Apparatus and method for recovering carbon fibers and glass fibers from composite material
The apparatus and method efficiently recover carbon and glass fibers from waste blades by crushing, pyrolyzing, and separating them using controlled atmospheres and density-based methods, addressing the recycling challenge of composite materials.
Patent Information
- Application Number
- JP2024017959
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-05
- Filing Date
- 2024-02-08
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-02-08
AI Technical Summary
The disposal of waste blades from wind power generators, which are made of composite materials like carbon fiber reinforced plastics or glass fiber reinforced plastics, is challenging due to their difficulty in recycling and the increasing landfill burden.
A recovery apparatus and method involving a pretreatment unit, first and second reaction units, and a separation unit to separate carbon fibers and glass fibers from waste blades through crushing, rolling, pyrolysis, and density-based separation, with controlled temperature and oxygen levels to maintain a reducing atmosphere.
Enables the effective recovery of carbon fibers and glass fibers from waste blades in a single process, achieving high purity and reducing environmental waste.
Smart Images

Figure 2024149385000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an apparatus and method for recovering carbon and glass fibers from composite materials. [Background technology]
[0002] Wind power generation is a method of generating electricity by using the kinetic energy of the wind to rotate blades, converting it into mechanical energy, and then converting that mechanical energy into electrical energy. It is increasingly being used as an alternative to existing power generation methods that mainly use fossil fuels.
[0003] A wind turbine has multiple blades attached to the rotating shaft of the generator. The blades are made long and wide to produce more electrical energy. The larger the blade, the heavier it becomes. However, the blades must be made as light as possible for energy efficiency. Also, as the blades constantly collide with the wind, their strength must be improved to ensure durability. To solve this problem, carbon fiber reinforced plastic or glass fiber reinforced plastic is used as the material for the blades. Composite materials containing carbon fiber and glass fiber are light yet strong, and are used in a variety of fields other than blades, such as the automotive, space, aviation, and defense industries.
[0004] However, when wind turbine blades break or reach the end of their life, disposal of the waste blades becomes an issue. Generally, composite materials such as carbon fiber reinforced plastics or glass fiber reinforced plastics are difficult to recycle and are mostly landfilled. However, it is impossible to continue to landfill the increasing amount of composite material waste, and the need for disposal methods other than landfilling or recycling methods has been continuously raised.
[0005] Therefore, there is a need to develop an apparatus and method capable of recovering carbon fibers or glass fibers from used waste blades. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Republic of Korea Patent No. 10-1810284 (Name: Method for separating carbon fiber from waste carbon fiber reinforced plastic) Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a recovery device and a recovery method capable of separating carbon fibers or glass fibers from a composite material.
[0008] The present invention aims to provide an apparatus and method for recovering carbon fibers and glass fibers from composite materials, which can recover carbon fibers and glass fibers, respectively, from waste composite materials discarded in the fields of scrap blades, aerospace and defense industries, etc., in a single process. [Means for solving the problem]
[0009] An apparatus for recovering carbon fibers and glass fibers from a composite material according to an embodiment of the present invention includes a pre-treatment unit, a first reaction unit, a second reaction unit, and a separation unit. The pre-treatment unit may include a crushing module for crushing waste blades, and a rolling module for rolling the crushed waste blades. The first reaction unit may perform primary pyrolysis on the pre-treated crushing blades. The second reaction unit may perform secondary pyrolysis on the crushing blades subjected to primary pyrolysis. The separation unit may include a separation section for separating a result of secondary pyrolysis into a first material and a second material, a first chamber for accommodating the first material, and a second chamber for accommodating the second material.
[0010] The apparatus for recovering carbon and glass fibers from a composite material according to an embodiment of the present invention may further include a cutting unit for cutting the blade to a predetermined length.
[0011] The apparatus for recovering carbon fibers and glass fibers from a composite material according to an embodiment of the present invention may further include a temperature control unit for controlling the temperature inside the pre-treatment unit, the first reaction unit, and the second reaction unit.
[0012] In the apparatus for recovering carbon fibers and glass fibers from composite materials according to one embodiment of the present invention, the crushing module may be provided with a suction section for sucking in dust within the crushing module.
[0013] In an apparatus for recovering carbon fibers and glass fibers from a composite material according to an embodiment of the present invention, the pre-treatment unit may include a screening module between the crushing module and the rolling module.
[0014] In the apparatus for recovering carbon fibers and glass fibers from a composite material according to an embodiment of the present invention, the input section of the rolling module may include a first input section and a second input section.
[0015] In the apparatus for recovering carbon fibers and glass fibers from a composite material according to an embodiment of the present invention, nitrogen is supplied when the second input port is opened.
[0016] In an apparatus for recovering carbon and glass fibers from composite materials according to one embodiment of the present invention, gas exhausted from the interior of the rolling module can be recirculated into the rolling module.
[0017] In the apparatus for recovering carbon fibers and glass fibers from a composite material according to an embodiment of the present invention, the temperature inside the first reaction unit may be 400 to 500°C.
[0018] In the apparatus for recovering carbon and glass fibers from composite materials according to one embodiment of the present invention, the oil vapor generated in the first reaction unit is cooled in the temperature control unit and extracted as oil.
[0019] In an apparatus for recovering carbon fibers and glass fibers from composite materials according to one embodiment of the present invention, the second reaction unit may be provided with a sensor for measuring the oxygen concentration in the second reaction unit and an external air tank for supplying external air into the second reaction unit.
[0020] A method for recovering carbon fiber and glass fiber from a composite material according to an embodiment of the present invention includes the steps of crushing a waste blade cut in a longitudinal direction, continuously feeding the crushed waste blade into a rolling module, rolling the crushed waste blade, a first pyrolysis step of primarily pyrolyzing the rolled crushed blade, a second pyrolysis step of secondarily pyrolyzing the primarily pyrolyzed crushed blade, and separating a resultant of the second pyrolysis step. The temperatures in the rolling step, the first pyrolysis step, and the second pyrolysis step are regulated by a temperature regulating unit.
[0021] The method for recovering carbon fibers and glass fibers from a composite material according to one embodiment of the present invention may further include a step of screening the crushed waste blades after the step of crushing the waste blades.
[0022] In a method for recovering carbon fibers and glass fibers from a composite material according to an embodiment of the present invention, the input section of the rolling module may include a first input section and a second input section, and in the step of continuously inputting the crushed waste blades into the rolling module, the first input section and the second input section are opened sequentially.
[0023] In the method for recovering carbon fibers and glass fibers from a composite material according to an embodiment of the present invention, exhaust gas inside a rolling module during the rolling step can be recirculated into the rolling module.
[0024] In the method for recovering carbon fibers and glass fibers from a composite material according to an embodiment of the present invention, the temperature in the first pyrolysis step may be 400 to 500°C. Effect of the Invention
[0025] According to an embodiment of the present invention, carbon or glass fibers can be effectively separated from a composite material.
[0026] According to an embodiment of the present invention, carbon fibers and glass fibers can be recovered from waste blades in a single process. [Brief description of the drawings]
[0027] [Figure 1] FIG. 1 is a block diagram illustrating a carbon fiber and glass fiber recovery apparatus for a composite material according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram showing a pre-treatment unit in an apparatus for recovering carbon fibers and glass fibers from composite materials according to an embodiment of the present invention. [Diagram 3] A diagram showing a separation unit in an apparatus for recovering carbon fibers and glass fibers from a composite material according to an embodiment of the present invention. [Figure 4] 1 is a flowchart showing a method for recovering carbon fibers and glass fibers from a composite material according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] Although the present invention can be implemented in various ways, a specific embodiment will be described in detail in the detailed description, but it is not intended to limit the present invention to the specific embodiment, and it should be understood that the present invention includes all modifications, equivalents, or alternatives within the spirit and technical scope of the present invention.
[0029] The terms used in the present invention are merely used to describe specific embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless the context clearly indicates otherwise. In the present invention, the terms "include" or "have" are intended to specify the presence of features, numbers, steps, operations, components, parts, or combinations thereof described in the specification, and should be understood not to preclude the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.
[0030] Hereinafter, a preferred embodiment of the present invention will be described in detail with reference to the accompanying drawings. At this time, it should be noted that in the accompanying drawings, the same components are represented by the same reference numerals as much as possible. Also, detailed description of known functions and configurations that may obscure the gist of the present invention will be omitted. For the same reason, in the accompanying drawings, some components are exaggerated, omitted, or illustrated in a schematic manner.
[0031] FIG. 1 is a block diagram showing an outline of an apparatus for recovering carbon fibers and glass fibers from composite materials according to an embodiment of the present invention, FIG. 2 is a diagram showing a pre-processing unit in an apparatus for recovering carbon fibers and glass fibers from composite materials according to an embodiment of the present invention, and FIG. 3 is a diagram showing a separation unit in an apparatus for recovering carbon fibers and glass fibers from composite materials according to an embodiment of the present invention.
[0032] As shown in FIG. 1, the composite material separating apparatus 1000 according to the present invention includes a cutting unit 1100, a pre-treatment unit 1200, a first reaction unit 1300, a second reaction unit 1400, a separation unit 1500 and a temperature adjustment unit 1600.
[0033] The cutting unit 1100 cuts the collected waste blades to a predetermined size. The waste blades are as long as 50 m, so it is not easy to feed them into a crusher. Therefore, the waste blades are cut in the longitudinal direction to facilitate smooth feeding into the crushing equipment. To facilitate smooth loading and unloading, the waste blades are cut to lengths of 10 m or less, using a wire saw or the like. The waste blades may be moved from the place where they are collected to the cutting device, but to facilitate the movement, the cutting operation may be performed immediately at the place where they are collected.
[0034] The cut waste blades are crushed and rolled in the pre-treatment unit 1200. As shown in Fig. 2, the pre-treatment unit 1200 includes a crushing module 1210, a rolling module 1220, and a screening module 1230. The waste blades cut to a predetermined length are fed into the crushing module 1210 and crushed. The waste blades are crushed to a thickness of 20 mm or less.
[0035] A large amount of dust is generated during the crushing process of the waste blades. The input port of the crushing module 1210 is sealed to prevent the dust from flowing out of the crushing module 1210. A positive pressure hood is provided on the upper end of the crushing module 1210. Exhaust gas can flow in through the positive pressure hood. The exhaust gas is supplied from a temperature control unit, which will be described later.
[0036] In addition, the crushing module 1210 may include a dust suction unit to remove dust within the crushing module 1210. The dust suction unit may suck in dust within the crushing module 1210 generated during the crushing process of the waste blades and collect it in a predetermined space. To collect dust, air may be continuously circulated within the crushing module 1210.
[0037] The crushed scrap blades are transported to the rolling module 1220 for rolling. Conveyors are used to transport the scrap blades to each unit and each module in the recovery process. Multiple conveyors may be provided consecutively or overlapping along the scrap blade travel path.
[0038] Meanwhile, the waste blades crushed in the crushing module 1210 are screened in the screening module 1230 before being fed into the rolling module 1220. The crushed waste blades have different particle sizes. When the waste blades with different particle sizes are pyrolyzed in the first reaction unit, the small waste blade fragments may be carbonized quickly and contaminate the primary pyrolysis result. Therefore, the crushed waste blades can be filtered on a screen, and if the size of the crushed particles is less than a predetermined size, they can be separated under the screen. The screen may be vibrated to facilitate the separation of small particles. The mesh size of the screen may be 5 mm. Through screening, the waste blade particles with a particle size of 5 mm or more are transported to the rolling module 1220.
[0039] The dust and screened particles collected by suction in the crushing module 1210 can be transferred to a separate combustion line for pyrolysis.
[0040] The crushed blades from which small particles have been removed while passing through the screen are moved to the rolling module 1220. The crushed waste blades are continuously fed into the rolling module 1220 in predetermined amounts.
[0041] The crushed waste blades are not uniform in particle size, and it is not easy to feed them in a fixed amount. In order to feed the crushed waste blades in a fixed amount, the present invention employs a semi-batch type feeder. In order to feed a fixed amount of waste blades into the rolling module 1220, the feed section of the rolling module 1220 may have a double-lid structure. The feed section of the rolling module 1220 may include a first feed section and a second feed section. The first feed section and the second feed section may be controlled to be opened sequentially, not simultaneously. The first feed section and the second feed section may be opened in a sliding manner, and the degree to which they are opened can be adjusted according to the amount to be fed. In this embodiment, the feed section forms a double structure, but is not limited thereto, and may include three or more gates on the feed port side. Each gate can be moved within a predetermined range by a gate valve. By opening each of the multiple gates, a desired amount of crushed waste blades can be fed into the rolling module 1220. In addition, such a semi-batch method allows the waste blades to be continuously fed into the rolling module 1220, and the waste blades rolled in the first reaction unit 1300 can be continuously supplied.
[0042] In addition, due to the dual structure of the input part of the rolling module 1220, when the crushed waste blades are input into the rolling module 1220, the inflow of oxygen can be minimized. The first input part of the rolling module 1220 is opened with the second input part closed. After the first input part is opened and a predetermined amount of waste blades is input, the first input part is closed and the rolling module 1220 is sealed, and the second input part is opened. At the same time as the second input part is opened, nitrogen purging is performed. Nitrogen is supplied into the rolling module while the second input part is open, and when the second input part is closed again, the supply of nitrogen is stopped. The waste blades are input into the rolling chamber of the rolling module 1220 by opening the second input part. Due to the dual sealing structure and the supply of nitrogen, the inflow of oxygen into the rolling module 1220 can be minimized.
[0043] A reducing atmosphere can be maintained inside the chamber of the rolling module 1220. To maintain the reducing atmosphere, gas exhausted from inside the chamber of the rolling module 1220 can be recirculated inside the rolling module. The exhaust gas includes nitrogen, carbon dioxide, and the like. One or more oxygen measuring sensors are disposed inside the rolling module 1220. The oxygen concentration inside the rolling module 1220 is continuously measured and controlled to be less than 10% inside the rolling module 1220. If the oxygen concentration is high, there is a risk of fire.
[0044] The crushed waste blades fed into the rolling module 1220 are rolled by a number of rollers. To facilitate the pyrolysis reaction, the fragments of the waste blades must be smaller than a certain size. The crushed waste blades are rolled to have smaller particle sizes. The rolled crushed waste blades are continuously fed to the first reaction unit 1300.
[0045] A predetermined temperature is maintained inside the rolling module 1220. The temperature inside the rolling module 1220 is maintained at room temperature, so that moisture inside the rolling module 1220 can be removed.
[0046] The rolled crushed waste blades are transported by a conveyor to the first reaction unit 1300. The rolled crushed waste blades are subjected to primary pyrolysis in the first reaction unit 1300. In order to continuously pyrolyze the waste blades, the first reaction unit 1300 is supplied with the continuously rolled waste blades from the rolling module 1220. The waste blades are indirectly heated by hot air, and the heat source of the burner that generates the hot air may be pyrolysis gas or natural gas. High-temperature hot air is supplied to the inside of the first reaction unit 1300 by the temperature adjustment unit 1600. The temperature inside the first reaction unit may be 400 to 500°C.
[0047] A rotary kiln is used in the first reaction unit 1300 so that heat is evenly applied to the rolled waste blades. In general, a rotary kiln is a cylindrical rotary furnace with an inclination, in which reactants are continuously fed into an inlet located at one end, and the reaction product is discharged from an outlet located at the other end. Hot air is circulated inside the rotary kiln to pyrolyze the crushed waste blades contained therein. Waste blades are drawn in from one side of the first reaction unit 1300, and primary pyrolysis reactants are continuously discharged from the other side. The crushed waste blades rotate and move to the outlet side, and heat is evenly applied to them. Although a rotary kiln is used in this embodiment, various types of furnaces such as a screw can be applied.
[0048] The oxygen concentration in the first reaction unit 1300 must be maintained at 10% or less. A sensor may be disposed inside the first reaction unit 1300 to continuously measure the oxygen concentration. In another embodiment, a sensor may be disposed in the exhaust line to measure the oxygen concentration in the exhaust gas.
[0049] The residence time of the crushed waste blades in the first reaction unit 1300 may be 9 hours or less. If the residence time is 9 hours or more, the reaction product is excessively carbonized, resulting in a decrease in economic efficiency.
[0050] In the first reaction unit 1300, the resins such as epoxy and wood contained in the waste blades are gasified, leaving behind lumps of carbon fiber and glass fiber. At this time, the resins that have not yet been gasified are carbonized (char) and remain on the surfaces of the carbon fiber and glass fiber.
[0051] As a result of the first pyrolysis process, oil vapor is generated in addition to gas and char. The oil vapor is cooled while passing through the cooler of the temperature control unit 1600, and some of it is extracted as gas and some as oil. The oil vapor is cooled by water. The gas generated from the oil vapor has a calorific value and can be used as a heat source for indirect heating by flowing into the gas tank of the temperature control unit 1600.
[0052] In addition, a part of the exhaust gas discharged from the first reaction unit 1300 is supplied to the rolling module 1220. This makes it possible to reduce the oxygen concentration in the rolling module 1220 and to increase the temperature in the rolling module 1220.
[0053] Some of the char remaining on the surface of the carbon and glass fibers can be removed by screening. The product discharged from the first reaction unit 1300 is screened before being transported to the second reaction unit. The screen separates the carbon and glass fibers from the char. A screen with a mesh diameter of 50 mm or less can be used to separate the char.
[0054] The carbon and glass fiber mass with some of the char removed is moved to the second reaction unit 1400. In this step, the carbon and glass fibers may have char between the fibers. In the second reaction unit 1400, such char is removed so that only the carbon and glass fibers remain.
[0055] The lumps of carbon and glass fibers containing char are subjected to secondary pyrolysis in the second reaction unit 1400. For the secondary pyrolysis, high-temperature gas and superheated steam are supplied to the second reaction unit 1400. The heat source of the burner that generates the hot air may be pyrolysis gas or natural gas. The temperature inside the second reaction unit 1400 may be 400 to 500°C. The resin and char remaining in the lumps of carbon and glass fibers are decomposed by the secondary pyrolysis.
[0056] The residence time of the carbon fiber and glass fiber agglomerates in the second reaction unit 1400 may be 3 hours or less. At this time, if the oxygen concentration in the second reaction unit 1400 is high, oxidation of the heated object may occur, so the oxygen concentration is maintained at 10% or less.
[0057] The oxygen concentration in the second reaction unit 1400 can be adjusted by an external air tank and a chimney described later. The second reaction unit 1400 may further include an external air tank, which supplies external air to the second reaction unit 1400. The chimney supplies combustion gas to the second reaction unit 1400. The external air tank and the chimney mix 70-80% combustion gas and 20-30% external air to control the oxygen concentration to 10% or less. For this purpose, a plurality of sensors are installed in the second reaction unit 1400 to continuously sense the oxygen concentration. If the oxygen concentration exceeds 15%, the mixing ratio of the combustion gas is increased, and if the oxygen concentration is less than 7%, the mixing ratio of the external air is increased to adjust the oxygen concentration. In this embodiment, a sensor is disposed in the second reaction unit 1400, but in other embodiments, a sensor may be disposed in the exhaust line to measure the oxygen concentration in the exhausted gas.
[0058] The secondary pyrolysis leaves behind pure carbon and glass fibers.
[0059] In this embodiment, the first reaction unit 1300 and the second reaction unit 1400 have separate chambers, but the first pyrolysis process and the second pyrolysis process are carried out in one chamber. In this case, the control logic is set so that the resultant is screened after the first pyrolysis is completely completed, and the screened resultant is subjected to the second pyrolysis.
[0060] The heat sources for the primary and secondary pyrolysis may be pyrolysis gas and natural gas.
[0061] As shown in FIG. 3, the separation unit 1500 may include a separation section 1510, a first chamber 1520, and a second chamber 1530. The separation section 1510 separates the result of the second reaction unit 1400 into r-CF (recycled carbon fiber) and r-GF (recycled glass fiber). The r-CF and r-GF can be separated by utilizing the density difference. Methods that utilize the density difference include a dry method and a wet method. The dry method uses air flow, and generates an air flow in the result of the second pyrolysis moving on a conveyor to move the light carbon fiber.
[0062] The wet method is a method for separating the carbon fibers and the glass fibers using a liquid having a density intermediate between the densities of the carbon fibers and the glass fibers.
[0063] The carbon fibers and glass fibers separated by the separation unit 1510 can move to a first chamber 1520 and a second chamber 1530, respectively. The separation of the carbon fibers and the glass fibers is carried out on a conveyor.
[0064] The temperature adjustment unit 1600 adjusts the temperature and oxygen concentration inside the pre-treatment unit 1200, the first reaction unit 1300, and the second reaction unit 1400. The temperature adjustment unit 1600 may include a chimney, a gas tank, and a cooler.
[0065] The gas tank supplies pyrolysis gas and natural gas as a heat source for heating the first reaction unit 1300 and the second reaction unit 1400. The chimney discharges the combustion gas discharged from the first reaction unit 1300 and the second reaction unit 1400 to the outside of the device. The chimney also supplies the combustion gas discharged from the first reaction unit 1300 to the second reaction unit 1400, transfers the heat of the first reaction unit 1300 to the second reaction unit 1400, and adjusts the oxygen concentration inside the second reaction unit 1400.
[0066] Oil vapor is generated during the pyrolysis process in the first reaction unit 1300. The oil vapor flows into the cooler of the temperature control unit 1600 and is cooled. When the oil vapor is cooled, oil is extracted, and the remaining pyrolysis gas is supplied to the first reaction unit 1300 and the second reaction unit 1400 through a gas tank.
[0067] In the present invention, the waste blades are crushed, pyrolyzed, and separated into carbon fibers and glass fibers in one process, and are moved to each unit by a conveyor. One or more conveyors are connected to each other, so that the residence time in each unit can be adjusted.
[0068] FIG. 4 is a flow chart illustrating a method for recovering carbon fibers and glass fibers from a composite material according to an embodiment of the present invention.
[0069] In order to separate composite materials according to the present invention, first, the waste blades are cut in the longitudinal direction (S1100) as shown in Fig. 4. The collected waste blades are cut to lengths of 10 m or less. The waste blades are cut using a wire saw or the like. The cut waste blades can be easily moved and fed into a crusher.
[0070] Next, the waste blades cut in the longitudinal direction are crushed (S1200). The waste blades are fed into the crushing module 1210 and crushed. The waste blades are crushed to a thickness of 20 mm or less. A large amount of dust is generated during the crushing process of the waste blades, and the input part of the crushing module 1210 is sealed to prevent the dust from flowing out of the crushing module 1210. In addition, the dust suction part can suck in the dust generated during the crushing process of the waste blades and collect it in a predetermined space. To collect the dust, air can be continuously circulated within the crushing module 1210.
[0071] After the waste blades are crushed, the crushed waste blades can be screened to remove particles below a predetermined particle size. The crushed waste blades have different particle sizes. When waste blades of different particle sizes are pyrolyzed in the first reaction unit, blade fragments with smaller particle sizes may be carbonized and contaminate the primary pyrolysis result. Therefore, the crushed waste blades can be moved on a screen, and if the size of the crushed particles is below a predetermined size, they can be separated under the screen. The screen may be vibrated to facilitate the separation of small particles.
[0072] The crushed waste blades are continuously fed into the rolling module (S1300). The crushed waste blades are not uniform in particle size, and it is not easy to feed them in a fixed amount. A semi-batch type feeder is adopted to feed the crushed waste blades in a fixed amount. In order to feed a fixed amount of the waste blades into the rolling module, the feed part of the rolling module may have a double-lid structure. The feed part of the rolling module may include a first feed part and a second feed part. The first feed part and the second feed part may be controlled to be opened sequentially rather than simultaneously. The first feed part and the second feed part may be opened in a sliding manner, and the degree to which they are opened can be adjusted according to the amount to be fed. In addition, nitrogen purging is performed simultaneously with the opening of the second feed part. Nitrogen is fed into the rolling module while the second feed part is open, and when the second feed part is closed again, the supply of nitrogen is stopped. This can minimize the inflow of oxygen into the rolling module.
[0073] The crushed waste blades are rolled (S1400). The crushed waste blades fed into the rolling module are rolled by a number of rollers. To facilitate the pyrolysis reaction, the fragments of the waste blades must be smaller than a certain size. The crushed waste blades are rolled to have smaller particle sizes.
[0074] A reducing atmosphere can be maintained inside the chamber of the rolling module. To maintain the reducing atmosphere, gas exhausted from inside the rolling module can be recirculated into the rolling module. The oxygen concentration inside the rolling module is continuously measured and controlled to be less than 10% inside the rolling module 1220.
[0075] The rolled crushing blade is subjected to primary pyrolysis (S1500). The temperature control unit can supply heated gas to the inside of the first reaction unit. The heat source of the burner that generates the heated gas, i.e., hot air, may be pyrolysis gas or natural gas. The temperature inside the first reaction unit may be 400 to 500°C. The temperature in the first pyrolysis step is adjusted by the temperature control unit.
[0076] A rotary kiln calciner is used in the first reaction unit so that heat is uniformly applied to the rolled waste blades. During the primary pyrolysis, the oxygen concentration in the first reaction unit can be maintained at 10% or less. The residence time of the crushed waste blades in the first reaction unit can be 9 hours or less.
[0077] In the first reaction unit, the epoxy and other resins and wood contained in the waste blades are gasified, leaving behind clumps of carbon and glass fibers. At this time, the resins that have not yet been gasified are carbonized (char) and remain on the surfaces of the carbon and glass fibers. In addition to gas and char, oil vapor is produced as a result of the first pyrolysis process. The oil vapor is cooled and some is extracted as gas and some as oil. The oil vapor is cooled by water. The pyrolysis gas extracted from the oil vapor has a calorific value and can be flowed to the temperature control unit and used as an indirect heat source. The result of the first pyrolysis process is screened before being subjected to the secondary pyrolysis.
[0078] The crushing blades subjected to the primary pyrolysis are subjected to secondary pyrolysis (S1600). The lumps of carbon fiber and glass fiber containing char are subjected to secondary pyrolysis in the second reaction unit. For the secondary pyrolysis, high-temperature gas and superheated steam are supplied to the second reaction unit 1400. The heat source of the burner that generates the hot air may be pyrolysis gas or natural gas. The temperature in the second reaction unit 1400 may be 400 to 500°C. The temperature in the secondary pyrolysis step is regulated by a temperature regulation unit. The resin and char remaining in the lumps of carbon fiber and glass fiber are decomposed by the secondary pyrolysis.
[0079] The residence time of the carbon fiber and glass fiber agglomerates in the second reaction unit may be 3 hours or less. At this time, if the oxygen concentration in the second reaction unit is high, oxidation of the heated object may occur, so the oxygen concentration is maintained at 10% or less.
[0080] During secondary pyrolysis, the oxygen concentration in the second reaction unit can be adjusted by the external air tank and chimney. The external air tank supplies external air to the second reaction unit, and the chimney supplies combustion gas. The external air tank and chimney mix 70-80% combustion gas and 20-30% external air to control the oxygen concentration to 10% or less. To this end, multiple sensors are installed in the second reaction unit to continuously sense the oxygen concentration. If the oxygen concentration exceeds 15%, the mixing ratio of combustion gas is increased, and if the oxygen concentration is less than 7%, the mixing ratio of external air is increased to adjust the oxygen concentration.
[0081] The second pyrolysis leaves behind pure carbon and glass fibers.
[0082] The result of the second pyrolysis step is separated (S1700). The result of the second pyrolysis can be separated into r-CF (recycled carbon fiber) and r-GF (recycled glass fiber). The r-CF and r-GF can be separated by utilizing the density difference.
[0083] The separated carbon fibers and glass fibers can move to the first and second chambers, respectively. The separation of the carbon fibers and glass fibers is carried out on the conveyor.
[0084] Although one embodiment of the present invention has been described above, a person having ordinary knowledge in the art may modify and change the present invention in various ways by adding, changing, deleting or adding components without departing from the spirit of the present invention as set forth in the claims, and this also falls within the scope of the claims of the present invention. [Explanation of symbols]
[0085] 1000: Carbon and glass fiber recovery equipment from composite materials 1100: Cutting unit 1200: Pre-processing unit 1210: Crushing module 1220: Rolling module 1230: Screening module 1300: First reaction unit 1400: Second reaction unit 1500: Separation unit 1510: Separation section 1520: First chamber 1530: Second chamber 1600: Temperature control unit
Claims
1. A pre-processing unit including a crushing module for crushing waste blades and a rolling module for rolling the crushed waste blades; a first reaction unit for primary pyrolysis of the pretreated waste blades; a second reaction unit for secondarily pyrolyzing the waste blades that have been subjected to the first pyrolysis; a separation unit for separating the secondary pyrolysis product into a first material and a second material, the separation unit having a first chamber for receiving the first material, and a second chamber for receiving the second material.
2. 2. The apparatus for recovering carbon and glass fibers from composite materials according to claim 1, further comprising a cutting unit for cutting the blade to a predetermined length.
3. 2. The apparatus for recovering carbon fibers and glass fibers from composite materials according to claim 1, further comprising a temperature control unit for controlling temperatures inside the pre-treatment unit, the first reaction unit, and the second reaction unit.
4. The apparatus for recovering carbon and glass fibers from composite materials according to claim 1 , wherein the pre-treatment unit comprises a screening module between the crushing module and the rolling module.
5. 2. The apparatus for recovering carbon fibers and glass fibers from a composite material according to claim 1, wherein the input section of the rolling module comprises a first input section and a second input section.
6. 6. The apparatus for recovering carbon fibers and glass fibers from composite materials according to claim 5, wherein nitrogen is supplied when the second input port is opened.
7. 2. The apparatus for recovering carbon and glass fibers from composite materials according to claim 1, wherein gas exhausted from the interior of said rolling module is recirculated into said rolling module.
8. 2. The apparatus for recovering carbon and glass fibers from composite materials according to claim 1, wherein the temperature inside the first reaction unit is 400 to 500° C.
9. 4. The apparatus for recovering carbon fibers and glass fibers from composite materials according to claim 3, wherein the oil vapor generated in the first reaction unit is cooled in the temperature control unit and extracted as oil.
10. The apparatus for recovering carbon fibers and glass fibers from composite materials according to claim 1, characterized in that the second reaction unit is provided with a sensor for measuring an oxygen concentration in the second reaction unit and an external air tank for supplying external air into the second reaction unit.
11. A crushing step of crushing the waste blade cut in the longitudinal direction; A step of continuously feeding the crushed waste blades into a rolling module; A rolling step of rolling the crushed waste blades; A first pyrolysis step of primarily pyrolyzing the rolled waste blade; A second pyrolysis step of secondarily pyrolyzing the waste blades that have been subjected to the first pyrolysis; and a separation step of separating the result of the second pyrolysis step, A method for recovering carbon fibers and glass fibers from a composite material, wherein the temperatures in the rolling step, the first pyrolysis step, and the second pyrolysis step are controlled by a temperature control unit.
12. After the step of crushing the waste blades, The method for recovering carbon and glass fibers from composite materials according to claim 11, further comprising the step of screening the crushed waste blades.
13. The input section of the rolling module includes a first input section and a second input section, In the step of continuously feeding the crushed waste blades into a rolling module, 12. The method for recovering carbon fibers and glass fibers from a composite material according to claim 11, wherein the first input section and the second input section are opened in sequence.
14. The method for recovering carbon fibers and glass fibers from a composite material according to claim 11, characterized in that, in the rolling step, exhaust gas inside the rolling module is recirculated into the rolling module.
15. 12. The method for recovering carbon fibers and glass fibers from a composite material according to claim 11, wherein the temperature in the first pyrolysis step is 400 to 500°C.
Citation Information
Patent Citations
Pyrolysis recovery system and method for chopped glass fibers of wind power blades
CN115608753A
Wet type treatment process for making best utilization of thermal deco mposition residual and minimization of refuse
JP1977077471A
Pyrolysis System and Method for Recovering Carbon Fibers from Carbon Fiber-Containing Resins
JP2016521295A
Device and method for converting waste matter containing waste plastic into fuel
WO2014112223A1
Method of collecting carbon fiber from waste carbon fiber reinforced plastic