Multilayer ceramic capacitor

A two-layer side margin structure with varying compositions and densities in the multilayer ceramic capacitors addresses void-related moisture infiltration issues, improving reliability by promoting denser sintering.

JP2024149822AActive Publication Date: 2024-10-18MURATA MFG CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024137787
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2014-05-21
Filing Date
2024-08-19
Publication Date
2024-10-18
Estimated Expiration
2035-04-01

AI Technical Summary

Technical Problem

The existing manufacturing method for multilayer ceramic capacitors results in increased voids in the side margins during firing, leading to moisture infiltration and reduced reliability.

Method used

A multilayer ceramic capacitor design with a two-layer side margin structure, where the inner and outer parts of the side margin have different compositions and densities, reducing voids and preventing moisture intrusion.

Benefits of technology

The design effectively suppresses moisture infiltration, enhancing the reliability of the multilayer ceramic capacitors by promoting denser sintering and reducing voids in the side margin portions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149822000001_ABST
    Figure 2024149822000001_ABST
Patent Text Reader

Abstract

To provide a multilayer ceramic capacitor with improved reliability by preventing moisture from penetrating into the ceramic body.SOLUTION: A multilayer ceramic capacitor 10 includes a rectangular parallelepiped ceramic body 12 and external electrodes 40, 42 arranged on the ceramic body 12. The ceramic body 12 includes an inner layer portion 26 including internal electrodes 22, 24, outer layer portions 28, 30 arranged to sandwich the inner layer portion 26 in the stacking direction, and side margin portions 32, 34 arranged to sandwich the inner layer portion 26 and the outer layer portions 28, 30 in the width direction, with the amount of voids decreasing from the inside to the outside of the side margin portions 32, 34.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a multilayer ceramic capacitor. [Background technology]

[0002] In recent years, there has been a demand for large-capacity, yet compact, multilayer ceramic capacitors. Such multilayer ceramic capacitors have, for example, a ceramic body formed in a rectangular parallelepiped shape in which inner ceramic layers (dielectric ceramic layers) and internal electrodes are alternately stacked, with outer ceramic layers provided on the upper and lower surfaces of the stack, and external electrodes are formed on both end surfaces of the ceramic body. Side margins are formed on both side surfaces of the ceramic body to prevent connection with the external electrodes.

[0003] As a method for manufacturing the multilayer ceramic capacitor as described above, a manufacturing method described in Patent Document 1 is disclosed. That is, in this method for manufacturing a multilayer ceramic capacitor, a mother laminate is formed by stacking a plurality of ceramic green sheets on the surfaces of which conductive films that become internal electrodes are formed, and the mother laminate is cut so that the conductive films are exposed on the side surfaces on which external electrodes are not formed. Then, ceramic slurry that becomes side margin portions is applied to both side surfaces to form uniform side margin portions with little variation. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 61-248413 Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the method for manufacturing a multilayer ceramic capacitor described in Patent Document 1, the ceramic slurry used to form the side margin portion is composed of the same dielectric ceramic material as the ceramic slurry used to form the ceramic layers for the inner layers. In the firing step of this method for manufacturing a multilayer ceramic capacitor, when firing is performed under conditions for forming the ceramic layers for the inner layers, voids increase inside the side margin portion, and it is not possible to prevent moisture from entering from the side margin portion through the voids, resulting in a problem of reduced reliability of the multilayer ceramic capacitor.

[0006] SUMMARY OF THE PRESENT DISCLOSURE OF THE PRESENT DISCLOSURE OBJECTS AND SUMMARY OF THE PRESENT DISCLOSURE OBJECTS OF THE PRESENT DISCLOSURE SUMMARY ... [Means for solving the problem]

[0007] The multilayer ceramic capacitor according to the present invention is a multilayer ceramic capacitor comprising a rectangular ceramic body and external electrodes arranged on the ceramic body, wherein the ceramic body has an inner layer portion including an internal electrode, an outer layer portion arranged so as to sandwich the inner layer portion in the stacking direction, and a side margin portion arranged so as to sandwich the inner layer portion and the outer layer portion in the width direction, and the amount of voids decreases from the inside to the outside of the side margin portion.

[0008] The multilayer ceramic capacitor according to the present invention has a side margin portion which is an area where no internal electrodes are present, and the side margin portion has fewer voids from its inside to its outside. This makes it possible to suppress the intrusion of moisture from the side margin portion toward the inside of the ceramic body, thereby providing a multilayer ceramic capacitor with improved reliability. Effect of the Invention

[0009] According to the present invention, it is possible to provide a multilayer ceramic capacitor with improved reliability by suppressing the infiltration of moisture toward the inside of the ceramic body.

[0010] The above and other objects, features and advantages of the present invention will become more apparent from the following detailed description of the preferred embodiments of the present invention, which proceeds with reference to the accompanying drawings. [Brief description of the drawings]

[0011] [Figure 1] 1 is a schematic perspective view showing an example of the appearance of a multilayer ceramic capacitor according to the present invention; [Diagram 2] FIG. 2 is a cross-sectional diagram showing a cross section taken along line AA in FIG. [Diagram 3] FIG. 2 is a cross-sectional diagram showing a cross section taken along line BB in FIG. [Figure 4] FIG. 1 is an explanatory diagram for explaining a method for manufacturing a multilayer ceramic capacitor, in which (a) is a perspective view that shows a state in which a conductive film is formed on a ceramic green sheet, and (b) is a perspective view that shows a state in which the ceramic green sheets on which the conductive film is formed are stacked. [Diagram 5] 5 is a schematic perspective view showing an example of the appearance of a laminate chip manufactured by the method for manufacturing the multilayer ceramic capacitor shown in FIG. 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] An example of a multilayer ceramic capacitor according to the present invention will be described. Fig. 1 shows a schematic perspective view of a multilayer ceramic capacitor, which is an example of the appearance of a multilayer ceramic capacitor composed of a ceramic body and external electrodes, and Fig. 2 shows a cross-sectional diagram showing a cross section taken along line AA in Fig. 1. Also, Fig. 3 shows a cross-sectional diagram showing a cross section taken along line BB in Fig. 1.

[0013] The multilayer ceramic capacitor 10 according to this embodiment is generally composed of a ceramic body 12 and external electrodes 40, 42 formed on both end surfaces of the ceramic body 12, respectively.

[0014] The size of the multilayer ceramic capacitor 10 according to the present invention has combinations of dimensions in the length (L) direction, width (W) direction, and lamination (T) direction, such as 1.6 mm × 0.8 mm × 0.8 mm, 1.0 mm × 0.5 mm × 0.5 mm, 0.6 mm × 0.3 mm × 0.3 mm, and 0.4 mm × 0.2 mm × 0.2 mm.

[0015] The ceramic body 12 is formed in a rectangular parallelepiped shape, and has a first end face 13 and a second end face 14 extending along the width (W) direction and the stacking (T) direction, a first side face 15 and a second side face 16 extending along the length (L) direction and the stacking (T) direction, and a first main face 17 and a second main face 18 extending along the length (L) direction and the width (W) direction. In the ceramic body 12, the first end face 13 and the second end face 14 face each other, the first side face 15 and the second side face 16 face each other, and the first main face 17 and the second main face 18 face each other. The first side face 15 and the second side face 16 are perpendicular to the first end face 13 and the second end face 14, and the first main face 17 and the second main face 18 are perpendicular to the first end face 13 and the first side face 16. Furthermore, the corners and edges of the ceramic body 12 are preferably rounded.

[0016] The ceramic body 12 is composed of an inner layer portion 26 composed of a plurality of inner layer ceramic layers (dielectric ceramic layers) 20 and a plurality of first inner electrodes 22 and second inner electrodes 24 disposed at the interfaces between the plurality of inner layer ceramic layers 20, outer layer portions 28, 30 in which outer layer ceramic layers are disposed so as to sandwich the inner layer portion 26 in the stacking (T) direction, and side margin portions 32, 34 in which side margin ceramic layers are disposed so as to sandwich the inner layer portion 26 and the outer layer portions 28, 30 in the width (W) direction. In other words, the inner layer portion 26 is a region sandwiched between the first and second inner electrodes 22, 24 disposed closest to the first main surface 17 or the second main surface 18. The side margin portions 32, 34 are regions in which the first inner electrode 22 and the second inner electrode 24 are not present when the ceramic body 12 is viewed from the stacking (T) direction.

[0017] The ceramic layer 20 for the inner layer is composed of dielectric ceramic particles having a perovskite structure, the main component of which is a perovskite type compound containing Ba and Ti. At least one of Si, Mg, and Ba is added as an additive to the main component, and the additive exists between the ceramic particles. The thickness of the ceramic layer 20 for the inner layer after firing is preferably 0.3 μm or more and 10 μm or less.

[0018] The upper and lower outer layer portions 28, 30 are each made of the same dielectric ceramic material as the inner ceramic layer 20. The outer layer portions 28, 30 may be made of a dielectric ceramic material different from that of the inner ceramic layer 20. The thickness of the outer layer portions 28, 30 after firing is preferably 15 μm or more and 40 μm or less.

[0019] The first internal electrode 22 and the second internal electrode 24 face each other in the thickness direction via the inner-layer ceramic layer 20. A capacitance is formed at a portion where the first internal electrode 22 and the second internal electrode 24 face each other via the inner-layer ceramic layer 20.

[0020] A left end of the first internal electrode 22 is extended to a first end face 13 of the ceramic body 12 and electrically connected to an external electrode 40. A right end of the second internal electrode 24 is extended to a second end face 14 of the ceramic body 12 and electrically connected to an external electrode 42.

[0021] The first and second internal electrodes 22, 24 are made of, for example, Ni, Cu, etc. The thickness of the first and second internal electrodes 22, 24 is preferably 0.3 μm or more and 2.0 μm or less.

[0022] The side margins 32, 34 have a two-layer structure including outer parts 32a, 34a located on the side of the ceramic body 12 and inner parts 32b, 34b located on the first and second internal electrodes 22, 24 side. The side margins 32, 34 are made of a dielectric ceramic material having a perovskite structure mainly composed of BaTiO3 or the like. At least one of Si, Mg, and Ba is added as an additive to the main components, and the additive exists between the ceramic particles. The thickness of the side margins 32, 34 after firing is preferably 5 μm or more and 40 μm or less. The present invention is particularly effective when the thickness is 20 μm or less. Preferably, the inner parts 32b, 34b are thinner than the outer parts 32a, 34a. Specifically, the thickness of the outer parts 32a, 34a is preferably 5 μm or more and 20 μm or less, and the thickness of the inner parts 32b, 34b is preferably 0.1 μm or more and 20 μm or less. Due to the difference in sintering properties between the outer parts 32a, 34a and the inner parts 32b, 34b, it is easy to see that the side margin parts 32, 34 have a two-layer structure by using an optical microscope. The side margin parts 32, 34 may be multiple layers, not just two layers of the outer parts 32a, 34a and the inner parts 32b, 34b.

[0023] The thickness of the outer layers 28, 30 or the thickness of the side margin portions 32, 34 are determined by polishing the ceramic body 12 so that its length is reduced to approximately half in a direction perpendicular to the plane formed by the stacking (T) direction and width (W) direction, and measuring the length from the end of the internal electrode (including the end where the ceramic dielectric is diffused) toward the outside for every 10th layer, and averaging the measurements.

[0024] In the side margins 32, 34, the gap decreases from the inner portion 32b toward the outer portion 32a and from the inner portion 34b toward the outer portion 34a.

[0025] In this way, when sintering the laminate chip having the side margins 32, 34 formed therein, even under conditions for sintering the inner layer portion in which the internal electrodes are provided in the ceramic body 12, the amount of voids can be reduced from the inside to the outside of the side margins 32, 34, and therefore the infiltration of moisture from the side margins 32, 34 toward the inside of the ceramic body 12 is suppressed, thereby improving the moisture resistance of the laminated ceramic capacitor. Therefore, a laminated ceramic capacitor with improved reliability can be provided.

[0026] Here, voids refer to spaces or spaces that are mixed with glass-filled areas. The number of voids can be confirmed by counting voids by imaging an area of ​​30 μm × 30 μm with a SEM at a magnification of 5000.

[0027] Moreover, the grain size, which is the particle size of the ceramic particles in the inner parts 32b, 34b of the side margin parts 32, 34, is smaller than the grain size in the outer parts 32a, 34a, and the density is increased. In particular, the grain size at the ends of the first and second internal electrodes 22, 24 near the side margin parts 32, 34 is smaller than the grain size in the outer parts 32a, 34a.

[0028] This void can be observed by polishing the ceramic body 12 in the same manner as when measuring the thickness of the side margin portions 32, 34, and then taking an SEM photograph at a magnification of 5000 times when the external dimensions of the multilayer ceramic capacitor 10 are, for example, 0.6 mm × 0.3 mm × 0.3 mm, and counting the points that appear to be voids.

[0029] In addition, by taking SEM images at magnifications of 20,000 to 50,000 times, selecting grains within the imaging range, and calculating the average size (for example, 50 grains), it is possible to grasp the difference in grain size between the outer portions 32a, 34a and the inner portions 32b, 34b.

[0030] The amount of Ba, which is an additive between the ceramic particles of the inner layer 20 of the inner layer portion 26 and the outer portions 32a, 34a and the inner portions 32b, 34b of the side margin portions 32, 34, is The inner layer ceramic layer 20 of the inner layer portion 20<the outer portions 32a, 34a<the inner portions 32b, 34b, It is.

[0031] In this way, it is preferable that the side margin portion is formed in two layers, an inner portion on the internal electrode side and an outer portion on the side surface side, and the Ba content of the inner portion is greater than the Ba content of the outer portion, thereby improving the reliability of the multilayer ceramic capacitor having the side margin portion.

[0032] That is, the Ba content between ceramic particles made of the ceramic dielectric decreases from the inside to the outside of the side margin portion of the ceramic body 12. Therefore, when sintering a laminated chip having side margin portions 32, 34 formed therein, even under conditions for sintering an inner layer portion in which internal electrodes are provided in the ceramic body 12, grain growth of the dielectric ceramic particles in the region outside the side margin portions 32, 34 can be promoted, allowing for denser sintering. This reduces voids in the dielectric ceramic layer constituting the outside of the side margin portions, thereby preventing moisture from penetrating from the side margin portions 32, 34 toward the inside of the ceramic body 12.

[0033] The content of Ba, which is an additive, differs between the ceramic particles in the side margin portions 32 and 34. The difference in the Ba content can be found by TEM analysis.

[0034] The content of Ba in the outer portion 32a, 34a and the inner portion 32b, 34b of the side margin portion 32, 34 is, in terms of a molar ratio to Ti:1 mol, at the center value, The outer portions 32a and 34a have a Ba of greater than 1.000 and less than 1.020. The inner portions 32b and 34b have a Ba of greater than 1.020 and less than 1.040. In this way, the reliability of the multilayer ceramic capacitor having the side margin portion can be improved.

[0035] In addition, by polishing the ceramic body 12 from the side margin portions 32, 34, and dissolving the powders obtained by polishing the outer portions 32a, 34a and the inner portions 32b, 34b in acid and performing ICP emission spectroscopy analysis, it is possible to confirm that the above-mentioned molar ratios are achieved in the outer portions 32a, 34a and the inner portions 32b, 34b.

[0036] Furthermore, within these ranges, it is preferable that the Ba content between the ceramic particles of the inner parts 32b, 34b is more than 100% and less than 140% more than that of the outer parts 32a, 34a. This can improve the reliability of the multilayer ceramic capacitor having side margins.

[0037] The external electrodes 40, 42 have a triple structure consisting of an electrode layer 40a, 42a containing Cu formed by baking, a first plating layer 40b, 42b containing Ni formed on the surface of the electrode layer 40a, 42a to prevent solder erosion, and a second plating layer 40c, 42c containing Sn formed on the surface of the first plating layer 40b, 42b.

[0038] 1, the number of voids decreases from the inside to the outside of the side margin portions 32, 34. That is, in the multilayer ceramic capacitor shown in Fig. 1, the number of voids is smaller in the outer portions 32a, 34a than in the inner portions 32b, 34b of the side margin portions 32, 34. This suppresses the intrusion of moisture from the side margin portions 32, 34 toward the inside of the ceramic body 12 via the voids, thereby improving the moisture resistance of the multilayer ceramic capacitor 10.

[0039] 1, Ba between the ceramic particles decreases from the inner parts 32b, 34b of the side margin parts 32, 34 toward the outer parts 32a, 34a (i.e., from the inside to the outside of the side margin parts 32, 34). Ba diffuses from the inner parts 32b, 34b to the inner layer ceramic layer 20 between the inner parts 32b, 34b and the ends of the first and second internal electrodes 22, 24, so that the amount of Ba increases near the side margin parts 32, 34 of the first and second internal electrodes 22, 24. Therefore, grain growth of the ceramic particles at the ends of the first and second internal electrodes 22, 24 can be suppressed, and reliability between the internal electrodes can be improved.

[0040] 1, the outer portions 32a, 34a of the side margin portions 32, 34 have a small amount of Ba, which promotes grain growth of the ceramic particles and allows for denser sintering, thereby improving resistance to moisture penetration from the outside.

[0041] Next, a method for manufacturing a multilayer ceramic capacitor will be described. Fig. 4 is an explanatory diagram for explaining the method for manufacturing a multilayer ceramic capacitor, where (a) is a perspective view showing a state in which a conductive film is formed on a ceramic green sheet, and (b) is a perspective view showing a state in which the ceramic green sheets on which the conductive film is formed are stacked. Fig. 5 is a schematic perspective view showing an example of an overview of a laminate chip manufactured by the method for manufacturing a multilayer ceramic capacitor shown in Fig. 4. The method will be described in detail below.

[0042] (1) Formation of ceramic body First, a perovskite compound containing Ba and Ti is prepared as a dielectric ceramic material. Dielectric powder obtained from this dielectric ceramic material is mixed with additives such as at least one of Si, Mg, and Ba, an organic binder, an organic solvent, a plasticizer, and a dispersant in a predetermined ratio to prepare a ceramic slurry. This ceramic slurry is molded into a plurality of ceramic green sheets 50a (50b) on a resin film (not shown). The ceramic green sheets 50a (50b) are molded using, for example, a die coater, a gravure coater, a microgravure coater, or the like.

[0043] Next, as shown in Fig. 4(a), the conductive paste for the internal electrodes is printed in stripes in the X direction on the surface of the ceramic green sheet 50a (50b) and dried to form the conductive film 52a (52b) that will become the internal electrode 22 (24). Various printing methods can be used, such as screen printing, inkjet printing, and gravure printing. The thickness of the conductive film 52a (52b) is preferably 1.5 µm or less.

[0044] 4(b), the plurality of ceramic green sheets 50a, 50b on which the conductive films 52a, 52b are printed are shifted in a direction (Y direction: width direction of the conductive films 52a, 52b) perpendicular to the printing direction (X direction) of the conductive films 52a, 52b and stacked. Furthermore, a predetermined number of ceramic green sheets on which no conductive film is formed and which will become the outer layer portions 28, 30 are stacked as necessary on the upper and lower surfaces of the ceramic green sheets 50a, 50b which will become the inner layer portion 26 stacked in this manner, to obtain a mother laminate.

[0045] Next, the mother laminate obtained is pressed. The method for pressing the mother laminate may be a rigid press, a hydrostatic press, or the like.

[0046] The pressed mother laminate is then cut into a chip shape to obtain a laminate chip 60 as shown in Fig. 5. The mother laminate can be cut by various methods such as press cutting, dicing, laser cutting, etc.

[0047] By going through the above steps, one end face of the laminate chip 60 has only the conductive film 52a of the ceramic green sheet 50a exposed, and the other end face has only the conductive film 52b of the ceramic green sheet 50b exposed.

[0048] Moreover, on both side surfaces of the laminate chip 60, the conductive film 52a of the ceramic green sheet 50a and the conductive film 52b of the ceramic green sheet 50b are exposed.

[0049] (2) Formation of side margins Next, ceramic green sheets for side margins are prepared, which will become the side margins 32 and 34. This will be described in more detail below.

[0050] First, a perovskite compound containing Ba and Ti is prepared as a dielectric ceramic material. Dielectric powder obtained from this dielectric ceramic material is mixed with at least one of Si, Mg, and Ba as additives, a binder resin, an organic solvent, a plasticizer, and a dispersant in a predetermined ratio to prepare a ceramic slurry.

[0051] Here, the ceramic slurry that becomes the outer parts 32a, 34a of the side margin parts 32, 34 is adjusted to have a molar ratio of Ba greater than 1.000 and less than 1.020 per mol of Ti. Also, the ceramic slurry that becomes the inner parts 32b, 34b of the side margin parts 32, 34 is adjusted to have a molar ratio of Ba greater than 1.020 and less than 1.040 per mol of Ti.

[0052] In addition, the amount of polyvinyl chloride (PVC) contained in the ceramic slurry that will become the outer portions 32a, 34a of the side margin portions 32, 34 is greater than the amount of polyvinyl chloride (PVC) contained in the ceramic slurry that will become the inner portions 32b, 34b of the side margin portions 32, 34.

[0053] Furthermore, the solvent contained in the ceramic slurry that will become the inner parts 32b, 34b of the side margin parts 32, 34 is appropriately selected to prevent sheet attack on the ceramic green sheets for the outer part. The ceramic green sheets for the inner part also have the role of adhering to the laminate chip 60.

[0054] Then, the prepared ceramic slurry that will become the outer portions 32a, 34a of the side margin portions 32, 34 is applied onto the resin film and dried to prepare ceramic green sheets for the outer portions.

[0055] Next, the ceramic slurry that will become the inner parts 32b, 34b of the side margin parts 32, 34 is applied to the surface of the ceramic green sheet for the outer part and dried to form a ceramic green sheet for the inner part, resulting in the production of a two-layer ceramic green sheet for the side margin.

[0056] Here, the thickness of the ceramic green sheets for the inner portion is formed to be thinner than that of the ceramic green sheets for the outer portion. For example, the thickness of the ceramic green sheets for the outer portion is formed to be 5 μm or more and 20 μm or less after firing, and the thickness of the ceramic green sheets for the inner portion is formed to be 0.1 μm or more and 20 μm or less after firing. It is preferable that the ceramic green sheets for the outer portion are thicker than the ceramic green sheets for the inner portion. In addition, an interface exists between the outer portions 32a, 34a and the inner portions 32b, 34b, and this interface can relieve the stress applied to the multilayer ceramic capacitor 10.

[0057] The above-mentioned two-layered ceramic green sheet for the side margin was produced by printing the ceramic green sheet for the inner part on the surface of the ceramic green sheet for the outer part, but the ceramic green sheet for the outer part and the ceramic green sheet for the inner part may be formed in advance and then bonded together to produce the ceramic green sheet for the side margin having a two-layered structure.

[0058] Next, the side margin ceramic green sheets are peeled off from the resin film.

[0059] Next, one side surface or the other side surface of the laminate chip 60 where the conductive films 52a, 52b are exposed is pressed against the inner portion ceramic green sheet of the peeled side margin ceramic green sheet, and punched out to form layers that will become the side margin portions 32, 34. At this time, it is preferable to apply an organic solvent that will serve as an adhesive to the side surface of the laminate chip 60 in advance.

[0060] Next, the laminate chip 60, on which the layers that will become the side margin portions 32, 34 are formed, is degreased under specified conditions in a nitrogen atmosphere, and then fired at a specified temperature in a nitrogen-hydrogen-water vapor mixed atmosphere to form a sintered ceramic body 12.

[0061] Next, an external electrode paste mainly composed of Cu is applied to both ends of the sintered ceramic body 12 and baked to form electrode layers 40a, 42a electrically connected to the first and second internal electrodes 22, 24. Furthermore, first plating layers 40b, 42b are formed by Ni plating on the surfaces of the electrode layers 40a, 42a, and second plating layers 40c, 42c are formed by Sn plating on the surfaces of the first plating layers 40b, 42b, to form the external electrodes 40, 42.

[0062] In the manner described above, the multilayer ceramic capacitor 10 shown in FIG. 1 is manufactured.

[0063] The side margins 32, 34 can also be formed by applying a ceramic slurry for the side margins to both side surfaces of the laminate chip 60 where the conductive films 52a, 52b are exposed.

[0064] That is, ceramic slurry that will become the inner portions 32b, 34b is applied to both side surfaces of the laminate chip 60 where the conductive films 52a, 52b are exposed, and then dried, and ceramic slurry that will become the outer portions 32a, 34a is further applied thereto.

[0065] In this case, the thickness of the ceramic slurry that will become the inner portions 32b, 34b or the thickness of the ceramic slurry that will become the outer portions 32a, 34a can be adjusted by adjusting the amount of resin contained in each ceramic slurry.

[0066] The side margins 32, 34 may be formed by masking both end faces of the laminate chip 60 with resin or the like, dipping the entire laminate chip 60 into a ceramic slurry that will become the inner parts 32b, 34b, drying it, and then dipping it further into a ceramic slurry that will become the outer parts 32a, 34a. In this case, the side margins 32, 34 are formed in a two-layer structure so as to cover the outer layer parts 28, 30 as well.

[0067] (Experimental Example) 1. Examples and Comparative Examples In the experimental examples, samples of multilayer ceramic capacitors of the following examples and comparative examples were manufactured and evaluated by a humidity load test.

[0068] (Example) In the embodiment, the multilayer ceramic capacitor 10 shown in FIG. 1 was manufactured by the above-mentioned method. In this case, the outer dimensions of the multilayer ceramic capacitor 10 were 0.6 mm in length, 0.3 mm in width, and 0.3 mm in height. In the embodiment, the molar ratio of Ba to Ti:1 mol in the side margin portions 32 and 34 was 1.020 for the outer portions 32a and 34a, and 1.028 for the inner portions 32b and 34b. The thickness of the side margin portions 32 and 34 was 20 μm, the thickness of the outer portions 32a and 34a was 16 μm, and the thickness of the inner portions 32b and 34b was 4 μm. The thickness of the inner ceramic layer 20 was 0.83 μm per layer, the thickness of the first and second internal electrodes 22 and 24 per layer was 0.40 μm, and the thickness of the outer layer portion 28 and the outer layer portion 30 was 25 μm, respectively. The thickness values ​​are all values ​​after firing. The number of laminated inner ceramic layers 20 was 280.

[0069] (Comparative Example) In the comparative example, a multilayer ceramic capacitor was manufactured under the same conditions as in the example, except that the molar ratio of Ba to Ti:1 mol was uniformly set to 1.020 for the additive Ba in the side margin portion.

[0070] (Moisture resistance load test) A humidity load test was carried out on each sample of the examples and comparative examples. The humidity load test was carried out under conditions of a relative humidity of 95%, a temperature of 40°C, and a rated voltage of 6.3 V. The insulation resistance value of each sample was measured, and a value of 1.0×10 6 When the insulation resistance deteriorated within 100 [Ω], the sample was judged to be defective. For this humidity load test, 36 samples each of the example and the comparative example were prepared.

[0071] As a result of the humidity load test, the number of samples determined to be defective in the comparative multilayer ceramic capacitor was 36 out of 36.

[0072] On the other hand, in the multilayer ceramic capacitor of the embodiment, the number of samples determined to be defective was 0 out of 36.

[0073] Therefore, in all the samples in the examples, highly reliable multilayer ceramic capacitors were obtained.

[0074] The present invention is not limited to the above-described embodiment, and various modifications may be made within the scope of the present invention. Furthermore, the thicknesses of the ceramic layers, the number of layers, the area of ​​the opposing electrodes, and the outer dimensions of the ceramic electronic component are not limited to those described above. [Explanation of symbols]

[0075] 10 Multilayer ceramic capacitors 12 Ceramic body 13 First end face 14 Second end face 15 First aspect 16 The second aspect 17 First main surface 18 Second main surface 20. Ceramic layer for inner layer 22 First internal electrode 24 Second internal electrode 26 Inner Layer 28, 30 outer layer 32, 34 Side margin 32a, 34a Outer part 32b, 34b inner part 40, 42 external electrode 40a, 42a electrode layer 40b, 42b First plating layer 40c, 42c Second plating layer 50a, 50b Ceramic green sheet 52a, 52b conductive film 60 Stacked Chip

Claims

1. A rectangular parallelepiped ceramic body; an external electrode disposed on the ceramic body; A multilayer ceramic capacitor comprising: The ceramic body is an inner layer portion including an internal electrode; outer layer portions arranged to sandwich the inner layer portion in a stacking direction; a side margin portion disposed so as to sandwich the inner layer portion and the outer layer portion in a width direction; having The multilayer ceramic capacitor has a void volume that decreases from the inside to the outside of the side margin portion.

2. A rectangular parallelepiped ceramic body; an external electrode disposed on the ceramic body; A multilayer ceramic capacitor comprising: The ceramic body is A first internal electrode and a second internal electrode; a side margin portion which is a region in which the first internal electrode and the second internal electrode are not present as viewed from the lamination direction; having The multilayer ceramic capacitor has a void volume that decreases from the inside to the outside of the side margin portion.

3. A rectangular parallelepiped ceramic body; an external electrode disposed on the ceramic body; A multilayer ceramic capacitor comprising: The ceramic body is an inner layer portion including an internal electrode; outer layer portions arranged to sandwich the inner layer portion in a stacking direction; a side margin portion disposed so as to sandwich the inner layer portion and the outer layer portion in a width direction; Equipped with The internal electrode includes a first internal electrode and a second internal electrode, a grain size at ends of the first internal electrode and the second internal electrode in the vicinity of the side margin portion is smaller than the grain size on the front surface side of the ceramic body.

4. A rectangular parallelepiped ceramic body; an external electrode disposed on the ceramic body; A multilayer ceramic capacitor comprising: The ceramic body is A first internal electrode and a second internal electrode; a side margin portion which is a region in which the first internal electrode and the second internal electrode are not present as viewed from the lamination direction; having a grain size at ends of the first internal electrode and the second internal electrode in the vicinity of the side margin portion is smaller than the grain size on the front surface side of the ceramic body.

5. A rectangular parallelepiped ceramic body; an external electrode disposed on the ceramic body; A multilayer ceramic capacitor comprising: The ceramic body is an inner layer portion including an internal electrode; outer layer portions arranged to sandwich the inner layer portion in a stacking direction; a side margin portion disposed so as to sandwich the inner layer portion and the outer layer portion in a width direction; having The multilayer ceramic capacitor has a Ba content between ceramic particles made of a ceramic dielectric material that decreases from the inside to the outside of the side margin portion.

6. A rectangular parallelepiped ceramic body; an external electrode disposed on the ceramic body; A multilayer ceramic capacitor comprising: The ceramic body is A first internal electrode and a second internal electrode; a side margin portion which is a region in which the first internal electrode and the second internal electrode are not present as viewed from the lamination direction; Equipped with The multilayer ceramic capacitor has a Ba content between ceramic particles made of a ceramic dielectric material that decreases from the inside to the outside of the side margin portion.

Citation Information

Patent Citations

  • Electronic components, dielectric porcelain composition, and method for manufacturing the same

    JP2005145791A

  • Multilayer chip capacitor and manufacturing method thereof

    JP2006179873A

  • Multi-layered ceramic electronic component

    JP2009016796A

  • Multilayer ceramic electronic component

    JP2010050263A

  • Ceramic electronic component and manufacturing method therefor

    JP2012004236A