Electrostatic charge image development toner, manufacturing method of electrostatic charge image development toner, and image formation method

A core-shell toner with specific ester waxes addresses the challenges of heat-resistant storage, low-temperature fixing, and fold-fixing properties while reducing wax contamination by ensuring uniform wax distribution and compatibility, enhancing stability and fixability.

JP2024149049AInactive Publication Date: 2024-10-18KONICA MINOLTA INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023062713
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-07
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing toners for developing electrostatic images face challenges in achieving excellent heat-resistant storage properties, low-temperature fixing properties, and fold-fixing properties while suppressing wax contamination in image forming apparatuses, as previous methods using multiple types of waxes result in non-uniform shell formation and wax precipitation.

Method used

A core-shell type toner with a specific coverage rate of the shell part, containing at least two types of ester waxes with different melting points and crystallization temperatures, where the melting point of one ester wax is lower than the other and the crystallization temperature is above 65°C, ensuring compatibility and effective wax distribution.

Benefits of technology

The solution provides a toner with enhanced heat-resistant storage stability, low-temperature fixability, and improved fold-fixing ability while minimizing wax contamination in image forming apparatuses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149049000009
    Figure 2024149049000009
  • Figure 2024149049000001
    Figure 2024149049000001
  • Figure 2024149049000002
    Figure 2024149049000002
Patent Text Reader

Abstract

To provide electrostatic charge image development toner that is excellent in heat-resistant storage property, low-temperature fixation property, and folding fixation property and that can suppress contamination by wax in an image formation apparatus, a manufacturing method of the same, and an image formation method.SOLUTION: Electrostatic charge image development toner includes core-shell type toner base particles containing at least a binder resin and a release agent. The binder resin contains a styrene-acrylic resin. A shell part covers the surface of the core particles with a coverage rate in a range of 60-99%. and 90 mass% or more of the release agent is an ester wax. The ester wax contains at least two types of release agent A and release agent B. When the melting points of the release agent A and the release agent B are represented as Ta and Tb, respectively, the following formula (1) is satisfied, and when the crystallization temperature of the release agent B is represented as Tc, the following formula (2) is satisfied. The formula (1): Ta<Tb. The formula (2): 65°C≤Tc.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a toner for developing an electrostatic image, a method for producing the toner for developing an electrostatic image, and an image forming method. The present invention particularly relates to a toner for developing electrostatic images which is excellent in heat-resistant storage property, low-temperature fixing property and folding fixing property, and which can suppress contamination of the inside of an image forming apparatus by wax. [Background technology]

[0002] In recent years, there has been a demand for reducing the amount of thermal energy used when fixing a toner image in order to meet the needs of higher printing speeds, a wider range of paper types, and reduced environmental impact. One example of a means for reducing the thermal energy is to use a plurality of types of wax having excellent melting or releasability. For example, in Patent Document 1, the toner contains two types of ester wax, which provides excellent low-temperature fixing properties, suppresses contamination of the fixing member, and provides image stability. However, the method described in Patent Document 1 forms a non-uniform shell, which causes the ester wax to precipitate on the surface, making it impossible to ensure heat resistance. In Patent Document 2, low-temperature fixability, storage stability, and developability are achieved by incorporating two types of ester waxes and one type of hydrocarbon wax. However, the method described in Patent Document 2 cannot ensure the prevention of contamination inside the image forming apparatus due to the presence of the hydrocarbon wax. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2010-145553 A [Patent Document 2] JP 2017-44980 A Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention has been made in consideration of the above problems and circumstances. The problem to be solved by the present invention is to provide a toner for developing electrostatic images, which has excellent heat-resistant storage properties, low-temperature fixing properties and folding fixing properties, and which can suppress contamination by wax in an image forming apparatus, a method for producing the toner, and an image forming method. [Means for solving the problem]

[0005] In the process of investigating the causes of the above problems in order to solve the above problems, the present inventors have found the importance of satisfying the following a) to c), which allows the toner to have excellent heat-resistant storage properties, low-temperature fixing properties, and folding fixing properties, and prevents wax from contaminating the inside of an image forming apparatus. a) The toner base particles have a core-shell structure, and the coverage rate of the shell is within a specific range. b) 90% or more by weight of the total release agent is ester wax c) The ester wax contains at least two types of release agent A and release agent B, and the melting points of these and the crystallization temperature of release agent B satisfy specific conditions. That is, the above-mentioned problems of the present invention are solved by the following means.

[0006] 1. A toner for developing electrostatic images, comprising core-shell type toner base particles containing at least a binder resin and a release agent, The binder resin contains a styrene-acrylic resin, The surface of the core particle is covered with the shell at a coverage rate of 60 to 99%, 90% by mass or more of the release agent is an ester wax, The ester wax contains at least two types of release agent A and release agent B, When the melting points of the release agent A and the release agent B are Ta and Tb, respectively, the following formula (1) is satisfied, and When the crystallization temperature of the release agent B is Tc, the following (2) is satisfied: 2. A toner for developing electrostatic images. Formula (1): Ta <Tb Formula (2): 65℃≦Tc

[0007] 2. The shell of the toner base particle contains at least one of styrene-acrylic resin and polyester. 2. The toner for developing electrostatic images according to claim 1,

[0008] 3. The content of at least one of the release agent A and the release agent B in the total amount of the release agents is within the range of 5 to 15% by mass. 2. The toner for developing electrostatic images according to claim 1,

[0009] 4. The release agent A has two or more ester groups, The release agent B is an ester wax having a smaller number of ester groups than the release agent A. 2. The toner for developing electrostatic images according to claim 1,

[0010] 5. A toner for developing electrostatic images, comprising core-shell type toner base particles containing at least a binder resin and a release agent, The binder resin contains a styrene-acrylic resin, The surface of the core particle is covered with the shell at a coverage rate of 60 to 99%, 90% by mass or more of the release agent is an ester wax, The ester wax contains at least two types of release agent A and release agent B, When the melting points of the release agent A and the release agent B are Ta and Tb, respectively, the following formula (1) is satisfied: When the crystallization temperature of the release agent B is Tc, the following (2) is satisfied, The content of at least one of the release agent A and the release agent B relative to the total amount of the release agents is within a range of 5 to 15% by mass, and The release agent A has two or more ester groups, The release agent B is an ester wax having a smaller number of ester groups than the release agent A. 2. A toner for developing electrostatic images. Formula (1): Ta <Tb Formula (2): 65℃≦Tc

[0011] 6. A method for producing the toner for developing electrostatic images according to any one of items 1 to 5, comprising the steps of: a step of incorporating a styrene-acrylic resin as a binder resin and coating the surfaces of the core particles with a shell portion so that the coverage rate is within the range of 60 to 99%; and selecting the release agent A and the release agent B so that 90 mass % or more of the release agent is an ester wax, the ester wax contains at least two types of release agent A and release agent B, and the release agent A and the release agent B are selected so that when the melting points of the release agent A and the release agent B are Ta and Tb, respectively, the following formula (1) is satisfied, and when the crystallization temperature of the release agent B is Tc, the following formula (2) is satisfied. 2. A method for producing a toner for developing an electrostatic image, comprising the steps of: Formula (1): Ta <Tb Formula (2): 65℃≦Tc

[0012] 7. An image forming method using a toner for developing an electrostatic image, comprising the steps of: The toner for developing an electrostatic image is the toner for developing an electrostatic image according to any one of items 1 to 5. 1. An image forming method comprising: Effect of the Invention

[0013] According to the above-mentioned means of the present invention, it is possible to provide a toner for developing electrostatic images, which is excellent in heat resistance storage property, low-temperature fixing property and fold fixing property and can suppress contamination by wax inside an image forming apparatus, a method for producing a toner for developing electrostatic images, and an image forming method. Although the mechanism by which the effects of the present invention are manifested or the mechanism by which the effects of the present invention are acted upon has not been clearly understood, it is speculated as follows. By containing two or more ester waxes with different melting points, the release agent A, which is a low melting point ester wax, plasticizes the core resin and reduces the viscosity of the resin, improving the low temperature fixability. In addition, the release agent B, which is a high melting point ester wax, reduces the viscosity of the resin, making it easier for the release agent B to come out of the toner, improving the releasability of the toner. Furthermore, by specifying the crystallization temperature of release agent B as described above, release agent B becomes a crystal nucleus, which can promote the crystallization of release agent A. Furthermore, release agents A and B are compatible with each other to form a single crystal, which suppresses wax contamination inside the image forming apparatus. Furthermore, by specifying the coverage rate of the core particle surface by the shell to be 60 to 99%, it is possible to prevent the ester wax from coming out of the toner during storage, thereby ensuring heat-resistant storage properties. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a schematic diagram showing an example of a cross-sectional structure of a toner base particle according to the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The toner for developing electrostatic images of the present invention is a toner for developing electrostatic images, which comprises core-shell type toner base particles containing at least a binder resin and a release agent, The binder resin contains a styrene-acrylic resin, The surface of the core particle is covered with the shell at a coverage rate of 60 to 99%, 90% by mass or more of the release agent is an ester wax, The ester wax contains at least two types of release agent A and release agent B, When the melting points of the release agent A and the release agent B are Ta and Tb, respectively, the following formula (1) is satisfied, and When the crystallization temperature of the release agent B is Tc, the following (2) is satisfied: It is characterized by: Formula (1): Ta <Tb Formula (2): 65℃≦Tc This feature is a technical feature common to or corresponding to each of the following embodiments.

[0016] In an embodiment of the present invention, the shell portion of the toner base particle preferably contains at least one of styrene-acrylic resin and polyester. When the shell portion contains styrene-acrylic resin, the core particle and the shell portion become more compatible with each other, and the coverage rate of the shell portion can be increased. When the shell portion contains polyester, the core particle and the shell portion become incompatible with each other, and heat-resistant storage stability is improved.

[0017] The content of at least one of the release agent A and the release agent B with respect to the total amount of the release agents is preferably within a range of 5 to 15% by mass. When the content of the release agent A, which is a low melting point ester wax, is within the above range, the effect of low-temperature fixing (plasticization of resin) is improved. When the content of the release agent B, which is a high melting point ester wax, is within the above range, the effect of suppressing wax contamination in the image forming apparatus is improved. Therefore, when the content of both the release agent A and the release agent B are within the above range, it is possible to promote both improvement of low-temperature fixing property and suppression of wax contamination in the image forming apparatus.

[0018] It is preferable that the release agent A has two or more ester groups, and the release agent B is an ester wax having a smaller number of ester groups than the release agent A. When the release agent A has two or more ester groups, the polarity of the release agent A is closer to that of the resin of the core particles, improving low-temperature fixability. When the release agent B has a smaller number of ester groups than the release agent A, the polarity of the release agent B is further away from that of the core particles than that of the release agent A, and therefore the release agent B does not plasticize with the resin of the core particles and functions as a crystal nucleus.

[0019] The toner for developing an electrostatic image according to another embodiment of the present invention is a toner for developing an electrostatic image, comprising core-shell type toner base particles containing at least a binder resin and a release agent, The binder resin contains a styrene-acrylic resin, The surface of the core particle is covered with the shell at a coverage rate of 60 to 99%, 90% by mass or more of the release agent is an ester wax, The ester wax contains at least two types of release agent A and release agent B, When the melting points of the release agent A and the release agent B are Ta and Tb, respectively, the following formula (1) is satisfied: When the crystallization temperature of the release agent B is Tc, the following (2) is satisfied, The content of at least one of the release agent A and the release agent B relative to the total amount of the release agents is within a range of 5 to 15% by mass, and The release agent A has two or more ester groups, The release agent B is an ester wax having a smaller number of ester groups than the release agent A. It is characterized by: Formula (1): Ta <Tb Formula (2): 65℃≦Tc This makes it possible to provide a toner for developing electrostatic images which is excellent in heat resistance storage property, low temperature fixing property and folding fixing property, and which can suppress contamination of the inside of an image forming apparatus by wax.

[0020] The method for producing the toner for developing electrostatic images of the present invention includes the steps of: incorporating a styrene-acrylic resin as a binder resin and coating the surfaces of core particles with a shell portion so that the coverage is within the range of 60 to 99%; and comprising: a step of selecting the release agent such that 90 mass % or more of the release agent is an ester wax, the ester wax contains at least two types of release agent A and release agent B, and the release agent A and the release agent B are selected so that when the melting points of the release agent A and the release agent B are Ta and Tb, respectively, the following formula (1) is satisfied, and when the crystallization temperature of the release agent B is Tc, the following formula (2) is satisfied. Formula (1): Ta <Tb Formula (2): 65℃≦Tc This makes it possible to produce a toner for developing electrostatic images which is excellent in heat resistance storage property, low temperature fixing property and folding fixing property, and which can suppress contamination of the inside of an image forming apparatus by wax.

[0021] The toner for developing electrostatic images of the present invention is suitably used in an image forming method.

[0022] The present invention, its components, and embodiments for carrying out the present invention will be described below. In this application, the symbol "to" is used to mean that the numerical values ​​before and after the symbol "to" are included as lower and upper limits.

[0023] [Outline of the toner for developing electrostatic images of the present invention] The toner for developing electrostatic images of the present invention is a toner for developing electrostatic images comprising core-shell toner base particles containing at least a binder resin and a release agent, the binder resin comprises a styrene-acrylic resin, the surface of the core particle is covered with a shell portion at a coverage rate in the range of 60 to 99%, 90 mass % or more of the release agent is an ester wax, the ester wax comprises at least two types of release agent A and release agent B, and when the melting points of the release agent A and the release agent B are Ta and Tb, respectively, the following formula (1) is satisfied, and when the crystallization temperature of the release agent B is Tc, the following formula (2) is satisfied. Formula (1): Ta <Tb Formula (2): 65℃≦Tc

[0024] Hereinafter, the toner for developing electrostatic images of the present invention will also be simply referred to as "toner". The toner of the present invention includes toner particles having toner base particles and an external additive disposed on the surface of the toner base particles. In this specification, "toner base particles" are those that constitute the base of "toner particles." The "toner base particles" according to the present invention contain at least a binder resin and a release agent (wax). If necessary, the toner base particles may contain other components such as a colorant and a charge control agent. The "toner base particles" are called "toner particles" when an external additive is added. And, "toner" refers to an aggregate of toner particles.

[0025] [Toner base particles] The toner base particles according to the present invention are of a core-shell type having a core particle and a shell portion that covers the core particle, that is, the toner base particles have a core-shell structure. By having the toner base particles have a core-shell structure, the properties such as glass transition point, melting point, hardness, etc. can be changed between the core particle and the shell part, making it possible to design toner particles according to the purpose. For example, the core particles contain a binder resin, a colorant, a release agent, etc., and a shell portion can be formed by aggregating and fusing a resin with a relatively high glass transition point (Tg) to the surface of the core particles with a relatively low glass transition point (Tg). The binder resin constituting the core particles is not particularly limited, but styrene-acrylic resin, amorphous polyester, crystalline polyester, and the like are preferred. The binder resin constituting the shell is not particularly limited, but amorphous polyester, styrene-acrylic resin, and the like are preferred. The content of the binder resin constituting the shell portion is preferably within a range of 5 to 30% by mass in the toner base particles.

[0026] <Core-shell structure> The cross section of the core-shell structure of the toner base particle can be observed by known observation means such as a transmission electron microscope (TEM), a scanning probe microscope (SPM), or a scanning electron microscope (SEM).

[0027] The entire surface of the core particle does not have to be covered with the shell portion, but the coverage of the core particle with the shell portion is within the range of 60 to 99%, more preferably 70% or more, and even more preferably 75% or more. If the coverage is less than 60%, the shell portion cannot cover the surface of the core particle, resulting in poor heat resistance, whereas if the coverage is more than 99%, the components of the core particle are difficult to extract, resulting in poor fixability.

[0028] The coverage of the core particle with the shell portion can be determined by the following method. 1 to 2 mg of toner particles are dyed with ruthenium tetroxide (RuO4). After dyeing, the toner particles are dispersed in a photocurable embedding resin, which is then photocured to form a block. The embedding resin may be, for example, the photocurable resin "D-800" (manufactured by JEOL Ltd.). From the formed block, an ultrathin sample with a thickness of 60 to 100 nm is cut out. Ultra-thin samples are observed under a transmission electron microscope. Twenty toner particles having a cross-sectional diameter within a range of the volume-based median diameter (D50% diameter) ±10% are randomly photographed and used for measurement. In the cross section of the toner base particle, the "interface length between the shell and the embedding resin" and the "perimeter of the toner base particle" are measured. The coverage rate of the core particles by the shell is calculated by the following formula, where A is the "interface length between the shell and the embedding resin" and B is the "circumferential length of the toner base particle." Coverage rate [%] = A / B × 100 The average value of the coverage of the 20 toner base particles is used as the coverage of the core particle in the present invention.

[0029] Fig. 1 shows a schematic diagram of the cross-sectional structure of a toner base particle when photographed with a scanning electron microscope by the above-mentioned method. As shown in Fig. 1, a toner base particle 1 has a core particle 2 and a shell portion 3 that covers the surface of this core particle 2. The shell portion 3 consists of one or more shell regions 31 . The thick solid line represents the interface Ise between the shell and the embedding resin. The thin solid line represents the interface Ice between the core particle and the embedding resin. The dotted line represents the interface Ics between the core particle and the shell. The above A (the length of the interface between the shell and the embedding resin) is the total length of Ise. The above B (the circumference of the toner base particle) is the total length of Ise and Ice.

[0030] The volume-based median diameter (D50% diameter) of the toner particles is determined by the following method. 0.02 g of toner particles are mixed with 20 mL of surfactant solution, and then ultrasonic dispersion is performed for 1 minute to prepare a toner particle dispersion liquid. For the surfactant solution, for example, a neutral detergent containing a surfactant component is diluted 10 times with pure water for the purpose of dispersing the toner particles. The median diameter can be measured using an apparatus in which a Multisizer 3 (Beckman Coulter) is connected to a computer system for data processing. The toner particle dispersion is injected with a pipette into a beaker containing ISOTON II (electrolyte, manufactured by Beckman Coulter) in the sample stand of the device until the measurement concentration falls within the range of 5 to 10%. The measuring machine count is set to 25,000 and the median diameter is measured. The aperture diameter of the Multisizer 3 used is 100 μm. The measurement range of 1 to 30 μm is divided into 256 parts to calculate the frequency, and the particle size with the largest volume cumulative fraction of 50% is defined as the volume-based median size (D50% size).

[0031] The means for setting the coverage rate of the core particles by the shell portion within the range of 60 to 99% is not particularly limited, but examples thereof include adjustments of the amount of the shell portion, the temperature and stirring speed when fusing the shell material, etc. Specifically, the amount of the shell portion is preferably within a range of 5 to 20% by mass relative to the toner base particles. The temperature at which the shell material is fused is preferably within the range of 75 to 85°C. The stirring speed when fusing the shell material is preferably within the range of 200 to 300 rpm.

[0032] [Toner base particles] The core-shell toner base particles of the present invention contain a binder resin and a release agent. The binder resin contains a styrene-acrylic resin. The binder resin is a styrene-acrylic resin, which prevents excessive seepage of the release agent during fixing and suppresses wax adhesion. The binder resin may preferably contain polyester in addition to styrene-acrylic resin. Resins other than polyester may also be used. Such resins are not particularly limited, and known resins may be used, and may be one type or multiple types.

[0033] <Styrene-acrylic resin> The styrene-acrylic resin is formed by addition polymerization of at least a styrene monomer and a (meth)acrylic acid ester monomer. The styrene monomer includes styrene represented by the structural formula CH2=CH-C6H5, as well as styrene derivatives having known side chains or functional groups in the styrene structure.

[0034] ((Meth)acrylic acid ester monomer) The (meth)acrylic acid ester monomer includes acrylic acid esters and methacrylic acid esters represented by CH(Ra)=CHCOORb (Ra represents a hydrogen atom or a methyl group, and Rb represents an alkyl group having 1 to 24 carbon atoms), as well as acrylic acid ester derivatives and methacrylic acid ester derivatives having known side chains or functional groups in the structure of these esters. Examples of the (meth)acrylic acid ester monomer include acrylic acid ester monomers such as methyl acrylate, ethyl acrylate, isopropyl acrylate, n-butyl acrylate, t-butyl acrylate, isobutyl acrylate, n-octyl acrylate, 2-ethylhexyl acrylate, stearyl acrylate, lauryl acrylate, and phenyl acrylate; and methacrylic acid ester monomers such as methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, isopropyl methacrylate, isobutyl methacrylate, t-butyl methacrylate, n-octyl methacrylate, 2-ethylhexyl methacrylate, stearyl methacrylate, lauryl methacrylate, phenyl methacrylate, diethylaminoethyl methacrylate, and dimethylaminoethyl methacrylate.

[0035] In this specification, the term "(meth)acrylic acid ester monomer" is a general term for "acrylic acid ester monomer" and "methacrylic acid ester monomer" and means one or both of them. For example, "methyl (meth)acrylate" means one or both of "methyl acrylate" and "methyl methacrylate".

[0036] The (meth)acrylic acid ester monomer may be one or more kinds. For example, it is possible to form a copolymer using a styrene monomer and two or more kinds of acrylic acid ester monomers, to form a copolymer using a styrene monomer and two or more kinds of methacrylic acid ester monomers, or to form a copolymer using a styrene monomer, an acrylic acid ester monomer, and a methacrylic acid ester monomer in combination.

[0037] (styrene monomer) Examples of styrene monomers include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, p-phenylstyrene, p-ethylstyrene, 2,4-dimethylstyrene, p-tert-butylstyrene, pn-hexylstyrene, pn-octylstyrene, pn-nonylstyrene, pn-decylstyrene, and pn-dodecylstyrene.

[0038] (Preferred composition of styrene-acrylic resin) From the viewpoint of controlling the plasticity of the styrene-acrylic resin, the content of structural units derived from styrene monomers in the styrene-acrylic resin is preferably within a range of 40 to 90 mass%, more preferably within a range of 50 to 85 mass%, even more preferably within a range of 60 to 80 mass%, and even more preferably within a range of 65 to 75 mass%. The content of structural units derived from the (meth)acrylic acid ester monomer in the styrene-acrylic resin is preferably within a range of 10 to 60 mass%, more preferably within a range of 15 to 50 mass%, even more preferably within a range of 20 to 40 mass%, and even more preferably within a range of 15 to 35 mass%.

[0039] (Other monomers) The styrene-acrylic resin may further contain structural units derived from other monomers than the styrene monomer and the (meth)acrylic acid ester monomer. The other monomer is preferably a compound that forms an ester bond with a hydroxy group (-OH) derived from a polyhydric alcohol or a carboxy group (-COOH) derived from a polycarboxylic acid. In other words, the styrene-acrylic resin is preferably a polymer that can be addition polymerized with the styrene monomer and the (meth)acrylic acid ester monomer, and is further polymerized with a compound (amphoteric compound) having a carboxy group or a hydroxy group.

[0040] (Amphoteric Compound) Examples of the amphoteric compound include compounds having a carboxy group, such as acrylic acid, methacrylic acid, maleic acid, itaconic acid, cinnamic acid, fumaric acid, maleic acid monoalkyl esters, and itaconic acid monoalkyl esters, and compounds having a hydroxy group, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and polyethylene glycol mono(meth)acrylate.

[0041] (Preferable content of structural units derived from amphoteric compounds) The content of the constitutional unit derived from the amphoteric compound in the styrene-acrylic resin is preferably within a range of 0.5 to 20% by mass, and more preferably within a range of 5 to 10% by mass. In one embodiment of the present invention, in the styrene-acrylic resin, the total content of the constituent units derived from the styrene monomer, the content of the constituent units derived from the (meth)acrylic acid ester monomer, and the content of the constituent units derived from the amphoteric compound is 100 mass%.

[0042] (Method of synthesis of styrene-acrylic resin) The styrene-acrylic resin can be synthesized by polymerizing monomers using a known oil-soluble or water-soluble polymerization initiator. Examples of the oil-soluble polymerization initiator include azo- or diazo-based polymerization initiators and peroxide-based polymerization initiators.

[0043] (Azo or diazo polymerization initiator) Examples of the azo or diazo polymerization initiator include 2,2'-azobis-(2,4-dimethylvaleronitrile), 2,2'-azobisisobutyronitrile, 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis-4-methoxy-2,4-dimethylvaleronitrile and azobisisobutyronitrile.

[0044] (Peroxide-based polymerization initiator) Examples of the peroxide polymerization initiator include benzoyl peroxide, methyl ethyl ketone peroxide, diisopropyl peroxycarbonate, cumene hydroperoxide, t-butyl hydroperoxide, di-t-butyl peroxide, dicumyl peroxide, 2,4-dichlorobenzoyl peroxide, lauroyl peroxide, 2,2-bis-(4,4-t-butylperoxycyclohexyl)propane, and tris-(t-butylperoxy)triazine.

[0045] (Water-soluble radical polymerization initiator) When synthesizing styrene-acrylic resin particles by emulsion polymerization, a water-soluble radical polymerization initiator can be used as the polymerization initiator. Examples of water-soluble radical polymerization initiators include persulfates such as potassium persulfate and ammonium persulfate, azobisaminodipropane acetate, azobiscyanovaleric acid and its salts, and hydrogen peroxide.

[0046] (Preferable weight average molecular weight of styrene-acrylic resin) From the viewpoint of easy control of the plasticity of the styrene-acrylic resin, the weight average molecular weight (Mw) is preferably within the range of 5,000 to 150,000. Moreover, the weight average molecular weight is more preferably within the range of 10,000 to 70,000, even more preferably within the range of 15,000 to 60,000, even more preferably within the range of 20,000 to 40,000, and even more preferably within the range of 25,000 to 35,000.

[0047] The toner base particles according to the present invention preferably contain at least one of the styrene-acrylic resin and polyester in the shell portion. In the toner base particles according to the present invention, the core particles also preferably contain at least one of the styrene-acrylic resin and polyester.

[0048] <Polyester> The polyester used as the binder resin for the shell portion or the core particles may be either a crystalline polyester or an amorphous polyester, but is preferably an amorphous polyester from the viewpoint of electrostatic chargeability.

[0049] In the present invention, the term "crystalline resin" refers to a resin having a melting point, i.e., a clear endothermic peak during heating, in an endothermic curve obtained by differential scanning calorimetry (DSC). The term "clear endothermic peak" refers to a peak having a half-width of 15°C or less in an endothermic curve obtained when the temperature is increased at a heating rate of 10°C / min. On the other hand, the term "amorphous resin" refers to a resin in which a baseline curve indicating the occurrence of glass transition is observed in an endothermic curve obtained by performing the same differential scanning calorimetry as above, but no clear endothermic peak is observed.

[0050] (Crystalline polyester) The crystalline polyester is a resin exhibiting crystallinity among known polyesters obtained by polycondensation reaction of a divalent or higher carboxylic acid (polycarboxylic acid) or its derivative with a divalent or higher alcohol (polyalcohol) or its derivative.

[0051] The polycarboxylic acid component for forming the crystalline polyester is a compound containing two or more carboxy groups in one molecule.Specific examples include saturated aliphatic dicarboxylic acids such as succinic acid, sebacic acid, and dodecanedioic acid; alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid; aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, and terephthalic acid; trivalent or higher polycarboxylic acids such as trimellitic acid and pyromellitic acid; and anhydrides or alkyl esters having 1 to 3 carbon atoms of these carboxylic acid compounds.As the polycarboxylic acid component for forming the crystalline polyester, it is preferable to use saturated aliphatic dicarboxylic acids.These may be used alone or in combination of two or more.

[0052] The polyhydric alcohol component for forming the crystalline polyester is a compound containing two or more hydroxyl groups in one molecule. Specifically, for example, aliphatic diols such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, neopentyl glycol, and 1,4-butenediol; trihydric or higher polyhydric alcohols such as glycerin, pentaerythritol, trimethylolpropane, and sorbitol; and the like. As the polyhydric alcohol component for forming the crystalline polyester, it is preferable to use an aliphatic diol. These may be used alone or in combination of two or more.

[0053] The method for producing the crystalline polyester is not particularly limited, and the crystalline polyester can be produced by a general polyester polymerization method in which the above-mentioned polyvalent carboxylic acid and polyhydric alcohol are reacted in the presence of a catalyst. As the production method, for example, it is preferable to use a direct polycondensation method or an ester exchange method depending on the type of monomer.

[0054] Also, a linear aliphatic hydroxycarboxylic acid can be used in combination with the polyvalent carboxylic acid and / or polyhydric alcohol. Examples of linear aliphatic hydroxycarboxylic acids for forming crystalline polyesters include 5-hydroxypentanoic acid, 6-hydroxyhexanoic acid, 7-hydroxypentanoic acid, 8-hydroxyoctanoic acid, 9-hydroxynonanoic acid, 10-hydroxydecanoic acid, 12-hydroxydodecanoic acid, 14-hydroxytetradecanoic acid, 16-hydroxyhexadecanoic acid, 18-hydroxyoctadecanoic acid, and lactone compounds cyclized from these hydroxycarboxylic acids, or alkyl esters with alcohols having 1 to 3 carbon atoms. These may be used alone or in combination of two or more.

[0055] Furthermore, when forming the crystalline polyester, it is preferable to use a polyvalent carboxylic acid and a polyhydric alcohol component, since this makes it easy to control the reaction and allows a resin having a desired molecular weight to be obtained.

[0056] Examples of catalysts that can be used in the production of crystalline polyesters include titanium catalysts such as titanium tetraethoxide, titanium tetrapropoxide, titanium tetraisopropoxide, and titanium tetrabutoxide, and tin catalysts such as dibutyltin dichloride, dibutyltin oxide, and diphenyltin oxide.

[0057] The use ratio of the polyvalent carboxylic acid component and the polyhydric alcohol component is preferably such that the equivalent ratio [OH] / [COOH] of the hydroxyl group [OH] of the polyhydric alcohol component to the carboxyl group [COOH] of the polyvalent carboxylic acid component is within the range of 1.5 / 1 to 1 / 1.5, more preferably 1.2 / 1 to 1 / 1.2.

[0058] The acid value of the crystalline polyester is preferably within the range of 5 to 30 mgKOH / g, more preferably 10 to 25 mgKOH / g, and even more preferably 15 to 25 mgKOH / g. This acid value is the mass of potassium hydroxide (KOH) required to neutralize the acid contained in 1 g of a sample, expressed in mg units. The acid value of the resin is measured according to the following procedure in accordance with JIS K0070-1992.

[0059] (Preparation of reagents) Dissolve 1.0 g of phenolphthalein in 90 mL of ethyl alcohol (95% by volume), add ion-exchanged water to make 100 mL, and prepare a phenolphthalein solution. Dissolve 7 g of JIS special grade potassium hydroxide in 5 mL of ion-exchanged water, and add ethyl alcohol (95% by volume) to make 1 liter. Place in an alkali-resistant container to avoid contact with carbon dioxide, leave for 3 days, then filter to prepare a potassium hydroxide solution. Standardization follows the description of JIS K0070-1992.

[0060] (Main Exam) Weigh out 2.0 g of the crushed sample into a 200 mL Erlenmeyer flask, add 100 mL of a toluene / ethanol (toluene:ethanol volume ratio 2:1) mixture, and dissolve for 5 hours. Next, add a few drops of the prepared phenolphthalein solution as an indicator, and titrate with the prepared potassium hydroxide solution. The end point of the titration is when the indicator remains a pale red color for about 30 seconds.

[0061] (Blank test) The same procedure as in the main test described above is carried out, except that no sample is used (i.e., only a mixed solution of toluene / ethanol (toluene:ethanol is 2:1 by volume) is used).

[0062] The titration results of the main test and the blank test are substituted into the following formula (a) to calculate the acid value.

[0063] Equation (a) A = [(CB) × f × 5.6] / S A: Acid value (mgKOH / g) B: Amount of potassium hydroxide solution added during blank test (mL) C: Amount of potassium hydroxide solution added during this test (mL) f: Factor of 0.1 mol / L potassium hydroxide ethanol solution S: mass of sample (g)

[0064] The weight average molecular weight (Mw) of the crystalline polyester is preferably 3000 to 100000 from the viewpoint of reliably achieving both sufficient low-temperature fixability and excellent long-term heat-resistant storage stability. The weight average molecular weight is more preferably 4000 to 50000, and particularly preferably 5000 to 20000. The ratio of the diol component and the dicarboxylic acid component used is preferably 1.5 / 1 to 1 / 1.5, more preferably 1.2 / 1 to 1 / 1.2, in terms of the ratio [OH] / [COOH] of the hydroxyl group equivalent of the diol component to the carboxyl group equivalent of the dicarboxylic acid component.

[0065] (amorphous polyester) Amorphous polyesters are obtained by a polycondensation reaction between a divalent or higher carboxylic acid (polycarboxylic acid) and a divalent or higher alcohol (polyalcohol). There are no particular limitations on the specific amorphous polyester, and any amorphous polyester conventionally known in the art can be used.

[0066] The specific method for producing the amorphous polyester is not particularly limited, and the resin can be produced by polycondensing (esterifying) a polyvalent carboxylic acid and a polyhydric alcohol using a known esterification catalyst.

[0067] The weight average molecular weight (Mw) of the amorphous polyester is not particularly limited, but is, for example, preferably in the range of 5,000 to 100,000, and more preferably in the range of 5,000 to 50,000. When the weight average molecular weight (Mw) is 5,000 or more, the heat-resistant storage stability of the toner can be improved, and when it is 100,000 or less, the low-temperature fixability can be further improved.

[0068] Examples of the polyvalent carboxylic acid and polyhydric alcohol used in the preparation of the amorphous polyester are not particularly limited, but include the following.

[0069] <Polycarboxylic acids> Examples of the carboxylic acids include aromatic carboxylic acids such as terephthalic acid, isophthalic acid, phthalic anhydride, trimellitic anhydride, pyromellitic acid, and naphthalenedicarboxylic acid; aliphatic carboxylic acids such as maleic anhydride, fumaric acid, succinic acid, alkenyl succinic anhydride, and adipic acid; and alicyclic carboxylic acids such as cyclohexanedicarboxylic acid. These polyvalent carboxylic acids may be used alone or in combination of two or more.

[0070] Among these polyvalent carboxylic acids, it is preferable to use aromatic carboxylic acids. In order to obtain a crosslinked or branched structure and to ensure better fixability, it is preferable to use a trivalent or higher carboxylic acid (such as trimellitic acid or its acid anhydride) in combination with a dicarboxylic acid. Examples of trivalent or higher carboxylic acids include 1,2,3-benzenetricarboxylic acid, 1,2,4-benzenetricarboxylic acid, 1,3,5-benzenetricarboxylic acid, 11,2,4-naphthalenetricarboxylic acid, and the like, as well as their anhydrides and lower alkyl esters. These may be used alone or in combination of two or more. Good too.

[0071] <Polyhydric alcohol> Examples of the polyhydric alcohol include aliphatic diols such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, butanediol, hexanediol, neopentyl glycol, and glycerin, alicyclic diols such as cyclohexanediol, cyclohexanedimethanol, and hydrogenated bisphenol A, and aromatic diols such as an ethylene oxide adduct of bisphenol A and a propylene oxide adduct of bisphenol A. These polyhydric alcohols may be used alone or in combination of two or more.

[0072] Among these polyhydric alcohols, aromatic diols and alicyclic diols are preferred, and aromatic diols are more preferred. In order to ensure better fixation, trihydric or higher polyhydric alcohols (glycerin, trimethylolpropane, pentaerythritol) may be used in combination with the diol to form a crosslinked or branched structure.

[0073] In addition, a monocarboxylic acid and / or a monoalcohol may be further added to the polyester obtained by polycondensation of a polyvalent carboxylic acid and a polyhydric alcohol to esterify the hydroxyl group and / or the carboxyl group at the polymerization terminal, thereby adjusting the acid value of the polyester.

[0074] Examples of the monocarboxylic acid include acetic acid, acetic anhydride, benzoic acid, trichloroacetic acid, trifluoroacetic acid, propionic anhydride, etc. Examples of the monoalcohol include methanol, ethanol, propanol, octanol, 2-ethylhexanol, trifluoroethanol, trichloroethanol, hexafluoroisopropanol, phenol, etc.

[0075] The amorphous polyester used in the present invention may be a hybrid amorphous polyester in which a vinyl-based polymer segment composed of a styrene-acrylic polymer or the like and a polyester-based polymer segment composed of an amorphous polyester are bonded via a bireactive monomer.

[0076] The content ratio of the vinyl-based polymerization segment is preferably within a range of 5 to 30% by mass, and more preferably within a range of 10 to 20% by mass, based on the total mass of the hybrid amorphous polyester.

[0077] When the hybrid amorphous polyester contains a vinyl-based polymerization segment in the range of 5 to 30% by mass, the balance between charge retention and charge leakage can be controlled.

[0078] <Release agent> The toner base particles according to the present invention contain a releasing agent. The releasing agent is a component that seeps out from the toner particles during fixing and enhances the fixing and releasing properties of the toner. At least 90% by mass of the release agent is an ester wax. The ester wax contains at least two types of release agent A and release agent B. When the melting points of the release agent A and the release agent B are Ta and Tb, respectively, the following formula (1) is satisfied, and when the crystallization temperature of the release agent B is Tc, the following formula (2) is satisfied. Formula (1): Ta <Tb Formula (2): 65℃≦Tc

[0079] When the ester wax contains three types of release agents, any two of the three types of release agents may satisfy the formulas (1) and (2).

[0080] As the release agent, a hydrocarbon wax may be used in combination with the ester wax (ester wax). Such wax may be a synthetic product, or a commercially available product may be refined and used. The method of purification is to dissolve the wax in n-hexane or heptane, etc. Recrystallization is one method.

[0081] Hydrocarbon wax is not compatible with polyester or styrene-acrylic resin. Therefore, the hydrocarbon wax is easily moved to the outside of the toner particles during fixing, improving the low-temperature fixing property of the toner. In addition, because the hydrocarbon wax has low viscosity, it is localized in minute recesses on the image surface, and is less likely to deteriorate tack resistance.

[0082] The ester wax is easy to exude from the toner particles. In addition, since the ester wax has a polar moiety, after exuding from the toner particles, it can exist in a finely dispersed state in the polyester on the image surface. This contributes to low-temperature fixability.

[0083] The release agent according to the present invention contains at least two kinds of ester waxes. From the viewpoint of releasability and resin plasticization effect, it is necessary that the release agent contains two or more kinds of ester waxes.

[0084] (Wax type) Examples of ester waxes include carnauba wax, montan wax, behenic acid behenate, trimethylolpropane tribehenate, pentaerythritol tetrabehenate, pentaerythritol diacetate dibehenate, glycerin tribehenate, 1,18-octadecanediol distearate, trimellitate tristearyl, and distearyl maleate.

[0085] Examples of the hydrocarbon wax include polyolefin waxes such as polyethylene wax and polypropylene wax, petroleum-derived paraffin wax, microcrystalline wax, and synthetic waxes such as Fischer-Tropsch wax and polyethylene wax.

[0086] (Ester wax content) The toner of the present invention contains 90% by mass or more of ester wax in the total release agent. If the content of ester wax is less than 90% by mass, the crystallization of the wax is not promoted, and wax contamination in the image forming device cannot be suppressed. If the ester wax accounts for 90% by mass or more of the total release agent, the ester waxes are easily compatible or crystallized with each other, and wax contamination in the image forming device can be suppressed.

[0087] (Melting point of ester wax) The melting points of the two types of ester waxes (release agent A: Ta, release agent B: Tb) satisfy formula (1). Formula (1): Ta <Tb

[0088] The low melting point ester wax (release agent A) is compatible with the resin and exerts a plasticizing effect. The high melting point ester wax (release agent B) provides releasability when the viscosity of the resin decreases and acts as a crystal nucleus for the two types of ester wax. If the melting points of release agent A and release agent B are the same, the ester waxes will be mutually soluble and the above-mentioned effects cannot be achieved. For this reason, it is necessary for the two waxes to have a difference in melting point.

[0089] (Crystallization temperature of release agent B) In the toner of the present invention, the crystallization temperature Tc of the release agent B satisfies the following formula (2). If the crystallization temperature Tc of the release agent B is less than 65° C., the crystallization of the release agent B does not proceed. As a result, the function as a crystal nucleus with the release agent A cannot be exerted. Formula (2): 65℃≦Tc

[0090] The release agent A preferably has two or more ester groups. The release agent B is preferably an ester wax having a smaller number of ester groups than the release agent A.

[0091] Examples of the release agent A include distearyl maleate (melting point: 55° C. / crystallization temperature: 50° C.), stearyl sebacate (melting point: 57° C. / crystallization temperature: 51° C.), ethylene glycol stearate (melting point: 69° C. / crystallization temperature: 63° C.), glycerin tribehenate (melting point: 70° C. / crystallization temperature: 65° C.), stearyl stearate (melting point: 71° C. / crystallization temperature: 62° C.), tristearyl trimellitate (melting point: 74° C. / crystallization temperature: 71° C.), 1,18-octadecanediol distearate (melting point: 76° C. / crystallization temperature: 70° C.), and pentaerythritol stearate (melting point: 77° C. / crystallization temperature: 70° C.).

[0092] Examples of the release agent B include behenic acid behenate (melting point: 73°C / crystallization temperature: 65°C), trimethylolpropane tribehenate (melting point: 76°C / crystallization temperature: 70°C), pentaerythritol tetrabehenate (melting point: 82°C / crystallization temperature: 64°C), carnauba wax (melting point: 83°C / crystallization temperature: 77°C), montan wax (melting point: 83°C / crystallization temperature: 80°C), ethylene glycol stearate (melting point: 84°C / crystallization temperature: 75°C), pentaerythritol tetrabehenate (melting point: 84°C / crystallization temperature: 81°C), and pentaerythritol diacetate dibehenate (melting point: 90°C / crystallization temperature: 85°C).

[0093] The content of at least one of the release agent A and the release agent B in the total amount of the release agent is preferably within a range of 5 to 15% by mass, and more preferably within a range of 7 to 13% by mass.

[0094] <Coloring agent> The toner base particles according to the present invention may contain a colorant. As the colorant, known inorganic or organic colorants can be used. As the colorant, carbon black, magnetic powder, various organic or inorganic pigments, dyes, etc. can be used. In particular, it is preferable to use a chromatic pigment. As the inorganic pigment, it is preferable to use a phthalocyanine pigment. The amount of the colorant added is in the range of 1 to 30% by mass, preferably 2 to 20% by mass, based on the toner particles.

[0095] <Charge control agent> The toner base particles according to the present invention may contain a charge control agent. The charge control agent may be a known compound such as a nigrosine dye, a metal salt of naphthenic acid or a higher fatty acid, an alkoxylated amine, a quaternary ammonium salt, an azo metal complex, or a metal salt of salicylic acid. The charge control agent makes it possible to obtain a toner with excellent charging properties. The content of the charge control agent is preferably within a range of usually 0.1 to 5.0 parts by mass with respect to 100 parts by mass of the binder resin.

[0096] <External additives> The toner base particles according to the present invention may have their surfaces treated with an external additive, which can improve the fluidity, chargeability, cleaning properties, etc. Examples of the external additive include inorganic oxide fine particles such as silica fine particles, alumina fine particles, and titanium oxide fine particles, inorganic stearic acid compound fine particles such as aluminum stearate fine particles and zinc stearate fine particles, and inorganic titanic acid compound fine particles such as strontium titanate and zinc titanate, etc. These may be used alone or in combination of two or more.

[0097] From the viewpoint of improving heat-resistant storage stability and environmental stability, it is preferable that these inorganic particles are subjected to a gloss treatment, which is preferably carried out using a silane coupling agent, a titanium coupling agent, a higher fatty acid, a silicone oil, or the like. The amount of the external additive added is preferably within a range of 0.05 to 5 parts by mass, and more preferably within a range of 0.1 to 3 parts by mass, based on 100 parts by mass of the toner base particles. When a plurality of external additives are used, the total amount of the additives is preferably within the above range.

[0098] <Toner particle size> The average particle size of the toner particles according to the present invention is preferably, for example, 3 to 10 μm, more preferably 5 to 8 μm, in terms of the volume-based median diameter. This average particle size can be controlled by the concentration of the coagulant used during production, the amount of organic solvent added, the fusion time, the composition of the binder resin, etc. By having the volume-based median diameter fall within the above range, extremely fine dot images at a 1200 dpi level can be faithfully reproduced.

[0099] The volume-based median diameter of the toner particles is measured and calculated using a measuring device consisting of a "Multisizer 3" (manufactured by Beckman Coulter) connected to a computer system equipped with the data processing software "Software V3.51." Specifically, first, 0.02 g of the measurement sample (toner) is added to 20 mL of surfactant solution (a surfactant solution prepared by diluting, for example, a neutral detergent containing a surfactant component 10 times with pure water in order to disperse the toner particles) and allowed to mix. Then, ultrasonic dispersion is performed for 1 minute to prepare a toner dispersion. This toner dispersion is poured with a pipette into a beaker containing an "ISOTON II" (manufactured by Beckman Coulter) in the sample stand until the concentration indicated on the measuring device reaches 8%. By keeping the concentration within the above range, reproducible measurement values ​​can be obtained. In the measurement device, the number of measured particles is set to 25,000, the aperture diameter is set to 100 μm, and the measurement range of 2 to 60 μm is divided into 256 parts to calculate the frequency value. The particle diameter of the largest 50% of the volume cumulative fraction is determined to be the volume-based median diameter.

[0100] <Average circularity of toner particles> The average circularity of the toner particles according to the present invention is preferably within a range of 0.930 to 1.000, and more preferably within a range of 0.950 to 0.995, from the viewpoints of the stability of the charging characteristics and the low-temperature fixing ability. When the average circularity is within the above range, individual toner particles are less likely to be crushed, contamination of the frictional charging member is suppressed, and the chargeability of the toner is stabilized. Also, the image formed has high image quality.

[0101] The average circularity of the toner particles is a value measured using "FPIA-3000" (manufactured by Sysmex Corporation). Specifically, the measurement sample (toner) is mixed with an aqueous solution containing a surfactant, and dispersed by ultrasonic dispersion treatment for 1 minute. After that, images are taken using an "FPIA-3000" (manufactured by Sysmex) under the measurement conditions of HPF (high magnification imaging) mode at an appropriate concentration of 3,000 to 10,000 HPF detections. The circularity of each toner particle is calculated according to the following formula (y), and the circularity of each toner particle is added and divided by the total number of toner particles. If the HPF detection number is within the above range, reproducibility is obtained. Formula (y): Circularity = (perimeter of a circle with the same projected area as the particle image) / (perimeter of the projected image of the particle)

[0102] [Toner manufacturing method] The toner manufacturing method of the present invention is characterized by comprising: a step of incorporating a styrene-acrylic resin as a binder resin and coating the surfaces of core particles with a shell portion so that the coverage is within the range of 60 to 99%; and a step of using an ester wax that accounts for 90 mass % or more of a release agent, which contains at least two types of release agents A and B as the ester wax, and selecting the release agent A and the release agent B so that when the melting points of the release agent A and the release agent B are Ta and Tb, respectively, the following formula (1) is satisfied, and when the crystallization temperature of the release agent B is Tc, the following formula (2) is satisfied. Formula (1): Ta <Tb Formula (2): 65℃≦Tc

[0103] The method for producing the toner of the present invention is not particularly limited as long as it includes the above-mentioned coating step and the step of selecting the release agent A and the release agent B, and examples of the method include a pulverization method, an emulsion dispersion method, a suspension polymerization method, a dispersion polymerization method, an emulsion polymerization method, an emulsion polymerization aggregation method, and other known methods. In particular, the emulsion polymerization aggregation method is preferred from the viewpoints of production cost and production stability.

[0104] In the emulsion polymerization aggregation method, first, an aqueous dispersion in which binder resin particles (hereinafter also referred to as "binder resin particles") are dispersed in an aqueous medium is mixed with an aqueous dispersion in which colorant particles (hereinafter also referred to as "colorant particles") are dispersed. Next, the binder resin particles and the colorant particles are aggregated and thermally fused to form toner particles, thereby producing a toner.

[0105] The binder resin particles may have a multi-layer structure of two or more layers made of binder resins with different compositions. For example, the binder resin particles having such a structure and a two-layer structure are obtained by preparing a dispersion of resin particles by a polymerization treatment (first-stage polymerization) according to a conventional method. Then, a polymerization initiator and a polymerizable monomer are added to this dispersion, and the system is polymerized (second-stage polymerization).

[0106] Here, the term "aqueous dispersion" refers to a dispersion in which a dispersing body (particles) is dispersed in an aqueous medium. The aqueous medium refers to a medium whose main component (50% by mass or more) is water. The components other than water include organic solvents that dissolve in water. Examples of the organic solvent include methanol, ethanol, isopropanol, butanol, acetone, methyl ethyl ketone, tetrahydrofuran, etc. Among these, alcohol-based organic solvents such as methanol, ethanol, isopropanol, and butanol, which are organic solvents that do not dissolve resins, are particularly preferred.

[0107] An example of the emulsion polymerization aggregation method for producing the toner according to the present invention includes the following steps (a) to (i). In the following, an example will be given in which a styrene-acrylic resin, which is an amorphous vinyl resin, is used for the core particles and an amorphous polyester is used for the shell, but the present invention is not limited to this. (a) A step of preparing an aqueous dispersion in which amorphous resin particles (hereinafter also referred to as "amorphous resin particles") are dispersed in an aqueous medium. (b) A step of preparing an aqueous dispersion in which colorant particles are dispersed in an aqueous medium. (c) A step of aggregating and fusing the amorphous resin particles and the colorant particles in an aqueous medium to form associated particles. (d) A process of ripening the aggregated particles by thermal energy to control the shape and obtain toner particles. (e) Cooling the toner particle dispersion (f) A crystallization promotion step of reheating the cooled toner particle dispersion to promote crystallization. (g) A step of filtering the toner particles from the aqueous medium and removing surfactants and the like from the toner particles. (h) drying the washed toner particles;

[0108] Furthermore, the emulsion polymerization aggregation method may include, if necessary, (j) a step of adding an external additive to the dried toner particles.

[0109] (a) A process for preparing an aqueous dispersion of amorphous resin particles In this step, an aqueous dispersion of amorphous resin particles is prepared from the amorphous resin. An aqueous dispersion of styrene-acrylic resin particles for the core particles and an aqueous dispersion of amorphous polyester particles for the shell are prepared as follows.

[0110] (a1) Preparation of an aqueous dispersion of styrene-acrylic resin particles Aqueous dispersions of styrene-acrylic resin particles can be prepared by miniemulsion polymerization using vinyl monomers. That is, for example, a vinyl monomer is added to an aqueous medium containing a surfactant, and mechanical energy is applied to form droplets. Next, a polymerization reaction is caused to proceed in the droplets by radicals from a water-soluble radical polymerization initiator. An oil-soluble polymerization initiator may be contained in the droplets.

[0111] (Surfactant) As the surfactant used in this step, various conventionally known anionic surfactants, cationic surfactants, nonionic surfactants, etc. can be used.

[0112] (Polymerization initiator) As the polymerization initiator used in this step, various conventionally known initiators can be used. Specific examples of polymerization initiators that are preferably used include persulfates (potassium persulfate, ammonium persulfate, etc.). In addition, azo compounds (4,4'-azobis4-cyanovaleric acid and its salts, 2,2'-azobis(2-amidinopropane) salts, etc.), peroxide compounds, azobisisobutyronitrile, etc. may also be used.

[0113] (Chain transfer agent) In this step, a commonly used chain transfer agent can be used for the purpose of adjusting the molecular weight of the amorphous resin. The chain transfer agent is not particularly limited, and examples thereof include mercaptans such as 2-chloroethanol, octyl mercaptan, dodecyl mercaptan, and t-dodecyl mercaptan, and styrene dimer.

[0114] (a2) A process for preparing an aqueous dispersion of amorphous polyester particles The aqueous dispersion of amorphous polyester particles can be prepared by synthesizing an amorphous polyester and dispersing the amorphous polyester in the form of fine particles in an aqueous medium. Specifically, the oil phase liquid is prepared by dissolving or dispersing the amorphous polyester in an organic solvent, and then the oil phase liquid is dispersed in an aqueous medium by phase inversion emulsification or the like to form oil droplets having a desired particle size, and then the organic solvent is removed to prepare the oil phase liquid.

[0115] The amount of the aqueous medium used is preferably within a range of 50 to 2000 parts by mass, and more preferably within a range of 100 to 1,000 parts by mass, relative to 100 parts by mass of the oil phase liquid. A surfactant may be added to the aqueous medium in order to improve the dispersion stability of the oil droplets. Examples of the surfactant include the same surfactants as those listed in the above steps.

[0116] The organic solvent used for preparing the oil phase liquid is preferably one having a low boiling point and low solubility in water, from the viewpoint of easy removal treatment after the formation of oil droplets.Specific examples of the organic solvent include methyl acetate, ethyl acetate, methyl ethyl ketone, methyl isobutyl ketone, toluene, xylene, etc.These organic solvents can be used alone or in combination of two or more. The amount of the organic solvent used is usually within the range of 1 to 300 parts by mass based on 100 parts by mass of the amorphous polyester. The emulsification and dispersion of the oil phase liquid can be carried out by utilizing mechanical energy.

[0117] The toner base particles according to the present invention contain a releasing agent, which can be introduced in this step. Specifically, it can be introduced into the toner particles by dissolving or dispersing it in advance in a solution of a vinyl monomer for forming a styrene-acrylic resin, or in an oil phase liquid. The release agent can also be introduced into the toner particles by separately preparing a dispersion of release agent particles consisting of only the release agent, and aggregating the release agent particles together with the styrene / acrylic resin particles and the colorant particles in the aggregation and fusion process. However, it is preferable to adopt a method in which the release agent is introduced in advance in this process.

[0118] Here, 90% by mass or more of the entire release agent is made to be ester wax. The ester wax contains at least two types of release agent A and release agent B, and the release agent A and the release agent B are selected so as to satisfy the above formulas (1) and (2). The release agent A and the release agent B have been described above and will not be described here.

[0119] Furthermore, the toner base particles according to the present invention may contain other internal additives, such as a charge control agent, if necessary. Such internal additives can be introduced into the toner particles by, for example, dissolving or dispersing them in advance in the vinyl monomer solution (or the oil phase liquid of the amorphous polyester) used to form the styrene-acrylic resin in this process.

[0120] Such internal additives can also be introduced into the toner particles by separately preparing a dispersion of internal additive particles consisting of only the internal additives, and aggregating the internal additive particles together with the styrene / acrylic resin particles and the colorant particles in the aggregation / fusion step. However, it is preferable to adopt a method of introducing the internal additives in advance in this step.

[0121] The average particle size of the styrene-acrylic resin particles is preferably in the range of 100 to 400 nm in terms of volume-based median diameter. The volume-based median diameter of the styrene-acrylic resin particles is a value measured using "Microtrac UPA-150" (manufactured by Nikkiso Co., Ltd.).

[0122] (b) Preparation of an aqueous dispersion of colorant particles This step is carried out as necessary when it is desired to prepare toner particles containing a colorant, and is a step for dispersing the colorant in the form of fine particles in an aqueous medium to prepare an aqueous dispersion of colorant particles. An aqueous dispersion of colorant particles can be obtained by dispersing a colorant in an aqueous medium to which a surfactant has been added at a critical micelle concentration (CMC) or higher. The colorant can be dispersed by utilizing mechanical energy. The dispersing machine to be used is not particularly limited, but preferably includes an ultrasonic dispersing machine, a mechanical homogenizer, a pressure dispersing machine such as a Manton-Gaulin or pressure homogenizer, a sand grinder, a medium type dispersing machine such as a Getzmann mill or a diamond fine mill.

[0123] The colorant particles in a dispersed state preferably have a volume-based median diameter within the range of 10 to 300 nm, more preferably 100 to 200 nm, and particularly preferably 100 to 150 nm. In the present invention, the volume-based median diameter of the colorant particles is a value measured using an electrophoretic light scattering photometer "ELS-800" (manufactured by Otsuka Electronics Co., Ltd.).

[0124] (c) Agglomeration / fusion process In this process, the styrene-acrylic resin particles, colorant particles, and, if necessary, particles of other toner components are aggregated and then fused together by heating. Specifically, a flocculant at or above its critical flocculation concentration is added to an aqueous dispersion in which the above particles are dispersed in an aqueous medium, and the temperature is raised to above the glass transition point of the styrene-acrylic resin, causing the particles to flocculate and fuse. The fusion temperature for fusing the styrene-acrylic resin particles may be equal to or higher than the glass transition point of the styrene-acrylic resin, particularly (glass transition point of the styrene-acrylic resin + 10°C) to (glass transition point of the styrene-acrylic resin + 50°C), and particularly preferably (glass transition point of the styrene-acrylic resin + 15°C) to (glass transition point of the styrene-acrylic resin + 40°C).

[0125] (Flocculant) The flocculant used in this step is not particularly limited, but is preferably selected from metal salts such as alkali metal salts and alkaline earth metal salts. Examples of metal salts include monovalent metal salts such as sodium, potassium, and lithium; divalent metal salts such as calcium, magnesium, manganese, and copper; and trivalent metal salts such as iron and aluminum. Specific examples of metal salts include sodium chloride, potassium chloride, lithium chloride, calcium chloride, magnesium chloride, zinc chloride, copper sulfate, magnesium sulfate, and manganese sulfate. Among these, it is particularly preferable to use divalent metal salts, since they can promote aggregation with a smaller amount. These salts may be used alone or in combination of two or more.

[0126] In the present invention, since the toner particles have a core-shell structure, for example, in this step, the styrene-acrylic resin particles and the colorant particles are aggregated and fused to form core particles.

[0127] Thereafter, amorphous polyester particles for forming the shell are aggregated on the core particles and fused to form the shell portion. Here, in the present invention, a step of covering the surface of the core particle with the shell portion is carried out so that the coverage is within the range of 60 to 99%. Specifically, in this process, in order to set the coverage rate of the core particles by the shell portion within the range of 60 to 99%, it is preferable to set the amount of the dispersion of the amorphous polyester particles to be aggregated for the shell to be added within the range of 5 to 20% by mass relative to the toner base particles. The temperature at which the amorphous polyester particles for the shell are fused to the core particles is preferably within a range of 75 to 85°C. Furthermore, it is preferable that the stirring speed during the fusion of the amorphous polyester particles for the shell to the core particles is within the range of 200 to 300 rpm.

[0128] (d) Aging process This step is performed as necessary. In the aging step, the toner particles obtained in the aggregation and fusion step are aged by thermal energy until they have a desired shape to form toner particles. Specifically, the aging treatment is carried out by heating and stirring the system in which the associated particles are dispersed, and adjusting the heating temperature, stirring speed, heating time, etc. until the shape of the associated particles reaches a desired circularity.

[0129] (f) Cooling process This step is a step in which the dispersion of toner particles is cooled. As a condition for the cooling treatment, it is preferable to cool at a cooling rate of 1 to 20° C. / min. The specific method for the cooling treatment is not particularly limited, and examples thereof include a method of cooling by introducing a refrigerant from the outside of the reaction vessel, and a method of cooling by directly introducing cold water into the reaction system.

[0130] (h) Filtration and washing process This process is a process in which the toner particles are separated from the cooled dispersion liquid of the toner particles into a solid-liquid separation, and the toner cake obtained by the solid-liquid separation is washed to remove any attached substances such as surfactants and coagulants. The toner cake is an aggregate of toner particles in a wet state that have been coagulated into a cake shape. The solid-liquid separation is not particularly limited, and may be performed using a centrifugation method, a reduced pressure filtration method using a Nutsche or the like, a filtration method using a filter press or the like, etc. In addition, in the washing, it is preferable to wash with water until the electrical conductivity of the filtrate reaches 10 μS / cm.

[0131] (i) Drying process This step is a step of drying the washed toner cake, and can be carried out in accordance with a drying step generally performed in known methods for producing toner particles. Specifically, examples of the dryer used for drying the toner cake include a spray dryer, a vacuum freeze dryer, and a reduced pressure dryer. It is preferable to use a stationary shelf dryer, a mobile shelf dryer, a fluidized bed dryer, a rotary dryer, an agitator dryer, or the like. The moisture content of the dried toner particles is preferably 5% by mass or less, more preferably 2% by mass or less. If the dried toner particles are aggregated by weak interparticle attractive forces, the aggregates may be subjected to a crushing treatment. Here, as the crushing treatment device, a mechanical crushing device such as a jet mill, a Henschel mixer, a coffee mill, or a food processor can be used.

[0132] (j) Additive addition process This step is carried out as necessary when an external additive is added to the toner particles. The toner particles according to the present invention can be used as a toner as it is. However, in order to improve the flowability, chargeability, cleaning property, etc., the toner particles may be used in a state where external additives such as a so-called fluidizing agent and a cleaning aid are added to the toner particles. As the external additive, various additives may be used in combination. The total amount of these external additives added is preferably within a range of 0.05 to 5 parts by mass, and more preferably 0.1 to 3 parts by mass, per 100 parts by mass of the toner particles. As a mixer for the external additives, a mechanical mixer such as a Henschel mixer or a coffee mill can be used.

[0133] In the above-mentioned toner manufacturing method, a styrene-acrylic resin is used for the core particles and an amorphous polyester is used for the shell portion, but the following combinations may be used. An amorphous polyester may be used for the core particles and a styrene-acrylic resin may be used for the shell portion. In addition, an amorphous polyester may be used for both the core particles and the shell portion. In addition, a crystalline polyester may be used for the core particles and a styrene-acrylic resin or an amorphous polyester may be used for the shell portion. In addition, a styrene-acrylic resin may be used for both the core particles and the shell portion. The aqueous dispersion of the crystalline polyester particles can be prepared as follows.

[0134] (k) A process for preparing an aqueous dispersion of crystalline polyester particles The aqueous dispersion of crystalline polyester particles can be prepared by synthesizing a crystalline polyester and dispersing the crystalline polyester in the form of fine particles in an aqueous medium. Specifically, the crystalline polyester is dissolved or dispersed in an organic solvent to prepare an oil phase liquid, and then the oil phase liquid is dispersed in an aqueous medium by phase inversion emulsification or the like to form oil droplets having a desired particle size, and then the organic solvent is removed to prepare the oil phase liquid.

[0135] The amount of the aqueous medium used is preferably within a range from 50 to 2000 parts by mass, and more preferably within a range from 100 to 1000 parts by mass, relative to 100 parts by mass of the oil phase liquid. A surfactant may be added to the aqueous medium in order to improve the dispersion stability of the oil droplets. Examples of the surfactant include the same surfactants as those listed in the above steps.

[0136] The organic solvent used for preparing the oil phase liquid is preferably one having a low boiling point and low solubility in water, from the viewpoint of easy removal treatment after the formation of oil droplets.Specific examples of the organic solvent include methyl acetate, ethyl acetate, methyl ethyl ketone, methyl isobutyl ketone, toluene, xylene, etc.These organic solvents can be used alone or in combination of two or more. The amount of the organic solvent used is usually within the range of 1 to 300 parts by mass based on 100 parts by mass of the crystalline polyester. The emulsification and dispersion of the oil phase liquid can be carried out by utilizing mechanical energy.

[0137] The average particle size of the crystalline polyester particles is preferably in the range of 100 to 400 nm in terms of volume-based median diameter. In the present invention, the volume-based median diameter of the crystalline polyester particles is a value measured using "Microtrac UPA-150" (manufactured by Nikkiso Co., Ltd.).

[0138] Although the embodiment of the present invention has been specifically described above, the embodiment of the present invention is not limited to the above example, and various modifications can be made.

[0139] [Developer] The toner for developing electrostatic images of the present invention can be used as a magnetic or non-magnetic one-component developer, but may also be mixed with a carrier to be used as a two-component developer. When the toner is used as a two-component developer, the carrier may be magnetic particles made of a conventionally known material such as a metal such as iron, ferrite, magnetite, or an alloy of such a metal with a metal such as aluminum or lead. Ferrite particles are particularly preferred as the carrier.

[0140] As the carrier, a coated carrier in which the surface of magnetic particles is coated with a coating agent such as resin, or a dispersion type carrier in which fine magnetic powder is dispersed in a binder resin may be used. The volume-based median diameter (d50) of the carrier is preferably within the range of 20 to 100 μm, and more preferably within the range of 25 to 80 μm. The volume-based median diameter (d50) of the carrier can be measured, for example, by a laser diffraction particle size distribution measuring device HELOS (manufactured by SYMPATEC) equipped with a wet disperser.

[0141] [Image forming method] The image forming method of the present invention is characterized by using the above-mentioned toner for developing electrostatic images of the present invention. In the image forming method of the present invention, for example, an electrostatic image formed on a photoreceptor is developed to obtain a toner image, and the toner image is transferred to an image support. Thereafter, the toner image transferred to the image support is fixed to the image support by a fixing process using a heat and pressure fixing method, thereby obtaining a printed matter on which a visible image is formed.

[0142] The toner of the present invention can be used in a monochrome image forming method or a full-color image forming method. In the full-color image forming method, any image forming method can be applied, such as a four-cycle image forming method consisting of four types of color developing devices for yellow, magenta, cyan, and black, and one photosensitive member, or a tandem image forming method in which image forming units having color developing devices and photosensitive members for each color are installed for each color. EXAMPLES

[0143] The present invention will be specifically described below with reference to examples, but the present invention is not limited thereto. In the following examples, unless otherwise specified, the operations were performed at room temperature (25°C). Furthermore, unless otherwise specified, "%" and "parts" mean "% by mass" and "parts by mass", respectively.

[0144] [Release agent] The release agents used are as shown in the table below. [Table 1]

[0145] [Table 2]

[0146] [Table 3]

[0147] [Wax melting point / crystallization temperature] <Melt point measurement method> The melting point of the release agent was measured by DSC. Specifically, 5 mg of the sample was sealed in an aluminum pan, KIT NO. B0143013, and set in a sample holder of a thermal analyzer Diamond DSC (PerkinElmer), and the temperature was changed in the following order: increase, decrease, and increase again. In the first and second heating steps, the temperature was raised from 0° C. to 100° C. at a heating rate of 10° C. / min and held at 100° C. for 1 minute. During cooling, the temperature was lowered from 100° C. to 0° C. at a rate of 10° C. / min, and the temperature was held at 0° C. for 1 minute. The temperature at the top of the endothermic peak in the endothermic curve obtained during the second heating was measured as the melting point (Tm).

[0148] <Method for measuring crystallization temperature> The crystallization temperature of the release agent was measured by DSC. Specifically, 5 mg of the sample was sealed in an aluminum pan, KIT NO. B0143013, and set in a sample holder of a thermal analyzer Diamond DSC (PerkinElmer), and the temperature was changed in the following order: increase, decrease, and increase again. In the first and second heating steps, the temperature was raised from 0° C. to 100° C. at a heating rate of 10° C. / min and held at 100° C. for 1 minute. During cooling, the temperature was lowered from 100° C. to 0° C. at a rate of 10° C. / min, and the temperature was held at 0° C. for 1 minute. The temperature at the top of the exothermic peak in the exothermic curve obtained during cooling was measured as the crystallization temperature (Tc).

[0149] [Production of Toner 1] <Preparation of styrene-acrylic resin particle dispersion [S1]> (First stage polymerization) A 5 L reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, and a nitrogen introduction device was charged with 8 parts by mass of sodium dodecyl sulfate and 3,000 parts by mass of ion-exchanged water. The inside temperature was raised to 80° C. while stirring at a stirring speed of 230 rpm under a nitrogen stream. After the temperature was raised, a solution in which 10 parts by mass of potassium persulfate was dissolved in 200 parts by mass of ion-exchanged water was added, and the liquid temperature was raised to 80° C. again, and the following mixed monomer liquid was added dropwise over 1 hour. Styrene 480.0 parts by mass n-Butyl acrylate 250.0 parts by mass Methacrylic acid 68.0 parts by mass After the dropwise addition, polymerization was carried out by heating and stirring at 80° C. for 2 hours to prepare a base particle dispersion liquid.

[0150] (Second stage polymerization) A solution of 7.8 parts by mass of sodium polyoxyethylene (2) dodecyl ether sulfate dissolved in 2,429 parts by mass of ion-exchanged water was charged into a 5 L reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, and a nitrogen introducing device, and heated to 98° C. After heating, 57 parts by mass, calculated as solid content, of the amorphous vinyl resin particle dispersion prepared by the above first-stage polymerization and a mixed solution of the following monomers, chain transfer agent, and release agent dissolved at 90° C. were added. Styrene (St) 264.1 parts by mass 2-Ethylhexyl acrylate (2EHA) 98.2 parts by weight Methacrylic acid 80% aqueous solution (MAA80) 39.3 parts by weight (Methacrylic acid solid content 30.6 parts by mass) n-Octyl-3-mercaptopropionate (chain transfer agent) 4.1 parts by mass Ester wax A-1 (release agent A) 63.6 parts by weight Ester wax B-1 (release agent B) 254.3 parts by weight A mixing and dispersion process was carried out for 1 hour using a mechanical disperser CLEARMIX (registered trademark) with a circulation path (manufactured by M-Technique Co., Ltd.) to prepare a dispersion containing emulsified particles (oil droplets). A polymerization initiator solution of 5.4 parts by mass of potassium persulfate dissolved in 103 parts by mass of ion-exchanged water was added to this dispersion. This system was heated and stirred at 84°C for 1 hour to polymerize, preparing an amorphous vinyl resin particle dispersion.

[0151] (Third stage polymerization) 400 parts by mass of ion-exchanged water was further added to the amorphous vinyl resin particle dispersion obtained by the second-stage polymerization and mixed thoroughly. Then, a solution in which 7.3 parts by mass of potassium persulfate was dissolved in 138 parts by mass of ion-exchanged water was added. Furthermore, a mixture of the following monomers and chain transfer agent was added dropwise over 1 hour under a temperature condition of 82°C. Styrene (St) 378.0 parts by mass Butyl acrylate (BA) 170.0 parts by mass Methacrylic acid 80% aqueous solution (MAA80) 43.8 parts by mass (Methacrylic acid solid content 34.0 parts by mass) Methyl methacrylate (MMA) 54.0 parts by mass n-Octyl-3-mercaptopropionate 8.2 parts by mass After the dropwise addition was completed, polymerization was carried out by heating and stirring for 2 hours, and then the mixture was cooled to 28°C to prepare a styrene-acrylic resin (amorphous vinyl resin) particle dispersion [S1].

[0152] <Preparation of amorphous polyester particle dispersion [AP1]> (Synthesis of amorphous polyester [ap1]) The following materials were charged into a reaction vessel equipped with a stirrer, a nitrogen inlet tube, a temperature sensor and a rectification column. <Polycarboxylic acids> Terephthalic acid 85 parts by mass Trimellitic acid 6 parts by mass Fumaric acid 18 parts by mass Dodecenylsuccinic anhydride 80 parts by mass <Polyhydric alcohol> Bisphenol A propylene oxide adduct 381 parts by mass Bisphenol A ethylene oxide adduct 62 parts by mass

[0153] The temperature of the reaction system was raised to 190°C over 1 hour, and after confirming that the reaction system was uniformly stirred, Ti(OBu)4 was added as a catalyst in an amount of 0.006% by mass based on the total amount of polycarboxylic acid. The temperature of the reaction system was then raised from the same temperature to 240°C over 6 hours while distilling off the water produced. The dehydration condensation reaction was continued for 6 hours while maintaining the temperature at 240°C to carry out the polymerization reaction, thereby obtaining amorphous polyester [ap1].

[0154] (Preparation of amorphous polyester particle dispersion) 200 parts by mass of amorphous polyester [ap1] was dissolved in 200 parts by mass of ethyl acetate, and while stirring the solution, an aqueous solution in which sodium polyoxyethylene lauryl ether sulfate was dissolved in 800 parts by mass of ion-exchanged water to a concentration of 1% by mass was slowly added dropwise. After removing the ethyl acetate from this solution under reduced pressure, the pH was adjusted to 8.5 with ammonia. Then, the solid content was adjusted to 20% by mass. In this way, an amorphous polyester particle dispersion [AP1] in which fine particles of amorphous polyester [ap1] were dispersed in an aqueous medium was prepared.

[0155] <Preparation of Colorant Particle Dispersion> A solution of 90 parts by mass of sodium dodecyl sulfate added to 1600 parts by mass of ion-exchanged water was stirred, and 420 parts by mass of copper phthalocyanine (CI Pigment Blue 15:3) was gradually added thereto. A colorant particle dispersion was prepared by dispersing using a stirring device, Clearmix (M Technique Co., Ltd.). The colorant particles in the dispersion had a volume-based median diameter of 110 nm.

[0156] <Toner manufacturing> In a reaction vessel equipped with a stirrer, a temperature sensor, and a cooling tube, 540 parts by mass (solid content equivalent) of styrene-acrylic resin particle dispersion [S1] as the dispersion for the core and 332 parts by mass of ion-exchanged water were added. At room temperature (25°C), a 5 mol / L aqueous solution of sodium hydroxide was added to adjust the pH to 10. Further, 31 parts by mass (solid content equivalent) of the colorant particle dispersion liquid was added, and a solution in which 72.5 parts by mass of an aqueous magnesium chloride solution was dissolved in 72.5 parts by mass of ion-exchanged water was added thereto at 30° C. over a period of 10 minutes with stirring. After leaving it for 3 minutes, the temperature was raised to 80°C over 60 minutes. After reaching 80°C, the stirring speed was adjusted so that the particle size growth rate was 0.01 μm / min, and the particles were allowed to grow until the volume-based median diameter measured with a Coulter Multisizer 3 (manufactured by Coulter Beckman) reached 6.0 μm.

[0157] Next, 60 parts by mass (solid content equivalent) of amorphous polyester particle dispersion [AP1] was added as a shell dispersion over 30 minutes. When the supernatant of the reaction solution became transparent, an aqueous solution of 94.6 parts by mass of sodium chloride dissolved in 378.4 parts by mass of ion-exchanged water was added to stop the growth of particle size. The mixture was then heated to 80° C. and stirred to promote fusion of the particles. When the average circularity of the toner particles reached 0.970, the mixture was cooled to 30° C. at a cooling rate of 2.5° C. / min. The average circularity was measured using a measuring device FPIA-3000 (manufactured by Sysmex Corporation) with the number of HPF detections set at 4000 particles.

[0158] Next, the toner cake was subjected to solid-liquid separation, and the dehydrated toner cake was washed by repeating the operation of redispersing the toner cake in ion-exchanged water and separating the solid and liquid three times. After washing, the toner cake was dried at 40° C. for 24 hours to obtain toner base particles.

[0159] To 100 parts by mass of the obtained toner base particles, 0.6 parts by mass of hydrophobic silica particles (number average primary particle size: 12 nm, hydrophobicity: 68), 1.0 part by mass of hydrophobic titanium oxide particles (number average primary particle size: 20 nm, hydrophobicity: 63), and 1.0 part by mass of sol-gel silica (number average primary particle size = 110 nm) were added. Then, the mixture was mixed for 20 minutes at 32°C and a rotor circumferential speed of 35 mm / sec using a Henschel mixer (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.). After mixing, coarse particles were removed using a sieve with 45 μm openings, and toner 1 was obtained.

[0160] [Production of Toners 2-4, 6-14 and 18-22] Toners 2 to 4, 6 to 14, and 18 to 22 were produced in the same manner as Toner 1, except that the release agent used in the second polymerization step was changed as shown in Table IV below. The content of the release agent shown in Tables VI and VII is the "wax content (mass %) in the toner base particles." The parts by mass of the release agent shown in Table IV are calculated based on the content of the release agent shown in Tables VI and VII.

[0161] [Production of Toner 5] Toner 5 was produced in the same manner as Toner 1, except that the release agent used in the second polymerization step was changed as shown in the table below, and the shell dispersion was changed to the following styrene-acrylic resin particle dispersion [S2]. Ester Wax A-2 (Release Agent A) 158.9 parts by weight Ester wax B-1 (release agent B) 79.5 parts by weight (Preparation of styrene-acrylic resin particle dispersion [S2]) Styrene-acrylic resin particle dispersion [S2] was prepared by carrying out the polymerization reaction and post-reaction treatment in the same manner as in the first-stage polymerization of the above (Preparation of styrene-acrylic resin particle dispersion [S1]), except that the mass parts of each monomer were changed as follows: Styrene 508 parts by weight n-Butyl acrylate 245 parts by weight Methacrylic acid 57 parts by mass

[0162] [Production of Toner 15] Toner 15 was produced in the same manner as Toner 1, except that in the production of Toner 1, the release agent used in the second-stage polymerization was changed as shown in the table below, and the core dispersion was changed to the amorphous polyester particle dispersion [AP2] shown below. (Preparation of amorphous polyester particle dispersion [AP2]) An amorphous polyester particle dispersion [AP2] was prepared in the same manner as in the preparation of the amorphous polyester particle dispersion [AP1], except that the number of parts of each monomer was changed as follows and the ester wax was changed as follows. Terephthalic acid 79 parts by mass Trimellitic acid 6 parts by mass Fumaric acid 16 parts by mass Isophthalic acid 74 parts by weight Bisphenol A propylene oxide adduct 354 parts by mass Bisphenol A ethylene oxide adduct 58 parts by mass Ester Wax A-1 (Release Agent A) 143 parts by weight Ester wax B-2 (release agent B) 143 parts by weight

[0163] [Production of Toner 16] Toner 16 was produced in the same manner as Toner 1, except that the release agent used in the second polymerization step was changed as shown in the table below, the core dispersion was changed to the amorphous polyester resin [AP3] shown below, and the shell dispersion was changed to the styrene-acrylic resin particle dispersion [S2]. (Preparation of amorphous polyester particle dispersion [AP3]) An amorphous polyester particle dispersion [AP2] was prepared in the same manner as in the preparation of the amorphous polyester particle dispersion [AP1], except that the number of parts of each monomer was changed as follows and the ester wax was changed as follows. Terephthalic acid 79 parts by mass Trimellitic acid 6 parts by mass Fumaric acid 16 parts by mass Isophthalic acid 74 parts by weight Bisphenol A propylene oxide adduct 354 parts by mass Bisphenol A ethylene oxide adduct 58 parts by mass Ester Wax A-2 (Release Agent A) 158.9 parts by weight Ester wax B-3 (release agent B) 63.6 parts by weight

[0164] [Toner 17 Production] Toner 17 was produced in the same manner as Toner 1, except that in the production of Toner 1, the release agent used in the second-stage polymerization was changed as shown in the table below, and the shell dispersion was changed to the following crystalline polyester particle dispersion [CP1]. (Preparation of Crystalline Polyester Particle Dispersion [CP1]) A crystalline polyester particle dispersion [CP1] was prepared in the same manner as in the preparation of the amorphous polyester particle dispersion [AP1], except that the parts of each monomer were changed as follows. Sebacic acid 279 parts by mass 1,6-Hexanediol 156 parts by mass

[0165]

Table 4

[0166] [Manufacture of Developers 1 to 22] For toners 1 to 22, ferrite carriers with a volume average particle diameter of 60 μm coated with silicone resin were added and mixed so that the toner particle concentration became 6% by mass, thereby manufacturing developers 1 to 22, respectively.

[0167] The types of the dispersion for the core and the dispersion for the shell were summarized in the following table. Also, regarding the ester wax used for each toner, whether the conditions of Formula (1) Ta < Tb and Formula (2) 65°C ≤ Tc were satisfied or not were shown in the following table. In the following table, “Y” means that the conditions of each formula are satisfied, and “N” means that the conditions of each formula are not satisfied.

[0168]

Table 5

[0169]

Table 6

[0170]

Table 7

[0171] The “ester wax content rate” described in Table VI and Table VII represents the content rate (mass%) of the ester wax with respect to the entire release agent.

[0172] [Coating Rate of the Shell Part] The coating rate of the shell in the toner base particles was calculated from the cross section of the toner base particles. Specifically, the cross section of each toner base particle was photographed at 10,000 to 20,000 times magnification with an electron microscope JSM-7401F (manufactured by JEOL Ltd.) at an acceleration voltage of 30 kV. The photographed image was used to measure the length of the interface between the shell region and the encapsulating resin and the perimeter of the cross section of the toner base particle using an image processing analyzer LUZEX AP (manufactured by Nireco Corporation). The coverage rate of the shell was calculated by the following formula, where A is the length of the interface between the shell region and the embedding resin, and B is the cross-sectional circumference of the toner base particle. (Coverage rate) = A / B x 100

[0173] <Heat-resistant storage> 0.5 g of toner was placed in a 10 ml glass bottle with an inner diameter of 21 mm, the bottle was capped, and the bottle was shaken 600 times at room temperature using a Tap Denser KYT-2000 (manufactured by Seishin Enterprises). After that, the bottle was left for 2 hours in an environment of 57.5°C and 35% RH with the cap removed. Next, the toner was placed on a 48 mesh (350 μm mesh) sieve while being careful not to break up the toner aggregates. Then, it was set in a powder tester (manufactured by Hosokawa Micron Corporation), fixed with a presser bar and a knob nut, adjusted to a vibration intensity with a feed width of 1 mm, and vibrated for 10 seconds. After that, the ratio (mass%) of the toner amount remaining on the sieve was measured. The toner cohesion rate was calculated according to the following formula. Toner cohesion rate (%) = mass of toner remaining on sieve (g) / 0.5 (g) x 100 The heat-resistant storage stability of the toner was evaluated according to the following criteria, and the evaluation was used as an index of storage stability. The toner cohesion rate is preferably less than 35% by weight, more preferably less than 25% by weight, and even more preferably less than 15% by weight. (standard) AAA: Toner cohesion rate is less than 15% by mass (toner has excellent heat-resistant storage properties) AA: Toner coagulation rate is 15% by mass or more and less than 25% by mass (good heat-resistant storage properties of toner) A: Toner cohesion rate is 25% by mass or more and less than 35% by mass (heat resistance storage stability of toner is slightly poor, but acceptable level) B: Toner cohesion rate is 35% by mass or more (the toner has poor heat resistance for storage and cannot be used)

[0174] <Under-offset property> Under-offset refers to an image defect in which the toner layer is not sufficiently melted by the heat applied when passing through a fixing device, causing the image to peel off from a transfer material such as recording paper. For image evaluation, a developing device of a commercially available color multifunction printer "bizhub PRO (registered trademark) C6500 (manufactured by Konica Minolta, Inc.)" was used. The toner and developer prepared above were loaded in this developing device in order, and evaluation was performed. The device was modified so that the fixing temperature, toner adhesion amount, and system speed could be freely set. The evaluation paper was "NPi wood-free paper (128g / m 2 ) (manufactured by Nippon Paper Industries Co., Ltd.) was used. Toner adhesion amount: 11.3 g / m 2 A solid image was fixed at a fixing speed of 300 mm / sec, the temperature of the upper fixing belt was set at 110 to 200°C, and the temperature of the lower fixing roller was set at 100°C. When fixing was performed at 5°C intervals, the minimum fixing temperature of the upper fixing belt at which no under-offset occurred was evaluated and used as an index of low-temperature fixing ability. The lower the minimum fixing temperature, the better the fixing ability. The under offset property is more preferably less than 135°C, and even more preferably less than 130°C. (standard) AA: Less than 130℃ A: 130℃ or higher and less than 135℃ B:135℃ or higher

[0175] <Evaluation of fold fixation> The fixing device of a copier "bizhub PRO (registered trademark) C6501" (manufactured by Konica Minolta, Inc.) was modified so that the surface temperature of the fixing heat roller could be changed within the range of 100 to 210° C. The above-mentioned developers (1) to (20) were loaded into this modified device, respectively. The evaluation paper was "NPi wood-free paper (128g / m 2) (manufactured by Nippon Paper Industries Co., Ltd.) was used. At normal temperature and humidity (temperature 20°C, relative humidity 55%), the toner adhesion amount was 8 mg / 10 cm 2 A fixing experiment for fixing a solid image was carried out by repeatedly changing the fixing temperature setting from 95°C to 200°C in increments of 5°C. Next, the prints obtained in the fixing experiments at each fixing temperature were folded by a folding machine so that a load was applied to the solid image. Compressed air of 0.35 MPa was blown onto the folded image, and the image condition at the fold was visually evaluated and ranked on the following five-point scale. (Rank criteria) Rank 5: No creases at all Rank 4: Some peeling along the folds Rank 3: Fine linear peeling along the crease Rank 2: Thick linear peeling along the crease Rank 1: Large peeling along the crease The temperature at which rank 3 was reached was determined as the folding and fixing temperature, and the deviation width of the under-offset temperature from this folding and fixing temperature was used as an index. The fold fixability is preferably under offset (UO) plus 15° C. or more and less than 20° C., more preferably plus 12° C. or more and less than 15° C., and even more preferably less than plus 12° C. In the following criteria, "AAA", "AA" and "A" were considered to be acceptable. (standard) AAA: Under offset (UO) plus 12°C or less AA: Under offset (UO) plus 12°C or more and less than 15°C A: Under offset (UO) plus 15°C or more and less than 20°C B: Under offset (UO) plus 20°C or more

[0176] <Wax adhesion> The fixing device of a multifunction printer "bizhub PRESS (registered trademark) C1070" (manufactured by Konica Minolta, Inc.) was used. This fixing device was modified so that the surface temperature of the upper fixing belt could be changed in the range of 140 to 220°C, and the surface temperature of the lower fixing roller could be changed in the range of 120 to 200°C. Each developer was loaded in turn into this modified machine, and A4 size (basis weight 157 g / m2) was printed in a normal temperature and humidity environment (temperature 20°C, humidity 50% RH). 2 ) Glossy coated paper, toner adhesion of 8.0 g / m 2 A solid image of 10 ... The fixing speed during the fixing process was 460 mm / sec, and the fixing temperature (surface temperature of the fixing upper belt) was set to the under-offset temperature + 35°C. After printing 100 sheets, the wax adhesion condition on the transport roller was visually checked in the following 10 stages. Ranking was done by floor. (Rank criteria) Rank 10: No wax adhesion observed Rank 9: Almost no wax adhesion is observed. Rank 8: A very small amount of wax is found, but the quality is not affected. Rank 7: Some wax adhesion is observed, but there is almost no problem with the quality. Rank 6: Wax adhesion was confirmed, not usable Rank 5: Too much wax attached, not practical Rank 4: Too much wax attached, not practical Rank 3: Excessive wax adhesion confirmed, not practical Rank 2: Too much wax attached, not practical Rank 1: Excessive wax adhesion was detected and it is not practical to use. After the above ranking, the samples were evaluated according to the following criteria, with "AA" and "A" being considered as acceptable. (standard) AA: Rank 10-9: No wax adhesion observed A: Rank 8~7: Some wax adhesion is observed, but the quality is not affected. B: Rank 6~1: Wax adhesion is confirmed and it is not practical to use.

[0177] [Table 8]

[0178] As shown by the above results, it is recognized that the toner of the present invention is superior in heat-resistant storage stability, low-temperature fixability and fold fixability, and can suppress the adhesion of wax, as compared with the toner of the comparative example. [Explanation of symbols]

[0179] 1 Toner base particles 2. Core Particles 3. Shell 31 Shell Region

Claims

1. A toner for developing an electrostatic image, comprising core-shell type toner base particles containing at least a binder resin and a release agent, The binder resin contains a styrene-acrylic resin, The surface of the core particle is covered with the shell portion at a coverage rate of 60 to 99%. 90% by mass or more of the release agent is an ester wax, The ester wax contains at least two types of release agent A and release agent B, When the melting points of the release agent A and the release agent B are Ta and Tb, respectively, the following formula (1) is satisfied, and When the crystallization temperature of the release agent B is Tc, the following condition (2) is satisfied:

2. A toner for developing electrostatic images. Formula (1): Ta<Tb Formula (2): 65°C≦Tc

2. The shell portion of the toner base particle contains at least one of a styrene-acrylic resin and a polyester.

2. The toner for developing electrostatic images according to claim 1.

3. The content of at least one of the release agent A and the release agent B in the total amount of the release agents is within a range of 5 to 15% by mass.

2. The toner for developing electrostatic images according to claim 1.

4. The release agent A has two or more ester groups, The release agent B is an ester wax having a smaller number of ester groups than the release agent A.

2. The toner for developing electrostatic images according to claim 1.

5. A toner for developing an electrostatic image, comprising core-shell type toner base particles containing at least a binder resin and a release agent, The binder resin contains a styrene-acrylic resin, The surface of the core particle is covered with the shell portion at a coverage rate of 60 to 99%, 90% by mass or more of the release agent is an ester wax, The ester wax contains at least two types of release agent A and release agent B, When the melting points of the release agent A and the release agent B are Ta and Tb, respectively, the following formula (1) is satisfied: When the crystallization temperature of the release agent B is Tc, the following (2) is satisfied: The content of at least one of the release agent A and the release agent B relative to the total amount of the release agents is within a range of 5 to 15% by mass, and The release agent A has two or more ester groups, The release agent B is an ester wax having a smaller number of ester groups than the release agent A.

2. A toner for developing electrostatic images. Formula (1): Ta<Tb Formula (2): 65°C≦Tc

6. A method for producing the toner for developing an electrostatic image according to any one of claims 1 to 5, comprising the steps of: a step of incorporating a styrene-acrylic resin as a binder resin and coating the surfaces of the core particles with the shell portion so that the coverage is within a range of 60 to 99%; and a step of selecting the release agent A and the release agent B so that 90% by mass or more of the release agent is an ester wax, the ester wax contains at least two types of release agent A and release agent B, and the release agent A and the release agent B satisfy the following formula (1) when the melting points of the release agent A and the release agent B are Ta and Tb, respectively, and satisfy the following formula (2) when the crystallization temperature of the release agent B is Tc.

2. A method for producing a toner for developing an electrostatic image, comprising the steps of: Formula (1): Ta<Tb Formula (2): 65°C≦Tc

7. An image forming method using a toner for developing an electrostatic image, comprising the steps of: The toner for developing an electrostatic image is the toner for developing an electrostatic image according to any one of claims 1 to 5.

1. An image forming method comprising:

Citation Information

Patent Citations

  • toner

    JP2010145553A

  • Toner

    JP2017044980A