Polyimide resin, insulation film-forming material, method for producing semiconductor device and semiconductor device

A polyimide resin with specific structures addresses bonding defects and heat resistance issues in C2W bonding, ensuring high solubility and reliability for semiconductor devices with reduced costs.

JP2024149293APending Publication Date: 2024-10-18HD MICROSYSTEMS LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023063088
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-07
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

In three-dimensional semiconductor chip packaging, C2W bonding faces issues such as foreign matter generation causing bonding defects due to voids in the insulating film, and organic materials like epoxy resins and cyclic olefin resins have insufficient heat resistance, leading to bonding failures and high equipment costs for clean rooms.

Method used

A polyimide resin with specific structural formulas (E) and (G) is developed, offering excellent solvent solubility and insulation reliability, which forms insulating films with improved imidization rates at low temperatures, reducing void formation and enhancing bonding reliability.

Benefits of technology

The polyimide resin ensures high solubility, improved insulation reliability, and reduced bonding defects, enabling efficient and reliable semiconductor device manufacturing with lower equipment costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149293000022
    Figure 2024149293000022
  • Figure 2024149293000023
    Figure 2024149293000023
  • Figure 2024149293000024
    Figure 2024149293000024
Patent Text Reader

Abstract

To provide a polyimide resin with superior solvent solubility and superior insulation reliability.SOLUTION: A polyimide resin includes a structure represented by the formula (E) and a structure represented by the formula (G). In formula (E), C is a divalent linking group including an ether bond. In formula (G), D is a divalent linking group with two or more atoms linked in the main chain. In formula (G). the m-bond content is greater than 0%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a polyimide resin, an insulating film forming material, a method for manufacturing a semiconductor device, and a semiconductor device. [Background technology]

[0002] In recent years, three-dimensional mounting of semiconductor chips has been considered in order to improve the integration degree of LSIs (Large Scale Integrated Circuits). Non-Patent Document 1 discloses an example of three-dimensional mounting of semiconductor chips.

[0003] When three-dimensionally mounting semiconductor chips using C2W (Chip-to-Wafer) bonding, the use of hybrid bonding technology used in W2W (Wafer-to-Wafer) bonding is being considered to achieve fine bonding of wiring between devices.

[0004] In C2W hybrid bonding, there is a risk of misalignment due to the thermal expansion of the substrate, chip, etc. caused by heating during bonding. To address this issue, Patent Document 1 discloses an example of a technology that can lower the bonding temperature by using a cyclic olefin resin. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2019-204818 A [Non-patent literature]

[0006] [Non-Patent Document 1] FC Chen et al., “System on Integrated Chips(SoIC TM) for 3D Heterogeneous Integration”, 2019 IEEE 69th Electronic Components and Technology Conference (ECTC), p.594-599(2019) Summary of the Invention [Problem to be solved by the invention]

[0007] When three-dimensionally mounting semiconductor chips using C2W bonding, unlike W2W bonding, foreign matter (cutting debris) may be generated during the process of dividing into semiconductor chips, and there is a risk that this foreign matter may adhere to the bonding interface of the semiconductor chips (surface of the insulating film of hybrid bonding). The use of inorganic materials such as silicon dioxide (SiO2) for this insulating film has been considered, but since inorganic materials are hard materials, the foreign matter that adheres to the insulating film may create large voids in the insulating film, for example, voids with a width nearly 1000 times the height of the foreign matter, at the bonding interface. For this reason, even if the hybrid bonding technology used in W2W bonding is simply applied to C2W bonding, there is a risk that the generation of such voids may cause bonding failure, which results in a problem of a decrease in the yield of semiconductor device manufacturing. On the other hand, if a clean room and equipment with a high level of cleanliness are used to prevent these bonding failures, a large amount of capital investment is required for the clean room, etc.

[0008] Furthermore, when an organic material such as an epoxy resin or a cyclic olefin resin such as benzocyclobutene is used as the material for the insulating film, the heat resistance of the organic material is insufficient, and the insulating film is exposed to high temperatures during C2W bonding, which may cause the organic material to deteriorate and lead to poor bonding at the interface between the substrate and the insulating film.

[0009] The present inventors have investigated the use of an insulating material containing a polyimide precursor, which is an organic material with excellent heat resistance, from the viewpoint of suppressing poor bonding due to the occurrence of voids and deterioration of organic materials as described above. However, when an insulating material containing a polyimide precursor is applied to C2W bonding, it has been found that the imidization reaction, which is a ring-closing reaction, does not proceed easily at low temperatures, and the insulating reliability of the obtained cured product may be reduced.

[0010] On the other hand, when an attempt is made to use a polyimide resin instead of a polyimide precursor from the viewpoint of improving insulation reliability, there is a problem that the polyimide resin is difficult to dissolve in a solvent, making it difficult to apply the polyimide resin to an insulating material.

[0011] The present disclosure has been made in view of the above, and has an object to provide a polyimide resin having excellent solubility in a solvent and excellent insulation reliability, an insulating film-forming material containing the polyimide resin, a method for manufacturing a semiconductor device using the insulating film-forming material, and a semiconductor device including an insulating film formed from the insulating film-forming material. [Means for solving the problem]

[0012] Specific means for achieving the above object are as follows. <1> A polyimide resin comprising a structure represented by the following formula (E) and a structure represented by the following formula (G).

[0013] [ka]

[0014] [ka]

[0015] In formula (E), C is a divalent linking group containing an ether bond, and in formula (G), D is a divalent linking group having two or more atoms linked to the main chain, and the proportion of m-bonds contained in formula (G) is greater than 0%. <2> In the formula (G), D contains an aromatic ring and an ether bond. <1> The polyimide resin according to claim 1. <3> The structure represented by the formula (E) is any of the structures represented by the formulas (I) to (O). <1> or <2> The polyimide resin according to claim 1.

[0016] [ka] <4> Having a structural unit represented by the following general formula (1): <1> ~ <3> 10. The polyimide resin according to claim 9,

[0017] [ka] In the general formula (1), X represents a tetravalent organic group represented by the above formula (E), and Y represents a divalent organic group represented by the above formula (G). <5> <1> ~ <4> 13. An insulating film forming material comprising the polyimide resin according to any one of claims 1 to 12. <6> (B) Further containing a solvent <5> The insulating film forming material according to claim 1 . <7> For forming insulating film by hybrid bonding <5> or <6> The insulating film forming material according to claim 1 . <8> <5> ~ <7> 13. A method for manufacturing a semiconductor device, comprising the steps of: forming at least one of a first organic insulating film and a second organic insulating film using the insulating film forming material according to claim 12; and bonding the first organic insulating film and the second organic insulating film together. <9> forming a first electrode on a first substrate body and then forming a first organic insulating film around the first electrode to prepare a first semiconductor substrate having the first organic insulating film and the first electrode provided on one surface of the first substrate body; forming a second electrode on a second substrate body and then forming a second organic insulating film around the second electrode to prepare a second semiconductor substrate having the second organic insulating film and the second electrode provided on one surface of the second substrate body; singulating the second semiconductor substrate to obtain a plurality of semiconductor chips; a step of bonding the first organic insulating film of the first semiconductor substrate and the second organic insulating film of the semiconductor chip to each other and joining the first electrode of the first semiconductor substrate to the second electrode of the semiconductor chip; Includes <8> A method for manufacturing the semiconductor device according to claim 1. <10> a first semiconductor substrate having a first substrate body, the first organic insulating film and a first electrode provided on one surface of the first substrate body; a semiconductor chip having a semiconductor chip substrate body and a second organic insulating film and a second electrode provided on one surface of the semiconductor chip substrate body; the first organic insulating film of the first semiconductor substrate and the second organic insulating film of the semiconductor chip are bonded to each other, and the first electrode of the first semiconductor substrate and the second electrode of the semiconductor chip are bonded to each other, At least one of the first organic insulating film and the second organic insulating film is <5> ~ <7> 13. A semiconductor device comprising an organic insulating film formed by curing the insulating film forming material according to any one of claims 1 to 22. Effect of the Invention

[0018] According to the present disclosure, it is possible to provide a polyimide resin having excellent solubility in a solvent and excellent insulation reliability, an insulating film-forming material containing the polyimide resin, a method for manufacturing a semiconductor device using the insulating film-forming material, and a semiconductor device including an insulating film formed from the insulating film-forming material. [Brief description of the drawings]

[0019] [Figure 1] FIG. 1 is a cross-sectional view that illustrates an example of a semiconductor device manufactured by a method for manufacturing a semiconductor device according to an embodiment of the present invention. [Diagram 2] 2A to 2C are diagrams sequentially showing a method for manufacturing the semiconductor device shown in FIG. [Diagram 3] FIG. 3 is a diagram showing in more detail the bonding method in the method for manufacturing the semiconductor device shown in FIG. [Figure 4] 4A to 4C are views showing a method for manufacturing the semiconductor device shown in FIG. 1, sequentially illustrating steps subsequent to the step shown in FIG. [Diagram 5] FIG. 5 is a diagram showing an example in which the method for manufacturing a semiconductor device according to an embodiment of the present invention is applied to Chip-to-Wafer (C2W). [Figure 6] FIG. 2A is a top view showing the samples produced in the examples and comparative examples, and FIG. 2B is a cross-sectional view taken along line AA in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Hereinafter, the embodiments for carrying out the present disclosure will be described in detail. However, the present disclosure is not limited to the following embodiments. In the following embodiments, the components (including element steps, etc.) are not essential unless otherwise specified. The same applies to the numerical values ​​and their ranges, and do not limit the present disclosure.

[0021] In the present disclosure, "A or B" may include either A or B, or may include both. In the present disclosure, the term "step" includes not only a step that is independent of other steps, but also a step that cannot be clearly distinguished from other steps as long as the purpose of the step is achieved. In the present disclosure, a numerical range indicated using "~" includes the numerical values ​​before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in the present disclosure in stages, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value of the numerical range may be replaced with a value shown in the examples. In the present disclosure, each component may contain multiple types of corresponding substances. When multiple types of substances corresponding to each component are present in the composition, the content or amount of each component means the total content or amount of the multiple substances present in the composition, unless otherwise specified. In the present disclosure, the terms "layer" and "film" include cases where the layer or film is formed over the entire area when the area in which the layer or film is present is observed, as well as cases where the layer or film is formed over only a portion of the area. In the present disclosure, the term "insulating film" is a concept that also encompasses an insulating layer. In the present disclosure, when a functional group has a substituent, the number of carbon atoms in the functional group means the total number of carbon atoms including the number of carbon atoms in the substituent. When an embodiment of the present disclosure is described with reference to the drawings, the configuration of the embodiment is not limited to the configuration shown in the drawings. In addition, the size of the members in each drawing is conceptual, and the relative relationship between the sizes of the members is not limited to this.

[0022] <Polyimide resin> The polyimide resin of the present disclosure (hereinafter also referred to as "component (A)") contains a structure represented by the following formula (E) and a structure represented by the following formula (G).

[0023] [ka]

[0024] [ka]

[0025] In formula (E), C is a divalent linking group containing an ether bond, and in formula (G), D is a divalent linking group having two or more atoms linked to the main chain, and the proportion of m-bonds contained in formula (G) is greater than 0%.

[0026] The component (A) has excellent solubility in a solvent and excellent insulating reliability. The reason for this is presumed to be as follows. However, the following presumption is not intended to limit the insulating film-forming material of the present disclosure, but is merely an example. Since component (A) contains the structure represented by formula (E) and the structure represented by formula (G), which are relatively flexible skeletons, the solubility in a solvent is improved. Furthermore, by using component (A) as the base polymer of the insulating material, the imidization rate in low-temperature curing is improved, and as a result, the insulating reliability of the insulating film is improved.

[0027] In addition, it is preferable that the component (A) does not have a carboxyl group in the molecule, which, unlike polyamic acids that have a carboxyl group in the molecule, results in excellent storage stability at room temperature and further improved insulation reliability.

[0028] The component (A) is used, for example, in an insulating film forming material, which is a material used to form an insulating film. The component (A) may be used for purposes other than forming an insulating film.

[0029] The component (A) preferably has a structural unit represented by the following general formula (1): This tends to provide a semiconductor device equipped with an insulating film that exhibits high reliability.

[0030] [ka]

[0031] In the general formula (1), X represents a tetravalent organic group represented by the above formula (E), and Y represents a divalent organic group represented by the above formula (G). The component (A) may have a plurality of structural units represented by the above general formula (1), and X and Y in the plurality of structural units may be the same or different. The component (A) may or may not contain a structural unit in which X is a tetravalent organic group having a structure other than that of formula (E). The component (A) may or may not contain a structural unit in which Y is a divalent organic group having a structure other than that of formula (G).

[0032] In general formula (1), the tetravalent organic group represented by X preferably has 12 to 40 carbon atoms, more preferably 12 to 35 carbon atoms, and even more preferably 12 to 30 carbon atoms. In X, each benzene ring in formula (E) may have a substituent or may be unsubstituted. Examples of the substituent on the aromatic ring include an alkyl group, a fluorine atom, a halogenated alkyl group, a hydroxyl group, and an amino group. In formula (E), two adjacent benzene rings may be linked at two positions by at least one of a single bond and a linking group via a divalent linking group containing an ether bond (C in formula (E)), thereby forming a 5- or 6-membered ring containing the linking group between the two benzene rings.

[0033] Examples of the structure represented by formula (E) include a structure containing an ether bond (-O-) and a phenylene group, a structure which is an ether bond (-O-), and a structure containing an ether bond and an alkylene group.

[0034] Examples of the structure represented by formula (E) include groups represented by the following formulae (I) to (O).

[0035] [ka]

[0036] Examples of the structure containing an ether bond (-O-) and a phenylene group include the groups represented by the above formulae (J) to (O). An example of the structure which is an ether bond (-O-) is the group represented by the above formula (I).

[0037] Examples of the structure containing an ether bond and an alkylene group include groups represented by the following formulae (P) to (R).

[0038] [ka]

[0039] In general formula (1), the divalent organic group represented by Y preferably has 4 to 25 carbon atoms, more preferably 6 to 20 carbon atoms, and further preferably 12 to 18 carbon atoms. The divalent organic group represented by Y has a structure represented by formula (G). The structure represented by formula (G) is a structure in which two aromatic rings are bonded to a main chain via a divalent linking group (D in formula (G)) in which two or more atoms are linked, and the proportion of m-bonds contained in formula (G) is greater than 0%. The proportion of m-bonds contained in formula (G) may be 50% to 100%, or may be 100%. The proportion of m-bonds means the proportion of the number of aromatic rings substituted at the m-position (meta position) to the total number of aromatic rings contained in formula (G), and preferably means the proportion of the number of aromatic rings which constitute the main chain and are substituted at the m-position (meta position) to the total number of aromatic rings which constitute the main chain in formula (G).

[0040] From the viewpoints of the heat resistance of the polyimide resin and the solubility of the polyimide resin in a solvent, D in formula (G) preferably contains an aromatic ring and an ether bond, and is more preferably a group represented by the following formula (G1).

[0041] [ka]

[0042] The content of the structural unit represented by general formula (1) in component (A) is preferably 60 mol% or more, more preferably 70 mol% or more, and even more preferably 80 mol% or more, based on the total structural units. The upper limit of the content is not particularly limited, and may be 100 mol%.

[0043] The component (A) may be synthesized using a tetracarboxylic dianhydride and a diamine compound. In this case, in the general formula (1), X corresponds to a residue derived from the tetracarboxylic dianhydride, and Y corresponds to a residue derived from the diamine compound. The component (A) may be synthesized using a tetracarboxylic acid instead of the tetracarboxylic dianhydride.

[0044] There are no particular limitations on the molecular weight of the component (A), and for example, the weight average molecular weight is preferably 10,000 to 200,000, and more preferably 10,000 to 100,000. The weight average molecular weight can be measured, for example, by gel permeation chromatography, and can be calculated using a standard polystyrene calibration curve.

[0045] Component (A) may have a nonvolatile crosslinking group at the end of the main chain. The nonvolatile crosslinking group is a functional group capable of crosslinking reaction that is located at the end of the main chain of component (A) and does not volatilize due to heating, drying, etc. The nonvolatile crosslinking group may be a functional group containing an unsaturated double bond.

[0046] Examples of compounds used to form a nonvolatile crosslinking group at the main chain end of component (A) (hereinafter also referred to as a nonvolatile crosslinking group forming compound) include maleic anhydride, 5-norbornene-2,3-dicarboxylic anhydride, itaconic anhydride, methacrylic anhydride, 2-isocyanatoethyl methacrylate, 2-isocyanatoethyl acrylate, 4-ethynylphthalic anhydride, 4-vinylphthalic anhydride, di-t-butyl dicarbonate, etc. These compounds react with amino groups derived from diamine compounds to obtain compounds having a nonvolatile crosslinking group at the main chain end. The non-volatile crosslinking group-forming compounds may be used alone or in combination of two or more.

[0047] <Insulating film forming materials> The insulating film forming material of the present disclosure includes the polyimide resin of the present disclosure. The insulating film forming material of the present disclosure is a material used for forming an insulating film, and the use of the insulating film to be produced is not particularly limited, and it can be applied to uses that require insulating properties. For example, the insulating film forming material of the present disclosure may be a material for forming an insulating film by hybrid bonding.

[0048] The insulating film forming material of the present disclosure is used for W2W (Wafer-to-Wafer) bonding, C2W (Chip-to-Wafer) bonding, When insulating films are bonded to each other for hybrid bonding, it is sufficient that at least one of the insulating films is formed from the insulating film forming material of the present disclosure, and it is preferable that both insulating films are formed from the insulating film forming material of the present disclosure.

[0049] Furthermore, the insulating film obtained by curing the insulating film forming material of the present disclosure has a lower elastic modulus and is softer than a molded product made of an inorganic material. Therefore, when insulating films are bonded together, even if a foreign substance or the like is present on the surface of one insulating film (hereinafter also referred to as a "first insulating film") or the surface of the other insulating film (hereinafter also referred to as a "second insulating film"), the insulating film at the bonding interface tends to easily deform and the foreign substance can be contained within the insulating film without generating a large void in the insulating film.

[0050] The glass transition temperature of the insulating film obtained by curing the insulating film-forming material of the present disclosure is preferably 100°C to 400°C, and more preferably 150°C to 350°C, from the viewpoint of bonding at low temperatures.

[0051] The glass transition temperature of an insulating film is measured as follows. First, an insulating film is obtained by heating an insulating film forming material for 2 hours in a nitrogen atmosphere at a predetermined curing temperature (for example, 150°C to 375°C) at which a curing reaction can be performed. The obtained insulating film is cut to prepare a rectangular parallelepiped of 5 mm x 50 mm x 3 mm, and dynamic viscoelasticity is measured in a temperature range of 50°C to 350°C using a tensile tool in a dynamic viscoelasticity measuring device (for example, RSA-G2 manufactured by TA Instruments) under the conditions of a frequency of 1 Hz and a heating rate of 5°C / min. The glass transition temperature (Tg) is the temperature at the peak top part in tan δ obtained from the ratio of the storage elastic modulus and loss elastic modulus obtained by the above method.

[0052] The insulating film forming material of the present disclosure has a thermal expansion coefficient of 150 ppm / K or less when cured, more preferably 100 ppm / K or less, and even more preferably 70 ppm / K or less. This makes the thermal expansion coefficient of the insulating film, which is the cured product, equal to or close to that of the electrode, so that even if heat is generated during use of the semiconductor device, damage to the semiconductor device due to the difference in thermal expansion coefficient between the insulating film and the electrode can be suppressed. The thermal expansion coefficient is the rate at which the length of the insulating film expands due to a temperature rise per temperature, and can be calculated by measuring the change in the length of the insulating film at 100°C to 150°C using a thermomechanical analyzer or the like.

[0053] ((B) Solvent) The insulating film forming material of the present disclosure may contain a (B) solvent (hereinafter also referred to as "component (B)"). The component (B) preferably contains at least one selected from the group consisting of compounds represented by the following formulas (3) to (10). The component (B) may be used alone or in combination of two or more types.

[0054] [ka]

[0055] [ka]

[0056] In formulas (3) to (10), R 1 , R 2 , R 8 , R 10 , R 11 , R 13 and R 14 are each independently an alkyl group having 1 to 4 carbon atoms; R 3 ~R 7 , R 9 and R 12 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. s is an integer of 0 to 8, t is an integer of 0 to 4, r is an integer of 0 to 4, u is an integer of 0 to 3, v is an integer of 0 to 3, w is an integer of 0 to 4, and x is an integer of 0 to 5.

[0057] In formula (3), s is preferably 0. In formula (4), R 2 The alkyl group having 1 to 4 carbon atoms is preferably a methyl group or an ethyl group. t is preferably 0, 1 or 2, and more preferably 1. In formula (5), R 3 The alkyl group having 1 to 4 carbon atoms is preferably a methyl group, an ethyl group, a propyl group, or a butyl group. 4 and R 5 The alkyl group having 1 to 4 carbon atoms is preferably a methyl group or an ethyl group. In formula (6), R 6 ~R 8 The alkyl group having 1 to 4 carbon atoms is preferably a methyl group or an ethyl group. r is preferably 0 or 1, and more preferably 0. In formula (7), R 9 and R 10 The alkyl group having 1 to 4 carbon atoms is preferably a methyl group or an ethyl group. u is preferably 0 or 1, and more preferably 0. In formula (8), R 11The alkyl group having 1 to 4 carbon atoms is preferably a methyl group or an ethyl group. u is preferably 0 or 1, and more preferably 0. In formula (9), R 12 The alkyl group having 1 to 4 carbon atoms is preferably a methyl group or an ethyl group. 13 The alkyl group having 1 to 4 carbon atoms is preferably a methyl group or an ethyl group. w is preferably 0 or 1, and more preferably 0. In formula (10), R 14 The alkyl group having 1 to 4 carbon atoms is preferably a methyl group or an ethyl group. x is preferably 0 or 1, and more preferably 0.

[0058] Specific examples of the component (B) include the following compounds.

[0059] [ka] [ka]

[0060] In the insulating film forming material of the present disclosure, from the viewpoint of reducing toxicity such as reproductive toxicity, the content of N-methyl-2-pyrrolidone (NMP) may be 1 mass % or less based on the total amount of the insulating film forming material, and may be 3 mass % or less based on the total amount of the component (A).

[0061] In the insulating film forming material of the present disclosure, the content of the component (B) is preferably 1 to 10,000 parts by mass, and more preferably 50 to 10,000 parts by mass, per 100 parts by mass of the component (A).

[0062] The insulating film forming material of the present disclosure may contain a resin component other than component (A). From the viewpoint of heat resistance, examples of the resin component other than component (A) include polyimide precursors such as polyamic acid, polyamic acid ester, polyamic acid salt, and polyamic acid amide, polyimide resins other than the polyimide resins of the present disclosure (other polyimide resins), novolac resins, acrylic resins, polyether nitrile resins, polyether sulfone resins, epoxy resins, polyethylene terephthalate resins, polyethylene naphthalate resins, and polyvinyl chloride resins. The resin components other than the component (A) may be used alone or in combination of two or more.

[0063] In the insulating film forming material of the present disclosure, the content of component (A) relative to the total amount of resin components is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 100% by mass, and even more preferably 90% by mass to 100% by mass.

[0064] When the insulating film-forming material of the present disclosure contains a resin component other than the component (A) (e.g., a polyimide precursor), the ratio of the resin component other than the component (A) (e.g., a polyimide precursor) to the total of the component (A) and the resin component other than the component (A) may be 15% by mass to 50% by mass, or may be 10% by mass to 20% by mass.

[0065] The insulating film forming material of the present disclosure may or may not contain a resin component such as a cyclic olefin resin such as benzocyclobutene, an epoxy resin, etc. From the viewpoint of obtaining an insulating film with superior heat resistance and mechanical properties, and from the viewpoint of suitably suppressing poor bonding between an insulating film and an electrode and poor bonding between insulating films when performing hybrid bonding, the content of the cyclic olefin resin and the content of the epoxy resin are each independently preferably 30% by mass or less, more preferably 0% by mass to 10% by mass, and even more preferably 0% by mass to 5% by mass, based on the total amount of the insulating film forming material of the present disclosure.

[0066] The insulating film forming material of the present disclosure may contain, as necessary, at least one of a polymerizable monomer, a photopolymerization initiator, a thermal polymerization initiator, a polymerization inhibitor, an antioxidant, a coupling agent, a surfactant, a leveling agent, a rust inhibitor, a nitrogen-containing compound, or a dicarboxylic acid.

[0067] The method for preparing the insulating film forming material of the present disclosure is not particularly limited, and may be any method that involves mixing the above-mentioned components.

[0068] <Semiconductor device> The semiconductor device of the present disclosure comprises a first substrate body, a first semiconductor substrate having the first organic insulating film and a first electrode provided on one surface of the first substrate body, a semiconductor chip substrate body, and a semiconductor chip having a second organic insulating film and a second electrode provided on one surface of the semiconductor chip substrate body, wherein the first organic insulating film of the first semiconductor substrate and the second organic insulating film of the semiconductor chip are bonded together, the first electrode of the first semiconductor substrate and the second electrode of the semiconductor chip are bonded together, and at least one of the first organic insulating film and the second organic insulating film is an insulating film formed by hardening the insulating film forming material of the present disclosure. The semiconductor device of the present disclosure has excellent insulation reliability because at least one of the first organic insulating film and the second organic insulating film is an insulating film formed by curing the insulating film forming material of the present disclosure. Moreover, the semiconductor device of the present disclosure can be manufactured, for example, by the manufacturing method of a semiconductor device described below.

[0069] <Method of Manufacturing Semiconductor Device> The method for manufacturing a semiconductor device according to the present disclosure includes forming at least one of a first organic insulating film and a second organic insulating film using the insulating film forming material according to the present disclosure, and bonding the first organic insulating film and the second organic insulating film together. More specifically, the semiconductor device can be manufactured through the following steps (1) to (5). Step (1) A first semiconductor substrate is prepared, the first semiconductor substrate having a first substrate body, and the first organic insulating film and a first electrode provided on one surface of the first substrate body. Step (2) A second semiconductor substrate is prepared, the second semiconductor substrate having a second substrate body, and the second organic insulating film and a plurality of second electrodes provided on one surface of the second substrate body. Step (3): The second semiconductor substrate is diced into individual semiconductor chips, each of which includes the second organic insulating film and at least one of the second electrodes. Step (4): The first organic insulating film of the first semiconductor substrate and the second organic insulating film of the semiconductor chip are bonded to each other. Step (5): The first electrode of the first semiconductor substrate and the second electrode of the semiconductor chip are bonded to each other.

[0070] In the step (1), the first semiconductor substrate may be prepared by forming a first electrode on a first substrate body and then forming a first organic insulating film around the first electrode. In the step (1), the second semiconductor substrate may be prepared by forming a second electrode on the second substrate body and then forming a second organic insulating film around the second electrode.

[0071] Hereinafter, an embodiment of the semiconductor device of the present disclosure and an embodiment of the manufacturing method of the semiconductor device of the present disclosure will be described in detail with reference to the drawings. In the following description, the same or corresponding parts are given the same reference numerals, and duplicated descriptions will be omitted. Furthermore, unless otherwise specified, the positional relationships such as up, down, left, and right are based on the positional relationships shown in the drawings. Furthermore, the dimensional ratios of the drawings are not limited to the ratios shown in the drawings.

[0072] (An example of a semiconductor device) Fig. 1 is a cross-sectional view showing a schematic example of a semiconductor device according to the present disclosure. As shown in Fig. 1, the semiconductor device 1 is, for example, an example of a semiconductor package, and includes a first semiconductor chip 10 (a first semiconductor substrate), a second semiconductor chip 20 (a semiconductor chip), a pillar portion 30, a redistribution layer 40, a substrate 50, and a circuit substrate 60.

[0073] The first semiconductor chip 10 is a semiconductor chip such as an LSI (large-scale integrated circuit) chip or a CMOS (Complementary Metal Oxide Semiconductor) sensor, and has a three-dimensional mounting structure in which the second semiconductor chip 20 is mounted downward. The second semiconductor chip 20 is a semiconductor chip such as an LSI or memory, and is a chip component having a smaller area in a plan view than the first semiconductor chip 10. The second semiconductor chip 20 is bonded to the back surface of the first semiconductor chip 10 by chip-to-chip (C2C) bonding. The first semiconductor chip 10 and the second semiconductor chip 20 are finely bonded to each other by hybrid bonding, the details of which will be described later, with the respective terminal electrodes and the insulating films around them being firmly bonded to each other without misalignment.

[0074] The pillar portion 30 is a connection portion in which a plurality of pillars 31 formed of a metal such as copper (Cu) are sealed with a resin 32. The plurality of pillars 31 are conductive members extending from the upper surface of the pillar portion 30 to the lower surface. The plurality of pillars 31 may have a cylindrical shape with a diameter of, for example, 3 μm to 20 μm (for example, a diameter of 5 μm), and may be arranged so that the center-to-center distance between each pillar 31 is 15 μm or less. The plurality of pillars 31 flip-chip connect the lower terminal electrode of the first semiconductor chip 10 and the upper terminal electrode of the rewiring layer 40. By using the pillar portion 30, the semiconductor device 1 can form a connection electrode without using a technique called TMV (Through mold via), which is a technique of drilling holes in a mold and soldering the mold. The pillar portion 30 has a thickness approximately the same as that of the second semiconductor chip 20, for example, and is arranged on the side of the second semiconductor chip 20 in the horizontal direction. In addition, multiple solder balls may be arranged instead of the pillar portion 30, and the lower terminal electrode of the first semiconductor chip 10 and the upper terminal electrode of the redistribution layer 40 may be electrically connected by the solder balls.

[0075] The rewiring layer 40 is a wiring layer having a terminal pitch conversion function, which is a function of the package substrate, and is a layer in which a rewiring pattern is formed of polyimide, copper wiring, etc. on the insulating film on the lower side of the second semiconductor chip 20 and on the lower surface of the pillar portion 30. The rewiring layer 40 is formed in a state in which the first semiconductor chip 10 (first semiconductor substrate 100), the second semiconductor chip 20, etc. are turned upside down (see (d) of FIG. 4).

[0076] The rewiring layer 40 electrically connects the terminal electrodes on the underside of the second semiconductor chip 20 and the terminal electrodes of the first semiconductor chip 10 via the pillar parts 30 to the terminal electrodes of the substrate 50. The terminal pitch of the substrate 50 is wider than the terminal pitch of the pillars 31 and the terminal pitch of the second semiconductor chip 20. Various electronic components 51 may be mounted on the substrate 50. Furthermore, when there is a large difference between the terminal pitches of the rewiring layer 40 and the substrate 50, an inorganic interposer or the like may be used between the rewiring layer 40 and the substrate 50 to electrically connect the rewiring layer 40 and the substrate 50.

[0077] The circuit board 60 is a board on which the first semiconductor chip 10 and the second semiconductor chip 20 are mounted, and has a plurality of through electrodes therein electrically connected to a board 50 connected to the first semiconductor chip 10, the second semiconductor chip 20, and electronic components 51, etc. In the circuit board 60, the terminal electrodes of the first semiconductor chip 10 and the second semiconductor chip 20 are electrically connected to terminal electrodes 61 provided on the rear surface of the circuit board 60 by the plurality of through electrodes.

[0078] (An example of a manufacturing method for a semiconductor device) Next, an example of a method for manufacturing the semiconductor device 1 will be described with reference to Fig. 2 to Fig. 4. Fig. 2 is a diagram sequentially showing a method for manufacturing the semiconductor device shown in Fig. 1. Fig. 3 is a diagram showing in more detail a bonding method (hybrid bonding) in the method for manufacturing the semiconductor device shown in Fig. 2. Fig. 4 is a diagram sequentially showing steps subsequent to the steps shown in Fig. 2 in the method for manufacturing the semiconductor device shown in Fig. 1.

[0079] The semiconductor device 1 can be manufactured, for example, through the following steps (a) to (n). (a) A step of preparing a first semiconductor substrate 100 corresponding to a first semiconductor chip 10. (b) A step of preparing a second semiconductor substrate 200 corresponding to the second semiconductor chip 20. (c) A process of polishing the surface 101a of the first semiconductor substrate 100 using a polishing method such as a CMP method or polishing using a surface planer so that each surface 103a of the terminal electrodes 103 is at the same position or protrudes from the surface 102a of the insulating film 102 (see (a) of Figure 3). (d) A process of polishing the surface 201a of the second semiconductor substrate 200 using a polishing method such as a CMP method or polishing using a surface planer so that each surface 203a of the terminal electrodes 203 is at the same position or protrudes from the surface 202a of the insulating film 202 (see (a) of Figure 3). (e) As shown in FIG. 2(b), a step of dicing the second semiconductor substrate 200 to obtain a plurality of semiconductor chips 205. (f) A step of aligning the terminal electrodes 203 of each of the multiple semiconductor chips 205 with the terminal electrodes 103 of the first semiconductor substrate 100 as shown in (c) of FIG. (g) A step of bonding the insulating film 102 of the first semiconductor substrate 100 and each insulating film 202b of the multiple semiconductor chips 205 to each other (see FIG. 2(d) and FIG. 3(b)). At this time, heat H, pressure, or both may be applied. (h) A step of bonding the terminal electrodes 103 of the first semiconductor substrate 100 to the terminal electrodes 203 of each of the plurality of semiconductor chips 205 (see FIG. 3(c)). (i) A step of forming a plurality of pillars 300 (corresponding to pillars 31) between a plurality of semiconductor chips 205 on the connection surface of the first semiconductor substrate 100 (see FIG. 4(a)). (j) A step of molding a resin 301 onto the connection surface of the first semiconductor substrate 100 so as to cover the semiconductor chip 205 and the pillars 300 to obtain a semi-finished product M1 (see FIG. 4(b)). (k) A process of obtaining a semi-finished product M2 by grinding and thinning the resin 301 side of the semi-finished product M1 molded in the process (j) (see FIG. 4(c)). (l) A step of forming a wiring layer 400 corresponding to the rewiring layer 40 on the semi-finished product M2 thinned in the step (k) (see FIG. 4(d)). (m) A step of cutting the semi-finished product M3 on which the wiring layer 400 has been formed in the step (l) along the cutting lines A so as to obtain individual semiconductor devices 1 (see FIG. 4(d)). (n) A step of inverting the semiconductor device 1a individualized in the step (m) and placing it on the substrate 50 and the circuit board 60 (see FIG. 1).

[0080] For example, in the method for manufacturing a semiconductor device of the present disclosure, step (1) corresponds to the above-mentioned steps (a) and (c), step (2) corresponds to the above-mentioned steps (b) and (d), step (3) corresponds to step (e), step (4) corresponds to step (g), and step (5) corresponds to step (h). Furthermore, the insulating film forming material of the present disclosure may be an insulating film forming material for use in producing at least one of the first organic insulating film and the second organic insulating film in the method for manufacturing a semiconductor device.

[0081] Step (a) is a step of preparing a first semiconductor substrate 100, which is a silicon substrate on which an integrated circuit composed of semiconductor elements and wiring connecting them is formed, corresponding to a plurality of first semiconductor chips 10. In step (a), as shown in FIG. 2(a), a plurality of terminal electrodes 103 (first electrodes) made of copper, aluminum, etc. are provided at predetermined intervals on one surface 101a of a first substrate body 101 made of silicon, etc., and an insulating film 102 (first insulating film) which is a cured product obtained by curing an insulating film forming material of the present disclosure is provided. When the insulating film forming material is a photosensitive material such as a negative-type photosensitive insulating film forming material or a positive-type photosensitive insulating film forming material, the insulating film 102 may be provided on the one surface 101a of the first substrate body 101 before providing the plurality of terminal electrodes 103, or the insulating film 102 may be provided on the one surface 101a of the first substrate body 101 before providing the plurality of terminal electrodes 103. When the insulating film forming material is a non-photosensitive material, the insulating film 102 may be provided after the terminal electrodes 103 are provided on the first surface 101a of the first substrate body 101.

[0082] Step (b) is a step of preparing a second semiconductor substrate 200, which is a silicon substrate on which an integrated circuit having semiconductor elements and wiring connecting them is formed, corresponding to a plurality of second semiconductor chips 20. In step (b), as shown in (a) of FIG. 2, a plurality of terminal electrodes 203 (a plurality of second electrodes) made of copper, aluminum, or the like are continuously provided on one surface 201a of a second substrate body 201 made of silicon or the like, and an insulating film 202 (a second insulating film) which is a cured product obtained by curing an insulating film forming material of the present disclosure is provided. When the insulating film forming material is a photosensitive material such as a negative-type photosensitive insulating film forming material or a positive-type photosensitive insulating film forming material, the insulating film 202 may be provided on the one surface 201a of the second substrate body 201 before the plurality of terminal electrodes 203 are provided, or the insulating film 202 may be provided on the one surface 201a of the second substrate body 201 before the plurality of terminal electrodes 203 are provided. When the insulating film forming material is a non-photosensitive material, the insulating film 202 may be provided after the multiple terminal electrodes 203 are provided on the one surface 201a of the second substrate main body 201.

[0083] The insulating films 102 and 202 used in steps (a) and (b) are not limited to a configuration in which both are cured products obtained by curing the insulating film-forming material of the present disclosure, and at least one of the insulating films 102 and 202 may be a cured product obtained by curing the insulating film-forming material of the present disclosure.

[0084] In addition, although FIG. 1 shows an example of C2C bonding, the Chip-to-Wafer (C The present invention may be applied to bonding in a C2W process. In the C2W process, a semiconductor wafer 410 (first semiconductor substrate) is prepared, which has a substrate body 411 (first substrate body), an insulating film 412 (first insulating film) provided on one surface of the substrate body 411, and a plurality of terminal electrodes 413 (first electrodes). Furthermore, a semiconductor substrate (second semiconductor substrate) is prepared, which has a substrate body 421 (second substrate body), an insulating film 422 (second insulating film) provided on one surface of the substrate body 421, and a plurality of terminal electrodes 423 (second electrodes). Then, one surface of the semiconductor wafer 410 and one surface of the second semiconductor substrate before being singulated into the semiconductor chips 420 are polished by a polishing method such as a CMP method or polishing using a surface planer, as in the above steps (c) and (d). Thereafter, a singulation process similar to that in step (e) is performed on the second semiconductor substrate, and a plurality of semiconductor chips 420 are obtained.

[0085] 5(a), the terminal electrodes 423 of the semiconductor chip 420 are aligned with the terminal electrodes 413 of the semiconductor wafer 410 (step (f)). Then, the insulating film 412 of the semiconductor wafer 410 and the insulating film 422 of the semiconductor chip 420 are attached to each other (step (g)), and the terminal electrodes 413 of the semiconductor wafer 410 and the terminal electrodes 423 of the semiconductor chip 420 are bonded to each other (step (h)), to obtain a semi-finished product shown in FIG. 5(b). As a result, the insulating film 412 and the insulating film 422 are bonded to each other to form an insulating bonded portion S3, and the semiconductor chip 420 is attached to the semiconductor wafer 410 mechanically and with high accuracy. Also, the terminal electrodes 413 and the corresponding terminal electrodes 423 are bonded to each other to form an electrode bonded portion S4, and the terminal electrodes 413 and 423 are bonded to each other mechanically and electrically.

[0086] In step (h), as shown in FIG. 2(d), after the bonding in step (g) is completed, heat H, pressure, or both are applied to bond the terminal electrode 103 of the first semiconductor substrate 100 to each of the terminal electrodes 203 of the semiconductor chips 205 as hybrid bonding (see FIG. 3(c)). When the terminal electrodes 103 and 203 are made of copper, the annealing temperature in step (g) is preferably 150° C. or higher and 400° C. or lower, and more preferably 200° C. or higher and 300° C. or lower. In particular, by using the insulating film forming material of the present disclosure, it is possible to set the annealing temperature low. By such bonding process, the terminal electrode 103 and the corresponding terminal electrode 203 are bonded to form an electrode bonding portion S2, and the terminal electrode 103 and the terminal electrode 203 are mechanically and electrically firmly bonded to each other. The electrode bonding in step (h) may be performed after the bonding in step (g) or may be performed simultaneously with the bonding in step (g).

[0087] 5(c) and 5(d), a plurality of semiconductor chips 420 are bonded to a semiconductor wafer 410, which is a semiconductor wafer, in a similar manner to obtain a semiconductor device 401. Note that the plurality of semiconductor chips 420 may be bonded to the semiconductor wafer 410 one by one by hybrid bonding, or may be bonded to the semiconductor wafer 410 collectively by hybrid bonding.

[0088] In the manufacturing method of such a semiconductor device 401, at least one of the insulating film 412 of the semiconductor wafer 410 and the insulating film 422 of the semiconductor chip 420 is an insulating film that is a cured product obtained by curing the insulating film forming material of the present disclosure, as in the manufacturing method of the above-mentioned semiconductor device 1. Therefore, a semiconductor device provided with an insulating film having excellent insulating reliability can be obtained.

[0089] (Modification) In the semiconductor device and the method for manufacturing the semiconductor device according to the present disclosure, a configuration in which the first electrode and the second electrode are joined has been described, but the present invention is not limited to this configuration. For example, in the semiconductor device of the present disclosure, the first electrode and the second electrode may be through electrodes that penetrate the first semiconductor substrate and the second semiconductor substrate. The method for manufacturing a semiconductor device according to the present disclosure may be, for example, a method for manufacturing a semiconductor device by using the insulating film forming material according to the present disclosure in forming at least one of a first organic insulating film and a second organic insulating film, and by carrying out the following steps (1)' to (5)'. Step (1)' A first semiconductor substrate is prepared, the first semiconductor substrate having a first substrate body and the first organic insulating film provided on one surface of the first substrate body. Step (2)' A second semiconductor substrate is prepared, the second semiconductor substrate having a second substrate body and the second organic insulating film provided on one surface of the second substrate body. Step (3)' The second semiconductor substrate is divided into individual pieces to obtain a plurality of semiconductor chips each having the second organic insulating film. Step (4)' The first organic insulating film of the first semiconductor substrate and the second organic insulating film of the semiconductor chip are bonded to each other. Step (5)' A through hole is provided in a part of the bonded first semiconductor substrate and second semiconductor substrate, and a through electrode is provided in the through hole. In the above (5)', the method for providing the through holes and the method for providing the through electrodes are not particularly limited. For example, the through holes may be provided by etching or the like, and the through electrodes may be provided by electrolytic plating, electroless plating, sputtering or the like. EXAMPLES

[0090] The present disclosure will be described in more detail below with reference to examples and comparative examples. Note that the present disclosure is not limited to the following examples.

[0091] (Synthesis Example 1 (Synthesis of A1)) 50g of 3,3',4,4'-biphenylethertetracarboxylic dianhydride (ODPA) and 46g of 1,3-bis(3-aminophenoxy)benzene were dissolved in 640g of 3-methoxy-N,N-dimethylpropionamide. The resulting solution was stirred at 30°C for 2 hours to obtain polyamic acid. Then, 52g of pyridine and 34g of acetic anhydride were added to the resulting polyamic acid solution and heated at 45°C for 5h. This reaction solution was dropped into distilled water, and the precipitate was collected by filtration and dried under reduced pressure to obtain polyimide resin A1. The weight average molecular weight of A1 was determined by gel permeation chromatography (GPC) in terms of standard polystyrene. The weight average molecular weight of A1 was 27,000. Specifically, a solution in which 0.5 mg of A1 was dissolved in 1 mL of a solvent [tetrahydrofuran (THF) / dimethylformamide (DMF) = 1 / 1 (volume ratio)] was used, and the measurement was performed under the following conditions. (Measurement conditions) Measuring device: Shimadzu Corporation SPD-M20A Pump: Shimadzu Corporation LC-20AD Column oven: Shimadzu Corporation: CTO-20A Measurement conditions: Column Gelpack GL-S300MDT-5 x 2 Eluent: THF / DMF=1 / 1 (volume ratio) LiBr(0.03mol / L), H3PO4(0.06mol / L) Flow rate: 1.0 mL / min, detector: UV 270 nm, column temperature: 40°C Standard polystyrene: Calibration curves created using Tosoh TSKgel standard Polystyrene Types F-1, F-4, F-20, F-80, and A-2500

[0092] (Synthesis Example 2 (Synthesis of A2)) 82g of 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride (BPADA) and 46g of 1,3-bis(3-aminophenoxy)benzene were dissolved in 640g of 3-methoxy-N,N-dimethylpropionamide. The resulting solution was stirred at 30°C for 2 hours to obtain polyamic acid. Then, 52g of pyridine and 34g of acetic anhydride were added to the resulting polyamic acid solution and heated at 45°C for 5h. This reaction solution was dropped into distilled water, and the precipitate was collected by filtration and dried under reduced pressure to obtain polyimide resin A2. The weight average molecular weight of A2 was determined in the same manner as A1, using gel permeation chromatography (GPC) and standard polystyrene equivalent, and was found to be 25,000.

[0093] (Synthesis Example 3 (Synthesis of A3)) 49 g of 3,3',4,4'-biphenylethertetracarboxylic dianhydride (ODPA) and 27 g of 4,4'-diaminodiphenylether were dissolved in 640 g of 3-methoxy-N,N-dimethylpropionamide. The resulting solution was stirred at 30°C for 2 hours to obtain polyamic acid. Then, 52 g of pyridine and 34 g of acetic anhydride were added to the resulting polyamic acid solution and heated at 45°C for 5 hours. The precipitate was collected by filtration, washed, and dried under reduced pressure to obtain polyimide resin A3. The weight average molecular weight of A3 was determined in the same manner as A1, using gel permeation chromatography (GPC) and standard polystyrene equivalent, and was found to be 23,000.

[0094] (Synthesis Example 4 (Synthesis of A4)) 49g of 3,3',4,4'-biphenylethertetracarboxylic dianhydride (ODPA) and 42g of 1,4-bis(4-aminophenoxy)benzene were dissolved in 640g of 3-methoxy-N,N-dimethylpropionamide. The resulting solution was stirred at 30°C for 2 hours to obtain polyamic acid. Then, 52g of pyridine and 34g of acetic anhydride were added to the resulting polyamic acid solution and heated at 45°C for 5h. The precipitate was collected by filtration, washed, and dried under reduced pressure to obtain polyimide resin A4. The weight average molecular weight of A4 was determined in the same manner as A1, using gel permeation chromatography (GPC) and standard polystyrene equivalent, and was found to be 23,000.

[0095] (Synthesis Example 5 (Synthesis of A5)) 47 g of 3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA) and 42 g of 1,3-bis(3-aminophenoxy)benzene were dissolved in 640 g of 3-methoxy-N,N-dimethylpropionamide. The resulting solution was stirred at 30°C for 2 hours to obtain polyamic acid. The resulting solution was stirred at 30°C for 2 hours to obtain polyamic acid. Then, 52 g of pyridine and 34 g of acetic anhydride were added to the resulting polyamic acid solution and heated at 45°C for 5 hours. The precipitate was collected by filtration, washed, and dried under reduced pressure to obtain polyimide resin A5. The weight average molecular weight of A5 was determined in the same manner as A1, using gel permeation chromatography (GPC) and standard polystyrene equivalent, and was found to be 22,000.

[0096] (Synthesis Example 6 (Synthesis of A6)) 50g of 3,3',4,4'-biphenylethertetracarboxylic dianhydride (ODPA) and 46g of 1,3-bis(3-aminophenoxy)benzene were dissolved in 640g of 3-methoxy-N,N-dimethylpropionamide. The resulting solution was stirred at 30°C for 2 hours to obtain polyamic acid A6. This reaction solution was dropped into distilled water, and the precipitate was collected by filtration and dried under reduced pressure to obtain polyimide resin A6. The weight average molecular weight of A6 was determined in the same manner as A1 by gel permeation chromatography (GPC) using standard polystyrene standards, and was found to be 21,000.

[0097] [Examples 1 to 8, Comparative Examples 1 to 5] (Preparation of insulating film forming material) The insulating film-forming materials of Examples 1 to 8 and Comparative Examples 1 to 5 were prepared as follows using the components and blending amounts shown in Table 1. The blending amount of each component in Table 1 is in parts by mass. In addition, "-" in Table 1 means that the corresponding component is not blended. In each of the Examples and Comparative Examples, a mixture of each component was kneaded overnight at room temperature in a general solvent-resistant container, and then pressure filtered using a filter with a 0.2 μm pore size. The following evaluations were performed using the obtained insulating film-forming materials.

[0098] The components in Table 1 are as follows: Component (A) and other components A1 to A6: Polyimide resins A1 to A5 and polyamic acid A6 synthesized in the above Synthesis Examples 1 to 6 ·(B) Component B1: 3-Methoxy-N,N-dimethylpropionamide B2: γ-butyrolactone B3: Cyclohexanone B4: 1-Methylimidazole

[0099] [Evaluation of resin solubility] For the insulating film forming materials of Examples 1 to 8 and Comparative Examples 1 to 5, the case where no insoluble resin content was found in the insulating film forming material after preparation was rated as A, and the case where insoluble resin content was found in the insulating film forming material after preparation was rated as B. The results are shown in Table 1.

[0100] [Evaluation of imidization rate] For the insulating film forming materials of Examples 1 to 8 and Comparative Examples 1 to 5, the infrared absorption spectrum of the cured product after the curing reaction was performed under the conditions of 200° C. and 2 hours was measured, and the absorption peak of the imide structure (for example, the CN stretching vibration of the imide ring: 1370 cm -1 around 1500 cm) and absorption peaks due to aromatic rings (e.g., C=N stretching vibration of aromatic rings: 1500 cm -1 The intensity ratio of the two regions was calculated. For the insulating film forming materials of Examples 1 to 8 and Comparative Examples 1 to 5, the infrared absorption spectrum was also measured for the cured products after a curing reaction under conditions of 375°C and 1 hour, and the above-mentioned intensity ratio was calculated. The imidization rate was calculated from the intensity ratio at 200°C when the intensity ratio at 375°C was taken as 100%. When the calculated imidization rate was 90% or more, it was evaluated as A, and when the imidization rate was less than 90%, it was evaluated as B. The results are shown in Table 1.

[0101] [Evaluation of room temperature storage stability] The storage stability at room temperature was evaluated for the insulating film forming materials of Examples 1 to 8 and Comparative Examples 1 to 5. Specifically, each insulating film forming material was left at about 25° C. for 4 weeks, and evaluated for viscosity change. A case in which the viscosity change rate after 4 weeks from the initial viscosity was less than 10% was rated as A, a case in which it was 10% or more but less than 20% was rated as B, and a case in which it was 20% or more was rated as C. The results are shown in Table 1.

[0102] [Evaluation of insulation reliability] The insulation reliability of the insulating film was evaluated by the HAST (Highly Accelerated Temperature and Humidity Stress Test). After sputtering titanium and copper on one surface of a silicon wafer (Si substrate with SiO2 film) and polyimide as shown in FIG. 6, multiple copper electrodes were provided by electrolytic plating at intervals as shown in FIG. 6, and unnecessary sputtered layers were removed. An insulating film was prepared by hardening the insulating film forming material of each Example and Comparative Example between the electrodes under the following conditions. First, the insulating film forming material was spin-coated on the silicon wafer using a coating device spin coater, and a drying process was performed to form a resin film. The obtained resin film was exposed to light using a proximity exposure machine "Mask Aligner MA8" (manufactured by SUSS MicroTec Co., Ltd.) at an exposure amount such that the remaining film rate after development was about 80% or more. After that, the resin film was heated in a clean oven at 230°C for a predetermined time in a nitrogen atmosphere to harden it, thereby preparing an insulating film. Furthermore, the insulating film provided between the electrodes was treated for 300 hours under HAST conditions of 130°C, 85% RH, and 3.3 V, 5 V, or 10 V. Furthermore, under the HAST conditions, the insulation resistance value of the insulating film was observed after 100 hours or 300 hours, and the insulation reliability was evaluated in each example and comparative example. Insulation resistance value 1 e+6 If the measurement was less than 1 Ω once or less, the rating was A. If the test time was less than 300 hours, the insulation resistance value was 1 e+6 When less than Ω was observed twice or more, the rating was B. The results are shown in Table 1.

[0103] [Table 1]

[0104] As shown in Table 1, the evaluation results were good in Examples 1 to 8. On the other hand, in Comparative Examples 1 to 3, which used any of the polyimide resins A3 to A5, the solubility in the solvent was insufficient. Furthermore, in Comparative Examples 4 and 5, which used the polyamic acid A6, the room temperature stability and insulation reliability were insufficient. [Explanation of symbols]

[0105] Reference Signs List 1, 1a, 401...semiconductor device, 10...first semiconductor chip, 20...second semiconductor chip, 30...pillar portion, 40...rewiring layer, 50...substrate, 60...circuit board, 61...terminal electrode, 100...first semiconductor substrate, 101...first substrate body, 101a...one surface, 102...insulating film (first insulating film), 103...terminal electrode (first electrode), 103a...surface, 200...second semiconductor substrate, 201...second substrate body, 201a...one surface, 202...insulating film (second insulating film), 203...terminal electrode (second electrode), 203a...surface, 205 ...semiconductor chip, 300...pillar, 301...resin, 410...semiconductor wafer (first semiconductor substrate), 411...substrate body (first substrate body), 412...insulating film (first insulating film), 413...terminal electrode (first electrode), 420...semiconductor chip (second semiconductor substrate), 421...substrate body (second substrate body), 422...insulating film (second insulating film), 423...terminal electrode (second electrode), A...cutting line, H...heat, M1 to M3...semi-finished product, S1...insulating joint portion, S2...electrode joint portion, S3...insulating joint portion, S4...electrode joint portion.

Claims

1. A polyimide resin comprising a structure represented by the following formula (E) and a structure represented by the following formula (G). [Formula 1] [Case 2] In formula (E), C is a divalent linking group containing an ether bond, and in formula (G), D is a divalent linking group having two or more atoms linked to the main chain, and the proportion of m-bonds contained in formula (G) is greater than 0%.

2. The polyimide resin according to claim 1 , wherein D in the formula (G) contains an aromatic ring and an ether bond.

3. 2. The polyimide resin according to claim 1, wherein the structure represented by formula (E) is any one of the structures represented by formulas (I) to (O). [C3]

4. The polyimide resin according to claim 1, having a structural unit represented by the following general formula (1): [C4] In the general formula (1), X represents a tetravalent organic group represented by the formula (E) above, and Y represents a divalent organic group represented by the formula (G) above.

5. An insulating film forming material comprising the polyimide resin according to any one of claims 1 to 4.

6. The insulating film forming material according to claim 5 , further comprising (B) a solvent.

7. The insulating film forming material according to claim 5, for forming an insulating film by hybrid bonding.

8. A method for manufacturing a semiconductor device, comprising the steps of: forming at least one of a first organic insulating film and a second organic insulating film using the insulating film forming material according to claim 5; and bonding the first organic insulating film and the second organic insulating film together.

9. forming a first electrode on a first substrate body and then forming a first organic insulating film around the first electrode to prepare a first semiconductor substrate having the first organic insulating film and the first electrode provided on one surface of the first substrate body; forming a second electrode on a second substrate body and then forming a second organic insulating film around the second electrode to prepare a second semiconductor substrate having the second organic insulating film and the second electrode provided on one surface of the second substrate body; singulating the second semiconductor substrate to obtain a plurality of semiconductor chips; a step of bonding the first organic insulating film of the first semiconductor substrate and the second organic insulating film of the semiconductor chip to each other and joining the first electrode of the first semiconductor substrate to the second electrode of the semiconductor chip; The method for manufacturing a semiconductor device according to claim 8 , comprising:

10. a first semiconductor substrate having a first substrate body and the first organic insulating film and a first electrode provided on one surface of the first substrate body; a semiconductor chip having a semiconductor chip substrate body and a second organic insulating film and a second electrode provided on one surface of the semiconductor chip substrate body; the first organic insulating film of the first semiconductor substrate and the second organic insulating film of the semiconductor chip are bonded to each other, and the first electrode of the first semiconductor substrate and the second electrode of the semiconductor chip are bonded to each other, 6. A semiconductor device, wherein at least one of the first organic insulating film and the second organic insulating film is an organic insulating film formed by curing the insulating film forming material according to claim 5.

Citation Information

Patent Citations

  • Soluble polyimide

    JP2005272655A

  • Novel polyimide resin

    JP2007099842A

  • Resin composition, laminate, printed wiring board, and method of producing the same

    JP2015074660A

  • Polyimide, polyimide solution, resin film, polyimide composition, crosslinked polyimide, coverlay film, and circuit board

    JP2017145344A

  • Polyimide and photosensitive resin composition

    JP2018203959A