Shield gas for copper material welding
The use of a helium and argon gas mixture in a double nozzle TIG welding torch for copper materials enhances penetration and minimizes weld burn, addressing the need for effective shielding gases in copper welding.
Patent Information
- Application Number
- JP2023063705
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2024-10-23
AI Technical Summary
Existing welding technologies lack a suitable shielding gas for copper materials that can achieve good penetration while minimizing weld burn during the welding process.
A shielding gas composition for copper materials comprising helium gas in a specific range (5-75% by volume) and argon gas as the remainder, used in a double nozzle TIG welding torch, enhances arc energy and thermal conductivity to improve penetration and suppress weld burn.
The proposed shielding gas achieves improved penetration and reduces weld burn during copper material welding, ensuring efficient and stable welding outcomes.
Smart Images

Figure 2024150336000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a shielding gas for copper welding. [Background technology]
[0002] A known TIG (Tungsten Inert Gas) welding torch includes a tungsten electrode, a first nozzle forming a first gas flow passage surrounding the tungsten electrode, and a second nozzle forming a second gas flow passage surrounding the first nozzle. Patent Document 1 discloses that when welding ferritic stainless steel using a torch having such a double nozzle structure, a mixed gas of argon gas and helium gas is used as a shielding gas flowing through the first gas flow passage. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2013-86136 A Summary of the Invention [Problem to be solved by the invention]
[0004] In welding using a torch with a double nozzle structure as described above, a shielding gas suitable for welding copper materials is desired. [Means for solving the problem]
[0005] The present disclosure has been made in consideration of the above, and has as one object to provide a shielding gas for copper welding that can obtain good penetration while suppressing weld burns when welding copper materials. Effect of the Invention
[0006] According to the shielding gas of the present disclosure, when welding copper materials, good penetration can be obtained while suppressing weld burns. [Brief description of the drawings]
[0007] [Figure 1] FIG. 2 is a schematic cross-sectional view showing an example of a tip portion of a torch. [Diagram 2] 1 is a flowchart showing each step in a welding method for copper materials. [Diagram 3] FIG. 2 is a schematic diagram showing a sample used in the examples. [Figure 4] FIG. 13 is a diagram showing an example of a state in which a molten pool formed in a sample has solidified. [Diagram 5] FIG. 13 is a diagram showing an example of a sample with a weld burn score of 4. [Figure 6] FIG. 13 is a diagram showing an example of a sample with a weld burn score of 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] [Overview of the embodiment] First, the embodiments of the present disclosure will be described. The shielding gas for copper welding according to the present disclosure is a shielding gas for copper welding used for welding a base metal made of copper as one or both of a first shielding gas flowing through a first gas flow passage surrounding a tungsten electrode and a second shielding gas flowing through a second gas flow passage surrounding the first gas flow passage. The shielding gas for copper welding contains 5% by volume or more and 75% by volume or less of helium gas, and the remainder is substantially composed of argon gas.
[0009] During welding, a potential difference is formed between the tungsten electrode and the base material while the first and second shielding gases are discharged from the torch. An arc is generated between the tungsten electrode and the base material due to the potential difference between the tungsten electrode and the base material. A part of the first shielding gas and a part of the second shielding gas discharged from the torch are ionized by the heat of the arc. The ionized shielding gas becomes a conductor of the arc. Here, helium gas has a higher electrical resistance than that of argon gas. Therefore, by using the above-mentioned copper welding shielding gas as one or both of the first and second shielding gases, the energy of the arc becomes higher due to the electrical resistance of helium gas compared to the case where argon gas is used. As a result, good penetration is obtained. And, helium gas has a higher thermal conductivity than that of argon gas. Therefore, by using the above-mentioned copper welding shielding gas as one or both of the first and second shielding gases, the base material is cooled more efficiently by helium gas compared to the case where argon gas is used. This prevents welding burns caused by oxidation of the base material, and thus allows good penetration when welding copper materials while preventing welding burns.
[0010] In the above-mentioned copper welding shielding gas, the copper may be oxygen-free copper. The copper welding shielding gas is also suitable for welding oxygen-free copper.
[0011] The above-mentioned shielding gas for copper welding may be used as a first shielding gas, and may contain 5% by volume or more and 20% by volume or less of helium gas, with the remainder being substantially argon gas. The first shielding gas is discharged from the torch closer to the arc than the second shielding gas. Therefore, the first shielding gas is more likely to contribute to penetration than the second shielding gas. By using the shielding gas for copper welding as the first shielding gas, the efficiency of penetration by the helium gas is improved. Even if the content of helium gas in the shielding gas for copper welding used as the first shielding gas is set to 20% by volume or less, sufficient penetration can be obtained. In addition, by setting the content of helium gas in the shielding gas for copper welding used as the first shielding gas to 20% by volume or less, welding burns due to the heat of the arc are suppressed while sufficient penetration is obtained. As a result, when welding copper materials, good penetration can be efficiently obtained while suppressing welding burns.
[0012] The above-mentioned copper welding shielding gas may be used as a second shielding gas, and may contain 10% by volume or more and 75% by volume or less of helium gas, with the remainder being substantially argon gas. The second shielding gas is discharged from the torch farther from the arc than the first shielding gas. Therefore, the second shielding gas is less affected by the arc than the first shielding gas. By using the copper welding shielding gas as the second shielding gas, the cooling efficiency of the base material by the helium gas is improved. By setting the content of helium gas in the copper welding shielding gas used as the second shielding gas to 10% by volume or more, better penetration can be obtained. In addition, by setting the content of helium gas in the copper welding shielding gas used as the second shielding gas to 10% by volume or more, welding burns are suppressed by the improvement in the cooling efficiency of the base material. As a result, when welding copper materials, better penetration can be obtained while suppressing welding burns.
[0013] The above-mentioned shielding gas for copper welding may be used as a second shielding gas, and may contain 20% by volume or more and 50% by volume or less of helium gas, with the remainder being substantially argon gas. By setting the helium gas content in the shielding gas for copper welding used as the second shielding gas to 20% by volume or more, better penetration can be obtained. The helium gas in the second shielding gas may be mixed into the first shielding gas. The amount of penetration by the first shielding gas changes depending on the amount of helium gas mixed from the second shielding gas into the first shielding gas. By setting the helium gas content in the shielding gas for copper welding used as the second shielding gas to 50% by volume or less, the change in the amount of penetration when helium gas is mixed from the second shielding gas into the first shielding gas is suppressed. This makes it possible to obtain better penetration more stably when welding copper materials.
[0014] [Specific Example of the Embodiment] Next, an example of a specific embodiment of a torch used for welding copper materials and a copper welding shielding gas of the present disclosure will be described with reference to the drawings. In the following drawings, the same or corresponding parts are given the same reference numerals and the description thereof will not be repeated.
[0015] [Torch structure] Fig. 1 is a schematic cross-sectional view showing an example of a tip portion of a torch 1. Referring to Fig. 1, torch 1 includes a tungsten electrode 10, a first nozzle 11, and a second nozzle 12. Torch 1 is a TIG welding torch, and is a torch having a so-called double nozzle structure.
[0016] The tungsten electrode 10 is formed, for example, in a rod shape. The tungsten electrode 10 includes a cylindrical outer peripheral surface 100 having a central axis along the longitudinal direction of the tungsten electrode 10, and a tip portion 101 connected to the outer peripheral surface 100 and having a tapered shape. The tungsten electrode 10 and the base material 9 are connected to a power source (not shown). The tungsten electrode 10 is made of a tungsten material containing, for example, about 2% cerium oxide as a dopant for increasing the electron emission rate.
[0017] The first nozzle 11 includes a cylindrical first inner peripheral surface 110 facing the outer peripheral surface 100 of the tungsten electrode 10, and a cylindrical first outer peripheral surface 111 arranged concentrically with the first inner peripheral surface 110. A first gas flow path P1 is formed between the first inner peripheral surface 110 and the tungsten electrode 10. That is, the first nozzle 11 forms a first gas flow path P1 surrounding the tungsten electrode 10. A first shielding gas (inner shielding gas) flows through the first gas flow path P1. The first shielding gas is discharged from an opening at the tip of the first nozzle 11. The dashed arrow in FIG. 1 conceptually indicates the direction in which the first shielding gas flows.
[0018] The second nozzle 12 includes a cylindrical second inner peripheral surface 120 facing the first outer peripheral surface 111 of the first nozzle 11, and a cylindrical second outer peripheral surface 121 arranged concentrically with the second inner peripheral surface 120. A second gas flow path P2 is formed between the second inner peripheral surface 120 and the first nozzle 11. That is, the second nozzle 12 forms a second gas flow path P2 surrounding the first gas flow path P1. A second shielding gas (outer shielding gas) flows through the second gas flow path P2. The second shielding gas is discharged from an opening at the tip of the second nozzle 12. The dashed arrow in FIG. 1 conceptually indicates the direction in which the second shielding gas flows.
[0019] The base material 9 is made of, for example, a copper material. The copper material is, for example, pure copper, oxygen-free copper, tough pitch copper, etc. Pure copper is a copper material with a copper purity of 99.99% or more, for example, C1011 specified in JIS H 3510. Oxygen-free copper is a copper material with a copper purity of 99.96% or more, for example, C1020 specified in JIS H 3100. Tough pitch copper is a copper material with a copper purity of 99.90% or more, for example, C1100 specified in JIS H 3100.
[0020] When the base material 9 is a copper material, a shielding gas for copper welding is used as one or both of the first and second shielding gases, which contains 5% by volume to 75% by volume of helium gas and the remainder is substantially argon gas. "The remainder is substantially argon gas" means that the remainder of the shielding gas for copper welding contains only unavoidable impurities in addition to argon gas. "Avoidable impurities" are impurities that are present in raw materials or that are inevitably mixed in during the manufacturing process, and are essentially unnecessary but difficult to completely remove, and are tolerated as unavoidable. The content of the unavoidable impurities is preferably 0.1% by volume or less. In addition, the content of water as an unavoidable impurity is preferably 80 ppm by volume or less.
[0021] When used as a first shielding gas, the shielding gas for copper welding may contain 5 volume % or more and 20 volume % or less of helium gas, with the remainder being substantially argon gas. When used as a second shielding gas, the shielding gas for copper welding may contain 10 volume % or more and 75 volume % or less of helium gas, with the remainder being substantially argon gas. When used as a second shielding gas, the shielding gas for copper welding preferably contains 20 volume % or more and 50 volume % or less of helium gas, with the remainder being substantially argon gas.
[0022] [Method of welding copper materials] Fig. 2 is a flow chart showing each step in the method for welding copper materials. Next, a welding method for welding a pair of base materials 9 made of copper materials (a method for welding copper materials) using the torch 1 described above will be described with reference to Figs. 1 and 2.
[0023] The method for welding copper materials includes the steps of: preparing a pair of base materials 9 to be joined (ST1); forming a molten pool across the pair of base materials 9 by forming an arc between the tungsten electrode 10 of the torch 1 and the base material 9 while releasing a first shielding gas and a second shielding gas from the torch 1 (ST2); melting the base material 9 along the boundary line between the base materials 9 by moving the torch 1 along the boundary line while releasing the first shielding gas and the second shielding gas from the torch 1 toward the molten pool (ST3); and solidifying the molten base material 9 along the boundary line (ST4).
[0024] In step ST2, a potential difference is formed between the tungsten electrode 10 and the base material 9. Due to the potential difference between the tungsten electrode 10 and the base material 9, an arc is generated between the tungsten electrode 10 and the base material 9. In steps ST2 and ST3, the base material 9 is melted by the heat of the arc. In addition, a part of the first shielding gas and a part of the second shielding gas are ionized by the heat of the arc. The ionized shielding gas becomes a conductor of the arc.
[0025] The above-mentioned shielding gas for copper welding is used as one or both of the first and second shielding gases. For example, the first and second shielding gases are discharged from the torch 1 at a flow rate of 0.2 L / min or less and 20.0 L / min or more. In step ST3, the torch 1 may be moved while swinging so as to cross the direction in which the weld line extends, that is, so-called weaving may be performed. Also, a filler metal made of, for example, copper or a copper alloy may be used.
[0026] Next, the shielding gas for copper welding according to the present disclosure will be described in more detail with reference to examples, but the present disclosure should not be construed as being limited to the descriptions of these examples.
[0027] [Evaluation test 1] FIG. 3 is a schematic diagram showing sample S used in the examples. FIG. 4 is a diagram showing an example of a state in which the molten pool WP formed in sample S has solidified. FIG. 5 is a diagram showing an example of sample S with a weld burn score of 4. FIG. 6 is a diagram showing an example of sample S with a weld burn score of 1. In FIGS. 3 to 6, the X direction indicates the length direction of the base material 90. The Y direction indicates the thickness direction of the base material 90. The Z direction indicates the width direction of the base material 90. FIGS. 5 and 6 show sample S viewed from the upper edge 91 side of the base material 90 in the thickness direction (Y direction) of the base material 90. In FIGS. 5 and 5, the upper edge 91 of the base material 90 faces downward in the figures. In FIGS. 5 and 6, a scale is shown for comparison along with sample S to help understand the degree of burning of the base material 90 in sample S.
[0028] In order to evaluate the penetration amount and weld burn when welding was performed, a sample S was prepared according to the above-mentioned copper welding method. Specifically, as shown in FIG. 3, a tip of a torch 1 was directed toward an upper edge 91 of a plate-shaped base material 90 made of oxygen-free copper, and a molten pool WP was formed at a corner of the base material 90. The formed molten pool WP was solidified to prepare a sample S. The base material 90 has a plate thickness T of 5 mm. A gas containing 0% to 75% by volume of helium gas and the remainder substantially consisting of argon gas was used as the first shielding gas (inner shielding gas). A gas containing 90% to 100% by volume of argon gas was used as the second shielding gas (outer shielding gas). A welder A350P manufactured by Daihen Corporation was used as the welding machine.
[0029] The penetration amount and weld burn were evaluated for the sample S prepared under the above conditions. With reference to FIG. 4, the penetration amount is the product of the depth D, the length L, and the width W of the molten pool WP solidified in the base metal 90 multiplied by the depth L and the width W. The weld burn is the degree of burning (degree of oxidation) of the base metal 90, and was visually judged comprehensively by three evaluators. As the score of the weld burn, as shown in FIG. 5, the sample S in which the base metal 90 was less burned was given a score of "4". The degree of burning of the base metal 90 with a weld burn score of 4 is equivalent to the degree of burning of the base metal 90 when the sample S was prepared using argon gas as both the first shielding gas and the second shielding gas. The sample S in which the degree of burning of the base metal 90 was greater than that with a weld burn score of "4" was given a score of "3" and the sample S in which the degree of burning of the base metal 90 was greater than that with a weld burn score of "2", and the sample S in which the degree of burning of the base metal 90 was conspicuous was given a score of "1" as shown in FIG. 6.
[0030] Table 1 shows the results of evaluation test 1. From the left, Table 1 shows the content (volume %) of argon gas in the first shielding gas, the content (volume %) of helium gas in the first shielding gas, the content (volume %) of argon gas in the second shielding gas, the content (volume %) of helium gas in the second shielding gas, the number of samples S prepared using the first shielding gas and the second shielding gas having the compositions on the left, and the average amount of penetration (mm 3 ) and the average weld burn score for the sample group consisting of the number of samples S shown on the left. Note that "-" in the table indicates that the target gas was not included.
[0031] [Table 1]
[0032] <Evaluation results of penetration amount> As shown in Table 1, when a gas containing 100% argon gas by volume was used as the first shielding gas, the penetration was 10.4 mm 3In contrast, when the first shielding gas contained 5% to 75% by volume of helium gas and the remainder was essentially argon gas, the penetration was 12.5 mm 3 Over 120.0mm 3 Among these, when a gas containing more than 10% by volume and not more than 75% by volume of helium gas and the remainder being substantially argon gas was used, the penetration amount was 21.7 mm 3 Over 120.0mm 3 Among these, when a gas containing more than 15% by volume and not more than 75% by volume of helium gas and the remainder being substantially argon gas was used, the penetration amount was 27.2 mm 3 Over 120.0mm 3 It was less and even better.
[0033] <Weld burn evaluation results> As shown in Table 1, when a gas containing 50 volume % or more and 75 volume % or less of helium gas with the remainder consisting essentially of argon gas was used as the first shielding gas, the weld burn score was always 2. In contrast, when a gas containing 10 volume % or more and 20 volume % or less of helium gas with the remainder consisting essentially of argon gas was used as the first shielding gas, the weld burn score was always 3, which was excellent. Also, when a gas containing 5 volume % or more and less than 10 volume % of helium gas with the remainder consisting essentially of argon gas was used as the first shielding gas, the weld burn score was 4, which was excellent.
[0034] <Overall rating> When a gas containing 5% to 20% by volume of helium gas and the remainder substantially consisting of argon gas was used as the first shielding gas, both the penetration amount and the weld burn score were excellent. Among these, when a gas containing more than 10% to 20% by volume of helium gas and the remainder substantially consisting of argon gas was used, the penetration amount was even better. Among these, when a gas containing 20% by volume of helium gas (more than 15% to 20% by volume) and the remainder substantially consisting of argon gas was used, the penetration amount was the best.
[0035] [Evaluation test 2] Sample S was prepared according to the above-mentioned copper welding method for the purpose of evaluating the amount of penetration and weld burn when welding was performed. In evaluation test 2, a gas containing 90% by volume or more and 100% by volume or less of argon gas was used as the first shielding gas (inner shielding gas). A gas containing 0% by volume or more and 75% by volume or less of helium gas, with the remainder being essentially argon gas, was used as the second shielding gas (outer shielding gas). The other preparation conditions and evaluation target of sample S were the same as those of evaluation test 1 above.
[0036] Table 2 shows the results of evaluation test 2. Table 2 shows, from the left, the content (volume %) of argon gas in the first shielding gas, the content (volume %) of helium gas in the first shielding gas, the content (volume %) of argon gas in the second shielding gas, the content (volume %) of helium gas in the second shielding gas, the number of samples S prepared using the first shielding gas and the second shielding gas having the compositions on the left, and the average amount of penetration (mm 3 ), the average weld burn score for the sample group consisting of the number of samples S shown on the left, and the standard deviation of the penetration amount for the sample group consisting of the number of samples shown on the left. Note that "-" in the table indicates that the target gas is not included. The standard deviation value is calculated as the square root of the unbiased variance.
[0037] [Table 2]
[0038] <Evaluation results of penetration amount> As shown in Table 2, when a gas containing 100% argon gas by volume was used as the second shielding gas, the penetration was 10.4 mm 3 Over 12.9mm 3 In contrast, when the second shielding gas contained 10% to 75% by volume of helium gas and the remainder was essentially argon gas, the penetration was 19.4 mm 3 Over 50.0mm 3 Among these, when a gas containing 20% by volume or more and 75% by volume or less of helium gas and the remainder being substantially argon gas was used, the penetration amount was 25.0 mm 3 Over 50.0mm 3 It was less and even better.
[0039] As shown in Table 2, when a gas containing 75 volume % helium gas and the remainder essentially consisting of argon gas was used as the second shielding gas, the standard deviation of the penetration amount was 11.96. In contrast, when a gas containing 50 volume % or less helium gas and the remainder essentially consisting of argon gas was used as the second shielding gas, the standard deviation of the penetration amount was 5.85 or less, and the change in the penetration amount was suppressed.
[0040] <Weld burn evaluation results> As shown in Table 2, when a gas containing 100% by volume of argon gas was used as the second shielding gas, the weld burn score was 3 or 4. When a gas containing 10% by volume of helium gas and the remainder essentially consisting of argon gas was used as the second shielding gas, the weld burn score was 3. When a gas containing 50% by volume or more and 75% by volume or less of helium gas and the remainder essentially consisting of argon gas was used as the second shielding gas, the weld burn score was 3 in all cases. When a gas containing 20% by volume of helium gas, which is more than 10% by volume and less than 50% by volume, and the remainder essentially consisting of argon gas was used as the second shielding gas, the weld burn score was 4.
[0041] <Overall rating> When a gas containing 10% by volume or more and 75% by volume or less of helium gas and the remainder substantially consisting of argon gas was used as the second shielding gas, the amount of penetration was superior compared to when a gas containing 100% by volume of argon gas was used. Among these, when a gas containing 20% by volume or more and 75% by volume or less of helium gas and the remainder substantially consisting of argon gas was used as the second shielding gas, the amount of penetration was even superior. In addition, when a gas containing 10% by volume or more and 75% by volume or less of helium gas and the remainder substantially consisting of argon gas was used as the second shielding gas, the weld burn score was equivalent compared to when a gas containing 100% by volume of argon gas was used. Among these, when a gas containing 20% by volume of helium gas (more than 10% by volume and less than 50% by volume) and the remainder substantially consisting of argon gas was used, the weld burn score was the best. In other words, when a gas containing 10 volume % or more and 75 volume % or less of helium gas, with the remainder essentially consisting of argon gas, was used as the second shielding gas, the penetration amount was superior while the weld burn score was the same compared to when a gas containing 100 volume % of argon gas was used.
[0042] When a gas containing 50 volume % or less of helium gas and the remainder substantially consisting of argon gas was used as the second shielding gas, the penetration amount was more stably obtained. That is, when a gas containing 20 volume % or more and 50 volume % or less of helium gas and the remainder substantially consisting of argon gas was used as the second shielding gas, an even better penetration amount was more stably obtained.
[0043] It should be understood that the embodiments and examples disclosed herein are illustrative in all respects and are not limiting in any respect. The scope of the present invention is defined by the claims, not the above description, and is intended to include all modifications within the meaning and scope of the claims. [Explanation of symbols]
[0044] 1 torch, 10 tungsten electrode, 11 first nozzle, 12 second nozzle, 100 outer peripheral surface, 101 tip, 110 first inner peripheral surface, 111 first outer peripheral surface, 120 second inner peripheral surface, 121 second outer peripheral surface, 9 base material, 90 base material, 91 upper edge, D depth, L depth, width W, T plate thickness, S sample, WP molten pool
Claims
1. A copper welding shielding gas used for welding a base metal made of copper, wherein one or both of a first shielding gas flowing through a first gas flow passage surrounding a tungsten electrode and a second shielding gas flowing through a second gas flow passage surrounding the first gas flow passage, A shielding gas for copper welding, comprising 5% by volume or more and 75% by volume or less of helium gas, with the remainder being substantially argon gas.
2. 2. The shielding gas for welding copper materials according to claim 1, wherein the copper material is oxygen-free copper.
3. 3. The shielding gas for copper welding according to claim 1, which is used as the first shielding gas and contains 5% by volume or more and 20% by volume or less of helium gas, with the remainder being substantially argon gas.
4. 3. The shielding gas for copper welding according to claim 1, which is used as the second shielding gas and contains 10% by volume or more and 75% by volume or less of helium gas, with the remainder being substantially argon gas.
5. 3. The shielding gas for copper welding according to claim 1, which is used as the second shielding gas and contains 20% by volume or more and 50% by volume or less of helium gas, with the remainder consisting essentially of argon gas.
Citation Information
Patent Citations
TIG welding method for ferritic stainless steel plate
JP2013086136A