Denitrification method of molten steel
The denitrification treatment using Mg or Ca alloys sprayed onto the surface of molten steel under controlled conditions addresses the high nitrogen issue in electric furnace steelmaking, enhancing denitrification efficiency and reducing refractory erosion.
Patent Information
- Application Number
- JP2023062300
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2024-10-18
AI Technical Summary
The challenge in steelmaking using electric furnaces is the high initial nitrogen concentration due to increased air mixing, which negatively affects the final product properties, necessitating a more efficient denitrification method in secondary refining.
A denitrification treatment method involving spraying a refining agent containing volatile elements like Mg or Ca alloys onto the surface of molten steel under reduced pressure, ensuring a wide coverage area and controlled concentrations of O and S to enhance the reaction interface and mass transfer.
This method effectively reduces nitrogen concentration in molten steel, promoting efficient denitrification while minimizing refractory erosion and maintaining low operational costs.
Smart Images

Figure 2024148825000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for denitrifying molten steel to perform denitrification efficiently. [Background technology]
[0002] Conventionally, vacuum degassing treatment has been performed using equipment such as RH and REDA to remove the impurity gas components carbon, nitrogen, and hydrogen from molten steel. In general, it is effective to increase the reaction interfacial area and promote mass transfer to promote the degassing reaction, and this is achieved by injecting gas into the molten steel to generate bubbles, thereby increasing the gas-liquid interfacial area and strengthening stirring.
[0003] One example of a method for generating bubbles is to increase the amount of bubbles generated by increasing the flow rate of Ar as a reflux gas in an RH-type vacuum degassing apparatus. However, excessively increasing the Ar flow rate to intensify mixing also promotes refractory erosion, so there is a practical upper limit to the flow rate of the reflux gas. In addition, the bubbles generated by blowing are coarse, so the efficiency of increasing the gas-liquid interfacial area is low.
[0004] On the other hand, there is a method in which molten steel with dissolved gas components is placed in a vacuum to create a supersaturated state, generating bubbles from within the molten steel. In this case, bubbles are generated by the gasification reaction, so they are finer than bubbles generated by injecting gas into the molten steel, and this has the advantage of being more efficient in increasing the gas-liquid interfacial area.
[0005] Patent Document 1 discloses a desulfurization and denitrification treatment method capable of sufficiently penetrating refining agent powders such as desulfurization agents and denitrification agents into molten steel under reduced pressure, in which when introducing desulfurization and denitrification powders containing oxides, carbides, fluorides, chlorides, etc. containing alkali metals and alkaline earth metals, the desulfurization and denitrification powders are blown onto the molten steel surface from the top blowing lance using carrier gas at a feed rate in the range of 0.1 to 1 kg / min ton, with the distance between the top blowing lance and the molten steel surface being set to 0.5 to 2 m. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 6-322431 Summary of the Invention [Problem to be solved by the invention]
[0007] In recent years, steelmaking technology using electric furnaces has been widely adopted due to environmental considerations. However, in steelmaking using electric furnaces, there is a tendency for air to get into the furnace, compared to steelmaking using the blast furnace-converter method, which was the mainstream in the past, and the initial nitrogen concentration is likely to be high. Since nitrogen in steel has a negative effect on the properties of the final product, it is necessary to reduce the concentration to an appropriate level, and a more efficient denitrification method in secondary refining is required. The method described in Patent Document 1 is a method for simultaneously performing desulfurization and denitrification, but the conditions are not necessarily suitable when specializing in denitrification.
[0008] In view of the above problems, an object of the present invention is to provide a method for denitrifying molten steel, which is capable of efficiently denitrifying molten steel. [Means for solving the problem]
[0009] The present inventors have studied the difference between the suitable conditions for the desulfurization treatment and the suitable conditions for the denitrification treatment. In the desulfurization treatment of the secondary refining, the desulfurization treatment is performed so that the refining agent is entrained in the molten steel in order to increase the contact interface area between the molten steel and the refining agent. Specifically, the refining agent is dispersed inside the molten steel by injecting the refining agent from an injection lance immersed in the molten steel or from a top blowing lance. On the other hand, in terms of the denitrification reaction, the present inventors have found that in the denitrification treatment using a volatile element, it is more important to increase the reaction interface area and the mass transfer coefficient at the molten steel surface by contacting the refining agent containing a volatile element with the free surface of the molten steel in a vacuum tank than to disperse the refining agent into the inside of the molten steel.
[0010] The present invention is as follows. [1] A method for denitrifying molten steel, comprising the steps of: spraying a refining agent from a top lance under reduced pressure on molten steel having an O concentration of less than 0.0015% by mass and an S concentration of less than 0.0020% by mass in a vacuum degassing apparatus; The refining agent is a powder containing one or more selected from the group consisting of metallic Mg, Mg alloys, metallic Ca, and Ca alloys, A method for denitrification of molten steel, characterized in that when the refining agent is sprayed onto the surface of the molten steel, the refining agent is sprayed onto an area of 50% or more of the surface area of the stationary molten steel in a vacuum vessel. [2] The method for denitrification of molten steel according to the above-mentioned [1], characterized in that a refining agent is sprayed on the molten steel surface in an amount such that the total amount of substance of metallic Mg, metallic Ca, Mg alloys and Ca alloys is 5 mol / t-steel or more and less than 100 mol / t-steel. [3] The method for denitrification of molten steel according to the above [1] or [2], characterized in that the refining agent is sprayed so that the spraying area of the refining agent does not overlap with the wall surface of the vacuum vessel. Effect of the Invention
[0011] According to the present invention, it is possible to provide a method for denitrifying molten steel that can efficiently denitrify molten steel. [Brief description of the drawings]
[0012] [Figure 1] FIG. 13 is a diagram for explaining the range of spraying of the refining agent. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, an embodiment of the present invention will be described in detail. First, the immersion tube of an RH-type vacuum degassing device is immersed in the molten steel in the ladle, and the vacuum chamber is evacuated to reduce the pressure. Then, reflux gas is blown into the molten steel to circulate the molten steel, and the refining agent is blown upward onto the surface of the molten steel together with a carrier gas (an inert gas such as Ar) under reduced pressure (for example, less than 10 kPa), to promote denitrification. Here, as will be described in detail later, the refining agent contains volatile elements, which dissolve in the molten steel and become supersaturated under reduced pressure, generating fine bubbles of the volatile elements. Nitrogen in the molten steel adheres to these fine bubbles, thereby causing denitrification. Note that vacuum degassing devices other than the RH type may also be used.
[0014] It is also known that the interfacial chemical reaction has a large effect on denitrification, and the rate of the interfacial chemical reaction of denitrification can be increased by reducing the surface active elements sulfur and oxygen. In other words, in order to improve the denitrification effect, it is important to keep the O and S concentrations in the molten steel low, in addition to generating fine bubbles. Therefore, as a prerequisite for carrying out the denitrification treatment under the conditions described below, the O concentration in the molten steel is less than 0.0015 mass% and the S concentration is less than 0.0020 mass%. If either of these concentrations does not satisfy the conditions, the rate of the interfacial chemical reaction of denitrification will be low, and the denitrification reaction will not proceed sufficiently.
[0015] Note that, before carrying out the denitriding treatment according to this embodiment, a desulfurization treatment may be carried out in advance to bring the O concentration and S concentration in the molten steel into the above-mentioned conditions. The method of the desulfurization treatment may be a known method and is not particularly limited, but the desulfurization treatment may be carried out in another degassing apparatus before evacuation in the above-mentioned RH-type vacuum degassing apparatus, or the desulfurization treatment may be carried out first by evacuation in the same RH-type vacuum degassing apparatus, and the denitrification treatment may be carried out continuously while still in the evacuation state.
[0016] Next, the detailed conditions of the denitrification treatment will be described. First, the conditions of the refining agent sprayed under reduced pressure will be described.
[0017] [One or more selected from the group consisting of metallic Mg, Mg alloys, metallic Ca, and Ca alloys] As described above, these are components necessary for generating fine bubbles in molten steel. Examples of Mg include Mg-Si alloy, Mg-Ni alloy, Mg-Al alloy, etc. Examples of Ca alloy include FeSiCa alloy, Ca-Si alloy, Ca-Ni alloy, etc. In addition, since metallic Mg and metallic Ca are elements that easily evaporate, the use of Mg alloy or Ca alloy can suppress the decrease in yield due to evaporation. On the other hand, when using Mg alloy or Ca alloy, it is preferable to use them depending on the type of steel to be finally produced. For example, when using Mg-Si alloy as Mg alloy, it is preferable to use it when producing a steel type with a high Si concentration because Si remains in the molten steel.
[0018] [Other ingredients] The refining agent may also contain other components. For example, it may contain CaO to perform a continuous denitrification treatment after the completion of the desulfurization treatment or to prevent resulfurization. In addition, it may contain CaO and Al as calcium aluminate for the purpose of lowering the melting point and promoting slag formation. 2 O 3 Furthermore, fluorite (CaF 2 ).
[0019] [Amount of refining agent sprayed] Next, the amount of refining agent sprayed will be described. The amount of refining agent sprayed is preferably such that the total amount of substance of Mg and Ca in metal Mg, metal Ca, Mg alloy, and Ca alloy is 5 moles / t-steel or more and less than 100 moles / t-steel. If the total amount of substance of Mg and Ca is less than 5 moles / t-steel, the amount of bubbles generated may be insufficient, and the denitrification effect may be insufficient. Also, if the total amount of substance of Mg and Ca is 100 moles / t-steel or more, the denitrification effect will be saturated, and the refining agent will accumulate on the molten steel surface, resulting in unnecessary costs.
[0020] In addition, the unit consumption of the refining agent to be sprayed is preferably set to an amount such that the total amount of substance of the Mg and Ca components falls within the above-mentioned range. When the amount of refining agent to be sprayed is small, in order to ensure the denitrification effect, it is preferable to increase the total ratio of metallic Mg, Mg alloy, metallic Ca, and Ca alloy in the refining agent so that the total amount of substance of the Mg and Ca components falls within the above-mentioned range. For the above reasons, it is preferable that the unit consumption of the refining agent to be sprayed is 1 kg / t-steel or more.
[0021] Even when the amount of refining agent sprayed is increased, it is preferable to lower the total ratio of metallic Mg, Mg alloys, metallic Ca, and Ca alloys in the refining agent so that the total amount of substance of the Mg and Ca contents falls within the above-mentioned range. However, since the refining agent accumulates on the molten steel surface when the amount of refining agent sprayed is increased and the denitrification effect is saturated or reduced, it is preferable to set the unit consumption of the sprayed refining agent to 16 kg / t-steel or less.
[0022] [Particle size of refining agent] As described above, the refining agent is sprayed onto the molten steel surface from the top blowing lance using carrier gas. Therefore, the refining agent is in the form of powder. Although there is no particular restriction on the particle size of the refining agent, if the particle size is too small, the yield will decrease due to scattering, and if the particle size is too large, it will cause clogging of the powder supply path, so it is preferable that the average particle size of the refining agent powder is 0.01 mm or more and 1.5 mm or less.
[0023] [Spraying conditions] Next, the spraying conditions of the refining agent will be described. In the denitrification treatment using volatile elements such as Mg and Ca, it is important to bring the refining agent containing the volatile element into contact with the free surface of the molten steel in the vacuum tank to increase the reaction interface area and the mass transfer coefficient at the molten steel surface. In this embodiment, in order to inject the refining agent from above onto as wide an area as possible of the molten steel surface in the vacuum tank, when the refining agent powder is sprayed onto the molten steel surface using a carrier gas from a top blowing lance, the refining agent powder is sprayed onto 50% or more of the stationary molten steel surface area in the vacuum tank. The gas flow rate of the carrier gas is not particularly limited as long as the refining agent spraying range can be secured to 50% or more of the stationary molten steel surface area as described above, but is preferably 1 Nm 3 / min~5Nm 3 / min is preferable.
[0024] Next, a method for calculating the area of the refining agent spray range will be described with reference to Fig. 1. Fig. 1 is a diagram for explaining the refining agent spray range. As shown in Fig. 1(a), the lance height is H 0 (m) and the half angle of the jet spread is θ (deg), the radius of the refining agent's spray range is the length of OU, so the area of the refining agent's spray range is approximately πH 0 2 tan 2 θ. Here, the lance height H 0 is the distance from the stationary molten steel surface of the molten steel 1 in the vacuum vessel to the nozzle tip of the top blowing lance 2. Furthermore, the jet spread half angle θ is the half angle of gas spread from the nozzle tip. The jet spread half angle θ can be calculated from an empirical formula that uses the flow rate of the carrier gas, the density of the carrier gas, the pressure at the nozzle outlet, and the inner diameter of the nozzle. The jet spread half angle θ can also be calculated by offline numerical flow analysis.
[0025] Figure 1(b) is a diagram for explaining the refining agent blowing range as viewed vertically in the vacuum vessel. When the top blowing lance is oriented vertically to the molten steel surface and is located at the center of the vacuum vessel as viewed vertically, the refining agent blowing range is the area surrounded by a circumference U as shown in Figure 1(b). The size of the refining agent blowing range is determined by the lance height H 0 can be adjusted by changing
[0026] Although the example shown in Figure 1 shows an example of a single-hole nozzle, a top-blowing lance having multiple nozzles on the periphery of the tip may also be used. In this case, the refining agent spray range is the sum of the circles formed by the spray from each nozzle. The refining agent spray range can also be calculated by offline numerical flow analysis. In this way, the size of the refining agent spray range can be adjusted by changing the number and shape of the nozzle at the tip of the top-blowing lance.
[0027] In addition, if the refining agent is sprayed over an excessively wide range, some of the refining agent will collide with the wall of the vacuum vessel, causing the refractory material on the wall of the vacuum vessel to melt and wear, so it is preferable that the refining agent spray range does not overlap with the wall of the vacuum vessel when spraying the refining agent on the molten steel surface. In the example shown in FIG. 1(b), the top blowing lance is located at the center of the vacuum vessel as viewed from the vertical direction, but it does not have to be located at the center of the vacuum vessel as long as the refining agent powder can be sprayed over 50% or more of the surface area of the stationary molten steel in the vacuum vessel. In addition, the top blowing lance does not necessarily have to be oriented perpendicular to the surface of the molten steel, and the refining agent may be sprayed from an oblique direction as long as the refining agent powder can be sprayed over 50% or more of the surface area of the stationary molten steel in the vacuum vessel.
[0028] As described above, when the refining agent powder is sprayed onto the molten steel surface using carrier gas from the top blowing lance, the refining agent powder is sprayed onto 50% or more of the stationary molten steel surface area in the vacuum vessel, thereby increasing the reaction interfacial area and the mass transfer coefficient on the molten steel surface and promoting the denitrification reaction. EXAMPLES
[0029] Next, an embodiment of the present invention will be described, but the conditions in the embodiment are merely an example of conditions adopted to confirm the feasibility and effects of the present invention, and the present invention is not limited to this example of conditions. Various conditions can be adopted in the present invention as long as they do not deviate from the gist of the present invention and achieve the object of the present invention.
[0030] A ladle containing 100 tons of molten steel was transported under an RH-type vacuum degassing apparatus, the immersion tube was immersed in the molten steel, and the vacuum chamber was depressurized to 133 Pa. Then, reflux gas was blown into the molten steel to circulate it, and the refining agent shown in Table 1 was blown onto the molten steel surface in the vacuum chamber together with carrier gas from a top blowing lance installed in the vacuum chamber, and desulfurization was performed until the pre-treatment [S] concentration value shown in Table 1 was reached. The inner radius of the vacuum chamber was 0.5 m, and the top blowing lance was a straight single-hole nozzle with an inner diameter of 10 cm. The refining agent was a powder with an average particle size of 0.15 to 0.75 mm, and Ar gas was used as the carrier gas.
[0031] The molten steel after desulfurization was sampled to determine the concentration of each component in the molten steel. The C concentration in the molten steel after desulfurization (before denitrification) was 0.05 mass%, the Si concentration was 0.2 mass%, the Mn concentration was 0.25 mass%, the P concentration was 0.02 mass%, the Al concentration was 0.15 mass%, and the N concentration was 0.006 mass%. The O concentration was the value shown in the [O] concentration before treatment in Table 1.
[0032] Next, while the vacuum chamber was being evacuated, the height of the top blowing lance was adjusted so that the powder spray area ratio (the ratio of the powder (refining agent) sprayed area to the stationary molten steel surface area in the vacuum chamber) was the value shown in Table 1, and the same refining agent shown in Table 1 was sprayed onto the molten steel surface in the vacuum chamber. The flow rate of the carrier gas at this time was 2.5 Nm 3 The powder injection rate was set to 5 kg / t-steel per minute, the refining agent injection time was 2 minutes, and the powder consumption rate was 5 kg / t-steel. 0 and the jet divergence half angle θ.
[0033] After the denitrification treatment, the molten steel was sampled to measure the N concentration in the molten steel, and the state of the refractory in the slag line on the inner wall of the vacuum vessel was also observed. Those in which the N concentration after treatment was 0.0020 mass% or less and the refractory wear rate was 0.5 mm / ch or less were evaluated as ⊚, and those in which the N concentration after treatment was 0.0020 mass% or less but the refractory wear rate was more than 0.5 mm / ch were evaluated as ◯. Those in which the N concentration after treatment was more than 0.0020 mass% were evaluated as x.
[0034] [Table 1]
[0035] The underlines in the table indicate conditions outside the scope of the present invention. In Examples 1 to 6 of the present invention, denitrification was good and the target composition was achieved. In addition, the rate of corrosion of the vacuum vessel refractory was slow, and there were no problems with repair time or cost. In Example 7, the refining agent was sprayed to a height of 200 mm from the stationary molten steel surface on the side wall of the vacuum vessel, so that the corrosion of the refractory was large, but the denitrification effect was at a high level.
[0036] On the other hand, in Comparative Example 8, only CaO powder was used as the refining agent, and Mg and Ca, which generate volatile gases, were not included, so the denitrification effect was low and the N concentration after treatment was high. In Comparative Example 9, the spray area ratio was small at 46%, so the denitrification effect was low and the nitrogen concentration after treatment was high. In Comparative Example 10, the O concentration in the molten steel before treatment was high at 0.0016 mass%, so the denitrification rate was slow and the N concentration after treatment was high. In Comparative Example 11, the S concentration in the molten steel before treatment was high at 0.0021 mass%, so the denitrification rate was slow and the N concentration after treatment was high. [Explanation of symbols]
[0037] 1. Molten Steel 2 Top blowing lance
Claims
1. A method for denitrifying molten steel, comprising the steps of: spraying a refining agent from a top blowing lance under reduced pressure on molten steel having an O concentration of less than 0.0015% by mass and an S concentration of less than 0.0020% by mass in a vacuum degassing apparatus; The refining agent is a powder containing one or more selected from the group consisting of metallic Mg, Mg alloys, metallic Ca, and Ca alloys, A method for denitrification of molten steel, characterized in that when the refining agent is sprayed onto the surface of the molten steel, the refining agent is sprayed onto an area of 50% or more of the surface area of the stationary molten steel in the vacuum vessel.
2. The method for denitrification of molten steel according to claim 1, characterized in that a refining agent is sprayed onto the surface of the molten steel in an amount such that the sum of the amounts of Mg and Ca in metallic Mg, metallic Ca, Mg alloys and Ca alloys is 5 mol / t-steel or more and less than 100 mol / t-steel.
3. 3. The method for denitrification of molten steel according to claim 1, wherein the refining agent is sprayed so that the spraying area of the refining agent does not overlap with the wall surface of the vacuum vessel.
Citation Information
Patent Citations
Method for desulfurizing and denitriding molten steel
JP1994322431A