicon substrate, which is sample 24. A glass substrate was used as sample 25 as a reference example.

[0043] For each sample, Table 1 shows the material and crystal type constituting the ingot, the outer dimensions (width, height) [mm] of the plate-shaped member obtained by slicing the ingot, the number of corners located on the outline when the plate-shaped member is viewed in plan from the first processed surface side, and the thickness t2 of the plate-shaped member [mm]. The external dimensions (width, length) of the sliced ​​plate-like members were measured using a three-dimensional measuring machine (Quick Vision manufactured by Mitutoyo Corporation). The external dimensions (width, length) [mm] were rounded off to the first decimal place to obtain integers as significant figures. The thickness t2 of the plate-shaped member after the slicing process, the thickness t3 of the plate-shaped member after the grinding process described below, and the thickness t4 of the plate-shaped member after the polishing process were all measured using an optical interferometer type flatness measuring device. The conditions for determining the thickness of the plate-shaped member were to measure the thickness at the center measurement point of the plate-shaped member and the thickness at the four corner measurement points of the plate-shaped member after each process, and to determine the average values ​​of these as the thicknesses t2, t3, and t4. The center measurement point P1 is the point where one imaginary line connecting the corners arranged diagonally at the outline of the plate-shaped member when viewed in a plane intersects with the other imaginary line. The corner measurement points are points around each corner that are 10 mm inward from the first edge and the second edge that constitute the corner. The values ​​obtained by rounding off the first decimal place were used as significant figures for t2, t3, and t4 [mm]. For the circular plate-like member of sample 19, the thickness was measured at the center and at four points 10 mm inward from the edge of the circle, and t2, t3, and t4 were calculated as the average values.

[0044] For each sample, the type of equipment used for the grinding process (lapping machine and surface grinding machine), the materials used for the abrasive grains and grindstones in the grinding process, the thickness t3 [mm] of the silicon substrate after the grinding process and before the polishing process, whether or not an etching process was performed, whether or not a polishing process was performed, the hydrogen ion exponent (pH) of the finishing slurry in the polishing process, and the thickness t4 [mm] of the silicon substrate after the polishing process are shown in Table 2. The hydrogen ion exponent [pH] was rounded off to one decimal place to obtain the significant digit.

[0045] Table 3 also shows the TTV of each sample prepared through the polishing process, the maximum peak height Rp of the first surface (mirror surface), the value obtained by dividing the TTV by the area S1 of the first surface (TTV / S1), and the arithmetic mean roughness Ra of the first surface. The outline shape and dimensions of the plate-like member after the polishing process in plan view from the first surface side are the same as the outline and dimensions of the plate-like member after the base slice is fixed, so the area S1 was calculated by multiplying the vertical and horizontal dimensions in Table 1. Value (TTV / S1) [mm -1 ] is rounded off to the ninth decimal place to obtain the significant digit. The area for forming the circuit, which is the measurement target for TTV, maximum peak height Rp, arithmetic mean roughness Ra, and thickness t4, is the entire first surface. The TTV of the silicon substrate after the polishing process was calculated as the difference (tmax-tmin) between the maximum thickness tmax and the minimum thickness tmin measured using a flatness measuring device based on an optical interferometer. The maximum thickness tmax and the minimum thickness tmin were measured while the second surface of the silicon substrate was fixed by suction to the mounting surface of the flatness measuring device, and the mounting surface of the flatness measuring device was used as the reference surface, and the maximum thickness tmax and the minimum thickness tmin from the reference surface to the first surface were measured. The TTV [μm] was rounded off to one decimal place to obtain the significant digit. Both the maximum peak height Rp and the arithmetic mean roughness Ra were measured using a white light interferometer (Nexview, a white light interferometer manufactured by Zygo Corporation). For each sample, the arithmetic mean roughness Ra and the maximum peak height Rp were measured at five arbitrary observation points on the first surface, including the periphery, and the average values ​​obtained were taken as the arithmetic mean roughness Ra and the maximum peak height Rp of the sample. Each observation point was a square field of view of 1500 μm in length and 1500 μm in width. For both the maximum peak height Rp [nm] and the arithmetic mean roughness Ra [nm], the values ​​obtained by rounding off to one decimal place were used as significant figures.

[0046] [Table 1]

[0047] [Table 2]

[0048] [Table 3]

[0049] (Evaluation method for each sample) In evaluating the outer shape, thickness, thickness variation, and first surface roughness of each sample produced, we confirmed whether the entire first surface could be used for circuit formation, whether a 2 μm-wide fine wiring pattern could be formed on the first surface, and whether the first surface could be transported by a material hand when performing film formation processing, etc.

[0050] (A) Criteria for whether or not to use the entire first page A test was deemed to have passed if the following (a1) and (a2) were satisfied, and was deemed to have failed if at least one of (a1) and (a2) was not satisfied. Of the tests that passed, a test in which the maximum peak height Rp was 50.0 nm or less was rated as "excellent." Note that (a1) is an item for judging whether the silicon substrate can be divided with a good yield, and (a2) is an item for judging the efficiency of using the entire surface, and if there are any parts with large steps where the maximum peak height Rp is large, the efficiency of using the entire surface decreases. (a1) The silicon substrate has a rectangular shape. (a2) The maximum peak height Rp is 100.0 nm or less.

[0051] (B) Criteria for determining whether or not a 2 μm-wide fine wiring pattern can be formed on the first surface A sample was deemed to have passed if it met the following (b1) and (b2), and was deemed to have failed if it did not meet at least one of (b1) and (b2). Of the passed samples, a sample with a TTV of 50.0 μm or less and a maximum peak height Rp of 50.0 nm or less was rated as "excellent." Note that (b1) is an item for judging the thickness variation that may affect circuit formation, and (b2) is an item for judging the roughness of the first surface that may affect circuit formation, because in areas with a large maximum peak height Rp and large steps, it is difficult to form fine wiring. (b1) The TTV is 100.0 μm or less. (b2) The maximum peak height Rp is 100.0 nm or less.

[0052] (C) Criteria for the admissibility of transportation If the following condition (c1) was met, it was deemed to have passed, and if it was not met, it was deemed to have failed. (c1) is an item to judge whether the silicon substrate, with one side dimension between 300 mm and 900 mm, can maintain its shape when it is transported up and down and left and right by a robot arm (material hand) during circuit formation, and whether it is a transportable weight. (c1) Thickness t4 is 0.5 mm or less and 2.0 mm or less.

[0053] The feasibility of using the entire first surface, forming fine patterns, and transporting is shown in Table 4. In Table 4, pass is indicated with "〇", among which "excellent" is indicated with "◎", and fail is indicated with "NG".

[0054] [Table 4]

[0055] (About evaluation) In the samples 1 to 17, the outer shape seen from the first surface side is a square or a rectangle, so that the entire first surface can be used for circuit formation without waste. Furthermore, the TTV is 100.0 μm or less, so that the variation in the thickness of the silicon substrate is small, and the maximum peak height Rp of the first surface is 100.0 nm or less, so that the roughness is small, so that a fine wiring pattern can be formed. Furthermore, the thickness t4 of the silicon substrate is 0.5 mm or more and 2.0 mm or less, so that the plate-like shape can be maintained even during transportation. Compared with the sample 17 made of single crystal silicon, the samples 1 to 11, 13, and 14 made of columnar crystal silicon tend to have higher values ​​of TTV, maximum peak height Rp, and arithmetic mean roughness Ra, which is thought to be due to the influence of grain boundaries. It was also confirmed that Samples 1 to 11, 13, and 14 made of columnar crystal silicon have a higher bending strength and can be prevented from cracking, compared to Sample 17 made of single crystal silicon. In addition, the first surface could be finished to a flatness equal to or better than that of the glass substrate of the reference example. In addition, among samples 1 to 17, the value (TTV / S1) of the samples in which the usability of the entire first surface was "excellent" was 0.12 × 10 ―6 [mm -1 ] or less, and the arithmetic mean roughness Ra was 1.8 nm or less. For samples with a fine pattern formation ability of "excellent," the value (TTV / S1) was 0.11 × 10 ―6 [mm -1 ] or less, and the arithmetic mean roughness Ra was 0.6 nm or less. In the samples in which the feasibility of forming a fine pattern was "excellent," the feasibility of using the entire first surface was also "excellent," and in this case, the TTV was 17.9 μm or less, and the maximum peak height Rp was 45.6 nm or less. In the case of sample 18, since the silicon substrate is thin, warping occurs in the silicon substrate during transportation, which is not preferable. In addition, the thickness of the silicon substrate in Sample 19 makes it heavy and difficult to transport. Furthermore, packaging it as an interposer undesirably increases the thickness of the entire chip. Sample 20 has a large TTV (thickness variation of the silicon substrate), and Sample 21 has a large maximum peak height Rp of 104.3 nm, resulting in a rough first surface, making it impossible to form a fine wiring pattern. In Sample 22, the silicon substrate is circular, so the peripheral area cannot be used for circuit formation. In Sample 23, unlike the manufacturing method of the present invention, a polishing step was not performed, and therefore the first surface was formed roughly, making it difficult to form a fine wiring pattern. In Sample 24, the TTV (thickness variation of the silicon substrate) was large, and it was not possible to form a fine wiring pattern. It is believed that the etching process caused a difference in the amount of etching between the grain boundaries on the first surface and other areas, which resulted in a large TTV. [Explanation of symbols]

[0056] 1,1A Square Silicon Substrate 11 First edge 12 Second edge 13 Corner 15 Notch 110 Front page 120 Second side 130 Outer edge 200 Fixed Plate 210 Placement surface

Claims

1. The thickness is 0.5 mm or more and 2.0 mm or less, The total thickness variation (hereinafter referred to as TTV) in the first surface for forming a circuit is 100.0 μm or less, The rectangular silicon substrate further characterized in that the first surface has a maximum peak height Rp of 100.0 nm or less.

2. 2. The rectangular silicon substrate according to claim 1, which is made of polycrystalline silicon.

3. TTV is the area of ​​the first surface (S1 [mm 2 ]) (TTV / S1) is 1.00 x 10 ―6 [mm -1 2. The rectangular silicon substrate according to claim 1, wherein the surface roughness of the rectangular silicon substrate is equal to or less than 1 mm.

4. 2. The rectangular silicon substrate according to claim 1, wherein the first surface has an arithmetic mean roughness Ra of 2.0 nm or less.

5. A method for manufacturing a rectangular silicon substrate having a first surface for forming a circuit and a second surface opposite to the first surface, comprising the steps of: a slicing step of slicing the silicon ingot to form a rectangular plate-shaped member; a grinding step of grinding both surfaces of the plate-like member; a polishing step of mechanically polishing one surface of the plate-like member that has been subjected to the grinding step to form the square silicon substrate having the first surface; a polishing step, and a step between the grinding step and the polishing step, wherein chemical etching is not performed, and the square silicon substrate is formed to a thickness of 0.5 mm or more and 2.0 mm or less.

6. 6. The method for producing a square silicon substrate according to claim 5, wherein the polishing step uses a finishing slurry made of finishing abrasive grains and a liquid having a hydrogen ion exponent of 7.0 or more and 9.0 or less.

Citation Information

Patent Citations

  • Inspecting apparatus of coated hoop form materials

    JP1979001683A

  • Crystal silicon wafer, method of manufacturing the same crystal silicon solar cell, and method of manufacturing the same

    JP2006202831A

  • Silicon ingot, silicon wafer, solar cell, and silicon part

    JP2015006990A

  • Silicon member and method for manufacturing silicon member

    JP2017208571A