Magnetic tunnel junction structure and method of manufacturing the same

A chromium-based seed layer and cobalt-platinum-iridium bilayer pinning structure stabilizes MTJ stacks in MRAM cells, addressing the issue of SAF coupling loss during high-temperature annealing and maintaining consistent TMR, thus improving MRAM cell reliability.

JP2024150436AInactive Publication Date: 2024-10-23APPLIED MATERIALS INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024097845
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-03-13
Filing Date
2024-06-18
Publication Date
2024-10-23
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The loss of synthetic antiferromagnetic (SAF) coupling in magnetic tunnel junction (MTJ) stacks during high-temperature annealing processes compromises the integrity of magnetic random access memory (MRAM) cells, leading to instability in electrical resistance states.

Method used

The use of a chromium-based seed layer and a pinning layer composed of cobalt and platinum-iridium bilayers, along with a structural blocking layer, to stabilize the MTJ stack and maintain perpendicular magnetic anisotropy even after annealing at high temperatures.

Benefits of technology

The proposed MTJ stack design maintains structural integrity and desired magnetic properties, ensuring consistent tunneling magnetoresistance (TMR) of 100% to 175% even after annealing at 400 degrees Celsius for 0.5 to 3 hours, enhancing the reliability of MRAM cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150436000001_ABST
    Figure 2024150436000001_ABST
Patent Text Reader

Abstract

To provide an improved magnetic tunnel junction (MTJ) stack and a device including the same.SOLUTION: A magnetic tunnel junction (MTJ) structure 200 maintains desirable magnetic properties subsequent to high temperature annealing, and employs seed layers 206 of one or more layer of chromium (Cr), NiCr, NiFeCr, RuCr, IrCr, or CoCr, or combinations thereof. These seed layers are used in combination with one or more pinning layers. A first pinning layer 208 in contact with the seed layer contains a single layer of cobalt, or contains cobalt in combination with bilayers of cobalt and platinum (Pt), iridium (Ir), nickel (Ni), or palladium (Pd). The second pinning layer 212 has a same composition and configuration as the first pinning layer, or has a different composition or configuration therefrom.SELECTED DRAWING: Figure 2A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] FIELD OF THE DISCLOSURE

[0001] Embodiments of the present disclosure generally relate to fabricating magnetic tunnel junction structures for magnetic random access memory (MRAM) applications. [Background technology]

[0002]

[0002] Spin-transfer torque magnetic random access memory (STT-MRAM) employs a magnetic tunnel junction structure in its memory cells, in which two ferromagnetic layers are separated from each other by a thin insulating or "dielectric" layer. One of the magnetic layers has a fixed magnetic polarity, and the other has a magnetic polarity that can be selectively changed between two states. If the magnetic layers have perpendicular magnetic anisotropy, the polarity of the changeable polarity layer can be switched between the same polarity as the fixed polarity layer or the opposite polarity to the fixed polarity layer in the depth direction of the stack of film layers comprising the magnetic tunnel junction ("MTJ") structure. The electrical resistance across the MTJ is a function of the polarity of the changeable polarity layer relative to the fixed polarity layer. If the polarities of the two layers are the same in the depth direction of the MTJ, the electrical resistance across the MTJ is low, and if they are opposite in the depth direction of the MTJ, the electrical resistance across the MTJ is high. Thus, the electrical resistance across the memory cell can be used to indicate a value of 1 or 0, and thus data values ​​can be stored, for example, by using a low resistance state as having a data value of 1 and a high resistance state as having a data value of 0.

[0003]

[0003] When the MTJ is a synthetic antiferromagnetic (SAF) that includes two or more ferromagnetic layers separated by a nonmagnetic layer, the SAF coupling can be lost after high-temperature processing, for example, processing at temperatures above about 400 degrees Celsius.

[0004] To form an MTJ stack, a stack of film layers including a seed layer containing platinum (Pt) or ruthenium (Ru) is used to form a MTJ stack with a suitable crystal orientation (here, a cubic center of gravity). <111> The film stack is then annealed at approximately 400 degrees Celsius for approximately 0.5 to 3 hours to properly form the MRAM cell. However, during this annealing, the crystal lattice and resulting crystal and magnetic pole orientation in the pinning layer is lost, or at least partially lost, resulting in the loss of the desired (SAF) coupling.

[0005]

[0005] Therefore, there is a continuing need for improved MTJ stacks. Summary of the Invention

[0006]

[0006] The present disclosure generally relates to the design and fabrication of magnetic tunnel junction (MTJ) stacks for use in memory cells. In one embodiment, a device includes a magnetic tunnel junction stack. The magnetic tunnel junction stack includes a seed layer in contact with a buffer layer, the seed layer including chromium (Cr), and a first pinning layer in contact with the seed layer. The first pinning layer is formed from a plurality of bilayers, each bilayer of the plurality of bilayers including a first intermediate layer formed from cobalt (Co) and a second intermediate layer formed from platinum (Pt), iridium (Ir), nickel (Ni), or palladium (Pd). The MTJ stack further includes a coupling layer in contact with the first pinning layer and a second pinning layer in contact with the coupling layer.

[0007] In another embodiment, a magnetic tunnel junction stack includes a seed layer formed on the buffer layer, the seed layer comprising chromium (Cr), and a first pinning layer formed on the seed layer, the first pinning layer comprising a first plurality of bilayers. Each bilayer of the first plurality of bilayers includes a first intermediate layer formed from cobalt (Co) and a second intermediate layer formed from at least one of platinum (Pt), iridium (Ir), nickel (Ni), or palladium (Pd). The MTJ stack may further include a bonding layer formed on the first pinning layer and a second pinning layer formed on the bonding layer, the second pinning layer comprising cobalt (Co).

[0008] In another embodiment, a magnetic tunnel junction stack includes a seed layer having a thickness of 1 Å to 100 Å and including chromium (Cr) formed on the buffer layer, and a first pinning layer having a thickness of 1 Å to 100 Å formed on the seed layer, the first pinning layer including a first plurality of bilayers and a first cobalt overlayer formed on the first plurality of bilayers. The MTJ stack further includes a coupling layer formed between the first pinning layer and the first cobalt overlayer, a second pinning layer having a thickness of 1 Å to 100 Å formed on the coupling layer, the second pinning layer including a second plurality of bilayers, and a structural blocking layer formed on the second pinning layer. The structural blocking layer includes at least one of tantalum (Ta), molybdenum (Mo), or tungsten (W) and has a thickness of 1 Å to 8 Å. The MTJ stack further includes a magnetic reference layer formed on the structural blocking layer, a tunnel barrier layer formed on the magnetic reference layer, and a magnetic storage layer formed on the tunnel barrier layer.

[0009]

[0009] So that the features of the present disclosure described above can be understood in detail, a more particular description of the present disclosure briefly summarized above will be had by reference to embodiments, some of which are illustrated in the accompanying drawings. It should be noted, however, that the accompanying drawings depict only exemplary embodiments and therefore should not be considered to limit the scope of the present disclosure, as other equally effective embodiments may also be acceptable. [Brief explanation of the drawings]

[0010] [Figure 1A] 1 is a schematic diagram of an exemplary magnetic tunnel junction (MTJ) stack. [Figure 1B]

[0011] 1B is a flow diagram of a method for manufacturing a memory device including the magnetic tunnel junction (MTJ) stack of FIG. 1A according to an embodiment of the present disclosure. [Figure 2A]

[0012] FIG. 1 is a schematic diagram of an MTJ stack according to an embodiment of the present disclosure. [Figure 2B]

[0013] FIG. 2 is a close-up view of a buffer layer of an MTJ stack according to an embodiment of the present disclosure. [Figure 2C]

[0014] FIG. 2 is a close-up view of a first pinning layer of an MTJ stack according to an embodiment of the present disclosure. [Figure 2D]

[0015] FIG. 2 is a close-up view of the second pinning layer of the MTJ stack according to an embodiment of the present disclosure. [Figure 2E]

[0016] FIG. 2 is a close-up view of an exemplary magnetic memory layer of an MTJ stack according to an embodiment of the present disclosure. [Figure 2F]

[0017] FIG. 2 is a close-up view of an exemplary capping layer of an MTJ stack according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE INVENTION

[0011]

[0018] For ease of understanding, where possible, the same reference numerals have been used to designate identical elements that are common to multiple figures. It is believed that elements and features of one embodiment may be beneficially incorporated in other embodiments without further recitation.

[0012]

[0019] Embodiments of the present disclosure relate to magnetic tunnel junction (MTJ) stacks and STT MRAM memory cells and memories. Here, the MTJ stack is incorporated into a film stack including top and bottom electrodes, and the MTJ stack is sandwiched between them and can be used to form multiple memory cells used in magnetoresistive random access memories (MRAMs). Within each MTJ stack in an MRAM, there are two magnetic layers: one magnetic layer has a fixed polarity and the other has a polarity that can be switched by applying a voltage across the layer or a current through the magnetic layer. The electrical resistance across the MRAM changes based on the relative polarity between the first and second magnetic layers. The first and second magnetic layers are referred to herein as the magnetic reference layer and the magnetic storage layer. Memory cells formed from MTJ stacks operate when there is a voltage applied across the memory cell or a current passing through the memory cell. In response to the application of a voltage of sufficient strength, the polarity of the switchable magnetic layer can be changed. Additionally, the resistance of the memory cell can be determined by measuring the current versus voltage relationship across the memory cell at a relatively low voltage below the threshold required to switch the magnetic polarity of the magnetic storage layer.

[0013]

[0020] The basic MTJ stack described herein is formed using multiple deposition chambers to deposit thin film layers on a substrate and ultimately pattern and etch the deposited film layers. The deposition chamber used to form the MTJ stack described herein includes a physical vapor deposition (PVD) chamber. Here, the PVD chamber is used to form the multiple thin film layers of the MTJ stack. Thus, the MTJ stack includes a buffer layer, a seed layer on the buffer layer, a first pinning layer on the seed layer, a synthetic antiferromagnetic (SAF) coupling layer on the first pinning layer, a second pinning layer on the SAF layer, and a blocking layer on the second pinning layer. In the PVD operation described herein, an inert or noble gas, such as argon (Ar), helium (He), krypton (Kr), and / or xenon (Xe), is ionized into a plasma in a sputtering chamber while the chamber is maintained at a reduced pressure. The PVD process chamber further includes at least one sputtering target and a substrate disposed opposite the generally planar surface of the sputtering target. The sputtering target is either connected to a power supply so as to be electrically driven, or self-established as a cathode in the power supply's circuit via the plasma, e.g., grounding a grounded portion of the sputtering chamber. The substrate is disposed on a pedestal or other structure within the sputtering chamber, which may be at a floating potential, connected to ground, or biased to form an anode within the cathode target for the plasma to an anode or ground circuit. Positively ionized portions of the inert gas atoms within the sputtering chamber are electrically attracted to the negatively biased target, and thus ions of the plasma bombard the target, thereby ejecting atoms of the target material, which are deposited on the substrate, forming a thin film of the target material(s) on the substrate.

[0014]

[0021] To form a thin film of the compound, a sputtering target containing the compound can be used in a PVD chamber with an Ar plasma. In another example, multiple sputtering targets, each containing one or more elements of the compound to be formed as a film on a substrate, are present in the PVD chamber and used with an Ar plasma to form the desired compound. Furthermore, the PVD operation used herein to form layers of an MTJ stack uses either a metal-oxide or metal-nitride sputtering target to form the metal-oxide and metal-nitride. In an alternative embodiment, a metal-oxide or metal-nitride layer is formed in a PVD chamber by sputtering one or more sputtering targets of the metals of the metal oxide or metal nitride while an Ar plasma and either oxygen (O) or nitrogen (N) are present in the PVD chamber. In one embodiment, a PVD chamber has multiple sputtering targets disposed therein, and each sputtering target in the PVD chamber is biased by a power supply to establish a negative bias thereon either by directly applying a negative DC bias, by using a waveform to electrically drive or self-establish a cathodic state on the target, or a combination thereof. In this embodiment, a shield inside the PVD chamber is configured to block one or more of the multiple targets, protecting other sputtering targets in the chamber from the plasma while allowing ions of a plasma formed in the PVD chamber to bombard at least one of the targets and eject or sputter target material atoms therefrom to form a thin film on a substrate. In this embodiment, one or more targets are exposed to an Ar plasma, and their sputtering sequentially or simultaneously forms a desired film composition on the substrate. When O or N is used in addition to the Ar plasma to generate film layers on the substrate, respectively, separate PVD chambers are used to form metal-oxide and metal-nitride layers.

[0015]

[0022] The PVD system may include one or more PVD sputtering chambers coupled to a central robotic substrate transfer chamber configured to move substrates between a loading station coupled thereto and a sputtering chamber coupled thereto. The PVD system may be, for example, a 10×10 -9 The PVD chamber is maintained at a base vacuum of 100 Torr, thereby preventing the substrate on which the MTJ stack is formed from being exposed to the external atmosphere when it is transferred between PVD chambers and between PVD chambers during the fabrication of the MTJ film layer stack thereon. Prior to forming the first film layer of the MTJ film layer stack on the substrate, the substrate is degassed in the vacuum chamber and pre-cleaned using an Ar gas plasma or in a He / H gas plasma in a dedicated pre-clean chamber connected to the central robotic transfer chamber. While fabricating the MTJ stack using one or more PVD chambers, one or more noble or inert sputtering gases, such as Ar, Kr, He, or Xe, can be placed in each of the PVD chambers. The gases are ionized to generate a plasma within the chamber, and the ions of the plasma bombard the negatively biased sputtering target(s), ejecting surface atoms from the target and depositing a thin film of the target material(s) on a substrate positioned within the PVD sputtering chamber. In one embodiment, the process pressure within the one or more PVD chambers can be about 2 mTorr to about 3 mTorr. Depending on the embodiment, the chamber of the PVD platform is maintained at a temperature between −200 degrees Celsius and 600 degrees Celsius during fabrication of at least the seed layer, first and second pinning layers, SAF layer, and buffer layer of the MTJ stack.

[0016]

[0023] FIG. 1A is a schematic diagram of a magnetic tunnel junction (MTJ) stack. FIG. 1A shows a conventional MTJ stack 100A including a substrate 102 having a conductive layer of tungsten (W), tantalum nitride (TaN), titanium nitride (Ti), or other metal layer formed therefrom. In some embodiments, the substrate 102 includes one or more transistors, bit or source lines, and other memory lines (previously fabricated therein or thereon), or other elements used in MRAM memory previously fabricated or formed thereon. The substrate on which the MTJ stack is formed may have dimensions including a diameter of less than 200 mm, a diameter of 200 mm, a diameter of about 300 mm, a diameter of about 450 mm, or other diameters, and may have a circular, rectangular, or square plate shape.

[0017]

[0024] The buffer layer 104 of the conventional MTJ stack 100A is formed on the substrate 102 by sputtering one or more targets in a PVD chamber with the substrate therein, here Co x Fe y B z , TaN, Ta, or a combination thereof. The seed layer 106 is formed on the buffer layer 104 via sputtering in a PVD chamber. The buffer layer 104 is used in the conventional MTJ stack 100A to improve adhesion of the seed layer 106 to the substrate. Here, the seed layer 106 includes platinum (Pt) or ruthenium (Ru) and is formed by sputtering a target of Pt or Ru or an alloy thereof in a PVD chamber having the substrate therein. The seed layer 106 can be used to improve adhesion and seeding of subsequently deposited layers in the conventional MTJ stack 100A by reducing or eliminating the lattice mismatch between the buffer layer 104 and the seed layer 106.

[0018]

[0025] A first pinning layer 108 is formed on the seed layer 106 by sputtering. The first pinning layer 108 here includes a cobalt (Co) layer, one or more Co-containing bilayers, or a combination of a cobalt layer and one or more Co-containing bilayers. A synthetic antiferromagnetic (SAF) coupling layer 110 is here formed on the first pinning layer 108 by sputtering. The SAF coupling layer 110 may be formed from ruthenium (Ru), rhodium (Rh), Cr, or iridium (Ir) sputtered from its target. A second pinning layer 112 is formed on the SAF coupling layer 110 by sputtering. The second pinning layer 112 is formed here from a single cobalt (Co) layer, at least one cobalt-platinum bilayer, or a combination of a cobalt layer and one or more Co-containing bilayers, e.g., Co-Pt bilayers, formed by sputtering a target composed of Co, Pt, or Co-Pt, respectively. The SAF coupling layer 110 is positioned between the first pinning layer 108 and the second pinning layer 112, such that the surface atoms of the first pinning layer 108 and the second pinning layer 112 align with the surface atoms of the SAF coupling layer 110 upon exposure to a magnetic field, thereby pinning the orientation of the first pinning layer 108 and the second pinning layer 112. The first pinning layer 108 and the second pinning layer 112 each exhibit a similar magnetic moment and therefore respond similarly when an external magnetic field is applied to the conventional MTJ stack 100A. The SAF coupling layer 110 maintains the anti-parallel alignment of the magnetic moments of the first pinning layer 108 and the second pinning layer 112 .

[0019]

[0026] A structural blocking layer 114, now comprising tantalum (Ta), molybdenum (Mo), tungsten (W), or a combination thereof, is formed over the second pinning layer 112. The structural blocking layer 114 is used because of its crystal structure that is different from the crystal structures of the first pinning layer 108 and the second pinning layer 112. The structural blocking layer 114 prevents the formation of shorts between the conventional MTJ stack 100A and metal contacts that may be coupled to the conventional MTJ stack 100A to form an MRAM memory cell.

[0020]

[0027] Furthermore, in the conventional MTJ stack 100A, the magnetic reference layer 116 is formed on the structural blocking layer 114 by sputtering in a PVD chamber. A tunnel barrier layer 118 is formed on the magnetic reference layer 116, and a magnetic storage layer 120 is formed on the tunnel barrier layer 118. Each of the tunnel barrier layer 118, the magnetic reference layer 116, and the magnetic storage layer 120 is formed by sputtering in the presence of an Ar plasma in one or more PVD chambers. The magnetic reference layer 116 and the magnetic storage layer 120 are each formed of Co, which may have different compositions. x Fe y B z The magnetic storage layer 120 may include one or more layers of Ta, Mo, W, or Hf, or a combination thereof. The tunnel barrier layer 118 includes an insulating material and may be made of a dielectric material such as MgO. The composition and thickness of the tunnel barrier layer 118 are selected to generate a large tunneling magnetoresistance ratio (TMR) in the tunnel barrier layer 118 of the conventional MTJ stack 100A. The TMR is the ratio of the antiparallel state of resistance (R ap ) to the parallel state (R p ) and is calculated by the formula ((R ap -R p ) / R p) can be expressed as a percentage. When a bias is applied to the conventional MTJ stack 100A, the tunnel barrier layer 118 is traversed by spin-polarized electrons, and the transmission of electrons through the tunnel barrier layer 118 results in electrical conductivity between the magnetic reference layer 116 and the magnetic storage layer 120.

[0021]

[0028] A capping layer 122 is formed on the magnetic storage layer 120 by sputtering in a PVD chamber, and includes multiple interlayers. The multiple interlayers of the capping layer 122 include a first capping interlayer 122A made of a dielectric material such as MgO. A second capping interlayer 122B including a metallic material such as Ru, Ir, Ta, or a combination thereof is formed on the first capping interlayer 122A. The first capping interlayer 122A acts as an etch stop layer for hard mask etching and protects the MTJ stack 100A from corrosion. The second capping interlayer 122B is configured to be in electrical communication with a transistor or contact when the conventional MTJ stack 100A is later patterned, as shown in FIG. 1B and described below. A hard mask layer 124 is formed in a PVD chamber by sputtering and is formed on top of the second capping interlayer 122B to protect the conventional MTJ stack 100A and may be patterned during subsequent operation.

[0022]

[0029] FIG. 1B is a flow diagram of a method 100B for fabricating an MTJ stack 100A and a memory device including the MTJ stack fabricated according to embodiments of the present disclosure and shown in FIGS. 2A-2F. Method 100B is performed in part in multiple PVD chambers of a PVD system configured to deposit thin film layers by sputtering. A substrate 102 can be moved between and among the sputtering chambers via a central robotic transfer chamber in the PVD system to form various thin film layers, including those in FIG. 1A and those fabricated according to embodiments of the present disclosure, as shown and described below. In another example, as described above, multiple sputtering targets are disposed within the PVD chamber, and a shield inside the PVD chamber is configured to selectively protect the multiple sputtering targets from exposure to the plasma or expose certain targets to the plasma. The shield is rotated during various operations of method 100B to sequentially or simultaneously expose two or more targets to the plasma within the PVD chamber.

[0023]

[0030] 1A are therefore referenced herein with respect to method 100B. Operations of method 100B are performed in one or more PVD chambers using one or more gases including argon (Ar), helium (He), krypton (Kr), xenon (Xe), oxygen (O), or nitrogen (N). The process pressure in the PVD chambers may be about 2 mTorr to about 3 mTorr during method 100B. Depending on the embodiment, the PVD chamber may be maintained at a temperature between −200° C. and 600° C. during fabrication of the pinning and seed layers of the MTJ stack.

[0024]

[0031] The substrate 102 can be moved between and among PVD chambers depending on the composition of the sputtering target(s) used for each layer of the MTJ stack 100A, or, as described herein, multiple targets can be connected to a power source and shields configured to selectively protect portions of the targets, thereby exposing one or more targets sequentially or simultaneously to form a desired film composition, or both techniques can be performed. During sputtering in the PVD chamber, Ar ions from the plasma bombard one or more exposed sputtering targets, ejecting surface atoms of the sputtering targets and depositing them as a thin film on the substrate. In method 100B, in operation 128A, a substrate, such as the substrate 102 of FIG. 1A, undergoes operations including outgassing, pre-cleaning in an Ar gas plasma or a He / H plasma, and moving between processing chambers through or via a central robot substrate transfer chamber. In operation 128B, the substrate 102 is transferred from the central robot substrate transfer chamber to one of the multiple PVD chambers. Subsequently, in operation 130, the buffer layer 104 is deposited on the substrate 102 by sputtering at a target in a PVD chamber. A power of 1 kW to 100 kW is applied to one or more PVD chambers described herein to ionize a portion of the Ar and generate the plasma used in operation 130. The ejected surface atoms of the target are deposited on the substrate 102 to form the buffer layer 104. During the formation of the buffer layer 104 in operation 130, Co x Fe y B zOne or more sputtering targets comprising TaN, TaN, and / or Ta are used in a PVD chamber with an Ar plasma to form buffer layer 104. In one embodiment in which buffer layer 104 is or includes Ta, buffer layer 104 is sputtered in a PVD chamber using a Ta target and an Ar plasma. In one example in which buffer layer 104 is or includes TaN, operation 130 is performed when nitrogen gas (N) is present in the PVD chamber with an Ar plasma and a Ta sputtering target to form TaN buffer layer 104. In another example in which buffer layer 104 is or includes TaN, operation 130 is performed in a PVD chamber using a TaN sputtering target and an Ar plasma to form TaN buffer layer 104. During the formation of buffer layer 104 and subsequent layers, one or more PVD chambers used are maintained at reduced pressure.

[0025]

[0032] Subsequently, in operation 132, the seed layer 106 is deposited on the buffer layer 104 by sputtering a target in the PVD chamber. In one embodiment of operation 132, the seed layer 106 is formed in the same PVD chamber used to form the buffer layer 104, but using a different sputtering target than the sputtering target used to form the buffer layer 104. In one example of method 100B according to embodiments of the present disclosure, the seed layer 206 shown in FIG. 2A below may be fabricated in operation 132 in a PVD chamber using an Ar plasma and one or more sputtering targets. FIG. 2A illustrates a coordinate system with an x-axis 226 perpendicular to a y-axis 228. Thicknesses described herein may be measured in the direction of the y-axis 228. In one example of forming the seed layer 206, the sputtering target in the PVD chamber used to form the seed layer is composed of Cr or a combination of Cr with one or more of Ni, Fe, Ru, Ir, and Co. In another embodiment, the sputtering target(s) used in the PVD chamber in operation 132 comprises one or more alloy targets including NiCr, NiCrFe, RuCr, IrCr, CoCr, or combinations thereof. Seed layer 206 can be formed to a thickness of 100 Å or less. In one embodiment, seed layer 206 comprises NiCr and is fabricated in the PVD chamber using a NiCr target. In this embodiment, Ar is introduced into the PVD chamber at a flow rate of approximately 5 sccm to 60 sccm, and in some embodiments, the flow rate of Ar into the chamber is approximately 25 sccm. In another embodiment, Ar is introduced into the PVD chamber at a flow rate of 10 sccm to 40 sccm, and in some embodiments, at a flow rate of 25 sccm. To form the plasma used for sputtering, a power of approximately 50 W to 1200 W at a negative voltage is applied to the sputtering target in the presence of Ar. In some embodiments, the power applied to the sputtering target at the negative voltage is between 100 W and 800 W, and in another embodiment, the power applied to the sputtering target is about 500 W.

[0026]

[0033] The first pinning layer 108 is deposited on the seed layer 106 in operation 134 by sputtering a target in a PVD chamber. The first pinning layer 108 is shown as an example of a conventional MTJ stack 100A and can be formed in operation 134 in a PVD chamber by sputtering one or more targets in the presence of an Ar plasma. In an example where the first pinning layer 108 is Co, a Co sputtering target is used in the presence of an Ar plasma in the PVD chamber. In an example where the first pinning layer 108 includes one or more bilayers of cobalt and another element, operation 134 uses a Co sputtering target and another sputtering target of the other element of the bilayer. Depending on the embodiment, the Co sputtering target and the sputtering target of the other metal can be sputtered in the same PVD chamber in the presence of an Ar plasma, or each layer of the bilayer can be formed in a separate PVD chamber.

[0027]

[0034] According to one embodiment of the present disclosure, first pinning layer 208, as shown in FIGS. 2A and 2C, is formed in operation 134 using a PVD chamber. In this embodiment, first pinning layer 208 is formed in operation 134 in a PVD chamber using xenon (Xe) or argon (Ar), which are introduced into the PVD chamber at a flow rate of approximately 2 sccm to 40 sccm, and a power of 50 W to 10,000 W is applied to the target at a negative voltage to generate a plasma. In another embodiment, Xe or Ar is introduced into the PVD chamber at a flow rate of 5 sccm to 20 sccm, and in some embodiments, at a flow rate of 10 sccm. In another embodiment, the power applied to the sputtering target is 100 W to 800 W, and in another embodiment, the power applied to the sputtering target may be 400 W. Depending on the composition of first pinning layer 208, Xe may be used in the sputtering operation in the PVD chamber in operation 134 because Xe is a heavier gas than Ar and therefore produces ions with a higher atomic weight and therefore impact the target with more energy than ions formed using Ar or other lighter gases. In one embodiment of first pinning layer 208 in the present disclosure, Xe, Ar, or a mixture thereof is introduced into the PVD chamber at a flow rate of from about 10 sccm, and 400 W of power is applied to the target at a negative voltage to generate an Ar plasma. In one embodiment, first pinning layer 208 is fabricated from cobalt (Co) as a single layer about 1 Å to about 18 Å thick by sputtering a Co target. In another embodiment, first pinning layer 208 is fabricated from one or more bilayers of various materials, as shown in FIG. 2C. In various embodiments, the bilayer used to form first pinning layer 208 includes a first intermediate layer of Co and a second intermediate layer of another element. The bilayer of first pinning layer 208 may be formed in operation 134 in a PVD chamber that includes multiple targets, including a Co target and a target formed from the other element, or in separate PVD chambers.In separate PVD chambers, one PVD chamber contains a Co target and another PVD chamber contains a target of the other element. In one example where multiple targets are disposed in a single PVD chamber in the presence of an Ar plasma and / or a Xe plasma, each of the Co target and the other metal target may be selectively exposed using a shield as described herein to form a bilayer Co interlayer and an interlayer of the other element to form a resulting bilayer. These depositions may be repeated in operation 134 in multiple iterations to form multiple bilayers of first pinning layer 208.

[0028]

[0035] In operation 136, SAF bonding layer 110 is deposited on first pinning layer 108 by sputtering a Ru, Cr, Rh, or Ir target in the presence of an Ar plasma in the PVD chamber. Second pinning layer 112 is deposited on the SAF bonding layer in the PVD chamber in operation 138. In one example, second pinning layer 112 is formed from Co using a Co target and an Ar plasma in the PVD chamber. In another example, second pinning layer 112 includes a bilayer that may or may not include a Co layer formed in contact with the bilayer. In this example, second pinning layer 112 is formed in the PVD chamber using a Co sputtering target and a second metal sputtering target, and a shield is adjusted to separately expose each of the Co sputtering target and the second metal sputtering target in at least one iteration to form one or more bilayers of second pinning layer 112. In other embodiments, each layer of the bilayer of second pinning layer 112 may be formed in a different PVD chamber, where one PVD chamber contains a Co sputtering target and another PVD chamber contains a sputtering target of a second metal.

[0029]

[0036] 2A and 2D , second pinning layer 212 is deposited in a PVD chamber using Ar and / or Xe gas in operation 138, depending on the material being sputtered. In one embodiment of the present disclosure, second pinning layer 212 is fabricated as a single layer from cobalt (Co) in operation 138 using a Co sputtering target in the presence of an Ar plasma or a plasma consisting of Ar and Xe. In another example, second pinning layer 212 includes a bilayer including a first intermediate layer formed from Co and a second intermediate layer of one or more second metals, such as Pt, Ir, Ni, or Pd. In another example, which may be combined with other examples herein, second pinning layer 212 may be formed from a single Co layer alone or a single Co layer combined with at least one bilayer of a first intermediate layer of Co and a second intermediate layer of at least one different metal. In this example, second pinning layer 212 is formed in a PVD chamber using a Co sputtering target and a second metal sputtering target, and a shield is adjusted to separately expose each of the Co sputtering target and the second metal sputtering target in at least one iteration to form one or more bilayers of second pinning layer 212. Because Xe is a heavier gas than Ar and therefore can interact more effectively with heavier metals, including Pt, during the sputtering process in the PVD chamber, xenon can be used to deposit second pinning layer 212 when a metal such as Pt is used to form second pinning layer 212. In one embodiment where Xe is used, Xe gas is introduced into the PVD chamber at a flow rate of about 2 sccm to about 40 sccm, or 5 sccm to 20 sccm, and in some embodiments, Xe gas is introduced into the PVD chamber at a flow rate of about 10 sccm. During the formation of the second pinning layer 212, a power of 50 W to about 1000 W is applied to the target at a negative voltage to generate and maintain an Ar and / or Xe plasma.In some examples, a power of 100 W to 600 W is applied to the target at a negative voltage to generate and sustain the Ar and / or Xe plasma, and in some embodiments, a power of about 200 W is used.

[0030]

[0037] The structural blocking layer 114 is formed in an operation 140 in a PVD chamber. The chamber includes sputtering targets containing Ta, Mo, and / or W, depending on the intended composition of the structural blocking layer 114. When two or more sputtering targets of Ta, Mo, and W are used, each target may be used in a separate PVD chamber, or two or more sputtering targets may be sputtered sequentially or simultaneously in the PVD chamber using the shielding adjustments described above, depending on the intended composition of the structural blocking layer 114. The magnetic reference layer 116 is then deposited on the structural blocking layer 114 in operation 142, and may be formed in the PVD chamber in which the other layers of the MTJ stack 100A may also be formed. This may be the case, for example, when both the buffer layer 104 and the magnetic reference layer 116 are made of Co. x Fe y B z If it is based, it may depend on the composition of other layers such as the buffer layer 104. The magnetic reference layer 116 is Co x Fe y B z or by using individual sputtering targets of Co, Fe, or B, or by a combination of alloy sputtering targets and single element sputtering targets, e.g., a CoFe target and a B target.

[0031]

[0038] The tunnel barrier layer 118 is deposited on the magnetic reference layer 116 in operation 144. In one implementation of operation 144, the tunnel barrier layer 118 is formed in a PVD chamber using a metal-oxide target, such as MgO, in the presence of an Ar plasma. In an alternative embodiment, the tunnel barrier layer 118 is formed in operation 144 in a PVD chamber using a metal target, such as Mg, Ti, Hf, Ta, or Al, in the presence of an Ar plasma and O to form the metal-oxide of the tunnel barrier layer 118. In operation 146, the magnetic memory layer 120 is formed in the PVD chamber. The formation of the magnetic memory layer 120 can be done in various ways depending on the intended composition. Additionally, the magnetic memory layer 120 can be formed using a Co x Fe y B z In some embodiments, which may be combined with other embodiments, the magnetic storage layer 120 may include one or more layers of Ta, Mo, W, or Hf. Thus, deposition of the magnetic storage layer 120 in a PVD chamber may involve the use of an Ar plasma, Co x Fe y B z The sputtering targets may include alloy targets, individual targets of Co, Fe, and B, or a combination of alloy and elemental targets, such as a CoFe target and a B target. In embodiments where the magnetic storage layer 120 includes Ta, Mo, W, or Hf, a sputtering target of Ta, Mo, W, or Hf is used in the chamber with a plasma formed from Ar.

[0032]

[0039] In one embodiment, the magnetic storage layer 120 is Co x Fe y B z In another example, the magnetic storage layer 120 may be formed in a single PVD chamber in the presence of a plasma generated using Ar by adjusting shields to expose or protect one or more targets such as those used to form the Ta, Mo, W, or Hf layers. x Fe y B z The layer was deposited by Co x Fey B z In another embodiment, the alloy is sputtered in a PVD chamber using a Co alloy target. x Fe y B z The layer is formed in a PVD chamber using individual Co, Fe, and B targets in the presence of an Ar plasma. x Fe y B z The layers are formed in a PVD chamber using alloy and elemental targets, such as CoFe and B targets, in the presence of an Ar plasma. Ta, Mo, W, or Hf layers may be sputtered in a PVD chamber using a Ta target, a Mo target, a W target, or a Hf target.

[0033]

[0040] In operation 148, the capping layer 122 is deposited on the magnetic storage layer 120. In one embodiment, the first capping interlayer 122A of the capping layer 222 is formed during operation 148 in a PVD chamber that may be different from the PVD chamber in which the non-oxide layer is formed because both Ar plasma and O2 are present in the PVD chamber when the oxide layer is formed. The first capping interlayer 122A is deposited in the PVD chamber by sputtering an Mg target, and a plasma formed from ionized Ar and O2 is also present in the PVD chamber. In another example implementation of operation 148, the first capping interlayer 122A is formed in the PVD chamber using an MgO sputtering target and an Ar plasma. In an example implementation in which the first capping interlayer 122A is formed from the same material (e.g., Mg) as the tunnel barrier layer 118, the PVD chamber used in operation 144 may be the same PVD chamber used in operation 148 to form the first capping interlayer 122A. Second capping interlayer 122B is deposited on first capping interlayer 122A in operation 150. Operation 150 may be performed in a separate PVD chamber from the one used to sputter first capping interlayer 122A if O is used in operation 148 because there is no O used in the PVD chamber to form first capping interlayer 122A. Second capping interlayer 122B is formed in the PVD chamber using an Ar plasma and one or more sputtering targets comprised of Ru, Ir, and / or Ta. Depending on the composition of second capping interlayer 122B, operation 150 may be performed, for example, in the PVD chamber also used to form SAF bond layer 110 in operation 136.

[0034]

[0041] Further, in the method 100B, in operation 152, a hard mask layer 124 is deposited on the second capping interlayer 122B in a PVD chamber. Depending on the type of hard mask layer 124 used in the MTJ stack 100A, operation 152 may be performed in the presence or absence of O. For example, if the hard mask layer 124 is a metal-oxide hard mask, O may be used with one or more metal targets to form the metal-oxide layer during operation 152, or a metal-oxide sputtering target may be used to deposit the hard mask layer 124, in which case O is not used to form the hard mask layer 124 in operation 150. In some embodiments, when the hard mask layer 124 is amorphous carbon or spin-on carbon, operation 152 is performed in a CVD chamber.

[0035]

[0042] Further, in method 100B, the MTJ stack 100A (or MTJ stack 200 shown below in FIG. 2A ) formed in operations 128A-152 may undergo one or more processes collectively denoted by operation 154 of method 100B. These operations may include high-temperature (on the order of 400 degrees Celsius) operations. In one example, the process in operation 154 may include a pre-patterning anneal operation, followed by an MTJ patterning operation. In an alternative embodiment, the MTJ patterning in operation 154 may include multiple processes, such as patterning the hard mask layer 124, and may further include etching the MTJ stack 100A to form a plurality of individual pillars from the MTJ stack after the hard mask layer 124 is patterned.

[0036]

[0043] In an alternative embodiment, in operation 154, a thermal annealing operation is performed to repair, compact, and strengthen the lattice structure of the film stack, including the magnetic storage layer(s) and magnetic reference layer(s) in the MTJ stack 100A. The thermal annealing performed in operation 154 can act to further crystallize the material of at least the magnetic reference layer(s) 116 and the magnetic storage layer(s) 120. The crystallization of the magnetic reference layer(s) and magnetic storage layer(s) as deposited of these layers establishes perpendicular anisotropy in the MTJ stack 100A while maintaining desired electrical and mechanical properties. An embodiment of an MTJ stack fabricated following the operations of method 100B is shown and described below. The embodiment may further include maintaining the as-deposited fcc (fcc) pinning layer after the thermal annealing operation performed in operation 154 and / or during additional or alternative back-end processing operations that occur at elevated temperatures on the order of 400 degrees Celsius. <111> It is configured to maintain a crystalline structure.

[0037]

[0044] MTJ stacks fabricated according to embodiments of the present disclosure employ chromium-based seed layers, including seed layers comprising at least one of chromium (Cr), nickel chromium (NiCr), iron nickel chromium (NiFeCr), ruthenium chromium (RuCr), iridium chromium (IrCr), or cobalt chromium (CoCr), as opposed to the conventional use of Ru or Ir for the seed layer. The seed layer is disposed within the film stack from which memory cells are defined between the first pinning layer and the buffer layer. The Cr-containing seed layer described herein improves adhesion of the first pinning layer due to the lattice match between the seed layer and the first pinning layer, which helps stabilize the first pinning layer and layers formed on top of the first pinning layer. In one example, the seed layer directly contacts both the first pinning layer and the buffer layer, while in other examples, a transition layer exists between the sheet layer and the first pinning layer or between the seed layer and the buffer layer. The pinning layers described herein may be fabricated from cobalt, or may be fabricated as one or more bilayers each containing cobalt, or as a combination of a bilayer structure and a cobalt overlayer, as described below. As described herein, an “overlayer” is a layer formed on another structure, which may include one or more layers, including a bilayer. Depending on the embodiment, the first pinning layer and the second pinning layer may include the same layer structure, materials, and / or thickness, or may have different layer structures, materials, and / or thicknesses. Using the MTJ stacks described herein, the crystal structure of the SAF layer and the magnetic coupling between the magnetic reference layer and the magnetic storage layer remain substantially constant crystalline even after annealing the layers at about 400° C. for a period of 0.5 to at least 3 hours. Furthermore, in embodiments herein, the MTJ stack continues to exhibit tunneling magnetoresistance (TMR) of 100% to 175% even after annealing at about 400 degrees Celsius for 0.5 hours to at least 3 hours.

[0038]

[0045] 2A is a schematic diagram of an MTJ stack 200 according to one embodiment of the present disclosure. In the illustrated embodiment, a buffer layer 204 is formed on a conductive portion of a substrate 202 or on a conductive thin film of the substrate 202 via sputtering in a PVD chamber. The substrate 202 may include tungsten (W), tantalum nitride (TaN), titanium nitride (TiN), or other metal layer. The buffer layer 204 improves adhesion of a seed layer 206 to the substrate 202, which aids in the formation and performance of subsequently deposited layers of the MTJ stack 200. The buffer layer 204 is made of Co x Fe y B z In various embodiments, the buffer layer 104 comprises Co, Ta, and / or TaN and is formed in one or more PVD deposition operations in a PVD chamber in the presence of an Ar plasma. x Fe y B z The buffer layer 204 may be formed in a PVD chamber using a sputtering target that is an alloy, or by using individual sputtering targets of Co, Fe, or B, or by a combination of an alloy sputtering target and a single element sputtering target, such as a CoFe target and a B target. In one example where a Ta layer is included in the buffer layer 204, the Ta layer may be formed in a PVD chamber using a Ta target and an Ar plasma.

[0039]

[0046] In one example, the buffer layer 204 includes TaN and is sputtered onto the substrate 202 in a PVD chamber using a Ta target in the presence of both an Ar plasma and N2, where the N2 reacts with the Ta material sputtered from the Ta target to form a TaN layer. In another example, a TaN sputtering target is used in a PVD chamber with an Ar plasma to form the buffer layer 204. In one example, the buffer layer 204 is sputtered directly onto and in contact with a conductive layer on the substrate 202. In another example, a conductive transition layer is present between the conductive layer on the substrate 202 and the buffer layer 204, which does not affect the performance of the MTJ stack. The buffer layer 204 is optional in the illustrated embodiment and may not be used in some embodiments described herein. The total thickness of the buffer layer 204 is from 0 Å (no buffer layer used) to about 60 Å. In one embodiment, buffer layer 204 is a Ta, TaN, or Co layer sputtered to a thickness of 10 Å directly on and in contact with the conductive layer on substrate 202. x Fe y B z In another embodiment, the buffer layer 204 is a combination of multiple layers, each layer of the buffer layer 204 being Ta, TaN, or Co. x Fe y B z and has a thickness of 1 Å to 60 Å. Ta or Co x Fe y B z In one embodiment, where TaN is used for buffer layer 204 instead of Co, the thickness may be 20 Å. x Fe y B z In one embodiment of buffer layer 204 using Co alone, the layer has a thickness of 10 Å. In another embodiment of buffer layer 204, Ta or TaN is used in combination with Co x Fe y B z The thickness of the buffer layer 204 is 20 Å.

[0040]

[0047] The seed layer 206 is deposited in a PVD chamber by sputtering one or more targets. The seed layer 206 is deposited on the buffer layer 204. The seed layer 206 includes Cr, NiCr, NiCrFe, RuCr, IrCr, CoCr, or a combination thereof. The seed layer 206 may be formed as one or more layers of Cr, NiCr, NiCrFe, RuCr, IrCr, or CoCr, and may include a combination or alloy combination of these elements in a single layer. The formation of the seed layer 206 in the PVD chamber is described in detail above in operation 132. In one embodiment, the seed layer 206 has a thickness of 100 Å or less, and in one example, the seed layer 206 has a thickness of about 30 Å to about 60 Å. In one example, the seed layer 206 is formed directly on and in contact with the buffer layer 204. In another example, there is a transition layer between the seed layer 206 and the buffer layer 204 that does not affect the performance of the MTJ stack.

[0041]

[0048] Further, in the MTJ stack 200, a first pinning layer 208 is formed on the seed layer 206 in a PVD chamber. The formation of the first pinning layer 208 is described in detail above in operation 134 of method 100B of FIG. 1B and is performed in a PVD chamber using an ionized Ar plasma and one or more sputtering targets. In one example, the first pinning layer 208 is fabricated as a single layer of cobalt (Co) having a thickness of about 1 Å to about 18 Å. In another example, the first pinning layer 208 is fabricated from one or more bilayers of different materials, each of which may include two intermediate layers. The first pinning layer 208 may include one or more bilayers alone or in combination with a Co layer, as shown in FIG. 2C. In one example where more than one bilayer is included in the first pinning layer 208, each bilayer includes a first intermediate layer of Co and a second intermediate layer of another element. The first pinning layer 208 is formed by sputtering a Co target using an Ar plasma, followed by sputtering a second target of Pt, Ir, Ni, or Pd using the Ar plasma. In an example where Pt is used with Co to form the bilayer, a Xe plasma can be used instead of or in addition to the Ar plasma. In an embodiment where one or more bilayers are used to form the first pinning layer, repeated deposition cycles can be performed in a PVD chamber by shielding a target that does not contain Co to form a first intermediate layer of the bilayer (the first intermediate layer includes Co). The Co target and other targets are then shielded to expose a second target containing a second element used in the second intermediate layer of the bilayer. This can be repeated in an iterative manner to form one or more bilayers of the first pinning layer 208. In one example, the first pinning layer 208 is formed in a PVD chamber directly on and in contact with the seed layer 206. In other embodiments, there is a transition layer between the seed layer 206 and the first pinning layer 208 that does not affect the performance of the MTJ stack.

[0042]

[0049] A synthetic antiferromagnet (SAF) coupling layer 210 is sputter-deposited on the first pinning layer 208 in a PVD chamber, and a second pinning layer 212 is sputter-deposited on the SAF coupling layer 210. The SAF coupling layer 210 is formed in the PVD chamber using a Ru sputtering target, a Rh sputtering target, a Cr sputtering target, or an Ir sputtering target in the presence of a plasma generated from ionized Ar gas. The SAF coupling layer 210 has a thickness of about 3 Å to about 10 Å. In one embodiment, the second pinning layer 212 is fabricated by sputtering a cobalt (Co) target in the PVD chamber in the presence of a plasma generated from ionized Ar gas. In one example, the SAF coupling layer 210 is formed directly on and in contact with the first pinning layer 208 and the second pinning layer 212. In other embodiments, there is a transition layer between the SAF coupling layer 210 and one or both of the first pinning layer 208 or the second pinning layer 212 that does not affect the performance of the MTJ stack.

[0043]

[0050] Formation of second pinning layer 212 is shown in act 138 of method 100B of FIG. 1B above. In one example where second pinning layer 212 includes one or more bilayers of Co and another element, second pinning layer 212 is formed by sputtering a Co target using an Ar plasma, followed by sputtering a second target of Pt, Ir, Ni, or Pd using an Ar plasma. Repeated deposition cycles in a PVD chamber using a Co target and a second target in the presence of an Ar plasma can be used to form the one or more bilayers of second pinning layer 212. In one example, second pinning layer 212 is sputtered as a single Co layer having a thickness of about 1 Å to about 10 Å. In another example, second pinning layer 212 has a thickness of about 5 Å. An alternative configuration of second pinning layer 212 is shown in FIG. 2D .

[0044]

[0051] Further, in the MTJ stack 200, a structural blocking layer 214 is optionally formed on the second pinning layer 212 by sputtering in a PVD chamber. The structural blocking layer 214 prevents the formation of a short circuit between the MTJ stack 200 and a metal contact that may be connected to the MTJ stack 200 to form an MRAM memory cell. During sputtering of the structural blocking layer 214, one or more individual Ta, Mo, or W sputtering targets may be used in the PVD chamber with an Ar plasma, depending on the intended composition of the layer. In another embodiment, during the formation of the structural blocking layer 214, one or more alloy targets including an alloy of Ta, Mo, and / or W may be used in the PVD chamber with an Ar plasma. The structural blocking layer 214 is <100> It has a body-centered cubic (bcc) structure oriented in the direction, and each has a face-centered cubic <111> This contrasts with seed layer 206 and first and second pinning layers 208 and 212, which may be oriented in any direction. Structure blocking layer 214 has a thickness of 0 (no layer) to about 8 Å, and in one example is sputter deposited to a thickness of 4 Å. In one example, structure blocking layer 214 is formed directly on and in contact with second pinning layer 212 during sputter deposition. In other examples, there is a transition layer between structure blocking layer 214 and second pinning layer 212 that does not affect the performance of the MTJ stack.

[0045]

[0052] The magnetic reference layer 216 is formed on the structural blocking layer 214 by sputter deposition in a PVD chamber in the presence of an Ar plasma. The magnetic reference layer 216 may be formed in the PVD chamber using a single Co-Fe-B alloy sputtering target, or by using two or more of a Co sputtering target, an Fe sputtering target, or a B sputtering target. In another embodiment, the magnetic reference layer 216 may be formed in the PVD chamber in the presence of an Ar plasma using an alloy target and an elemental target, such as a CoFe target and a B target. The magnetic reference layer 216 may be sputtered to a thickness of 1 Å to 15 Å, and in one embodiment, may be formed to a thickness of 10 Å. The magnetic reference layer 216 may be formed using a CoFe target and an elemental target. x Fe y B z In one embodiment, z is about 10% to about 40% by weight, y is about 20% to about 60% by weight, and x is less than or equal to 70% by weight. In another embodiment, which may be combined with other embodiments herein, z is at least 20% by weight. In one embodiment, the magnetic reference layer 216 is formed directly on and in contact with the structural blocking layer 214. In another embodiment, there is a transition layer between the magnetic reference layer 216 and the structural blocking layer 214 that does not affect the performance of the MTJ stack.

[0046]

[0053] A tunnel barrier layer 218 is formed on the magnetic reference layer 216 using sputtering of a target in an Ar plasma in a PVD chamber. The tunnel barrier layer 218 may be made of magnesium oxide (MgO), hafnium dioxide (HfO), titanium dioxide (TiO), tantalum oxide (TaO), or other suitable materials. xThe tunnel barrier layer 218 may comprise a metal-oxide, such as aluminum oxide (Al2O3), aluminum oxide (Al2O3), or other material suitable for various applications. Therefore, the tunnel barrier layer 218 may be formed in the presence of Ar in a PVD chamber using a metal-oxide sputtering target. Alternatively, the tunnel barrier layer 218 may be formed in the presence of Ar and O2 in a PVD chamber using a metal sputtering target of the desired metal-oxide. Here, the metal oxide layer is formed when the metal layer sputtered from the metal sputtering target is exposed to O2. The tunnel barrier layer 218 has a thickness of 1 Å to 15 Å, and in some embodiments, a thickness of 10 Å. In one example, the tunnel barrier layer 218 is formed directly on and in contact with the magnetic reference layer 216. In another example, there is a transition layer between the tunnel barrier layer 218 and the magnetic reference layer 216 that does not affect the performance of the MTJ stack.

[0047]

[0054] In one embodiment, the MTJ stack 200 further includes a magnetic storage layer 220 formed on the tunnel barrier layer 218 using a sputtering operation in a PVD chamber as described herein. The magnetic storage layer 220 is Co x Fe y B z In some embodiments, magnetic storage layer 220 may alternatively or additionally include one or more layers of Ta, Mo, W, or Hf. Thus, deposition of magnetic storage layer 220 in a PVD chamber may involve the use of Ar plasma, Co x Fe y B z This may include using alloy targets, or individual targets of Co, Fe, and B, or a combination of alloy and elemental targets, such as a CoFe target and a B target. In embodiments where the magnetic storage layer 220 includes Ta, Mo, W, or Hf, a sputtering target of Ta, Mo, W, or Hf is used in the chamber with a plasma generated from Ar.

[0048]

[0055] The magnetic storage layer 220 has a thickness of about 5 Å to about 20 Å, depending on factors including one or more materials used to form the magnetic storage layer 220. In one embodiment, the magnetic storage layer is Co x Fe y B z where z is about 10% to about 40% by weight, y is about 20% to about 60% by weight, and x is less than or equal to 70% by weight. In this embodiment, the magnetic storage layer 220 has a thickness of 5 Å to 40 Å, and in some embodiments, the target layer thickness is 20 Å. In one embodiment, the magnetic storage layer 220 is formed directly on and in contact with the tunnel barrier layer 218. In other embodiments, there is a transition layer between the magnetic storage layer 220 and the tunnel barrier layer 218 that does not affect the performance of the MTJ stack. The magnetic storage layer is shown in FIG. 2E below.

[0049]

[0056] Further, in one embodiment of the MTJ stack 200, the capping layer 222 is formed on the magnetic memory layer 220 and includes multiple intermediate layers forming the capping layer 222, including an oxide containing iron (Fe). Additionally, in some embodiments, a hard mask layer 224 is formed directly on and in contact with the capping layer 222. In another example, the hard mask layer 224 is formed on the capping layer 222 with a transition layer between the capping layer 222 and the hard mask layer 224, which does not affect the performance of the MTJ stack 200. The hard mask layer 224 may be formed from a metal-oxide, amorphous carbon, ceramic, metallic material, or a combination thereof. In one example, the magnetic memory layer 220 is formed directly on and in contact with the capping layer 222. In other examples, there is a transition layer between the magnetic memory layer 220 and the capping layer 222 that does not affect the performance of the MTJ stack 200. Capping layer 222 is shown below in FIG. 2F.

[0050]

[0057] In one embodiment of the MTJ stack 200, the MTJ stack 200 includes a seed layer 206 made of NiCr, a first pinning layer 208 made of a Co / Pt bilayer stack, and a second pinning layer 212 made of Co. In this embodiment, the MTJ stack 200 exhibits a TMR of 175% when annealed at, for example, about 400 degrees Celsius for 0.5 hours. The TMR of the MTJ stack 200 remains at about 175% when annealed at about 400 degrees Celsius for 3 hours.

[0051]

[0058] 2B is an expanded view of buffer layer 204 according to an embodiment of the present disclosure. Buffer layer 204 may include tantalum (Ta) or TaN, or a layered stack of Ta and TaN, and in some examples, Co. x Fe y B z , alone or in combination with Ta, TaN, or a Ta / TaN layered stack. In one embodiment of the buffer layer 204, the buffer layer 204 includes at least one bilayer 204D. The at least one bilayer 204D includes a first buffer interlayer 204A and a second buffer interlayer 204B formed in an alternating manner on the substrate 202 for at least one repetition of the at least one bilayer 204D. In this embodiment, the first buffer interlayer 204A includes Ta and the second buffer interlayer 204B includes TaN, with the first buffer interlayer 204A in contact with the substrate 202. In another embodiment, the first buffer interlayer 204A includes TaN and the second buffer interlayer 204B includes Ta, such that the TaN is in direct contact with the substrate 202.

[0052]

[0059] Another embodiment of the buffer layer 204 is shown in FIG. 2A. x Fe y B z is used solely for the buffer layer 204, and is therefore in direct contact with the substrate 202. In another embodiment, as shown in FIG. 2B, a third buffer layer 204C is formed on the at least one bilayer 204D. In this embodiment, the third buffer layer 204C is made of Co x Fe y B zThe third buffer layer 204C (Co) is fabricated from a SiO 2 film and formed to have a thickness of up to 10 Å. Depending on the configuration of the buffer layer 204, the thickness of the buffer layer 204 may range from 1 Å to 60 Å. x Fe y B z In one embodiment where y is employed, z is from about 10% to about 40% by weight, y is from about 20% to about 60% by weight, and x is 70% or less by weight.

[0053]

[0060] 2C is a close-up view of the first pinning layer 208, according to one embodiment of the present disclosure. In one embodiment, the first pinning layer 208 is fabricated from at least one bilayer 230; when two or more bilayers are employed, the bilayers can be said to form a bilayer stack 234. Each bilayer 230 is fabricated from a first intermediate layer 208A and a second intermediate layer 208B. The bilayers of the first pinning layer 208 are (X / Y) n , (208A / 208B) nwhere each bilayer is a combination of X and Y materials, and n is the number of bilayers in first pinning layer 208. In one embodiment, X is Co and Y is one of Pt, Ir, Ni, or Pd. In FIG. 2C , n=4, but in alternative embodiments, n is 1 to 10. In one embodiment, at least one bilayer 230 has a thickness of about 2 Å to about 15 Å. In one example, first intermediate layer 208A includes Co and has a thickness of about 1 Å to about 7 Å, and second intermediate layer 208B has a thickness of about 1 Å to about 8 Å. In another example, the desired layer thickness of each of first intermediate layer 208A and second intermediate layer 208B is about 2.4 Å to about 5 Å. In yet another embodiment, first pinning layer 208 includes at least one bilayer 230 formed directly on and in contact with seed layer 206, and a Co overlayer 208C formed on top of at least one bilayer 230. In this example, overlayer 208C has a thickness of about 1 Å to about 10 Å. Depending on the embodiment, first pinning layer 208, which may include one or more layers including at least one bilayer 230 as described herein, has an overall thickness of 0.3 nm to about 18 nm. In other examples, there are one or more transition layers between first pinning layer 208 and seed layer 206 that do not adversely affect the properties of the MTJ stack.

[0054]

[0061] FIG. 2D is an expanded view of second pinning layer 212 according to an embodiment of the present disclosure. In one embodiment, second pinning layer 212 is fabricated from a single cobalt layer, as shown in FIG. 2A. In an alternative embodiment, second pinning layer 212 is fabricated from at least one bilayer 232. At least one bilayer 232 includes a first intermediate layer 212A formed from Co and a second intermediate layer 212B formed from one or more of Pt, Ir, Ni, or Pd. When two or more bilayers, such as bilayer 232, are employed in second pinning layer 212, the multiple bilayers may be referred to as a bilayer stack 236. Thus, in operation 138 of FIG. 1B, when more than one bilayer is used, a separate sputtering target may be used to form each layer of the bilayer. At least one bilayer 232 of second pinning layer 212 may be fabricated from an (X / Y) n , (212A / 212B) n 2D, n=4, while in alternative embodiments, n is 1 to 10. In one embodiment, at least one bilayer 232 has an overall thickness of about 2 Å to about 15 Å. In one example, first interlayer 212A is a Co layer having a thickness of about 1 Å to about 7 Å, and second interlayer 212B has a thickness of about 1 Å to about 8 Å. In another example, first interlayer 212A and second interlayer 212B each have a thickness of about 2.4 Å to about 5 Å.

[0055]

[0062] In yet another embodiment, the second pinning layer 212 includes at least one bilayer 232 formed directly on and in contact with the SAF coupling layer 210, and further includes a Co overlayer 212C on top of the at least one bilayer 232. In some embodiments, a transition layer may be employed between the at least one bilayer 232 and the second pinning layer 212, or between the at least one bilayer 232 and the SAF coupling layer 210, or both, and such transition layer(s) does not affect the performance of the MTJ stack. In this example, the overlayer 212C has a thickness of about 1 Å to about 10 Å. Depending on the embodiment, the overall thickness of the second pinning layer 212 is 0.3 nm to about 18 nm. The second pinning layer 212 may include one or more layers, including the at least one bilayer 232, as described herein.

[0056]

[0063] In one embodiment, first pinning layer 208 and second pinning layer 212 each have at least one of the same composition and the same thickness. In an alternative embodiment, first pinning layer 208 and second pinning layer 212 each have a different composition and / or thickness. In one embodiment, first pinning layer 208 is Co, and second pinning layer 212 is formed from one or more bilayers. Each bilayer of second pinning layer 212 includes a first intermediate layer of Co and a second intermediate layer of Pt. In another embodiment, first pinning layer 208 is Co, and second pinning layer 212 is formed from one or more Co / Ni bilayers. In yet another embodiment, first pinning layer 208 includes one or more bilayers, each bilayer including a first intermediate layer of Co and a second intermediate layer of Ni, and second pinning layer 212 includes one or more bilayers, each bilayer including a first intermediate layer of Co and a second intermediate layer of Pt. In yet another embodiment, first pinning layer 208 includes one or more bilayers, each bilayer including a first intermediate layer of Co and a second intermediate layer of Pt, and second pinning layer 212 includes one or more bilayers, each bilayer including a first intermediate layer of Co and a second intermediate layer of Ni.

[0057]

[0064] 2E is an enlarged view of an exemplary magnetic storage layer 220 according to an embodiment of the present disclosure. As shown in FIG. 2E, the first magnetic layer 220A of the magnetic storage layer 220 and the second magnetic layer 220B of the magnetic storage layer 220 are each made of Co x Fe y B z The magnetic storage layer 220 is fabricated from a first magnetic layer 220A, a second magnetic layer 220B, and a third layer 220C disposed between the first magnetic layer 220A and the second magnetic layer 220B. The third layer 220C enhances the pinning moment perpendicular to the substrate plane (e.g., a plane perpendicular to the substrate 202), which promotes magnetic anisotropy, i.e., the directional dependence of the magnetic properties of the structure.

[0058]

[0065] 2F is an enlarged view of an exemplary capping layer 222 according to one embodiment of the present disclosure. The overall thickness of the capping layer 222 is 2 Å to 120 Å, and in some embodiments, the overall desired thickness of the capping layer (e.g., including all of the interlayers as shown in FIG. 2F) is about 60 Å. In one embodiment, the capping layer 222 includes multiple interlayers. The first capping interlayer 222A is made of MgO or another iron-containing oxide formed directly on the magnetic memory layer 220 and has a thickness of about 2 Å to about 10 Å. On top of the first capping interlayer 222A, a second capping interlayer 222B of Ru, Ir, or a combination thereof is formed with a thickness of 1 Å to about 30 Å. In one embodiment, optionally, a third capping interlayer 222C is formed on the second capping interlayer 222B with a thickness of 1 Å to about 30 Å from Ta. Thus, some embodiments of capping layer 222 do not include third capping interlayer 222C. In one embodiment, optionally, second capping interlayer 222D is formed on third capping interlayer 222C and is formed from Ru, Ir, or a combination thereof to a thickness of up to 50 Å. In various embodiments, capping layer 222 includes only first capping interlayer 222A, or first capping interlayer 222A and second capping interlayer 222B, or first capping interlayer 222A, second capping interlayer 222B, and third capping interlayer 222C, i.e., first, second, and third capping layers 222A-222C. In some embodiments, a transition layer may be used between some or all of the first capping interlayer 222A, the second capping interlayer 222B, and the third capping interlayer 222C, or may be between the capping layer 222 and the magnetic memory layer 220, so that the performance of the MTJ stack is not adversely affected by the transition layer(s).

[0059]

[0066] The MTJ stacks described herein exhibit improved performance after processing at temperatures above 400°C, facilitated by the lattice match between the seed layer structure and the first pinning layer structure resulting from the use of a Cr seed layer or a Cr-containing seed layer in combination with a first pinning layer also containing Cr. The lattice match between the seed layer structure and the first pinning layer structure prevents the formation of roughness at the interface between the seed layer and the first pinning layer. Such roughness can result in a lack of planarity in one or more layers. Thus, the MTJ stack can maintain its structural integrity and desired magnetic and electrical properties. Furthermore, in the embodiments described herein, the combination of the first and second pinning layer compositions with the seed layer can enhance desired magnetic properties even after high-temperature processing.

[0060]

[0067] While the forgoing is directed to embodiments of the present disclosure, other and further embodiments of the present disclosure may be devised without departing from the basic scope thereof, the scope of which is defined by the following claims.

Claims

1. 1. A device comprising a magnetic tunnel junction stack, the magnetic tunnel junction stack comprising: a seed layer in contact with the buffer layer and comprising chromium (Cr); a first pinning layer in contact with the seed layer, the first pinning layer including a plurality of bilayers, each bilayer of the plurality of bilayers including a first intermediate layer formed from cobalt (Co) and a second intermediate layer formed from platinum (Pt), iridium (Ir), nickel (Ni), or palladium (Pd); a bonding layer in contact with the first pinning layer; and A device comprising a second pinning layer in contact with the bonding layer.

2. 2. The device of claim 1, wherein the first pinning layer and the second pinning layer each comprise 1 to 10 bilayers, the first pinning layer has a total thickness of 0.3 nm to 18 nm, and the second pinning layer has a total thickness of 0.3 nm to 18 nm.

3. 10. The device of claim 1 , wherein the first pinning layer further comprises a cobalt layer in contact with a first of the plurality of bilayers and in contact with the bonding layer, the cobalt layer having a thickness of 1 Å to 10 Å.

4. The device of claim 1 , wherein the first pinning layer has a thickness of 1 to 100 Å and the seed layer has a thickness of 1 to 100 Å.

5. The device of claim 1 , wherein the second pinning layer is formed as a single Co layer and has a thickness of 1 Å to 10 Å.

6. 2. The device of claim 1, wherein the second pinning layer is formed from a plurality of bilayers, each bilayer of the plurality of bilayers including a first intermediate layer formed from cobalt (Co) and a second intermediate layer formed from at least one of platinum (Pt), iridium (Ir), nickel (Ni), or palladium (Pd), and the second pinning layer has a thickness of 0.3 nm to 18 nm.

7. a structural blocking layer in contact with the second pinning layer; a magnetic reference layer in contact with the structure blocking layer; a tunnel barrier layer in contact with the magnetic reference layer; a magnetic memory layer in contact with the tunnel barrier layer; and The magnetic memory further includes a capping layer formed on the magnetic storage layer, the capping layer being formed from an oxide containing iron (Fe) and having a thickness of 2 Å to 10 Å. The device of claim 1 .

8. 1. A magnetic tunnel junction stack, comprising: a seed layer formed on the buffer layer and including chromium (Cr); a first pinning layer formed on the seed layer, the first pinning layer including a first plurality of bilayers, each bilayer of the first plurality of bilayers including a first intermediate layer formed from cobalt (Co) and a second intermediate layer formed from at least one of platinum (Pt), iridium (Ir), nickel (Ni), or palladium (Pd); a bonding layer formed on the first pinning layer; and a second pinning layer formed on the bonding layer, the second pinning layer comprising cobalt (Co).

9. 9. The stack of claim 8, wherein the first pinning layer further comprises a cobalt layer having a thickness of 1 Å to 10 Å formed on the first plurality of bilayers and in contact with the bonding layer, the first pinning layer having a thickness of 1 Å to 100 Å and the second pinning layer having a thickness of 1 Å to 100 Å.

10. a structural blocking layer on the second pinning layer, the structural blocking layer comprising at least one of tantalum (Ta), molybdenum (Mo), or tungsten (W) and having a thickness of 1 Å to 8 Å; a magnetic reference layer on the structure blocking layer; a tunnel barrier layer on the magnetic reference layer; and The stack of claim 8 further comprising a magnetic memory layer on the tunnel barrier layer.

11. The stack of claim 8 , wherein the seed layer has a thickness of 30 Å to 60 Å and comprises two or more layers.

12. 1. A magnetic tunnel junction stack, comprising: a seed layer formed on the buffer layer, the seed layer comprising chromium (Cr), the seed layer having a thickness of 1 Å to 100 Å; a first pinning layer formed on the seed layer and having a thickness of 1 Å to 100 Å, the first pinning layer including a first plurality of bilayers and a first cobalt overlayer formed on the first plurality of bilayers; a bonding layer formed between the first pinning layer and the first cobalt overlayer; a second pinning layer formed on the bonding layer and having a thickness of 1 Å to 100 Å, the second pinning layer comprising a second plurality of bilayers; a structural blocking layer formed on the second pinning layer, the structural blocking layer comprising at least one of tantalum (Ta), molybdenum (Mio), or tungsten (W), and having a thickness of 1 Å to 8 Å; a magnetic reference layer formed on the structure blocking layer; a tunnel barrier layer formed on the magnetic reference layer; and A stack including a magnetic memory layer formed on the tunnel barrier layer.

13. 13. The stack of claim 12, wherein each bilayer of the first plurality of bilayers includes a first intermediate layer formed from cobalt (Co) and a second intermediate layer formed from at least one of platinum (Pt), iridium (Ir), nickel (Ni), or palladium (Pd), and the number of bilayers in the first plurality of bilayers is between 2 and 10.

14. 13. The stack of claim 12, wherein the seed layer has a thickness of 30 Å to 60 Å and the first cobalt overlayer has a thickness of 1 Å to 10 Å.

15. 13. The stack of claim 12, wherein the second pinning layer includes a second cobalt overlayer formed on top of the second plurality of bilayers, the second cobalt overlayer in contact with the structural blocking layer.

Citation Information

Patent Citations

  • Magnetic tunnel junction element and forming method thereof

    JP2007288196A

  • Magnetic resistance element and electronic device

    JP2018032805A

  • Magnetic Random Access Memory with Multilayered Seed Structure

    US20170352701A1

  • Magnetoresistive effect element

    WO2016189772A1