Polyvinyl acetal resin, and resin composition for ceramic green sheet

The development of a polyvinyl acetal resin with specific molecular weight and group content addresses the issues of undissolved matter and strength in ceramic green sheets, improving dispersibility and electrical properties, and ensuring reliable multilayer ceramic capacitors.

WO2024247894A1PCT designated stage expired Publication Date: 2024-12-05SEKISUI CHEMICAL CO LTD

Patent Information

Application Number
PCT/JP2024/019061
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-26
Filing Date
2024-05-23
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional polyvinyl acetal resins used in ceramic green sheets for multilayer ceramic capacitors result in poor quality due to undissolved matter, leading to voids, decreased dispersibility, and electrical property degradation, with insufficient strength and susceptibility to delamination and dimensional changes as the sheets become thinner.

Method used

A polyvinyl acetal resin with a Z average molecular weight of 700,000 to 2,500,000 and a molecular weight differential distribution value at LogM=6.00 of 5.00 to 110.0, along with specific acetal and hydroxyl group content, is developed to enhance dispersibility, strength, and resistance to delamination and dimensional changes during drying.

Benefits of technology

The optimized polyvinyl acetal resin improves the wettability and dispersion stability of ceramic powder, resulting in ceramic green sheets with high strength and reliability, reducing voids and electrical property degradation, and enhancing the quality of multilayer ceramic capacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024019061_05122024_PF_FP_ABST
    Figure JP2024019061_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides: a polyvinyl acetal resin; and a resin composition for a ceramic green sheet, which have excellent ceramic powder dispersibility and dispersion stability and can afford a ceramic green sheet that has high strength and hardly causes delamination or dimensional change during drying, and with which a highly reliable multilayer ceramic capacitor can be produced. The present invention is a polyvinyl acetal resin having a Z average molecular weight (Mz) of 700,000-2,500,000, and having a molecular weight differential distribution value of 5.00-110.0 at Lоg M = 6.00.
Need to check novelty before this filing date? Find Prior Art

Description

Polyvinyl acetal resin and resin composition for ceramic green sheet

[0001] The present invention relates to a polyvinyl acetal resin and a resin composition for ceramic greens.

[0002] In recent years, electronic components mounted in various electronic devices have become increasingly miniaturized and multilayered, resulting in widespread use of multilayer electronic components such as multilayer circuit boards, laminated coils, and multilayer ceramic capacitors. Multilayer ceramic capacitors, among others, are generally manufactured through the following process. First, a plasticizer, dispersant, etc. are added to a solution of a binder resin, such as polyvinyl butyral resin or poly(meth)acrylate resin, dissolved in an organic solvent. Then, ceramic raw material powder is added and uniformly mixed using a mixing device such as a bead mill or ball mill. After degassing, a ceramic slurry composition with a constant viscosity is obtained. This slurry composition is cast onto a support surface, such as a release-treated polyethylene terephthalate film or SUS plate, using a doctor blade or reverse roll coater. The resulting ceramic green sheets are then heated to remove volatiles such as the solvent, and the sheets are peeled off from the support to obtain ceramic green sheets. Next, multiple sheets of the resulting ceramic green sheets, each coated with a conductive paste for internal electrodes by screen printing, are alternately stacked and heated and pressed together to form a laminate. Thereafter, the laminate is subjected to a process of thermally decomposing and removing binder resin components and the like contained in the laminate, a so-called degreasing process, and then external electrodes are sintered onto the end faces of the ceramic sintered body obtained by firing, to obtain a multilayer ceramic capacitor.

[0003] Resin compositions for ceramic green sheets used in the production of ceramic green sheets are generally prepared as solutions of polyvinyl acetal resins in organic solvents such as methyl ethyl ketone, toluene, alcohol, and mixtures thereof. However, conventional polyvinyl acetal resins often contain traces of undissolved matter when dissolved in organic solvents. The presence of such undissolved matter can lead to voids during the degreasing and firing processes and reduced dispersibility of ceramic powders, resulting in poor electrical properties of the resulting products. Therefore, when polyvinyl acetal resins are used in ceramic green sheets, they must be blended with organic and inorganic compounds, dissolved in an organic solvent, and then filtered to remove the undissolved matter.

[0004] In response to this, Patent Document 1 proposes a polyvinyl acetal resin in which a 5 wt % solution of the polyvinyl acetal resin is dissolved in a 1:1 mixed solvent of methyl ethyl ketone and / or toluene and ethanol, and the resulting solution is filtered using a filter with 5 μm openings at a filtration temperature of 25° C. and a filtration pressure of 10 mmHg, resulting in a decrease in filtration flow rate of less than 10%. Furthermore, it is said that the use of such a polyvinyl acetal resin results in less undissolved matter when dissolved in an organic solvent, enabling the filtration time to be shortened, thereby improving productivity.

[0005] Japanese Patent Application Laid-Open No. 2005-325342

[0006] Meanwhile, in recent years, with the increasing functionality and miniaturization of electronic devices, multilayer ceramic capacitors are required to have larger capacitance and be smaller, and ceramic green sheets are also required to be thinner. However, when the polyvinyl acetal resin described in Patent Document 1 is used, there is a problem that the strength of the resulting ceramic green sheets is insufficient. Furthermore, during the process of laminating and drying the ceramic green sheets, delamination (interlayer peeling) and dimensional changes may occur. When delamination and dimensional changes occur as the ceramic green sheets are made thinner, there is a problem that the laminate may have poor appearance after cutting.

[0007] An object of the present invention is to provide a polyvinyl acetal resin and a resin composition for ceramic green sheets that can be used to obtain ceramic green sheets that have excellent dispersibility and dispersion stability of ceramic powder, are high in strength, and are resistant to delamination and dimensional change during drying, and that can be used to fabricate highly reliable multilayer ceramic capacitors.

[0008] The present disclosure (1) is a polyvinyl acetal resin having a Z-average molecular weight (Mz) of 700,000 or more and 2,500,000 or less, and a molecular weight differential distribution value at Log M = 6.00 of 5.00 or more and 110.0 or less. The present disclosure (2) is a polyvinyl acetal resin having a hydroxyl group amount relative to the Z-average molecular weight (hydroxyl group amount / Z-average molecular weight) of 1.30 × 10 -5 The polyvinyl acetal resin according to Disclosure (1) is as described above. Disclosure (3) is the polyvinyl acetal resin according to Disclosure (1) or (2), in which the amount of acetal groups is 50 to 83 mol%. Disclosure (4) is a resin composition for a ceramic green sheet, comprising the polyvinyl acetal resin according to any one of Disclosures (1) to (3) and a plasticizer. The present invention is described in detail below.

[0009] As a result of extensive investigations, the present inventors have found that a polyvinyl acetal resin having a Z-average molecular weight and a molecular weight differential distribution value at Log M = 6.00 within a predetermined range has excellent dispersibility and dispersion stability for ceramic powder, and can provide ceramic green sheets that are high in strength and are resistant to delamination and dimensional change during drying, thereby enabling the production of highly reliable multilayer ceramic capacitors, which has led to the completion of the present invention.

[0010] The polyvinyl acetal resin of the present invention has a Z-average molecular weight (Mz) of 700,000 or more and 2,500,000 or less, and a molecular weight differential distribution value at Log M = 6.00 of 5.00 or more and 110.0 or less. By containing such a polyvinyl acetal resin, it is possible to obtain a ceramic green sheet that has high strength and is resistant to delamination and dimensional change during drying.

[0011] The Z-average molecular weight (Mz) of the polyvinyl acetal resin of the present invention is 700,000 or more and 2,500,000 or less. By setting the Mz within this range, wettability with ceramic powder can be improved, thereby improving dispersion stability. The Mz is preferably 750,000 or more, more preferably 800,000 or more, and preferably 2,400,000 or less, more preferably 2,300,000 or less, and even more preferably 1,490,000 or less. That is, the Z-average molecular weight is 700,000 to 2,500,000, preferably 750,000 to 2,400,000, more preferably 750,000 to 2,300,000, and even more preferably 800,000 to 1,490,000. The Mz can be measured by gel permeation chromatography (GPC) using N-methylpyrrolidone as the solvent and an appropriate standard (eg, a polystyrene standard).

[0012] The molecular weight differential distribution value at Log M = 6.00 of the polyvinyl acetal resin of the present invention is 5.00 or more and 110.0 or less. By setting it within this range, a good balance between dispersibility and strength can be achieved. The molecular weight differential distribution value at Log M = 6.00 is preferably 7.00 or more, more preferably 8.00 or more, and preferably 100.0 or less, more preferably 95.0 or less. That is, the molecular weight differential distribution value at Log M = 6.00 is 5.00 to 110.0, preferably 7.00 to 100.0, more preferably 8.00 to 95.0.

[0013] In the present invention, the "molecular weight differential distribution value at Log M = 6.00" refers to the differential distribution value when the logarithm of the molecular weight M, log M, is 6.00. This does not simply mean that the molecular weight is high, but rather refers to the proportion of high molecular weight components in the resin. As an example of the molecular weight differential distribution value, FIG. 1 shows a molecular weight differential distribution curve with Log M on the horizontal axis and the molecular weight differential distribution value on the vertical axis. Note that the molecular weight differential distribution value is not a value detected by optical measurement, but rather "a value obtained by differentiating the concentration fraction by the logarithm of the molecular weight." In the present invention, the molecular weight differential distribution value when Log M is 6.00 is specified to be 5.00 or more and 110.0 or less. The molecular weight differential distribution value at Log M = 6.00 can be measured by GPC (gel permeation chromatography) using a sample prepared by dissolving the polyvinyl acetal resin to be measured in tetrahydrofuran (THF) at a concentration of 0.2 wt %.

[0014] The molecular weight differential distribution value at Mz and Log M = 6.00 can be adjusted, for example, by changing the average degree of polymerization and degree of saponification of the raw material polyvinyl alcohol resin, and the temperature and time conditions of the acetalization reaction, and by appropriately setting the amount of acetal groups, hydroxyl groups, acetyl groups, etc. of the polyvinyl acetal resin. In particular, the molecular weight differential distribution value at Mz and Log M = 6.00 can be adjusted by changing the holding temperature, holding time, temperature rise time, and temperature rise rate during the acetalization reaction, which will be described later.

[0015] The polyvinyl acetal resin of the present invention preferably has a structural unit having an acetal group represented by the following formula (1), a structural unit having a hydroxyl group represented by the following formula (2), and a structural unit having an acetyl group represented by the following formula (3):

[0016]

[0017] In the above formula (1), R 1 represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms.

[0018] In the above formula (1), R 1is an alkyl group having 1 to 20 carbon atoms, examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, a hexyl group, a heptyl group, a 2-ethylhexyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, a dodecyl group, a tridecyl group, a tetradecyl group, a pentadecyl group, an octadecyl group, etc. Of these, a methyl group and an n-propyl group are preferred.

[0019] In the polyvinyl acetal resin of the present invention, the content of the structural unit having an acetal group represented by the above formula (1) (hereinafter also referred to as "acetal group amount") is preferably 50 mol% in lower limit and 83 mol% in upper limit. When the acetal group amount is 50 mol% or more, the solubility in organic solvents can be improved. When the acetal group amount is 83 mol% or less, the polyvinyl acetal resin can have excellent tensile strength. The acetal group amount is more preferably 55 mol% in lower limit and 80 mol% in upper limit. That is, the acetal group amount is preferably 50 to 83 mol%, and more preferably 55 to 80 mol%. The acetal group amount may be, for example, 1 The amount of acetal groups can be measured by H-NMR. Since the acetal groups of the polyvinyl acetal resin are obtained by acetalizing two hydroxyl groups of polyvinyl alcohol, the amount of acetal groups is calculated by counting the two acetalized hydroxyl groups.

[0020] In the polyvinyl acetal resin of the present invention, the content of the structural unit having a hydroxyl group represented by the general formula (2) (hereinafter also referred to as the "hydroxyl group amount") is preferably 18 mol% in lower limit and 40 mol% in upper limit. When the hydroxyl group amount is 18 mol% or more, the polyvinyl acetal resin can have high toughness. When the hydroxyl group amount is 40 mol% or less, the solubility in organic solvents can be sufficiently improved. The hydroxyl group amount is more preferably 22 mol% in lower limit and 38 mol% in upper limit. That is, the hydroxyl group amount is preferably 18 to 40 mol%, and more preferably 22 to 38 mol%. The hydroxyl group amount may be, for example, 1 It can be measured by H-NMR.

[0021] In the polyvinyl acetal resin of the present invention, the content of the structural unit having an acetyl group represented by the general formula (3) (hereinafter also referred to as the "acetyl group amount") is preferably 0.1 mol% at the lower limit and 22.0 mol% at the upper limit. When the acetyl group amount is 0.1 mol% or more, it is possible to suppress the increase in viscosity of the slurry composition for a ceramic green sheet due to intramolecular and intermolecular hydrogen bonding of hydroxyl groups in the polyvinyl acetal resin. When the acetyl group amount is 22.0 mol% or less, it is possible to improve the handleability of the polyvinyl acetal resin without excessively increasing its flexibility. The acetyl group amount is more preferably 0.5 mol% at the lower limit and 15.0 mol% at the upper limit. That is, the acetyl group amount is preferably 0.1 to 22.0 mol%, and more preferably 0.5 to 15.0 mol%. The acetyl group amount may be, for example, 1 It can be measured by H-NMR.

[0022] The hydroxyl group amount relative to the Z-average molecular weight of the polyvinyl acetal resin of the present invention (hydroxyl group amount / Mz) is 1.30×10 -5 By adjusting the amount of hydroxyl groups to the above lower limit or more, high dispersibility can be obtained. The amount of hydroxyl groups / Mz is preferably 1.40×10 -5 More preferably, it is 1.50 x 10 or more. -5 More preferably, it is 2.70×10 or more.-5 Preferably, it is 2.65×10 or less. -5 More preferably, it is 2.60 x 10 or less. -5 More preferably, the amount of hydroxyl groups / Mz is 1.30×10 or less. -5 ~2.70 x 10 -5 Preferably, it is 1.40 × 10 -5 ~2.65 x 10 -5 More preferably, it is 1.50 × 10 -5 ~2.60 x 10 -5 It is more preferable that:

[0023] The polyvinyl acetal resin of the present invention has an average degree of polymerization of preferably 500 or more preferably 600, from the viewpoint of maintaining mechanical strength when producing a thin film ceramic green sheet. Furthermore, from the viewpoint of solubility in organic solvents and dissolution viscosity, the average degree of polymerization is preferably 10,000 or more preferably 9,000. That is, the average degree of polymerization is preferably 500 to 10,000, more preferably 600 to 9,000. The average degree of polymerization of the polyvinyl acetal resin is the same as that of the raw material polyvinyl alcohol. The average degree of polymerization can be measured in accordance with JIS K 6726.

[0024] The polyvinyl acetal resin of the present invention can usually be produced by acetalizing a polyvinyl alcohol resin.

[0025] The polyvinyl alcohol resin can be, for example, a conventionally known polyvinyl alcohol resin, such as a resin produced by saponifying a polyvinyl acetate resin with an alkali, an acid, aqueous ammonia, or the like. The polyvinyl alcohol resin can be fully saponified, but it does not need to be fully saponified as long as it has at least one unit having two consecutive hydroxyl groups at the meso and racemo positions at at least one location on the main chain; it can also be a partially saponified polyvinyl alcohol resin. Furthermore, the polyvinyl alcohol resin can also be a copolymer of vinyl alcohol and a monomer copolymerizable with vinyl alcohol, such as an ethylene-vinyl alcohol copolymer resin or a partially saponified ethylene-vinyl alcohol copolymer resin. Examples of the polyvinyl acetate resin include ethylene-vinyl acetate copolymers.

[0026] The polyvinyl alcohol resin preferably has a degree of saponification of 75 mol% or more. The degree of saponification is more preferably 76 mol% or more and 99.4 mol% or less, and even more preferably 78 mol% or more and 98 mol% or less. That is, the degree of saponification is preferably 76 to 99.4 mol%, and more preferably 78 to 98 mol%. By using the polyvinyl alcohol resin, the Mz can be set within a predetermined range.

[0027] The acetalization is preferably carried out in an aqueous solvent, a mixed solvent of water and a water-compatible organic solvent, or an organic solvent. Examples of the water-compatible organic solvent include alcohol-based organic solvents. Examples of the organic solvent include alcohol-based organic solvents, aromatic organic solvents, aliphatic ester-based solvents, ketone-based solvents, lower paraffin-based solvents, ether-based solvents, amide-based solvents, and amine-based solvents. Examples of the alcohol-based organic solvent include methanol, ethanol, n-propanol, isopropanol, n-butanol, and tert-butanol. Examples of the aromatic organic solvent include xylene, toluene, ethylbenzene, and methyl benzoate. Examples of the aliphatic ester-based solvent include methyl acetate, ethyl acetate, butyl acetate, methyl propionate, ethyl propionate, methyl butyrate, ethyl butyrate, methyl acetoacetate, and ethyl acetoacetate. Examples of the ketone solvents include acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, methylcyclohexanone, benzophenone, and acetophenone. Examples of the lower paraffin solvents include hexane, pentane, octane, cyclohexane, and decane. Examples of the ether solvents include diethyl ether, tetrahydrofuran, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, and propylene glycol diethyl ether. Examples of the amide solvents include N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and acetanilide. Examples of the amine solvents include ammonia, trimethylamine, triethylamine, n-butylamine, di-n-butylamine, tri-n-butylamine, aniline, N-methylaniline, N,N-dimethylaniline, and pyridine. These solvents can be used alone or in combination of two or more. Among these, ethanol, n-propanol, isopropanol, and tetrahydrofuran are particularly preferred from the viewpoints of solubility in the resin and ease of purification.

[0028] The acetalization is preferably carried out in the presence of an acid catalyst. The acid catalyst is not particularly limited, and examples thereof include mineral acids such as sulfuric acid, hydrochloric acid, nitric acid, and phosphoric acid, carboxylic acids such as formic acid, acetic acid, and propionic acid, and sulfonic acids such as methanesulfonic acid, ethanesulfonic acid, benzenesulfonic acid, and paratoluenesulfonic acid. These acid catalysts may be used alone or in combination of two or more compounds. Among these, hydrochloric acid, nitric acid, and sulfuric acid are preferred, and hydrochloric acid is particularly preferred.

[0029] Examples of the aldehyde used in the acetalization include aldehydes having a chain aliphatic group, a cyclic aliphatic group, or an aromatic group having 1 to 10 carbon atoms. Conventionally known aldehydes can be used as these aldehydes. The aldehyde used in the acetalization reaction is not particularly limited, and examples include aliphatic aldehydes and aromatic aldehydes. Examples of the aliphatic aldehyde include formaldehyde, acetaldehyde, propionaldehyde, n-butyraldehyde, isobutyraldehyde, n-valeraldehyde, n-hexylaldehyde, 2-ethylbutyraldehyde, 2-ethylhexylaldehyde, n-heptylaldehyde, n-octylaldehyde, n-nonylaldehyde, n-decylaldehyde, and amylaldehyde. Examples of the aromatic aldehyde include benzaldehyde, cinnamaldehyde, 2-methylbenzaldehyde, 3-methylbenzaldehyde, 4-methylbenzaldehyde, p-hydroxybenzaldehyde, m-hydroxybenzaldehyde, phenylacetaldehyde, and β-phenylpropionaldehyde. These aldehydes may be used alone or in combination of two or more. Among these, preferred aldehydes are formaldehyde, acetaldehyde, butylaldehyde, 2-ethylhexylaldehyde, and n-nonylaldehyde, which have excellent acetalization reactivity and can provide a sufficient internal plasticizing effect to the resulting resin, thereby imparting good flexibility. Furthermore, formaldehyde, acetaldehyde, and butylaldehyde are more preferred because they can provide an adhesive composition that is particularly excellent in impact resistance and adhesion to metals.

[0030] The amount of the aldehyde to be added can be appropriately determined depending on the amount of acetal groups in the target polyvinyl acetal resin. In particular, it is preferable to add the aldehyde in an amount of from 50 mol % to 95 mol %, more preferably from 55 mol % to 90 mol %, based on 100 mol % of polyvinyl alcohol, because this allows the acetalization reaction to proceed efficiently and makes it easy to remove unreacted aldehyde.

[0031] The acetalization reaction is preferably carried out by raising the temperature at a predetermined temperature rise rate and then maintaining the temperature for a certain period of time. The temperature rise time in the acetalization reaction is preferably 120 minutes or more and 420 minutes or less, and more preferably 180 minutes or more and 360 minutes or less. That is, the temperature rise time is preferably 120 to 420 minutes, and more preferably 180 to 360 minutes. The temperature rise rate is preferably 0.1°C / min or more and 0.4°C / min or less. That is, the temperature rise rate is preferably 0.1 to 0.4°C / min. By raising the temperature for the above temperature rise time and at the above temperature rise rate, the molecular weight differential distribution value at Mz and LogM = 6.00 can be set within a predetermined range.

[0032] The retention time in the acetalization reaction is preferably 1 hour or more and 10 hours or less, more preferably 2 hours or more and 9 hours or less, and even more preferably 2.6 hours or more. That is, the retention time is preferably 1 to 10 hours, and more preferably 2 to 9 hours or less. By setting the retention time as described above, the Mz can be set within a predetermined range. The retention temperature in the acetalization reaction is preferably 30°C or more and 80°C or less, and more preferably 40°C or more and 70°C or less. That is, the retention temperature is preferably 30 to 80°C, and more preferably 40 to 70°C. By setting the retention temperature as described above, the Mz and the molecular weight differential distribution value at LogM = 6.00 can be set within a predetermined range.

[0033] The present invention also relates to a resin composition for a ceramic green sheet, which comprises the polyvinyl acetal resin of the present invention and a plasticizer. The resin composition for a ceramic green sheet of the present invention may contain components such as an antioxidant, a surfactant, an ultraviolet absorber, and an antifoaming agent, as long as the effects of the present invention are not impaired.

[0034] As a method for producing the resin composition for a ceramic green sheet of the present invention, for example, a plasticizer and other additives that are added as needed can be added to a polyvinyl acetal resin obtained by acetalizing a polyvinyl alcohol resin with an aldehyde, and then mixed to obtain a resin composition for a ceramic green sheet.

[0035] The resin composition for ceramic green sheets of the present invention contains a plasticizer. Addition of the plasticizer can significantly improve the mechanical strength and flexibility of the resulting ceramic green sheet. Examples of the plasticizer include phthalate diesters such as dioctyl phthalate (DOP) and dibutyl phthalate (DBP), adipic acid diesters such as dioctyl adipate, and alkylene glycol diesters such as triethylene glycol-di-2-ethylhexanoate, tetraethylene glycol-di-2-ethylhexanoate, triethylene glycol-di-2-ethylbutyrate, tetraethylene glycol-di-2-ethylbutyrate, tetraethylene glycol-di-heptanoate, and triethylene glycol-di-heptanoate.

[0036] In the resin composition for a ceramic green sheet of the present invention, the content of the plasticizer relative to 100 parts by weight of the polyvinyl acetal resin is preferably 7 parts by weight in lower limit, more preferably 8.5 parts by weight in lower limit, and preferably 18 parts by weight in upper limit, more preferably 13.5 parts by weight in upper limit.

[0037] A slurry composition for a ceramic green sheet can be prepared by mixing an organic solvent and ceramic powder with the resin composition for a ceramic green sheet of the present invention.

[0038] The organic solvent is not particularly limited as long as it can dissolve the polyvinyl acetal resin, and examples thereof include ketones such as acetone, methyl ethyl ketone, dipropyl ketone, and diisobutyl ketone. Other examples include alcohols such as methanol, ethanol, isopropanol, and butanol, and aromatic hydrocarbons such as toluene and xylene. Further examples include esters such as methyl propionate, ethyl propionate, butyl propionate, methyl butanoate, ethyl butanoate, butyl butanoate, methyl pentanoate, ethyl pentanoate, butyl pentanoate, methyl hexanoate, ethyl hexanoate, butyl hexanoate, 2-ethylhexyl acetate, and 2-ethylhexyl butyrate. Other examples include methyl cellosolve, ethyl cellosolve, butyl cellosolve, terpineol, dihydroterpineol, butyl cellosolve acetate, butyl carbitol acetate, terpineol acetate, and dihydroterpineol acetate. In particular, alcohols, ketones, aromatic hydrocarbons and mixed solvents thereof are preferred in terms of coating and drying properties, with a mixed solvent of ethanol and toluene and a mixed solvent of methyl ethyl ketone and toluene being more preferred.

[0039] The content of the organic solvent in the ceramic green sheet slurry composition is determined depending on the type of polyvinyl acetal resin used and is not particularly limited, but if the content is too low, the solubility required for kneading is difficult to exhibit. On the other hand, if the content is too high, the viscosity of the ceramic green sheet slurry composition becomes too low, which can result in poor handling when producing ceramic green sheets. Therefore, the content of the organic solvent is preferably 20% by weight or more and 80% by weight or less.

[0040] Examples of the ceramic powder include powders of metal or nonmetal oxides or non-oxides used in ceramic production. These powders may be single compositions, compounds, or mixtures. The constituent elements of the metal oxides or non-oxides, both cations and anions, may be single elements or multiple elements, and may further contain additives added to improve the properties of the oxides or non-oxides. Specific examples include oxides, carbides, nitrides, borides, sulfides, etc. of Li, K, Mg, B, Al, Si, Cu, Ca, Sr, Ba, Zn, Cd, Ga, In, Y, lanthanides, actinides, Ti, Zr, Hf, Bi, V, Nb, Ta, W, Mn, Fe, Co, Ni, etc. Specific examples of oxide powders containing multiple metal elements, commonly referred to as double oxides, can be classified based on their crystal structure, such as NaNbO, which has a perovskite structure. 3 , SrZrO 3 , PbZrO 3 , SrTiO 3 , BaZrO 3 , PbTiO 3 , BaTiO 3 Examples of materials that have a spinel structure include MgAl 2 O 4 , ZnAl 2 O 4 , CoAl 2 O 4 , NiAl 2 O4, MgFe 2 O 4 Examples of materials with an ilmenite structure include MgTiO 3 , MnTiO 3 , FeTiO 3 As a material having a garnet structure, GdGa 5 O 12 , Y 6 Fe 5 O 12 Among these, the modified polyvinyl acetal resin of the present invention is BaTiO 3 It exhibits high properties compared to ceramic green sheets mixed with powder.

[0041] The average particle size of the ceramic powder is not particularly limited, but for example, for producing a thin ceramic green sheet (thickness of 5 μm or less), it is preferably 0.5 μm or less.

[0042] The slurry composition for a ceramic green sheet may contain other polyvinyl acetal resins other than the polyvinyl acetal resin of the present invention, as well as other resins such as acrylic resins and ethyl cellulose, within the range that does not impair the effects of the present invention. In such cases, the content of the polyvinyl acetal resin of the present invention relative to the total binder resins is preferably 50% by weight or more.

[0043] If necessary, a dispersant, an antioxidant, an ultraviolet absorber, a surfactant, a filler, etc. may be appropriately added to the above-mentioned slurry composition for a ceramic green sheet, and in some cases, a small amount of other resin such as an acrylic resin or a urethane resin may also be added.

[0044] The method for producing the slurry composition for ceramic green sheets is not particularly limited, and examples thereof include a method in which the polyvinyl acetal resin of the present invention, an organic solvent, a ceramic powder, and various additives to be added as needed are mixed using various mixers such as a ball mill, a blender mill, and a three-roll mill.

[0045] The ceramic green sheet slurry composition is applied to the ceramic green sheet, followed by heating and drying to obtain a ceramic green sheet. The ceramic green sheet can be used to manufacture a ceramic electronic component. For example, a ceramic electronic component can be manufactured by applying an electrode layer paste to the surface of the ceramic green sheet, stacking the ceramic green sheets on which the electrode layers have been formed, and then heat-pressing the resulting laminate, followed by degreasing and firing the laminate.

[0046] The method for applying the slurry composition for a ceramic green sheet is not particularly limited, and examples thereof include methods using a roll coater, a die coater, a curtain coater, etc. As for other specific methods, conventionally known methods can be used.

[0047] The ceramic electronic component is not particularly limited, and examples thereof include a multilayer ceramic capacitor, a multilayer ceramic inductor, a capacitor, a piezoelectric actuator, a multilayer varistor, a multilayer thermistor, an EMI filter, an aluminum nitride multilayer substrate, and an alumina multilayer substrate.

[0048] The method for producing the ceramic electronic component includes a step of applying an electrode layer paste to the surface of the ceramic green sheet. The electrode layer paste can be obtained by dissolving, for example, a polyvinyl acetal resin, ethyl cellulose, or acrylic resin as a binder resin in an organic solvent and dispersing a conductive powder or the like. These resins may be used alone or in combination. An electrode layer paste containing a polyvinyl acetal resin is preferred because it exhibits excellent adhesion to the ceramic green sheet during the thermocompression bonding step.

[0049] In the method for producing a ceramic electronic component, the ceramic green sheets having electrode layers formed thereon are prepared as described above, and then ceramic green sheets having electrode layers formed thereon that are prepared in the same manner are stacked and thermocompression-bonded to obtain a laminate, which is then degreased and fired, thereby obtaining a multilayer ceramic electronic component that solves problems such as sheet attack and cracking. Note that the thermocompression-bonding step and the steps of degreasing and firing the laminate are not particularly limited, and conventionally known methods can be used.

[0050] According to the present invention, it is possible to provide a polyvinyl acetal resin and a resin composition for a ceramic green sheet, which can produce a ceramic green sheet having high strength and being resistant to delamination and dimensional change during drying, and which can produce a multilayer ceramic capacitor with excellent reliability. Furthermore, by using the polyvinyl acetal resin of the present invention, the dispersibility and dispersion stability of ceramic powder can be significantly improved.

[0051] FIG. 1 is a diagram showing an example of a molecular weight differential distribution curve.

[0052] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to these examples.

[0053] Example 1 300 g of polyvinyl alcohol resin (average degree of polymerization: 1,700, degree of saponification: 99.0 mol%) was added to 300 g of pure water and dissolved by stirring at 90° C. for approximately 2 hours. This solution was cooled to 20° C., and 120 g of hydrochloric acid with a concentration of 35 wt % and 140 g of n-butyl aldehyde were added thereto. The temperature was increased at a rate of 0.2° C. / min (heating time: 250 min). The mixture was maintained at 70° C. for 3 hours to carry out an acetalization reaction. After completion of the reaction, the mixture was neutralized, washed with water, and dried in a conventional manner to obtain a white powder of polyvinyl acetal resin.

[0054] (Preparation of Resin Composition for Ceramic Green Sheet) 1.25 parts by weight of the obtained polyvinyl acetal resin was added to 48.75 parts by weight of an ethanol / toluene mixed solvent (weight ratio 1:1), and the mixture was stirred and dissolved to obtain a resin composition for ceramic green sheet.

[0055] (Production of Resin Sheet) The obtained resin composition for a ceramic green sheet was applied to a release-treated PET film using a coater so that the thickness after drying would be 20 μm, and then the film was dried by heating at 70° C. for 60 minutes to produce a resin sheet.

[0056] (Preparation of Slurry Composition) 2 parts by weight of the obtained polyvinyl acetal resin and 2 parts by weight of dioctyl phthalate (DOP) were added to 96 parts by weight of an ethanol / toluene mixed solvent (weight ratio 1:1) and stirred and dissolved to prepare a resin solution. Also, 3 parts by weight of polyvinyl acetal resin "BL-1" (manufactured by Sekisui Chemical Co., Ltd.) was added to 40 parts by weight of an ethanol / toluene mixed solvent (weight ratio 1:1) and stirred and dissolved. Next, 100 parts by weight of barium titanate powder (manufactured by Sakai Chemical Industry Co., Ltd., BT01) was added and stirred for 180 minutes in a bead mill (manufactured by Imex, Ready Mill) to prepare an inorganic dispersion. 100 parts by weight of the resin solution was added to the obtained inorganic dispersion and stirred in a bead mill to obtain a slurry composition. During stirring, sampling was carried out every 5 minutes, and 0.1 parts by weight of the obtained slurry composition was added to 10 parts by weight of an ethanol / toluene mixed solvent (weight ratio 1:1), and the mixture was stirred using an ultrasonic disperser (US-303, manufactured by SND Corporation) to prepare a solution for dispersion evaluation. Particle size distribution was measured using a laser diffraction particle size distribution analyzer (LA-910, manufactured by Horiba, Ltd.), and stirring was stopped when the D50 value of the particle size distribution reached 1.0 μm.

[0057] Example 2 3000 g of pure water was added to 300 g of polyvinyl alcohol resin (average degree of polymerization 3,000, degree of saponification 98.9 mol%), and the mixture was stirred at 90° C. for about 2 hours to dissolve the resin. The solution was cooled to 20° C., and 120 g of hydrochloric acid with a concentration of 35 wt % and 140 g of n-butyl aldehyde were added thereto. The temperature was increased at a rate of 0.2° C. / min (heating time: 250 min). The mixture was maintained at 70° C. for 3 hours to carry out an acetalization reaction. The reaction was then completed, and the mixture was neutralized, washed with water, and dried in a conventional manner to obtain a white powder of polyvinyl acetal resin, a resin composition for a ceramic green sheet, a resin sheet, and a slurry composition.

[0058] Example 3 300 g of polyvinyl alcohol resin (average degree of polymerization 5,000, degree of saponification 98.9 mol%) was added to 300 g of pure water and dissolved by stirring at 90° C. for about 2 hours. This solution was cooled to 20° C., and 120 g of hydrochloric acid with a concentration of 35 wt % and 140 g of n-butyl aldehyde were added thereto. The temperature was increased at a rate of 0.2° C. / min (heating time: 250 min). The mixture was maintained at 70° C. for 2 hours to carry out an acetalization reaction. After completion of the reaction, the mixture was neutralized, washed with water, and dried by conventional methods to obtain a white powder of polyvinyl acetal resin, a resin composition for a ceramic green sheet, a resin sheet, and a slurry composition.

[0059] Example 4 300 g of polyvinyl alcohol resin (average degree of polymerization 9,000, degree of saponification 98.9 mol%) was added to 300 g of pure water and dissolved by stirring at 90° C. for about 2 hours. This solution was cooled to 20° C., and 120 g of hydrochloric acid with a concentration of 35 wt % and 140 g of n-butyl aldehyde were added thereto. The temperature was increased at a rate of 0.2° C. / min (heating time: 250 min). The mixture was maintained at 70° C. for 3 hours to carry out an acetalization reaction. After completion of the reaction, the mixture was neutralized, washed with water, and dried by conventional methods to obtain a white powder of polyvinyl acetal resin, a resin composition for a ceramic green sheet, a resin sheet, and a slurry composition.

[0060] Example 5 300 g of polyvinyl alcohol resin (average degree of polymerization 1,700, degree of saponification 98.8 mol%) was added to 300 g of pure water and dissolved by stirring at 90° C. for about 2 hours. This solution was cooled to 20° C., and 120 g of hydrochloric acid with a concentration of 35 wt % and 140 g of n-butyl aldehyde were added thereto. The temperature was increased at a rate of 0.16° C. / min (heating time: 250 min). The mixture was maintained at 60° C. for 3 hours to carry out an acetalization reaction. After completion of the reaction, the mixture was neutralized, washed with water, and dried by conventional methods to obtain a white powder of polyvinyl acetal resin, a resin composition for a ceramic green sheet, a resin sheet, and a slurry composition.

[0061] Example 6 300 g of polyvinyl alcohol resin (average degree of polymerization 800, degree of saponification 98.8 mol%) was added to 300 g of pure water and dissolved by stirring at 90° C. for about 2 hours. This solution was cooled to 20° C., and 150 g of hydrochloric acid with a concentration of 35 wt % and 145 g of n-butyl aldehyde were added thereto. The temperature was increased at a rate of 0.16° C. / min (heating time: 250 min). The mixture was maintained at 60° C. for 3 hours to carry out an acetalization reaction. After completion of the reaction, the mixture was neutralized, washed with water, and dried by conventional methods to obtain a white powder of polyvinyl acetal resin, a resin composition for a ceramic green sheet, a resin sheet, and a slurry composition.

[0062] Comparative Example 1 3000 g of pure water was added to 300 g of polyvinyl alcohol resin (average degree of polymerization: 300, degree of saponification: 99.0 mol%), and the mixture was stirred for about 2 hours at 90° C. to dissolve the resin. This solution was cooled to 20° C., and 150 g of hydrochloric acid with a concentration of 35 wt % and 145 g of n-butyl aldehyde were added thereto. The temperature was increased at a rate of 0.5° C. / min (heating time: 10 minutes). The mixture was maintained at 25° C. for 4 hours to carry out an acetalization reaction. After completion of the reaction, the mixture was neutralized, washed with water, and dried by conventional methods to obtain a white powder of polyvinyl acetal resin, a resin composition for a ceramic green sheet, a resin sheet, and a slurry composition.

[0063] Comparative Example 2 3000 g of pure water was added to 300 g of polyvinyl alcohol resin (average degree of polymerization: 500, degree of saponification: 98.5 mol%), and the mixture was stirred for about 2 hours at 90° C. to dissolve the resin. This solution was cooled to 20° C., and 150 g of hydrochloric acid with a concentration of 35 wt % and 145 g of n-butyl aldehyde were added thereto. The temperature was increased at a rate of 0.5° C. / min (heating time: 10 minutes). The mixture was maintained at 25° C. for 3 hours to carry out an acetalization reaction. After completion of the reaction, the mixture was neutralized, washed with water, and dried by conventional methods to obtain a white powder of polyvinyl acetal resin, a resin composition for a ceramic green sheet, a resin sheet, and a slurry composition.

[0064] Comparative Example 3 3000 g of pure water was added to 300 g of polyvinyl alcohol resin (average degree of polymerization 800, degree of saponification 99.0 mol%), and the mixture was stirred at 90° C. for about 2 hours to dissolve the resin. This solution was cooled to 20° C., and 150 g of hydrochloric acid with a concentration of 35 wt % and 145 g of n-butyl aldehyde were added thereto. The temperature was increased at a rate of 0.7° C. / min (heating time: 7 minutes). The mixture was maintained at 25° C. for 3 hours to carry out an acetalization reaction. After completion of the reaction, the mixture was neutralized, washed with water, and dried by conventional methods to obtain a white powder of polyvinyl acetal resin, a resin composition for a ceramic green sheet, a resin sheet, and a slurry composition.

[0065] Comparative Example 4 300 g of polyvinyl alcohol resin (average degree of polymerization 9,000, degree of saponification 99.0 mol%) was added to 300 g of pure water and dissolved by stirring at 90° C. for about 2 hours. This solution was cooled to 20° C., and 150 g of hydrochloric acid with a concentration of 35 wt % and 145 g of n-butyl aldehyde were added thereto. The temperature was increased at a rate of 0.7° C. / min (heating time: 10 minutes). The mixture was maintained at 25° C. for 2.5 hours to carry out an acetalization reaction. After completion of the reaction, the mixture was neutralized, washed with water, and dried by conventional methods to obtain a white powder of polyvinyl acetal resin, a resin composition for a ceramic green sheet, a resin sheet, and a slurry composition.

[0066] Comparative Example 5 300 g of polyvinyl alcohol resin (average degree of polymerization 8,800, degree of saponification 99.0 mol%) was added to 300 g of pure water and dissolved by stirring at 90° C. for about 2 hours. This solution was cooled to 20° C., and 150 g of hydrochloric acid with a concentration of 35 wt % and 150 g of n-butyl aldehyde were added thereto. The temperature was increased at a rate of 0.7° C. / min (heating time: 7 minutes). The mixture was maintained at 25° C. for 2.5 hours to carry out an acetalization reaction. After completion of the reaction, the mixture was neutralized, washed with water, and dried by conventional methods to obtain a white powder of polyvinyl acetal resin, a resin composition for a ceramic green sheet, a resin sheet, and a slurry composition.

[0067] Comparative Example 6 3000 g of pure water was added to 300 g of polyvinyl alcohol resin (average degree of polymerization 800, degree of saponification 98.7 mol%) and dissolved by stirring for about 2 hours at 90° C. This solution was cooled to 20° C., and 150 g of hydrochloric acid with a concentration of 35 wt % and 160 g of n-butyl aldehyde were added thereto. The mixture was maintained at 20° C. for 3 hours to carry out an acetalization reaction, and the reaction was completed. The mixture was then neutralized, washed with water, and dried by conventional methods to obtain a white powder of polyvinyl acetal resin, a resin composition for a ceramic green sheet, a resin sheet, and a slurry composition.

[0068] (Evaluation) The polyvinyl acetal resins, resin compositions for ceramic green sheets, resin sheets, and slurry compositions obtained in the Examples and Comparative Examples were evaluated as follows. The results are shown in Table 1.

[0069] (1) Evaluation of Polyvinyl Acetal Resin (1-1) Amount of Acetal Group, Amount of Hydroxyl Group, and Amount of Acetyl Group The polyvinyl acetal resin obtained was analyzed using an AV400 spectrometer (manufactured by Bruker). 1 H-NMR measurement was carried out to calculate the amount of acetal groups, hydroxyl groups, and acetyl groups. 6 The solution was dissolved in water to a concentration of 1.6% by weight to prepare a measurement solution. 1 H-NMR measurements were carried out at 80°C.

[0070] (1-2) Mz, molecular weight differential distribution value at Log M = 6.00 The obtained polyvinyl acetal resin was dissolved in tetrahydrofuran (THF) at a concentration of 0.2 wt %, and measurement was performed using a GPC apparatus HLC-8220 (manufactured by Tosoh Corporation). From the measurement results obtained, the Z-average molecular weight Mz was calculated using a molecular weight calibration curve prepared using monodisperse polystyrene standard samples. In addition, from the obtained molecular weight differential distribution curve, the molecular weight differential distribution value at Log M = 6.00 was measured. Note that a TSKgel Super HZ (manufactured by Tosoh Corporation) was used as the column.

[0071] (2) Evaluation of Resin Sheet (2-1) Tensile Modulus, Elongation at Break, and Stress at Break The obtained resin sheet was subjected to measurement of the stress at break (MPa), elongation at break (%), and tensile modulus (MPa) at a tensile speed of 20 mm / min using a tensile tester (AUTOGRAPH AGS-J, manufactured by Shimadzu Corporation) in accordance with JIS K 7113.

[0072] (3) Evaluation of Slurry Composition (3-1) Dispersibility (Preparation of Dispersibility Evaluation Solution) 0.1 parts by weight of the obtained slurry composition was added to 10 parts by weight of an ethanol / toluene mixed solvent (weight ratio 1:1), and the mixture was stirred with an ultrasonic disperser (manufactured by SND Corporation, US-303) to prepare a dispersibility evaluation solution.

[0073] (Dispersibility Evaluation) The particle size distribution of the obtained solution for dispersibility evaluation was measured 60 minutes after the end of stirring. The particle size distribution measurement was carried out using a laser diffraction particle size distribution meter (LA-910 manufactured by Horiba, Ltd.), and the average particle diameter was measured.

[0074] (3-2) Dispersion Stability Using the solution for dispersibility evaluation obtained in (3-1) above, particle size distribution was measured after leaving it at 23° C. for 1 week, and the average particle diameter was measured.

[0075] (4) Evaluation of Ceramic Green Sheet (Preparation of Ceramic Green Sheet) The obtained slurry composition was applied to a release-treated PET film using a coater so that the thickness after drying would be 20 μm, and then heated and dried to prepare a ceramic green sheet.

[0076] (4-1) Tensile Modulus, Elongation at Break, and Stress at Break (Preparation of Ceramic Green Sheets) 1 part by weight of polyvinyl acetal resin (BL-1, manufactured by Sekisui Chemical Co., Ltd.) was added to a mixed solvent of 20 parts by weight of toluene and 20 parts by weight of ethanol and stirred to dissolve. Next, 100 parts by weight of barium titanate powder (BT01, manufactured by Sakai Chemical Industry Co., Ltd., average particle size 0.1 μm) was added to the resulting solution and stirred for 180 minutes using a bead mill (Ready Mill, manufactured by Imex Co., Ltd.) to prepare an inorganic dispersion. The resin compositions for ceramic green sheets obtained in the Examples and Comparative Examples were added to the resulting inorganic dispersion and stirred for 90 minutes using a bead mill. The resulting inorganic dispersion was then coated onto a release-treated PET film using a coater to a thickness of 20 μm after drying. The resulting mixture was then heated and dried at 40°C for 30 minutes, and the PET film was peeled off to prepare a ceramic green sheet. The resulting ceramic green sheets were subjected to measurement of the stress at break (MPa), tensile modulus (MPa), and elongation at break (%) in accordance with JIS K 7113 using a tensile tester (AUTOGRAPH AGS-J, manufactured by Shimadzu Corporation) at a tension speed of 20 mm / min.

[0077] (4-2) Cutting cross section state After measuring "(4-1) Tensile modulus, elongation at break and stress at break", the fractured surface was observed with an SEM and evaluated according to the following evaluation criteria: ◎: No chips, cracks or scratches on the fractured surface ○: No chips or cracks on the fractured surface but scratches present △: No chips on the fractured surface but cracks present ×: Chips on the fractured surface and inter-sheet peeling present

[0078] (4-3) Dimensional Change Rate Ceramic green sheets were prepared in the same manner as in "(4-1) Tensile Modulus, Elongation at Break, and Stress at Break." The obtained ceramic green sheets were dried at 70°C for 3 hours, and the dimensional change rates before and after drying at 70°C were calculated and evaluated according to the following criteria: ◎: 2% or less ○: More than 2% and 3% or less △: More than 3% and 4% or less ×: More than 4%

[0079]

[0080] According to the present invention, it is possible to provide a polyvinyl acetal resin and a resin composition for a ceramic green sheet that can produce a ceramic green sheet that has excellent dispersibility and dispersion stability of ceramic powder, high strength, and is resistant to delamination and dimensional change during drying, and that can produce a highly reliable multilayer ceramic capacitor.

Claims

1. A polyvinyl acetal resin having a Z-average molecular weight (Mz) of 700,000 or more and 2,500,000 or less, and a molecular weight differential distribution value at Log M = 6.00 of 5.00 or more and 110.0 or less.

2. The amount of hydroxyl groups relative to the Z-average molecular weight (amount of hydroxyl groups / Z-average molecular weight) is 1.30×10 -5 The polyvinyl acetal resin according to claim 1 .

3. The polyvinyl acetal resin according to claim 1 or 2, wherein the amount of acetal groups is 50 to 83 mol %.

4. A resin composition for a ceramic green sheet, comprising the polyvinyl acetal resin according to claim 1 or 2 and a plasticizer.

Citation Information

Patent Citations

  • Polyvinyl acetal resin and method for producing polyvinyl acetal resin

    JP2005325342A

  • Preparation of polyvinyl butyral

    JP1981082806A

  • Ceramic slurry for green sheet forming and green sheet

    JP1995017769A

  • Production of polyvinyl acetal resin

    JP1998158328A

  • Polyvinyl acetal resin, composition for ceramic green sheet, ceramic green sheet and laminated ceramic capacitor

    JP2020056015A

Cited By

  • Polyvinyl acetal resin, resin solution, slurry for ceramic green sheet, ceramic green sheet, and multilayer ceramic capacitor

    WO2026211962A1

  • Polyvinyl acetal resin, slurry for ceramic green sheet, ceramic green sheet, and multilayer ceramic capacitor

    WO2026211963A1