Laminate film

A laminated film with a core and skin layer composition addresses winding misalignment and ethylene accumulation issues in polypropylene films, enhancing the stability and insulation of build-up films for electronic components.

JP2024149773AActive Publication Date: 2024-10-18OJI HLDG CORP
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2024135127
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-10-18
Estimated Expiration
2040-11-11

AI Technical Summary

Technical Problem

Polypropylene films used as protective films in build-up films for electronic components suffer from winding misalignment due to vibrations during transport, and the addition of anti-blocking agents can affect insulation performance by transferring to the thermosetting resin, leading to uneven thickness and reduced insulation.

Method used

A laminated film with a core layer made of homopolypropylene and a skin layer containing a propylene-based elastomer, ethylene-propylene block copolymer, and ethylene-propylene random copolymer, with specific ethylene and butene content and loss tangent characteristics, is used to suppress winding misalignment and reduce ethylene component accumulation.

Benefits of technology

The laminated film effectively prevents winding misalignment and reduces ethylene component deposition on rolls, maintaining insulation performance and ensuring smooth rolling of build-up films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149773000001
    Figure 2024149773000001
Patent Text Reader

Abstract

To provide a novel laminate film in which, in the case where a protective film of an adhesive layer of build-up film is wound together with a base film to form a winding body, generation of winding slippage between the protective film and the base film of the winding body is preferably suppressed when physical external force is added to the winding body, and furthermore, accumulation of an ethylene component on a longitudinal stretching roll in a film production step can be reduced.SOLUTION: A laminate film comprises: a core layer made of composition (B) containing homopolypropylene (b1); and a skin layer which is formed on at least one surface side of the core layer, and made of composition (A) containing propylene-based elastomer (a1), ethylene / propylene block copolymer (a2), and ethylene / propylene random copolymer (a3), where the composition (A) has loss tangent tanδ of 0.06 or more at vibration frequency 1 Hz and temperature 20°C, and the composition (A) has the total content ratio of ethylene and butene of 8.0 mass% or more.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminated film, specifically to a laminated film having a core layer and a skin layer, which is used, for example, as a protective film for a build-up film used in the manufacture of electronic components. [Background technology]

[0002] Polypropylene films are widely used as industrial material films, including for packaging, due to their light weight and excellent thermal and mechanical stability. In particular, in recent years, polypropylene films have been widely used as protective materials and release materials in the manufacturing process of electronic components and electronic substrates, the manufacturing process of thermosetting resin members such as fiber-reinforced plastics, the manufacturing process of photosensitive films, and the like, taking advantage of their low surface energy. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 6354634 [Patent Document 2] JP 2018-204002 A [Patent Document 3] Patent No. 6341049 [Patent Document 4] JP 2017-66395 A [Patent Document 5] WO2018 / 079161 Summary of the Invention [Problem to be solved by the invention]

[0004] For example, polypropylene films are used as protective films for protecting adhesive layers in build-up films used in the manufacture of electronic components, and are wound, stored, distributed, and used as build-up film rolls. The build-up film has a laminated structure in which a base film (such as a PET film), an adhesive layer (uncured or semi-cured thermosetting resin that serves as a sealant for electronic substrates), and a protective film are laminated. In such build-up films, in the winding process after laminating a protective film on the adhesive layer applied to the base film, the adhesive layer (uncured or semi-cured thermosetting resin) is soft, so that if the winding tension is increased, the adhesive layer is likely to protrude from the end face of the roll. For this reason, in the winding process, the film is wound with a low winding tension so that the thermosetting resin does not protrude. This causes a problem that, in the transport process of the roll of the build-up film, the protective film (polypropylene film) and the base film included in the roll are likely to be misaligned due to vibrations of the conveyor, etc.

[0005] In addition, in order to improve the processability of polypropylene films, it is common to add an antiblocking agent to adjust the frictional force. However, the polypropylene film used in the build-up film may affect the insulating performance of the thermosetting resin (insulating member that seals the electronic substrate) that it comes into contact with, so there is a limit to the addition of antiblocking agents and the like. Specifically, if the polypropylene film surface is made uneven by adding an antiblocking agent, when the polypropylene film (protective film) is peeled off from the thermosetting resin, the antiblocking agent present on the polypropylene film surface may fall off and transfer to the thermosetting resin. The part of the thermosetting resin surface to which the antiblocking agent has been transferred may have a thinner layer thickness of the thermosetting resin than other parts, and the insulating performance may be reduced. For this reason, there is a limit to the addition of fine particles such as antiblocking agents to the polypropylene film used in the build-up film.

[0006] As a polypropylene film that is given a suitable winding property without blending an antiblocking agent, for example, a film containing polypropylene and a polyolefin other than polypropylene and having a suitable roughness on the film surface due to the compatibility of the resins is known (Patent Document 1). Such a polypropylene film is considered to be suitable for processability as a work-in-progress. However, when the film described in Patent Document 1 is used as a protective film for a build-up film, the roughening of the film surface makes it difficult for winding misalignment to occur due to a decrease in the contact area with the mating base film (PET film, etc.) caused by air entrainment during winding. On the other hand, when the film surface is roughened, the actual contact area with the mating base film (PET film, etc.) that has high smoothness is reduced, so there is a problem that winding misalignment is likely to occur between the protective film (polypropylene film) and the base film (PET film, etc.) due to vibration during transport of the roll wound as a build-up film.

[0007] Also, as a method for preventing the winding slippage of a build-up film roll, for example, a laminated film is known that includes a core layer and a skin layer laminated on at least one side of the core layer, and the ethylene content in the skin layer is adjusted within a predetermined range to suppress the winding slippage between the core layer and the mating substrate film (PET film, etc.) (Patent Document 2). However, the laminated film described in Patent Document 2 can control the winding slippage of the build-up film roll to a level that can be used as a product by adjusting the ethylene content in the skin layer within a predetermined range, but the prevention of the winding slippage of the build-up film roll is insufficient and there is room for improvement. Furthermore, in the laminated film described in Patent Document 2, low molecular weight components derived from ethylene in the skin layer gradually accumulate on the surface of the roll used in the production of the thermoplastic film. Thereafter, the accumulated ethylene components are retransferred to the film, causing foreign matter defects, so there is a problem that the ethylene content in the skin layer must be reduced as much as possible.

[0008] Also, in order to improve conformability to various surfaces, elastomer-containing films and sheets are known that utilize the property (flexibility) of using elastomers (rubber) to flexibly follow the shape changes of the other object (Patent Documents 3 to 5). However, the films described in Patent Documents 3 to 4 are intended to improve the adhesive strength with the other object that they come into contact with, and are not a means for preventing slippage when rolling. Also, the film described in Patent Document 5 is intended to improve vibration damping (the action of converting vibrations into thermal energy and attenuating them) by providing an elastomer layer and controlling the loss tangent of the elastomer layer, and is not a means for preventing slippage when rolling.

[0009] The present invention has as its main object the provision of a novel laminated film that, when the laminated film is wound together with a base film as a protective film for a pressure-sensitive adhesive layer to form a roll, when a physical external force is applied to the roll, suitably suppresses the occurrence of a winding misalignment between the protective film of the roll and the base film, and further, can reduce the accumulation of ethylene components on the surface of a transport roll such as a longitudinal stretching roll in a film manufacturing process. The laminated film can be suitably used as a protective film for the pressure-sensitive adhesive layer of a build-up film used in the manufacture of electronic components. The laminated film can also be used as a protective film in various fields such as the manufacturing process of a thermosetting resin member (pressure-sensitive adhesive layer) such as fiber-reinforced plastics. The present invention also has as its object the provision of a novel rolled body using the laminated film, in which the occurrence of a winding misalignment is suppressed.

[0010] The present inventors have conducted intensive research to solve the above problems, and have found that, in a laminated film having a core layer and a skin layer laminated on at least one side of the core layer, the skin layer is formed from a predetermined resin composition containing a propylene-based elastomer (a1), the ethylene and butene contents in the skin layer are set within a predetermined range, and the loss tangent tanδ of the skin layer of the cast raw sheet (unstretched) is controlled, so that when the skin layer is wound together with a base film as a protective film for a pressure-sensitive adhesive layer to form a roll, when a physical external force is applied to the roll, the occurrence of winding slippage between the protective film and the base film of the roll can be suitably suppressed, and further, the accumulation of ethylene components on the roll surface in the film manufacturing process can be reduced. The present invention was completed through further research based on this knowledge.

[0011] That is, the present invention includes the following. Item 1. A core layer made of a composition (B) containing homopolypropylene (b1); A propylene-based elastomer (a1) formed on at least one side of the core layer; a skin layer made of a composition (A) containing an ethylene-propylene block copolymer (a2) and an ethylene-propylene random copolymer (a3); Equipped with The composition (A) has a loss tangent tanδ of 0.06 or more at a vibration frequency of 1 Hz and a temperature of 20° C., The composition (A) is a laminated film having a total content of ethylene and butene of 8.0% by mass or more. Item 2. The laminate film according to item 1, wherein the composition (A) has an ethylene content of 35.0 mass% or less. Item 3. The composition (A) contains the propylene-based elastomer (a1) in an amount of 5 to 65 parts by mass and the ethylene-propylene block copolymer (a2) in an amount of 30 to 40 parts by mass. 90 parts by mass, and the content of the ethylene-propylene random copolymer (a3) ​​is 5 to 65 parts by mass. Item 4. The laminate film according to any one of items 1 to 3, which is used as a protective film for a pressure-sensitive adhesive layer of a build-up film. Item 5. A roll formed by winding a build-up film including the laminate film according to any one of items 1 to 3. Effect of the Invention

[0012] According to the present invention, a novel laminated film can be provided that, when the laminated film is wound together with a base film as a protective film for the adhesive layer of a build-up film to form a roll, when a physical external force is applied to the roll, the occurrence of a winding slippage between the protective film of the roll and the base film of the roll can be suitably suppressed, and further, the accumulation of ethylene components on a longitudinal stretching roll in a film manufacturing process can be reduced. Such a laminated film can be suitably used, for example, as a protective film for the adhesive layer of a build-up film used in the manufacture of electronic components. Another object of the present invention is to provide a novel roll that uses the laminated film and is suppressed from causing a winding slippage. The roll can be configured as a roll of a build-up film for electronic components. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The laminated film according to the present embodiment includes a core layer made of a composition (B) containing homopolypropylene (b1), and a skin layer laminated on at least one side of the core layer. The skin layer contains a propylene-based elastomer (a1), an ethylene-propylene block copolymer (a2), and an ethylene-propylene random copolymer (a3). The skin layer has a loss tangent tanδ of 0.06 or more at a vibration frequency of 1 Hz and a temperature of 20° C. The total content of ethylene and butene in the skin layer is 8.0 mass % or more. The laminated film according to the present embodiment has these characteristics, and thus can exhibit the above-mentioned effect of the present invention, that is, "when the laminated film according to the present embodiment is wound together with a base film as a protective film for a pressure-sensitive adhesive layer to form a roll, when a physical external force is applied to the roll, the occurrence of a winding slip between the protective film and the base film of the roll is suitably suppressed, and further, the accumulation of ethylene components on the roll surface in the film manufacturing process can be reduced."

[0014] The roll according to the present embodiment is a roll of a laminate using the laminate film according to the present embodiment as a protective film. For example, the roll can be a roll formed by winding a build-up film including the laminate film according to the present embodiment. A specific configuration of the roll according to the present embodiment is a laminate in which a base film, a pressure-sensitive adhesive layer, and the laminate film according to the present embodiment are laminated in this order, and the pressure-sensitive adhesive layer and either the skin layer or the core layer of the laminate film are in contact with each other, and the laminate can be wound around a core. The roll according to the present embodiment uses the laminate film according to the present embodiment as a protective film, so that when a physical external force is applied to the roll, the occurrence of a winding misalignment between the protective film and the base film of the roll is suitably suppressed.

[0015] The laminated film according to the present embodiment and the roll using the laminated film will be described in detail below. In this specification, the term "to" in a numerical range means "at least" or "not more than." In other words, the term "α to β" means "at least α and not more than β" or "at least β and not more than α," and includes both α and β as a range.

[0016] <1. Laminated film> The laminated film according to this embodiment includes a core layer and a skin layer laminated on at least one side of the core layer.

[0017] The thickness of the laminated film according to this embodiment can be appropriately selected depending on the application of the laminated film. For example, from the viewpoint of suitably using the laminated film according to this embodiment as a protective film for a build-up film used in the manufacture of electronic components, the thickness is preferably 200 μm or less, more preferably 100 μm or less, even more preferably 80 μm or less, and particularly preferably 60 μm or less, and the lower limit of the thickness is, for example, 3 μm or more, preferably 5 μm or more, and more preferably 10 μm or more. The thickness of the laminated film can be measured using a micrometer (JIS B-7502) in accordance with JIS C-2151.

[0018] The laminate film according to this embodiment is preferably a stretched laminate film, and more preferably a biaxially stretched laminate film.

[0019] (Core layer) The resin forming the core layer is not particularly limited as long as it can function as a support for the skin layer, but a polypropylene resin is preferred.

[0020] Examples of polypropylene resins suitable for forming the core layer include a propylene homopolymer, a copolymer of propylene and ethylene, and a copolymer of propylene, ethylene and an α-olefin having 4 to 20 carbon atoms (for example, at least one of ethylene, butene, pentene, hexene, etc.). Among these, it is preferable to use one type of polypropylene homopolymer alone or a mixture of two or more types, because it is easy to increase the mechanical strength and heat resistance of the core layer and further, it is possible to appropriately roughen the surface of the core layer.

[0021] The content of polypropylene resin in the resin forming the core layer is not particularly limited, but from the viewpoint of functioning as a support for the skin layer, it is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 98% by mass or more.

[0022] The melt flow rate (MFR) of the polypropylene resin is preferably 0.5 g / 10 min to 9.0 g / 10 min, more preferably 1.0 g / 10 min to 6.0 g / 10 min, and even more preferably 2.0 g / 10 min to 5.0 g / 10 min. When the melt flow rate of the polypropylene resin is equal to or higher than the lower limit, sufficient resin fluidity is obtained, the thickness of the cast raw sheet is easily controlled, and a film stretched with high accuracy in the width direction is easily produced, which is preferable. In addition, when the melt flow rate of the polypropylene resin is equal to or lower than the upper limit, the mechanical properties of the obtained sheet are easily improved, and the stretchability is easily improved, which is preferable. In this specification, the MFR of the resin can be measured at 230° C. and a load of 21.18 N using a melt flow indexer (for example, a melt indexer manufactured by Toyo Seiki Seisakusho Co., Ltd.) in accordance with JIS K-7210 (1999).

[0023] The weight average molecular weight (Mw) of the polypropylene resin is preferably 200,000 to 600,000, more preferably 250,000 to 500,000. When the weight average molecular weight Mw of the polypropylene resin is equal to or higher than the lower limit, sufficient resin fluidity is obtained, the thickness of the cast raw sheet is easily controlled, and a film suitable for a core layer that is stretched with high accuracy in the width direction is easily produced, which is preferable. In addition, when the weight average molecular weight Mw of the polypropylene resin is equal to or lower than the upper limit, the mechanical properties of the obtained sheet are easily improved, and a film suitable for a core layer with improved stretchability is obtained, which is preferable.

[0024] The molecular weight distribution (Mw / Mn) of the polypropylene resin, calculated as the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn), is preferably 4 or more, more preferably 4.5 or more. If the molecular weight distribution (Mw / Mn) of the polypropylene resin is equal to or more than the lower limit, β crystals can be sufficiently generated in the cast raw sheet before stretching, and it is easy to obtain a suitable strength for the core layer, which is preferable. The upper limit of the molecular weight distribution (Mw / Mn) of the polypropylene resin is not particularly limited, but is preferably 10 or less.

[0025] The weight average molecular weight (Mw) and number average molecular weight (Mn) of the polypropylene resin can be measured by gel permeation chromatography (GPC). There is no particular limitation on the GPC device used in the GPC method, and a commercially available high-temperature GPC measuring instrument capable of analyzing the molecular weight of polyolefins (for example, a high-temperature GPC measuring instrument with built-in differential refractometer (RI), manufactured by Tosoh Corporation, HLC-8121GPC-HT) can be used. In this case, for example, the measurement can be performed using the GPC column, column temperature, eluent, and flow rate described in the examples. Usually, a calibration curve is prepared using standard polystyrene, and the weight average molecular weight (Mw) and number average molecular weight (Mn) are obtained by polystyrene conversion.

[0026] The thickness of the core layer can be appropriately selected depending on the application of the laminated film according to this embodiment. For example, from the viewpoint of suitably using the laminated film according to this embodiment as a protective film for a build-up film used in the manufacture of electronic components, the thickness of the core layer can be 50% or more and 93% or less of the total thickness of the laminated film. The thickness of the core layer can be measured by cutting the laminated film and observing the cross section with a microscope.

[0027] (Skin layer) The skin layer is laminated on at least one side of the core layer. In the laminate film according to the present embodiment, at least one surface may be constituted by the surface of the skin layer.

[0028] In the laminated film according to the present embodiment, the core layer comes into contact with the surface of the object to be protected, thereby suitably protecting the object to be protected. For example, when the laminated film is used as a protective film for the pressure-sensitive adhesive layer, and the pressure-sensitive adhesive layer applied to the base film and the core layer come into contact with each other, the laminated film is wound together with the base film to form a roll, and when a physical external force is applied to the roll, the occurrence of a winding misalignment between the protective film and the base film of the roll can be suitably suppressed.

[0029] The skin layer may be laminated on both sides of the core layer. In the laminated film according to the present embodiment, the surfaces of both sides are constituted by the surfaces of the skin layer, so that the skin layer of the laminated film can suitably protect the object to be protected, and furthermore, it is possible to suitably suppress the occurrence of winding misalignment between the protective film and the base film of the roll. When the skin layer is formed on both sides of the core layer, the resin composition forming each skin layer, the thickness of the skin layer, the surface characteristics of the skin layer, etc. may be the same or different.

[0030] In the laminated film according to the present embodiment, a skin layer may be laminated on one side of the core layer, and a layer different from the skin layer may be laminated on the other side of the core layer. It is preferable that the layer different from the skin layer is also made of a polypropylene resin.

[0031] The skin layer includes a propylene-based elastomer (a1) and a propylene-based copolymer. Specifically, the skin layer can be formed from a resin composition (A) including the propylene-based elastomer (a1), an ethylene-propylene block copolymer (a2), and an ethylene-propylene random copolymer (a3).

[0032] In the skin layer, the mass ratio of the propylene-based elastomer (a1), the ethylene-propylene block copolymer (a2), and the ethylene-propylene random copolymer (a3) ​​(propylene-based elastomer (a1):ethylene-propylene block copolymer (a2):ethylene-propylene random copolymer (a3)) is not particularly limited, but from the viewpoints of optimizing the surface characteristics (dynamic friction coefficient, etc.) of the skin layer, reducing the deposition of the ethylene component on the roll surface in the film production process, and optimizing the effects of the present invention, the mass ratio is preferably about 5:90:5 to 40:40:20, more preferably about 5:90:5 to 30:40:30, even more preferably about 5:90:5 to 30:60:10, and particularly preferably about 5:90:5 to 20:70:10.

[0033] The contents of the propylene-based elastomer (a1), ethylene-propylene block copolymer (a2) and ethylene-propylene random copolymer (a3) ​​in the skin layer are not particularly limited, but from the viewpoint of fully exerting the effects of the present invention, the propylene-based elastomer (a1) is preferably in the range of 5 to 65 parts by mass, the ethylene-propylene block copolymer (a2) is preferably in the range of 30 to 90 parts by mass, and the ethylene-propylene random copolymer (a3) ​​is preferably in the range of 5 to 65 parts by mass. Also, from the viewpoint of effectively suppressing the stain of the ethylene component on the roll surface, the propylene-based elastomer (a1) is more preferably in the range of 5 to 55 parts by mass, the ethylene-propylene block copolymer (a2) is more preferably in the range of 30 to 80 parts by mass, and the ethylene-propylene random copolymer (a3) ​​is more preferably in the range of 15 to 65 parts by mass. From the viewpoint of effectively suppressing the occurrence of winding slippage, it is more preferable that the propylene-based elastomer (a1) is in the range of 15 to 55 parts by mass, the ethylene-propylene block copolymer (a2) is in the range of 30 to 70 parts by mass, and the ethylene-propylene random copolymer (a3) ​​is in the range of 15 to 55 parts by mass.

[0034] Similarly, the content of the propylene-based elastomer (a1), the ethylene-propylene block copolymer (a2) and the ethylene-propylene random copolymer (a3) ​​in the skin layer is preferably in the range of 5 to 65 mass% for the propylene-based elastomer (a1), 30 to 90 mass% for the ethylene-propylene block copolymer (a2) and 5 to 65 mass% for the ethylene-propylene random copolymer (a3). From the viewpoint of effectively suppressing the stain of the ethylene component on the roll surface, the content of the propylene-based elastomer (a1) is more preferably in the range of 5 to 55 mass%, the ethylene-propylene block copolymer (a2) is 30 to 80 mass%, and the ethylene-propylene random copolymer (a3) ​​is 15 to 65 mass%. From the viewpoint of effectively suppressing the occurrence of winding slippage, it is more preferable that the propylene-based elastomer (a1) is in the range of 15 to 55 mass%, a2 is in the range of 30 to 70 mass%, and the ethylene-propylene random copolymer (a3) ​​is in the range of 15 to 55 mass%.

[0035] The propylene-based elastomer (a1) used in the composition (A) is a propylene-ethylene-α-olefin terpolymer containing structural units derived from propylene, structural units derived from ethylene, and structural units derived from an α-olefin having 4 to 20 carbon atoms. Specific examples of the α-olefin having 4 to 20 carbon atoms include 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-hexadecene, 3-methyl-1-butene, and 4-methyl-1-pentene.

[0036] The propylene-based elastomer (a1) used in the composition (A) may be, for example, a propylene-ethylene-1-butene copolymer. A copolymer having 50 to 87 mol % of propylene-derived structural units, 10 to 25 mol % of ethylene-derived structural units, and 3 to 25 mol % of 1-butene-derived structural units is preferred.

[0037] The propylene-based elastomer (a1) used in the composition (A) is preferably a copolymer having an ethylene content of 1 to 15 mass %, more preferably a copolymer having an ethylene content of 3 to 12 mass %.

[0038] The propylene-based elastomer (a1) used in the composition (A) is preferably a copolymer having a 1-butene content of 1 to 15 mass %, more preferably a copolymer having a 1-butene content of 1 to 12 mass %.

[0039] The MFR of the propylene-based elastomer (a1) is preferably from 3 to 14 g / 10 min, more preferably from 5 to 12 g / 10 min, from the viewpoint of moldability.

[0040] The ethylene-propylene block copolymer (a2) used in the composition (A) is preferably a block copolymer having an ethylene content of 1 to 15 mass %, more preferably a block copolymer having an ethylene content of 3 to 12 mass %.

[0041] The MFR of the ethylene-propylene block copolymer (a2) is preferably from 3 to 12 g / 10 min, more preferably from 5 to 10 g / 10 min, from the viewpoint of moldability.

[0042] The weight average molecular weight (Mw) of the ethylene-propylene block copolymer (a2) is not particularly limited, but is preferably 200,000 to 600,000, and more preferably 300,000 to 500,000. The molecular weight distribution (Mw / Mn), calculated as the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn), is preferably 4 or more, and more preferably 5 or more. The method for measuring these weight average molecular weight (Mw) and number average molecular weight (Mn) is the same as the method for measuring the polypropylene resin described above.

[0043] The ethylene-propylene random copolymer (a3) ​​used in the composition (A) is preferably a random copolymer having an ethylene content of 0.5 to 6 mass %, more preferably a random copolymer having an ethylene content of 1 to 5 mass %.

[0044] The MFR of the ethylene-propylene random copolymer (a3) ​​is preferably from 5 to 14 g / 10 min, more preferably from 7 to 12 g / 10 min, from the viewpoint of moldability.

[0045] The weight average molecular weight (Mw) of the ethylene-propylene random copolymer (a3) ​​is not particularly limited, but is preferably 200,000 to 600,000, more preferably 300,000 to 500,000. The molecular weight distribution (Mw / Mn) calculated as the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn) is preferably 4 or more, more preferably 5 or more. The method for measuring these weight average molecular weight (Mw) and number average molecular weight (Mn) is the same as the method for measuring the polypropylene resin described above.

[0046] In the laminate film according to this embodiment, the propylene content in the skin layer is preferably 65% ​​by mass or more, more preferably 70% by mass or more, further preferably 80% by mass or more, and particularly preferably 85% by mass or more.

[0047] In the laminated film according to the present embodiment, the total content of ethylene and butene in the skin layer may be 8.0% by mass or more. From the viewpoint of making the surface characteristics (dynamic friction coefficient, etc.) of the skin layer favorable and reducing the deposition of the ethylene component on the roll surface in the film production process, and favorably exerting the effects of the present invention, the total content of ethylene and butene in the skin layer is preferably in the range of 8.0 to 35.0% by mass, more preferably in the range of 8.0 to 25.0% by mass. From the same viewpoint, the content of ethylene in the skin layer is preferably 35.0% by mass or less, more preferably 25.0% by mass or less, even more preferably 15.0% by mass or less, even more preferably 10.0% by mass or less, and particularly preferably 9.5% by mass or less. The lower limit of the ethylene content is, for example, 5.0% by mass or more, 7.0% by mass or more, etc. From the same viewpoint, the butene content in the skin layer is preferably 35.0% by mass or less, more preferably 25.0% by mass or less, further preferably 5.0% by mass or less, and particularly preferably 3.0% by mass or less. The lower limit of the butene content is preferably, for example, 0.1% by mass or more, 0.3% by mass or more, 0.5% by mass or more, etc. The ethylene and butene contents in the skin layer are derived from the ethylene units and butene units contained in the propylene-based elastomer (a1), the ethylene-propylene block copolymer (a2), and the ethylene-propylene random copolymer (a3). The ethylene and butene contents in the skin layer are determined using a nuclear magnetic resonance apparatus or the like. More specifically, in the present invention, AVANCE NEO700 manufactured by Bruker is used, and the observation nucleus is 13 Measured at C (176.08MHz).

[0048] The measurement mode is inverse gated decoupling (quantitative method), the shift standard is 5-propylene unit chain (mmmm) (21.95 ppm), the number of accumulations is 2048, and the temperature is 130°C.

[0049] The monomer composition was calculated from the integral value of the main chain methylene carbon based on the monomer chain, with reference to documents such as "GJ Ray et al., Macromolecules 1977, 10, p. 773-778" and "Y.-D. Zhang et al., Polym. J. 2003, 35, p. 551-559." The total content of ethylene and butene in the skin layer was calculated by measuring the ethylene content and butene content of each of the resins used to form the skin layer using the above-mentioned method, and taking into account the blending ratio of each resin in the skin layer. value.

[0050] The laminate film according to this embodiment is prepared by cutting a skin layer single-layer cast raw sheet made of composition (A) into a rectangular shape, and the loss tangent tanδ measured using a dynamic viscoelasticity device is 0.06 or more at a vibration frequency of 1 Hz and a temperature of 20° C. Since the surface of the skin layer of the laminate film according to this embodiment has such surface characteristics, it is possible to suitably exhibit the effects of the present invention described above.

[0051] A skin layer single-film cast raw sheet made of composition (A) is cut into a strip of 40 mm lengthwise and 8 mm widthwise, and the loss tangent tan δ at a vibration frequency of 1 Hz and a temperature of 20° C. is measured by the following measurement method. Note that, as a more specific measurement method, the method described in the Examples is adopted.

[0052] [loss tangent tanδ] Dynamic viscoelasticity is measured using a dynamic viscoelasticity measuring device (for example, a "Viscoelasticity measuring device (model: DMS6100)" manufactured by Seiko Instruments Inc.). A skin layer single-film cast original sheet made of composition (A) was cut into a rectangular shape, and the temperature dependence of the skin layer single-film cast original sheet made of composition (A) was measured in accordance with JIS-K7244 (1999 edition) under the measurement conditions of a tensile mode, a vibration frequency of 1 Hz, a chuck distance of 20 mm, and a heating rate of 5°C / min. From the measurement results, the loss tangent tanδ at 20°C was calculated from the temperature dispersion of the loss tangent.

[0053] The laminated film according to this embodiment has a surface tension of 5.56 gf / cm2, measured by overlapping the surface of the skin layer and the biaxially oriented polyester film. 2 The coefficient of dynamic friction under pressure is 1.0 or more. Furthermore, the coefficient of dynamic friction measured by overlapping the surface of the skin layer with a biaxially oriented polyester film is 33.33 gf / cm 2 The coefficient of dynamic friction under pressure is 1.0 or more. Since the surface of the skin layer of the laminated film according to this embodiment has such surface characteristics, it is possible to preferably exhibit the effects of the present invention described above.

[0054] For the surface of the skin layer, 5.56gf / cm 2 Dynamic friction force D1 under pressure: 33.33gf / cm 2 The kinetic friction force D2 under pressure is measured by the following friction force measurement method. Note that, as a more specific measurement method, the method described in the examples is adopted.

[0055] [Frictional force] Various frictional forces are measured using a surface property measuring device (for example, "HEIDON Tribogear (model: TYPE14FW)" manufactured by Shinto Scientific Co., Ltd.). The laminated film is cut into a length of 20 cm in the vertical direction and 3 cm in the horizontal direction to prepare a test film. Next, the test film is pressed against a 30 mm flat indenter (contact area 9 cm) without any wrinkles. 2 ) in the test film. At this time, the skin layer of the test film is set on the outside. Next, a biaxially oriented polyester film (arithmetic mean height (Sa) 0.001 μm, root mean square height (Sq) 0.001 μm, root mean square slope (Sdq) 0.001, interface area development ratio (Sdr) 0.000%, core level difference (Sk) 0.002 μm, protruding valley height (Svk) 0.001 μm, protruding valley space volume (Vvv) 0.000 ml / m) used for measuring the frictional force of the skin layer was 2 , Core space volume (Vvc) 0.001 ml / m 2 , core volume (Vmc) 0.001ml / m 2A biaxially oriented polyester film (0.08μm in height, 0.08μm in maximum height (Sz), 50μm in thickness) is cut into a length of 20cm lengthwise and 8cm widthwise, and set on a movable table without wrinkles so that the untreated side that has not been subjected to surface modification treatment such as corona discharge is facing up. The biaxially oriented polyester film has an arithmetic mean height Sa (ISO25178) of 0.001μm, a maximum height Sz (ISO25178) of 0.08μm, a thickness (JIS C-2318) of 50μm, a static friction coefficient (JIS K-7125) of 0.46, a dynamic friction coefficient (JIS K-7125) of 0.40, a haze (JIS K-7105) of 0.9%, and a total light transmittance (JIS K-7105) of 92.0%, and is used to measure the static and dynamic friction coefficients by contacting the skin layer.

[0056] In this state, the surface of the skin layer of the test film is overlapped with the biaxially oriented polyester film and measured. The strength is 5.56 gf / cm 2 The coefficient of dynamic friction D1 under pressure is calculated using a table speed of 100 mm / min and a vertical load of 50 gf (equivalent to 5.56 gf / cm 2 ), displacement of 60 mm or more (one-way movement), data sampling speed every 50 ms, measurement temperature of 23°C, and measurement humidity of 50% RH. The dynamic friction coefficient D1 (average value between displacements of 1 to 60 mm) is extracted from the values ​​obtained from each of the three measurements.

[0057] In addition, the surface of the skin layer of the test film was overlapped with a biaxially stretched polyester film and measured, and the strength was 33.33 gf / cm 2 The coefficient of dynamic friction under pressure, D2, is calculated as follows: table speed 100 mm / min, vertical load 300 gf (equivalent pressure 33.33 gf / cm 2 ), displacement of 60 mm or more (one-way movement), data sampling speed every 50 ms, measurement temperature of 23°C, measurement humidity of 50% RH. The dynamic friction coefficient D2 (average value between displacements of 1 to 60 mm) is extracted from the values ​​obtained from each of the three measurements.

[0058] The laminate film of this embodiment is preferably a surface-roughened laminate film in which the surface of the skin layer is roughened. Specifically, in order to more suitably exert the effects of the present invention described above, the surface roughness of the skin layer of the laminate film of this embodiment preferably satisfies at least one of the following (a) to (e), more preferably satisfies two or more, even more preferably satisfies three or more, and particularly preferably satisfies all of them.

[0059] (a) The root mean square height (Sq) is 0.48 to 1.12 μm. (b) The interface area development ratio (Sdr) is 0.54 to 3.01%. (c) The level difference (Sk) of the core portion is 1.03 to 2.78 μm. (d) The protruding peak height (Spk) is 0.68 to 1.42 μm. (e) The protruding valley height (Svk) is 0.17 to 0.64 μm.

[0060] The above physical property related to the surface roughness of the skin layer is measured by the following surface roughness measuring method. Note that, as a more specific measuring method, the method described in the Examples is adopted.

[0061] [Surface roughness] An optical interference non-contact surface shape measuring instrument (for example, "VertScan2.0 (model: R5500GML)" manufactured by Ryoka Systems Co., Ltd.) is used. As a measurement sample, a film is cut into an arbitrary size of about 20 cm square, and after wrinkles are sufficiently removed, it is set on the measurement stage using an electrostatic contact plate or the like. First, the measurement is performed in WAVE mode, a 530 white filter and a 1× BODY lens barrel are applied, and a 10× objective lens is used to measure (470 μm × 353 μm) per field of view. This operation is performed for 10 points at 1 cm intervals in the flow direction from the center of the surface of the skin layer of the target sample film in both the flow direction and width direction. Next, the obtained data is subjected to noise removal processing using a median filter (3 × 3), and then Gaussian filter processing with a cutoff value of 176 μm is performed to remove waviness components. This makes it possible to properly measure the surface condition of the skin layer. Next, an analysis is performed using the "ISO parameters" in the "Bearing" plug-in function of the "VS-Viewer" analysis software of "VertScan2.0", to obtain Sq (μm), Sdr (%), Sk (μm), Spk (μm), and Svk (μm), and the average value of each value obtained at the above 10 locations is calculated.

[0062] The thickness of the skin layer can be appropriately selected depending on the application of the laminated film according to this embodiment. For example, from the viewpoint of suitably using the biaxially stretched surface film according to this embodiment as, for example, a protective film for a build-up film used in the manufacture of electronic components, the lower limit is preferably 0.05 μm or more, more preferably 0.1 μm or more, and even more preferably 1 μm or more, and the upper limit is preferably 80 μm or less, more preferably 50 μm or less, even more preferably 30 μm or less, and particularly preferably 10 μm or less. In addition, the thickness of the skin layer is preferably 0.5% or more, more preferably 1% or more, even more preferably 3% or more, even more preferably 5% or more, and especially preferably 10% or more, based on the entire thickness of the laminated film. In addition, the thickness of the skin layer is preferably 50% or less, more preferably 30% or less, even more preferably 25% or less, even more preferably 20% or less, and especially preferably 15% or less, based on the entire thickness of the biaxially stretched surface film. When a skin layer is formed on both sides of the laminated film according to this embodiment, the thickness of the skin layer on each side is preferably within the thickness range described above. In addition, when a skin layer is formed on both sides of the laminate film according to the present embodiment, the thickness of each skin layer may be the same as or different from each other. The thickness of the skin layer can be measured by cutting the laminate film and observing the cross section with a microscope.

[0063] The skin layer and the core layer each preferably have an ash content of 100 ppm or less. Ash is caused by polymerization catalyst residues and the like, and causes minute foreign matter (fish eyes). If the ash content is 100 ppm or less, preferably 50 ppm or less, it is possible to prevent fish eyes. The ash content can be adjusted by controlling the type and amount of catalyst used during polymerization of the resin that constitutes the skin layer and the core layer, respectively.

[0064] In this specification, the ash content of the skin layer and the core layer are measured in accordance with ISO3451-1 as follows: The resin forming the skin layer or the core layer is placed in a crucible, heated in a muffle furnace at 750°C for 1 hour, and the mass of the residue in the crucible is measured. The ratio of the mass of the residue in the crucible to the mass of the resin placed in the crucible is then calculated, and this is taken as the ash content.

[0065] The skin layer and the core layer may each contain an additive. The additive is not particularly limited, and known additives added to resin films can be used. The additive can be an additive generally used in polypropylene resins. Examples of additives include stabilizers such as antioxidants, chlorine absorbers, and ultraviolet absorbers, lubricants, plasticizers, flame retardants, antistatic agents, and colorants. Such additives may be added to the skin layer or the core layer to the extent that the effects of the present invention are not impaired. However, from the viewpoint of suitably using the biaxially stretched surface film according to this embodiment as a protective film for a build-up film used in the manufacture of electronic components, it is preferable not to add a component, such as an antiblocking agent, to the skin layer that may transfer to the member to be protected and affect the properties of the member to be protected.

[0066] The laminated film according to the present embodiment can be suitably used as a protective film for the pressure-sensitive adhesive layer of a build-up film used in the manufacture of electronic components, etc. The laminated film can also be used as a protective film in various fields, such as the manufacturing process of thermosetting resin members such as fiber-reinforced plastics.

[0067] The laminated film according to the present embodiment can be obtained as a film in which the core layer and the skin layer are laminated, for example, by extrusion molding a resin composition that forms the core layer and the skin layer. For example, when the laminated film is produced as a biaxially stretched laminated film, it can be produced by extrusion molding a resin composition that forms the core layer and the skin layer, by a step (i) of producing a cast raw sheet in which the core layer before stretching and the skin layer before stretching are laminated, and a step (ii) of biaxially stretching the cast raw sheet. Specific examples of the steps (i) and (ii) are shown below.

[0068] In step (i), the resin compositions forming the core layer and the skin layer are melt-kneaded at 200 to 260°C in an extruder, respectively, and then joined in a joining device and extruded from a T-die. At this time, it is preferable to remove coarse foreign matter from each resin using a polymer filter upstream of the joining device.

[0069] The joining can be performed by known methods such as a method in a pipe prior to the T-die, a method using a lamination unit provided at the resin inlet of the T-die (feed block method), a method in which the resin is laminated after being widened in the T-die (manifold lamination method), etc. Of these, the manifold lamination method is superior in terms of lamination thickness accuracy, but an appropriate method can be selected from these methods taking into consideration economic efficiency, etc.

[0070] Next, the thus extruded laminate having two or more layers is brought into close contact with at least one metal drum (cooling drum) whose drum surface is controlled at 20 to 100°C using an air knife, and formed into a sheet to obtain a cast raw sheet having a thickness of, for example, 500 to 5000 μm.

[0071] Next, in step (ii), the cast raw sheet before stretching is stretched to produce a biaxially stretched laminate film. The stretching is preferably biaxially stretched in the flow (longitudinal, also called MD) direction and the width (transverse, also called TD) direction, but may be biaxially stretched in an oblique direction as necessary.

[0072] The stretching method includes a tubular method, a tenter method, a method of stretching between rolls with a difference in peripheral speed, etc., and biaxial stretching can be performed simultaneously or sequentially. Since it is easy to obtain a biaxially stretched laminate film with no thickness unevenness and good flatness, the simultaneous biaxial stretching method by the tenter method, the sequential biaxial stretching method by the tenter method, and the sequential biaxial stretching method in which the film is stretched in the machine direction between rolls with a difference in peripheral speed and then stretched in the width direction by the tenter method are preferred.

[0073] In the sequential biaxial stretching method, for example, a cast raw sheet is first kept at a temperature of 100 to 160°C, passed between rolls with a speed difference, or introduced into a tenter, and stretched 3 to 8 times in the machine direction, and then relaxed by about 0 to 10% as necessary. Subsequently, the uniaxially stretched film is introduced into a tenter and stretched 6 to 12 times in the width direction at a temperature of 120 to 185°C, and then relaxed by about 0 to 10% as necessary, heat-set, and wound up.

[0074] In the simultaneous biaxial stretching method, the cast raw sheet is introduced into a tenter and stretched to the above-mentioned stretch ratio in the machine direction and width direction at a temperature of 120 to 185°C, and then relaxed by about 0 to 10% as necessary and heat-set. Thereafter, the ends of the obtained biaxially stretched laminate film are trimmed as necessary and then wound up.

[0075] <2. Laminate> The laminate according to the present embodiment is a laminate using the laminate film according to the present embodiment. The laminate according to the present embodiment has a configuration in which a base film, a pressure-sensitive adhesive layer, and the laminate film according to the present embodiment described above are laminated in this order.

[0076] The laminated film according to this embodiment is as described above.

[0077] In the laminate according to the present embodiment, the laminate film according to the present embodiment protects the adhesive layer formed on the base film. The materials and thicknesses of the base film and the thermosetting resin are appropriately selected according to the application of the laminate according to the present embodiment. For example, a build-up film used in the manufacture of electronic components has a laminate structure in which an adhesive layer (an uncured or semi-cured thermosetting resin such as an epoxy resin that serves as a sealant for electronic boards) and a protective film are laminated on a base film such as a polyethylene terephthalate film, and when the roll according to the present embodiment is used as a roll of a build-up film, it is preferable that the base film is a polyethylene terephthalate film and the adhesive layer is formed of an uncured or semi-cured epoxy resin.

[0078] The thickness of the base film is not particularly limited, but is, for example, about 10 to 150 μm. The thickness of the adhesive layer is not particularly limited, but is, for example, greater than or equal to the conductor thickness of the inner layer circuit board to be laminated, and is about the conductor thickness + (10 to 120) μm.

[0079] Furthermore, when the laminate film according to this embodiment is also used as a protective film in various fields such as the manufacturing process of thermosetting resin members such as fiber-reinforced plastics, it is preferable that the base film is a polyethylene terephthalate film and the adhesive layer is an uncured or semi-cured epoxy resin.

[0080] The thickness of the laminate is not particularly limited, but is, for example, about 50 to 450 μm.

[0081] <3. Roll body> The roll according to the present embodiment is a roll of a laminate using the laminate film according to the present embodiment. For example, the roll may be a roll formed by winding a build-up film including the laminate film according to the present embodiment. The laminate constituting the roll is as described in the above section <2. Laminate>, and has a configuration in which a base film, a pressure-sensitive adhesive layer, and the laminate film according to the present embodiment described above are laminated in this order, and the pressure-sensitive adhesive layer is in contact with one side of either the skin layer or the core layer of the laminate film. The laminate is in a form wound around a core.

[0082] The laminated film according to this embodiment is as described above.

[0083] In the roll according to the present embodiment, the laminated film according to the present embodiment protects the adhesive layer formed on the base film. The materials and thicknesses of the base film and the thermosetting resin are appropriately selected according to the use of the roll according to the present embodiment (specifically, the use of the above-mentioned laminate in the form of the roll). For example, a build-up film used in the manufacture of electronic components has a laminate structure in which an adhesive layer (an uncured or semi-cured thermosetting resin such as an epoxy resin that serves as a sealant for electronic boards) and a protective film are laminated on a base film such as a polyethylene terephthalate film, and when the roll according to the present embodiment is used as a roll of a build-up film, it is preferable that the base film is a polyethylene terephthalate film and the adhesive layer is formed of an uncured or semi-cured epoxy resin.

[0084] The thicknesses of the base film and the pressure-sensitive adhesive layer are as described above in the section <2. Laminate>.

[0085] Furthermore, as described above, when the laminate film according to this embodiment is also used as a protective film in various fields such as the manufacturing process of thermosetting resin members such as fiber-reinforced plastics, it is preferable that the base film is a polyethylene terephthalate film and the adhesive layer is an uncured or semi-cured epoxy resin.

[0086] The thickness of the laminate constituting the roll is as described above in the section <2. Laminate>.

[0087] The winding core is cylindrical or columnar, and the laminate is wound around the winding core in the circumferential direction.

[0088] The material of the core is not particularly limited, and examples thereof include plastics that are less prone to deformation, fiber-reinforced plastics, paper, metals (iron, SUS, aluminum, etc.), etc. Among these, fiber-reinforced plastics are preferred because they are lightweight and have high strength. Examples of fiber-reinforced plastic cores include those formed by molding carbon fiber, glass fiber, etc. into a cylindrical shape and impregnating and curing a curable resin such as an unsaturated polyester resin.

[0089] The size of the winding core can be set according to the size of the intended winding body. The outer diameter of the circular cross section of the winding core is, for example, about 50 to 200 mm, and more preferably about 80 to 100 mm. EXAMPLES

[0090] The present invention will be described in detail below with reference to examples and comparative examples. However, the present invention is not limited to the examples. In addition, unless otherwise specified, parts and % indicate "parts by mass" and "% by mass", respectively.

[0091] [Example 1] (Core layer) Only pellets of homopolypropylene (b1) (MFR at 230°C = 3.5 g / 10 min, weight average molecular weight (MW) 290,000, number average molecular weight (Mn) 64,000, molecular weight distribution (Mw / Mn) 4.5) were fed from a hopper into extruder I and melted to prepare a resin composition for forming the core layer.

[0092] (Skin layer) A propylene-based elastomer (a1) (MFR at 230°C = 6.0 g / 10 min, ethylene content 0.49 mass% (calculated from the measured ethylene content of 14.2 mol%), butene content 0.34 mass% (calculated from the measured butene content of 4.9 mol%)), an ethylene-propylene block copolymer (a2) (MFR at 230°C = 8.0 g / 10 min, ethylene content 10.27 mass% (calculated from the measured ethylene content of 16.2 mol%)), and an ethylene-propylene random copolymer (a3) ​​(MFR at 230°C = 10 g / 10 min, ethylene content 0.20 mass% (calculated from the measured ethylene content of 6.0 mol%)) were dry-blended in the compounding ratios shown in Table 1, melt-kneaded at 230°C using a kneading extruder, and pelletized. Next, the pellets were charged into an extruder II from a hopper and melted to prepare a resin composition for forming a skin layer.

[0093] [Making laminated film] The resin compositions (A) and (B) forming the skin layer and the core layer were extruded from a multi-manifold die at 230°C through a polymer filter to form a laminated film having a two-type three-layer structure of skin layer / core layer / skin layer, and the laminated film was cooled and solidified while being pressed by air pressure using an air knife onto a cooling drum whose surface temperature was adjusted to 45°C, to obtain a cast raw sheet having a thickness of 920 μm. Next, the cast raw sheet was heated to 130°C while in contact with a metal roll, and then stretched about 4.6 times in the flow direction between rolls with a difference in peripheral speed. Next, the uniaxially stretched film was introduced into a hot air oven while being clamped with a clip, preheated to 180°C, stretched about 10 times in the width direction, and then heat-set at 170°C while relaxing by about 10% in the width direction, to continuously obtain a laminated film having a thickness of about 20 μm. The thickness of the skin layer was 2.5 μm, and the thickness of the core layer was 15 μm. The ends of the obtained laminated film were trimmed, and then the laminated film was wound around a core to obtain a roll of the laminated film.

[0094] [Examples 2 to 8] In the preparation of the resin composition (A) forming the skin layer of Example 1, except that the compounding ratio shown in Table 1 was used, the same procedure as in Example 1 was carried out to obtain roll-shaped laminate films.

[0095] [Comparative Example 1] A roll-shaped laminate film was obtained in the same manner as in Example 1, except that in the preparation of the resin composition forming the skin layer of Example 1, the propylene-based elastomer (a1) used in the skin layer was replaced with low-density polyethylene to give the compounding ratio shown in Table 1.

[0096] [Comparative Example 2] A roll-shaped laminate film was obtained in the same manner as in Example 1, except that in the preparation of the resin composition forming the skin layer in Example 1, the propylene-based elastomer (a1) and the ethylene-propylene random copolymer (a3) ​​used in the skin layer were not used, and the entire resin composition was replaced with the ethylene-propylene block copolymer (a2) in the blending ratio shown in Table 1.

[0097] [Comparative Example 3] A roll-shaped laminate film was obtained in the same manner as in Example 1, except that in the preparation of the resin composition forming the skin layer in Example 1, the propylene-based elastomer (a1) used in the skin layer was not used and was replaced with an ethylene-propylene block copolymer (a2) and an ethylene-propylene random copolymer (a3) ​​in the blending ratio shown in Table 1.

[0098] [Comparative Example 4] A roll-shaped laminate film was obtained in the same manner as in Example 1, except that in the preparation of the resin composition forming the skin layer in Example 1, the propylene-based elastomer (a1), the ethylene-propylene block copolymer (a2), and the ethylene-propylene random copolymer (a3) ​​used in the skin layer were not used, and the entire resin composition was replaced with homopolypropylene (b1) (MFR at 230°C = 3.5 g / 10 min) in the blending ratio shown in Table 1.

[0099] [Preparation of single-skin layer cast raw sheet] The resin composition (A) forming each skin layer in each of the Examples and Comparative Examples was extruded from a multi-manifold die at 230° C. through a polymer filter to form a single-film cast raw sheet consisting of only the skin layer, and the sheet was cooled and solidified while being pressed by air pressure using an air knife onto a cooling drum whose surface temperature was adjusted to 45° C., to obtain a cast raw sheet having a thickness of 150 μm. The cast raw sheet was used for measuring the loss tangent tanδ described later.

[0100] [Measurement of molecular weight and molecular weight distribution] The weight average molecular weight, number average molecular weight, and molecular weight distribution of homopolypropylene were measured by size exclusion chromatography (SEC), and the detailed measurement conditions were as follows. Apparatus: HLC-8321GPC / HT (detector: differential refractometer (RI)) (manufactured by Tosoh Corporation) Column: TSKgel guard column HHR(30)HT(7.5mmI.D.×7.5cm)×1 + TSKgel GMHHR-H(20)HT(7.8mmI.D.×30cm)×3 (Tosoh Corporation) Eluent: 1,2,4-trichlorobenzene (Fujifilm Wako Pure Chemical GPC grade) + BHT (0.05%) Flow rate: 1.0mL / min Detection condition: polarity-(-) Injection volume: 0.3mL Column temperature: 140℃ System temperature: 40℃ Sample concentration: 1mg / mL Sample pretreatment: The sample was weighed, and dissolved in a solvent (1,2,4-trichlorobenzene with 0.1% BHT) at 140°C for 1 hour by shaking. It was then heated and filtered through a 0.5μm sintered filter. Calibration curve: A calibration curve of a quintic approximation curve was created using standard polystyrene from Tosoh Corporation. However, the molecular weight was converted to the molecular weight of polypropylene using the Q-factor. From the calibration curve and SEC chromatogram obtained, the number average molecular weight (Mn), weight average molecular weight (Mw), and Z average molecular weight (Mz) were obtained using the analysis software for the measurement device. The molecular weight distribution (Mw / Mn) was obtained using the values ​​of Mw and Mn. The molecular weight distribution (Mz / Mn) was also obtained using the values ​​of Mz and Mn.

[0101] [loss tangent tanδ] The dynamic viscoelasticity measuring device used was a "Viscoelasticity measuring device (model: DMS6100)" manufactured by Seiko Instruments Inc. As a measurement sample, a skin layer single-film cast raw sheet made of composition (A) was cut into a strip of 40 mm in the vertical direction and 8 mm in the horizontal direction, and the temperature dependency of the cast raw sheet was measured under the measurement conditions shown below in accordance with JIS-K7244 (1999 edition). Test mode: Tensile mode Chuck distance: 20mm Vibration frequency: 1Hz Distortion amplitude: 10μm Tension Gain: 1.2 Initial force amplitude: 100mN Temperature range: -60~150℃ Heating rate: 5℃ / min Measurement atmosphere: Nitrogen Measurement thickness: The sheet thickness in [Preparation of skin layer single-film cast raw sheet] above was used. From the measurement results, the loss tangent tan δ with a temperature dispersion of 20° C. was calculated. The results are shown in Table 1.

[0102] [Surface roughness] A "VertScan2.0 (model: R5500GML)" manufactured by Ryoka Systems Co., Ltd. was used as an optical interference type non-contact surface shape measuring instrument. As a measurement sample, each laminated film of the examples and comparative examples was cut into an arbitrary size of about 20 cm square, and in a state where wrinkles were sufficiently stretched so that they were no longer wrinkled, they were set on the measurement stage using an electrostatic contact plate or the like. First, the measurement was performed using WAVE mode, a 530white filter and a 1×BODY lens barrel were applied, and a measurement was performed per field of view (470 μm × 353 μm) using a 10x objective lens. This operation was performed for 10 points at 1 cm intervals in the flow direction from the center of the surface of the skin layer of the target sample film in both the flow direction and width direction. Next, the obtained data was subjected to noise removal processing using a median filter (3 × 3), and then Gaussian filter processing with a cutoff value of 176 μm was performed to remove the waviness components. This made it possible to properly measure the surface condition of the skin layer. Next, an analysis was performed using the "ISO parameters" in the "Bearing" plug-in function of the "VS-Viewer" analysis software for "VertScan2.0," and Sq (μm), Sdr (%), Sk (μm), Spk (μm), and Svk (μm) were obtained, and the average values ​​obtained at the above 10 points were calculated. The results are shown in Table 1.

[0103] [Frictional force] The surface property measuring device used was a "HEIDON Tribogear (model: TYPE14FW)" manufactured by Shinto Scientific Co., Ltd. Each laminate film of the Examples and Comparative Examples was cut into a length of 20 cm in the vertical direction and 3 cm in the horizontal direction to prepare a test film. Next, the test film was pressed against a 30 mm flat indenter (contact area 9 cm2) without any wrinkles. 2) in which the skin layer of the test film was set on the outside. Next, a biaxially oriented polyester film (arithmetic mean height (Sa) 0.001 μm, root mean square height (Sq) 0.001 μm, root mean square slope (Sdq) 0.001, interface area development ratio (Sdr) 0.000%, core level difference (Sk) 0.002 μm, protruding valley height (Svk) 0.001 μm, protruding valley space volume (Vvv) 0.000 ml / m) used for measuring the frictional force of the skin layer was 2 , Core space volume (Vvc) 0.001 ml / m 2 , core volume (Vmc) 0.001ml / m 2 A piece of aluminum foil (maximum height (Sz) 0.08 μm, thickness 50 μm) was cut into a length of 20 cm and a width of 8 cm, and placed on a movable table without any wrinkles, with the untreated side that had not been subjected to surface modification treatment such as corona discharge facing up.

[0104] In this state, the surface of the skin layer of the test film is overlapped with the biaxially oriented polyester film and measured. The strength is 5.56 gf / cm 2 The coefficient of dynamic friction D1 under pressure is calculated using a table speed of 100 mm / min and a vertical load of 50 gf (equivalent to 5.56 gf / cm 2 ), displacement of 60 mm or more (one-way movement), data sampling speed every 50 ms, measurement temperature 23°C, measurement humidity 50% RH. The dynamic friction coefficient D1 (average value for displacements of 1 to 60 mm) was extracted from the values ​​obtained from each measurement, three times. The results are shown in Table 1.

[0105] In addition, the surface of the skin layer of the test film was overlapped with a biaxially stretched polyester film and measured, and the strength was 33.33 gf / cm 2 The dynamic friction force D2 under pressure is calculated as follows: table speed 100 mm / min, vertical load 300 gf (pressure conversion value 33.33 gf / cm 2 ), displacement of 60 mm or more (one-way movement), data sampling speed every 50 ms, measurement temperature 23°C, measurement humidity 50% RH. The kinetic friction force D2 (average value between displacements of 1 to 60 mm) was extracted from the values ​​obtained from each of the three measurements. The results are shown in Table 1.

[0106] [Evaluation of winding misalignment of rolled bodies] A base film having an adhesive layer (580 mm wide x 300 m, non-silicone PET separator film, adhesive layer: epoxy adhesive (thermosetting resin)) was prepared. The base film and each laminate film prepared in the examples and comparative examples (slit to 580 mm wide) were laminated together so that the skin layer of the laminate film and the adhesive layer of the base film were in contact with each other to prepare a laminate, which was used as an evaluation sample. The evaluation sample was wound around a core (length 620 mm, diameter 92.5 mm) at a speed of 50 m / min to form a roll. Next, the roll was packed in a cardboard box, and after a vibration test (level 3) according to the method specified in JIS-Z0232, the unevenness of the film roll end surface was evaluated in four stages: "excellent: A+", "good: A", "average: B" and "poor: C", and evaluation was performed according to the following criteria, with "average: B" or higher being considered as passing. The results are shown in Table 1. A+: The unevenness of the film roll edge is 0 mm to 1.0 mm. A: The unevenness of the film roll edge is more than 1.0 mm and less than 3.0 mm B: The unevenness of the film roll edge is more than 3.0 mm and less than 5.0 mm C: The unevenness of the film roll edge exceeds 5.0 mm

[0107] [Roll dirt evaluation] The ethylene component stains on the roll surfaces were evaluated by cleaning the longitudinal stretching rolls before the start of film production, and visually observing the stains one hour after the start of film production. The condition difference of the longitudinal stretching roll surfaces was evaluated on a four-level scale of "excellent: A+", "good: A", "fair: B", and "poor: C", with "fair: B" or higher being considered a pass, and the evaluation was based on the following criteria. The results are shown in Table 1. A+: Same as before film formation A: Almost no dirt B: Very slight stains can be seen C: Cloudy white stains are clearly visible

[0108] [Table 1]

Claims

1. A core layer made of a composition (B) containing homopolypropylene (b1); a skin layer formed on at least one side of the core layer and made of a composition (A) containing a propylene-based elastomer (a1), an ethylene-propylene block copolymer (a2), and an ethylene-propylene random copolymer (a3); Equipped with The composition (A) has a loss tangent tanδ of 0.06 or more at a vibration frequency of 1 Hz and a temperature of 20° C., The composition (A) has a total content of ethylene and butene of 8.0 mass% or more.

2. The laminate film according to claim 1 , wherein the composition (A) has an ethylene content of 35.0 mass % or less.

3. 3. The laminate film according to claim 1, wherein the composition (A) has a content of the propylene-based elastomer (a1) of 5 to 65 parts by mass, a content of the ethylene-propylene block copolymer (a2) of 30 to 90 parts by mass, and a content of the ethylene-propylene random copolymer (a3) ​​of 5 to 65 parts by mass.

4. The laminate film according to any one of claims 1 to 3, which is used as a protective film for a pressure-sensitive adhesive layer of a build-up film.

5. A roll comprising a build-up film including the laminate film according to any one of claims 1 to 3 wound up.

Citation Information

Patent Citations

  • Polyolefin resin film

    EP3730541A1

  • Biaxially oriented film

    JP2015186907A

  • Surface protective film

    JP2018145365A

  • Multilayer film and articles made from the same

    JP2018532616A

  • Laminate film

    JP2022077360A