Oxime ester based photo-radical polymerization initiators
An oxime ester compound with an anthracene skeleton addresses the inefficiencies of existing photopolymerization initiators with UV-LEDs and laser diodes by providing high photosensitivity and controlled polymerization, enabling effective curing and pattern formation.
Patent Information
- Application Number
- JP2023063104
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-07
- Publication Date
- 2024-10-18
AI Technical Summary
Existing photopolymerization initiators are less effective with UV-LEDs and laser diodes due to their monochromatic light emission, leading to poor surface curing and oxygen inhibition, necessitating a high-activity initiator for these light sources.
Development of an oxime ester compound with an anthracene skeleton that absorbs light in the 350 nm to 420 nm range, generating active radical species for efficient polymerization, even with UV-LEDs and laser diodes.
The oxime ester compound with an anthracene skeleton exhibits high photosensitivity and radical polymerization ability, ensuring effective curing and preventing polymerization in unexposed areas, allowing precise pattern formation.
Smart Images

Figure 2024149305000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a photoradical polymerization initiator, and in particular to an oxime ester-based photoradical polymerization initiator. [Background technology]
[0002] Photopolymerizable compositions can be polymerized and cured by irradiation with light such as ultraviolet rays. This technology of curing with light is used in a variety of applications, such as paints for woodworking, coating materials for metals, inks for screen printing and offset printing, dry film resists used in electronic substrates, hologram materials, sealants, overcoat materials, resins for stereolithography, adhesives, etc.
[0003] This photopolymerizable composition is mainly composed of a polymerizable compound and a polymerization initiator that initiates polymerization of the polymerizable compound by light. Polymerization methods include radical polymerization, cationic polymerization, and anionic polymerization, of which radical polymerization has been used most widely for a long time. In the case of radical polymerization, a polymerizable compound and a photoradical polymerization initiator are used.
[0004] Photoradical polymerization initiators are classified into hydrogen abstraction type and intramolecular cleavage type. In the case of hydrogen abstraction type, the photoradical polymerization initiator absorbs light of a specific wavelength and becomes excited, and the excited species causes a hydrogen abstraction reaction from the surrounding hydrogen donor, generating active radical species, which become polymerization initiation species and start the polymerization of the radical polymerizable compound. On the other hand, the photoradical polymerization initiator of intramolecular cleavage type absorbs light of a specific wavelength and breaks a bond at a specific site, generating a radical at the broken site, which becomes a polymerization initiation species and starts the polymerization of the radical polymerizable compound.
[0005] Known examples of hydrogen abstraction type photoradical polymerization initiators include benzophenone-based photoradical polymerization initiators and thioxanthone-based photoradical polymerization initiators. Benzophenone-based photoradical polymerization initiators include methyl o-benzoylbenzoate, benzophenone, and 4-phenylbenzophenone, and commercially available products include OMNIRAD4PBZ (OMNIRAD is a registered trademark of IGM Group BV) and OMNIRADOMBB. Thioxanthone-based photoradical polymerization initiators include 2,4-diethylthioxanthone and 2-isopropylthioxanthone.
[0006] On the other hand, known examples of intramolecular cleavage type photoradical polymerization initiators include alkylphenone-based photoradical polymerization initiators, aminoalkylphenone-based photoradical polymerization initiators, acylphosphine oxide-based photoradical polymerization initiators, and oxime ester-based photoradical polymerization initiators.
[0007] Among these photoradical polymerization initiators, oxime ester photoradical polymerization initiators are particularly often used due to their excellent photosensitivity. Commercially available oxime ester photoradical polymerization initiators include Irgacure OXE-01, Irgacure OXE-02, Irgacure OXE-03, Irgacure OXE-04 (all manufactured by BASF), ADEKA OPT-N-1919, ADEKA Arcles NCI-930, ADEKA Arcles NCI-831 (all manufactured by ADEKA), TR-PBG-304, TR-PBG-326, TR-PBG-3057 (all manufactured by Changzhou Strong Electronic New Materials Co., Ltd.), etc.
[0008] These oxime ester-based photoradical polymerization initiators have both a structure that absorbs ultraviolet light and a structure that generates radicals. The light energy absorbed by the structure that absorbs ultraviolet light is transferred to the structure that generates radicals, which causes the cleavage of the NO bond of the oxime, which is the structure that generates radicals, to generate iminyl radicals and alkyloxy radicals. These radicals further decompose to generate highly active radicals, so that polymerization can be initiated with a small amount of exposure. For example, when the radically polymerizable composition is a colored composition, the ultraviolet transmittance of the coating film may be reduced, resulting in a reduced degree of curing of the coating film. However, oxime ester-based photoradical polymerization initiators are preferably used because they have high quantum efficiency. In order to transfer excitation energy from the structure that absorbs ultraviolet light to the structure that generates radicals, the two are directly bonded or bonded via a bonding group such as a ketone group.
[0009] For example, Patent Document 1 discloses an initiator having an oxime ester structure as a radical generating structure, an aromatic polycyclic structure as a structure absorbing ultraviolet light, and a direct bond or a ketone group as a structure transmitting light energy. Patent Document 2 discloses an initiator having an oxime ester structure as a radical generating structure, a carbazole ring as a structure absorbing ultraviolet light, and a direct bond as a structure transmitting light energy. Patent Document 3 discloses an initiator having an oxime ester structure as a radical generating structure, a fluorene ring as a structure absorbing ultraviolet light, and a direct bond or a ketone group as a structure transmitting light energy. In all of these oxime ester compounds, the radical generating structure and the ultraviolet absorbing structure are bonded by a direct bond or a ketone group, that is, the absorbed light energy is transmitted through a π bond in the molecule.
[0010] Oxime ester compounds that are described as containing an anthracene skeleton as a structure that absorbs ultraviolet light have also been disclosed. For example, Patent Document 1 lists anthraceneyl groups such as 9-anthryl as Ar1 and Ar2, which are structures that absorb ultraviolet light, and anthracenediyl groups such as 9,10-anthracenediyl as M1 and M2. However, all of these compounds are oxime ester compounds in which the oxime ester structure and the anthracene skeleton are directly bonded to each other, or which have a structure that contains a carbonyl group as a bonding group.
[0011] Furthermore, Patent Document 4 discloses compounds (10), (19), (59), (75), (76), and (77) that have an anthracenyl group as a substituent having a structure that absorbs ultraviolet light. However, in all of these compounds, the oxime ester group and the anthracene ring are bonded via a ketone group. Furthermore, Patent Document 5 discloses that X in general formula (1) also includes an anthracene ring, but X and the oxime ester group are directly bonded.
[0012] Meanwhile, high-pressure mercury lamps are usually used as a light source for irradiating ultraviolet rays, but in recent years LEDs (light-emitting diodes) have come to be used as the irradiation source. Unlike high-pressure mercury lamps, LEDs have the advantage of generating less heat and having a long lifespan, and so the development of ultraviolet curing technology using LEDs is accelerating. Typical LEDs are ultraviolet LEDs and blue LEDs. UV LEDs with central wavelengths of 405 nm, 395 nm, 385 nm, and other LEDs have been developed. In addition, for printed wiring board applications, a method is used in which patterns created using CAD are directly drawn using laser light, and 405 nm blue-violet laser diodes have also been developed as light sources for this purpose.
[0013] While high pressure mercury lamps have a line spectrum in the wide ultraviolet region of 250 to 450 nm, UV-LEDs and laser diodes basically have a single line spectrum. Compared to high pressure mercury lamp light sources that emit ultraviolet rays in a wide wavelength range, UV-LED lamps and the like, which are monochromatic light sources, have the disadvantages that they are single light, do not emit light in the short wavelength region of 300 nm or less, and have relatively weak irradiation intensity, so if existing photopolymerization initiators are used as they are, they are prone to surface curing failure, the polymerization reaction is easily affected by oxygen inhibition, and the surface curing properties of the coating film are significantly inferior. For this reason, photopolymerization initiators with high activity are required for UV-LED lamps, and oxime ester photopolymerization initiators are also being actively studied.
[0014] For example, Patent Document 6 discloses an initiator having an oxime ester structure as a radical generating structure, an aromatic polycyclic ring substituted with a nitro group as a structure absorbing ultraviolet light, and a direct bond or a ketone group as a structure transmitting light energy. Patent Document 7 discloses an initiator having an oxime ester structure as a radical generating structure, a coumarin ring as a structure absorbing ultraviolet light, and a ketone group as a structure transmitting light energy. [Prior art documents] [Patent documents]
[0015] [Patent Document 1] JP 2001-233842 A [Patent Document 2] JP 2004-359639 A [Patent Document 3] Special Publication No. 2020-517804 [Patent Document 4] JP 2007-210991 A [Patent Document 5] JP 2008-179611 A [Patent Document 6] Special Publication No. 2017-508738 [Patent Document 7] Special Publication No. 2020-528914 Summary of the Invention [Problem to be solved by the invention]
[0016] An object of the present invention is to provide a novel photoradical polymerization initiator that is sensitive to energy rays including light having a wavelength in the range of 350 nm to 420 nm, has high radical polymerization initiation ability, and is highly practical, in particular, a photoradical polymerization initiator that is highly active even when irradiated with a single-wavelength UV-LED or laser diode. [Means for solving the problem]
[0017] As a result of extensive investigations into the structure and photopolymerization properties of anthracene compounds, the present inventors have found that the oxime ester compound having an anthracene skeleton of the present invention absorbs light in the wavelength range of 350 nm to 420 nm, and that upon absorbing the light, the oxime ester decomposes to generate radical species. The inventors have also found that, due to this action, the oxime ester compound having an anthracene skeleton of the present invention is useful as a photoradical polymerization initiator active in the wavelength range of 350 nm to 420 nm, and that it exhibits remarkably excellent photosensitivity even when irradiated with a UV-LED or laser diode having a single wavelength in the wavelength range, and have thus completed the present invention.
[0018] That is, the present invention is summarized as follows: First, the first invention resides in an oxime ester compound having an anthracene skeleton represented by the following general formula (1).
[0019] [ka]
[0020] In the general formula (1), R 1 and R 2each independently represents a linear or branched alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, a cycloalkylalkyl group having 4 to 12 carbon atoms, an alkylcycloalkyl group having 4 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms; R 3 represents a linear or branched alkyl group having 1 to 10 carbon atoms; A represents a linear or branched alkylene group having 1 to 20 carbon atoms; m represents an integer of 0 to 3; and n represents an integer of 1 to 3.
[0021] A second invention resides in the oxime ester compound having an anthracene skeleton according to the first invention, characterized in that A is a methylene group.
[0022] A third invention resides in an oxime ester compound having an anthracene skeleton represented by the following general formula (2).
[0023] [ka]
[0024] In the general formula (2), R 1 and R 2 each independently represents a linear or branched alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, a cycloalkylalkyl group having 4 to 12 carbon atoms, an alkylcycloalkyl group having 4 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms; R 3 represents a linear or branched alkyl group having 1 to 10 carbon atoms, and A represents a linear or branched alkylene group having 1 to 20 carbon atoms. m represents an integer of 0 to 3. m represents an integer of 0 to 3.
[0025] A fourth invention resides in the oxime ester compound having an anthracene skeleton according to the third invention, characterized in that A is a methylene group.
[0026] The fifth invention is R 2is a methyl group.
[0027] A sixth invention resides in a method for producing an oxime ester compound having an anthracene skeleton represented by the following general formula (1), by etherifying a hydroxy group of an anthracene compound having a hydroxy group represented by the following general formula (3) with an etherifying agent having a ketone group, then oximating the ketone group with an oximating agent, and thereafter esterifying the hydroxyoxime group.
[0028] [ka]
[0029] In the general formula (3), R 3 each independently represents a linear or branched alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, a cycloalkylalkyl group having 4 to 12 carbon atoms, an alkylcycloalkyl group having 4 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms; R 3 represents a linear or branched alkyl group having 1 to 10 carbon atoms, m represents an integer of 0 to 3, and n represents an integer of 1 to 3.
[0030] [ka]
[0031] In the general formula (1), R 1 and R 2 each independently represents a linear or branched alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, a cycloalkylalkyl group having 4 to 12 carbon atoms, an alkylcycloalkyl group having 4 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms; R 3represents a linear or branched alkyl group having 1 to 10 carbon atoms; A represents a linear or branched alkylene group having 1 to 20 carbon atoms; m represents an integer of 0 to 3; and n represents an integer of 1 to 3.
[0032] A seventh invention resides in a method for producing an oxime ester compound having an anthracene skeleton represented by the following general formula (2), by etherifying a hydroxy group of an anthracene compound having a hydroxy group represented by the following general formula (9) with an etherifying agent having a ketone group, subsequently oximating the ketone group with an oximating agent, and then esterifying the hydroxyoxime group.
[0033] [ka]
[0034] In the general formula (9), R 3 represents a linear or branched alkyl group having 1 to 10 carbon atoms. m represents an integer of 0 to 3.
[0035] [ka]
[0036] In the general formula (2), R 1 and R 2 each independently represents a linear or branched alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, a cycloalkylalkyl group having 4 to 12 carbon atoms, an alkylcycloalkyl group having 4 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms; R 3 represents a linear or branched alkyl group having 1 to 10 carbon atoms, A represents a linear or branched alkylene group having 1 to 20 carbon atoms, and m represents an integer of 0 to 3.
[0037] An eighth aspect of the present invention resides in a photoradical polymerization initiator containing the oxime ester compound having an anthracene skeleton according to any one of the first to fifth aspects of the present invention.
[0038] A ninth aspect of the present invention resides in a polymerizable composition comprising the photoradical polymerization initiator according to the eighth aspect of the present invention and a radically polymerizable compound.
[0039] A tenth aspect of the present invention resides in a polymerizable composition according to the ninth aspect of the present invention, further comprising an alkali-soluble resin.
[0040] An eleventh invention resides in a method for photopolymerizing a polymerizable composition, comprising irradiating the polymerizable composition according to the ninth invention with energy rays including light having a peak wavelength in the wavelength range of 350 nm to 420 nm.
[0041] A twelfth invention resides in a method for photopolymerizing a polymerizable composition, comprising irradiating the polymerizable composition according to the tenth invention with energy rays including light having a peak wavelength in the wavelength range of 350 nm to 420 nm.
[0042] A thirteenth invention resides in the photopolymerization method of the polymerizable composition according to the eleventh invention, characterized in that the light source emitting light having a peak wavelength in the wavelength range of 350 nm to 420 nm is an ultraviolet LED or a 405 nm semiconductor laser having a peak wavelength at any one of 365 nm, 385 nm, 395 nm, 405 nm, or 415 nm.
[0043] A fourteenth invention resides in the photopolymerization method of the polymerizable composition according to the twelfth invention, characterized in that the light source emitting light having a peak wavelength in the wavelength range of 350 nm to 420 nm is an ultraviolet LED or a 405 nm semiconductor laser having a peak wavelength at any one of 365 nm, 385 nm, 395 nm, 405 nm, or 415 nm. Effect of the Invention
[0044] The oxime ester compound having an anthracene skeleton of the present invention is a compound that absorbs light having a wavelength in the range of 350 nm to 420 nm, and a polymerizable composition containing the oxime ester compound having an anthracene skeleton of the present invention as a photoradical polymerization initiator absorbs light having a wavelength in the range of 350 nm to 420 nm and polymerizes and hardens. In particular, it shows remarkably excellent photosensitivity even when irradiated with a UV-LED or a laser diode having light of a single wavelength in the wavelength range of 350 nm to 420 nm. [Brief description of the drawings]
[0045] [Figure 1] 1 is a graph showing the change over time in the amount of heat generated after irradiation with light for the oxime ester having an anthracene skeleton of the present invention and OXE02, a known oxime ester-based photopolymerization initiator.
[0046] The objects, features and advantages of the present invention will become more apparent from the following detailed description. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0047] The present invention will now be described in detail.
[0048] (Oxime ester compounds having anthracene skeleton) First, the present invention relates to an oxime ester compound having an anthracene skeleton represented by the following general formula (1).
[0049] [ka]
[0050] In the general formula (1), R 1 and R 2 each independently represents a linear or branched alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, a cycloalkylalkyl group having 4 to 12 carbon atoms, an alkylcycloalkyl group having 4 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms; R 3represents a linear or branched alkyl group having 1 to 10 carbon atoms; A represents a linear or branched alkylene group having 1 to 20 carbon atoms; m represents an integer of 0 to 3; and n represents an integer of 1 to 3.
[0051] In general formula (1), R 1 or R 2 Examples of the alkyl group having 1 to 20 carbon atoms represented by the formula (1) include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, an isopentyl group, a tert-pentyl group, a hexyl group, a heptyl group, an octyl group, an isooctyl group, a 2-ethylhexyl group, a tert-octyl group, a nonyl group, an isononyl group, a decyl group, an isodecyl group, an undecyl group, a dodecyl group, a tetradecyl group, a hexadecyl group, an octadecyl group, an icosyl group, etc. Examples of the cycloalkyl group having 3 to 12 carbon atoms include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cyclooctyl group, etc.
[0052] Examples of the cycloalkylalkyl group having 4 to 12 carbon atoms include cycloalkylmethyl such as cyclopropylmethyl, cyclobutylmethyl, cyclopentylmethyl, cyclohexylmethyl, cycloheptylmethyl, cyclooctylmethyl, cyclononylmethyl, and cyclodecylmethyl; cycloalkylethyl such as 2-cyclobutylethyl, 2-cyclopentylethyl, 2-cyclohexylethyl, 2-cycloheptylethyl, 2-cyclooctylethyl, 2-cyclononylethyl, and 2-cyclodecylethyl; cycloalkylpropyl such as 3-cyclobutylpropyl, 3-cyclopentylpropyl, 3-cyclohexylpropyl, 3-cycloheptylpropyl, 3-cyclooctylpropyl, 3-cyclononylpropyl, and 3-cyclodecylpropyl; and cycloalkylbutyl such as 4-cyclobutylbutyl, 4-cyclopentylbutyl, 4-cyclohexylbutyl, 4-cycloheptylbutyl, 4-cyclooctylbutyl, 4-cyclononylbutyl, and 4-cyclodecylbutyl. Examples of the alkylcycloalkyl group having 4 to 12 carbon atoms include a 1-methylcyclopentyl group, a 1-methylcyclohexyl group, and a 1-methyl-4-isopropylcyclohexyl group.
[0053] Examples of the aryl group having 6 to 20 carbon atoms include a phenyl group, a tolyl group, a xylyl group, a 4-ethylphenyl group, a 4-tert-butylphenyl group, a naphthyl group, an anthryl group, a phenanthryl group, and an indenyl group. Examples of the aralkyl group having 7 to 20 carbon atoms include a benzyl group, an α-methylbenzyl group, an α-ethylbenzyl group, a phenethyl group, an α-methylphenethyl group, a β-methylphenethyl group, an α,α-dimethylbenzyl group, an α,α-dimethylphenethyl group, a 4-methylphenethyl group, a 4-methylbenzyl group, a 3-methylbenzyl group, a 2-methylbenzyl group, a 4-ethyl and substituted or unsubstituted aralkyl groups such as arylbenzyl group, 2-ethylbenzyl group, 4-isopropylbenzyl group, 4-tert-butylbenzyl group, 2-tert-butylbenzyl group, 4-tert-pentylbenzyl group, 4-cyclohexylbenzyl group, 4-n-octylbenzyl group, 4-tert-octylbenzyl group, 4-allylbenzyl group, 4-benzylbenzyl group, 4-phenethylbenzyl group, 4-phenylbenzyl group, 4-(4'-methylphenyl)benzyl group, 2-furfuryl group, diphenylmethyl group, 1-naphthylmethyl group, and 2-naphthylmethyl group.
[0054] In general formula (1), R 3 Examples of the alkyl group having 1 to 20 carbon atoms represented by the formula (I) include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, an isopentyl group, a tert-pentyl group, a hexyl group, a heptyl group, an octyl group, an isooctyl group, a 2-ethylhexyl group, a tert-octyl group, a nonyl group, an isononyl group, a decyl group, an isodecyl group, an undecyl group, a dodecyl group, a tetradecyl group, a hexadecyl group, an octadecyl group, and an icosyl group.
[0055] In general formula (1), examples of the alkylene group having 1 to 20 carbon atoms represented by A include a methylene group, ethylene group, propylene group, butylene group, pentylene group, hexylene group, heptylene group, octylene group, nonylene group, decylene group, undecylene group, dodecylene group, tridecylene group, tetradecylene group, pentadecylene group, hexadecylene group, heptadecylene group, octadecylene group, nonadecylene group, and icosylene group, and the alkylene group may be branched with an alkyl group.
[0056] In general formula (1), the number n of substituents containing an oxime ester group is 2, and the compound in which the substituents are substituted at the 9th and 10th positions of the anthracene ring is the compound of the following general formula (2). The compound substituted at these positions is easy to obtain as a raw material and has high activity.
[0057] [ka]
[0058] In the general formula (2), R 1 and R 2 each independently represents a linear or branched alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, a cycloalkylalkyl group having 4 to 12 carbon atoms, an alkylcycloalkyl group having 4 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms; R 3 represents a linear or branched alkyl group having 1 to 10 carbon atoms, A represents a linear or branched alkylene group having 1 to 20 carbon atoms, and m represents an integer of 0 to 3.
[0059] In general formula (2), R 1 and R 2Examples of the alkyl group having 1 to 20 carbon atoms represented by the formula (1) include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, an isopentyl group, a tert-pentyl group, a hexyl group, a heptyl group, an octyl group, an isooctyl group, a 2-ethylhexyl group, a tert-octyl group, a nonyl group, an isononyl group, a decyl group, an isodecyl group, an undecyl group, a dodecyl group, a tetradecyl group, a hexadecyl group, an octadecyl group, an icosyl group, etc. Examples of the cycloalkyl group having 3 to 12 carbon atoms include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cyclooctyl group, etc.
[0060] Examples of the cycloalkylalkyl group having 4 to 12 carbon atoms include cycloalkylmethyl such as cyclopropylmethyl, cyclobutylmethyl, cyclopentylmethyl, cyclohexylmethyl, cycloheptylmethyl, cyclooctylmethyl, cyclononylmethyl, and cyclodecylmethyl; cycloalkylethyl such as 2-cyclobutylethyl, 2-cyclopentylethyl, 2-cyclohexylethyl, 2-cycloheptylethyl, 2-cyclooctylethyl, 2-cyclononylethyl, and 2-cyclodecylethyl; cycloalkylpropyl such as 3-cyclobutylpropyl, 3-cyclopentylpropyl, 3-cyclohexylpropyl, 3-cycloheptylpropyl, 3-cyclooctylpropyl, 3-cyclononylpropyl, and 3-cyclodecylpropyl; and cycloalkylbutyl such as 4-cyclobutylbutyl, 4-cyclopentylbutyl, 4-cyclohexylbutyl, 4-cycloheptylbutyl, 4-cyclooctylbutyl, 4-cyclononylbutyl, and 4-cyclodecylbutyl.
[0061] Examples of the alkylcycloalkyl group having 4 to 12 carbon atoms include a 1-methylcyclopentyl group, a 1-methylcyclohexyl group, and a 1-methyl-4-isopropylcyclohexyl group. Examples of the aryl group having 6 to 20 carbon atoms include a phenyl group, a tolyl group, a xylyl group, a 4-ethylphenyl group, a 4-tert-butylphenyl group, a naphthyl group, an anthryl group, a phenanthryl group, and an indenyl group. Examples of the aralkyl group having 7 to 20 carbon atoms include a benzyl group, an α-methylbenzyl group, an α-ethylbenzyl group, a phenethyl group, an α-methylphenethyl group, a β-methylphenethyl group, an α,α-dimethylbenzyl group, an α,α-dimethylphenethyl group, a 4-methylphenethyl group, a 4-methylbenzyl group, a 3-methylbenzyl group, a 2-methylbenzyl group, a 4-ethylbenzyl group, a 2-ethylbenzyl group, a 4-isopropylbenzyl group, a 4-tert-butylbenzyl group, a 2- Examples of substituted or unsubstituted aralkyl groups include tert-butylbenzyl group, 4-tert-pentylbenzyl group, 4-cyclohexylbenzyl group, 4-n-octylbenzyl group, 4-tert-octylbenzyl group, 4-allylbenzyl group, 4-benzylbenzyl group, 4-phenethylbenzyl group, 4-phenylbenzyl group, 4-(4'-methylphenyl)benzyl group, 2-furfuryl group, diphenylmethyl group, 1-naphthylmethyl group, and 2-naphthylmethyl group.
[0062] In general formula (2), examples of the alkylene group having 1 to 20 carbon atoms represented by A include a methylene group, ethylene group, propylene group, butylene group, pentylene group, hexylene group, heptylene group, octylene group, nonylene group, decylene group, undecylene group, dodecylene group, tridecylene group, tetradecylene group, pentadecylene group, hexadecylene group, heptadecylene group, octadecylene group, nonadecylene group, and icosylene group, and the alkylene group may be branched with an alkyl group.
[0063] Next, specific examples of the compound of general formula (1) will be shown.
[0064] In the general formula (1), n is 1 and R 2Representative specific examples of the compound in which is a methyl group and A is a methylene group include compounds of the following structural formulas.
[0065] [ka]
[0066] [ka]
[0067] In the general formula (1), n is 1 and R 2 Representative examples of compounds in which A is a methyl group and A is other than a methylene group include compounds of the following structural formulas.
[0068] [ka]
[0069] [ka]
[0070] [ka]
[0071] [ka]
[0072] In addition to the above compounds, the alkylene group of A may have a larger number of carbon atoms, or the alkylene group may be branched. In addition, compounds having a substituent such as an alkyl group on a cyclo ring or benzene ring may be exemplified. In addition, compounds having an alkyl group substituted on the anthracene ring of the above compounds may be exemplified.
[0073] In the general formula (1), n is 2 or more, and R 2Representative specific examples of the compound in which is a methyl group and A is a methylene group include compounds of the following structural formulas.
[0074] [ka]
[0075] [ka]
[0076] [ka]
[0077] [ka]
[0078] [ka]
[0079] The compound shown below, in which n is 2 and oxygen atoms are substituted at the 9th and 10th positions of the anthracene skeleton, is the compound of general formula (2).
[0080] [ka]
[0081] [ka]
[0082] In addition to the above compounds, the alkylene group of A may have a larger number of carbon atoms, or the alkylene group may be branched. In addition, compounds having a substituent such as an alkyl group on a cyclo ring or benzene ring may be exemplified. In addition, compounds having an alkyl group substituted on the anthracene ring of the above compounds may be exemplified.
[0083] A structure in which an oxygen atom is substituted on the anthracene skeleton is necessary to absorb light in the range of 350 nm to 420 nm, and an oxime ester structure is necessary to generate an active radical species. It is necessary that these two structures are contained and that these two are linked by an alkylene group.
[0084] Next, in the general formula (1), R 2 Specific examples are given using compounds where n is other than a methyl group and n is 2.
[0085] [ka]
[0086] [ka]
[0087] [ka]
[0088] [ka]
[0089] [ka]
[0090] [ka]
[0091] Among these exemplified compounds, the compounds in which A is a methylene group in general formula (1) or general formula (2) are preferred because of their high activity. In addition, the compounds in general formula (2) are preferred because they are easy to obtain high-purity raw materials and easy to synthesize. 1is a methyl group, a tert-butyl group, a phenyl group, R 2 is preferably a methyl group or a phenyl group. 1 is a methyl group, a tert-butyl group, R 2 is particularly preferably a methyl group. Specific compounds are preferably the compounds (2-1), (2-4), (2-7), (2-21), (2-24) and (2-25) in terms of their particularly high activity, and the compounds (2-1) and (2-4) are particularly preferably from the standpoint of ease of synthesis and high activity.
[0092] (Manufacturing method) The compound of the present invention represented by general formula (1) can be obtained by etherifying the hydroxy group of an anthracene compound having a hydroxy group represented by the following general formula (3) with an etherifying agent having a ketone group, then oximating the ketone group with an oximating agent, and then esterifying the hydroxyoxime group.
[0093] [ka]
[0094] In the general formula (3), R 3 represents a linear or branched alkyl group having 1 to 10 carbon atoms, m represents an integer of 0 to 3, and n represents an integer of 1 to 3.
[0095] [ka]
[0096] In the general formula (1), R 1 and R 2 each independently represents a linear or branched alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, a cycloalkylalkyl group having 4 to 12 carbon atoms, an alkylcycloalkyl group having 4 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms; R 3represents a linear or branched alkyl group having 1 to 10 carbon atoms; A represents a linear or branched alkylene group having 1 to 20 carbon atoms; m represents an integer of 0 to 3; and n represents an integer of 1 to 3.
[0097] That is, as shown in the following reaction scheme-1, an anthracene compound having a hydroxy group represented by general formula (3) is etherified with an etherifying agent having a ketone group represented by general formula (6) to produce a compound represented by general formula (4). Next, as shown in reaction scheme-2, the ketone group of the obtained compound of general formula (4) is oximed, and the hydroxy group of the obtained compound of general formula (5) is esterified with an esterifying agent represented by general formula (7) or (8) to produce the compound of general formula (1) of the present invention.
[0098] [ka]
[0099] In reaction formula 1, R 1 represents a linear or branched alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, a cycloalkylalkyl group having 4 to 12 carbon atoms, an alkylcycloalkyl group having 4 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms; R 3 represents a linear or branched alkyl group having 1 to 10 carbon atoms, A represents a linear or branched alkylene group having 1 to 20 carbon atoms, m represents an integer of 0 to 3, and n represents an integer of 1 to 3. X represents a chlorine atom or a bromine atom.
[0100] [ka]
[0101] In reaction scheme 2, R 1represents a linear or branched alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, a cycloalkylalkyl group having 4 to 12 carbon atoms, an alkylcycloalkyl group having 4 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms; R 3 represents a linear or branched alkyl group having 1 to 10 carbon atoms; A represents a linear or branched alkylene group having 1 to 20 carbon atoms; m represents an integer of 0 to 3; and n represents an integer of 1 to 3.
[0102] [ka]
[0103] In reaction scheme 3, R 1 and R 2 each independently represents a linear or branched alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, a cycloalkylalkyl group having 4 to 12 carbon atoms, an alkylcycloalkyl group having 4 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms; R 3 represents a linear or branched alkyl group having 1 to 10 carbon atoms, A represents a linear or branched alkylene group having 1 to 20 carbon atoms, m represents an integer of 0 to 3, and n represents an integer of 1 to 3. X represents a chlorine atom or a bromine atom.
[0104] Each reaction is described in detail below.
[0105] (Etherification) In the reaction of Reaction Scheme-1, the etherification agent used in the etherification of the anthracene compound having a hydroxy group represented by general formula (3) is a compound having a ketone group represented by the following general formula (6).
[0106] [ka]
[0107] In the general formula (6), R 1represents a linear or branched alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, a cycloalkylalkyl group having 4 to 12 carbon atoms, an alkylcycloalkyl group having 4 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms; A represents a linear or branched alkylene group having 1 to 20 carbon atoms; and X represents a chlorine atom or a bromine atom.
[0108] Examples of the etherifying agent include bromoacetone, chloroacetone, bromomethyl ethyl ketone, chloromethyl ethyl ketone, 2-bromo-3-pentanone, 2-chloro-3-pentanone, 1-bromo-3,3-dimethyl-2-butanone, 1-chloro-3,3-dimethyl-2-butanone, 1-bromo-3,3,3-trifluoroacetone, 1-chloro-3,3,3-trifluoroacetone, 2-chloroacetophenone, 2-bromoacetophenone, 2-chloroacetophenone phenacyl chloride, 2-bromoacetylnaphthalene, and 2-chloroacetylnaphthalene.
[0109] Examples of the anthracene compound of general formula (3) that can be used include 1-hydroxyanthracene, 2-hydroxyanthracene, 9-hydroxyanthracene, 1,4-dihydroxyanthracene, 9,10-dihydroxyanthracene, 1,5-dihydroxyanthracene, 2,6-dihydroxyanthracene, 1,2,10-trihydroxyanthracene, 1,8,9-trihydroxyanthracene, 1,2,7-trihydroxyanthracene, and the like, as well as alkyl group-substituted products thereof.
[0110] In the reaction of reaction formula-1, the ratio of the etherification agent to the anthracene compound is 1 to 30 times by mole, preferably 2 to 25 times by mole, based on the hydroxyl groups of the anthracene compound. If the ratio of the etherification agent to be added is less than 1 time by mole, the anthracene compound remains unreacted, which requires a lot of work to purify it, and if the ratio exceeds 30 times by mole, the reaction rate and yield do not increase, which is economically disadvantageous.
[0111] The reaction of reaction formula-1 is preferably carried out in the presence of a base compound. The base compound used is usually an inorganic alkali salt. Examples of the inorganic alkali salt include sodium hydroxide, potassium hydroxide, and lithium hydroxide. Organic bases such as pyridine, piperidine, trimethylamine, and triethylamine can also be used.
[0112] The reaction temperature of reaction formula-1 is 0°C or higher and 150°C or lower, preferably room temperature or higher and 80°C or lower. If the temperature is lower than 0°C, the reaction rate is too slow and the reaction takes too long, and if the temperature is higher than 150°C, side reactions occur and the purity of the product decreases. The reaction time is usually about 0.5 to 24 hours. After the reaction, if crystals of the product precipitate, the precipitate is filtered and dried, and if impurities precipitate, the precipitate is filtered off and the filtrate is concentrated to obtain general formula (4).
[0113] (Oxime) Next, in the reaction of Reaction Scheme-2, the ketone group of the compound of general formula (4) obtained in the reaction of Reaction Scheme-1 is oximed with an oxime-forming agent.
[0114] Hydroxylamine and / or hydroxylamine hydrochloride are used as the oximation agent. The amount of the oximation agent added is 1 to 30 times by mole, preferably 5 to 25 times by mole, based on the ketone group of the compound of general formula (4). If the amount is less than 1 mole, the raw material remains unreacted, which requires a lot of work to purify, and if the amount is more than 30 moles, the reaction rate and yield do not increase, which is economically disadvantageous.
[0115] The reaction of Reaction Formula-2 is usually carried out in an organic solvent. Examples of the organic solvent that can be used include aromatic solvents such as toluene, xylene, and ethylbenzene, ether solvents such as tetrahydrofuran and 1,4-dioxane, ketone solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone, amide solvents such as dimethylacetamide and dimethylformamide, halogenated carbon solvents such as methylene chloride, ethylene dichloride, and chlorobenzene, and alcohol solvents such as methanol, ethanol, and 1-propanol. In order to promote the reaction, a base such as sodium acetate, pyridine, piperidine, or triethylamine is added.
[0116] The reaction temperature of the reaction of Reaction Scheme-2 is the reflux temperature of the solvent used, and is usually in the range of 60 to 120° C. The compound of general formula (5) can be obtained by reacting for usually 0.1 to 20 hours.
[0117] (Esterification) In reaction formula-3, the hydroxy group in the oxime group of the compound represented by general formula (5) obtained in reaction formula-2 is esterified using an esterifying agent. The esterifying agent may be any commonly used esterifying agent. For example, an acid halide or an acid anhydride may be used as the esterifying agent, but an acid halide represented by general formula (7) or an acid anhydride represented by general formula (8) is preferred.
[0118] [ka]
[0119] In the general formula (7), R 2 represents a linear or branched alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, a cycloalkylalkyl group having 4 to 12 carbon atoms, an alkylcycloalkyl group having 4 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms, and X represents a chlorine atom or a bromine atom.
[0120] [ka]
[0121] In the general formula (8), R 2 represents a linear or branched alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, a cycloalkylalkyl group having 4 to 12 carbon atoms, an alkylcycloalkyl group having 4 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms.
[0122] Examples of the acid halide represented by the general formula (7) include acetyl chloride, acetyl bromide, propionic acid chloride, propionic acid bromide, butyric acid chloride, butyric acid bromide, benzoic acid chloride, benzoic acid bromide, phenylacetic acid chloride, phenylacetic acid bromide, o-methylbenzoic acid chloride, m-methylbenzoic acid chloride, and p-methylbenzoic acid chloride. Examples of the acid anhydride represented by the general formula (8) include acetic anhydride, propionic acid anhydride, butyric acid anhydride, valeric acid anhydride, and benzoic acid anhydride.
[0123] The ratio of the esterification agent to be added to the compound represented by formula (5) is 1 to 30 times by mole, preferably 2 to 25 times by mole, based on the oxime group of the compound represented by formula (5). If the amount is less than 1 time by mole, the compound represented by formula (5) remains unreacted, which requires a lot of work to purify it, whereas if the amount is more than 30 times by mole, the reaction rate and yield do not increase, which is economically disadvantageous.
[0124] In addition, in the reaction formula-3, a catalyst is used to accelerate the reaction. Either an acidic catalyst or a basic catalyst can be used as the catalyst. Examples of the acidic catalyst include sulfuric acid and p-toluenesulfonic acid, while examples of the basic catalyst include sodium hydroxide, sodium ethoxide, triethylamine, pyridine, piperidine, and 4,4-dimethylaminopyridine.
[0125] The reaction temperature of Reaction Scheme-3 is usually 0°C or higher and 150°C or lower. The reaction time is usually about 0.5 to 24 hours. As the reaction proceeds, the compound of general formula (1) is obtained.
[0126] After the esterification reaction, the compound represented by the general formula (1) can be obtained by typical post-treatment such as washing, concentration, and filtration.
[0127] The method for producing the compound of general formula (2) is such that the raw material anthracene compound in general formula (1) is limited to 9,10-dihydroxyanthracene and its alkyl-substituted derivatives, and other production conditions are the same.
[0128] (Photoradical polymerization initiator) The oxime ester compound represented by the general formula (1) or (2) of the present invention has an anthracene ring and an oxime ester group in its skeleton, the anthracene ring has the ability to absorb and excite light of 350 nm to 450 nm, and the oxime ester group has the ability to decompose and generate active radical species when it obtains excitation energy, so it can be used as a photoradical polymerization initiator. Surprisingly, the oxime ester compound represented by the general formula (1) or (2) of the present invention is different from known oxime ester radical polymerization initiators in that the skeleton that absorbs light and the oxime ester group that generates radical species are bonded not via a direct bond or a ketone group but via a σ bond (alkylene group), which is a non-conjugated bond. That is, in appearance, the light energy absorbed by the anthracene skeleton is transferred to the oxime ester group through the through space, and the oxime ester group is decomposed to generate radical species. There are no known examples of oxime ester-based photoradical polymerization initiators in which the light-absorbing backbone (donor) and the oxime ester group (acceptor) are bonded without an electronic bond such as a π bond.
[0129] Furthermore, surprisingly, the oxime ester compound of the present invention represented by general formula (1) or general formula (2) has the characteristic that, when irradiated with light having a wavelength in the range of 350 nm to 420 nm, it generates radical species and acts as a radical polymerization initiator to radically polymerize a radically polymerizable compound, whereas, in a dark place where it is not irradiated with light having a wavelength in the range of 350 nm to 420 nm, it conversely acts as a radical polymerization inhibitor that captures the radical species.
[0130] In general, it is known that radical polymerizable compounds such as methyl acrylate and styrene naturally generate radical species due to oxygen, heat, etc., even without a polymerization initiator, and undergo polymerization degradation. Therefore, to prevent degradation, polymerization inhibitors such as t-butylcatechol are added to radical polymerizable compounds such as methyl acrylate and styrene to capture and inactivate the generated radical species. However, this polymerization inhibitor actually inhibits polymerization during polymerization, which results in a longer lead time for radical polymerization or poor progress in the polymerization reaction. Therefore, when polymerizing, it is necessary to remove this polymerization inhibitor or add a polymerization initiator in an amount that is commensurate with the amount of the polymerization inhibitor that is inactivated.
[0131] In the case where unintended radical species are generated due to the influence of oxygen, heat, etc., the radical polymerizable composition containing the oxime ester compound represented by general formula (1) or general formula (2) of the present invention can prevent the radical polymerizable compound from being polymerized and deteriorated, by capturing the radical species with the oxime ester compound represented by general formula (1) or general formula (2) of the present invention. In other words, the composition has a feature that the radical polymerizable compound can be stored stably under light shielding.
[0132] For example, when a radical polymerizable composition is applied in a film form, a light-shielding film having a pattern is placed on the applied film, and polymerization of the radical polymerizable composition is started under irradiation with light in the wavelength range of 350 to 420 nm, only the area exposed to light is polymerized, and the area covered with the light-shielding film is not polymerized, so that a pattern of the polymerized product can be formed. However, in the case of a commonly used photoradical polymerization initiator, polymerization proceeds due to the generated radical species or radicals at the polymerization terminal in the vicinity of the shielded area not exposed to light, and the area not exposed to light is also cured, so that a clear pattern cannot be formed in many cases. On the other hand, by containing the oxime ester compound represented by the general formula (1) or general formula (2) of the present invention, the polymerization inhibition effect of the oxime ester compound represented by the general formula (1) or general formula (2) of the present invention allows radical species to be captured in the shielded area not exposed to light, so that the polymerization reaction does not proceed sufficiently, and the area exposed to light and the area not exposed to light can be clearly distinguished. As a result, a pattern with a sharp boundary between the area exposed to light and the area not exposed to light can be formed.
[0133] (Polymerizable composition) The oxime ester compound of the present invention can be added as a photoradical polymerization initiator to a radically polymerizable compound to prepare a polymerizable composition.
[0134] (Radical polymerizable compound) The radically polymerizable compound used in the polymerizable composition of the present invention is not particularly limited as long as it is a compound having radical polymerizability, and examples thereof include styrene, p-hydroxystyrene, vinyl acetate, acrylic acid, methacrylic acid, acrylonitrile, methacrylonitrile, acrylamide, acrylic acid esters, methacrylic acid esters, and / or oligomers thereof.
[0135] Examples of acrylic acid esters include monofunctional acrylates having one acrylate group, and bifunctional or polyfunctional acrylates having multiple acrylate groups. Examples of monofunctional acrylates include methyl acrylate, n-butyl acrylate, cyclohexyl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, phenoxypolyethylene glycol acrylate, 2-acryloyloxyethyl succinate, isostearyl acrylate, 2-(2-ethoxyethoxy)ethyl acrylate, stearyl acrylate, isobornyl acrylate (IBOA), tetrahydrofurfuryl acrylate, lauryl acrylate, 2-phenoxyethyl acrylate, isodecyl acrylate, isooctyl acrylate, tridecyl acrylate, and tetradecyl acrylate. Examples of the acrylates include butyl acrylate, caprolactone acrylate, ethoxylated nonylphenyl acrylate, isobornyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 4-hydroxybutyl acrylate, isobutyl acrylate, t-butyl acrylate, cyclohexyl acrylate, 2-methoxyethyl acrylate, methoxytriethylene glycol acrylate, 2-ethoxyethyl acrylate, benzyl acrylate, 3,3,5-trimethylcyclohexyl acrylate (TMCHA), and dicyclopentenyl acrylate (DCPA). Examples of bifunctional acrylates include ethoxylated bisphenol A diacrylate, 9,9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorene, tricyclodecane dimethanol diacrylate, 1,10-decanediol diacrylate, 1,9-nonanediol diacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, 1,3-butylene glycol diacrylate, 1,4-butanediol diacrylate, diethylene glycol diacrylate, 1,6-hexanediol diacrylate, tetraethylene glycol diacrylate, triethylene glycol diacrylate, tripropylene glycol diacrylate, ethoxylated (3) bisphenol A diacrylate, and alkoxylated neopentyl glycol diacrylate.
[0136] Examples of polyfunctional acrylates include ethoxylated isocyanuric acid triacrylate, ε-caprolactone-modified tris-(2-acryloxyethyl)isocyanurate, pentaerythritol triacrylate, trimethylolpropane triacrylate, ditrimethylolpropane tetraacrylate, ethoxylated pentaerythritol tetraacrylate, pentaerythritol tetraacrylate, dipentaerythritol hexaacrylate, tris(2-hydroxyethyl)isocyanurate triacrylate, ethoxylated trimethylolpropane triacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, ditrimethylolpropane tetraacrylate, dipentaerythritol pentaacrylate, etc. Furthermore, epoxy acrylate, urethane acrylate, polyester acrylate, polybutadiene acrylate, polyol acrylate, polyether acrylate, silicone resin acrylate, imide acrylate, etc. can also be used.
[0137] Similarly, examples of the methacrylate compound include monofunctional methacrylates, difunctional methacrylates, and polyfunctional methacrylates. Examples of the monofunctional methacrylates include methyl methacrylate, n-butyl methacrylate, cyclohexyl methacrylate, 2-ethylhexyl methacrylate, 2-hydroxyethyl methacrylate, phenoxyethylene glycol methacrylate, stearyl methacrylate, 2-methacryloyloxyethyl succinate, tetrahydrofurfuryl methacrylate, isodecyl methacrylate, lauryl methacrylate, 2-phenoxyethyl methacrylate, isobornyl methacrylate, and tridecyl methacrylate. Examples of bifunctional methacrylates include ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, ethoxylated bisphenol A dimethacrylate, tricyclodecane dimethanol dimethacrylate, 1,6-hexanediol dimethacrylate, 1,9-nonanediol dimethacrylate, neopentyl glycol dimethacrylate, glycerin dimethacrylate, tetraethylene glycol dimethacrylate, polyethylene glycol dimethacrylate, 1,4-butanediol dimethacrylate, diethylene glycol dimethacrylate, 1,3-butylene diol dimethacrylate, ethoxylated bisphenol A dimethacrylate, etc. Examples of polyfunctional methacrylates include trimethylolpropane trimethacrylate, etc.
[0138] These radical polymerizable compounds may be used alone or in combination of two or more kinds.
[0139] (Polymerizable resin) The photoradically polymerizable composition of the present invention may further contain a polymerizable resin. Examples of the polymerizable resin include photopolymerizable prepolymers, binder polymers such as acrylic resins, styrene resins, and epoxy resins, and alkali-soluble resins.
[0140] The photopolymerizable prepolymer is not particularly limited, and examples thereof include polyester acrylate, polyester methacrylate, epoxy acrylate, epoxy methacrylate, polyurethane acrylate, polyurethane methacrylate, etc. These photopolymerizable prepolymers may be used alone or in combination of two or more. Among these photopolymerizable prepolymers, polyurethane acrylate and polyurethane methacrylate are preferred.
[0141] (alkali soluble resin) As the alkali-soluble resin, a compound having a hydroxyl group and / or a carboxyl group and an ethylenically unsaturated bond group can be preferably used. A compound having a group that generates a hydroxyl group during the reaction and an ethylenically unsaturated bond group, such as an epoxy compound, may also be used.
[0142] Examples of the compound having a hydroxyl group and an ethylenically unsaturated bond group include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl acrylate, 2-acryloyloxyethyl-2-hydroxyethyl-phthalic acid, glycerol mono(meth)acrylate, dihydroxyacrylate, glycerol (meth)acrylate, pentaerythritol mono(meth)acrylate, and dipentaerythritol mono(meth)acrylate. Further examples include 2-hydroxy 3-acryloyloxypropyl methacrylate, pentaerythritol di(meth)acrylate, dipentaerythritol di(meth)acrylate, pentaerythritol diacrylate, isocyanuric acid EO modified diacrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, etc. Also included are glycidyl (meth)acrylate, etc. which generate hydroxyl groups by reaction, but are not limited thereto.
[0143] Examples of compounds having a carboxyl group and an ethylenically unsaturated bond group include acrylic acid, methacrylic acid, 2-acryloyloxyethyl succinate, crotonic acid, isocrotonic acid, tiglic acid, 3-methylcrotonic acid, 2-methyl-2-pentenoic acid, α-hydroxyacrylic acid, α-chloroacrylic acid, and cinnamic acid. Examples of the compounds include maleic acid, fumaric acid, itaconic acid, citraconic acid, and mesaconic acid. Examples of the compounds include mono(2-acryloyloxyethyl) succinate, mono(2-methacryloyloxyethyl) succinate, mono(2-acryloyloxyethyl) phthalate, and mono(2-methacryloyloxyethyl) phthalate. Examples of the compounds include ω-carboxypolycaprolactone monoacrylate and ω-carboxypolycaprolactone monomethacrylate.
[0144] The alkali-soluble resin may be not only a monomer but also an oligomerized alkali-soluble resin. As the oligomerized alkali-soluble resin, those generally used in negative resists can be used, and any resin may be used as long as it is soluble in an alkaline aqueous solution, and is not particularly limited. For example, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, n-decyl (meth)acrylate, n-butyl ... Examples of the copolymer include copolymers composed of one or more selected from among (meth)acrylic acid, itaconic acid, crotonic acid, maleic acid, fumaric acid, vinylacetic acid, and anhydrides thereof, and copolymers composed of one or more selected from among methyl acrylate, benzyl (meth)acrylate, styrene, γ-methylstyrene, N-vinyl-2-pyrrolidone, glycidyl (meth)acrylate, and the like, and a polymer in which an ethylenically unsaturated compound having a glycidyl group or a hydroxyl group is added to the above-mentioned copolymer.Further, for example, the following compounds may be used: carboxyl group-containing resins obtained by copolymerization of unsaturated carboxylic acids such as (meth)acrylic acid with unsaturated group-containing compounds such as styrene, α-methylstyrene, lower alkyl (meth)acrylates, and isobutylene; carboxyl group-containing urethane resins obtained by polyaddition reaction of diisocyanates such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates with carboxyl group-containing dialcohol compounds such as dimethylolpropionic acid and dimethylolbutanoic acid, and diol compounds such as polycarbonate-based polyols, polyether-based polyols, polyester-based polyols, polyolefin-based polyols, acrylic polyols, bisphenol A-based alkylene oxide adduct diols, and compounds having phenolic hydroxyl groups and alcoholic hydroxyl groups; and diisocyanate compounds such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates with polycarbonate-based polyols, polyether-based polyols, polyester-based polyols, polyolefin-based polyols, acrylic polyols, bisphenol A-based alkylene oxide adduct diols, and compounds having phenolic hydroxyl groups and alcoholic hydroxyl groups. Examples of the urethane resin include a terminal carboxyl group-containing urethane resin obtained by reacting an acid anhydride with the terminal of a urethane resin obtained by a polyaddition reaction of a diol compound such as a bisphenol A-based polyol, a polyester-based polyol, a polyolefin-based polyol, an acrylic polyol, a bisphenol A-based alkylene oxide adduct diol, or a compound having a phenolic hydroxyl group and an alcoholic hydroxyl group; a carboxyl group-containing urethane resin obtained by a polyaddition reaction of a diisocyanate and a (meth)acrylate or a partially acid anhydride-modified product thereof of a bifunctional epoxy resin such as a bisphenol A-based epoxy resin, a hydrogenated bisphenol A-based epoxy resin, a bisphenol F-based epoxy resin, a bisphenol S-based epoxy resin, a bixylenol-based epoxy resin, or a biphenol-based epoxy resin; a carboxyl group-containing urethane resin obtained by a polyaddition reaction of a carboxyl group-containing dialcohol compound and a diol compound; and a carboxyl group-containing urethane resin obtained by adding a compound having one hydroxyl group and one or more (meth)acryloyl groups in the molecule such as a hydroxyalkyl (meth)acrylate to convert the terminal to (meth)acrylic acid.Commercially available alkali-soluble resins include the Dianarl NR series (manufactured by Mitsubishi Rayon Co., Ltd.), Viscoat R-264, KS Resist 106 (manufactured by Osaka Organic Chemical Industry Co., Ltd.), Ebecryl 3800 (manufactured by Daicel-Allnex Corporation), Acricur RD-F8 (manufactured by Nippon Shokubai Co., Ltd.), and Foret ZAH-110 (manufactured by Soken Chemical & Engineering Co., Ltd.).
[0145] In addition, a hydrogen donor may be added to the polymerizable composition of the present invention in order to promote radical polymerization, within a range that does not impair the effects of the present invention. Examples of the hydrogen donor include alcohol hydrogen donors such as methanol, ethanol, n-propanol, isopropanol, n-butyl alcohol, isobutyl alcohol, sec-butyl alcohol, 1,2,4-butanetriol, 1,2,6-hexanetriol, 1,2,3-heptanetriol, 2,6-dimethyl-1,2,6-hexanetriol, 1,2,3-hexanetriol, 1,2,3-butanetriol, 3-methyl-1,3,5-pentanetriol, 3,7,11,15-tetramethyl-1,2,3-hexadecanetriol, ethylene glycol, glycerin, propylene glycol, diene Examples of the mercaptan hydrogen donors include 2-mercaptobenzothiazole, 2-mercaptobenzoxazole, 2-mercaptobenzimidazole, 2,5-dimercapto-1,3,4-thiadiazole, and 2-mercapto-2,5-dimethylaminopyridine. In addition, examples of amine hydrogen donors include 4,4'-bis(dimethylamino)benzophenone, 4,4'-bis(diethylamino)benzophenone, 4-diethylaminoacetophenone, 4-dimethylaminopropiophenone, ethyl-4-dimethylaminobenzoate, 4-dimethylaminobenzoic acid, and 4-dimethylaminobenzonitrile. Further examples include bis[4-(dimethylamino)phenyl]methane, bis[4-(diethylamino)phenyl]methane, and leuco crystal violet. These hydrogen donors may be used alone or in combination of two or more.
[0146] Furthermore, the polymerizable composition of the present invention may contain various resin additives such as pigments and / or dyes, diluents, dispersants, organic or inorganic fillers, leveling agents, surfactants, defoamers, thickeners, flame retardants, surface modifiers, penetration promoters, moisturizers, fixing agents, antifungal agents, preservatives, antioxidants, polymerization inhibitors, UV absorbers, light stabilizers, chelating agents, pH adjusters, stabilizers, lubricants, plasticizers, etc., in addition to the above, within the range that does not impair the effects of the present invention. Depending on the application, the composition may contain a solvent.
[0147] (Pigments) Examples of pigments that can be used in the present invention include the following (all shown by color index numbers): CI Pigment Yellow 12, 13, 14, 17, 20, 24, 55, 83, 86, 93, 109, 110, 117, 125, 137, 139, 147, 148, 153, 154, 166, 168, CI Pigment Orange 36, 43, 51, 55, 59, 61, CI Pigment Red 9, 97, 122, 123, 149, 168, 177, 180, 192, 215, 216, 217, 220, 223, 224, 226, 227, 228, 240, CI Pigment Violet 19, 23, 29, 30, 37, 40, 50, CI Pigment Examples include Blue 15, 15:1, 15:4, 15:6, 22, 60, 64, CI Pigment Green 7, 36, CI Pigment Brown 23, 25, 26, etc.
[0148] Examples of black pigments include carbon black and titanium black. Specific examples of carbon black include Special Black 4, Special Black 100, Special Black 250, Special Black 350, and Special Black 550 manufactured by Degussa; Raven 1040, Raven 1060, Raven 1080, and Raven 1255 manufactured by Colombian Carbon; and MA7, MA8, MA11, MA100, MA220, and MA230 manufactured by Mitsubishi Chemical Corporation.
[0149] (solvent) The photopolymerizable composition of the present invention may be adjusted in viscosity by using a solvent in order to impart coating suitability. Examples of the solvent include methanol, ethanol, toluene, cyclohexane, isophorone, cellosolve acetate, diethylene glycol dimethyl ether, ethylene glycol diethyl ether, xylene, ethylbenzene, methyl cellosolve, ethyl cellosolve, butyl cellosolve, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, diethylene glycol diethyl ether acetate, isoamyl acetate, ethyl lactate, methyl ethyl ketone, acetone, and cyclohexanone. These may be used alone or in combination of two or more.
[0150] The amount of the oxime ester compound represented by general formula (1) or general formula (2) of the present invention to be blended varies depending on the radical polymerizable compound used and the polymerization conditions. From the viewpoints of the effect as a radical polymerization initiator, sufficient radical polymerization inhibition effect, and economic efficiency, the amount is usually preferably 0.01 to 10 parts by weight, and more preferably 0.01 to 2 parts by weight, per 100 parts by weight of the radical polymerizable compound.
[0151] The photoradical polymerization initiator of the present invention may contain a photoradical polymerization initiator other than the oxime ester compound represented by general formula (1) or general formula (2) of the present invention, as long as the curing of the present invention is not impaired.
[0152] (Other photoradical polymerization initiators) Examples of photoradical polymerization initiators that can be used in combination with the oxime ester compound represented by general formula (1) or general formula (2) of the present invention include alkylphenone-based photoradical polymerization initiators, benzophenone-based radical polymerization initiators, anthraquinone-based photoradical polymerization initiators, etc. In terms of synergistic effect, (i) alkylphenone-based photoradical polymerization initiators and (ii) benzophenone-based radical polymerization initiators are preferred.
[0153] (i) Alkylphenone-based photoradical polymerization initiators The alkylphenone-based photoradical polymerization initiator used in the present invention is not particularly limited as long as it is a compound that has an alkylphenone structure and is excited and decomposed by light irradiation to generate radical species.
[0154] Various compounds are known as examples of alkylphenone-based photoradical polymerization initiators, among which at least one selected from the group consisting of 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methylpropan-1-one, 2-hydroxy-1-{[4-(2-hydroxy-2-methylpropionyl)benzyl]phenyl}-2-methylpropan-1-one and 2,2-dimethoxy-1,2-diphenylethan-1-one is preferred, and 1-hydroxycyclohexyl phenyl ketone is the most preferred. Commercially available alkylphenone-based photoradical polymerization initiators include OMNIRAD184 (OMNIRAD is a registered trademark of IGM Group BV), OMNIRAD1173, OMNIRAD2959, OMNIRAD127, OMNIRAD651, etc. Other examples include OMNIRADMBF and OMNIRAD754, which have a structure similar to that of alkylphenone-based photoradical polymerization initiators.
[0155] ((ii) Benzophenone-based photoradical polymerization initiators) The benzophenone-based photoradical polymerization initiator used in the present invention is not particularly limited as long as it is a compound that has a benzophenone structure, is excited by light irradiation, and causes a hydrogen abstraction reaction to generate radical species.
[0156] Various compounds are known as examples of benzophenone-based photoradical polymerization initiators, and among them, at least one selected from the group consisting of benzophenone, benzoylbenzoic acid, o-benzoyl methyl benzoate, 4-phenylbenzophenone, 4-methoxybenzophenone, 4-hydroxybenzophenone, 4,4'-dihydroxybenzophenone, acrylated benzophenone, 4-methylbenzophenone, 4,4'-dimethylbenzophenone, 4,4'-dimethoxybenzophenone, 3,3'-dimethyl-4-methoxybenzophenone, 2,4,6-trimethylbenzophenone, 3,3,4,4'-tetra(t-butylperoxycarbonyl)benzophenone, 4,4'-diphenoxybenzophenone, and fluorenone is preferred. In addition, the benzophenone may be a chain polymer compound, a branched polymer compound, or a dendritic polymer compound containing the benzophenone compound in the main chain, terminal, or side chain. Among these compounds, o-benzoyl methyl benzoate, benzophenone, and 4-phenylbenzophenone are most preferred. Commercially available benzophenone-based radical photopolymerization initiators include OMNIRAD4PBZ (OMNIRAD is a registered trademark of IGM Group BV) and OMNIRADOMBB.
[0157] (iv) Acylphosphine oxide-based photoradical polymerization initiators The acylphosphine oxide-based photoradical polymerization initiator used in the present invention is not particularly limited as long as it is a compound that has a phenylbisacylphosphine oxide structure and is excited and decomposed by light irradiation to generate radical species.
[0158] Various compounds are known as acylphosphine oxide-based photoradical polymerization initiators, among which at least one selected from the group consisting of benzoyl-diphenylphosphine oxide, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 2,3,5,6-tetramethylbenzoyl-diphenylphosphine oxide, 3,4-dimethylbenzoyl-diphenylphosphine oxide, 2,4,6-trimethylbenzoyl-phenylethoxyphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethyl-pentylphosphine oxide, and bis(2,6-dimethylbenzoyl)-ethylphosphine oxide is preferred. Commercially available acylphosphine oxide-based photoradical polymerization initiators include OMNIRADTPO, OMNIRADTPO-L, and OMNIRAD819.
[0159] ((v) Oxime ester-based photoradical polymerization initiators) The oxime ester-based photoradical polymerization initiator used in the present invention is not particularly limited as long as it is a compound that has an oxime ester structure and is excited and decomposed by light irradiation to generate radical species.
[0160] Various compounds are known as oxime ester photoradical polymerization initiators, among which at least one selected from the group consisting of N-benzoyloxy-1-(4-phenylsulfanylphenyl)octan-1-one-2-imine, N-acetyloxy-1-(4-phenylsulfanylphenyl)-3-cyclohexylpropan-1-one-2-imine, N-acetoxy-1-[9-ethyl-6-{2-methyl-4-(3,3-dimethyl-2,4-dioxacyclopentanylmethyloxy)benzoyl}-9H-carbazol-3-yl]ethan-1-imine and 1-[7-(2-methylbenzoyl)-9,9-dipropyl-9H-fluoren-2-yl]ethanone O-acetyloxime is preferred. Commercially available products of oxime ester photoradical polymerization initiators include Irgacure OXE01, Irgacure OXE02, Irgacure OXE03, etc.
[0161] ((vi) Biimidazole-based photoradical polymerization initiators) The biimidazole-based photoradical polymerization initiator used in the present invention is not particularly limited as long as it is a compound that has a biimidazole structure and is excited and decomposed by light irradiation to generate radical species.
[0162] Examples of the biimidazole-based photoradical polymerization initiator include 2,4,5-triarylimidazole dimers such as 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer, 2-(o-chlorophenyl)-4,5-di(methoxyphenyl)imidazole dimer, 2-(o-fluorophenyl)-4,5-diphenylimidazole dimer, 2-(o-methoxyphenyl)-4,5-diphenylimidazole dimer, and 2-(p-methoxyphenyl)-4,5-diphenylimidazole dimer.
[0163] Examples of the anthraquinone-based photoradical polymerization initiator that can be used in the present invention include 2-ethylanthraquinone, 2-t-butylanthraquinone, 2-phenoxyanthraquinone, 2-(phenylthio)anthraquinone, and 2-(hydroxyethylthio)anthraquinone.
[0164] Examples of α-aminoacetophenone-based photoradical polymerization initiators include 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one (trade name OMNIRAD907), 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone (trade name OMNIRAD369), and 2-dimethylamino-2-(4-methylbenzyl)-1-(4-morpholino-4-yl-phenyl)butan-1-one (trade name OMNIRAD379).
[0165] Examples of the triazine-based photoradical polymerization initiator include 2-(3,4-methylenedioxyphenyl)-4,6-bis(trichloromethyl)-1,3,5-triazine and 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-1,3,5-triazine.
[0166] Examples of the thioxanthone-based polymerization initiator include 2,4-diethylthioxanthone and 2-isopropylthioxanthone.
[0167] Examples of the acridine-based photoradical polymerization initiator include acridine, 1,7-bis(9,9'-acridinyl)heptane, 9-phenylacridine, 1,6-bis(9-acridinyl)hexane, 1,7-bis(9-acridinyl)heptane, 1,8-bis(9-acridinyl)octane, 1,9-bis(9-acridinyl)nonane, 1,10-bis(9-acridinyl)decane, 1,11-bis(9-acridinyl)undecane, and 1,12-bis(9-acridinyl)dodecane.
[0168] As described above, the oxime ester compound represented by general formula (1) or general formula (2) of the present invention alone has excellent activity as a photoradical polymerization initiator. However, by using another photoradical polymerization initiator in combination, the radical polymerizable compound can be polymerized at an even higher speed due to the synergistic effect of the photoradical polymerization initiator, and the compound can be applied to high-viscosity systems and systems with added pigments, and various physical properties such as surface properties and deep curing can be improved.
[0169] The addition ratio of the oxime ester compound represented by general formula (1) or general formula (2) of the present invention to the other photoradical polymerization initiator is not particularly limited, but the blending ratio of the photoradical polymerization initiator to the oxime ester compound represented by general formula (1) or general formula (2) of the present invention is preferably within the range of 99:1 to 1:99 by weight.
[0170] (Photopolymerization method) A polymer can be obtained by irradiating the photoradical polymerizable composition of the present invention with light to polymerize it. When irradiating the photoradical polymerizable composition with light to polymerize it and harden it, the photoradical polymerizable composition can be molded into a film and photopolymerized, or it can be molded into a block and photopolymerized. When molding into a film and photopolymerizing it, the liquid photoradical polymerizable composition is applied to a substrate such as a polyester film using a bar coater or the like so as to have a film thickness of 5 μm to 300 μm.
[0171] The substrates used are mainly films, paper, aluminum foil, metal, wood, plastic substrates, etc., but are not particularly limited. Materials used for the film as the substrate include polyvinyl chloride (PVC), polyethylene terephthalate (PET), polycarbonate (PC), polystyrene (PS), polyurethane (PU), polyethylene (PE), polypropylene (PP), etc. Examples include films or sheets of ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, ethylene-methacrylic acid copolymer, nylon, polylactic acid, polycarbonate, etc., cellophane, aluminum foil, or composite materials thereof. Paper such as fine paper, coated paper, art paper, imitation paper, thin paper, thick paper, various synthetic papers, etc., laminated with various films are also useful. In particular, plastic films such as PE and PP are preferred.
[0172] The method of applying the photoradical polymerizable composition of the present invention to the substrate film is not particularly limited, and for example, a bar coater, a roll coater, a gravure coater, a flexo coater, an air doctor coater, a blade coater, an air knife coater, a squeeze coater, an impregnation coater, a transfer roll coater, a kiss coater, a curtain coater, a cast coater, a spray coater, a die coater, a spin coater, an offset printing machine, a screen printing machine, etc. can be appropriately adopted. A method of applying the composition as droplets by an inkjet machine onto the substrate can also be adopted. Since the photoradical polymerizable composition of the present invention can be cured at a sufficient speed, it can be cured at the same time as being applied, and a cured film can be formed without going through complicated devices and processes. It is also possible to perform a heat treatment or the like after curing.
[0173] The coating film made of the photoradical polymerizable composition thus prepared is irradiated with energy rays of 1 to 1000 mW / cm 2 A photopolymerization product can be obtained by irradiating light with an intensity of about 100 nm. Examples of light sources used include high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, xenon lamps, gallium-doped lamps, black lights, ultraviolet LEDs with a central wavelength of 365 nm, 375 nm, 385 nm, 395 nm, or 405 nm, blue LEDs, white LEDs, Heraeus D bulbs, V bulbs, and the like. Natural light such as sunlight can also be used. The photoradical polymerization initiator of the present invention has ultraviolet absorption at 350 nm to 420 nm and has the ability to generate radical species by light in this wavelength range, so that an irradiation source that irradiates light with a wavelength range of 350 nm to 420 nm is particularly preferred, and in this sense, ultraviolet LEDs or semiconductor lasers with a central wavelength of 365 nm, 375 nm, 385 nm, 395 nm, or 405 nm are preferred. Examples of semiconductor lasers include blue-violet 405 nm semiconductor lasers, etc.
[0174] Photo-curable (Photo-DSC) In this example, the photocurability was evaluated by measuring the total calorific value by Photo-DSC as described below. A Hitachi High-Tech XDSC-7200 DSC measuring device was used, to which a photo-DSC measuring unit was attached so that DSC measurements could be performed while irradiating light. A Hayashi Lepic LA-410UV was used as the light source for light irradiation, and 405 nm light was extracted using a bandpass filter so that it could be irradiated onto the sample. The illuminance of the light was 50 mW / cm. 2 The light source was made to be guided to the top of the sample using glass fiber, and the shutter of the light source was made trigger-controlled so that DSC measurement could be performed simultaneously with the start of light irradiation. For the light DSC measurement, about 1 mg of the sample was precisely weighed in an aluminum pan for measurement, placed in the DSC measurement section, and then the light DSC unit was attached. Then, the inside of the measurement section was kept in a nitrogen atmosphere, and light was irradiated for 300 seconds from 30 seconds after the start of measurement. After the first measurement, the sample was measured again under the same conditions, and the value obtained by subtracting the second measurement result from the first measurement result was used as the heat generation measurement result of the photoradical polymerizable composition, and the total heat generation amount for 5 seconds and 5 minutes from the start of light irradiation was calculated. When polymerization of the photoradical polymerizable composition occurs, reaction heat is generated due to polymerization, but the reaction heat can be measured by the light DSC. Therefore, the progress of polymerization due to light irradiation can be measured by the light DSC. In this example, the total heat generation amount for 5 seconds and 5 minutes after light irradiation was measured, but as long as the same polymerizable compound is used, it can be considered that the larger the value, the more efficiently the polymerization proceeds when comparing the values. EXAMPLES
[0175] The present invention will be described in detail below with reference to examples, which are presented for illustrative purposes. That is, the following examples are not intended to be exhaustive or to limit the present invention to the exact form described. Thus, the present invention is not limited to the following described examples, unless it exceeds the spirit of the present invention. In addition, all parts and percentages are by weight, unless otherwise specified.
[0176] (Synthesis Example 1) Synthesis of 9,10-bis(methylcarbonylmethyleneoxy)anthracene In a 100mL four-neck flask equipped with a stirrer and a thermometer, 30g of the solvent methyl isobutyl ketone, 6.0g (59.5mmol) of the catalyst triethylamine, and 5.0g (23.8mmol) of 9,10-dihydroxyanthracene were added under a nitrogen atmosphere. While maintaining the temperature of the reaction system at 20-25°C, 10.9g (71.4mmol) of 90% bromoacetone was added dropwise over 10 minutes. After the dropwise addition, the mixture was stirred for another 2 hours. The reaction solution was then suction filtered and washed with pure water to obtain a pale yellow solid with a yield of 5.7g (74.1mol%).
[0177] IR(cm -1 ):1727,1378,1353,1170,1086,774,692,673,623. Melting point: 180-183℃ 1 H-NMR (400MHz, CDCl3): δ=2.446(s,6H),4.766(s,4H),7.509-7.533(m,4H),8.241-8.266(m,4H).
[0178] (Synthesis Example 2) Synthesis of 9,10-bis[(2-hydroxyimino)propyleneoxy]anthracene In a 50 mL four-neck flask equipped with a stirrer and a thermometer, 10 g of the solvent pyridine, 3.0 g (42.9 mmol) of hydroxylamine hydrochloride, and 2.5 g (7.8 mmol) of 9,10-bis(methylcarbonylmethyleneoxy)anthracene obtained in Synthesis Example 1 were added under a nitrogen atmosphere. The reaction system was stirred for 3 hours while maintaining the temperature at 90 to 95°C. The reaction solution was cooled, and 30 g of 1N hydrochloric acid was added. The precipitated solid was filtered by suction and washed with pure water to obtain an orange solid with a yield of 1.9 g (yield 72.3 mol%).
[0179] IR(cm -1 ):1365,1349,1323,1053,1019,949,936,759,690,642. Melting point: 210-215℃ (thermal decomposition) 1 H-NMR (400MHz, CDCl3): δ=2.313(s,6H),4.697(s,4H),7.802-7.825(m,4H),8.319-8.341(m,4H).
[0180] (Synthesis Example 3) Synthesis of 9,10-bis[(2-acetoxyimino)propyleneoxy]anthracene (Compound 2-1) In a 50 mL four-neck flask equipped with a stirrer and a thermometer, 10 g of the solvent pyridine, 23 mg (0.19 mmol) of the catalyst 4-dimethylaminopyridine, and 1.0 g (2.8 mmol) of the 9,10-bis[(2-hydroxyimino)propyleneoxy]anthracene obtained in Synthesis Example 2 were added under a nitrogen atmosphere. While maintaining the temperature of the reaction system at 30 to 35°C, 1.4 g (13.3 mmol) of acetic anhydride was added dropwise over 10 minutes. After the dropwise addition, the mixture was stirred for another 2 hours. The reaction solution was then concentrated under reduced pressure, and 10 g of pure water was added. This was filtered by suction and washed with pure water to obtain an orange solid with a yield of 0.92 g (72.4 mol%).
[0181] IR(cm -1 ):1762,1350,1194,1169,1166,1006,934,903,772,620. Melting point: 170-173℃ 1 H-NMR (400MHz, CDCl3): δ=2.258(s,6H),2.484(s,6H),4.843(s,4H),7.505-7.542(m,4H),8.242-8.279(m,4H).
[0182] (Synthesis Example 4) Synthesis of 9,10-bis(tert-butylcarbonylmethyleneoxy)anthracene In a 100mL four-neck flask equipped with a stirrer and a thermometer, 20g of methyl isobutyl ketone as a solvent, 6.0g (59.5mmol) of triethylamine as a catalyst, and 5.0g (23.8mmol) of 9,10-dihydroxyanthracene were added under a nitrogen atmosphere. While maintaining the temperature of the reaction system at 60-65°C, a solution of 12.6g (66.6mmol) of 95% 1-bromo pinacoline dissolved in 10g of methyl isobutyl ketone was added dropwise over 20 minutes. After the dropwise addition, the mixture was stirred for another 2 hours. The reaction solution was then cooled, and 50g of pure water was added to separate the liquid. The organic layer was taken out and filtered by suction to remove the precipitated insoluble matter. The filtrate was then concentrated under reduced pressure to obtain a light brown solid with a yield of 5.21g (yield 53.9mol%).
[0183] IR(cm -1 ):3240,2963,1388,1346,1078,1056,944,767,739,694,668. Melting point: 153-156℃ 1 H-NMR (400MHz, CDCl3): δ=1.239(s,18H),5.020(s,4H),7.493-7.518(m,4H),8.257-8.282(m,4H).
[0184] (Synthesis Example 5) Synthesis of 9,10-bis[(2-hydroxyimino)-3,3'-dimethylbutyleneoxy]anthracene In a 100 mL four-neck flask equipped with a stirrer and a thermometer, 14 g of the solvent pyridine, 2.1 g (30.7 mmol) of hydroxylamine hydrochloride, and 2.5 g (6.1 mmol) of 9,10-bis(tert-butylcarbonylmethyleneoxy)anthracene obtained in Synthesis Example 4 were added under a nitrogen atmosphere. The reaction system was stirred for 2 hours while maintaining the temperature at 90 to 95°C. The reaction solution was cooled, and 24 g of 1N hydrochloric acid was added. The precipitated solid was filtered by suction and washed with pure water to obtain an orange solid with a yield of 2.2 g (yield 81.9 mol%).
[0185] IR(cm -1 ):2968,1720,1388,1368,1060,973,772,673,560. Melting point: 145-148℃ (thermal decomposition) 1 H-NMR (400MHz, CDCl3): δ=1.377(s,18H),4.986(s,6H),7.483-7.509(m,4H),8.459-8.484(m,4H).
[0186] (Synthesis Example 6) Synthesis of 9,10-bis[(2-acetoxyimino)-3,3'-dimethylbutyleneoxy]anthracene (Compound 2-4) In a 50 mL four-neck flask equipped with a stirrer and a thermometer, 10 g of the solvent pyridine, 17 mg (0.14 mmol) of the catalyst 4-dimethylaminopyridine, and 1.0 g (2.3 mmol) of the 9,10-bis[(2-hydroxyimino)-3,3'-dimethylbutyleneoxy]anthracene obtained in Synthesis Example 5 were added under a nitrogen atmosphere. While maintaining the temperature of the reaction system at 30 to 35°C, 1.4 g (13.3 mmol) of acetic anhydride was added dropwise over 10 minutes. After the dropwise addition, the mixture was stirred for another 2 hours. The reaction solution was then concentrated under reduced pressure, and 10 g of pure water was added. This was filtered by suction and washed with pure water to obtain an orange solid with a yield of 0.50 g (41.9 mol%).
[0187] IR(cm -1 ):2965,1769,1390,1348,1198,1078,999,919,874,772,674. Melting point: 110-114℃ 1 H-NMR (400MHz, CDCl3): δ=1.490(s,18H),1.984(s,6H),5.005(s,4H),7.516-7.540(m,4H),8.323-8.347(m,4H).
[0188] (Synthesis Example 7) Synthesis of 9,10-bis(methylcarbonylbutyleneoxy)anthracene In a 100mL four-neck flask equipped with a stirrer and a thermometer, 30g of DMF as a solvent, 3.75g (5.82mmol) of 50% aqueous tetrabutylammonium chloride as a catalyst, and 11.8g (87.3mmol) of chlorohexanone were added under a nitrogen atmosphere. While maintaining the temperature of the reaction system at 110-120°C, 30.0g (29.1mmol) of 20.4% aqueous 9,10-dihydroxyanthracene solution was added dropwise over 1 hour. After the dropwise addition, the mixture was stirred for another 3 hours. The reaction solution was then cooled and subjected to suction filtration, and the obtained solid was washed with pure water to obtain a pale yellow solid with a yield of 6.3g (yield 52.8mol%).
[0189] IR(cm -1 ):2947, 1709, 1353, 1342, 1158, 1069, 1054, 786, 759, 682. Melting point: 89-91℃ 1 H-NMR (400MHz, CDCl3): 1.932-2.090(m, 8H), 2.204(s, 6H), 2.633(t, 4H), 4.179(t, 4H), 7.456-7.494(m, 4H), 8.237-8.262(m, 4H).
[0190] (Synthesis Example 8) Synthesis of 9,10-bis[(2-hydroxyimino)hexeneoxy]anthracene In a 100 mL four-neck flask equipped with a stirrer and a thermometer, 30 g of the solvent pyridine, 5.1 g (73.8 mmol) of hydroxylamine hydrochloride, and 6.0 g (14.8 mmol) of 9,10-bis(methylcarbonylbutyleneoxy)anthracene obtained in Synthesis Example 7 were added under a nitrogen atmosphere. The mixture was stirred for 3 hours while maintaining the temperature of the reaction system at 90 to 95°C. The reaction solution was cooled, and the precipitated solid was filtered by suction. The obtained solid was washed with pure water to obtain a white solid with a yield of 5.3 g (yield 81.8 mol%).
[0191] IR(cm -1 ): 3237, 2949, 1403, 1359, 1342, 1067, 945, 760. Melting point: 170-173℃ (thermal decomposition) 1 H-NMR (400MHz, DMSO): 1.784(s, 6H), 1.824(m, 4H), 1.973(m, 4H), 2.265(t, 4H), 4.110(t, 4H), 7.543-7.567(m, 4H), 8.207-8.247(m, 4H).
[0192] (Synthesis Example 9) Synthesis of 9,10-bis[(2-acetoxyimino)hexeneoxy]anthracene (Compound 2-30) In a 100 mL four-neck flask equipped with a stirrer and a thermometer, 40 g of the solvent pyridine, 84 mg (0.69 mmol) of the catalyst 4-dimethylaminopyridine, and 5.0 g (11.5 mmol) of the 9,10-bis[(2-hydroxyimino)hexeneoxy]anthracene obtained in Synthesis Example 8 were added under a nitrogen atmosphere. While maintaining the temperature of the reaction system at 30 to 35°C, 7.0 g (68.7 mmol) of acetic anhydride was added dropwise over 10 minutes. After the dropwise addition, the mixture was stirred for another 2 hours. The reaction solution was then concentrated under reduced pressure, and 20 g of pure water was added. This was filtered by suction and washed with pure water to obtain a yellow solid with a yield of 5.33 g (yield 89.4 mol%).
[0193] IR(cm -1 ): 2939, 1757, 1357, 1206, 1062, 985, 940, 873, 778, 681. Melting point: 123-126℃ 1 H-NMR (400MHz, CDCl3): 1.951-2.054(m, 8H), 2.062(s, 6H), 2.190(s, 6H), 2.532(t, 4H), 4.179(t, 4H), 7.475-7.492(m, 4H), 8.228-8.252(m, 4H).
[0194] [Photoradical polymerization curing speed] (Evaluation Example 1) As a radical polymerizable compound, 0.1 parts by weight of 9,10-bis[(2-acetoxyimino)propyleneoxy]anthracene (compound 2-1) was added as a photoradical polymerization initiator to 100 parts by weight of trimethylolpropane triacrylate, and the mixture was stirred and dissolved to obtain a photoradical polymerizable composition. When this photoradical polymerizable composition was subjected to Photo-DSC measurement, the total heat generation amount for 5 minutes from the start of light irradiation was 237 mJ / mg. The results are shown in Table 1.
[0195] (Evaluation Example 2) Photo-DSC measurement was carried out under the same conditions as in Evaluation Example 1, except that 0.1 parts by weight of 9,10-bis[(2-acetoxyimino)-3,3'-dimethylbutyleneoxy]anthracene (compound 2-4) was used as the photoradical polymerization initiator instead of 0.1 parts by weight of 9,10-bis[(2-acetoxyimino)propyleneoxy]anthracene. The total heat generation amount for 5 minutes from the start of light irradiation was 347 mJ / mg. The results are shown in Table 1.
[0196] (Evaluation Example 3) Photo-DSC measurement was carried out under the same conditions as in Evaluation Example 1, except that 0.1 parts by weight of 9,10-bis[(2-acetoxyimino)hexeneoxy]anthracene (compound 2-30) was used as the photoradical polymerization initiator instead of 0.1 parts by weight of 9,10-bis[(2-acetoxyimino)propyleneoxy]anthracene. The total heat generation amount for 5 minutes from the start of light irradiation was 138 mJ / mg. The results are shown in Table 1.
[0197] (Evaluation Comparison Example 1) Photo-DSC measurement was carried out under the same conditions as in Evaluation Example 1, except that 0.1 parts by weight of Irgacure OXE02 was used instead of 0.1 parts by weight of 9,10-bis[(2-acetoxyimino)propyleneoxy]anthracene as the photoradical polymerization initiator. The total heat generation amount for 5 minutes from the start of light irradiation was 204 mJ / mg. The results are shown in Table 1 (Irgacure is a registered trademark of BASF Co., Ltd.).
[0198] [Table 1]
[0199] As is clear from the results of Evaluation Examples 1, 2, and 3, the oxime ester compound having an anthracene skeleton of the present invention acts as a radical polymerization initiator by irradiation with light of a single long wavelength of 405 nm. Also, as is clear from a comparison with Evaluation Comparative Example 1, this initiation ability is superior to the results of using Irgacure OXE02 (ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(o-acetyloxime), a known oxime ester photopolymerization initiator that is said to have an absorption band suitable for long-wavelength exposure and high reactivity, and the oxime ester compound having an anthracene skeleton of the present invention has an excellent polymerization initiation effect. And, it is found that the activity of the compound in which A is a methylene group in the general formula is extremely high.
[0200] (Evaluation Example 4) Photo-DSC measurement was carried out under the same conditions as in Evaluation Example 1, except that 0.01 part by weight of 9,10-bis[(2-acetoxyimino)-3,3'-dimethylbutyleneoxy]anthracene (compound 2-4) was used as the photoradical polymerization initiator instead of 0.1 part by weight of 9,10-bis[(2-acetoxyimino)propyleneoxy]anthracene. The total heat generation amount for 5 minutes from the start of light irradiation was 208 mJ / mg. The results are shown in Table 2.
[0201] (Evaluation Example 5) Photo-DSC measurement was carried out under the same conditions as in Evaluation Example 1, except that 0.5 parts by weight of 9,10-bis[(2-acetoxyimino)-3,3'-dimethylbutyleneoxy]anthracene (compound 2-4) was used as the photoradical polymerization initiator instead of 0.1 parts by weight of 9,10-bis[(2-acetoxyimino)propyleneoxy]anthracene. The total heat generation amount for 5 minutes from the start of light irradiation was 443 mJ / mg. The results are shown in Table 2.
[0202] (Evaluation Example 6) Photo-DSC measurement was carried out under the same conditions as in Evaluation Example 1, except that 1 part by weight of 9,10-bis[(2-acetoxyimino)-3,3'-dimethylbutyleneoxy]anthracene (compound 2-4) was used as the photoradical polymerization initiator instead of 0.1 part by weight of 9,10-bis[(2-acetoxyimino)propyleneoxy]anthracene. The total heat generation amount for 5 minutes from the start of light irradiation was 505 mJ / mg. The results are shown in Table 2.
[0203] (Evaluation Example 7) Photo-DSC measurement was carried out under the same conditions as in Evaluation Example 1, except that 2 parts by weight of 9,10-bis[(2-acetoxyimino)-3,3'-dimethylbutyleneoxy]anthracene (compound 2-4) was used as the photoradical polymerization initiator instead of 0.1 parts by weight of 9,10-bis[(2-acetoxyimino)propyleneoxy]anthracene. The total heat generation amount for 5 minutes from the start of light irradiation was 497 mJ / mg. The results are shown in Table 2.
[0204] [Table 2]
[0205] As is clear from the results of photocuring rate evaluation Examples 4 to 8, the oxime ester compound having an anthracene skeleton of the present invention shows sufficient activity in photoradical polymerization even at a blending amount of 0.01 parts by weight. In particular, the total heat generation increases sharply at 0.1 parts by weight or more, and it is clear that the polymerization reaction is significantly promoted.
[0206] (Evaluation Example 8) As a radical polymerizable compound, 0.1 parts by weight of 9,10-bis[(2-acetoxyimino)propyleneoxy]anthracene (compound 2-1) was added as a photoradical polymerization initiator to 100 parts by weight of trimethylolpropane triacrylate, and the mixture was stirred and dissolved to obtain a photoradical polymerizable composition. When this photoradical polymerizable composition was subjected to Photo-DSC measurement, the total heat generation amount for 5 seconds from the start of light irradiation was 58 mJ / mg. The results are shown in Table 3.
[0207] (Evaluation Example 9) Photo-DSC measurement was carried out under the same conditions as in Evaluation Example 1, except that 0.1 parts by weight of 9,10-bis[(2-acetoxyimino)-3,3'-dimethylbutyleneoxy]anthracene (compound 2-4) was used as the photoradical polymerization initiator instead of 0.1 parts by weight of 9,10-bis[(2-acetoxyimino)propyleneoxy]anthracene. The total heat generation during the first 5 seconds from the start of irradiation was 161 mJ / mg. The results are shown in Table 3.
[0208] (Evaluation Comparison Example 2) Photo-DSC measurement was performed under the same conditions as in Evaluation Example 1, except that 0.1 parts by weight of Irgacure OXE02 was used instead of 0.1 parts by weight of 9,10-bis[(2-acetoxyimino)propyleneoxy]anthracene as the photoradical polymerization initiator. The total heat generation during the first 5 seconds from the start of irradiation was 3 mJ / mg. The results are shown in Table 3.
[0209] [Table 3]
[0210] Evaluation Examples 8 and 9 and Evaluation Comparative Example 2 are the results of measuring the amount of heat generated immediately (5 seconds) after light irradiation. As is clear from these results, the oxime ester compound having an anthracene skeleton of the present invention initiates polymerization immediately after irradiation, as compared with Irgacure OXE02, a known oxime ester photopolymerization initiator, and it is apparent that the compound quickly releases polymerization initiating species.
[0211] The results of the change in heat release over time are plotted in Figure 1, with the heat release on the vertical axis and the time after irradiation on the horizontal axis. The solid and dashed lines are the graphs for the oxime ester having an anthracene skeleton of the present invention, and the dotted line is Irgacure OXE02. It is clear that the oxime ester compound having an anthracene skeleton of the present invention shows extremely high activity immediately after irradiation.
Claims
1. An oxime ester compound having an anthracene skeleton represented by the following general formula (1): 【Chemistry 1】 (In the general formula (1), R 1 and R 2 each independently represents a linear or branched alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, a cycloalkylalkyl group having 4 to 12 carbon atoms, an alkylcycloalkyl group having 4 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms; R 3 represents a linear or branched alkyl group having 1 to 10 carbon atoms, A represents a linear or branched alkylene group having 1 to 20 carbon atoms, m represents an integer of 0 to 3, and n represents an integer of 1 to 3.
2. 2. The oxime ester compound having an anthracene skeleton according to claim 1, wherein A is a methylene group.
3. An oxime ester compound having an anthracene skeleton represented by the following general formula (2): 【Chemistry 2】 (In the general formula (2), R 1 and R 2 each independently represents a linear or branched alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, a cycloalkylalkyl group having 4 to 12 carbon atoms, an alkylcycloalkyl group having 4 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms; R 3 represents a linear or branched alkyl group having 1 to 10 carbon atoms, A represents a linear or branched alkylene group having 1 to 20 carbon atoms, and m represents an integer of 0 to 3.
4. 4. The oxime ester compound having an anthracene skeleton according to claim 3, wherein A is a methylene group.
5. R 2 The oxime ester compound having an anthracene skeleton according to any one of claims 1 to 4, characterized in that: is a methyl group.
6. A method for producing an oxime ester compound having an anthracene skeleton represented by the following general formula (1), by etherifying a hydroxy group of an anthracene compound having a hydroxy group represented by the following general formula (3) with an etherifying agent having a ketone group, then oximating the ketone group with an oximating agent, and then esterifying the hydroxyoxime group. 【Chemistry 3】 (In the general formula (3), R 3 represents a linear or branched alkyl group having 1 to 10 carbon atoms, m represents an integer of 0 to 3, and n represents an integer of 1 to 3. 【Chemistry 4】 (In the general formula (1), R 1 and R 2 each independently represents a linear or branched alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, a cycloalkylalkyl group having 4 to 12 carbon atoms, an alkylcycloalkyl group having 4 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms; R 3 represents a linear or branched alkyl group having 1 to 10 carbon atoms, A represents a linear or branched alkylene group having 1 to 20 carbon atoms, m represents an integer of 0 to 3, and n represents an integer of 1 to 3.
7. A method for producing an oxime ester compound having an anthracene skeleton represented by the following general formula (2), by etherifying a hydroxy group of an anthracene compound having a hydroxy group represented by the following general formula (9) with an etherifying agent having a ketone group, then oximating the ketone group with an oximating agent, and then esterifying the hydroxyoxime group. 【Chemistry 5】 (In the general formula (9), R 3 represents a linear or branched alkyl group having 1 to 10 carbon atoms; and m represents an integer of 0 to 3. 【Chemistry 6】 (In the general formula (2), R 1 and R 2 each independently represents a linear or branched alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, a cycloalkylalkyl group having 4 to 12 carbon atoms, an alkylcycloalkyl group having 4 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms; R 3 represents a linear or branched alkyl group having 1 to 10 carbon atoms, A represents a linear or branched alkylene group having 1 to 20 carbon atoms, and m represents an integer of 0 to 3.
8. A photoradical polymerization initiator comprising the oxime ester compound having an anthracene skeleton according to claim 1 .
9. A polymerizable composition comprising the photoradical polymerization initiator according to claim 8 and a radically polymerizable compound.
10. A polymerizable composition according to claim 9, further comprising an alkali-soluble resin.
11. A method for photopolymerizing a polymerizable composition, comprising irradiating the polymerizable composition according to claim 9 with energy rays containing light having a peak wavelength in the range of 350 nm to 420 nm.
12. A method for photopolymerizing a polymerizable composition, comprising irradiating the polymerizable composition according to claim 10 with energy rays containing light having a peak wavelength in the range of 350 nm to 420 nm.
13. The method for photopolymerizing a polymerizable composition according to claim 11, wherein the light source emitting light having a peak wavelength in the wavelength range of 350 nm to 420 nm is an ultraviolet LED or a 405 nm semiconductor laser having a peak wavelength of any of 365 nm, 385 nm, 395 nm, 405 nm, or 415 nm.
14. The method for photopolymerizing a polymerizable composition according to claim 12, wherein the light source emitting light having a peak wavelength in the wavelength range of 350 nm to 420 nm is an ultraviolet LED or a 405 nm semiconductor laser having a peak wavelength of any of 365 nm, 385 nm, 395 nm, 405 nm, or 415 nm.
Citation Information
Patent Citations
Photoinitiator of oxime ester
JP2001233842A
Oxime ester compound and photopolymerization initiator containing the same
JP2004359639A
Oxime ester compound, radical polymerization initiator, and polymerizable composition
JP2007210991A
Oxime ester-based compound, photopolymerization initiator, photopolymerizable composition, color filter and liquid crystal display
JP2008179611A
Nitro group-containing bisoxime ester-based photopolymerization initiator and its synthetic production method and application
JP2017508738A