Method for manufacturing color steel plate
A three-component urethane paint system with polyol, polyisocyanate, and organosilicate forms a stable and hydrophilic cured coating on colored steel sheets, addressing the instability issues of one-component urethane paints and maintaining coating quality over time.
Patent Information
- Application Number
- JP2023061509
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-05
- Publication Date
- 2024-10-18
AI Technical Summary
Existing colored steel sheets face issues with poor hydrophilicity and stability due to the interaction between tin catalysts in one-component urethane paint and organosilicates, leading to instability in the coating film.
A three-component urethane paint system is developed, comprising polyol, polyisocyanate, and organosilicate, which is applied and baked to form a cured coating film, avoiding the use of tin catalysts to enhance hydrophilicity and stability.
The method stabilizes the production of colored steel sheets with excellent hydrophilicity, ensuring good curability, processability, and minimal color and gloss changes, even after prolonged mixing times.
Smart Images

Figure 2024148411000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a color steel sheet. [Background technology]
[0002] The color steel sheet generally means a steel sheet having a coating film formed on the surface thereof, and is also called a painted steel sheet. Note that the color steel sheet in the present invention also includes a steel sheet having a coating film that does not contain either a pigment or a dye formed on the surface thereof.
[0003] In industrial production lines for colored steel sheets, colored steel sheets are generally produced by applying a paint to a steel sheet using a roll coater to form an uncured coating film, and then baking the uncured coating film in a heating furnace to form a cured coating film. In such industrial production lines, a one-component urethane paint (i.e., a paint containing a polyol and a blocked polyisocyanate) as described in Patent Document 1 has conventionally been used to form the cured coating film. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2002-179998 A Summary of the Invention [Problem to be solved by the invention]
[0005] For example, in the field of building materials, etc., there is a demand for color steel sheets with excellent anti-staining properties. As a means for improving the anti-staining properties of color steel sheets, it is known to improve the hydrophilicity of the coating film on the surface thereof so as to remove dirt that has adhered to the coating film due to rain or the like.
[0006] For example, it is known that organosilicates and / or condensates thereof are added to polyester-melamine paints to improve the hydrophilicity of the coating film obtained from the paints. However, the tin catalyst contained in one-component urethane paints acts on the organosilicates and / or condensates thereof, and therefore the urethane paints obtained by adding silicates to one-component urethane paints are inferior in stability as shown in Comparative Example 1 described later, and it is difficult to stably manufacture color steel sheets using the urethane paints.
[0007] The present invention has been made in light of the above-mentioned circumstances, and an object of the present invention is to provide a method for stably producing a color steel sheet having a cured coating film with excellent hydrophilicity by using a combination of a urethane coating material and an organosilicate and / or a condensate thereof. [Means for solving the problem]
[0008] The present invention capable of achieving the above object is as follows. [1] Component (A) containing a polyol; Component (B) containing a polyisocyanate; Formula (I):
[0009] [ka]
[0010] (In the above formula, R 1 ~R 4 each independently represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms. and (C) a component containing an organosilicate represented by the formula: (1) applying the resulting three-liquid urethane paint to a steel plate to form an uncured coating film; Step (2) of baking the uncured coating film to form a cured coating film. A method for producing a color steel sheet, comprising: [2] In step (1), Using a three-liquid mixing device, the component (A), the component (B), and the component (C) are mixed to prepare the three-liquid urethane coating material; The obtained three-liquid urethane coating material is supplied to a roll coater, The three-component urethane paint is applied to the steel plate using the roll coater. The method according to [1] above. [3] The method according to [1] or [2], wherein the baking of the uncured coating film in step (2) is carried out using a heating furnace, the atmospheric temperature of the heating furnace being 150 to 250°C, and the baking time being 20 to 80 seconds. Effect of the Invention
[0011] According to the present invention, a color steel sheet having a cured coating film with excellent hydrophilicity can be stably produced by using a combination of a urethane coating material and an organosilicate and / or a condensate thereof. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 shows a schematic cross-sectional view of a roll coater that can be used in one embodiment of the present invention. [Diagram 2] FIG. 2 shows a schematic cross-sectional view of a roll coater that can be used in another embodiment of the present invention. [Diagram 3] FIG. 3 shows a schematic cross-sectional view of a roll coater that can be used in another embodiment of the present invention. [Figure 4] FIG. 4 shows a schematic cross-sectional view of a roll coater that can be used in another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present invention is characterized in that a cured coating film is formed using a three-liquid urethane paint obtained by mixing component (A) containing a polyol, component (B) containing a polyisocyanate, and component (C) containing an organosilicate represented by the above formula (I) (hereinafter sometimes abbreviated as "organosilicate (I)") and / or its condensate.
[0014] In this specification, the term "three-component urethane paint" refers to a paint that is composed of component (A) containing a polyol, component (B) containing a polyisocyanate, and component (C) containing an organosilicate (I) and / or its condensate, and that is mixed together before application. On the other hand, the term "one-component urethane paint" refers to a paint that contains a polyol and a blocked polyisocyanate.
[0015] In this specification, "polyisocyanate" without the restriction of "blocked" means a polyisocyanate in which the isocyanate group (also called "isocyanato group") is not blocked with a blocking agent, while "blocked polyisocyanate" means a polyisocyanate in which the isocyanate group is blocked with a blocking agent.
[0016] Three-component urethane paints that use polyisocyanates are more reactive than one-component urethane paints that contain blocked polyisocyanates, and can form cured coatings that have sufficient performance even at low baking temperatures.
[0017] The cured coating film formed by the production method of the present invention may be any of a top coat, a primer layer or a back coat, but is preferably a top coat.
[0018] In this specification, the term "top coat" refers to a coating film that has properties for use as a building material, etc., and is formed on the outermost surface of a steel sheet. Examples of building materials include roofing materials and wall materials. In this specification, the term "primer layer" refers to a coating film for ensuring adhesion between the steel sheet and the top coat, or for ensuring the performance of the color steel sheet (for example, corrosion resistance, workability, etc.). In this specification, the term "reverse side coating" refers to a coating film formed on the surface (reverse side) opposite to the surface (front side) of a color steel sheet on which a top coat is formed.
[0019] The (A) component of the three-liquid polyurethane coating contains a polyol. Only one type of polyol may be used, or two or more types may be used in combination. Examples of polyols include polyester polyols, polyether polyols, silicone-modified polyester polyols, and fluorine-based polyols. From the viewpoint of weather resistance or processability, the polyol contained in the (A) component is preferably a polyester polyol.
[0020] Examples of carboxylic acids for forming polyester polyols include succinic acid, adipic acid, sebacic acid, dimer acid, maleic anhydride, phthalic anhydride, isophthalic acid, terephthalic acid, etc., and among these, adipic acid, phthalic anhydride, and isophthalic acid are preferred. To form polyester polyols, only one type of carboxylic acid may be used, or two or more types may be used in combination.
[0021] Examples of alcohols for forming polyester polyols include ethylene glycol, propylene glycol, diethylene glycol, neopentyl glycol, trimethylolpropane, pentaerythritol, 1,6-hexanediol, glycerin, etc., and among these, neopentyl glycol, trimethylolpropane, pentaerythritol, and 1,6-hexanediol are preferred. To form polyester polyols, only one type of alcohol may be used, or two or more types may be used in combination.
[0022] As the polyester polyol, polycaprolactone polyol obtained by ring-opening polymerization of ε-caprolactone using a polyhydric alcohol can also be used.
[0023] From the viewpoint of the viscosity of the coating material or the coating workability, the number average molecular weight of the polyester polyol is preferably 2,500 to 7,000, and more preferably 3,000 to 5,000. This number average molecular weight can be measured by GPC (gel permeation chromatography).
[0024] The polyester polyol is often added to component (A) in the form of a solution. From the viewpoint of reactivity or water resistance, the hydroxyl value of the polyester polyol solution is preferably 30 to 120 (mgKOH / g), more preferably 50 to 100 (mgKOH / g).
[0025] The (A) component of the three-liquid polyurethane coating usually contains a solvent in addition to the polyol. Examples of the solvent include xylol, aromatic hydrocarbons, cyclohexanone, isophorone, etc. The solvent may be used alone or in combination of two or more.
[0026] From the viewpoint of the viscosity of the coating material or coating workability, the solid content of component (A) is preferably 30 to 80% by weight, and more preferably 40 to 70% by weight, based on the total weight of component (A).
[0027] The (A) component of the three-liquid polyurethane coating may contain other components in addition to the polyol and the solvent. Examples of other components contained in the (A) component include pigments, aggregates, matting agents, defoamers, surface conditioners, scratch prevention agents, curing catalysts (excluding tin catalysts), and curing inhibitors.
[0028] In order to promote the urethane reaction between the polyol and the polyisocyanate, the (A) component of the three-liquid polyurethane coating preferably contains a curing catalyst (excluding tin catalysts). As the curing catalyst, an aluminum catalyst is preferable, and aluminum bis(ethylacetoacetate) monoacetylacetonate is more preferable. An example of a commercially available curing catalyst is "K-KAT5218" manufactured by King Industries, Inc. Here, "tin catalyst" means a catalyst containing a tin atom, and "aluminum catalyst" means a catalyst containing an aluminum atom.
[0029] In order to extend the pot life after mixing the components (A), (B), and (C), the component (A) of the three-component polyurethane coating preferably contains a curing inhibitor, such as acetylacetone.
[0030] In order to simultaneously promote the urethanization reaction and extend the pot life after mixing of components (A), (B), and (C), it is preferred that component (A) of the three-component polyurethane coating contains a combination of aluminum bis(ethylacetoacetate) monoacetylacetonate (e.g., "K-KAT5218" manufactured by King Industries, Inc.) and acetylacetone.
[0031] The (B) component of the three-liquid polyurethane coating contains a polyisocyanate. The polyisocyanate may be used alone or in combination of two or more. Examples of polyisocyanates include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 2,4'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate, xylylene diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, 1,6-hexamethylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, isophorone diisocyanate, and 1,4-cyclohexane diisocyanate. Among these, 1,6-hexamethylene diisocyanate (HMDI) and isophorone diisocyanate (IPDI) are preferred from the viewpoint of weather resistance or heat yellowing resistance.
[0032] As the polyisocyanate, a modified product of the above-mentioned diisocyanate (e.g., alcohol-modified diisocyanate), a condensate of the above-mentioned diisocyanate (e.g., biuret (dimer), isocyanurate (trimer)), or a modified product of the condensate (e.g., alcohol-modified isocyanurate), or an adduct of the above-mentioned diisocyanate may be used.
[0033] The (B) component of the three-liquid polyurethane coating usually contains a solvent in addition to the polyisocyanate. Examples of the solvent include methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), ethyl acetate, butyl acetate, xylol, etc. The solvent may be used alone or in combination of two or more.
[0034] From the viewpoints of handling and coating workability, the solid content of component (B) is preferably 30 to 80% by weight, more preferably 40 to 70% by weight, based on the total weight of component (B).From the viewpoints of workability and economy, the NCO content of component (B) is preferably 5 to 30% by weight, more preferably 10 to 20% by weight, based on the total weight of component (B).
[0035] The (A) and (B) components of the three-component polyurethane coating are preferably mixed so that the molar ratio of hydroxyl groups in the (A) component to isocyanate groups in the (B) component is within a desired range. The molar ratio of hydroxyl groups in the (A) component to isocyanate groups in the (B) component is preferably 100:70 to 100:130, more preferably 100:80 to 100:120, and most preferably about 100:100.
[0036] The (C) component of the three-liquid polyurethane coating contains an organosilicate represented by the above formula (I) and / or a condensate thereof. In this specification, the term "condensate of organosilicate (I)" includes a hydrolysis condensate of organosilicate (I). In addition, the term "hydrolysis condensate of organosilicate (I)" means a compound obtained by hydrolysis and condensation of organosilicate (I). The organosilicate (I) and its condensate may be used alone or in combination of two or more kinds.
[0037] R in formula (I) 1 ~R 4 each independently represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms. The alkyl group having 1 to 10 carbon atoms may be either linear or branched. Examples of the alkyl group having 1 to 10 carbon atoms include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, an isopentyl group, a neopentyl group, a tert-pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, and a decyl group.
[0038] R in formula (I) 1 ~R 4 are each independently preferably an alkyl group having 1 to 10 carbon atoms, more preferably an alkyl group having 1 to 4 carbon atoms, further preferably a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, or an isobutyl group, and particularly preferably a methyl group or an ethyl group. 1 ~R 4 are preferably the same as each other.
[0039] Examples of the organosilicate (I) include tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, tetraisopropoxysilane, tetrabutoxysilane, and tetraisobutoxysilane.
[0040] The condensate of organosilicate (I) is preferably a dimer to 20-mer. Here, the "condensate of organosilicate (I) which is a dimer to 20-mer" means a condensate formed from 2 to 20 units of organosilicate (I).
[0041] The organosilicate (I) and / or its condensate is preferably at least one selected from the group consisting of tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, tetraisopropoxysilane, tetrabutoxysilane, tetraisobutoxysilane, and hydrolysis condensates thereof, and more preferably a hydrolysis condensate of tetramethoxysilane, a hydrolysis condensate of tetraethoxysilane, or a mixture of a hydrolysis condensate of tetramethoxysilane and a hydrolysis condensate of tetraethoxysilane. The hydrolysis condensate is preferably a dimer to 20-mer. Here, the term "hydrolysis condensate that is a dimer to 20-mer" refers to a hydrolysis condensate formed from 2 to 20 of the tetraalkoxysilane (e.g., tetraethoxysilane).
[0042] The organosilicate (I) and / or its condensate may be one produced by a known method or may be a commercially available product, such as MKC silicate MS51, MS56, MS56S, MS57, MS56SB5, MS58B15, MS58B30, ES40, EMS31, and BTS (all manufactured by Mitsubishi Chemical Corporation, trade names), methyl silicate 51, ethyl silicate 40, ethyl silicate 40T, ethyl silicate 48, and EMS-485 (all manufactured by Colcoat Co., Ltd., trade names).
[0043] The (C) component of the three-liquid polyurethane coating usually contains a solvent in addition to the organosilicate (I) and / or its condensate. Examples of the solvent include xylol, toluene, aromatic hydrocarbons, cyclohexanone, etc. The solvent may be used alone or in combination of two or more.
[0044] From the viewpoint of ease of handling and coating workability, the solid content of component (C) is preferably 10 to 60% by weight, and more preferably 20 to 50% by weight, based on the total weight of component (C).
[0045] The content of the organosilicate (I) and / or its condensate in the three-liquid polyurethane coating material is preferably 0.5 to 10 parts by weight, more preferably 2 to 7 parts by weight, per 100 parts by mass of polyol, from the viewpoint of the expression of hydrophilicity of the coating film and the stability of the coating material when the three liquids are mixed. When both the organosilicate (I) and its condensate are used, the above content is the total content of these.
[0046] Since the tin catalyst acts on the organosilicate (I) and / or its condensate contained in component (C), it can adversely affect the stability of the three-liquid urethane coating after components (A), (B), and (C) are mixed. Therefore, it is preferable that none of components (A), (B), and (C) contain a tin catalyst.
[0047] In step (1) of the manufacturing method of the present invention, a three-liquid urethane coating is applied to a steel plate to form an uncured coating film. In step (1), it is preferable to use a three-liquid mixing device to mix components (A), (B), and (C) to prepare a three-liquid urethane coating, supply the resulting three-liquid urethane coating to a roll coater, and use the roll coater to apply the three-liquid urethane coating to the steel plate.
[0048] In this specification, the term "three-liquid mixing device" refers to a device that can automatically measure and mix liquid A (e.g., the above-mentioned component (A)), liquid B (e.g., the above-mentioned component (B)), and liquid C (e.g., the above-mentioned component (C)). A commercially available product can be used as the three-liquid mixing device. Examples of such commercially available products include 2K Comfort XL type (explosion-proof, three-liquid specification) manufactured by WAGNER.
[0049] The roll coater is preferably a device having a plurality of rolls. Hereinafter, a roll coater that can be used in one embodiment of the present invention will be described with reference to Fig. 1. Note that Fig. 1 is a schematic cross-sectional view, and the ratio of the size between each roll and the ratio of the size of each roll to the thickness of the steel sheet do not match the ratio of an actual device.
[0050] The arrows drawn inside the metering roll 1, the pickup roll 2, the application roll 3 and the backup roll 4 in FIG. 1 indicate the rotation direction of each roll, and the arrow drawn next to the steel plate 6 indicates the movement direction of the steel plate 6.
[0051] In one embodiment of the present invention, as shown in Fig. 1, a three-component urethane paint is supplied from a supply port 5 for the three-component urethane paint between a metering roll 1 and a pickup roll 2. In the roll coater shown in Fig. 1, a backup roll 4 is a roll for supporting a steel plate 6, an application roll 3 is a roll for applying the three-component urethane paint on the roll to the steel plate 6, a pickup roll 2 is a roll for transferring the three-component urethane paint on the roll to the application roll 3, and a metering roll 1 is a roll for adjusting the appearance or thickness of the coating film.
[0052] In Fig. 1, the rolls are in contact with each other. However, Fig. 1 is a schematic cross-sectional view, and in an actual roll coater, for example, a certain amount of space is provided between the metering roll 1 and the pick-up roll 2, which can be easily understood by a person skilled in the art, in order to adjust the coating thickness. In addition, a person skilled in the art can appropriately set the space between the rolls and the number of rotations of each roll according to the required coating thickness or appearance.
[0053] In one embodiment of the present invention, the three-liquid type urethane paint can be applied to a steel sheet using a roll coater having a roll and a supply port for the three-liquid type urethane paint as shown in Figure 1. More specifically, in one embodiment of the present invention, The machine has a metering roll 1, a pickup roll 2, an application roll 3, a backup roll 4, and a supply port 5 for a three-component urethane paint. A metering roll 1 and a pickup roll 2 are adjacent to each other, a pickup roll 2 and an application roll 3 are adjacent to each other, and an application roll 3 and a backup roll 4 are adjacent to each other. A supply port 5 for a three-liquid type urethane paint is provided between the metering roll 1 and the pickup roll 2, and A roll coater is used in which a steel sheet 6 moves between an application roll 3 and a backup roll 4. A three-component urethane paint is supplied between the metering roll 1 and the pickup roll 2 from a supply port 5 of the three-component urethane paint. The three-component urethane paint on the pickup roll 2 is transferred to the application roll 3, and A three-component urethane paint on an application roll 3 can be applied to a steel plate 6 .
[0054] A supply port for supplying the three-component urethane paint to the roll of a roll coater (for example, supply port 5 for the three-component urethane paint in FIG. 1) preferably has multiple slits. By using such a supply port having multiple slits, the three-component urethane paint can be supplied, for example, in the form of a curtain, so that the paint can be supplied uniformly to the roll.
[0055] In the manufacturing method of the present invention, a roll coater equipped with a doctor blade may be used to form a coating film with a more beautiful appearance. For example, a doctor blade 7 may be installed next to the metering roll 1 in the roll coater shown in FIG.
[0056] A roll coater equipped with a doctor blade that can be used in one embodiment of the present invention will be described below with reference to Fig. 2. In Fig. 2, the same reference numerals as in Fig. 1 are used for the same components as in Fig. 1. The arrows in Fig. 2 are the same as those in Fig. 1. Fig. 2 is also a schematic cross-sectional view like Fig. 1, and the ratio of the sizes between the rolls does not match the ratio of the actual device.
[0057] In the roll coater shown in Fig. 2, a doctor blade 7 is adjacent to the metering roll 1. This doctor blade 7 smoothes the appearance of the three-component urethane paint (i.e., the uncured coating film) supplied onto the metering roll 1. Also, as shown in Fig. 2, the three-component urethane paint can be supplied between the doctor blade 7 and the metering roll 1 from a supply port 5 for the three-component urethane paint. More specifically, in one embodiment of the present invention, The apparatus has a metering roll 1, a pickup roll 2, an application roll 3, a backup roll 4, a supply port 5 for a three-liquid urethane paint, and a doctor blade 7. The doctor blade 7 and the metering roll 1 are adjacent to each other, the metering roll 1 and the pickup roll 2 are adjacent to each other, the pickup roll 2 and the application roll 3 are adjacent to each other, and the application roll 3 and the backup roll 4 are adjacent to each other, A supply port 5 for a three-liquid type urethane paint is provided between the doctor blade 7 and the metering roll 1, and A roll coater is used in which a steel sheet 6 moves between an application roll 3 and a backup roll 4. A three-component urethane paint is supplied between the doctor blade 7 and the metering roll 1 from a supply port 5 of the three-component urethane paint. The three-component urethane paint on the pickup roll 2 is transferred to the application roll 3, and A three-component urethane paint on an application roll 3 can be applied to a steel plate 6 .
[0058] In addition, shielding plates may be attached to the sides of the doctor blade 7 and the metering roll 1 to prevent the three-component urethane paint supplied to the doctor blade 7 and the metering roll 1 from overflowing from the sides of these.
[0059] In the manufacturing method of the present invention, a roll coater without a metering roll may be used. Hereinafter, a roll coater without a metering roll used in one embodiment of the present invention will be described with reference to Figs. 3 and 4. In Figs. 3 and 4, the same reference numerals as in Figs. 1 and 2 are used for the same parts as in Figs. 1 and 2. The explanation of the arrows in Figs. 3 and 4 is the same as that of Fig. 1. In addition, Figs. 3 and 4 are schematic cross-sectional views similar to Fig. 1, and the ratio of the size between the rolls does not match the ratio of the actual device.
[0060] In one embodiment of the present invention, as shown in Fig. 3, a roll coater having a paint pan 8 can be used. In more detail, in one embodiment of the present invention, a roll coater having a pickup roll 2, an application roll 3, a backup roll 4, a supply port 5 for a three-liquid type urethane paint, and a paint pan 8 is used. The pickup roll 2 and the application roll 3 are adjacent to each other, and the application roll 3 and the backup roll 4 are adjacent to each other. A supply port 5 for a three-liquid type urethane paint is provided so as to supply the three-liquid type urethane paint to the paint pan 8; and A roll coater is used in which a steel sheet 6 moves between an application roll 3 and a backup roll 4. Three-component urethane paint is supplied from the supply port 5 to the paint pan 8, The three-component urethane paint supplied to the paint pan 8 is picked up onto the pickup roll 2. The three-component urethane paint on the pickup roll 2 is transferred to the application roll 3, and A three-component urethane paint on an application roll 3 can be applied to a steel plate 6 .
[0061] In the manufacturing method of the present invention, a roll coater equipped with a doctor blade may be used to form a coating film with a more beautiful appearance. For example, a doctor blade may be installed next to the pickup roll 2 in the roll coater shown in FIG.
[0062] In one embodiment of the present invention, as shown in Fig. 4, a roll coater can be used in which a doctor blade 7 is provided next to the application 2, and a supply port 5 for the three-liquid urethane paint is provided between the doctor blade 7 and the pickup roll 2. More specifically, in one embodiment of the present invention, The apparatus has a pickup roll 2, an application roll 3, a backup roll 4, a supply port 5 for a three-liquid urethane paint, and a doctor blade 7. The doctor blade 7 and the pickup roll 2 are adjacent to each other, the pickup roll 2 and the application roll 3 are adjacent to each other, and the application roll 3 and the backup roll 4 are adjacent to each other, A supply port 5 for a three-liquid urethane paint is provided between the doctor blade 7 and the pickup roll 2, and A roll coater is used in which a steel sheet 6 moves between an application roll 3 and a backup roll 4. A three-component urethane paint is supplied from a supply port 5 of the three-component urethane paint between the doctor blade 7 and the pickup roll 2, The three-component urethane paint on the pickup roll 2 is transferred to the application roll 3, and A three-component urethane paint on an application roll 3 can be applied to a steel plate 6 .
[0063] In addition, to prevent the three-component urethane paint supplied to the doctor blade 7 and the pickup roll 2 from overflowing from the sides thereof, shielding plates may be attached to the sides of the doctor blade 7 and the metering roll 1.
[0064] It is preferable to apply a three-liquid urethane paint to a steel sheet so that a desired thickness of the cured coating film after drying (after baking) can be obtained. The thickness of the cured coating film formed by the production method of the present invention after drying (after baking) is preferably 5 to 30 μm, more preferably 10 to 25 μm.
[0065] In step (2) of the production method of the present invention, the uncured coating film is baked to form a cured coating film. In industrial production lines for color steel sheets, the baking of the uncured coating film is usually carried out using a heating furnace. The atmospheric temperature of the heating furnace is preferably 150 to 250°C, more preferably 160 to 230°C, and even more preferably 170 to 220°C. The baking time of the uncured coating film is preferably 20 to 80 seconds, more preferably 20 to 70 seconds, and even more preferably 30 to 60 seconds. Here, the "baking time of the uncured coating film" means the time that the uncured coating film stays in the heating furnace.
[0066] The line speed of an industrial production line for color steel sheets (ie, the moving speed of the steel sheets) is usually 30 to 150 m / min, and preferably 50 to 120 m / min.
[0067] After the hardened coating film is formed by baking, the resulting color steel sheet is preferably cooled, more preferably water-cooled. Water cooling can be performed, for example, by using a water shower or mist.
[0068] Examples of steel sheets that can be used in the present invention include cold-rolled steel sheets, hot-dip galvanized steel sheets, electrolytic galvanized steel sheets, aluminum-zinc alloy plated steel sheets, aluminum plated steel sheets, stainless steel sheets, copper plated steel sheets, tin plated steel sheets, etc. The thickness of the steel sheets is preferably 0.1 to 2.0 mm, more preferably 0.25 to 1.6 mm. EXAMPLES
[0069] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following reference examples. Note that "%" and "parts" regarding the amounts of components described below mean "% by weight" and "parts by weight" unless otherwise specified.
[0070] <Comparative Example 1 and Examples 1 to 4> In Comparative Example 1, a comparative urethane paint was prepared by mixing a one-component urethane paint (HD6000 U White (1PC)) and component (C). In Examples 1 to 4, a three-liquid type urethane coating was prepared by mixing component (A) (HD6000 U White (2PC)), component (B), and component (C). In addition, the mixtures in Comparative Example 1 and Examples 1 to 4 were mixed manually, not with a three-liquid mixer, and the resulting coating materials were applied to steel plates using a bar coater, not with a roll coater.
[0071] The steel plate used was a commercially available galvalume steel plate (aluminum-zinc alloy plated steel plate, steel plate thickness: 0.35 mm, Al content in the plate: 55%, Zn content in the plate: 45%, plating weight on both sides: 150 g / m 2 ) was used.
[0072] A primer layer was formed by applying "Precolor Primer HP32" manufactured by Akzo Nobel Coatings Ltd. to the surface of the steel plate and drying it (dry thickness of primer layer: 5 μm). In addition, a back coat (thickness of back coat after drying: 8 μm) was formed by applying "Precolor No. 7000" manufactured by Akzo Nobel Coatings Co., Ltd. to the back surface of the steel sheet and drying it. A comparative urethane paint or a three-liquid type urethane paint was applied to the surface of the steel plate (the surface on which the primer layer was formed) and baked (dried) in the following manner to form a top coat.
[0073] The one-component urethane paint (HD6000 U White (1PC)) and component (A) of the three-component urethane paint (HD6000 U White (2PC)) were both manufactured by Akzo Nobel Coatings Co., Ltd. The following aggregates, matting agents, leveling agents, defoamers, and scratch prevention agents were added to these paints. The following tin catalyst was added to the one-component urethane paint (HD6000 U White (1PC)), and the following aluminum catalyst and curing inhibitor were added to the three-component urethane paint (A) (HD6000 U White (2PC)). The amounts of raw materials used in the one-component urethane paint (HD6000 U White (1PC)) and component (A) of the three-component urethane paint (HD6000 U White (2PC)) are shown in Table 1. The raw materials are as follows: Pigment: Titanium dioxide Polyester polyol solution: Polyol solution manufactured by Akzo Nobel Coating Co., Ltd. (carboxylic acid components constituting the ester: isophthalic acid, phthalic anhydride, and adipic acid; alcohol components constituting the ester: neopentyl glycol, trimethylolpropane, pentaerythritol, and 1,6-hexanediol; number average molecular weight of polyester polyol: 4,000; hydroxyl value of polyester polyol: 50 (mgKOH / g); solvent: cyclohexanone, xylol, aromatic hydrocarbons), Blocked polyisocyanate: Asahi Kasei Corporation's "Duranate TPA-B 80E" (HMDI isocyanurate type) Aggregate: Sekisui Plastics Co., Ltd. “Techpolymer MBX-30” Matting agent: "SYLYSIA 310P" manufactured by Fuji Silysia Chemical Ltd. Antifoaming agent: "Miki Leveling MK Concentrate" manufactured by Kyoeisha Chemical Co., Ltd. Scratch prevention agent: Kitamura Co., Ltd. "PTFE wax KTL-8N" Diluents (=solvents): cyclohexanone, xylol, aromatic hydrocarbons Tin catalyst: "Neostan U-100" (dibutyltin dilaurate) manufactured by Nitto Kasei Co., Ltd. Aluminum catalyst: "K-KAT5218" (aluminum bis(ethylacetoacetate) monoacetylacetonate) manufactured by King Industries, Inc. Curing inhibitor: Acetylacetone
[0074] The (B) component of the three-component urethane paint (1,6-hexamethylene diisocyanate (HMDI)-based hardener or isophorone diisocyanate (IPDI)-based hardener) was obtained from Akzo Nobel Coatings Co., Ltd. The solids content and NCO content of these (B) components (hardeners) are shown in Table 2.
[0075] The following organosilicates (I) and / or condensates thereof, which are component (C) of the three-liquid urethane coating, were used: "Ethyl Silicate 48" (manufactured by Colcoat Co., Ltd.) "EMS-485" (manufactured by Colcoat Co., Ltd.) A xylol solution of the organosilicate (I) and / or its condensate was used as component (C) (solid content of component (C)=concentration of organosilicate (I) and / or its condensate=37%).
[0076] In Examples 1 to 4, three-liquid type urethane coatings were prepared by manually mixing components (A), (B), and (C) in the amounts shown in Table 3. Specifically, components (A) and (B) were mixed in the amounts shown in Table 3 so that the molar ratio of hydroxy groups in component (A) to isocyanate groups in component (B) was 100:100. The content of organosilicate (I) and / or its condensate in the three-liquid type urethane coatings of Examples 1 to 4 was 5 parts per 100 parts of polyol.
[0077] <Paint application and baking> The comparative urethane paint or the three-liquid type urethane paint was applied to the steel plate using a bar coater so that the thickness of the cured coating film (top coat) after drying (after baking) would be 18 μm, and the cured coating film was formed by baking for 55 seconds under the conditions shown in Table 3 using an automatic discharge type dryer manufactured by Tojo Netsugaku Co., Ltd., to produce a colored steel plate. Note that the three-liquid type urethane paint using polyisocyanate has higher reactivity than the one-liquid type urethane paint containing a blocked polyisocyanate, and can form a cured coating film with sufficient performance even at a low baking temperature. Therefore, as shown in Table 3, in Examples 1 to 4, baking was performed at an atmospheric temperature lower than that of Comparative Example 1.
[0078] <Characteristics evaluation of color steel sheets> The properties of the obtained color steel sheet were evaluated as follows. The evaluation results are shown in Table 4.
[0079] (1) Curability A rubbing test was carried out using a rubbing tester (solvent: MEK, load: 1 kg), and the curability was evaluated according to the following criteria. (standard) ○: The primer layer was not exposed after 100 round trips ×: The primer layer was exposed after less than 100 reciprocations.
[0080] (2) Processability The obtained color steel sheet was folded in a T shape with the cured coating facing up and pressed with a press, after which a cellophane tape bending test was carried out on the folded part and the workability was evaluated according to the following criteria. (standard) ◯: The cured coating film did not peel off at all ×: The cured coating film peeled off.
[0081] (3) Blocking property Two color steel sheets were stacked so that their front surface (i.e., the surface on which the top coat was formed) and back surface (i.e., the surface on which the back coat was formed) were in contact with each other, and the resulting laminate was applied with a load of 40 kg / cm2 to the cured coating at 40°C. 2The laminate was pressed using a hot press so that a load of 1000 g was applied, and the pressurized state was maintained for 24 hours. After that, the pressurization was stopped and the laminate was cooled to room temperature, and then the blocking property was evaluated according to the following criteria. (standard) 〇: Two color steel sheets peeled off without any problems ×: The two color steel sheets were tightly attached and difficult to peel off.
[0082] (4) Color difference (ΔE) Immediately after mixing and stirring each component of the comparative urethane paint or the three-liquid type urethane paint, the paint was applied and baked as described in <Paint application and baking> to produce a colored steel plate. The colored steel plate thus obtained was used as a reference plate. After that, the comparative urethane paint or the three-liquid type urethane paint was additionally stirred for 1 hour, 2 hours, or 3 hours under the condition that the stirring blade speed of the stirrer was 500 revolutions / minute, and then the paint was applied and baked as described in <Paint application and baking> to produce a colored steel plate. The colored steel plate thus obtained was used as a test plate. The color difference (ΔE) of the obtained reference plate and test plate was measured according to the JIS Z 8722:2009 color measurement method using a spectrophotometer CM-M6 manufactured by Konica Minolta, Inc., and evaluated according to the following criteria. (standard) ○: ΔE is less than 0.3 ×: ΔE is 0.3 or more
[0083] (5) Gloss change rate Immediately after mixing and stirring each component of the comparative urethane paint or the three-liquid type urethane paint, the paint was applied and baked as described in <Application of paint and baking> to produce a colored steel plate. The colored steel plate thus obtained was used as a reference plate. Thereafter, the comparative urethane paint or the three-liquid type urethane paint was additionally stirred for 1 hour, 2 hours, or 3 hours under the condition that the stirring blade speed of the stirrer was 500 revolutions / minute, and then the paint was applied and baked as described in <Application of paint and baking> to produce a colored steel plate. The colored steel plate thus obtained was used as a test plate. The gloss values of the obtained reference plate and test plate were measured using VG7000 manufactured by Nippon Denshoku Kogyo Co., Ltd. Then, the following formula: Gloss change rate (%) = 100 x (gloss value of reference plate - gloss value of test plate) / gloss value of test plate The gloss change rate was calculated from the above and evaluated according to the following criteria. (standard) ○: Gloss change rate is less than ±10% ×: Gloss change rate is ±10% or more
[0084] (6) Rate of increase in flow time Immediately after mixing and stirring each component of the comparative urethane paint or the three-component urethane paint, the flow time (seconds) of these paints was measured using the flow cup method (hereinafter referred to as "initial flow time") (flow cup: FC#4 as specified in ASTM D1200, temperature: 25°C). The comparative urethane paint or the three-component urethane paint was then stirred for an additional hour, two hours, or three hours under conditions where the stirring blade speed of the stirrer was 500 revolutions per minute. The flow time (seconds) of the paint thus obtained using the flow cup method (hereinafter referred to as "flow time after x hours" (x: 1, 2, or 3)) was measured under the same conditions as the initial flow time. The following formula: Increase rate of flow time (%) = 100 x (initial flow time - flow time after x hours) / initial flow time The rate of increase in flow time was calculated and evaluated according to the following criteria. (standard) ○: The increase in flow time is less than 20% ×: The increase in flow time is 20% or more
[0085] (7) Hydrophilicity of the cured coating film Immediately after mixing and stirring each component of the comparative urethane paint or the three-liquid urethane paint, the paint was applied and baked as described in <Paint application and baking> to produce a colored steel plate. The colored steel plate thus obtained was immersed in 60°C hot water for 30 minutes, and the wettability of the cured coating film was visually confirmed and evaluated according to the following criteria. The comparative urethane paint or the three-liquid urethane paint was then additionally stirred for 1 hour, 2 hours, or 3 hours under conditions where the stirring blade speed of the stirrer was 500 rpm, and the paint was applied and baked as described in <Paint application and baking> to produce a colored steel plate. The colored steel plate thus obtained was immersed in 60°C hot water for 30 minutes, and the wettability of the cured coating film was visually confirmed and evaluated according to the following criteria. (standard) 〇: Sufficient wettability was confirmed ×: Sufficient wettability was not confirmed.
[0086] [Table 1]
[0087] [Table 2]
[0088] [Table 3]
[0089] [Table 4]
[0090] As is clear from the results shown in Table 4, Comparative Example 1, which used a comparative urethane paint (a mixture of one-component urethane paint and component (C)), had no problems with curing, workability, or blocking, but was poor in color difference (ΔE), gloss change rate, viscosity increase rate, and cured coating film hydrophilicity after additional stirring. On the other hand, Examples 1 to 4, which used a three-component urethane paint, had no problems with curing, workability, or blocking, and were good in color difference (ΔE), gloss change rate, flow time increase rate, and cured coating film hydrophilicity after additional stirring. [Industrial Applicability]
[0091] According to the manufacturing method of the present invention, a color steel sheet having a cured coating film with excellent hydrophilicity can be stably manufactured by using a combination of a urethane coating material and an organosilicate (I) and / or a condensate thereof. The color steel sheet obtained by the manufacturing method of the present invention is useful in the field of building materials, etc. [Explanation of symbols]
[0092] 1 Metering Roll 2 Pickup Roll 3 Application Roles 4. Backup Role 5 Supply port for 3-component urethane paint 6 steel plate 7 Doctor Blade 8 Paint Pan
Claims
1. A component (A) containing a polyol; Component (B) containing a polyisocyanate; Formula (I): 【Chemistry 1】 (In the above formula, R 1 ~R 4 each independently represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms. and (C) a component containing an organosilicate represented by the formula: (1) applying the resulting three-liquid urethane coating to a steel plate to form an uncured coating film; and Step (2) of baking the uncured coating film to form a cured coating film. A method for producing a color steel sheet, comprising:
2. In step (1), Using a three-liquid mixing device, the component (A), the component (B), and the component (C) are mixed to prepare the three-liquid urethane paint; The obtained three-liquid urethane coating material is supplied to a roll coater, The three-liquid urethane paint is applied to the steel plate using the roll coater. The method of claim 1.
3. 3. The method according to claim 1 or 2, wherein the baking of the uncured coating film in step (2) is carried out using a heating furnace, the atmospheric temperature of the heating furnace is 150 to 250° C., and the baking time is 20 to 80 seconds.
Citation Information
Patent Citations
Coating composition and coated steel sheet using the same
JP2002179998A