Dispersion of surface-treated silica-containing inorganic oxide particles and method for producing the same

The use of silane-bonded silica particles with controlled bridging oxygen structures addresses the stability issues in high temperature and salt conditions, maintaining dispersion stability and solvent compatibility.

JP2024149753AActive Publication Date: 2024-10-18NISSAN CHEM CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024134471
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-08-31
Filing Date
2024-08-09
Publication Date
2024-10-18
Estimated Expiration
2042-08-26

AI Technical Summary

Technical Problem

Existing dispersions of silica-containing inorganic oxide particles lack stability under high temperature and high salt conditions, leading to insufficient repulsive forces between particles.

Method used

A dispersion of silane-bonded silica-containing inorganic oxide particles is created using a hydrolyzable silane as a dispersoid in a liquid medium, with a specific ratio of silicon atoms in the hydrolyzate to those bonded to the particle surface, and controlled bridging oxygen structures to enhance repulsive forces, allowing compatibility with various solvents.

Benefits of technology

The dispersion achieves high stability under high temperature and high salt conditions, maintaining particle repulsion and compatibility with both aqueous and organic solvents, ensuring stable dispersion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149753000001
    Figure 2024149753000001
  • Figure 2024149753000002
    Figure 2024149753000002
  • Figure 2024149753000003
    Figure 2024149753000003
Patent Text Reader

Abstract

To provide a dispersion of inorganic oxide particles having high dispersion stability under high temperature and high salinity.SOLUTION: A dispersion comprises silane-bound inorganic oxide particles surface-modified with hydrolyzable silane as a dispersion and a liquid medium as a dispersion medium, and the dispersion medium comprises a hydrolyzate of the hydrolyzable silane. The ratio of (number of moles of silicon atoms in the hydrolyzate of hydrolyzable silane in the dispersion medium) / (number of moles of silicon atoms of silane bonded to the surface of the inorganic oxide particles) is 0.2 to 30. Q4, where the number of bridging oxygen between silicon atoms of the silica particles is 4 / 2 per one silicon atom in Si-NMR observation, is increased compared to the state before the silane surface modification. The inorganic oxide is at least one kind of inorganic oxide selected from the group consisting of silica, alumina, tin oxide, zirconium oxide, titanium oxide, and antimony oxide having an average particle diameter of 5 nm to 100 nm. Also provided are a single metal oxide and a complex metal oxide or a complex oxide having a core-shell structure.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a dispersion of silane-bonded silica-containing inorganic oxide particles having a silane-treated surface, and a method for producing the same. Hereinafter, the "silane-bonded silica-containing inorganic oxide particles" may also be referred to as "silica-containing inorganic oxide particles". [Background technology]

[0002] The dispersion liquid of silica-containing inorganic oxide particles, especially silica sol, is a liquid in which silica particles are dispersed in a dispersion medium, and as a method for highly dispersing silica particles, there is a method for increasing the absolute value of the zeta potential between silica particles to increase the repulsive force between silica particles.One of the methods is a method for modifying the surface of silica particles with a silane coupling agent having a cationic or anionic functional group when the dispersion medium is an aqueous solution, or a method for modifying the surface of silica particles with a silane coupling agent having a hydrophobic organic group when the dispersion medium is an organic solvent. For example, a method for producing an organic solvent-dispersed silica sol has been disclosed, which includes a step of surface-treating a hydrophilic inorganic oxide sol by adding a silicon alkoxide having two or more alkoxide groups bonded to a silicon atom, or a silicon alkoxide having one or more hydroxyl groups bonded to one or more silicon atoms and one or more alkoxide groups bonded to a silicon atom, and a step of replacing the dispersion medium with a non-alcoholic organic solvent in the presence of a primary alcohol having 3 to 12 carbon atoms (see Patent Document 1). A dispersion of surface-treated particles is disclosed, which comprises surface-treated particles in which a first organosilicon compound is bonded to the surface of metal oxide particles having a refractive index of 1.65 or more, a second organosilicon compound that is not bonded to the metal oxide particles, and an organic solvent, and in which the (first organosilicon compound) / (second organosilicon compound) ratio is 0.1 to 9.0 (see Patent Document 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication 2005-200294 [Patent Document 2] Patent Publication No. 2020-164374 Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention provides a dispersion of silica-containing inorganic oxide particles, particularly a dispersion of silica particles, which has high dispersion stability even under high temperature or high salt conditions. [Means for solving the problem]

[0005] The present invention provides, in a first aspect, a dispersion containing silane-bonded silica-containing inorganic oxide particles surface-modified with a hydrolyzable silane as a dispersoid and a liquid medium as a dispersion medium, the dispersion medium containing a hydrolyzate of the hydrolyzable silane, a ratio of (the number of moles of silicon atoms in the hydrolyzate of the hydrolyzable silane in the dispersion medium) / (the number of moles of silicon atoms of the silane bonded to the surface of the inorganic oxide particles) being 0.2 to 30, and the dispersion containing the silica-containing inorganic oxide particles in which, as measured by Si-NMR, Q4, in which the number of bridging oxygen atoms between silicon atoms of the silica particles is 4 / 2 per silicon atom, is increased compared to before surface modification with the silane; As a second aspect, the dispersion according to the first aspect, wherein the silica-containing inorganic oxide particles are silica particles having an average particle size of 5 nm to 100 nm, or at least one type of inorganic oxide particles selected from the group consisting of silica and alumina, tin oxide, zirconium oxide, titanium oxide, and antimony oxide, and the silica-containing inorganic oxide particles are silica particles, composite metal oxide particles of silica and another metal oxide, or composite oxide particles having a core-shell structure of silica and another metal oxide; As a third aspect, the hydrolyzable silane is represented by the formula (1) to the formula (3): [ka] (In formula (1), R 3is an alkyl group, a halogenated alkyl group, an alkenyl group, or an organic group having an epoxy group, a (meth)acryloyl group, a mercapto group, an amino group, a ureido group, or a cyano group, and is bonded to a silicon atom by a Si-C bond; R 4 represents an alkoxy group, an acyloxy group, or a halogen group; a represents an integer of 1 to 3; In formula (2) and formula (3), R 5 and R 7 is an alkyl group having 1 to 3 carbon atoms and bonded to a silicon atom by a Si-C bond, and R 6 and R 8 represents an alkoxy group, an acyloxy group, or a halogen group; Y represents an alkylene group, an NH group, or an oxygen atom; 5 and R 7 at least one of which is an alkyl group having 1 to 3 carbon atoms and bonded to a silicon atom via a Si-C bond, b is an integer of 1 to 3, c is an integer of 0 or 1, d is an integer of 1 to 3, and e is an integer of 1 to 3. The dispersion according to the first or second aspect, which is at least one silane compound selected from the group consisting of: As a fourth aspect, the dispersion according to the third aspect, wherein the hydrolyzate of the hydrolyzable silane in the dispersion medium contains a silane compound in which a in formula (1) is an integer of 1 and, with respect to T0, T1, T2, and T3 structures in which the ratios of bridging oxygen between silicon atoms are 0 / 2, 1 / 2, 2 / 2, and 3 / 2 per silicon atom as measured by Si-NMR, the (T2+T3) / (T0+T1) is a specific value (2 to 15) or the (T1+T2+T3) / (T0) ratio is a specific value (5 to 100); As a fifth aspect, the dispersion according to the third aspect, wherein the hydrolyzate of the hydrolyzable silane in the dispersion medium contains a silane compound in which a in formula (1) is an integer of 2 and the hydrolyzate has D0, D1 and D2 structures in which the ratios of bridging oxygen between silicon atoms are 0 / 2, 1 / 2 and 2 / 2 per silicon atom as measured by Si-NMR, respectively, and the (D1+D2) / (D0) ratio is 0.1 to 10 or the (D2) / (D0+D1) ratio is 0.01 to 10; As a sixth aspect, the dispersion according to any one of the first to fifth aspects, in which a value obtained by dividing the amount of water vapor adsorption to the silica-containing inorganic oxide particles by the amount of nitrogen gas adsorption, that is, (specific surface area calculated from the amount of water vapor adsorption) / (specific surface area calculated from the amount of nitrogen gas adsorption), is 0.15 to 0.95 compared to the silica-containing inorganic oxide particles before the addition of the silane compound. As a seventh aspect, the present invention relates to a method for producing a method for manufacturing a semiconductor device comprising the steps of (A) and (B) below: Step (A): obtaining an aqueous dispersion of the silica-containing inorganic oxide particles; Step (B): Add a hydrolyzable silane to the aqueous dispersion of the silica-containing inorganic oxide particles at a pH of 2.0 to 6.5 so that the ratio of the number of the silane per the surface area of ​​the particles is 0.3 to 100 particles / nm 2 and stirring the mixture at room temperature, followed by heating to a temperature within a range of 50 to 99° C., and the stirring time after heating is within a range of 1 to 7 times the stirring time at room temperature. As an eighth aspect, after the step (B), there is further a step (C): Step (C): A step of replacing the aqueous medium of the dispersion obtained in step (B) with an organic solvent. A method for producing a dispersion using the organic solvent as described in the seventh aspect as a dispersion medium. Effect of the Invention

[0006] Dispersions of inorganic oxide particles containing silica, particularly inorganic particles such as silica, ensure dispersion stability by the repulsive force between particles. For example, in the case of silica particles, silanol groups are present on the surface of the silica particles, and the negative charge of the silanol groups causes repulsion between particles. The absolute value of the charge changes depending on the pH and salts in the dispersion. There are surface-treated particles that are less susceptible to the effects of pH and salts. For example, in the case of silica particles, there are methods of surface-treating the silica particle surface with a hydrolyzable silane compound having a cationic functional group with a positive charge, and methods of surface-treating the silica particle surface with a hydrolyzable silane compound having an anionic functional group with a negative charge. These methods have repulsive force between particles due to electrical repulsion between cationic and anionic functional groups, respectively.

[0007] Although it depends on the density of the functional groups bonded to the surface of the silica particles, it is difficult to modify the entire particle surface with the functional groups, and the repulsive force between particles is not necessarily sufficient under certain pH or salt concentration conditions. Incidentally, the silane compound having a functional group added to the dispersion liquid of silica particles includes silanes having a functional group bonded to the surface of the silica particles (bonded silanes) and silanes having a functional group that are not bonded to the silica particles and are dissolved in the dispersion medium (hereinafter referred to as free silanes). The silanes having a functional group in the dispersion medium exist between the silica particles, and since they have the same functional group, a repulsive force occurs between the bonded silanes and the free silanes, and the silica particles generate a repulsive force not only between the particles but also between the silane monomers, resulting in a dispersion liquid with high dispersion stability.

[0008] In the present invention, it has been found that a specific ratio (0.2 to 30) of (the number of moles of silicon atoms in the hydrolyzate of the hydrolyzable silane in the dispersion medium) / (the number of moles of silicon atoms of the silane bonded to the surface of the inorganic oxide particles) provides a dispersion of silica particles with high dispersion stability. In addition, when the dispersion medium is an organic solvent, the silica particles have hydrophilicity based on silanol, which is different from the liquid property of the organic solvent, so the silanol groups of the silica particles are surface-treated with silane having a hydrophobic functional group to make them highly compatible with the organic solvent. It is difficult to modify the entire particle with silane having a hydrophobic functional group, so the parts of the silica particles that are not modified with the hydrophobic functional group can be made to have compatibility with a silane monomer having a hydrophobic functional group to make a dispersion liquid that is highly dispersible in organic solvents.

[0009] In the present invention, it is preferable that the hydrolyzable silane hydrolyzate in the dispersion medium is present with the repulsive force between the silica particles and the silane monomer being delocalized throughout the dispersion medium, and for this purpose, it is preferable that the polymerization of the free silane does not proceed excessively. For example, when using a silane having three hydrolyzable groups of the hydrolyzable silane, it is preferable that the (T2+T3) / (T0+T1) is a specific value (2 to 15, preferably 2 to 10), or the (T1+T2+T3) / (T0) ratio is a specific value (5 to 100, preferably 5 to 50) for T0, T1, T2, and T3 structures in which the ratio of bridging oxygen between silicon atoms is 0 / 2, 1 / 2, 2 / 2, and 3 / 2 per silicon atom in Si-NMR observation of the hydrolyzed compound of the silane compound. It is preferable that either one of these is satisfied, but it is more preferable that both are satisfied. In addition, when using a silane having two hydrolyzable groups as the hydrolyzable silane, it is preferable that the (D1+D2) / (D0) ratio is a specific value (0.1 to 10) or the (D2) / (D0+D1) ratio is a specific value (0.01 to 10) for D0, D1, and D2 structures in which the ratio of bridging oxygen between silicon atoms is 0 / 2, 1 / 2, and 2 / 2 per silicon atom in the hydrolyzed compound of the silane compound observed by Si-NMR. Either one of these may be satisfied, but it is more preferable to satisfy both.

[0010] In the case of silica-containing inorganic oxide particles, especially silica particles, the amount of water vapor adsorbed on the silica particles was measured using nitrogen gas. By adjusting the specific surface area calculated from the water vapor adsorption amount / (specific surface area calculated from the nitrogen gas adsorption amount), which is the value obtained by dividing the specific surface area by the amount of water vapor adsorption, to a range of 0.15 to 0.95 compared to the silica particles before the addition of the silane compound, it is possible to make the inorganic oxide particles into particles that have high compatibility over a wide range of media, from aqueous media to organic solvents. In the silica particles filled with these bonded silanes and free silanes, the number of bridging oxygen atoms between silicon atoms of the silica particles, Q4, which is 4 / 2 per silicon atom, is increased compared to before the surface modification with the silane, as determined by Si-NMR observation. For example, the increase ratio can be in the range of 1.01 to 1.5, or 1.01 to 1.15. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention relates to a dispersion containing, as a dispersoid, silane-bonded silica-containing inorganic oxide particles surface-modified with a hydrolyzable silane and a liquid medium as a dispersion medium, the dispersion medium containing a hydrolyzate of the hydrolyzable silane, in which a ratio of (the number of moles of silicon atoms in the hydrolyzate of the hydrolyzable silane in the dispersion medium) / (the number of moles of silicon atoms of the silane bonded to the surface of the inorganic oxide particles) is 0.2 to 30, preferably 0.2 to 15, and the above dispersion containing the silica-containing inorganic oxide particles in which, as measured by Si-NMR, the number of bridging oxygen atoms between silicon atoms of the silica particles is 4 / 2 per silicon atom, is increased compared to before surface modification with the silane.

[0012] In the present invention, the average particle diameter of an inorganic substance, for example, an aqueous silica sol (colloidal silica particles), refers to the specific surface area diameter measured by the nitrogen adsorption method (BET method) unless otherwise specified. The specific surface area diameter (average particle diameter (specific surface area diameter) D (nm)) measured by the nitrogen adsorption method (BET method) is calculated by dividing the specific surface area S (m 2 / g), it is given by the formula D(nm)=2720 / S. The silica-containing inorganic oxide particles are silica particles having an average particle diameter of 5 nm to 100 nm, preferably 5 to 60 nm, as measured by the BET method, or at least one inorganic oxide particle selected from the group consisting of silica and alumina, tin oxide, zirconium oxide, titanium oxide, and antimony oxide, and the silica-containing inorganic oxide particles include silica particles, composite metal oxides of silica and other metal oxides, and composite oxide particles having a core-shell structure of silica and other metal oxides. For example, silica particles are preferably used as the single metal oxide, and composite metal oxides include composite metal oxide particles of silica and alumina, and composite metal oxide particles of tin oxide and silica. In addition, composite oxide particles having a core-shell structure include composite oxide particles having a core of titanium oxide or titanium oxide and zirconium oxide and a shell of tin oxide and silica.

[0013] In the present invention, the silica-containing inorganic oxide particles are obtained as a dispersion having a concentration of, for example, 1 to 50% by mass in a dispersion medium. The dispersion of the present invention is prepared by the following steps (A) and (B): Step (A): obtaining an aqueous dispersion of the silica-containing inorganic oxide particles; Step (B): Add a hydrolyzable silane to the aqueous dispersion of the silica-containing inorganic oxide particles at a pH of 2.0 to 6.5 so that the ratio of the number of the silane per the surface area of ​​the particles is 0.3 to 100 particles / nm 2 and then heating to a temperature within a range of 50 to 99° C. after stirring at room temperature, and the stirring time after heating is 1 to 7 times the stirring time at room temperature. The aqueous dispersion of silica-containing inorganic oxide particles obtained in step (A) is obtained as a dispersion liquid of silica-containing inorganic oxide particles in an aqueous medium with a concentration of, for example, 1 to 50% by mass. For example, in the case of an aqueous silica sol, the aqueous silica sol is made from water glass as a starting material, and includes a) a step of obtaining active silicic acid by cation exchange of the water glass, and b) a step of obtaining silica particles by heating the active silicic acid. In step a), a mineral acid (e.g., hydrochloric acid, nitric acid, or sulfuric acid) is added to highly purify the active silicic acid, and the active silicic acid from which metal impurities other than silica have been eluted by cation exchange and anion exchange to remove metal impurities and unnecessary anions can be used. In step b), an alkali component (e.g., NaOH, KOH) is added to the active silicic acid to grow silica particles. In order to promote the particle growth of silica particles, a seed liquid and a feed liquid are prepared by adding an alkali to the activated silicic acid obtained in step a), and the seed liquid is heated while the feed liquid is supplied to increase the silica particle diameter, thereby making it possible to obtain an aqueous silica sol with a desired particle diameter. In step (B), the pH of the aqueous dispersion of the silica-containing inorganic oxide particles obtained in step (A) can be adjusted to 2.0 to 6.5, and a hydrolyzable silane can be added. An acid or an alkali can be used for adjusting the pH.

[0014] Examples of the acid include mineral acids such as hydrochloric acid, sulfuric acid, and nitric acid, and organic acids such as formic acid, oxalic acid, citric acid, acetic acid, lactic acid, malic acid, succinic acid, tartaric acid, butyric acid, fumaric acid, propionic acid, and ascorbic acid. Examples of the alkali include ammonia, amines, quaternary ammonium hydroxides, alkali metal hydroxides, alkali metal alkoxides, and alkali metal salts of aliphatic carboxylates. Amines include primary amines, secondary amines, and tertiary amines. Examples of primary amines include methylamine, ethylamine, n-propylamine, and i-propylamine. Examples of secondary amines include ethyl-n-propylamine, ethyl-i-propylamine, dipropylamine, di-i-propylamine, ethylbutylamine, n-propylbutylamine, dibutylamine, ethylpentylamine, n-propylpentylamine, i-propylpentylamine, dipentylamine, ethyloctylamine, i-propyloctylamine, butyloctylamine, and dioctylamine. Examples of the tertiary amine include triethylamine, ethyldinipropylamine, diethylnpropylamine, trinpropylamine, triipropylamine, ethyldibutylamine, diethylbutylamine, ipropyldibutylamine, diipropylbutylamine, tributylamine, ethyldipentylamine, diethylpentylamine, tripentylamine, methyldioctylamine, dimethyloctylamine, ethyldioctylamine, diethyloctylamine, and trioctylamine. The quaternary ammonium hydroxide is preferably a tetraalkylammonium hydroxide having a total of 4 to 40 carbon atoms, such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetra-n-propylammonium hydroxide, tetra-i-propylammonium hydroxide, tetrabutylammonium hydroxide, and ethyltrimethylammonium hydroxide. Examples of the alkali metal hydroxide include sodium hydroxide, potassium hydroxide, sodium carbonate, and potassium carbonate. Examples of the alkali metal alkoxide include sodium methoxide, sodium ethoxide, potassium methoxide, and potassium ethoxide. Examples of the alkali metal salt of an aliphatic carboxylate include alkali metal salts of saturated aliphatic carboxylates having 10 to 30 carbon atoms and alkali metal salts of unsaturated aliphatic carboxylates. Examples of the alkali metal salt of an aliphatic carboxylate include sodium and potassium. Examples of the alkali metal salt of a saturated aliphatic carboxylate include alkali metal salts of lauric acid, alkali metal salts of myristate, alkali metal salts of palmitic acid, and alkali metal salts of stearic acid. Examples of the alkali metal salts of unsaturated aliphatic carboxylic acids include alkali metal salts of oleic acid, alkali metal salts of linoleic acid, and alkali metal salts of linolenic acid.

[0015] As the hydrolyzable silane used in the step (B), at least one silane compound selected from the group consisting of the above formulae (1) to (3) can be used. In formula (1), R 3 is an alkyl group, a halogenated alkyl group, an alkenyl group, or an organic group having an epoxy group, a (meth)acryloyl group, a mercapto group, an amino group, a ureido group, or a cyano group, and is bonded to a silicon atom by a Si-C bond; R 4 represents an alkoxy group, an acyloxy group, or a halogen group; a represents an integer of 1 to 3; In formula (2) and formula (3), R 5 and R 7 is an alkyl group having 1 to 3 carbon atoms and bonded to a silicon atom by a Si-C bond, and R 6 and R 8 represents an alkoxy group, an acyloxy group, or a halogen group; Y represents an alkylene group, an NH group, or an oxygen atom; 5 and R 7 at least one of which is an alkyl group having 1 to 3 carbon atoms and is bonded to a silicon atom via a Si-C bond, b is an integer of 1 to 3, c is an integer of 0 or 1, d is an integer of 1 to 3, and e is an integer of 1 to 3.

[0016] The alkyl group is an alkyl group having 1 to 18 carbon atoms, and examples thereof include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, a cyclopropyl group, an n-butyl group, an i-butyl group, an s-butyl group, a t-butyl group, a cyclobutyl group, a 1-methyl-cyclopropyl group, a 2-methyl-cyclopropyl group, an n-pentyl group, a 1-methyl-n-butyl group, a 2-methyl-n-butyl group, a 3-methyl-n-butyl group, a 1,1-dimethyl-n-propyl group, a 1,2-dimethyl-n-propyl group, a 2,2-dimethyl-n-propyl group, a 1-ethyl- n-Propyl, cyclopentyl, 1-methylcyclobutyl, 2-methylcyclobutyl, 3-methylcyclobutyl, 1,2-dimethylcyclopropyl, 2,3-dimethylcyclopropyl, 1-ethylcyclopropyl, 2-ethylcyclopropyl, n-hexyl, 1-methylpentyl, 2-methylpentyl, 3-methylpentyl, 4-methylpentyl, 1,1-dimethylbutyl, 1,2-dimethylbutyl, 1,3-dimethylbutyl , 2,2-dimethyl-n-butyl, 2,3-dimethyl-n-butyl, 3,3-dimethyl-n-butyl, 1-ethyl-n-butyl, 2-ethyl-n-butyl, 1,1,2-trimethyl-n-propyl, 1,2,2-trimethyl-n-propyl, 1-ethyl-1-methyl-n-propyl, 1-ethyl-2-methyl-n-propyl, cyclohexyl, 1-methyl-cyclopentyl, 2-methyl-cyclopentyl, 3-methyl-cyclopentyl, 1-ethyl-cyclobutyl, 2-ethyl-cyclobutyl cyclopropyl, 3-ethyl-cyclobutyl, 1,2-dimethyl-cyclobutyl, 1,3-dimethyl-cyclobutyl, 2,2-dimethyl-cyclobutyl, 2,3-dimethyl-cyclobutyl, 2,4-dimethyl-cyclobutyl, 3,3-dimethyl-cyclobutyl, 1-n-propyl-cyclopropyl, 2-n-propyl-cyclopropyl, 1-i-propyl-cyclopropyl, 2-i-propyl-cyclopropyl, 1,2,2-trimethyl-cyclopropyl, 1,2,3-trimethyl-cyclopropyl, 2,2,Examples of the cyclopropyl group include, but are not limited to, 3-trimethyl-cyclopropyl group, 1-ethyl-2-methyl-cyclopropyl group, 2-ethyl-1-methyl-cyclopropyl group, 2-ethyl-2-methyl-cyclopropyl group, 2-ethyl-3-methyl-cyclopropyl group, hexyl group, heptyl group, octyl group, nonyl group, decyl group, undecyl group, dodecyl group, tridecyl group, tetradecyl group, pentadecyl group, hexadecyl group, heptadecyl group, and octadecyl group. Furthermore, examples of the alkylene group include alkylene groups derived from the above-mentioned alkyl groups.

[0017] The alkenyl group is an alkenyl group having 2 to 10 carbon atoms, and examples of such alkenyl groups include ethenyl, 1-propenyl, 2-propenyl, 1-methyl-1-ethenyl, 1-butenyl, 2-butenyl, 3-butenyl, 2-methyl-1-propenyl, 2-methyl-2-propenyl, 1-ethylethenyl, 1-methyl-1-propenyl, 1-methyl-2-propenyl, 1-pentenyl, 2-pentenyl, 3-pentenyl, 4-pentenyl, 1-n-propylethenyl, 1-methyl-1- butenyl group, 1-methyl-2-butenyl group, 1-methyl-3-butenyl group, 2-ethyl-2-propenyl group, 2-methyl-1-butenyl group, 2-methyl-2-butenyl group, 2-methyl-3-butenyl group, 3-methyl-1-butenyl group, 3-methyl-2-butenyl group, 3-methyl-3-butenyl group, 1,1-dimethyl-2-propenyl group, 1-i-propylethenyl group, 1,2-dimethyl-1-propenyl group, 1,2-dimethyl-2-propenyl group, 1-cyclopentenyl group, 2-cyclopentenyl group Examples of aryl groups include, but are not limited to, a cyclopentenyl group, a 3-cyclopentenyl group, a 1-hexenyl group, a 2-hexenyl group, a 3-hexenyl group, a 4-hexenyl group, a 5-hexenyl group, a 1-methyl-1-pentenyl group, a 1-methyl-2-pentenyl group, a 1-methyl-3-pentenyl group, a 1-methyl-4-pentenyl group, a 1-n-butylethenyl group, a 2-methyl-1-pentenyl group, and a 2-methyl-2-pentenyl group.

[0018] The alkoxy group includes an alkoxy group having 1 to 10 carbon atoms, such as a methoxy group, an ethoxy group, an n-propoxy group, an i-propoxy group, an n-butoxy group, an i-butoxy group, an s-butoxy group, a t-butoxy group, an n-pentyloxy group, a 1-methyl-n-butoxy group, a 2-methyl-n-butoxy group, a 3-methyl-n-butoxy group, a 1,1-dimethyl-n-propoxy group, a 1,2-dimethyl-n-propoxy group, a 2,2-dimethyl-n-propoxy group, a 1-ethyl-n-propoxy group, and an n-hexyloxy group, but is not limited to these.

[0019] Examples of the acyloxy group having 2 to 10 carbon atoms include, but are not limited to, a methylcarbonyloxy group, an ethylcarbonyloxy group, an n-propylcarbonyloxy group, an i-propylcarbonyloxy group, an n-butylcarbonyloxy group, an i-butylcarbonyloxy group, an s-butylcarbonyloxy group, a t-butylcarbonyloxy group, an n-pentylcarbonyloxy group, a 1-methyl-n-butylcarbonyloxy group, a 2-methyl-n-butylcarbonyloxy group, a 3-methyl-n-butylcarbonyloxy group, a 1,1-dimethyl-n-propylcarbonyloxy group, a 1,2-dimethyl-n-propylcarbonyloxy group, a 2,2-dimethyl-n-propylcarbonyloxy group, a 1-ethyl-n-propylcarbonyloxy group, an n-hexylcarbonyloxy group, a 1-methyl-n-pentylcarbonyloxy group, and a 2-methyl-n-pentylcarbonyloxy group. The halogen group includes fluorine, chlorine, bromine, iodine, and the like. The above (meth)acryloyl group refers to both an acryloyl group and a methacryloyl group. The above formulas (2) and (3) are preferably compounds capable of forming trimethylsilyl groups on the surface of silica particles. Examples of such compounds include the following. [ka] In the above formula, R 12is an alkoxy group, such as a methoxy group or an ethoxy group. This is a process in which the silane compound reacts with a hydroxyl group on the surface of a silica particle, for example, a silanol group in the case of a silica particle, to coat the surface of the silica particle with the silane compound through a siloxane bond.

[0020] The reaction temperature can be in the range of from 20° C. to the boiling point of the dispersion medium, for example, in the range of 20° C. to 100° C. The reaction time is about 0.1 to 6 hours.

[0021] Preferred functional groups are amino, epoxy, alkyl and phenyl groups, such as aminopropyl, aminoethylaminopropyl, methyl, phenyl, glycidoxypropyl, epoxycyclohexylethyl and trifluoropropyl groups. Examples of the corresponding silane compounds include aminopropyltrimethoxysilane, aminopropyltriethoxysilane, aminoethylaminopropyltrimethoxysilane, aminoethylaminopropyltriethoxysilane, aminoethylaminopropylmethyldimethoxysilane, aminoethylaminopropylmethyldiethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, glycidoxypropyltrimethoxysilane, glycidoxypropyltriethoxysilane, epoxycyclohexylethyltrimethoxysilane, epoxycyclohexylethyltriethoxysilane, trifluoropropyltrimethoxysilane, trifluoropropyltriethoxysilane, and the like.

[0022] The amount of the silane compound coated on the surface of the silica particles is such that the number of silicon atoms in the silane compound is 0.1 / nm 2 ~4.0 pieces / nm 2 The surface of the silica particles can be coated by adding a silane compound corresponding to the coating amount to the silica sol. Water is necessary for the hydrolysis of the silane compound, and if the sol is an aqueous solvent, then the aqueous solvent is used. The hydrolysis can be carried out with or without a catalyst. When performing the reaction without a catalyst, the surface of the silica particles acts as a catalyst, and a silica sol having a pH of 2.0 to 6.5 can be used.

[0023] When a catalyst is used, examples of the hydrolysis catalyst include metal chelate compounds, organic acids, inorganic acids, organic bases, and inorganic bases. Examples of the metal chelate compounds as the hydrolysis catalyst include triethoxy mono(acetylacetonato)titanium and triethoxy mono(acetylacetonato)zirconium. Examples of the organic acids as the hydrolysis catalyst include acetic acid and oxalic acid. Examples of the inorganic acids as the hydrolysis catalyst include hydrochloric acid, nitric acid, sulfuric acid, hydrofluoric acid, and phosphoric acid. Examples of the organic bases as the hydrolysis catalyst include pyridine, pyrrole, piperazine, and quaternary ammonium salts. Examples of the inorganic bases as the hydrolysis catalyst include ammonia, sodium hydroxide, and potassium hydroxide.

[0024] In the above step (B), hydrolyzable silane is added to the aqueous dispersion of inorganic oxide particles obtained in step (A), and after stirring at room temperature (for example, about 15 to 25 ° C) for 0.01 to 2 hours, the temperature is raised to within 50 to 99 ° C and stirring is performed for 0.01 to 14 hours, and it is preferable that the stirring time after heating to 50 to 99 ° C is within a range of 1 to 100 times or 1 to 7 times compared to the stirring time at room temperature. If the above ratio is within 1 time, the hydrolyzate of hydrolyzable silane is not sufficiently coated on the inorganic oxide particles (for example, silica particles), and the silane compound present in the dispersion medium is locally coated later, and uniform coating cannot be achieved. In addition, if it is 7 times or more, the ratios of T1, T2, T3, D1, and D2 structures decrease, which is not preferable in terms of the repulsive force of the particles.

[0025] In the present invention, a state in which the hydrolyzable silane hydrolysate is bonded to silica particles and a state in which the hydrolyzable silane hydrolysate is present in the dispersion medium coexist. Both contribute to the stability of the inorganic oxide sol (silica sol) when the ratio of (the number of moles of silicon atoms in the hydrolyzable silane hydrolysate in the dispersion medium) / (the number of moles of silicon atoms of the silane bonded to the inorganic oxide particle surface) is 0.2-30.

[0026] When the hydrolysate of the hydrolyzable silane of the present invention is bonded to silica particles, the amount of silanol in the silica particles is reduced, which is characterized by an increase in Q4, where the number of bridging oxygen atoms between silicon atoms of the silica particles is 4 / 2 per silicon atom, as observed by Si-NMR, compared to before surface modification with the silane.

[0027] When the hydrolyzate of the hydrolyzable silane is bonded to the silica particles, the specific surface area of ​​the silica particles is in a state where (specific surface area calculated from the amount of water vapor adsorption) / (specific surface area calculated from the amount of nitrogen gas adsorption), which is the value obtained by dividing the specific surface area calculated from the amount of water vapor adsorption to the silica particles by the specific surface area calculated from the amount of nitrogen gas adsorption, is 0.15 to 0.95 compared to the silica particles before the addition of the silane compound.

[0028] This value indicates that the silanol groups on the surface of the silica particles have been replaced by silane compounds having functional groups. The hydrolyzate of the hydrolyzable silane in the dispersion medium is characterized in that the hydrolyzate of the silane compound in formula (1) where a is an integer of 1 contains a silane compound in which the ratio of bridging oxygen between silicon atoms is 0 / 2, 1 / 2, 2 / 2, and 3 / 2 per silicon atom as measured by Si-NMR, and the (T2+T3) / (T0+T1) ratio is 2 to 10, or the (T1+T2+T3) / (T0) ratio is 5 to 100. Either one of these conditions may be satisfied, but it is more preferable to satisfy both. The hydrolyzate of the hydrolyzable silane in the dispersion medium is characterized in that the hydrolyzate of the silane compound in formula (1) where a is an integer of 2 contains a silane compound in which the ratio of bridging oxygen between silicon atoms is 0 / 2, 1 / 2, or 2 / 2 per silicon atom as measured by Si-NMR, and the ratio of (D1+D2) / (D0) is 0.1 to 10, or the ratio of (D2) / (D0+D1) is 0.01 to 10. Either one of these conditions may be satisfied, but it is more preferable to satisfy both.

[0029] The dispersion of the present invention thus obtained is subjected to step (C) after step (B): Step (C): A step of replacing the aqueous medium of the dispersion obtained in step (B) with an organic solvent is included, thereby obtaining a dispersion in which the organic solvent is the dispersion medium.

[0030] Examples of the organic solvent include organic solvents such as alcohols, ketones, ethers, esters, amides, and hydrocarbons. Examples of the alcohols include alcohols having 1 to 10 carbon atoms, such as methanol, ethanol, i-propanol, n-propanol, and butanol. Examples of the ketones include linear or cyclic aliphatic ketones having 3 to 30 carbon atoms, such as methyl ethyl ketone, diethyl ketone, methyl propyl ketone, methyl isobutyl ketone, diisobutyl ketone, methyl amyl ketone, and cyclohexanone. Examples of the ethers include linear or cyclic aliphatic ethers having 3 to 30 carbon atoms, such as diethyl ether and tetrahydrofuran. The ester is a straight-chain or cyclic ester having 2 to 30 carbon atoms, such as ethyl acetate, butyl acetate, sec-butyl acetate, methoxybutyl acetate, amyl acetate, n-propyl acetate, i-propyl acetate, ethyl lactate, butyl lactate, ethylene glycol monomethyl ether acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, phenyl acetate, phenyl lactate, and phenyl propionate. The amide is an aliphatic amide having 3 to 30 carbon atoms, such as dimethylacetamide, dimethylformamide, N-methylpyrrolidone, and N-ethylpyrrolidone. The hydrocarbon is a straight-chain or cyclic aliphatic or aromatic hydrocarbon having 6 to 30 carbon atoms, such as hexane, heptane, octane, nonane, decane, benzene, toluene, and xylene.

[0031] The silica-containing inorganic oxide sol (e.g., silica sol) of the present invention can be used for high salt dispersion medium sols, adhesives, release agents, semiconductor encapsulants, LED encapsulants, paints, film internal additives, hard coating agents, photoresist materials, printing inks, detergents, cleaners, various resin additives, insulating compositions, rust inhibitors, lubricants, metal processing oils, film coating agents, stripping agents, well treatment agents, and the like. EXAMPLES

[0032] (Measuring Equipment) The analysis of the aqueous silica sol (pH value, electrical conductivity, viscosity, DLS average particle size, and silane bond amount) and the analysis of the sample prepared using the aqueous silica sol after the room temperature salt resistance test or the high temperature salt resistance test were performed using the following apparatus. DLS average particle size (average particle size by dynamic light scattering method): A dynamic light scattering particle size measuring device, Zetasizer Nano (manufactured by the Malvern Division of Spectris Co., Ltd.), was used. pH: A pH meter (manufactured by DKK Toa Corporation) was used. Electrical conductivity: An electrical conductivity meter (manufactured by DKK Toa Corporation) was used. Viscosity: A BMII type viscometer (manufactured by Tokyo Keiki Co., Ltd.) was used. Silane bond amount: An organic trace element analyzer CHNS / O Analyzer (PerkinElmer Japan Co., Ltd.) or a TN measurement device TN-2100V Total Nitrogen Analyzer (Mitsubishi Chemical Analytech Co., Ltd.) was used. Si-NMR: AVANCED NEO (Bruker Corporation) was used. Nitrogen gas adsorption amount: MONOSORB (Quantachrome INSTRUMENTS) was used. Water vapor adsorption: A Q5000SA adsorption analyzer (TA Instruments Japan, Inc.) was used.

[0033] [Evaluation of Silica Sol] (Removal of silane (free silane) that is not bound to silica particles) 2g of aqueous silica sol and 4g of pure water were placed in a 15ml centrifugal filter unit (trade name: Amicon Ultra 15, Merck Ltd.), and centrifuged for 20 minutes at a centrifugal force of 2770G. After centrifugation, the liquid discharged from the bottom of the unit was discarded, and the same mass of pure water as the discarded liquid was added to the aqueous silica sol concentrated on the filter to redisperse it, and then centrifuged again for 20 minutes at a centrifugal force of 2770G. The above procedure was repeated a total of four times to obtain an aqueous silica sol from which the free silane had been removed.

[0034] (Measurement of carbon content) The aqueous silica sol from which the free silane had been removed was heated and dried at 100°C, and then pulverized in a mortar to obtain silica sol powder. The carbon content of the obtained silica sol powder was measured using an organic trace element metal analyzer, and the silane bond content was calculated from the obtained carbon content using the following formula. Surface treatment amount = (Cm ÷ Cn ÷ Sc × A) / (Ct × Cs) where Cm is the carbon content, Cn is the carbon molecular weight, Sc is the number of carbon atoms in the silane, A is Avogadro's number, Ct is the silica particle mass, and Cs is the silica specific surface area. The unit of the silane bond amount obtained by measuring the carbon amount is (pieces / nm 2 ).

[0035] (Measuring the amount of nitrogen) The nitrogen amount of the aqueous silica sol from which the free silane had been removed was measured using a TN measuring device, and the silane bond amount was calculated from the obtained nitrogen amount using the following formula. Surface treatment amount = (Nm ÷ Nn ÷ Sn × A) / (Ct × Cs) where Nm is the nitrogen content, Nn is the nitrogen molecular weight, Sn is the number of nitrogen atoms in the silane, A is Avogadro's number, Ct is the silica particle mass, and Cs is the silica specific surface area. The unit of the silane bond amount obtained by measuring the nitrogen amount is (pieces / nm 2 ).

[0036] (Measurement of water vapor adsorption amount) The aqueous silica sol obtained by removing the free silane was dried on a hot plate at 80°C to obtain silica gel, which was then crushed in a mortar and further dried at 150°C for 3 hours to obtain a dry silica powder. Based on the BET theory, the specific surface area (m 2 / g) was measured (water vapor BET method).

[0037] (Measurement of nitrogen gas adsorption amount) The aqueous silica sol obtained by removing the free silane was dried on a hot plate at 80°C to obtain silica gel, which was then crushed in a mortar and further dried at 150°C for 3 hours to obtain a dry silica powder. Based on the BET theory, the specific surface area (m 2 / g) was measured (BET method, i.e., nitrogen gas BET method).

[0038] (Salt tolerance evaluation) (Preparation of salt tolerance test samples) After a stirrer was put into a 200 ml polystyrene bottle, 3.6 g of each silica sol produced in the examples or comparative examples was put in and stirred with a magnetic stirrer. While stirring with a magnetic stirrer, 46.4 g of pure water and 100 g of a brine solution with a salt concentration of 6% by mass were put in and stirred for 1 hour. This was used as a salt resistance test sample for evaluating the heat resistance and salt resistance when the silica sol was adjusted to a silica concentration of 0.5% by mass under a salt concentration of 4% by mass. The pH, electrical conductivity, and DLS average particle size of the aqueous silica sol (silica particles) in the sample of the obtained salt resistance test sample were evaluated.

[0039] (Room temperature salt tolerance evaluation) 150 g of the salt tolerance test sample was placed in a 200 ml sealable polystyrene container, and after sealing, the polystyrene container was left to stand at 20°C for a predetermined time, after which the appearance, pH, electrical conductivity, and DLS average particle size of the aqueous silica sol (silica particles) in the sample of the salt tolerance test sample were evaluated. The salt resistance was evaluated by holding the sample at 20°C for a specified time (10 hours) and then judging the salt resistance based on the DLS average particle size measurement results of the aqueous silica sol (silica particles) in the sample (see Judgment of Salt Resistance below) and evaluating the appearance.

[0040] (Determination of salt tolerance) A: The ratio of the DLS average particle size after the salt tolerance test to the DLS average particle size before the test is 1.1 or less. B: The ratio of DLS average particle size after salt tolerance test to DLS average particle size before test is 1.2 to 1.5. C: The ratio of DLS average particle size after salt tolerance test to DLS average particle size before test is 1.6 to 2.4. D: The ratio of DLS average particle size after salt tolerance test to DLS average particle size before test is 2.5 to 20.0. E: The ratio of DLS average particle size after salt tolerance test to DLS average particle size before test is 20.1 or more, or the sample becomes cloudy and undergoes solid-liquid separation. The salt tolerance test results show that A is the most favorable, followed by B, C, D, and E in that order.

[0041] (High temperature and salt resistance rating-1) 65 g of the salt resistance test sample was placed in a 120 ml Teflon (registered trademark) sealable container, and the Teflon (registered trademark) container was placed in a dryer at 100°C. After keeping the container at 100°C for a specified time (10 hours), the appearance, pH, and electrical conductivity of the salt resistance test sample were measured. The DLS average particle size of the aqueous silica sol (silica particles) in the sample was evaluated. The high-temperature salt resistance was evaluated according to the same criteria as those for evaluating the salt resistance in the room temperature salt resistance evaluation described above.

[0042] (High temperature and salt resistance evaluation-2) The high-temperature salt resistance was evaluated by the same procedure as described above (Evaluation of high-temperature salt resistance-1), except that the dryer temperature was set to 120° C. and the holding time was set to 10 hours.

[0043] (Preparation of Aqueous Silica Sol) Example 1 In a 2000-ml glass eggplant flask, 1000 g of aqueous silica sol (Nissan Chemical Industries, Ltd., Snowtex (trade name) ST-O, silica concentration 20.5 mass%, average particle size 11.7 nm by BET method, average particle size 18.6 nm by DLS method) and a magnetic stirrer were placed, and the mixture was stirred with the magnetic stirrer until the silane compound was 0.5 particles / nm2 relative to the surface area of ​​the silica in the aqueous silica sol. 2 9.4 g of 3-glycidoxypropyltrimethoxysilane (Dynasylan GLYMO manufactured by Evonik) was added so that the temperature of the aqueous sol was 60°C. A cooling tube through which tap water was flowed was then placed on top of the eggplant flask, and the aqueous sol was heated to 60°C while refluxing, and was then kept at 60°C for 4 hours, including the time required for heating, and then cooled. The stirring time after heating to 60°C was within 1 to 7 times the stirring time at room temperature. After cooling to room temperature, the aqueous sol was taken out, and 1009.4 g of aqueous sol containing an aqueous silica sol surface-treated with a silane compound was obtained. The aqueous silica sol of Example 1 was evaluated for pH, electrical conductivity, viscosity, and average particle size by the DLS method. The silane bond amount of the aqueous silica sol of Example 1 was evaluated according to (Evaluation of silane bond amount). A salt tolerance test sample was prepared according to <Preparation of salt tolerance test sample> and after keeping it at 20°C for 10 hours according to <Evaluation of salt tolerance at room temperature>, the sample was taken out and the salt tolerance at room temperature was evaluated.

[0044] Example 2 For silica in an aqueous silica sol (Nissan Chemical Industries, Ltd., Snowtex (trade name) ST-O, average particle size by BET method: 11.7 nm, average particle size by DLS method: 18.6 nm), the silane compound was 8.0 particles / nm2 relative to the surface area of ​​the silica in the aqueous silica sol. 2 The same procedure as in Example 1 was repeated, except that 149.7 g of 3-glycidoxypropyltrimethoxysilane (Dynasylan GLYMO manufactured by Evonik) was added so that the aqueous sol concentration became 1,149.7 g. The aqueous silica sol of Example 2 was evaluated for pH, electrical conductivity, viscosity, and average particle size by DLS method. The silane bond amount of the aqueous silica sol of Example 2 was evaluated according to (Evaluation of silane bond amount). A salt tolerance test sample was prepared according to (Preparation of salt tolerance test sample) and held at 100°C for 10 hours according to (High temperature salt tolerance evaluation-1), after which the sample was taken out and the high temperature salt tolerance was evaluated.

[0045] Example 3 For silica in an aqueous silica sol (Nissan Chemical Industries, Ltd., Snowtex (trade name) ST-O, average particle size by BET method: 11.7 nm, average particle size by DLS method: 18.6 nm), the silane compound was found to have a surface area of ​​30.8 particles / nm2. 2 The same procedure as in Example 1 was repeated, except that 576.2 g of 3-glycidoxypropyltrimethoxysilane (Dynasylan GLYMO manufactured by Evonik) was added so that the aqueous sol became 1,576.2 g. The aqueous silica sol of Example 3 was evaluated for pH, electrical conductivity, viscosity, and average particle size by the DLS method. The silane bond amount of the aqueous silica sol of Example 3 was evaluated according to (Evaluation of silane bond amount). A salt tolerance test sample was prepared according to (Preparation of salt tolerance test sample) and held at 100°C for 10 hours according to (High temperature salt tolerance evaluation-1), after which the sample was taken out and the high temperature salt tolerance was evaluated.

[0046] Example 4 For silica in an aqueous silica sol (Nissan Chemical Industries, Ltd., Snowtex (trade name) ST-O, average particle size by BET method: 11.7 nm, average particle size by DLS method: 18.6 nm), the silane compound was 46.2 particles / nm2 relative to the surface area of ​​the silica in the aqueous silica sol. 2 The same procedure as in Example 1 was repeated, except that 864.3 g of 3-glycidoxypropyltrimethoxysilane (Dynasylan GLYMO manufactured by Evonik) was added so that the aqueous sol became 1,864.3 g. The aqueous silica sol of Example 4 was evaluated for pH, electrical conductivity, viscosity, and average particle size by DLS method. The silane bond amount of the aqueous silica sol of Example 4 was evaluated according to (Evaluation of silane bond amount). A salt tolerance test sample was prepared according to (Preparation of salt tolerance test sample) and held at 100°C for 10 hours according to (High temperature salt tolerance evaluation-1), after which the sample was taken out and the high temperature salt tolerance was evaluated.

[0047] Example 5 For silica in an aqueous silica sol (Nissan Chemical Industries, Ltd., Snowtex (trade name) ST-O, average particle size by BET method: 11.7 nm, average particle size by DLS method: 18.6 nm), the silane compound was 0.5 particles / nm2 relative to the surface area of ​​the silica in the aqueous silica sol. 2 The same procedure as in Example 1 was repeated, except that 5.4 g of methyltrimethoxysilane (KBM-13, manufactured by Shin-Etsu Chemical Co., Ltd.) was added so that the aqueous sol concentration became 1005.4 g. The aqueous silica sol of Example 5 was evaluated for pH, electrical conductivity, viscosity, and average particle size by the DLS method. The silane bond amount of the aqueous silica sol of Example 5 was evaluated according to (Evaluation of silane bond amount). A salt tolerance test sample was prepared according to (Preparation of salt tolerance test sample), and after keeping it at 20°C for 10 hours according to (Evaluation of salt tolerance at room temperature), the sample was taken out and the salt tolerance at room temperature was evaluated.

[0048] Example 6 Aqueous silica sol (Nissan Chemical Co., Ltd., Snowtex (trade name) ST-O, measured by the BET method) The average particle size by DLS method was 11.7 nm, and the average particle size by DLS method was 18.6 nm. The silane compound was 0.5 particles / nm2 relative to the surface area of ​​the silica in the aqueous silica sol. 2 The same procedure as in Example 1 was repeated, except that 4.8 g of dimethyldimethoxysilane (KBM-22, manufactured by Shin-Etsu Chemical Co., Ltd.) was added so that the aqueous sol concentration became 1004.8 g. The aqueous silica sol of Example 6 was evaluated for pH, electrical conductivity, viscosity, and average particle size by DLS method. The silane bond amount of the aqueous silica sol of Example 6 was evaluated according to (Evaluation of silane bond amount). A salt tolerance test sample was prepared according to (Preparation of salt tolerance test sample), and after keeping it at 20°C for 10 hours according to (Evaluation of salt tolerance at room temperature), the sample was taken out and the salt tolerance at room temperature was evaluated.

[0049] Example 7 For silica in an aqueous silica sol (Nissan Chemical Industries, Ltd., Snowtex (trade name) ST-O, average particle size by BET method: 11.7 nm, average particle size by DLS method: 18.6 nm), the silane compound was 0.5 particles / nm2 relative to the surface area of ​​the silica in the aqueous silica sol. 2 Become The same procedure as in Example 1 was repeated, except that 9.8 g of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane (KBM-303, manufactured by Shin-Etsu Chemical Co., Ltd.) was added as in Example 1, to obtain 1009.8 g of an aqueous sol. The aqueous silica sol of Example 7 was evaluated for pH, electrical conductivity, viscosity, and average particle size by DLS method. The silane bond amount of the aqueous silica sol of Example 7 was evaluated according to (Evaluation of silane bond amount). A salt tolerance test sample was prepared according to (Preparation of salt tolerance test sample), and after keeping it at 20°C for 10 hours according to (Evaluation of salt tolerance at room temperature), the sample was taken out and the salt tolerance at room temperature was evaluated.

[0050] Example 8 For silica in an aqueous silica sol (Nissan Chemical Industries, Ltd., Snowtex (trade name) ST-O, average particle size by BET method: 11.7 nm, average particle size by DLS method: 18.6 nm), the silane compound was 0.5 particles / nm2 relative to the surface area of ​​the silica in the aqueous silica sol. 2 The same procedure as in Example 1 was repeated to obtain 1,008.6 g of an aqueous sol, except that 8.6 g of trifluoropropyltrimethoxysilane (KBM-7103 manufactured by Shin-Etsu Chemical Co., Ltd.) was added so that the pH value became 8.6 g. The aqueous silica sol of Example 8 was evaluated for pH, electrical conductivity, viscosity, and average particle size by DLS method. The silane bond amount of the aqueous silica sol of Example 8 was evaluated according to (Evaluation of silane bond amount). A salt tolerance test sample was prepared according to (Preparation of salt tolerance test sample), and after keeping it at 20°C for 10 hours according to (Evaluation of salt tolerance at room temperature), the sample was taken out and the salt tolerance at room temperature was evaluated.

[0051] Example 9 For silica in an aqueous silica sol (Nissan Chemical Industries, Ltd., Snowtex (trade name) ST-O, average particle size by BET method: 11.7 nm, average particle size by DLS method: 18.6 nm), the silane compound was 8.0 particles / nm2 relative to the surface area of ​​the silica in the aqueous silica sol. 2 The same procedure as in Example 1 was repeated to obtain 1,254.3 g of an aqueous sol, except that a liquid obtained by previously mixing 114.1 g of lactic acid and 140.2 g of aminopropyltriethoxysilane (KBE-903 manufactured by Shin-Etsu Chemical Co., Ltd.) and stirring for 30 minutes was added so that the aqueous sol became The aqueous silica sol of Example 9 was evaluated for pH, electrical conductivity, viscosity, and average particle size by DLS method. The silane bond amount of the aqueous silica sol of Example 9 was evaluated according to (Evaluation of silane bond amount). A salt tolerance test sample was prepared according to (Preparation of salt tolerance test sample), and after keeping it at 20°C for 10 hours according to (Evaluation of salt tolerance at room temperature), the sample was taken out and the salt tolerance at room temperature was evaluated.

[0052] Example 10 114.1 g of lactic acid was added to silica in an aqueous silica sol (Nissan Chemical Industries, Ltd., Snowtex (trade name) ST-O, average particle size by BET method: 11.7 nm, average particle size by DLS method: 18.6 nm) and stirred with a magnetic stirrer, resulting in a silane compound concentration of 8.0 particles / nm2 relative to the surface area of ​​the silica in the aqueous silica sol. 2 The same procedure as in Example 1 was repeated, except that 113.6 g of aminopropyltrimethoxysilane (KBM-903, manufactured by Shin-Etsu Chemical Co., Ltd.) was added so that the aqueous sol concentration became 1,227.7 g. The aqueous silica sol of Example 10 was evaluated for pH, electrical conductivity, viscosity, and average particle size by the DLS method. The silane bond amount of the aqueous silica sol of Example 10 was evaluated according to (Evaluation of silane bond amount). A salt tolerance test sample was prepared according to (Preparation of salt tolerance test sample), and after keeping it at 20°C for 10 hours according to (Evaluation of salt tolerance at room temperature), the sample was taken out and the salt tolerance at room temperature was evaluated. .

[0053] Example 11 228.2 g of lactic acid was added to silica in an aqueous silica sol (Nissan Chemical Industries, Ltd., Snowtex (trade name) ST-O, average particle size by BET method: 11.7 nm, average particle size by DLS method: 18.6 nm) and stirred with a magnetic stirrer, resulting in a silane compound concentration of 8.0 particles / nm2 relative to the surface area of ​​the silica in the aqueous silica sol. 2 The same procedure as in Example 1 was repeated, except that 140.9 g of aminoethylaminopropyltrimethoxysilane (KBM-603, manufactured by Shin-Etsu Chemical Co., Ltd.) was added so that the aqueous sol concentration became 1,369.1 g. The aqueous silica sol of Example 11 was evaluated for pH, electrical conductivity, viscosity, and average particle size by the DLS method. The silane bond amount of the aqueous silica sol of Example 11 was evaluated according to (Evaluation of silane bond amount). A salt resistance test sample was prepared according to (Preparation of salt resistance test sample) and held at 120°C for 10 hours according to (High temperature salt resistance evaluation-2), and then the sample was taken out and the high temperature salt resistance was evaluated.

[0054] Example 12 228.2 g of lactic acid was added to silica in an aqueous silica sol (Nissan Chemical Industries, Ltd., Snowtex (trade name) ST-O, average particle size by BET method: 11.7 nm, average particle size by DLS method: 18.6 nm) and stirred with a magnetic stirrer, resulting in a silane compound concentration of 8.0 particles / nm2 relative to the surface area of ​​the silica in the aqueous silica sol. 2 The same procedure as in Example 1 was repeated, except that 130.7 g of aminoethylaminopropylmethyldimethoxysilane (KBM-602, manufactured by Shin-Etsu Chemical Co., Ltd.) was added so that the aqueous sol reached 1,358.9 g. The aqueous silica sol of Example 12 was evaluated for pH, electrical conductivity, viscosity, and average particle size by DLS method. The silane bond amount of the aqueous silica sol of Example 12 was evaluated according to (Evaluation of silane bond amount). A salt resistance test sample was prepared according to (Preparation of salt resistance test sample) and held at 120°C for 10 hours according to (High temperature salt resistance evaluation-2), and then the sample was taken out and the high temperature salt resistance was evaluated.

[0055] Example 13 For silica in an aqueous silica sol (Nissan Chemical Industries, Ltd., Snowtex (trade name) ST-OXS, silica concentration 10.5 mass%, average particle size 5.0 nm by BET method, average particle size 8.1 nm by DLS method), the silane compound was 8.0 particles / nm2 relative to the surface area of ​​the silica in the aqueous silica sol. 2 The same procedure as in Example 1 was repeated, except that 179.4 g of 3-glycidoxypropyltrimethoxysilane (Dynasylan GLYMO manufactured by Evonik) was added so that the aqueous sol concentration became 1,179.4 g. The aqueous silica sol of Example 13 was evaluated for pH, electrical conductivity, viscosity, and average particle size by the DLS method. The silane bond amount of the aqueous silica sol of Example 13 was evaluated according to (Evaluation of silane bond amount). A salt tolerance test sample was prepared according to (Preparation of salt tolerance test sample) and held at 100°C for 10 hours according to (High temperature salt tolerance evaluation-1), after which the sample was taken out and the high temperature salt tolerance was evaluated.

[0056] Example 14 Aqueous silica sol (Nissan Chemical Industries, Ltd., Snowtex (trade name) ST-OL, silica concentration 20.5 mass%, average particle size by BET method 45.0 nm, average particle size by DLS method 7 8.0 nm) compared with 32.7 silane compounds per nm surface area of ​​silica in aqueous silica sol. 2 The same procedure as in Example 1 was repeated, except that 159.0 g of 3-glycidoxypropyltrimethoxysilane (Dynasylan GLYMO manufactured by Evonik) was added so that the aqueous sol concentration became 1,159.0 g. The aqueous silica sol of Example 14 was evaluated for pH, electrical conductivity, viscosity, and average particle size by the DLS method. The silane bond amount of the aqueous silica sol of Example 14 was evaluated according to (Evaluation of silane bond amount). A salt tolerance test sample was prepared according to (Preparation of salt tolerance test sample) and held at 100°C for 10 hours according to (High temperature salt tolerance evaluation-1), after which the sample was taken out and the high temperature salt tolerance was evaluated.

[0057] Comparative Example 1 An aqueous silica sol (Snowtex (trade name) ST-O, manufactured by Nissan Chemical Industries, Ltd.) was used as the aqueous silica sol of Comparative Example 1. The pH, electrical conductivity, and viscosity of the aqueous silica sol of Comparative Example 1, and the DLS average particle size of the aqueous silica sol (silica particles) were evaluated. The silane bond amount of the aqueous silica sol of Comparative Example 1 was evaluated according to (Evaluation of silane bond amount). A salt tolerance test sample was prepared according to (Preparation of salt tolerance test sample), and after keeping it at 20°C for 10 hours according to (Evaluation of salt tolerance at room temperature), the sample was taken out and the salt tolerance at room temperature was evaluated.

[0058] Comparative Example 2 By the same procedure as in Example 2, 1149.7 g of an aqueous silica sol was obtained. 800 g of pure water was added to 200 g of the aqueous silica sol of Example 2, and the mixture was filtered by ultrafiltration until 200 g was discharged. 800 g of pure water was added again, and the same procedure was repeated four times to obtain 200 g of aqueous silica sol from which free silane had been removed. The aqueous silica sol of Comparative Example 2 was evaluated for pH, electrical conductivity, viscosity, and average particle size by DLS method. The silane bond amount of the aqueous silica sol of Comparative Example 2 was evaluated according to (Evaluation of silane bond amount). A salt tolerance test sample was prepared according to (Preparation of salt tolerance test sample) and held at 100°C for 10 hours according to (High temperature salt tolerance evaluation-1), after which the sample was taken out and the high temperature salt tolerance was evaluated.

[0059] Comparative Example 3 For silica in an aqueous silica sol (Nissan Chemical Industries, Ltd., Snowtex (trade name) ST-O, average particle size by BET method: 11.7 nm, average particle size by DLS method: 18.6 nm), the silane compound was 2.0 particles / nm2 relative to the surface area of ​​the silica in the aqueous silica sol. 2 The same procedure as in Example 1 was repeated, except that 35.1 g of methyltrimethoxysilane (KBM-13, manufactured by Shin-Etsu Chemical Co., Ltd.) was added so that the aqueous sol concentration became 1,035.1 g. The aqueous silica sol of Comparative Example 3 was evaluated for pH, electrical conductivity, viscosity, and average particle size by the DLS method. The silane bond amount of the aqueous silica sol of Comparative Example 3 was evaluated according to (Evaluation of silane bond amount). A salt tolerance test sample was prepared according to (Preparation of salt tolerance test sample), and after keeping it at 20°C for 10 hours according to (Evaluation of salt tolerance at room temperature), the sample was taken out and the salt tolerance at room temperature was evaluated.

[0060] Comparative Example 4 A 2000 ml glass eggplant flask was filled with aqueous silica sol (Nissan Chemical Industries, Ltd., Snowtex (trade name) ST-O, silica concentration = 20.5 mass%, BET method average particle size = 11.7 nm). After adding 1000 g of a silane compound (average particle size of 18.6 nm, DLS average particle size 18.6 nm) and a magnetic stirrer, the silane compound was mixed with the silica in the aqueous silica sol at a ratio of 8.0 particles / nm2 while stirring with a magnetic stirrer. 2 Then, 149.7 g of 3-glycidoxypropyltrimethoxysilane (Dynasylan GLYMO manufactured by Evonik) was added so that the aqueous sol became 1,149.7 g. The aqueous silica sol of Comparative Example 4 was evaluated for pH, electrical conductivity, viscosity, and average particle size by the DLS method. The silane bond amount of the aqueous silica sol of Comparative Example 4 was evaluated according to (Evaluation of silane bond amount). A salt tolerance test sample was prepared according to (Preparation of salt tolerance test sample), and after keeping it at 20°C for 10 hours according to (Evaluation of salt tolerance at room temperature), the sample was taken out and the salt tolerance at room temperature was evaluated.

[0061] Comparative Example 5 By the same procedure as in Example 9, 1254.3 g of an aqueous silica sol was obtained. 800 g of pure water was added to 200 g of the aqueous silica sol of Example 9, and the mixture was filtered by ultrafiltration until 200 g was discharged. 800 g of pure water was added again, and the same procedure was repeated four times to obtain 200 g of aqueous silica sol from which free silane had been removed. The aqueous silica sol of Comparative Example 5 was evaluated for pH, electrical conductivity, viscosity, and average particle size by the DLS method. The silane bond amount of the aqueous silica sol of Comparative Example 5 was evaluated according to (Evaluation of silane bond amount). A salt tolerance test sample was prepared according to (Preparation of salt tolerance test sample), and after keeping it at 20°C for 10 hours according to (Evaluation of salt tolerance at room temperature), the sample was taken out and the salt tolerance at room temperature was evaluated.

[0062] Comparative Example 6 By the same procedure as in Example 10, 1227.7 g of an aqueous silica sol was obtained. 800 g of pure water was added to 200 g of the aqueous silica sol of Example 10, and the mixture was filtered by ultrafiltration until 200 g was discharged. 800 g of pure water was added again, and the same procedure was repeated four times to obtain 200 g of aqueous silica sol from which free silane had been removed. The aqueous silica sol of Comparative Example 6 was evaluated for pH, electrical conductivity, viscosity, and average particle size by the DLS method. The silane bond amount of the aqueous silica sol of Comparative Example 6 was evaluated according to (Evaluation of silane bond amount).

[0063] Comparative Example 7 An aqueous silica sol (Snowtex (trade name) ST-OXS, manufactured by Nissan Chemical Industries, Ltd.) was used as the aqueous silica sol of Comparative Example 7. The pH, electrical conductivity, and viscosity of the aqueous silica sol of Comparative Example 7, and the DLS average particle size of the aqueous silica sol (silica particles) were evaluated. The silane bond amount of the aqueous silica sol of Comparative Example 7 was evaluated according to (Evaluation of silane bond amount). A salt tolerance test sample was prepared according to (Preparation of salt tolerance test sample), and after keeping it at 20°C for 10 hours according to (Evaluation of salt tolerance at room temperature), the sample was taken out and the salt tolerance at room temperature was evaluated.

[0064] Comparative Example 8 An aqueous silica sol (Snowtex (trade name) ST-OL, manufactured by Nissan Chemical Industries, Ltd.) was used as the aqueous silica sol of Comparative Example 8. The pH, electrical conductivity, and viscosity of the aqueous silica sol of Comparative Example 8, and the DLS average particle size of the aqueous silica sol (silica particles) were evaluated. The silane bond amount of the aqueous silica sol of Comparative Example 8 was evaluated according to (Evaluation of silane bond amount). Prepare a salt tolerance test sample according to (Preparation of salt tolerance test sample) and test it at room temperature. After keeping the samples at 20°C for 10 hours according to the method described above, the samples were taken out and the salt tolerance at room temperature was evaluated. A brine test sample was prepared according to (Preparation of salt tolerance test sample), and after keeping it at 20°C for 10 hours according to (Evaluation of room temperature salt tolerance), the sample was taken out and the room temperature salt tolerance was evaluated. Tables 1 to 6 show the compositions (concentrations of components) and salt resistance test results of the aqueous silica sols of the examples, and Tables 7 and 8 show the compositions (concentrations of components) and salt resistance test results of the aqueous silica sols of the comparative examples.

[0065] [Table 1]

[0066] [Table 2]

[0067] [Table 3]

[0068] [Table 4]

[0069] [Table 5]

[0070] [Table 6]

[0071] [Table 7]

[0072] [Table 8] The types (symbols) of silane compounds in the table are as follows: LTAC: Lauryl trimethyl ammonium chloride (product name: Catiogen TML), active ingredient 30.0%, manufactured by Daiichi Kogyo Seiyaku Co., Ltd. GPS: 3-glycidoxypropyltrimethoxysilane (product name: Dynasylan GLYMO), manufactured by Evonik Co., Ltd. ·MTMS: Methyltrimethoxysilane (product name: KBM-13), manufactured by Shin-Etsu Chemical Co., Ltd. ·DMS: Dimethyldimethoxysilane (product name: KBM-22), manufactured by Shin-Etsu Chemical Co., Ltd. EPCHS: (3,4-epoxycyclohexyl)ethyltrimethoxysilane (product name: KBM-303), manufactured by Shin-Etsu Chemical Co., Ltd. TFPS: Trifluoropropyltrimethoxysilane (product name: KBM-7103), manufactured by Shin-Etsu Chemical Co., Ltd. APTES: 3-aminopropyltriethoxysilane (product name: KBE-903), manufactured by Shin-Etsu Chemical Co., Ltd. APTMS: 3-aminopropyltrimethoxysilane (product name: KBM-903), manufactured by Shin-Etsu Chemical Co., Ltd. AEAPTMS: N-2-(aminoethyl)-3-aminopropyltrimethoxysilane (product name: KBM-603), manufactured by Shin-Etsu Chemical Co., Ltd. AEAPMDMS: N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane (product name: KBM-602), manufactured by Shin-Etsu Chemical Co., Ltd.

[0073] (Measurement of free silane bonding state) The aqueous silica sol of the present invention is expected to have a greater effect of improving the stability of silica particles depending on the form of the free silane contained therein. The form of the free silane was analyzed by adding 6 g of aqueous silica sol to a 15 ml centrifugal filter unit (trade name: Amicon Ultra 15 (Merck Co., Ltd.) and centrifuging it for 20 minutes at a centrifugal force of 2770 G, and analyzing the liquid containing the free silane discharged from the bottom of the unit by Si-NMR to calculate the content ratio of T structure or D structure. The T-structures were measured for Examples 2, 9, 10, 13, and 14, and the measurement results are shown in Table 9. The D-structure was measured for Example 12, and the measurement results are shown in Table 10.

[0074] [Table 9] [Table 10]

[0075] (Measurement of the bonding state of bonded silane) The aqueous silica sol of the present invention is expected to have a greater effect of improving the stability of silica particles by bonding a part of the silane compound to the surface of the silica particles. The form of the bonded silane was analyzed by analyzing the liquid obtained in (removal of free silane) by Si-NMR and calculating the proportion of Q structure. The Q structure was measured for Examples 2, 5, 6, 7, 8, 9, 10, 11, 12, 13, and 14, and Comparative Examples 1, 7, and 8, and the measurement results are shown in Table 11.

[0076] [Table 11]

[0077] (Specific surface area calculated from water vapor adsorption amount / specific surface area calculated from nitrogen gas adsorption amount) The aqueous silica sol of the present invention is expected to have a greater effect of improving the stability of silica particles by replacing the silanol groups on the silica particle surface with silane compounds having functional groups. The value obtained by dividing the specific surface area calculated from the amount of water vapor adsorption on silica particles by the specific surface area calculated from the amount of nitrogen gas adsorption, (specific surface area calculated from the amount of water vapor adsorption) / (specific surface area calculated from the amount of nitrogen gas adsorption), indicates that the silanol groups on the silica particle surface have been replaced with silane compounds having functional groups. The amount of water vapor adsorption and the amount of nitrogen gas adsorption were analyzed according to the procedures of (measurement of amount of water vapor adsorption) and (measurement of amount of nitrogen gas adsorption). The water vapor adsorption amount and nitrogen gas adsorption amount were measured for Examples 1, 2, 5, 7, 8, 13, and 14, and Comparative Examples 1, 3, 7, and 8. The values ​​after the silane compound treatment were divided by the values ​​before the silane compound treatment using the formula (specific surface area calculated from the water vapor adsorption amount) / (specific surface area calculated from the nitrogen gas adsorption amount), and the measurement results are shown in Table 12.

[0078] [Table 12] [Industrial Applicability]

[0079] The present invention can provide a dispersion of inorganic oxide particles, particularly a dispersion of silica particles, which has high dispersion stability even under high temperature or high salinity conditions.

Claims

1. The dispersion contains silane-bonded silica-containing inorganic oxide particles that have been surface-modified with a hydrolyzable silane as a dispersoid and a liquid medium as a dispersion medium, the dispersion medium containing a hydrolyzate of the hydrolyzable silane, and the ratio of (the number of moles of silicon atoms in the hydrolyzate of the hydrolyzable silane in the dispersion medium) / (the number of moles of silicon atoms of the silane bonded to the surface of the inorganic oxide particles) is 0.2 to 30.

2. The silane-bonded silica-containing inorganic oxide particles are silica particles having an average particle size of 5 nm to 100 nm or inorganic oxide particles having an average particle size of 5 nm to 100 nm, The dispersion according to claim 1, wherein the inorganic oxide particles are composite metal oxide particles of silica and at least one metal oxide selected from the group consisting of alumina, tin oxide, zirconium oxide, titanium oxide, and antimony oxide, or composite oxide particles having a core-shell structure of silica and at least one metal oxide selected from the group consisting of alumina, tin oxide, zirconium oxide, titanium oxide, and antimony oxide.

3. The hydrolyzable silane is represented by formula (1) to formula (3): 【Chemistry 1】 (In formula (1), R 3 is an alkyl group, a halogenated alkyl group, an alkenyl group, or an organic group having an epoxy group, a (meth)acryloyl group, a mercapto group, an amino group, a ureido group, or a cyano group, and is bonded to a silicon atom by a Si-C bond; R 4 represents an alkoxy group, an acyloxy group, or a halogen group; a represents an integer of 1 to 3; In formula (2) and formula (3), R 5 and R 7 is an alkyl group having 1 to 3 carbon atoms and bonded to a silicon atom by a Si-C bond; R 6 and R 8 represents an alkoxy group, an acyloxy group, or a halogen group; Y represents an alkylene group, an NH group, or an oxygen atom; 5 and R 7 at least one of which is an alkyl group having 1 to 3 carbon atoms and bonded to a silicon atom by a Si-C bond, b is an integer of 1 to 3, c is an integer of 0 or 1, d is an integer of 1 to 3, and e is an integer of 1 to 3.

2. The dispersion of claim 1, wherein the silane compound is at least one selected from the group consisting of:

4. The dispersion according to claim 3, wherein the hydrolyzate of the hydrolyzable silane in the dispersion medium includes a silane compound in which, for T0, T1, T2, and T3 structures in which the ratios of bridging oxygen between silicon atoms are 0 / 2, 1 / 2, 2 / 2, and 3 / 2 per silicon atom as measured by Si-NMR, (T2+T3) / (T0+T1) is a specific value (2 to 15) or the (T1+T2+T3) / (T0) ratio is a specific value (5 to 100).

5. The dispersion according to claim 3, wherein the hydrolyzate of the hydrolyzable silane in the dispersion medium includes a silane compound having a (D1+D2) / (D0) ratio of 0.1 to 10, or a (D2) / (D0+D1) ratio of 0.01 to 10, for D0, D1 and D2 structures in which the ratio of bridging oxygen between silicon atoms is 0 / 2, 1 / 2 and 2 / 2 per silicon atom as measured by Si-NMR.

6. 2. The dispersion according to claim 1, wherein Q4, in which the number of bridging oxygen atoms between silicon atoms of the silica particles is 4 / 2 per silicon atom as determined by Si-NMR measurement, is 76% to 92%.

7. The amount of bonded silane in the silane-bonded silica-containing inorganic oxide particles is 0.3 to 5.9 particles / nm 2 2. The dispersion of claim 1, wherein

8. The amount of free silane, which is a hydrolyzate of hydrolyzable silane, in the dispersion medium is 0.1 to 40.3 particles / nm 2 2. The dispersion of claim 1, wherein

9. The dispersion according to claim 1, wherein the water vapor adsorption amount of the silane-bonded silica-containing inorganic oxide particles divided by the nitrogen gas adsorption amount, that is, (specific surface area calculated from water vapor adsorption amount) / (specific surface area calculated from nitrogen gas adsorption amount), is 0.15 to 0.95 compared to the silica-containing inorganic oxide particles before the addition of the silane compound, and the silica-containing inorganic oxide particles include silane-bonded silica-containing inorganic oxide particles and / or non-silane-bonded silica-containing inorganic oxide particles.

10. 2. The dispersion according to claim 1, wherein a ratio of the DLS average particle size after a salt tolerance test (storage) to the DLS average particle size before a salt tolerance test (storage) is 2.4 or less in a room temperature salt tolerance evaluation in which a mixture of the aqueous dispersion of the silane-bonded silica-containing inorganic oxide particles and a brine solution to a silica concentration of 0.5% by mass and a salt concentration of 4% by mass is kept at 20° C. for 10 hours.

11. The following steps (A) and (B): Step (A): obtaining an aqueous dispersion of the silane-bonded silica-containing inorganic oxide particles and / or non-silane-bonded silica-containing inorganic oxide particles; 11. The method for producing the dispersion according to any one of claims 1 to 10, comprising the step of adding a hydrolyzable silane to an aqueous dispersion of the silane-bonded silica-containing inorganic oxide particles and / or non-silane-bonded silica-containing inorganic oxide particles in a ratio of the number of the silanes per surface area of ​​the particles in the range of 0.3 to 100 particles / nm2, stirring at room temperature, and then heating to a temperature within a range of 20 to 99°C, and the stirring time after heating is 1 to 100 times or less the stirring time at room temperature.

12. The method for producing the dispersion according to claim 11, further comprising a step of adjusting the pH of the aqueous dispersion of the silane-bonded silica-containing inorganic oxide particles to a range of 2.0 to 6.5 prior to the step (B).

13. After the above step (B), step (C) is further performed: The method for producing a dispersion using an organic solvent as a dispersion medium according to claim 11, further comprising: (C) replacing the aqueous medium of the dispersion obtained in (B) with an organic solvent.

Citation Information

Patent Citations

  • Process for producing hydrophobic silica powder

    JP2006169096A

  • Crude oil recovery chemical

    JP2021006595A

  • Process of producing inorganic oxide organosol

    JP2005200294A

  • Dispersion liquid of surface-treated particle, and curable composition containing dispersion liquid

    JP2020164374A