Manufacturing method for element

By employing a separate electrode as a mask and using screen printing for connection electrodes, the method addresses short circuits and layer deterioration in solar cell manufacturing, ensuring efficient production of integrated structures.

JP2024150628AActive Publication Date: 2024-10-23ENECOAT TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024117038
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-12-12
Filing Date
2024-07-22
Publication Date
2024-10-23
Estimated Expiration
2040-08-07

AI Technical Summary

Technical Problem

Existing methods for manufacturing solar cells with integrated structures face issues such as short circuits and deterioration of the photoelectric conversion layer due to etching processes, particularly when using gases like carbon tetrafluoride or oxygen gas, which cause material wrapping under the mask and damage to the masked parts.

Method used

The method involves using a separate electrode as a mask during etching and forming connection electrodes through screen printing, avoiding direct contact with the layers to prevent short circuits and layer deterioration.

Benefits of technology

This approach enables the manufacturing of solar cells and modules with integrated structures without causing short circuits and while minimizing photoelectric conversion layer degradation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150628000001_ABST
    Figure 2024150628000001_ABST
Patent Text Reader

Abstract

To provide a solar cell element in which the deterioration of a photoelectric conversion layer is suppressed without causing short-circuit due to etching.SOLUTION: A solar cell element includes a substrate 3, a first electrode 5a and a second electrode 5b formed apart from each other on the substrate 3, a photoelectric conversion layer formed in a region including the first electrode 5a and the second electrode 5b and including an electron transport layer 7a and an electron transport layer 7b, a perovskite layer 9a and a perovskite layer 9b, and a hole transport layer 11a and a hole transport layer 11b, a first back electrode 13a and a second back electrode 13b formed at positions respectively corresponding to the first electrode 5a and the second electrode 5b on the photoelectric conversion layer, and a connection electrode 15 connecting the first back electrode 13a and a part of the second electrode 5b, this part of the second electrode 5b and a part of the substrate 3 being exposed in a region where the photoelectric conversion layer does not exist and the first back electrode 13 and the second back electrode 13b do not exist.SELECTED DRAWING: Figure 8
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing elements such as solar cells and organic electroluminescence (EL) devices. [Background technology]

[0002] JP 2018-163938 A describes a solar cell.

[0003] For example, in order to obtain a solar cell module with a high voltage, it is desirable to connect cells in series on the same substrate to form a solar cell module with an integrated structure. When separating the power generation layer to obtain a module with an integrated structure, it was assumed that etching would be performed using a mask to remove parts of the perovskite layer and hole transport layer. However, such etching would also remove the masked parts, causing a short circuit. In particular, when the power generation layer is separated by dry etching using plasma of carbon tetrafluoride gas or oxygen gas, there is a problem that the etching can get under the mask, causing damage to the masked portion. Furthermore, there was a problem of deterioration of the photoelectric conversion layer during the production of solar cells. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2018-163938 A Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the invention described in this specification is to provide a method for manufacturing an element without causing shorts due to etching.An object of the invention described in this specification is to provide a method for manufacturing an element while suppressing deterioration of the photoelectric conversion layer.

[0006] Another object of the invention described in this specification is to provide a method for manufacturing a solar cell module having an integrated structure. [Means for solving the problem]

[0007] One invention described in this specification is based on the discovery that by etching an element material having a power generation layer using a separated electrode (e.g., a back electrode) as a mask, and then forming a connecting electrode, an element can be manufactured without causing a short circuit even when etching is performed.

[0008] An invention described in this specification relates to a method for manufacturing an element. The method for manufacturing an element includes preparing an element material, and then manufacturing the element through a process including a back electrode forming process, an etching process, and a connection electrode forming process. Examples of the element include a solar cell and a solar cell module having an integrated structure.

[0009] The element material includes electrodes formed on a substrate, the electrodes including a first electrode and a second electrode spaced apart from each other, and a photoelectric conversion layer formed in a region including the first electrode and the second electrode.

[0010] This method is forming a first back electrode and a second back electrode on the photoelectric conversion layer at positions corresponding to the first electrode and the second electrode, respectively, the first back electrode and the second back electrode being not connected; performing etching using the first back surface electrode and the second back surface electrode as a mask; and a connection electrode forming step of forming a connection electrode for connecting the first back surface electrode and the second back surface electrode.

[0011] A preferred example of this method is a process in which the connection electrode formation process forms the connection electrodes by screen printing. An example of a connection electrode formation process is a process in which the connection electrodes are formed by screen printing. Normally, the back electrodes must be formed by deposition using a mask. However, by using screen printing, the electrodes can be easily formed without damaging each layer.

[0012] In a preferred embodiment of this method, the device material is forming a first electron transport layer and a second electron transport layer on the first electrode and the second electrode, respectively; forming a perovskite layer on the first electron transport layer and the second electron transport layer; forming a hole transport layer on the perovskite layer; It is manufactured by

[0013] A preferred example of this method is where the device material is: forming a first hole transport layer and a second hole transport layer on the first electrode and the second electrode, respectively; forming a perovskite layer on the first hole transport layer and the second hole transport layer; forming an electron transport layer on the perovskite layer; It is manufactured by Effect of the Invention

[0014] An invention described in this specification can provide a method for manufacturing an element without causing short circuits due to etching.An invention described in this specification can provide a method for manufacturing an element while suppressing deterioration of the photoelectric conversion layer.

[0015] An invention described in this specification can provide a method for manufacturing a solar cell module having an integrated structure. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a flow chart showing an example of a method for manufacturing an element. [Diagram 2] FIG. 2 is a conceptual diagram showing an example of the element material. [Diagram 3] FIG. 3 is a conceptual diagram showing an example of an electrode. [Figure 4] FIG. 4 is a conceptual diagram showing the device material in the process of being manufactured after the electron transport layer formation step. [Diagram 5] FIG. 5 is a conceptual diagram showing the device material after the hole transport layer formation step. [Figure 6] FIG. 6 is a conceptual diagram showing the element in the process of being manufactured after the back electrode formation process. [Figure 7] FIG. 7 is a conceptual diagram showing the device in the process of being manufactured after the etching process. [Figure 8] FIG. 8 is a conceptual diagram showing the element in the process of being manufactured after the connection electrode formation step. [Figure 9] FIG. 9 is a conceptual diagram for explaining the solar cell in the first embodiment. [Figure 10] FIG. 10 is a conceptual diagram for explaining the solar cell in Examples 2 and 3. In FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, the embodiments for carrying out the present invention will be described with reference to the drawings. The present invention is not limited to the embodiments described below, and includes appropriate modifications of the embodiments described below within the scope obvious to those skilled in the art.

[0018] Examples of the element 1 are a solar cell and an organic EL element. An example of a solar cell is a perovskite solar cell. A perovskite solar cell includes, for example, an electrode, an electron transport layer, a perovskite layer (light absorbing layer), a hole transport layer, and a back electrode in this order. The perovskite solar cell may be of a normal type in which an n-type semiconductor layer is provided on an electrode, or of an inverted type in which a p-type semiconductor layer is provided on an electrode (a substrate, an electrode, a hole transport layer, a perovskite layer, an electron transport layer, an electrode, and a connection electrode are formed in this order). Below, a perovskite solar cell is described using as an example a perovskite solar cell including an electrode, an electron transport layer, a perovskite layer (light absorbing layer), a hole transport layer, and a back electrode in this order.

[0019] Fig. 1 is a flow chart showing an example of a method for manufacturing an element. As shown in Fig. 1, the method for manufacturing an element includes preparing an element material, followed by a back electrode forming process (S21), an etching process (S22), and a connection electrode forming process (S23).

[0020] Examples of the element are a solar cell, a solar cell module having an integrated structure, and an organic EL element. In addition to the respective configurations described below, these may appropriately adopt known elements that solar cells and organic EL elements have.

[0021] Fig. 2 is a conceptual diagram showing an example of an element material. As shown in Fig. 2, the element material has a substrate 3, an electrode 5 including a first electrode 5a and a second electrode 5b, a first electron transport layer 7a and a second electron transport layer 7b, a perovskite layer 9, and a hole transport layer 11. In this example, the first electron transport layer 7a, the second electron transport layer 7b, the perovskite layer 9, and the hole transport layer 11 function as a photoelectric conversion layer. The element material may have a photoelectric conversion layer including a first hole transport layer, a second hole transport layer, a perovskite layer, and an electron transport layer in this order.

[0022] Board 3 A known substrate for a perovskite solar cell or an organic EL element can be appropriately used as the substrate 3. Examples of the substrate are a glass substrate, an insulating substrate, a semiconductor substrate, a metal substrate, and a conductive substrate (including a conductive film). In addition, a substrate having at least one film selected from a metal film, a semiconductor film, a conductive film, and an insulating film formed on a part or all of the surface of the substrate can also be preferably used.

[0023] Examples of the constituent metals of the metal film include one or more metals selected from gallium, iron, indium, aluminum, vanadium, titanium, chromium, rhodium, nickel, cobalt, zinc, magnesium, calcium, silicon, yttrium, strontium, and barium. Examples of the constituent material of the semiconductor film include simple elements such as silicon and germanium, compounds containing elements of groups 3 to 5 and groups 13 to 15 of the periodic table, metal oxides, metal sulfides, metal selenides, metal nitrides, and the like. Examples of the constituent material of the conductive film include tin-doped indium oxide (ITO), fluorine-doped indium oxide (FTO), zinc oxide (ZnO), aluminum-doped zinc oxide (AZO), gallium-doped zinc oxide (GZO), tin oxide (SnO 2 ), indium oxide (In 2 O 3 ), tungsten oxide (WO 3 ) An example of the material constituting the insulating film is aluminum oxide (Al 2 O 3 ), titanium dioxide (TiO 2 ), silicon oxide (SiO 2 ), silicon nitride (Si 3 N 4 ), silicon oxynitride (Si 4 O 5 N 3 ).

[0024] Examples of the shape of the substrate include a plate-like shape such as a flat plate or a disk, a fiber-like shape, a rod-like shape, a cylindrical shape, a prismatic shape, a cylindrical shape, a spiral shape, a spherical shape, a ring shape, and a porous structure. Of these, a plate-like substrate is preferred. Examples of the thickness of the substrate are preferably 0.1 μm to 100 mm, and more preferably 1 μm to 10 mm.

[0025] electrode 5 The electrode is a layer that supports the electron transport layer and has the function of extracting electrons from the perovskite layer (light absorbing layer). The electrode is formed on the substrate 3 and includes a first electrode 5a and a second electrode 5b that are spaced apart. Spaced apart means that they are not in physical contact and that the first electrode 5a and the second electrode 5b are not short-circuited. The electrode is preferably a transparent electrode or a metal electrode.

[0026] Examples of transparent electrodes include tin-doped indium oxide (ITO) films and impurity-doped indium oxide (In 2 O 3 A metal electrode is a laminated film formed by laminating a tin-doped indium oxide (ITO) film, an impurity-doped zinc oxide (ZnO) film, and a fluorine-doped tin dioxide (FTO) film. A metal electrode means an electrode that contains a metal. Examples of metal electrodes are gold, silver, and copper. Metal electrodes are not limited to metals, but also include tin-doped indium oxide (ITO) films, impurity-doped indium oxide (In 2 O 3 ) film, an impurity-doped zinc oxide (ZnO) film, a fluorine-doped tin dioxide (FTO) film, or a laminated film formed by laminating these. These films may function as, for example, a diffusion prevention layer. The thickness of these electrodes is not particularly limited, and it is usually preferable to adjust the sheet resistance to 5 to 15 Ω / □ (per unit area). The electrodes can be obtained by a known film formation method depending on the material to be formed.

[0027] Fig. 3 is a conceptual diagram showing an example of electrodes. As shown in Fig. 3, the electrodes 5 include a first electrode 5a and a second electrode 5b, which may be separated so as not to be connected. In the example of Fig. 3, two electrodes are drawn, but the number of electrodes may be three or more.

[0028] Electron transport layer 7 The device material includes an electron transport layer. The electron transport layer 7 is formed to increase the active surface area of ​​the perovskite layer (light absorption layer), improve the photoelectric conversion efficiency, and facilitate electron collection. The electron transport layer may be a flat layer using an organic semiconductor material such as a fullerene derivative. The electron transport layer may also be a flat layer using an organic semiconductor material such as titanium oxide (TiO 2 ) (mesoporous TiO 2 (including tin oxide (SnO 2 The electron transport layer may be a layer containing a metal oxide such as zinc oxide (ZnO). The thickness of the electron transport layer is not particularly limited, and is preferably about 10 to 300 nm, and more preferably about 10 to 250 nm, from the viewpoint of being able to collect more electrons from the perovskite layer (light absorbing layer).

[0029] The electron transport layer has a first electron transport layer 7a and a second electron transport layer 7b formed on the first electrode 5a and the second electrode 5b, respectively. Usually, the electron transport layer is patterned to have the same shape as the electrode underneath. The first electron transport layer 7a and the second electron transport layer 7b have, for example, the same shapes as the first electrode 5a and the second electrode 5b, respectively. However, the same shape does not mean identical in the strict sense, and the same shape may be designed to be approximately the same shape.

[0030] Perovskite layer 9 The perovskite layer (light absorbing layer: photoactive layer) 9 in the perovskite solar cell is a layer that absorbs light and transfers excited electrons and holes to perform photoelectric conversion. The perovskite layer (light absorbing layer) contains a perovskite material or a perovskite complex. From the viewpoint of the balance between the light absorption efficiency and the electron and hole diffusion length and the absorption efficiency of light reflected by the electrode, the thickness of the perovskite layer (light absorbing layer) is preferably, for example, 50 to 1000 nm, and more preferably 200 to 800 nm. The thickness of the perovskite layer (light absorbing layer) of the present invention may be measured by a cross-sectional scanning electron microscope (cross-sectional SEM). Furthermore, the flatness of the perovskite layer (light absorbing layer) of the present invention is preferably such that the height difference is 50 nm or less (-25 nm to +25 nm) in a horizontal area of ​​500 nm x 500 nm on the surface as measured by a scanning electron microscope, and more preferably the height difference is 40 nm or less (-20 nm to +20 nm). This makes it easier to balance the light absorption efficiency and the exciton diffusion length, and further improves the absorption efficiency of light reflected by the electrode.

[0031] In the element material, the perovskite layer 9 is formed on the first electron transport layer 7a and the second electron transport layer 7b. In the example of Fig. 2, the perovskite layer is also formed in the portion (gap portion) on the substrate 3 where the first electrode 5a and the second electrode 5b are not present.

[0032] Hole transport layer 11 The hole transport layer 11 is a layer having the function of transporting charges. The hole transport layer 11 is a layer formed on the perovskite layer 9. For example, a conductor, a semiconductor, an organic hole transport material, etc. can be used for the hole transport layer. The material can function as a hole transport material that receives holes from the perovskite layer (light absorption layer) and transports the holes. The hole transport layer is formed on the perovskite layer (light absorption layer). Examples of the conductor and semiconductor include CuI and CuInSe 2 Compound semiconductors containing monovalent copper such as CuS; GaP, NiO, CoO, FeO, Bi 2 O 3 ,MoO 2 ,Cr 2 O 3Examples of the organic hole transport material include compounds containing metals other than copper, such as CuI, etc. Among them, from the viewpoint of more efficiently receiving only holes and obtaining higher hole mobility, semiconductors containing monovalent copper are preferred, and CuI is more preferred. Examples of the organic hole transport material include polythiophene derivatives such as poly-3-hexylthiophene (P3HT) and polyethylenedioxythiophene (PEDOT); fluorene derivatives such as 2,2',7,7'-tetrakis-(N,N-di-p-methoxyphenylamine)-9,9'-spirobifluorene (Spiro-OMeTAD); carbazole derivatives such as polyvinylcarbazole; triphenylamine derivatives such as poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA); diphenylamine derivatives; polysilane derivatives; polyaniline derivatives, etc. Among them, from the viewpoint of more efficiently receiving only holes and obtaining higher hole mobility, triphenylamine derivatives, fluorene derivatives, etc. are preferred, and PTAA, Spiro-OMeTAD, etc. are more preferred.

[0033] In order to further improve the hole transport properties, lithium bis(trifluoromethylsulfonyl)imide (LiTFSI), silver bis(trifluoromethylsulfonyl)imide, trifluoromethylsulfonyloxysilver, and NOSbF are added to the hole transport layer. 6 ,SbCl 5 ,SbF 5 The hole transport layer may contain an oxidizing agent such as tris(2-(1H-pyrazol-1-yl)-4-tert-butylpyridine)cobalt(III)tri[bis(trifluoromethane)sulfonimide]. The hole transport layer may also contain a basic compound such as t-butylpyridine (TBP), 2-picoline, or 2,6-lutidine. The content of the oxidizing agent and basic compound may be the amount that has been conventionally used. The thickness of the hole transport layer is preferably, for example, 50 to 500 nm, and more preferably 100 to 300 nm, from the viewpoint of more efficiently receiving only holes and obtaining higher hole mobility.

[0034] 1, the element material may be manufactured by a method including an electrode forming step (S11), an electron transport layer forming step (S12), a perovskite layer forming step (S13), and a hole transport layer forming step (S14).The element material may also be manufactured by a process including a step of forming a first hole transport layer and a second hole transport layer on a first electrode and a second electrode, respectively, a step of forming a perovskite layer on the first hole transport layer and the second hole transport layer, and a step of forming an electron transport layer on the perovskite layer.

[0035] Electrode formation process (S11) The electrode formation step (S11) is a step of forming electrodes on a substrate. The electrodes include a first electrode and a second electrode that are spaced apart. Methods for forming electrodes on a substrate are well known. Examples of well-known methods include etching using a resist pattern and patterning using a laser.

[0036] Electron transport layer formation step (S12) The electron transport layer forming step is a step of forming an electron transport layer (first electron transport layer 7a and second electron transport layer 7b) on the electrode 3 (first electrode 5a and second electrode 5b). The electron transport layer can be obtained by using a known film forming method according to the material to be formed. For example, it can be prepared by applying an aqueous dispersion of tin oxide fine particles at 3 to 15 mass % (particularly 5 to 10 mass %) on the electrode. The aqueous dispersion of tin oxide fine particles can be a known or commercially available product. The method of application is preferably spin coating. The application can be performed at, for example, about 15 to 30°C. After the electrode and the electron transport layer are formed on the substrate, etching with a resist pattern or patterning using a laser may be performed.

[0037] Fig. 4 is a conceptual diagram showing the device material in the process of being manufactured at a stage after the electron transport layer formation process. As shown in Fig. 4, an electron transport layer (first and second electron transport layers 7a, 7b) is formed on an electrode divided into multiple parts. In this example, an electrode divided into two parts is described. However, the electrode may be divided into three or more parts.

[0038] Perovskite layer formation process (S13) The perovskite layer forming step is a step of forming a perovskite layer 9 on the electron transport layer (the first electron transport layer 7a and the second electron transport layer 7b). The perovskite layer may be manufactured based on a known method.

[0039] An example of the perovskite layer forming process includes a process of applying a solution containing a perovskite compound to a substrate, a process of applying a poor solvent to the substrate, and a process of annealing the substrate, in this order. In order to apply the solution containing a perovskite compound to the substrate, spin coating, dip coating, screen printing, roll coating, die coating, transfer printing, spraying, or slit coating may be used. Among these, it is preferable to apply the solution to the substrate by spin coating. Spin coating is a method in which the substrate is rotated while dropping the solution, and the solution is applied to the substrate. The substrate carrying the solution may be rotated, and the solution may be further applied to the substrate. The rotation speed may be a maximum speed of 1,000 to 10,000 rpm for 30 seconds to 5 minutes, 2 to 15 seconds to reach the maximum speed, and 2 to 15 seconds to stop from the maximum speed.

[0040] Next, the step of applying a poor solvent to the substrate will be described. A poor solvent means a solvent that has the ability to dissolve a solute but does not have a high solubility for the solute. Examples of poor solvents include substituted aliphatic hydrocarbons such as dichloromethane and chloroform; aromatic hydrocarbons such as toluene and benzene; substituted aromatic hydrocarbons such as chlorobenzene, orthodichlorobenzene, and nitrobenzene; ethers such as acetic acid, diethyl ether, and tetrahydrofuran (THF); alcohols such as methanol, ethanol, isopropanol, butanol, and octanol; long-chain hydrocarbons such as hexane (especially C4-10 hydrocarbons); and acetonitrile. These poor solvents can be used alone or in combination of two or more. Among these, chlorobenzene or toluene is preferred.

[0041] Next, the process of annealing the substrate will be described. Annealing refers to a process of heating the substrate. The annealing process is preferably carried out promptly after the poor solvent is dropped or after the substrate stops moving after spin coating is completed. As shown in the examples described below, the annealing process preferably includes a process of gradually heating the substrate in a closed system containing solvent vapor. In the closed system, it is preferable that the vapor of the solvent contained in the solution containing the Sn-based perovskite compound is present, and it is preferable that the solvent is at saturated vapor pressure or a partial pressure of 90% or more of the saturated vapor pressure in the closed system.

[0042] Hole transport layer formation step (S14) The hole transport layer forming step is a step of forming a hole transport layer 11 on the perovskite layer 9. A known method may be appropriately adopted as a method for forming the hole transport layer. For example, it is preferable to form the hole transport layer 11 by applying (by spin coating, inkjet, die coater, etc.) a solution containing an organic hole transport material onto the perovskite layer (light absorbing layer) in a dry atmosphere and heating at 30 to 150°C (particularly 50 to 100°C). By forming the hole transport layer, the element material 21 can be obtained.

[0043] 5 is a conceptual diagram showing the element material after the hole transport layer forming step. As shown in FIG 5, a hole transport layer 11 is formed so as to cover the entire perovskite layer 9.

[0044] Back electrode formation process (S21) The back surface electrode formation step is a step of forming a first back surface electrode 13a and a second back surface electrode 13b on the element material 21 at positions on the hole transport layer 11 corresponding to the first electrode 5a and the second electrode 5b, respectively.

[0045] When the back electrodes 13a-13b are made of metal, they are also called metal electrodes. The back electrodes are arranged opposite the electrodes and formed on the hole transport layer, allowing charge to be exchanged with the hole transport layer. The back electrodes may be made of known materials used in the industry, such as platinum, titanium, stainless steel, aluminum, gold, silver, nickel, and other metals or alloys thereof. Of these, the metal electrodes are preferably made of materials that can be formed by a method such as vapor deposition, since the electrodes can be formed in a dry atmosphere.

[0046] By appropriately combining the above method with a known method, perovskite solar cells having layer structures other than those described above can also be manufactured.

[0047] FIG. 6 is a conceptual diagram showing an element in the middle of manufacture after the back electrode formation process. As shown in FIG. 6, the back electrode does not have to have the same shape as the electrode or the electron transport layer. In the example of FIG. 6, first and second back electrodes 13a and 13b are formed. A part of the back electrode does not have to cover the electrode or the electron transport layer so that a conductive connection can be made by the connection electrode. Also, a part of the back electrode may be present in a part where no electrode or electron transport layer is provided. For example, the first back electrode 13a has a main body part and a protruding part protruding from the main body part. And, no electrode or electron transport layer is provided below the protruding part (toward the substrate). On the other hand, the protruding part near the center of the first electrode 5a or the first electron transport layer 7a is not covered by the first back electrode 13a.

[0048] Etching process (S22) The etching process is a process of performing etching using the first back electrode 13a and the second back electrode 13b as a mask. Since the etching process is publicly known, a publicly known etching method can be appropriately adopted. An example of the etching is dry etching.

[0049] FIG. 7 is a conceptual diagram showing the element in the middle of manufacture after the etching process. As shown in FIG. 7, the etching removes the perovskite layer 9 and the hole transport layer 11 in the portion where the back electrode is not formed. Then, a part of the electron transport layer 7a-7b and a part of the electrodes 5a-5b in the portion where the back electrode is not present are exposed. The photoelectric conversion layers on the first electrode 5a and the second electrode 5b are also called the first photoelectric conversion layer 6a and the second photoelectric conversion layer 6b. The first photoelectric conversion layer 6a includes the first electron transport layer 7a, the first perovskite layer 9a, and the first hole transport layer 11a, and the second photoelectric conversion layer 6b includes the second electron transport layer 7b, the second perovskite layer 9b, and the second hole transport layer 11b.

[0050] Connection electrode formation process (S23) The connection electrode formation process is a process for forming the connection electrodes 15 for connecting the first back surface electrode 13a and the second back surface electrode 13b. An example of the connection electrode formation process is a process for forming the connection electrodes by screen printing. Normally, the back surface electrodes must be formed by deposition using a mask. However, by using screen printing, the electrodes can be easily formed without damaging each layer.

[0051] 8 is a conceptual diagram showing the element in the middle of manufacture after the connection electrode forming process. In this example, for example, the first back electrode 13a and the second electrode 5b are connected by the first connection electrode 15a. The second connection electrode 15b is provided on the second back electrode 13b.

[0052] After the connection electrode forming step, for example, a laser may be used to remove excess portions. Also, a sealing material layer (protective film) may be formed.

[0053] Encapsulant layer The sealing material layer 23 is provided to protect the photoelectric conversion unit. Examples of materials constituting the sealing material layer include thermoplastic resins such as ethylene-vinyl acetate copolymer (EVA), polyvinyl butyral (PVB), polyethylene terephthalate (PET), polyolefin (PO), and polyimide (PI), thermosetting resins such as epoxy, urethane, and polyimide, and inorganic materials such as glass, with EVA, PO, and glass being preferred.

[0054] The sealing material layer preferably has a thickness of, for example, 0.1 to 10 mm and a tensile modulus of elasticity of 0.005 to 0.05 GPa. These parameters are explained below.

[0055] The thickness of the encapsulant layer is, for example, preferably 0.1 to 10 mm, and more preferably 0.2 to 1.0 mm. When the encapsulant layer has such a thickness, the photoelectric conversion section can be sufficiently encapsulated and protected.

[0056] The tensile modulus of the sealing material layer is, for example, preferably 0.005 to 0.05 GPa, and more preferably 0.01 to 0.05 GPa. When the tensile modulus of the sealing material layer is in such a range, the stress due to the expansion and contraction of the surface protection substrate can be sufficiently alleviated.

[0057] Organic EL elements are publicly known elements, as described in, for example, JP 2017-123352 A and JP 2015-071619 A, and their manufacturing methods are also publicly known. An example of an organic EL element has a substrate, an anode, a cathode, and an organic layer disposed between the anode and the cathode. The organic layer is configured by stacking, in this order from the anode side, a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer, and an electron injection layer. EXAMPLES

[0058] The following describes in detail the invention described in this specification using examples. The invention described in this specification is not limited to the following examples, and includes those to which publicly known elements are appropriately added.

[0059] FIG. 9 is a conceptual diagram for explaining the solar cell in the first embodiment. A glass substrate 3 has an electrode 5 made of ITO (indium tin oxide) patterned in a predetermined shape, and an electron transport layer 7, a perovskite layer 9, and a hole transport layer 11 are applied in sequence. The electron transport layer 7 is made of colloidal SnO 2 It can be formed by spin-coating an aqueous solution and drying it. The perovskite layer 9 can be obtained with high quality by applying a specific material by the above-mentioned spin-coating and then further coating with a poor solvent. The hole transport layer 11 can be obtained by spin-coating a solution containing Spiro-MeOTAD and drying it. The above layers are formed by spin coating and are therefore laminated over the entire surface of the substrate.

[0060] In conventional technology, a process of patterning the laminated layers is often carried out before the formation of the back electrode, but this is not carried out in this embodiment. This is because a high-precision pattern is not suitable because it requires positional precision for the next back electrode as well.

[0061] First, the back electrode 13 is formed. As a method for forming the back electrode, a metal mask is used to create a pattern in advance, and the electrode is formed by a sputtering device using a desired material as a target. The metal mask is formed by adhering it to the laminated substrate 3. The target material is molybdenum oxide (MoO 3 ), copper (Cu), and indium tin oxide (ITO) were used.

[0062] Next, in order to remove the laminated film in the area where the back electrode 13 is not present, 4 and O 2 Dry etching is performed using a laser. At this time, the rear electrode serves as a mask and parts of the hole transport layer 11 and the perovskite layer 9 are removed. This makes it possible to expose parts of the electrode 5 in the area where there is no rear electrode 13. A pulse laser may also be used to remove the laminated film. Next, the connection electrode 15 is formed. It is formed by a sputtering device using a metal mask in the same manner as the back electrode. Alternatively, a conductive paste can be formed by screen printing. Through the above steps, a solar cell module with an integrated structure can be obtained.

[0063] In the example of Fig. 9, a photoelectric conversion layer (6a, 6b) including a photoactive layer is formed on three surface electrodes, and a back electrode is formed on the photoactive layer. The back electrodes are connected to each other in the upper region of Fig. 9, and the leftmost electrode is connected to a positive electrode and the rightmost electrode is connected to a negative electrode.

[0064] FIG. 10 is a conceptual diagram for explaining the solar cell in Examples 2 and 3. In FIG. In the second embodiment shown in Fig. 10(a), a connection region of the back electrode is provided in the adjacent central region of each front electrode, and the electrodes are connected to each other. In the third embodiment shown in Fig. 10(b), a connection region of the back electrode is provided in the adjacent region of each front electrode, and the electrodes are connected to each other. [Industrial Applicability]

[0065] The present invention can be used in technical fields related to solar cells and organic EL elements. [Explanation of symbols]

[0066] 1 element 3. Substrate 5 electrodes 6a First photoelectric conversion layer 6b Second photoelectric conversion layer 7a First electron transport layer 7b Second electron transport layer 9 Perovskite Layer 11 Hole transport layer 13a 1st back electrode 13b 2nd back electrode 15 Connection electrode 21 Device materials 23 Encapsulant layer

Claims

[Claim 1] A substrate; a first electrode and a second electrode formed on the substrate and spaced apart from each other; a photoelectric conversion layer formed in a region including the first electrode and the second electrode, the photoelectric conversion layer including an electron transport layer, a perovskite layer, and a hole transport layer; a first back surface electrode and a second back surface electrode formed on the photoelectric conversion layer at positions corresponding to the first electrode and the second electrode, respectively; the photoelectric conversion layer is not present in an area where the first back surface electrode and the second back surface electrode are not present, and a part of the substrate and a part of the second electrode are exposed in this area, and a connection electrode that connects the exposed part of the second electrode and the first back surface electrode; A solar cell element comprising:

Citation Information

Patent Citations

  • Perovskite solar module who once cuts

    CN208433423U

  • Method of manufacturing solar cell module, and solar cell module

    JP2017152510A

  • Perovskite photovoltaic cell module

    KR101666748B1

  • Perovskite solar cell module and fabrication method thereof

    US20190115487A1

  • Solar cell

    JP2018163938A