Adhesive preventive object
A fluorine coating layer with high hardness and large water droplet contact angle addresses fouling and contamination issues in semiconductor process equipment, improving maintenance efficiency and reducing costs through self-cleaning.
Patent Information
- Application Number
- JP2024003901
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-11-20
- Filing Date
- 2024-01-15
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2044-01-15
AI Technical Summary
Semiconductor process equipment experiences frequent fouling and contamination due to process materials and environmental substances, leading to shortened maintenance cycles and increased costs.
Application of a fluorine coating layer with high hardness, large water droplet contact angle, and low roughness to vacuum and non-vacuum parts to prevent scratches, deposition, and facilitate self-cleaning.
The fluorine coating layer effectively prevents scratches and deposition, reduces maintenance frequency, and enhances the self-cleaning capability of surfaces in various environments.
Smart Images

Figure 2024150394000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to objects, and in particular to adhesion-resistant objects. [Background technology]
[0002] In recent years, with the continuous and vigorous development of semiconductor technology, technological products have made great progress. In the process of semiconductor chips, semiconductor chips are generally placed in a process device to carry out the relevant process, and a vacuum pump is used to evacuate the air or gas in the process device and keep the process device in a negative pressure state, that is, to reach a certain degree of vacuum. However, in the semiconductor process, process materials such as process gases and process exhaust gases are easily deposited in the fluid passages, which leads to shorter and shorter repair cycles. This affects the manufacturing cost and schedule. In addition, since the air contains a lot of dust particles of various sizes and moisture with various degrees of dirt, any object that comes into contact with air (such as commonly seen ceramics, glass, and other structures and materials) is prone to the accumulation of dust, water stains, and dirt, and therefore requires fairly frequent cleaning, maintenance, or replacement. Similarly, since there are many living organisms, microorganisms, and substances in seawater and freshwater, objects that often come into contact with seawater (such as commonly seen ships) will experience various deposits (or adhesions). Summary of the Invention [Problem to be solved by the invention]
[0003] The main object of the present invention is to provide an adhesion-resistant object that can prevent scratches caused by collisions of process materials such as particles of a vacuum component by applying a fluorine coating layer having high hardness to a vacuum component or a non-vacuum component. [Means for solving the problem]
[0004] The adhesion-prevention object according to the present invention is characterized in that it comprises a main structure having at least one surface, and a fluorine coating layer covering the surface of the main structure, contacting a certain substance in a certain environment, and having a larger water droplet contact angle with respect to the substance, approximately the same or higher hardness, and lower roughness than the surface of the main structure.
[0005] The adhesion prevention object according to the present invention is characterized in that the main structure is an outlet tube of a process device, or a tube or member of a peripheral device of the process device.
[0006] The adhesion-resistant object according to the present invention is characterized in that the fluorine coating layer is located on the surface of a certain portion of the main structure, and the said portion is an inclined portion, a flat portion, or a curved portion of the main structure.
[0007] The adhesion-resistant object according to the present invention is characterized in that the fluorine coating layer has a higher resistance to acid corrosion and plasma etching than the surface of the main structure.
[0008] The adhesion prevention object according to the present invention is characterized in that the surface of the main structure forms a rough surface of a rough structure after the roughening treatment, and the surface roughness is increased.
[0009] The adhesion prevention object according to the invention is characterized in that the surface of the main structure has an increased surface roughness after undergoing roughening by pickling, laser or sandblasting.
[0010] The adhesion-resistant object according to the present invention is characterized in that the components of the fluorine coating layer are composed of 0.01 to 20% by weight of fluorocarbons, 5 to 50% by weight of alkoxysilane, 0.01 to 20% by weight of catalyst additive, and 10 to 90% by weight of solvent.
[0011] The adhesion-preventing object according to the present invention is characterized in that the fluorocarbon is selected from the group consisting of perfluoroalkane substances (PFAS), chlorofluorocarbons (CFCs), semifluorocarbons (HFCs), hydrofluorochlorocarbons (HCFCs), polytetrafluoroethylene (PTFE), and fluorinated ethylene propylene (FEP).
[0012] The adhesion prevention object according to the present invention is characterized in that the fluorocarbon is a fluorine-containing monomer or polymer containing 1 to 20 carbon atoms.
[0013] The adhesion-preventing object according to the present invention is characterized in that the alkoxysilane is selected from the group consisting of alkoxysilane oligomers, alkoxysilane compounds, alkoxysilane polymers, alkoxylsiloxane oligomers, alkoxylsiloxane compounds, alkoxylsiloxane polymers, alkoxylaminosiloxane oligomers, alkoxylaminosiloxane compounds, and alkoxylaminosiloxane polymers.
[0014] The adhesion prevention object according to the present invention is characterized in that the catalytic additive is selected from the group consisting of metals such as platinum, titanium, tin, zinc, aluminum, silver, calcium, magnesium, potassium, sodium, nickel, chromium, molybdenum, vanadium, copper, iron, cobalt, germanium, hafnium, lanthanum, lead, ruthenium, tantalum, tungsten, and zirconium, metal oxides, zirconium phosphates, and carboxylates.
[0015] The adhesion-preventing object according to the present invention is characterized in that the solvent is selected from the group consisting of alcohols, ketones, esters, fluoroalcohols, fluoroethers and ethers.
[0016] The adhesion-resistant object of the present invention is characterized in that the alkoxysilane has a reactive functional group, which undergoes a self-condensation reaction at room temperature for 1 to 7 days, or at a temperature of 40 to 60 degrees Celsius for 1 to 24 hours.
[0017] The adhesion prevention object of the present invention is characterized in that the environment is a vacuum environment, the substance is a process material, the adhesion prevention object is the process material that is used or discharged when performing a process in the vacuum environment in contact with a process equipment, the process performed in the process equipment is an atomic layer deposition (ALD) process, and the process material is titanium tetrachloride (TiCl4).
[0018] The adhesion prevention object of the present invention is characterized in that the environment is a vacuum environment, the substance is a process material, the adhesion prevention object is the process material that is used or discharged when performing a process in the vacuum environment in contact with a process device, the process performed in the process device is a metal-organic chemical vapor deposition (MOCVD) process, and the process material is a process gas or process exhaust gas.
[0019] The adhesion prevention object of the present invention is characterized in that the environment is a vacuum environment, the substance is a process material, the adhesion prevention object is the process material that is used or discharged when a process is performed in the vacuum environment in contact with a process device, the process performed in the process device is an aluminum pad (Al-pad) process, and the process material is a process gas reactant or process exhaust gas.
[0020] The adhesion prevention object according to the present invention is characterized in that the water droplet contact angle of the fluorine coating layer is in the range of 100 degrees to 120 degrees.
[0021] The adhesion-resistant object according to the present invention is characterized in that the temperature resistance of the fluorine coating layer reaches 600 degrees Celsius.
[0022] The adhesion prevention object according to the present invention is characterized in that the hardness of the fluorine coating layer is in the range of 8H to 9H.
[0023] The adhesion-resistant object according to the present invention is characterized in that the adhesive strength between the fluorine coating layer and the surface of the main structure is in a numerical range of 4B to 5B as obtained by a cross-cut test.
[0024] The adhesion prevention object according to the present invention is characterized in that the environment is a vacuum environment, a gas-phase environment, a liquid-phase environment, or a mixed gas-liquid environment.
[0025] The adhesion prevention object according to the present invention is characterized in that the main structure is a main structure, part, member, or material of an architectural structure, power generation equipment, means of transportation, or the like.
[0026] The adhesion-resistant object of the present invention is characterized in that the environment is an ozone water environment, and the fluorine coating layer increases its stability against ozone water in the ozone water environment by increasing the fluorine content in accordance with the ozone water environment. Effect of the Invention
[0027] The adhesion prevention object according to the present invention has the following effects. (1) By applying a fluorine coating layer having high hardness to the vacuum components, scratches caused by collisions of process materials such as particles on the vacuum components can be prevented. (2) By applying a fluorine coating layer having a larger water droplet contact angle to a vacuum component, deposition on the vacuum component can be prevented, and a self-cleaning effect and easy cleaning effect can be achieved. (3) The fluorine coating layer has good adhesion to the main structure, which makes it possible to prevent peeling during the process. (4) Anti-adhesive objects with a fluorine coating layer can save the cost and effort of frequent maintenance. (5) By coating the main structures, parts and components of building structures, electrical equipment, means of transportation and the like with a high-hardness hook coating layer, it is possible to prevent deposition due to contact with substances in the environment, and also to achieve the effects of self-cleaning and easy cleaning, and to prevent scratches caused by collisions with substances in the environment.
[0028] In order to better understand the technical features and achievable technical effects of the present invention, better embodiments and detailed descriptions are provided below. [Brief description of the drawings]
[0029] [Figure 1] 1A and 1B are diagrams showing a structure of a portion of an adhesion prevention object according to the present invention; [Diagram 2] FIG. 1 is a diagram showing an adhesion prevention object according to the present invention being applied to a process device. [Diagram 3] 1 is a cross-sectional structural view showing a first embodiment of an adhesion prevention object according to the present invention. [Figure 4] FIG. 4 is a cross-sectional structural view showing a second embodiment of an adhesion prevention object according to the present invention. [Diagram 5]FIG. 11 is a cross-sectional structural view showing a third embodiment of an adhesion prevention object according to the present invention. [Figure 6] FIG. 13 is a perspective view showing the structure of a fourth embodiment of an adhesion prevention object according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. The ratio of each member in the drawings of the embodiment of the present invention is shown for easy understanding of the description, and is not the actual ratio. Furthermore, the dimensional ratio of the assembly shown in the drawings is for explaining each part and its structure, and the present invention is not limited thereto. Meanwhile, for convenience of understanding, the same parts in the following embodiments will be described with the same reference numerals.
[0031] Furthermore, the terms used throughout the specification and claims generally have their ordinary meanings as used in the art, in the context disclosed herein, and in the particular context, unless otherwise specified. Some of the terms used to describe the present invention are explained below or elsewhere in this specification to provide those of ordinary skill in the art with additional guidance regarding the description of the present invention.
[0032] The use of "first", "second", "third", etc. in this description is not intended to denote a specific order or sequentiality, nor is it used to limit the invention, but is merely used to distinguish between components or operations that are described with the same terminology.
[0033] Secondly, when terms such as "including," "comprising," "having," and "containing" are used in this description, they are all open terms, meaning that they include but are not limited to.
[0034] Please refer to Fig. 1 to Fig. 6. Fig. 1 is a diagram showing the structure of a portion of a deposition prevention object according to the present invention. Fig. 2 is a diagram showing that a deposition prevention object according to the present invention is applied to a process device. Fig. 3 is a cross-sectional structural view showing a first embodiment of a deposition prevention object according to the present invention. Fig. 4 is a cross-sectional structural view showing a second embodiment of a deposition prevention object according to the present invention. Fig. 5 is a cross-sectional structural view showing a third embodiment of a deposition prevention object according to the present invention. Fig. 6 is a perspective view showing the structure of a fourth embodiment of a deposition prevention object according to the present invention.
[0035] The adhesion-preventing object according to the present invention has a fluorine coating layer covering the surface of the main structure, which can prevent the surface from coming into contact with substances in the environment and causing deposition, and can achieve a self-cleaning effect and an easy-to-clean effect, and can also prevent scratches caused by collision with substances in the environment. The above-mentioned environment is, for example, a vacuum environment, a gas-phase environment, a liquid-phase environment, or a gas-liquid mixed environment. In other words, the application of the adhesion-preventing object according to the present invention is not limited to a vacuum environment, and it can also be applied to environments other than a vacuum environment, and all of them fall within the scope of the claims of the present invention as long as they can obtain the effect of preventing deposition.
[0036] Please refer to FIG. 1 to FIG. 6. The adhesion prevention object 10 according to the present invention includes a main structure 20 and a fluorine coating layer 30. The fluorine coating layer 30 covers the main structure 20. The adhesion prevention object 10 according to the present invention can be applied to, for example, a vacuum environment or a non-vacuum environment. In the case of application to a vacuum environment, the adhesion prevention object 10 is, for example, a substance 110 (also called a process material) that is used or discharged when a process is performed in contact with a process device 100 in a vacuum environment. The vacuum environment is not limited to a specific vacuum level and may be determined according to the needs of the process device 100. The environment may be a non-vacuum environment, such as a gas phase environment, a liquid phase environment, or a gas-liquid mixed environment. The adhesion prevention object 10 according to the present invention contacts the substance 110 in the above environment. The fluorine coating layer 30 covers at least one surface 22 of the main structure 20. The fluorine coating layer 30 of the adhesion prevention object 10 according to the present invention covers, for example, the entire or part of the surface of the main structure 20, for example, the surface 22 of the portion 24 of the main structure 20. The portion 24 may be a position where deposition of process material often occurs, such as a bent portion or an inclined portion, which is not a flat portion, and is not limited to a back wall surface. Therefore, in the present invention, the above portion 24 is, for example, a bent portion of the main structure 20 shown in FIG. 3 or an inclined portion of the main structure 20 shown in FIG. 4, but the present invention is not limited thereto. The fluorine coating layer 30 of the present invention may cover a flat portion of the main structure 20 shown in FIG. 5. The main structure 20 of the adhesion prevention object 10 of the present invention may be, for example, an outlet pipe of the process device 100 as shown in FIG. 3 to FIG. 5, or a tube of a peripheral device (e.g., a vacuum pump) of the process device 100 as shown in FIG. 3 to FIG. 5, or a component such as a part of a Holweck pump having a spiral flow diverter trough 26 as shown in FIG. 6. Although many types of aspects of the main structure 20 of the adhesion prevention object 10 have been given as examples above, the present invention is not limited thereto, and all aspects of objects that can be applied to a vacuum environment belong to the scope of the claims of the present invention.For example, the adhesion-resistant object 10 and its main structure 20 according to the present invention may be, for example, a chamber or part of a vacuum pump, such as a rotor blade and / or a stator blade of a turbomolecular vacuum pump (TMP). For example, the adhesion-resistant object 10 and its main structure 20 according to the present invention may be, for example, a chamber or part of a valve structure. In brief, in the present invention, a fluorine coating layer 30 may be selectively formed on the surface of all objects that can come into contact with the substance 110.
[0037] One of the features of the adhesion prevention object according to the present invention is that the surface 22 of the main structure 20 is covered with a fluorine coating layer 30, and the fluorine coating layer 30 comes into contact with the material 110 used or discharged when the process device 100 performs the process, instead of the surface 22 of the main structure 20. The fluorine coating layer 30 covers the surface 22 of the main structure 20, for example, by application. The application method can be, for example, spraying, brushing, dipping, or wiping, but is not limited to these. For example, the present invention increases the surface roughness by directly applying the fluorine coating layer 30 in liquid phase to the surface 22 of the main structure 20, or by first performing a roughening process (roughening treatment) on the surface 22 of the main structure 20 before applying the fluorine coating layer 30 in liquid phase to the surface 22 of the main structure 20. The roughening process can be, for example, pickling, laser, sandblasting, or other processes, but is not limited to these. By forming many rough surfaces such as rough structures 120, such as grooves and notches, on the surface 22 of the main structure 20, it is possible to increase the adhesion between the fluorine coating layer 30 and the surface 22 of the main structure 20. The present invention is not limited to specific processes such as pickling, laser, sandblasting, etc., that is, the roughening process may employ any technical means as long as it can increase the surface roughness of the main structure 20, and therefore the description thereof will be omitted.
[0038] On the other hand, since air contains a lot of dust and water, and seawater and freshwater contain many organisms, microorganisms, and substances, objects that come into contact with air, seawater, or freshwater are prone to various deposits (also called adhesion), and therefore require fairly frequent cleaning, maintenance, or replacement. According to the adhesion prevention object 10 of the present invention, as shown in FIG. 1, the fluorine coating layer 30 covers the surface 22 of the main structure 20, so that the surface 22 can avoid contact with substances in the environment and the occurrence of various deposits, thereby achieving a self-cleaning effect and an easy-to-clean effect, and also preventing scratches caused by collisions with substances in the environment. For example, the above environment is, but is not limited to, a vacuum environment, a gas-phase environment, a liquid-phase environment, or a gas-liquid mixed environment. The above substances vary depending on the environment in which the adhesion prevention object 10 is placed, and therefore the description thereof is omitted. For example, the main structure 20 of the adhesion prevention object 10 of the present invention is, for example, the main structure, parts, members, or materials of an indoor or outdoor building structure, a power generation device, or a means of transportation. As a result, the main structure 20 can provide the original functions and effects, and the fluorine coating layer 30 can provide additional functions and effects, such as anti-deposition or anti-scratch effects, which can reduce the frequency of cleaning and repair and extend the maintenance cycle. Taking a building structure as an example, the main structure 20 of the adhesion prevention object 10 according to the present invention is a main structure, part, member or material of an indoor or outdoor building structure, such as, but not limited to, a structural material, a decorative material and a special material. For example, the structural material of the building structure is a main structure, part, member or material of an indoor or outdoor building structure, such as, but not limited to, metal, wood, stone, cement, concrete, stone, ceramics, glass, engineering plastics, composite materials or a combination thereof. In addition, the above glass is, for example, indoor glass (for example, bathroom glass) or outdoor glass (for example, window). This can prevent adhesion of scale and dust.The decorative materials of architectural structures are, but are not limited to, the main structures, parts, members or materials of indoor or outdoor architectural structures, such as coatings, paints, boards, ceramic tiles, glass, composite materials or combinations thereof. The dedicated materials of architectural structures are, but are not limited to, the main structures, parts, members or materials of indoor or outdoor architectural structures, such as waterproofing, moisture-proofing, corrosion-proofing, fire-retardant, flame-retardant, sound-insulating, heat-insulating, heat-retaining, sealing or combinations thereof. The above composite materials, such as foamed plastic (e.g., polyethylene, PET, etc.) sandwich panels, composite panels combining wood cores and lightweight hardwood surface materials (e.g., balsa, etc.), or aluminum composite panels (e.g., aluminum-plastic panels, etc.), have gradually been widely used in buildings, and are materials as architectural composite materials in the decoration and furniture fields, which can exert their effects, for example, the use of composite materials in buildings can reduce the weight of the entire building and effectively improve the earthquake resistance level of the building. Taking a power generating device as an example, the main structure 20 of the adhesion prevention object 10 according to the present invention is, for example, the main structure, parts, members, or materials of a power generating device such as a wind power generating device, a hydroelectric power generating device, a wave power generating device, or a solar power generating device. For example, the main structure 20 is, but is not limited to, the blades of a power generating device. Taking a means of transportation as an example, the main structure 20 of the adhesion prevention object 10 according to the present invention is, for example, the main structure, parts, members, or materials of various types of means of transportation (for example, a ship, a vehicle, an aircraft, etc.), the main structure being, for example, the hull of a ship, the fuselage of a vehicle, the fuselage of an aircraft, etc., but is not limited to, and the parts, members, or materials being, for example, the components or materials of various types of ships, vehicles, or airplanes, but is not limited to,. For example, if the main structure 20 of the adhesion prevention object 10 according to the present invention is the main structure, parts, members, or materials of a ship, it can be used to prevent the attachment of organisms such as barnacles and microorganisms and to prevent corrosion of seawater above or below the water surface.In brief, the adhesion prevention object 10 of the present invention can avoid physical reactions (such as scratches) or chemical reactions (such as deposition or rust) in contact with various types of materials in the environment in which it is placed (such as a vacuum environment, a gas-phase environment, a liquid-phase environment, or a mixed gas-liquid environment). Although the present invention has done its best to list possible application examples, the above uses are merely examples and are not intended to limit the scope of protection claimed in this specification, since the adhesion prevention object of the present invention can be used to replace major structures, parts, members, or materials of existing building structures, power generation equipment, and transportation means. All aspects of the object that can be used in a vacuum environment, a gas-phase environment, a liquid-phase environment, or a mixed gas-liquid environment are entirely within the scope of the claims of the present invention.
[0039] In the present invention, after applying the fluorine coating layer 30 in liquid phase to the surface 22 of the main structure 20, the self-condensation reaction is carried out at room temperature for about 1 to 7 days, or at a temperature of 40°C to 60°C for about 1 to 24 hours. That is, the fluorine coating layer 30 is solidified on the surface 22 of the main structure 20 to form a fluorine coating layer 30 in a hardened state. The thickness of the fluorine coating layer 30 may be in the range of 1 μm to 3,000 μm, or any numerical interval or upper and lower end point values within this range, for example, 10 μm to 300 μm. The physical and chemical properties of the fluorine coating layer 30 are better than those of the original physical and chemical properties of the surface 22 of the main structure 20. For example, in a vacuum environment, the fluorine coating layer 30 has a larger water droplet contact angle θ with respect to the material 110 than the surface 22 of the main structure 20, i.e., the water droplet contact angle between the fluorine coating layer 30 and the material 110 (which may range from about 100 degrees to 140 degrees, or any numerical interval or upper and lower end point values within this range, for example, 106.5 degrees) is larger than the water droplet contact angle between the surface 22 and the material 110 (which ranges from about 89 degrees to 95 degrees). In the present invention, by applying a fluorine coating layer 30 having a larger water droplet contact angle to a vacuum member, it is possible to prevent deposition on the vacuum member, and to obtain a self-cleaning effect and an easy-to-clean effect. The hardness of the fluorine coating layer 30 is approximately the same as or higher than the hardness of the surface 22 of the main structure 20. That is, the hardness of the fluorine coating layer 30 (which may range from about 8H to 9H, or any interval or upper or lower endpoint value within this range) is approximately the same as, equal to, or higher than the hardness of the surface 22 of the main structure 20 (which may range from about 4H to 6.5H). By applying a fluorine coating layer 30 having a high hardness to the vacuum member, the present invention can prevent the vacuum member from being scratched by collisions with process materials such as particles. The adhesion force between the fluorine coating layer 30 and the surface 22 of the main structure 20 (Cross-Cut test) ranges from about 4B to 5B.) is greater than the contact force applied by the material 110 to the fluorine coating layer 30 (for example, the external force or adsorption force of the material 110 colliding with the fluorine coating layer 30 when it is discharged). As a result, the adhesion of the fluorine coating layer 30 according to the present invention to the main structure 20 is good, and peeling can be avoided during the process. The fluorine coating layer 30 has a higher resistance to acid corrosion and plasma etching than the surface 22 of the main structure 20, and therefore the fluorine coating layer 30 according to the present invention can protect the vacuum member from acid etching and free radical erosion. The fluorine coating layer 30 has a lower roughness than the surface 22 of the main structure 20, i.e., the roughness (about 0.2) of the fluorine coating layer 30 is lower than the roughness of the surface 22 of the main structure 20. Furthermore, the fluorine coating layer 30 can have the effect of filling or infiltrating the rough structure 120 such as a groove or notch on the surface 22 of the main structure 20, thereby achieving a smoothing effect. On the other hand, the fluorine coating layer 30 according to the present invention can withstand a considerably high temperature, has a wide operating temperature range, and has a temperature tolerance range of about 600 degrees Celsius. The operating temperature range of the fluorine coating layer 30 is, for example, lower than about 600 degrees Celsius or about 600 degrees Celsius, and is preferably, for example, about 260 degrees Celsius to 600 degrees Celsius, and may be any numerical interval or upper and lower endpoint values lower than 600 degrees Celsius or 600 degrees Celsius. On the other hand, conventional water-repellent coatings and anti-soiling coatings usually cannot withstand high temperatures, for example, the operating temperature of conventional Teflon is lower than 260 degrees Celsius. Furthermore, the hardness of conventional water-repellent coatings and anti-soiling coatings is only about 1H to 3H, for example, the hardness of conventional Teflon is 1H to 2H. For this reason, conventional water-repellent coatings and anti-soiling coatings cannot withstand the high temperature, high vacuum, high corrosiveness, high impact, and high deposition environment when semiconductor processing is performed in the process equipment 100. In other words, the adhesion prevention object 10 of the present invention, by combining the fluorine coating layer 30 with the main structure 20, can save costs and manpower caused by frequent maintenance.
[0040] The components of the fluorine coating layer 30 according to the present invention are, for example, about 0.01-20% wt of fluorocarbons, about 5-50% wt of alkoxysilane, about 0.01%-20% wt of catalyst additive, and about 10-90% wt of solvent. The fluorocarbon is, for example, a fluorine-containing monomer or polymer having 1-20 carbon atoms. The fluorocarbon is, for example, a fluorine-containing monomer having about 3-20 carbon atoms and at least one terminal trifluoromethyl. The fluorocarbon is, for example, selected from the group consisting of perfluoroalkane substances (PFAS), chlorofluorocarbons (CFCs), semifluorocarbons (HFCs), fluoropolymers (PTFE, etc.), and hydrofluorochlorocarbons (HCFCs). The alkoxysilane is, for example, selected from the group consisting of an alkoxysilane oligomer, an alkoxysilane compound, an alkoxysilane polymer, an alkoxylsiloxane oligomer, an alkoxylsiloxane compound, an alkoxylsiloxane polymer, an alkoxylaminosiloxane oligomer, an alkoxylaminosiloxane compound, and an alkoxylaminosiloxane polymer. The catalyst additive is selected from the group consisting of metals such as platinum, titanium, tin, zinc, aluminum, silver, calcium, magnesium, potassium, sodium, nickel, chromium, molybdenum, vanadium, copper, iron, cobalt, germanium, hafnium, lanthanum, lead, ruthenium, tantalum, tungsten, zirconium, metal oxides, zirconium phosphates, and carboxylates.The catalyst additive may be selected from the group consisting of silicon oxide, aluminum oxide, titanium oxide, iron oxide, magnesium oxide, molybdenum oxide, calcium oxide and calcium chloride, and may have a size of, for example, nanometers, but the present invention is not limited thereto. Micro-nano size and even micron size catalyst additives or components are also included within the scope of the present invention. The solvent may be, for example, alcohol such as ethanol, propanol, butanol, but the present invention is not limited thereto, and the solvent according to the present invention is selected from the group consisting of alcohol, ketone, ester, fluoroalcohol, fluoroether and ether. The alkoxysilane according to the present invention has a reactive functional group, and the reactive functional group undergoes a self-condensation reaction at room temperature for 1 to 7 days (for example, 7 days) or at a temperature of 40 to 60 degrees Celsius for 1 to 24 hours (for example, 24 hours). In addition, the reactive functional group may be, for example, a silicone hydrogenation reactive functional group (such as alkenyl, acrylic, hydrogen atom bonded to silicon atom), a condensation reactive functional group (such as hydroxyl, alkoxy, acyloxy, etc.), or a peracid curing reactive functional group (such as alkyl, alkenyl, acrylic, hydroxyl, etc.). In addition, in one embodiment, the component of the fluorine coating layer 30 according to the present invention is, for example, an organic-inorganic polymer copolymer composed of fluorine, nanotitanium, silicon, and silicone elastomer. Those who have ordinary knowledge in the technical field to which the present invention belongs should know how to select and adjust the adhesion prevention object 10 having the fluorine coating layer 30 that can obtain the effects of the present invention based on the above content of this disclosure, so the description thereof is omitted.Meanwhile, the fluorine coating layer 30 of the adhesion prevention object 10 according to the present invention can have a fluorination degree increased according to the environment in which the adhesion prevention object 10 is placed (e.g., an ozone water environment such as a steam ozone stripping (VOS) process or its application), for example, by adding perfluoroalkyl substances (Per / Poly fluoro alkyl substances, PFAS) (e.g., Perfluorooctanoic acid (PFOA) or Perfluorooctane sulfonic acid (PFOS)), polytetrafluoroethylene (Polytetrafluoroet Hylene, PTFE) or fluorinated ethylene propylene (Fluorinated ethylene propylene, FEP). The present invention can improve the stability of ozone water in the environment by increasing the fluorination degree of the adhesion prevention object 10 in various application aspects.
[0041] In the surface hardness testing method of the present invention, the surface hardness of the fluorine coating layer 30 is tested with a hard pencil. For example, a hard pencil (Mitsubishi Standard Pencil) is placed on a dolly having a certain load at an angle of 45 degrees, and the dolly is pushed by hand so as to slide across the surface of the fluorine coating layer 30 of the adhesion-resistant object 10, and the surface hardness is confirmed when scratches caused by the pencil are generated. In the adhesion-resistant object 10 of the present invention, all test results of the surface hardness of the fluorine coating layer 30 covering the surface 22 of the main structure 20 are in the range of 1 kg load at 8H to 500 g load at 9H.
[0042] The cross-cut test of the present invention is carried out according to ASTM D3359 method B (cross-cut method) test, by using a grid knife to draw 10x10 (100) small grid lines of 1 mm x 1 mm on the surface of the test book. Each line has a depth sufficient to attach to the bottom layer of the foil layer 30 of the adhesion prevention object 10. Use a brush to remove debris from the test area, and use a standard tape (3M tape 600) or a tape with the same effect to apply to the tested grid lines, and increase the contact area and the magnitude of the force between the tape and the test area by wiping the tape with an eraser. Grab one end of the tape with your hand, and quickly peel off the tape at a 180 degree angle within 1.5 minutes ± 30 seconds, and then observe the peeling state of the fluorine coating layer 30. In the adhesion-prevention object 10 according to the present invention, the cross-cut test results of the fluorine-coating layer 30 according to the present invention covering the surface 22 of the main structure 20 are all in the range of 5B (the edges of the cuts are completely smooth, there is no peeling at the edges of the grid.) to 4B (small pieces peeled off at the intersections of the cuts, and the actual damage in the cross-hatched areas is ≦5%). This shows that the adhesion (adhesion) of the fluorine-coating layer 30 according to the present invention to the surface 22 of the main structure 20 is extremely high.
[0043] In the acid corrosion resistance test of the present invention, 0.05ml of 5% HCl (hydrochloric acid) is dropped onto the test sample and left for 24 hours until the HCl solution evaporates. During the evaporation process, the concentration of the HCl area increases, which enhances the corrosion diffusion effect. The corrosion diffusion area after 24 hours is observed. The test result is the corrosion area (mm 2 ) is about 45.13 mm, while the corroded area (mm 2 ) is only about 19.4 mm.
[0044] The present invention also carried out a plasma etching test. The results showed that under the same etching conditions (CHF3:Ar is 1:1, 60 minutes, oxide etching rate is 750nm / 30min), the fluorine coating layer 30 of the present invention is indeed more resistant to plasma etching than the surface 22 (anodized aluminum material) of the main structure 20. As far as the thermal stability test (Thermogravimetric Analyzer, TGA test) is concerned, in the test environment where the temperature rise rate is 5 degrees Celsius / min and the test atmosphere is N2, the weight of the fluorine coating layer 30 of the present invention is stable and gradually decreased within the test temperature range (600 degrees Celsius), and there is no sudden change in weight. This indicates that the fluorine coating layer 30 of the adhesion prevention object 10 of the present invention is not cracked.
[0045] The process performed in the process tool 100 is, for example, a semiconductor process. For example, the process performed in the process tool 100 is an atomic layer deposition (ALD) process, the process material is titanium tetrachloride (TiCl4), and the main structure 20 of the deposition prevention object 10 is, for example, but not limited to, a fluid transport pipe. For example, the process performed in the process tool 100 is a metal organic chemical vapor deposition (MOCVD) process, the process material is a process gas or a process exhaust gas, and the main structure 20 of the deposition prevention object 10 is, for example, but not limited to, an outlet pipe of a vacuum pump. For example, the process performed in the process tool 100 is an aluminum pad (Al-pad) process, and the process material is a process gas reactant or a process exhaust gas, for example, selected from the group consisting of N2, O2, Ar, SF6, He, HBr, CF4, CH4, Cl2, BCl3, and CHF3. The main structure 20 of the deposition prevention object 10 is, for example, but not limited to, a pump part with a flow guide spiral groove and an outlet pipe. The adhesion prevention object of the present invention has been actually tested, and as a result, it is all effective in the above processes. For example, in the aluminum pad process, the adhesion prevention object of the present invention can extend the maintenance cycle by about 20%, thereby reducing the funds and manpower required for frequent maintenance.
[0046] The adhesion prevention object according to the present invention has the following effects. (1) By applying a fluorine coating layer having high hardness to the vacuum components, scratches caused by collisions of process materials such as particles on the vacuum components can be prevented. (2) By applying a fluorine coating layer having a larger water droplet contact angle to a vacuum component, deposition on the vacuum component can be prevented, and a self-cleaning effect and easy cleaning effect can be achieved. (3) The fluorine coating layer has good adhesion to the main structure, which makes it possible to prevent peeling during the process. (4) Anti-adhesive objects with a fluorine coating layer can save the cost and effort of frequent maintenance. (5) By coating the main structures, parts and components of building structures, electrical equipment, means of transportation and the like with a high-hardness hook coating layer, it is possible to prevent deposition due to contact with substances in the environment, and also to achieve the effects of self-cleaning and easy cleaning, and to prevent scratches caused by collisions with substances in the environment.
[0047] The above description is illustrative only and not limiting. Any equivalent modifications or variations thereto that do not depart from the spirit and scope of the present invention are intended to be within the scope of the claims. [Explanation of symbols]
[0048] 10. Protective Objects 20 Main structure 22 Surface 24 parts 26 Spiral Diversion Trough 30 Fluorine coating layer 100 Process Equipment 110 Substance 120 Rough Structure θ Water droplet contact angle
Claims
1. a host structure having at least one surface; a fluorine coating layer covering the surface of the host structure, contacting a substance in a certain environment, and having a larger water droplet contact angle with respect to the substance, approximately the same or higher hardness, and lower roughness than the surface of the host structure; An adhesion prevention object comprising:
2. The deposition prevention object according to claim 1 , wherein the main structure is an outlet tube of a process device, or a tube or member of a peripheral device of the process device.
3. The adhesion-preventing object according to claim 1 , wherein the fluorine coating layer is located on the surface of a portion of the main structure, the portion being an inclined portion, a flat portion, or a curved portion of the main structure.
4. The adhesion-preventing object according to claim 1 , wherein the fluorine coating layer has higher resistance to acid corrosion and plasma etching than the surface of the main body structure.
5. The adhesion-preventing object according to claim 1 , characterized in that, after the roughening treatment, the surface of the main structure forms a rough surface of a rough structure, and the surface roughness is increased.
6. The anti-deposition object according to claim 1 , characterized in that the surface of the main structure has an increased surface roughness after undergoing roughening by pickling, laser or sandblasting.
7. The adhesion-preventing object according to claim 1, characterized in that the components of the fluorine coating layer are composed of 0.01 to 20% wt of fluorocarbons, 5 to 50% wt of alkoxysilane, 0.01 to 20% wt of a catalyst additive, and 10 to 90% wt of a solvent.
8. 8. The anti-adhesive object according to claim 7, wherein the fluorocarbon is selected from the group consisting of perfluoroalkane substances (PFAS), chlorofluorocarbons (CFCs), semifluorocarbons (HFCs), hydrofluorochlorocarbons (HCFCs), polytetrafluoroethylene (PTFE), and fluorinated ethylene propylene (FEP).
9. The deposition-resistant object according to claim 7, characterized in that the fluorocarbon is a fluorine-containing monomer or polymer containing 1 to 20 carbon atoms.
10. The alkoxysilane may be an alkoxysilane oligomer, an alkoxysilane compound, an alkoxysilane polymer, an alkoxylsiloxane oligomer, an alkoxylsiloxane compound, an alkoxylsiloxane polymer, an alkoxylaminosiloxane oligomer, an alkoxylaminosiloxane compound ...
8. The object according to claim 7, characterized in that the anti-deposition agent is selected from the group consisting of: alkoxylaminosiloxane polymers;
11. 8. The deposition-prevention object according to claim 7, characterized in that the catalytic additive is selected from the group consisting of metals such as platinum, titanium, tin, zinc, aluminum, silver, calcium, magnesium, potassium, sodium, nickel, chromium, molybdenum, vanadium, copper, iron, cobalt, germanium, hafnium, lanthanum, lead, ruthenium, tantalum, tungsten, zirconium, metal oxides, zirconium phosphates and carboxylates.
12. 8. The deposition-resistant object according to claim 7, characterized in that the solvent is selected from the group consisting of alcohols, ketones, esters, fluoroalcohols, fluoroethers and ethers.
13. The adhesion-preventing object according to claim 7, characterized in that the alkoxysilane has a reactive functional group, and the reactive functional group undergoes a self-condensation reaction at room temperature for 1 to 7 days, or at a temperature of 40 to 60 degrees Celsius for 1 to 24 hours.
14. The environment is a vacuum environment, the substance is a process material, the adhesion prevention object is the process material that is used or discharged when performing a process in the vacuum environment in contact with a process device, the process performed in the process device is an atomic layer deposition (ALD) process, and the process material is titanium tetrachloride (TiCl 4 2. The deposition prevention object according to claim 1, characterized in that:
15. The adhesion prevention object of claim 1, characterized in that the environment is a vacuum environment, the substance is a process material, the adhesion prevention object is the process material used or discharged when performing a process in the vacuum environment in contact with a process device, the process performed in the process device is a metal-organic chemical vapor deposition (MOCVD) process, and the process material is a process gas or process exhaust gas.
16. The adhesion prevention object of claim 1, characterized in that the environment is a vacuum environment, the substance is a process material, the adhesion prevention object is the process material used or discharged when performing a process in the vacuum environment in contact with a process device, the process performed in the process device is an aluminum pad (Al-pad) process, and the process material is a process gas reactant or a process exhaust gas.
17. The adhesion-preventing object according to claim 1 , wherein the water droplet contact angle of the fluorine coating layer is in the range of 100 degrees to 120 degrees.
18. The adhesion-resistant object according to claim 1 , wherein the temperature resistance of the fluorine coating layer reaches 600 degrees Celsius.
19. The adhesion-resistant object according to claim 1 , wherein the hardness range of the fluorine coating layer is 8H to 9H.
20. The adhesion-resistant object according to claim 1 , wherein the adhesion between the fluorine coating layer and the surface of the main structure is in a numerical range of 4B to 5B obtained by a cross-cut test.
21. The adhesion prevention object according to claim 1 , wherein the environment is a vacuum environment, a gas-phase environment, a liquid-phase environment, or a mixed gas-liquid environment.
22. The adhesion prevention object according to claim 1 , wherein the main structure is a main structure, part, member, or material of an architectural structure, power generation equipment, means of transportation, or the like.
23. The adhesion-preventing object according to claim 1 , wherein the environment is an ozone water environment, and the fluorine coating layer increases its stability against ozone water in the ozone water environment by increasing its fluorine content in response to the ozone water environment.
Citation Information
Patent Citations
Exhaust system and its maintenance method
JP2005187842A
Backsheet for solar modules and method for manufacturing the same
JP2013526033A
Curable composition and molded body
JP2015193747A
Apparatus and methods for pumping gases from a chamber
US20200095679A1