Glass cloth and manufacturing method for the same

By treating glass cloth with a silane coupling agent after heat cleaning in a controlled dew point atmosphere, the glass cloth maintains stable dielectric properties over time, addressing the issue of increased dielectric loss tangent in conventional cloths.

JP2024150149APending Publication Date: 2024-10-23SHIN ETSU CHEMICAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023063415
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-23

AI Technical Summary

Technical Problem

Conventional glass cloths used in printed wiring boards react with water over time, leading to an increase in dielectric loss tangent, especially at high frequencies, making it difficult to maintain stable dielectric properties.

Method used

Treat glass cloth with a silane coupling agent after heat cleaning in a controlled dew point atmosphere to reduce metal hydroxides and bound water, followed by silane treatment to stabilize dielectric properties.

Benefits of technology

The treated glass cloth exhibits a low and stable dielectric loss tangent over time, even at high frequencies, ensuring reliable transmission performance in future high-speed communications like 5G.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150149000003
    Figure 2024150149000003
  • Figure 2024150149000001
    Figure 2024150149000001
  • Figure 2024150149000002
    Figure 2024150149000002
Patent Text Reader

Abstract

To provide a glass cloth and a manufacturing method, capable of manufacturing a substrate with excellent reliability while having less secular change in dielectric tangent and low frequency dependence of the dielectric tangent in a high frequency range, and also to provide a prepreg, a lamination board, and a print wiring board.SOLUTION: In a glass cloth treated with a silane coupling agent, the change ratio of a dielectric tangent at 10 GHz, measured by the cavity resonator method, is 1.5 times or less after 30 days of storage at 30°C and 80% RH compared to the level before storage.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a glass cloth having a low dielectric tangent at high frequencies, a low frequency dependency of the dielectric tangent, and little change over time in the dielectric tangent, and a method for producing the same, as well as a prepreg, a laminate, and a printed wiring board. [Background technology]

[0002] Currently, with the high performance and high-speed communication of information terminals such as smartphones, the printed wiring boards used are becoming increasingly dense and extremely thin, as well as lowering the dielectric constant and dielectric loss tangent. As an insulating material for these printed wiring boards, laminates made by laminating prepregs obtained by impregnating glass cloth with thermosetting resins such as epoxy resins (hereinafter referred to as "matrix resins") and curing them under heat and pressure are widely used. It is known that the transmission loss of signals in a board is improved with materials having smaller dielectric constant (ε) and dielectric loss tangent (tanδ), as shown by the Edward A. Wolff formula: transmission loss ∝√ε×tanδ, and it is known that the dielectric loss tangent contributes greatly to the transmission loss, as shown in the above formula.

[0003] Therefore, a low dielectric tangent is required for glass cloth, and glass cloths with improved dielectric properties such as D glass, NE glass, L glass, and quartz glass have been proposed (Patent Documents 1 to 5). In addition, the frequency used in future 5G communication applications will be high frequencies of 10 GHz or more, and in order to achieve stable transmission speed performance at any frequency, it is required that the frequency dependence of the dielectric tangent at frequencies of 10 GHz or more is low. Patent Document 6 describes a glass cloth and substrate using quartz glass cloth that has a low dielectric tangent and low frequency dependence. However, the glass cloth reacts with water over time, which causes the dielectric tangent to increase, and this effect is particularly noticeable in glass cloths with low dielectric tangents, and a glass cloth with a stable dielectric tangent not only with frequency but also with changes over time is required. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 5-170483 [Patent Document 2] JP 2009-263569 A [Patent Document 3] JP 2009-19150 A [Patent Document 4] JP 2006-282401 A [Patent Document 5] JP 2021-195689 A [Patent Document 6] JP 2022-131074 A Summary of the Invention [Problem to be solved by the invention]

[0005] Generally, the raw material for glass cloth is SiO 2 , Al 2 O 3 , B 2 O 3 These metal oxides react with water to form SiOH and Al. 2 (OH) 3 , B(OH) 3Metal hydroxides such as these are easily generated, and since metal hydroxides have polarity, they form strong hydrogen bonds with water present nearby. The dielectric tangent of metal hydroxides and bound water increases uniformly at high frequencies of 10 GHz or more. Therefore, it has been difficult to suppress the deterioration of the dielectric tangent over time and reduce the frequency dependency by simply changing the composition of glass, which is a metal oxide. In particular, when the surface of the glass cloth is heated by heat cleaning, which is a manufacturing process for glass cloth, it reacts with moisture in the air to generate a large amount of metal hydroxide and bound water. Furthermore, if metal hydroxide and bound water are present on the surface, they will slowly react with the glass cloth by absorbing moisture in the air even at room temperature, and the metal hydroxide and bound water will increase in a chain reaction. Therefore, even if a substrate with a low dielectric tangent and low frequency dependency can be manufactured at the beginning, there is a problem that the dielectric tangent will deteriorate over time. Due to these circumstances, it has been difficult to manufacture glass cloth with little change over time and low frequency dependency using the conventional method.

[0006] The present invention has been made in consideration of the above problems, and has an object to provide a glass cloth and a manufacturing method thereof, as well as a prepreg, a laminate, and a printed wiring board, which are capable of producing a substrate that exhibits little change in dielectric tangent over time, has low frequency dependency of the dielectric tangent at high frequencies, and is highly reliable. [Means for solving the problem]

[0007] As a result of intensive research into achieving the above-mentioned object, the inventors have found that the above-mentioned problems can be solved by providing a glass cloth in which, when stored for 30 days under conditions of 30°C and 80% RH, the rate of change in dielectric tangent at 10 GHz after storage compared to before storage, as measured by a cavity resonator method, is 1.5 or less, and have thus completed the present invention.

[0008] Therefore, the present invention provides the following inventions. 1. Glass cloth treated with a silane coupling agent, which, when stored for 30 days under conditions of 30°C and 80% RH, has a change in dielectric tangent at 10 GHz after storage compared to before storage, measured by the cavity resonator method, of 1.5 or less. 2. When the dielectric loss tangent at 10 GHz, 28 GHz, and 40 GHz is plotted on the vertical axis and the frequency on the horizontal axis, the gradient of the approximation line connecting the dielectric loss tangent at each frequency is 2.00×10 -5 The glass cloth described in 1 below. 3. The slope of the approximate line after saving is 2.5 x 10 -5 2. A glass cloth according to the following paragraph 2. 4. The change in the slope of the approximation line after saving compared to before saving is 0.4 x 10 -5 4. The glass cloth according to 2 or 3 below. 5. The glass cloth according to any one of 1 to 4, which has a dielectric loss tangent of 0.0010 or less at 10 GHz. 6.SiO 2 6. The glass cloth according to any one of 1 to 5, wherein the glass cloth contains 70% by mass or more of the glass cloth. 7.SiO 2 7. The glass cloth according to 6, wherein the glass cloth has a content of 95 mass % or more. 8. A prepreg comprising the glass cloth according to any one of 1 to 7 and an organic resin. 9. A laminate comprising the glass cloth according to any one of 1 to 7 and an organic resin. 10. A printed wiring board comprising the glass cloth according to any one of 1 to 7 and an organic resin. 11. A method for producing a silane-treated glass cloth, comprising: a step of heat-cleaning a glass cloth having a sizing agent attached thereto in a gas having a dew point of 15°C or less; and a silane treatment step of treating the heat-cleaned glass cloth with a silane coupling agent, A method for producing a silane-treated glass cloth, in which the amount of metal hydroxide and bound water in the glass cloth before the silane treatment step is 1,000 ppm or less. Effect of the Invention

[0009] According to the present invention, it is possible to provide a glass cloth having a small change in dielectric tangent over time and a low dielectric tangent at high frequencies, and a manufacturing method thereof. Prepregs, laminates, and printed wiring boards using such glass cloth have a significant effect of stably suppressing transmission loss in any environment or frequency in high-speed communications such as 5G, which will become increasingly common in the future. [Brief description of the drawings]

[0010] [Figure 1] FIG. 13 is a diagram showing how to determine the slope of an approximate straight line according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below. I. Physical properties of glass cloth The glass cloth of the present invention is a glass cloth treated with a silane coupling agent, and when stored for 30 days under conditions of 30°C and 80% RH, the rate of change of the dielectric loss tangent at 10 GHz after storage relative to before storage, measured by a cavity resonator method, is 1.5 or less. This rate of change is (dielectric loss tangent at 10 GHz after storage) / (dielectric loss tangent at 10 GHz before storage), and is preferably 1.3 or less, more preferably 1.2 or less. If the rate of change exceeds 1.5, the dielectric loss tangent changes significantly during storage, and when applied to a substrate, low transmission loss as designed cannot be obtained. The glass cloth and the treatment with the silane coupling agent will be described later. The details of the method for measuring the dielectric loss tangent by the cavity resonator method and the storage method will be described in the examples described later. Hereinafter, values ​​not described as "after storage" refer to values ​​of the glass cloth before or without storage.

[0012] The dielectric loss tangent at 10 GHz of the glass cloth after treatment with the silane coupling agent in the present invention is preferably low, and is preferably 0.0015 or less, more preferably 0.0010 or less, and even more preferably 0.0005 or less. In particular, as a method for lowering the dielectric loss tangent at 10 GHz, SiO 2 Examples of methods include increasing the amount of fluorine and reducing metal hydroxides and bound water.

[0013] Since the glass cloth of the present invention has a low frequency dependency of the dielectric tangent, the dielectric tangent at 28 GHz and 40 GHz is preferably 0.0020 or less, more preferably 0.0017 or less, more preferably 0.0015 or less, even more preferably 0.0014 or less, and particularly preferably 0.0010 or less.

[0014] In the glass cloth of the present invention, when the dielectric loss tangent at 10 GHz, 28 GHz, and 40 GHz measured by the cavity resonator method is plotted on the vertical axis and the frequency on the horizontal axis, the gradient of the approximation line connecting the dielectric loss tangent at each frequency is 2.00×10 -5 By setting the dielectric loss tangent in this range, a glass cloth having a lower dielectric loss tangent at high frequencies and a smaller change in the dielectric loss tangent over time can be obtained. The gradient of this approximation line is 1.50×10 -5 Less than or equal to 1.00×10 is preferable. -5 More preferably, it is equal to or less than 0, and particularly preferably equal to or less than 0. The lower limit is not particularly limited, and may be, for example, −1.00×10 -5 The slope of the approximation line is 2.0×10 -5 If the temperature exceeds this value, the substrate may not be able to achieve the same transmission loss at high frequencies as at low frequencies. Note that this is the value before storage.

[0015] The slope of the approximation line is measured by plotting the dielectric tangent (rounded off to the fifth decimal place) on the vertical axis and the frequency on the horizontal axis in a spreadsheet program such as Excel, calculating the approximation line, and displaying the value of the approximation line with three significant digits.

[0016] After 30 days of storage at 30℃ and 80% RH, the slope of the approximation line was 2.50×10 -5 Less than or equal to 1.70×10 is preferable. -5 Less than or equal to 1.20×10 is preferable. -5 The lower limit is not particularly limited, and is, for example, −1.00×10 -5 It is also possible to use the following.

[0017] The change in the slope of the approximation line after storage compared to before storage is 0.40 x 10 -5 Less than 0.30×10 is preferable. -5 The lower limit is not particularly limited, and may be, for example, 0.

[0018] II. Manufacturing method The method for producing the glass cloth of the present invention is not particularly limited as long as the glass cloth has the above-mentioned characteristics, and examples thereof include the following methods. Specifically, the method for producing the glass cloth includes a step of heat-cleaning the glass cloth having a sizing agent attached thereto in a gas having a dew point of 15° C. or less, and a silane treatment step of silane-treating the heat-cleaned glass cloth with a silane coupling agent, A method for producing a silane-treated glass cloth is preferred in which the amount of metal hydroxide and bound water in the glass cloth before the silane treatment step is 1,000 ppm or less.

[0019] [Glass cloth] The composition of the glass cloth used in the glass cloth of the present invention is not particularly limited. However, the rate of increase in the dielectric tangent of SiOH when the frequency increases is preferably 100% or more. 2 (OH) 3 or B(OH) 3 From a lower perspective, SiO 2 The amount is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 95% by mass or more of quartz glass, and even more preferably 99% by mass or more.

[0020] Glass cloth is produced by bundling glass filaments into strands, twisting them into yarns, and weaving them. The method for producing glass filaments is not particularly limited, but examples include a method of heating and stretching an ingot of a specified glass composition, and a method of heating and melting it to form molten glass, and then forming it into a thread-like shape using a bushing. In particular, SiO 2 When the ratio of is 95 mass % or more, the melting temperature becomes high and drawing using a bushing becomes difficult, so heating and drawing using an oxyhydrogen burner is performed.

[0021] Glass strands can be formed by applying a sizing agent to the surface of the drawn glass filaments and bundling them. The sizing agent is mainly made of starch, and softeners and lubricants can be added to impart functionality. The sizing agent composition is generally called a sizing agent. A known method can be used for the sizing agent treatment, and the type of sizing agent and the method of sizing agent treatment are not particularly limited, but a method that is less likely to cause fluff and thread breakage is appropriately selected. The sizing agent treatment reduces fluff and thread breakage. Examples of sizing agents include those containing starch, and treatment methods include immersion, application with a roller or belt applicator, spraying, etc.

[0022] The obtained glass strand is twisted to obtain a glass yarn. The frequency of twisting is preferably 0.1 to 5.0 times per 25 mm. A glass cloth is obtained by weaving the glass yarn. The glass cloth of the present invention has a basis weight of 10 to 100 g / m, although there is no particular limitation thereto. 3 The weaving method is not particularly limited, and examples thereof include weaving methods using an air jet loom, a water jet loom, a rapier loom, a shuttle loom, etc. When weaving is performed using an air jet loom, etc., PVA or starch can be attached as a secondary sizing agent to obtain further lubricity. The amount of sizing agent to be treated is not particularly limited as long as it is an amount that can achieve the purpose of the sizing treatment.

[0023] The glass cloth is preferably subjected to an opening treatment after weaving in order to enhance the impregnation with the resin. The opening method is not particularly limited, but examples include an opening treatment method using ultrasonic waves, a method using a high-pressure columnar water flow, and a method of spraying a diffusion spray into the atmosphere. In particular, a method using a gas-liquid mixed mist with an adjusted air-water volume ratio is preferable in that it can efficiently spread the fibers while suppressing misalignment and fluffing of the strands. The timing of opening is not particularly limited, but it is preferable to perform it before removing the sizing agent in order to utilize the slipperiness of the sizing agent.

[0024] [Oil removal process] The sizing agent remains attached to the surface of the glass cloth after weaving, and the silane coupling agent treatment of the glass cloth becomes insufficient, which is undesirable as it causes poor adhesion with the matrix resin. Therefore, a deoiling process is required after weaving in order to remove the attached sizing agent. The deoiling process is not particularly limited, but it is preferable to perform heat cleaning in an atmosphere with a dew point of 15°C or less as shown below in order not to increase the metal hydroxide on the surface. Since the sizing agent itself contains an organic group, the increase in the dielectric tangent due to the increase in frequency is suppressed, but since the dielectric tangent itself is high, the dielectric tangent at high frequencies may become high.

[0025] [Heat cleaning process] A preferred heat cleaning step of the present invention is a step of heat cleaning the glass cloth to which the sizing agent is attached in a gas having a dew point of 15° C. or less for the purpose of reducing the amount of metal hydroxide in the glass cloth as much as possible. The dew point is preferably 15° C. or less, more preferably 0° C. or less, and more preferably -50° C. or less. Heat cleaning under such conditions can be a factor in maintaining a low dielectric tangent not only at the initial stage but also after storage. The heating furnace used for heat cleaning is preferably one that can be heated to 100 to 900° C. and can be placed in a vacuum or a dry gas atmosphere with a dew point of 15° C. or less. There is no particular limitation as long as the heating furnace is of this type, and a gas furnace, an electric furnace, or a muffle furnace can be used.

[0026] Among these, it is preferable to use a heating furnace having a heat generating mechanism that generates 0.12 L or less of water per unit heat value (1,000 kcal). As long as it has such a heat generating mechanism, there is no particular limitation, and examples include an electric furnace, a muffle furnace, and the like, which includes a heating furnace having a heat generating mechanism capable of the above. In particular, an electric furnace is preferable because it does not involve combustion, and therefore the amount of water in the gas can be reduced to 0.12 L or less, and even less than 0.10 L.

[0027] The heating furnace preferably has a device for feeding a dry gas into the furnace, which may include a mechanism for generating a dry gas such as a compressor or an air dryer, piping for filling or introducing the dry gas and connecting the mechanism for generating the dry gas to the inside of the furnace, and an exhaust mechanism for exhausting the air from the inside of the furnace.

[0028] The method of filling the inside of the furnace with a gas having a dew point of 15° C. or less is not particularly limited as long as the inside of the furnace is a gas having a dew point of 15° C. or less, but includes a method of filling the inside of the furnace with a dry gas having a dew point of 15° C. or less before heating, or a method of introducing a dry gas having a dew point of 15° C. or less into the furnace. The introduction may be before heating, during heating, during temperature increase, during temperature maintenance, or during temperature decrease, and more than one of these may be selected and introduced. Among these, it is preferable to introduce a dry gas having a dew point of 15° C. or less, preferably 0° C. or less, into the furnace, and furthermore, it is preferable to introduce the dry gas into the furnace during temperature decrease. As the dry gas, a dry gas having a dew point of 15° C. or less selected from inert gases such as air, nitrogen, and argon may be used. Among these, dry air is preferable in terms of production efficiency. Examples of the device for generating the dry air include a compressor and an air dryer. In addition, the dew point in the present invention refers to the atmospheric pressure dew point. The dew point of the dry gas to be filled or introduced is 15° C. or less (moisture content: 12.8 g / m 3 ) is preferred, and 0°C (moisture content: 4.85g / m 3 ) or less, and -20°C or less (moisture content: 1.07g / m 3 ) is more preferable, and -60°C (moisture content: 0.0193g / m 3 In the present invention, the dew point refers to the atmospheric pressure dew point. The dew point of the dry gas to be filled or introduced is preferably 15° C. or less (moisture content: 12.8 g / m 3 ) is preferred, and 0°C (moisture content: 4.85g / m 3 ) or less, and -20°C or less (moisture content: 1.07g / m 3 ) is more preferable, and -60°C (moisture content: 0.0193g / m 3 ) The following are particularly preferred:

[0029] The dry gas that is charged and introduced into the furnace before heating has a dew point of 15° C. or less, preferably 0° C. or less, and from the standpoint of production efficiency and economic efficiency, dry air with a dew point of -20° C. or less is more preferable. The dew point of the dry gas introduced into the heating furnace is preferably 15° C. or lower, more preferably 0° C. or lower, further preferably −20° C. or lower, and particularly preferably −60° C. or lower. The amount of dry gas introduced is not particularly limited, but is preferably 0.5 to 20 times the volume of the drying furnace per hour, in order to sufficiently lower the dew point inside the furnace and keep the temperature inside the furnace constant.

[0030] The heating temperature for heat cleaning is preferably 200 to 900°C, more preferably 300 to 700°C, and can be 300°C or higher and less than 450°C. Similarly, the maximum heating temperature is preferably 200 to 900°C, more preferably 300 to 700°C, and can be 300°C or higher and less than 450°C. If the temperature is too low, the reaction described below does not proceed easily, and if it exceeds 900°C, the filaments of the cloth may fuse together and flexibility may be lost. There is no particular limitation regarding the heating during heat cleaning, and the cloth may be stored at a constant temperature, or may be heated at multiple temperatures in steps.

[0031] Regarding the heating time, conditions are preferred where the heating amount expressed by heating temperature (°C) of 100°C or more x heating time (h) is 450 (°C·h) or more in a vacuum or gas with a dew point of 15°C or less. For example, the heating amount of the present invention is maximum heating temperature: T (°C), warming time at maximum heating temperature: X (h: hours), temperature increase rate: Y°C / h, temperature decrease rate: Z°C / h, and if heating is performed in a vacuum or gas with a dew point of 15°C or less in all steps during temperature increase, temperature maintenance, and temperature decrease, the heating amount expressed by heating temperature (°C) of 100°C or more x heating time (h) is the total amount of heat during temperature increase, heat amount during warming, and heat amount during temperature decrease. If heating in a vacuum or gas with a dew point of 15°C or less is only during temperature decrease, the heating amount during temperature decrease is the heating amount of the present invention. Heat amount during heating: ((T-100)×(T-100) / Y)÷2 Heating amount when keeping warm: (T-100)×X Amount of heating when cooling down: ((T-100)×(T-100) / Z)÷2

[0032] If the heat amount is less than 450 (℃·h), there is not enough time to shift the equilibrium reaction shown below to the left sufficiently, and the dielectric tangent of the glass cloth does not decrease completely, which is unsuitable. The heat amount is not particularly limited as long as it is 450 (℃·h) or more, but from the viewpoint of production efficiency, 450 to 100,000 (℃·h) is preferable, and 3,000 to 100,000 (℃·h) is more preferable.

[0033] The heating may be divided into several steps during the temperature rise, temperature maintenance, and temperature fall, and the temperature may be maintained at a plurality of temperatures. Also, as long as the above-mentioned heating amount is satisfied, the maintenance time may not be necessary. The temperature rise and fall rates are not particularly limited, but from the viewpoint of productivity, 10°C / h or more is preferable, and from the viewpoint of preventing blackening of the sizing agent and strength of the quartz glass cloth, less than 200°C / h is preferable.

[0034] Regarding the heating rate, for example, when heating at temperatures above 450°C, especially above 500°C, microcracks are likely to occur in the glass filament due to thermal expansion of the filament. Therefore, a lower heating rate is more suitable for higher temperatures. Specifically, it is preferable to appropriately adjust the heating rate so that it is (℃ / h) = 100 (℃ / h) - (heating temperature (℃) - 400℃) / 6 or less. There is no particular lower limit, but from the viewpoint of productivity, it is preferable to have a rate of 5℃ / h or more. Furthermore, as long as it is within the above range, the heating may be performed in multiple steps. If heating is performed at a heating rate within this range, microcracks in the filaments due to sudden thermal expansion when the quartz glass cloth is heated can be suppressed, and breakage due to a decrease in the strength of the cloth during subsequent silane treatment or resin coating can be further suppressed.

[0035] In the heat cleaning process, MO+H 2In the reaction of O⇔M-OH (M is a metal such as Si, Al, or B), the lower the dew point and the higher the temperature, the more the equilibrium shifts to the left, and the more the metal hydroxides in the glass cloth can be reduced. However, if the generated water is not removed by adjusting the dew point, it will immediately be adsorbed into the glass cloth by hydrogen bonding, even if the metal hydroxides are reduced. Therefore, with the existing heat cleaning method using only gas furnaces or electric furnaces, moisture cannot be controlled and a large amount of metal hydroxides and especially bound water is generated. In addition, the above reaction proceeds simultaneously on the surface and inside of the glass cloth, and the metal hydroxides generated inside the glass cloth in particular cannot be reduced by post-treatment, so adjusting the dew point in heat cleaning is important. However, it is difficult to completely remove the internal metal hydroxides and bound water, and the effect of the small amount of metal hydroxides present can be countered by using a silane coupling agent described later.

[0036] As described above, the heat cleaning step may be a step of heat cleaning the glass cloth having a sizing agent attached thereto in a gas having a dew point of 15° C. or less. However, after the step of heat cleaning the glass cloth having a sizing agent attached thereto in a gas whose dew point is not adjusted, a heating step may be further included using the heating method of the heat cleaning step described above.

[0037] [Amount of metal hydroxide and bound water before silane treatment process] The amount of metal hydroxide and bound water in the glass cloth before the silane treatment step in the present invention is preferably 1,000 ppm (mass) or less, more preferably 600 ppm or less, more preferably 400 ppm or less, and even more preferably 300 ppm or less. The lower limit is not particularly limited and may be 0 ppm. By setting it in this range, the glass cloth aimed at in the present invention can be obtained more easily. If it exceeds 1,000 ppm, the influence of metal hydroxide and bound water becomes large.

[0038] The metal hydroxide and bound water in the glass cloth of the present invention can be measured as follows. Before the silane treatment process, 200g or more of glass cloth is collected and dried at 105℃ for 2 hours, then cooled to room temperature in a desiccator. After drying, the glass cloth is heated in a vacuum furnace at 1,300℃ for 2 hours, and the mass before and after heating is measured to calculate the metal hydroxide and bound water. Amount of metal hydroxide and bound water (ppm) = Mass of glass cloth after vacuum heating / Mass of glass cloth after drying x 10 6

[0039] The MO+H was heated at 1,300°C for 2 hours in a vacuum furnace where moisture had been completely removed. 2 The reaction O⇔M-OH (M is a metal such as Si, Al, or B) shifts completely to the left, and the water produced and the water bound to the metal hydroxide are completely removed from the glass cloth, allowing the amount of metal hydroxide and bound water contained in the glass cloth to be quantified. Note that while metal hydroxides can be measured by infrared spectroscopy and Si-NMR, water bound to metal hydroxides cannot be measured.

[0040] As a method for reducing the amount of metal hydroxide and bound water in the glass cloth before the silane treatment step to 1,000 ppm or less, in addition to performing heat cleaning under the above-mentioned dew point controlled conditions, it is preferable to store the heat cleaned glass cloth in a low dew point environment after the heat cleaning step and before the silane treatment step. Specifically, the storage conditions are preferably 168 hours or less in a space with a dew point of 15°C or less. The dew point is preferably 10°C or less, more preferably 5°C or less. The storage time is preferably 36 hours or less, more preferably 12 hours or less.

[0041] Methods for controlling the dew point during storage include using a room equipped with equipment for controlling temperature and humidity, such as a dehumidifier, or constantly supplying air with a dew point of 15°C or lower. The mechanism of the effect of controlling the storage conditions from after the heat cleaning process until the silane treatment process is not clear, but it may be thought of as follows, for example. When heat cleaning is performed at a low dew point, the amount of metal hydroxide is extremely reduced, but there is still a small amount of metal hydroxide and bound water on the surface. Even at room temperature, the metal hydroxide and bound water form MO+H 2 The reaction between O and M-OH (where M is a metal) proceeds gradually. Therefore, it is preferable to keep the humidity as low as possible and the time as short as possible after deoiling such as heat cleaning and before the silane treatment.

[0042] After the silane treatment process, the metal hydroxides and bound water on the surface react with the silane coupling agent, and the metal oxides and bound water present on the surface of the glass cloth are removed. In addition, the surface of the glass cloth after the silane treatment exhibits water repellency, so that the reaction of generating new metal hydroxides and bound water is extremely unlikely to occur. However, when the amount of metal hydroxides and bound water on the glass cloth before the silane treatment process exceeds 1,000 ppm, the amount of metal hydroxides and bound water on the surface also increases, so that they cannot be completely removed by the silane treatment and remain on the surface of the glass cloth, which has a negative effect on storage stability in particular. It is considered that the amount of metal hydroxides and bound water can also be reduced by increasing the amount of silane coupling agent to be treated. As will be described later, if 0.3 mass% or more of the silane coupling agent is attached, the SiOH group contained in the silane coupling agent itself becomes excessive, which has a negative effect on storage stability and frequency dependency. That is, the present invention is achieved by suppressing the metal oxides and bound water present on the glass cloth to 1,000 ppm before the silane treatment process and performing an appropriate amount of silane treatment.

[0043] [Silane treatment] The glass cloth of the present invention is obtained by surface-treating the surface of the glass cloth that has been degreased by heat cleaning with a silane coupling agent. The silane treatment liquid is not particularly limited, but from the viewpoint of productivity and environmental load, an aqueous solution in which 0.01 to 5 mass % of the silane coupling agent is dispersed is preferable, and the pH can be adjusted according to the type of silane coupling agent to be dispersed. The method of adjusting the pH is not particularly limited, but adjustment with acetic acid or ammonia is preferable according to the silane coupling agent used.

[0044] Examples of the silane coupling agent include trimethylmethoxysilane, trimethylethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, methylphenyldimethoxysilane, methylphenyldiethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, trimethoxysilane, triethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, phenylmethylvinylethoxysilane, naphthyltrimethoxysilane, naphthyltriethoxysilane, 1,4-bis(methoxydimethylsilyl)benzene, tetramethoxysilane, silane, tetraethoxysilane, n-propyltriethoxysilane, hexyltrimethoxysilane, octyltriethoxysilane, decyltrimethoxysilane, 1,6-bis(trimethoxysilyl)hexane, vinyltrimethoxysilane, vinyltriethoxysilane, p-styryltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-Epoxycyclohexyl)ethylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyldimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropyldiethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, N-(vinylbenzyl)- Examples of alkoxysilane compounds include 2-aminoethyl-3-aminopropyltrimethoxysilane and its hydrochloride, N-(vinylbenzyl)-2-aminoethyl-3-aminopropylmethyldimethoxysilane and its hydrochloride, 3-isocyanatepropyltriethoxysilane, tris-(trimethoxysilylpropyl)isocyanurate, 3-ureidopropyltriethoxysilane, 3-chloropropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, and bis(trisethoxysilylpropyl)tetrasulfide. These can be used alone or in combination of two or more. Among these, 3-aminopropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, and 3-glycidoxypropyltrimethoxysilane are preferred.

[0045] The method of applying the silane treatment solution is not particularly limited, but examples thereof include a method of impregnating glass fibers with the silane treatment solution, treatment by roll coating, etc. The method of drying the silane treatment solution is not particularly limited, but examples thereof include drying methods using hot air, infrared rays, and hot rolls.

[0046] The effects of silane coupling agents are generally known to be the increase in strength of glass cloth and the increase in affinity with resin when the resin is applied in the next process. In the present invention, it has been confirmed that the organic matter contained in the silane coupling agent has the effect of decreasing the dielectric tangent when the frequency increases, in contrast to metal hydroxides. In other words, it can counteract the increase in the dielectric tangent caused by the increase in frequency of the metal hydroxide present in a small amount inside the glass cloth. However, since the silane coupling agent itself contains SiOH groups, it is considered important to treat the metal oxide present on the surface of the glass cloth with an appropriate amount.

[0047] The amount of the silane coupling agent attached after the silane treatment is preferably more than 0 and 0.3 mass% or less, more preferably 0.01 to 0.1 mass% relative to the glass cloth. The amount of the silane coupling agent attached can be measured according to the ignition loss described in JIS R3420. By setting the amount of the silane coupling agent to 0.3 mass% or less, the increase in the dielectric tangent with frequency and time can be further suppressed. If the amount of the silane coupling agent attached is greater than the above range, the silane coupling agent becomes excessive relative to the glass cloth, and the SiOH group of the silane coupling agent, which is a metal hydroxide, is generated in excess, which may adversely affect the stability over time and the frequency dependency.

[0048] Furthermore, with regard to the amount of silane coupling agent attached after silane treatment, even if silane treatment is performed at the same concentration, the reaction amount of silane coupling agent varies depending on the amount of metal hydroxide and combined water on the surface of glass cloth. Therefore, the smaller the amount of metal hydroxide and combined water on the surface of glass cloth, the smaller the amount of silane coupling agent attached. Since the amount of metal hydroxide and combined water on the surface of glass cloth is proportional to the amount of metal hydroxide and combined water of the entire glass cloth, the amount of silane coupling agent attached to glass cloth is preferably in the range of X exceeding 0 and not more than 0.00100 in the following formula, and more preferably in the range of 0.00005 or more and not more than 0.00080. Amount of silane coupling agent attached to glass cloth (mass%) = Amount of metal hydroxide and bound water in the cloth before the silane treatment process (ppm) × Q Q is the amount of the silane coupling agent attached to the metal hydroxide and the bound water.

[0049] [Prepreg for printed circuit boards] Since the glass cloth of the present invention has high strength and excellent dielectric properties, a thinner prepreg for printed circuit boards having high strength and excellent dielectric properties can be obtained. Examples of the prepreg for printed circuit boards include a prepreg containing the above-mentioned glass cloth and an organic resin.

[0050] [Laminate] Since the glass cloth of the present invention has high strength and excellent dielectric properties, a thinner laminate having high strength and excellent dielectric properties can be obtained. Examples of the laminate include those containing the above glass cloth and an organic resin.

[0051] [Printed circuit board] The thin glass cloth of the present invention has high strength and excellent dielectric properties, so that a printed circuit board that is thinner, has high strength, and has excellent dielectric properties can be obtained. The printed circuit board can be one that contains the above-mentioned glass cloth and an organic resin. There is no particular limitation on the method for manufacturing the printed circuit board, and a general method for manufacturing a printed circuit board can be applied. As for the frequency dependence of the board, in the method described in the examples, the slope of the approximation line is 0.30×10 -5 Less than 0.05×10 is preferable. -5 Less than or equal to 0.00×10 is preferable. -5 The lower limit is not limited, and the slope may be less than 0, i.e., -1.0×10 -5 It is also possible to use the following.

[0052] The slope of the approximate line for the glass cloth substrate after 30 days of storage at 30°C and 80% RH is 0.90×10 -5 Less than 0.80×10 is preferable. -5 Less than or equal to 0.50×10 is preferable. -5The lower limit is not particularly limited, and is, for example, −1.0×10 -5 It is also possible to use the following.

[0053] The change in the slope of the approximation line of the board after storage compared to before storage was 0.50 x 10 -5 Less than 0.3×10 is preferable. -5 is more preferable, and 0.1×10 -5 The lower limit is not particularly limited, and may be, for example, 0.

[0054] The organic resin is not particularly limited, and examples thereof include cyanate ester resin, bismaleimide-cyanate ester resin, epoxy resin, polyfunctional maleimide resin, unsaturated group-containing polyphenylene ether resin, fluororesin, etc., which may be used alone or in combination of two or more. Among them, bismaleimide resin, polyfunctional maleimide resin, unsaturated group-containing polyphenylene ether resin, and fluororesin, which have low frequency dependence, are preferred. The frequency dependence of the resin is expressed by the slope of the approximate straight line of 2.50×10 -5 Less than or equal to 1.5×10 is preferable. -5 Less than 1.0×10 is preferable. -5 is more preferable. The lower limit is not limited, and the slope may be less than 0, i.e., negative. The dielectric tangent of the resin at 10 GHz is preferably 0.0025 or less, more preferably 0.020 or less, and even more preferably 0.0018 or less. The amount of organic resin used is within a known range. Inorganic fillers such as silica and milled fiber may be added to the organic resin. The slope of the approximate line representing the frequency dependence of the inorganic filler is 2.50×10 -5 Less than or equal to 1.5×10 is preferable. -5 Less than 1.0×10 is preferable. -5is more preferable. The lower limit is not limited, and the slope may be less than 0, i.e., -. The dielectric loss tangent of the inorganic filler is preferably 0.0020 or less, more preferably 0.015 or less, and even more preferably 0.0010 or less at 10 GHz. As a method for measuring the dielectric loss tangent of the inorganic filler, as described in Patent Document 6, the inorganic filler is mixed with the resin at a predetermined volume fraction, and the dielectric loss tangent of the inorganic filler is calculated from the rate of change in the dielectric loss tangent of the mixture of the resin and the inorganic filler. The amount of the organic resin or the organic resin to which the inorganic filler is added is preferably 30 to 90 mass %, more preferably 50 to 80 mass %, based on the total mass of the organic resin, the inorganic filler, and the glass cloth, from the viewpoint of sufficiently filling the inside and outside of the glass cloth with the organic resin to improve the insulation reliability. EXAMPLES

[0055] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0056] [Example 1] A fiber sizing agent (bundling agent) was prepared consisting of 3.0 mass % starch, 0.5 mass % beef tallow, 0.1 mass % polyoxyethylene lauryl ether (Emulmin-NL: manufactured by Sanyo Chemical Industries, Ltd.), and the remainder water. SiO 2 A silica glass ingot with a fiber diameter of 99.9% or more was heated and drawn to produce a silica glass fiber consisting of silica glass filaments with a diameter of 5.3 μm, and the above-mentioned fiber bundling agent was applied using an applicator (model number: LQ01A) manufactured by Shin-Etsu Engineering Co., Ltd., followed by bundling with a bundling machine and winding to produce a silica glass strand with 100 silica glass filaments. The wound silica glass strand was twisted at 24 T / m to produce a silica glass yarn.

[0057] The obtained quartz glass yarn was coated with an aqueous solution consisting of 1.5% by mass of partially saponified polyvinyl acetate and 1.5% by mass of starch as a secondary sizing agent (bundling agent), and then woven into quartz glass cloth at a weave density of IPC standard 1035 using an air jet loom. The fibers were then opened using a PSN slit nozzle manufactured by Ikeuchi Co., Ltd., with tap water at 25°C and 0.3 MPa and air compressed to 0.3 MPa, so that the air-water volume ratio was V2 / V1 = 35. The air permeability of the opened quartz glass cloth was 26.3 cm 3 / cm 2 / s. The quartz glass cloth after spreading was heat-cleaned by heating at 400°C for 72 hours in a NEMS electric furnace (model number: B80×85×200-3Z12-10) to remove the sizing agent and obtain a heat-cleaned (deoiled) quartz glass cloth. The heating rate for heat cleaning was 50°C / hour and the cooling rate was 15°C / hour. During the heating process, dry air with a dew point of -20°C, produced using a Hitachi inverter package oil-free Bebicon POD-15VNP, was fed in at 5 times the volume of the electric furnace per hour from the time of heating to the time of cooling. The heating amount, expressed as heating temperature (°C) above 100°C x heating time (h) in a vacuum or gas with a dew point of 15°C or less, is 25,500°C·h in total, as shown below. Heating amount during heating: ((400-100)×(400-100) / 50)÷2=900 Heating amount when keeping warm: (400-100)×72=21,600 Amount of heating when cooling down: ((400-100)×(400-100) / 15)÷2=3,000

[0058] The weight of the quartz glass cloth after deoiling is 26g / m 2The 1035 quartz glass cloth after heat cleaning (de-oiling) was removed from the heating furnace and stored for 24 hours in a room with a dew point of 5°C using a compressor-type dehumidifier DM-10 manufactured by Nakatomi. After that, it was immersed in an aqueous solution containing 0.2% by mass of 3-methacryloxypropyltrimethoxysilane (KBM-503, manufactured by Shin-Etsu Chemical Co., Ltd.) and 0.1% by mass of acetic acid, and dried at 110°C for 10 minutes in a constant temperature incubator DKN602 manufactured by Yamato Co., Ltd. to perform silane treatment, and a quartz glass cloth with an adhesion amount of 0.05% by mass of silane coupling agent was obtained.

[0059] [Example 2] Except for changing the concentration of the 3-methacryloxypropyltrimethoxysilane (KBM-503) aqueous solution to 0.4 mass%, the deoiled 1035 quartz glass cloth was treated in the same manner as in Example 1 to obtain a quartz glass cloth with an adhesion amount of 0.1 mass% of the silane coupling agent.

[0060] [Example 3] Except for changing the concentration of the 3-methacryloxypropyltrimethoxysilane (KBM-503) aqueous solution to 1.2 mass%, the deoiled 1035 quartz glass cloth was treated in the same manner as in Example 1 to obtain a quartz glass cloth with an adhesion amount of 0.3 mass% of the silane coupling agent.

[0061] [Example 4] The 0.2% by mass of 3-methacryloxypropyltrimethoxysilane (KBM-503, Shin-Etsu Chemical Co., Ltd.) was changed to an aqueous solution in which 0.1% by mass of 3-aminopropyltrimethoxysilane (KBM-903, Shin-Etsu Chemical Co., Ltd.) was dispersed, and the deoiled 1035 quartz glass cloth was treated in the same manner as in Example 1 to obtain a quartz glass cloth with an adhesion amount of 0.05% by mass of silane coupling agent.

[0062] [Example 5] The 0.2% by mass of 3-methacryloxypropyltrimethoxysilane (KBM-503, Shin-Etsu Chemical Co., Ltd.) was replaced with an aqueous solution containing 0.1% by mass of 3-glycidoxypropyltrimethoxysilane (KBM-403, Shin-Etsu Chemical Co., Ltd.), and the deoiled 1035 quartz glass cloth was treated in the same manner as in Example 1 to obtain a quartz glass cloth with a silane coupling agent adhesion amount of 0.05% by mass.

[0063] [Example 6] The 1035 quartz glass cloth after fiber spreading obtained in Example 1 was heat-cleaned by heating at 500°C for 48 hours in a NEMS electric furnace (model number: B80×85×200-3Z12-10) to remove the sizing agent and obtain a deoiled quartz glass cloth. During this process, the heat treatment was carried out by feeding 10 times the volume of the electric furnace per hour of dry air with a dew point of -70°C produced by a CKD Corporation Super Heatless Dryer SHD3025 from the time of temperature rise to the time of temperature fall. The heat cleaning was performed at a temperature rise rate of 50°C / hour and a temperature fall rate of 15°C / hour (heating amount 26,133°C·h). The basis weight of the deoiled quartz glass cloth was 26 g / m 2 The deoiled quartz glass cloth was removed from the heating furnace and stored for 24 hours in a room with a dew point of 5°C using a compressor-type dehumidifier DM-10 manufactured by Nakatomi. The quartz glass cloth was then immersed in an aqueous solution containing 0.2% by mass of KBM-503 and 0.1% by mass of acetic acid, and dried at 110°C for 10 minutes in a constant temperature incubator DKN602 manufactured by Yamato Co., Ltd. to perform silane treatment, thereby obtaining a quartz glass cloth with an adhesion amount of 0.03% by mass of silane coupling agent.

[0064] [Example 7] The 1035 quartz glass cloth after fiber spreading obtained in Example 1 was heat-cleaned by heating at 700°C for 10 hours in a NEMS electric furnace (model number: B80×85×200-3Z12-10) to remove the sizing agent and obtain a deoiled quartz glass cloth. In this case, the heat treatment was performed by feeding 10 times the volume of the electric furnace per hour of dry air with a dew point of -70°C produced by a CKD Corporation Super Heatless Dryer SHD3025 from the time of temperature increase to the time of temperature decrease. The heat cleaning was performed at a temperature increase rate of 25°C / hour and a temperature decrease rate of 15°C / hour (heating amount 25,200°C·h). The basis weight of the deoiled quartz glass cloth was 26g / m 2 The 1035 quartz glass cloth after deoiling was removed from the heating furnace and stored for 24 hours in a room with a dew point of 5°C using a compressor-type dehumidifier DM-10 manufactured by Nakatomi Co., Ltd. Then, the quartz glass cloth was immersed in an aqueous solution in which 0.2% by mass of KBM-503 and 0.1% by mass of acetic acid were dispersed, and the cloth was dried at 110°C for 10 minutes in a constant temperature incubator DKN602 manufactured by Yamato Co., Ltd. to perform silane treatment, and a quartz glass cloth with an adhesion amount of 0.02% by mass of silane coupling agent was obtained.

[0065] [Example 8] A fiber sizing agent was prepared, which consisted of 3.0 mass % starch, 0.5 mass % beef tallow, 0.1 mass % emulsifier, and the remainder water. SiO 2 74% by mass, B 2 O 3 is 22% by mass, K 2 O 1.5 mass%, Na 2 O is 1.5 mass%, Al 2 O 3 A D-glass ingot containing 0.5% by mass of ZnO and 0.5% by mass of CaO was heated and drawn to produce a D-glass fiber consisting of D-glass filaments with a diameter of 3.5 μm, and the above-mentioned fiber sizing agent was applied using an applicator (model number: LQ01A) manufactured by Shin-Etsu Engineering Co., Ltd., followed by bundling with a bundling machine and winding to produce a D-glass strand containing 100 D-glass filaments. The wound D-glass strand was twisted at 24 T / m to produce a D-glass yarn. The obtained D-glass yarn was coated with an aqueous solution consisting of 1.5% by mass of partially saponified polyvinyl acetate and 1.5% by mass of starch as a secondary bundling agent, and then an air jet loom was used to weave D-glass cloth at a weave density of IPC standard 1035. Using a PSN slit nozzle manufactured by Ikeuchi Co., Ltd., the yarn was opened using tap water at 25°C and 0.3 MPa and air compressed to 0.3 MPa so that the air-water volume ratio was V2 / V1 = 35. The air permeability of the opened D-glass cloth was 30.2 cm. 3 / cm 2 / s. After weaving, the D-glass cloth was heat-cleaned by heating at 700°C for 10 hours in a Nemus electric furnace (model number: B80×85×200-3Z12-10) to remove the sizing agent and obtain a deoiled quartz glass cloth. During this process, dry air with a dew point of -70°C, produced by a CKD Corporation Super Heatless Dryer SHD3025, was fed in at 10 times the volume of the electric furnace per hour from the time the temperature was increased to the time it was decreased. The heating rate for heat cleaning was 25°C / hour and the temperature decrease rate was 15°C / hour (heating amount 25,200°C·h). The basis weight of the deoiled D-glass cloth was 25g / m 2 It was.

[0066] The deoiled D-glass cloth was removed from the heating furnace and stored for 24 hours in a room with a dew point of 5°C using a compressor-type dehumidifier DM-10 manufactured by Nakatomi. The D-glass cloth was then immersed in an aqueous solution containing 0.2% by mass of KBM-503 and 0.1% by mass of acetic acid, and dried at 110°C for 10 minutes in a constant temperature incubator DKN602 manufactured by Yamato Co., Ltd., to perform silane treatment, thereby obtaining a D-glass cloth with an adhesion amount of 0.07% by mass of silane coupling agent. The silane treatment was also performed in a room with a dew point of 10°C, and the time during which the dew point exceeded 15°C from the time of deoiling until the time of silane treatment was 0 hours.

[0067] [Example 9] The deoiled 1035 quartz glass cloth obtained in Example 1 was removed from the heating furnace and stored for 168 hours in a room with a dew point of 15°C, using a compressor-type dehumidifier DM-10 manufactured by Nakatomi Co., Ltd. Then, it was immersed in an aqueous solution containing 0.2% by mass of KBM-503 and 0.1% by mass of acetic acid, and dried at 110°C for 10 minutes in a constant temperature incubator DKN602 manufactured by Yamato Co., Ltd. to perform silane treatment, and a quartz glass cloth with an adhesion amount of 0.07% by mass of silane coupling agent was obtained.

[0068] [Comparative Example 1] The dielectric loss tangent of the deoiled 1035 quartz glass cloth obtained in Example 1 was measured immediately without being subjected to a silane treatment.

[0069] [Comparative Example 2] The deoiled 1035 quartz glass cloth obtained in Example 1 was removed from the heating furnace and stored for 240 hours in a room with a dew point of 15°C using a compressor-type dehumidifier DM-10 manufactured by Nakatomi Co., Ltd. Then, it was immersed in an aqueous solution containing 0.2% by mass of 3-methacryloxypropyltrimethoxysilane (KBM-503) and 0.1% by mass of acetic acid, and dried at 110°C for 10 minutes in a constant temperature incubator DKN602 manufactured by Yamato Co., Ltd. to perform silane treatment, thereby obtaining a quartz glass cloth with an adhesion amount of 0.07% by mass of silane coupling agent.

[0070] 1. Amount of metal hydroxide and bound water 200 g of glass cloth before the silane treatment process obtained in the examples and comparative examples was collected and dried at 105°C for 2 hours in a Yamato constant temperature incubator DKN602, and then cooled in a desiccator. The dried glass cloth was heated at 1,300°C for 2 hours in a vacuum heating and baking furnace VASTA. The vacuum state was maintained from the time the temperature was increased to the time the temperature was decreased. Amount of metal hydroxide and bound water (ppm) = Mass of glass cloth after vacuum heating / Mass of glass cloth after drying x 10 6

[0071] 2. Dew point measurement The dew point was measured using a dew point monitor MG-40 manufactured by Orion Co., Ltd. However, since the dew point during heating cannot be measured, when dry air is introduced into the heating furnace, the dew point inside the furnace is the dew point of the dry air, and when dry air is not introduced, the average dew point of the outside air where the heating furnace is located every 12 hours is used as the dew point.

[0072] 3. Amount of silane coupling agent attached The measurement was carried out by heating at 625°C for 2 hours according to the ignition loss method specified in JIS R3420.

[0073] 4. Amount of adhesion relative to the amount of metal hydroxide and bound water Amount of adhesion relative to the amount of metal hydroxide and bound water = [Amount of silane coupling agent adhered to glass cloth (mass%)] / [Amount of metal hydroxide and bound water in cloth before silane treatment process (ppm)]

[0074] 5. Measurement of dielectric tangent The obtained glass cloth was dried at 105°C for 2 hours in a constant temperature incubator DKN602 manufactured by Yamato Co., Ltd., and then cooled in a desiccator. The dielectric loss tangent at 10 GHz, 28 GHz, and 40 GHz was then measured using a cavity resonator (TE011 mode) manufactured by AET Co., Ltd. The thickness of the glass cloth was measured using the theoretical film thickness. Theoretical film thickness t (μm) = Area weight (g / m 2 ) / specific gravity (g / cm 3 ) Calculated from.

[0075] 6.Slope of the approximation line A graph was created with the dielectric tangent measured in step 1 on the vertical axis and frequency on the horizontal axis, and an approximation line was obtained as shown in Figure 1, and the slope of the graph was calculated.

[0076] 7. Dielectric tangent and rate of change of dielectric tangent after storage The glass cloth measured in 1 was left to stand for 30 days in an Espec small environmental tester (SH-222) under conditions of 30°C and 80%, then dried again at 105°C for 2 hours and allowed to cool in a desiccator, after which the dielectric tangent at 10 Hz was measured in the same manner as in 1. The rate of change is expressed as (dielectric tangent after storage) / (dielectric tangent before storage).

[0077] 8.Slope of the approximate line of the substrate (frequency dependence) and the amount of change in the approximate line The cloth treated with a silane coupling agent before storage and the cloth treated with a silane coupling agent after storage for 30 days under conditions of 30 ° C and 80% in the same manner as in 7 above were immersed in a toluene solution containing 55 mass % of bismaleimide resin: SLK-3000 (trade name manufactured by Shin-Etsu Chemical Co., Ltd.) and 2 mass % of radical initiator: Percumyl D (NOF Corporation), and dried at 110 ° C for 10 minutes to form a prepreg. Three layers of prepreg were stacked and cured at 180 ° C for 1 hour at 0.5 MPa using a vacuum press to obtain a substrate. The dielectric loss tangent of the obtained substrate was measured using a cavity resonator (TE011 mode) manufactured by AET Co., Ltd., and the frequency dependency was measured in the same manner as in 6 above. The change in the slope of the approximation line of the substrate using the cloth before and after 30 days of storage was 0.5 × 10 -5 The following items were deemed to have passed the test.

[0078] [Table 1]

[0079] [Table 2]

[0080] KBM-503: 3-Methacryloxypropyltrimethoxysilane KBM-903: 3-Aminopropyltrimethoxysilane KBM-403: 3-Glycidoxypropyltrimethoxysilane

[0081] The substrate of the embodiment was boiled at 100°C for 2 hours, the surface moisture was wiped off, and the substrate was submerged in a solder bath heated to 260°C for 30 seconds, and then submerged in a cooling agent of -78°C consisting of acetone and dry ice for 30 seconds. Three sets of submersion in a solder bath at 260°C and acetone at 78°C were performed. There was no peeling between the glass cloth and the resin of the substrate of the embodiment. From these results, it was confirmed that the substrate of the embodiment was highly reliable.

[0082] As can be seen from Tables 1 and 2, when the glass cloth of the examples was stored for 30 days under conditions of 30°C and 80% RH, the rate of change in the dielectric tangent at 10 GHz compared to before storage was low, the dielectric tangent was low at high frequencies, and the frequency dependency of the dielectric tangent was low, and as described above, a substrate with excellent reliability could be produced. In Comparative Example 1, since no silane treatment was performed, the initial value of the dielectric tangent at 10 GHz was excellent, but the rate of change was high and the frequency dependency was large. In Comparative Example 2, the rate of change was high, the slope of the approximation line was steep, and the frequency dependency was large.

[0083] The substrate using the glass cloth of the present invention has a remarkable effect of stably suppressing transmission loss at any frequency in high-speed communications such as 5G, which will increase in the future. The present invention is not limited to the above embodiment. The above embodiment is an example, and any one that has substantially the same configuration as the technical idea described in the claims of the present invention and has the same action and effect is included in the technical scope of the present invention.

Claims

1. A glass cloth treated with a silane coupling agent, which, when stored for 30 days under conditions of 30°C and 80% RH, has a rate of change in dielectric tangent at 10 GHz after storage relative to before storage, as measured by a cavity resonator method, of 1.5 or less.

2. When the dielectric loss tangents at 10 GHz, 28 GHz, and 40 GHz are plotted on the vertical axis and the frequency on the horizontal axis, the gradient of the approximation line connecting the dielectric loss tangents at each frequency is 2.00×10 -5 The glass cloth according to claim 1, wherein

3. The slope of the approximate line after saving is 2.5 x 10 -5 The glass cloth according to claim 2, wherein:

4. The change in the slope of the approximation line after storage compared to before storage is 0.4 × 10 -5 The glass cloth according to claim 2, wherein:

5. 2. The glass cloth according to claim 1, which has a dielectric loss tangent of 0.0010 or less at 10 GHz.

6. SiO 2 The glass cloth according to claim 1, wherein the glass cloth has a content of 70% by mass or more.

7. SiO 2 The glass cloth according to claim 6, wherein the glass cloth has a content of 95 mass % or more.

8. A prepreg comprising the glass cloth according to any one of claims 1 to 7 and an organic resin.

9. A laminate comprising the glass cloth according to any one of claims 1 to 7 and an organic resin.

10. A printed wiring board comprising the glass cloth according to any one of claims 1 to 7 and an organic resin.

11. A method for producing a silane-treated glass cloth, comprising: a step of heat-cleaning a glass cloth having a sizing agent attached thereto in a gas having a dew point of 15° C. or less; and a silane treatment step of treating the heat-cleaned glass cloth with a silane coupling agent, A method for producing a silane-treated glass cloth, in which the amount of metal hydroxide and bound water in the glass cloth before the silane treatment step is 1,000 ppm or less.

Citation Information

Patent Citations

  • Glass fiber for fiber reinforced plastics and fiber reinforced plastic product

    JP1993170483A

  • Resin substrate having dielectric property with less frequency dependence

    JP2022131074A

  • Method for producing quartz glass fiber, quartz glass strand, quartz glass yarn and quartz glass cloth

    JP2006282401A

  • Heat transfer prepreg and method for producing the same and heat transfer printed circuit board using the same

    JP2009019150A

  • Prepreg comprising thin layer quartz glass cloth, and wiring plate using the same

    JP2009263569A