Method for selecting and manufacturing nickel-cobalt-manganese active material for positive electrode

By employing thermal mass spectrometry to select and manufacture nickel-cobalt-manganese-based active materials with controlled mass loss and nickel content, the storage characteristics of non-aqueous electrolyte secondary batteries are improved, addressing the deterioration issue in high nickel ratio materials.

JP2024151002AActive Publication Date: 2024-10-24PRIME PLANET ENERGY & SOLUTIONS INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023064101
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-11
Publication Date
2024-10-24
Estimated Expiration
2043-04-11

AI Technical Summary

Technical Problem

The use of nickel-cobalt-manganese active materials with high nickel ratios in non-aqueous electrolyte secondary batteries leads to deteriorated storage characteristics.

Method used

A method involving thermal mass spectrometry to select and manufacture nickel-cobalt-manganese-based active materials by controlling the mass loss rate and ensuring a nickel content ratio of 70 mol% or more, using single crystal particles, and forming a positive electrode plate with a specific mass reduction rate to reduce stored gas and improve storage characteristics.

Benefits of technology

The method enhances the storage characteristics of non-aqueous electrolyte secondary batteries by reducing the amount of stored gas, thereby improving battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024151002000001_ABST
    Figure 2024151002000001_ABST
Patent Text Reader

Abstract

To provide a method for selecting and manufacturing a nickel-cobalt-manganese-based active material for a positive electrode, which can improve the storage characteristics of a non-aqueous electrolyte secondary battery, a nickel-cobalt-manganese-based active material for a positive electrode, a mixture containing the same, a positive electrode plate, and a non-aqueous electrolyte secondary battery.SOLUTION: A method for selecting a nickel-cobalt-manganese-based active material for a positive electrode includes a thermogravimetric analysis step of determining a mass reduction rate (mass% / min) of a nickel-cobalt-manganese-based active material at a temperature of 100 to 600°C and at a heating rate of 5°C / min by thermogravimetric analysis, and a determination step of determining whether the nickel-cobalt-manganese-based active material satisfies the formula (1), when Wd is the mass reduction rate (mass% / min).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for selecting and producing a nickel-cobalt-manganese-based active material for a positive electrode, and further to a nickel-cobalt-manganese-based active material for a positive electrode, a mixture containing the same, a positive electrode plate, and a nonaqueous electrolyte secondary battery. [Background technology]

[0002] International Publication No. 2020 / 174794 (Patent Document 1) proposes a nonaqueous electrolyte secondary battery that has a high capacity and suppresses resistance increases and the occurrence of internal short circuits by increasing the nickel ratio in a nickel-containing lithium composite oxide. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2020 / 174794 Summary of the Invention [Problem to be solved by the invention]

[0004] In a non-aqueous electrolyte secondary battery, when a nickel-cobalt-manganese based active material having a high nickel ratio (for example, 70 mol % or more) is used, the storage characteristics of the non-aqueous electrolyte secondary battery may deteriorate.

[0005] An object of the present disclosure is to provide a method for selecting and producing a nickel-cobalt-manganese-based active material for a positive electrode, which can improve the storage characteristics of a non-aqueous electrolyte secondary battery, a nickel-cobalt-manganese-based active material for a positive electrode, a mixture containing the same, a positive electrode plate, and a non-aqueous electrolyte secondary battery. [Means for solving the problem]

[0006] The present disclosure provides the following methods for selecting and producing a nickel-cobalt-manganese-based active material for a positive electrode, a nickel-cobalt-manganese-based active material for a positive electrode, a mixture containing the same, a positive electrode plate, and a nonaqueous electrolyte secondary battery. [1] A method for selecting a nickel-cobalt-manganese-based active material for a positive electrode, comprising: A thermogravimetric analysis step of determining the mass loss rate (mass% / min) of the nickel-cobalt-manganese active material at a temperature of 100 to 600 ° C. and a heating rate of 5 ° C. / min by thermogravimetric analysis; and When the mass reduction rate (mass % / min) is Wd, the nickel-cobalt-manganese-based active material has a mass reduction rate satisfying the following formula: (1) Wd≦1.10 A determination step for determining whether the above condition is satisfied. The method for selecting a nickel-cobalt-manganese-based active material for a positive electrode includes the steps of: [2] The method for selecting a nickel-cobalt-manganese-based active material for a positive electrode according to [1], wherein the thermogravimetric analysis step includes a sampling step of collecting a nickel-cobalt-manganese-based active material for thermogravimetric analysis from a battery in a charged state. [3] The method for selecting a nickel-cobalt-manganese-based active material for a positive electrode according to [1] or [2], wherein the nickel-cobalt-manganese-based active material has a nickel content of 70 mol % or more. [4] The method for selecting a nickel-cobalt-manganese-based active material for a positive electrode according to any one of [1] to [3], wherein the nickel-cobalt-manganese-based active material contains single crystal particles. [5] A method for producing a nickel-cobalt-manganese-based active material for a positive electrode, comprising a selection step of carrying out the method for selecting a nickel-cobalt-manganese-based active material for a positive electrode according to any one of [1] to [4]. [6] A nickel-cobalt-manganese-based active material for positive electrodes, which has a mass loss rate per minute of 1.10 mass% / min or less in thermogravimetric analysis at 100 to 600°C at a heating rate of 5°C / min. [7] The nickel-cobalt-manganese-based active material for a positive electrode according to [6], having a nickel content of 70% or more. [8] The nickel-cobalt-manganese-based active material for a positive electrode according to [6] or [7], which contains single crystal particles. [9] A nickel-cobalt manganese-based active material mixture for a positive electrode, comprising the nickel-cobalt manganese-based active material for a positive electrode according to any one of [6] to [8] and a nickel-cobalt manganese-based active material different from the nickel-cobalt manganese-based active material for a positive electrode.

[10] The nickel-cobalt manganese-based active material mixture for a positive electrode according to [9], wherein the nickel-cobalt manganese-based active material for a positive electrode contains single crystal particles, and a nickel-cobalt manganese-based active material different from the nickel-cobalt manganese-based active material for a positive electrode contains polycrystalline particles.

[11] A positive electrode plate having a positive electrode active material layer containing the nickel-cobalt-manganese-based positive electrode active material according to any one of [6] to [8].

[12] A non-aqueous electrolyte secondary battery comprising the positive electrode plate according to

[11] . Effect of the Invention

[0007] According to the present disclosure, it is possible to provide a method for selecting and producing a nickel-cobalt-manganese-based active material for a positive electrode, which can improve the storage characteristics of a non-aqueous electrolyte secondary battery, a nickel-cobalt-manganese-based active material for a positive electrode, a mixture containing the same, a positive electrode plate, and a non-aqueous electrolyte secondary battery. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a schematic flow chart of a method for selecting a nickel-cobalt-manganese based active material for a positive electrode in this embodiment. [Diagram 2] FIG. 2 is a schematic flow chart of a method for producing a nickel-cobalt-manganese based active material for a positive electrode in this embodiment. [Diagram 3] FIG. 3 is a schematic diagram showing an example of the configuration of the positive electrode plate in this embodiment. [Figure 4] FIG. 4 is a schematic flow chart showing a method for manufacturing a positive electrode plate in this embodiment. [Diagram 5] FIG. 5 is a schematic diagram showing an example of the configuration of a battery in this embodiment. [Figure 6]FIG. 6 is a schematic diagram showing an example of the configuration of the electrode body in this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings, but the present disclosure is not limited to the following embodiments. In all of the drawings, the scale of each component is appropriately adjusted to make it easier to understand, and the scale of each component shown in the drawings does not necessarily match the scale of the actual component.

[0010] In this specification, elements expressed in the singular form include the plural form unless otherwise specified. For example, a "particle" can mean not only "one particle" but also "an aggregate of particles (powder, powder, particle group)."

[0011] <Selection method for nickel-cobalt-manganese active materials for positive electrodes> The method for selecting a nickel-cobalt-manganese-based active material for a positive electrode (hereinafter also referred to as a NCM active material for a positive electrode) in this embodiment (hereinafter also referred to as a selection method) includes a thermogravimetric analysis step A for determining the mass reduction rate (mass % / min) (hereinafter also referred to as mass reduction rate) of the nickel-cobalt-manganese-based active material (hereinafter also referred to as an NCM active material) at a temperature of 100 to 600°C and a heating rate of 5°C / min by thermogravimetric analysis, and a determination step B for determining whether the NCM active material satisfies formula (1). The NCM active material for a positive electrode can be used for the positive electrode of a non-aqueous electrolyte secondary battery (hereinafter also referred to as a battery). The battery will be described in detail later.

[0012] In the thermogravimetric analysis step A, the mass loss rate can be determined by thermogravimetric analysis. Thermogravimetric analysis can be performed by the following procedure. 20 mg of NCM active material for thermogravimetric analysis is weighed out on a pan for a thermogravimetric analyzer, set in a thermogravimetric analyzer, and then heated in an Ar atmosphere at a heating rate of 5°C / min and an upper limit temperature of 600°C to measure the mass loss from 100°C to 600°C, and calculate the mass loss rate per minute. Thermogravimetric analysis can be performed according to the method described in the Examples section below.

[0013] In the determination step B, a determination is made by thermogravimetric analysis as to whether or not the NCM active material satisfies formula (1). By using the NCM active material determined to satisfy formula (1) in the determination step B as the NCM active material for the positive electrode in the positive electrode active material layer, it is possible to reduce the amount of gas generated when the battery is stored at high temperature in a charged state (hereinafter also referred to as the amount of stored gas), and improve storage characteristics. Considering that the stored gas is usually generated by a side reaction between the electrolyte and the NCM active material contained in the positive electrode, it was surprising that a relationship was found between the mass reduction rate and the NCM active material, rather than between the composition, average particle size, and specific surface area of ​​the NCM active material.

[0014] From the viewpoint of storage properties, the right side of formula (1) is preferably 1.00 or less, more preferably 0.45 or less, and even more preferably 0.40 or less. The left side of formula (1) is usually 0 or more, and may be, for example, 0.0001 or more, or 0.001 or more, or 0.01 or more, or 0.1 or more.

[0015] The thermogravimetric analysis step A may include a sampling step of collecting the NCM active material for thermogravimetric analysis from a battery in a charged state. The battery has a positive electrode plate with a positive electrode active material layer containing the NCM active material. The battery is charged at a temperature of 25° C. and has a current of 0.2 mA / cm. 2 The battery was charged at a constant current density of 0.04 mA / cm until the voltage reached 4.35 V. 2 The battery can be charged by constant voltage charging until the positive electrode plate reaches a positive electrode active material layer. The positive electrode plate can be removed from the charged battery, and the NCM active material for thermogravimetric analysis can be extracted from the positive electrode active material layer of the positive electrode plate. The test cell may be, for example, a stacked type or a wound type. More specific methods for producing the test cell, charging the test cell, and extracting the NCM active material for thermogravimetric analysis from the charged test cell will be described in the Examples section below.

[0016] The NCM active material contains one or more nickel, cobalt and manganese-containing compounds. The nickel, cobalt and manganese-containing compounds can be single crystal particles or polycrystalline particles as described below. The nickel content ratio of the metal elements other than lithium in the NCM active material may be, for example, 70 mol% or more, preferably 75 mol% or more, more preferably 80 mol% or more, even more preferably 85 mol% or more, and particularly preferably 90 mol% or more. The nickel, cobalt and manganese-containing compound preferably contains nickel-cobalt-manganese composite hydroxide, more preferably lithium-nickel-cobalt-manganese composite oxide. The nickel-cobalt-manganese composite hydroxide may be obtained by, for example, a coprecipitation method. The nickel-cobalt-manganese composite hydroxide is, for example, a compound represented by the general formula: Ni x Co y Mn z It may be a compound represented by (OH)2 (wherein x+y+z=1). The lithium nickel cobalt manganese composite oxide may have a molar ratio of lithium to nickel, cobalt and manganese, Li:(Ni+Co+Mn), of, for example, 1.0 to 1.2:1.0.

[0017] The NCM active material can include, for example, a first layered metal oxide having the formula (i): Li 1-a1 Ni x1 Me 1 1-x1 O2(i) In formula (1), "a1" satisfies the relationship "-0.3≦a1≦0.3". "x1" satisfies the relationship "0.1≦x1≦0.95". "Me 1 " indicates at least one selected from the group consisting of Co, Mn, Al, Zr, Ti, V, Cr, Fe, Cu, Zn, Mo, Sn, Ge, Nb, and W.

[0018] The NCM active material is, for example, LiNi 0.7 Co 0.2 Mn 0.1 O2, LiNi 0.7 Co 0.1 Mn 0.2 O2 and LiNi0.75 Co 0.15 Mn 0.1 O2 and LiNi 0.75 Co 0.1 Mn 0.15 O2 and LiNi 0.8 Co 0.1 Mn 0.1 The NCM active material may contain at least one selected from the group consisting of LiNi 0.7 Co 0.2 Mn 0.1 O2, LiNi 0.7 Co 0.1 Mn 0.2 O2 and LiNi 0.75 Co 0.15 Mn 0.1 O2 and LiNi 0.75 Co 0.1 Mn 0.15 O2 and LiNi 0.8 Co 0.1 Mn 0.1 O2.

[0019] The NCM active material may include, for example, single crystal particles, polycrystalline particles, or both single crystal particles and polycrystalline particles. The single crystal particles and polycrystalline particles may be, for example, a single particle, or may be an aggregate consisting of, for example, 2 to 10 primary particles. Primary particles refer to particles in which grain boundaries cannot be visually confirmed in an SEM image of the particle. The single crystal particles and polycrystalline particles may be, for example, spherical, columnar, clumpy, etc. The NCM active material preferably includes single crystal particles, and more preferably is a single crystal particle.

[0020] The single crystal particles and polycrystalline particles may have any size. The average particle size D50 of the single crystal particles may be, for example, 1 μm to 20 μm, preferably 1 μm to 10 μm, and more preferably 1 μm to 5 μm. The average particle size D50 of the polycrystalline particles may be, for example, 1 μm to 40 μm, preferably 1 μm to 30 μm, and more preferably 1 μm to 20 μm. The average particle size D50 represents the particle size at which the cumulative particle volume from the small particle size side in the volume-based particle size distribution is 50% of the total particle volume. The average particle size can be measured by a laser diffraction / scattering method.

[0021] A single crystal particle is, for example, 0.4 m 2 / g or more 5.0m 2 The polycrystalline particles may have a BET specific surface area of ​​0.1 m 2 / g or more 5.0m 2 / g or less. In this specification, the BET specific surface area is measured by a BET multipoint method.

[0022] <Method of manufacturing NCM active material for positive electrode> The method for producing an NCM active material for a positive electrode in this embodiment includes a selection step in which the above-mentioned method for selecting an NCM active material for a positive electrode is performed. By including the selection step in the method for producing an NCM active material for a positive electrode, it is possible to provide an NCM active material for a positive electrode that can reduce the amount of storage gas in a battery and improve storage characteristics. The method for producing an NCM active material for a positive electrode may further include a preparation step of preparing an NCM active material. For example, as shown in FIG. 2, the method for producing an NCM active material for a positive electrode includes a preparation step C and a selection step D. The above description applies to the NCM active material prepared in the preparation step C.

[0023] In the preparation step C, an NCM active material can be prepared. When the NCM active material is a lithium nickel cobalt manganese composite oxide, for example, it can be prepared by mixing a lithium source such as lithium hydroxide with a nickel cobalt manganese composite hydroxide and calcining the mixture to obtain a lithium nickel cobalt manganese composite oxide having an aggregated structure, and then adding a metal oxide thereto and subjecting the mixture to a heat treatment.

[0024] In the selection step D, if the NCM active material is determined to satisfy the above formula (1), the NCM active material can be selected as an NCM active material for a positive electrode. If the selected NCM active material for a positive electrode has not been surface-treated, it may be surface-treated in a subsequent surface treatment step.

[0025] <NCM active material for positive electrode> The positive electrode NCM active material in this embodiment has a mass reduction rate of 1.10 mass% / min or less. The above explanation applies to the mass reduction rate. When the positive electrode NCM active material has the above mass reduction rate, it is possible to reduce the amount of stored gas in the battery and improve storage characteristics. The positive electrode NCM active material can be obtained by the above-mentioned method for producing the positive electrode NCM active material.

[0026] The mass loss rate of the NCM active material for the positive electrode is preferably 1.00 or less, more preferably 0.45 or less, and even more preferably 0.40 or less, from the viewpoint of reducing the amount of gas stored, and is usually 0 or more, for example, 0.0001 or more, or 0.001 or more, or 0.01 or more, or 0.1 or more.

[0027] The above description of the NCM active material applies to the NCM active material for the positive electrode, except for the mass reduction rate. The NCM active material for the positive electrode may be, for example, 70 mol% or more, preferably 75 mol% or more, more preferably 80 mol% or more, even more preferably 85 mol% or more, and particularly preferably 90 mol% or more. The NCM active material for the positive electrode preferably contains single crystal particles, and more preferably is a single crystal particle.

[0028] <NCM active material mixture for positive electrode> The NCM active material mixture for the positive electrode in this embodiment contains the above-mentioned NCM-based active material for the positive electrode (hereinafter also referred to as the first NCM active material) and an NCM-based active material different from the NCM active material for the positive electrode (hereinafter also referred to as the second NCM active material).

[0029] The second NCM active material contains one or more nickel-, cobalt- and manganese-containing compounds. The nickel content ratio of the metal elements excluding lithium in the second NCM active material may be, for example, 70 mol% or more, preferably 75 mol% or more, more preferably 80 mol% or more, even more preferably 85 mol% or more, and particularly preferably 90 mol% or more. The nickel-, cobalt- and manganese-containing compound preferably contains a nickel-cobalt-manganese composite hydroxide, more preferably a lithium nickel-cobalt-manganese composite oxide. The nickel-cobalt-manganese composite hydroxide may be obtained by, for example, a coprecipitation method. The nickel-cobalt-manganese composite hydroxide may be, for example, a compound represented by the general formula: Ni x Co y Mn z It may be a compound represented by (OH)2 (wherein x+y+z=1). The lithium nickel cobalt manganese composite oxide may have a molar ratio of lithium to nickel, cobalt and manganese, Li:(Ni+Co+Mn), of, for example, 1.0 to 1.2:1.0.

[0030] The second NCM active material can include, for example, a second layered metal oxide having the formula (ii): Li 1-a1 Ni x1 Me 2 1-x1 O2(ii) In formula (1), "a1" satisfies the relationship "-0.3≦a1≦0.3". "x1" satisfies the relationship "0.1≦x1≦0.95". "Me 2 " indicates at least one selected from the group consisting of Co, Mn, Al, Zr, Ti, V, Cr, Fe, Cu, Zn, Mo, Sn, Ge, Nb, and W.

[0031] The second NCM active material is, for example, LiNi 0.7 Co 0.2 Mn 0.1 O2, LiNi 0.7 Co 0.1 Mn 0.2 O2 and LiNi 0.75 Co 0.15 Mn 0.1 O2 and LiNi 0.75 Co 0.1 Mn 0.15 O2 and LiNi 0.8 Co 0.1 Mn 0.1 The second NCM active material may include at least one selected from the group consisting of LiNi 0.7 Co 0.2 Mn 0.1 O2, LiNi 0.7 Co 0.1 Mn 0.2 O2 and LiNi 0.75 Co 0.15 Mn 0.1 O2 and LiNi 0.75 Co 0.1 Mn 0.15 O2 and LiNi 0.8 Co 0.1 Mn 0.1 O2.

[0032] The second NCM active material may include, for example, single crystal particles, may include polycrystalline particles, or may include both single crystal particles and polycrystalline particles. The second NCM active material preferably includes polycrystalline particles, and more preferably is polycrystalline particles. The above explanations apply to the single crystal particles and polycrystalline particles.

[0033] In the NCM active material mixture for the positive electrode, preferably the first NCM active material comprises single crystal particles and the second NCM active material comprises polycrystalline particles, more preferably the first NCM active material is single crystal particles and the second NCM active material is polycrystalline particles.

[0034] <Positive electrode plate> FIG. 3 is a schematic diagram showing an example of the configuration of a positive electrode plate in this embodiment. The positive electrode plate 10 includes, for example, a positive electrode substrate 11 and a positive electrode active material layer 12. The positive electrode substrate 11 is a conductive sheet. The positive electrode substrate 11 may be, for example, an aluminum alloy foil or the like. The positive electrode substrate 11 may have a thickness of, for example, 10 μm to 30 μm. The thickness of the positive electrode substrate 11 can be measured by a constant pressure thickness measuring instrument (thickness gauge). The positive electrode active material layer 12 can be disposed on the surface of the positive electrode substrate 11. The positive electrode active material layer 12 can be disposed on one side or both sides of the positive electrode substrate 11.

[0035] The positive electrode active material layer 12 may have a thickness of, for example, 10 μm to 200 μm. The thickness of the positive electrode active material layer 12 is measured on a cross-sectional SEM image of the positive electrode active material layer 12. The observation surface may be parallel to the thickness direction of the positive electrode active material layer 12. The thickness of each positive electrode active material layer 12 is measured at five or more points. The thickness of the positive electrode active material layer 12 is defined as the arithmetic average of the thicknesses at the five or more points. The density of the positive electrode active material layer 12 is, for example, 3.0 to 3.8 g / cm. 3 It can be more than that.

[0036] The positive electrode active material layer 12 includes active material particles 23. The active material particles 23 include the above-mentioned NCM active material for a positive electrode, and are preferably the above-mentioned NCM active material for a positive electrode. The positive electrode active material layer 12 can further include active material particles 24 as shown in FIG. 3. When the positive electrode active material layer 12 includes active material particles 24, the active material particles 23 can be the above-mentioned first NCM active material, and the active material particles 24 can be the above-mentioned second NCM active material.

[0037] The positive electrode active material layer 12 may contain a binder and a conductive assistant, although not shown. Examples of the binder include polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyimide (PI), polyamide (PA), polyamideimide (PAI), butadiene rubber (BR), styrene butadiene rubber (SBR), nitrile-butadiene rubber (NBR), styrene-ethylene-butylene-styrene block copolymer (SEBS), carboxymethyl cellulose (CMC), and combinations thereof. The content of the binder in the positive electrode active material layer 12 may be, for example, 0.5 to 10 wt %, and is preferably 1.0 to 5 wt %, based on the total solid content of the positive electrode active material layer 12 being 100 wt %.

[0038] The conductive assistant may include, for example, carbon black such as acetylene black, other carbon materials (e.g., graphite, etc.), carbon nanotubes, etc. The content of the conductive assistant in the positive electrode active material layer 12 may be, for example, 0.05 to 2.0 wt%, and preferably 0.10 to 1.0 wt%, based on the total solid content of the positive electrode active material layer 12 (100 wt%).

[0039] The method for producing the positive electrode plate 10 includes the steps of preparing a positive electrode slurry (E), applying (F), drying (G) and compressing (H) as shown in FIG.

[0040] In the preparation of the positive electrode slurry (E), a positive electrode slurry containing active material particles is prepared. The positive electrode slurry is prepared by dispersing the active material particles in a dispersion medium. The organic solvent may contain at least one selected from the group consisting of, for example, N-methyl-2-pyrrolidone (NMP), tetrahydrofuran (THF), dimethylformamide (DMF), methyl ethyl ketone (MEK), and dimethyl sulfoxide (DMSO). The amount of the organic solvent used is arbitrary. The positive electrode slurry may have any solid content concentration (mass fraction of solid content). The slurry may have a solid content concentration of, for example, 40% to 80%. Any stirring device, mixing device, or dispersing device may be used for mixing.

[0041] The coating (F) may include forming a coating film by applying the positive electrode slurry to the surface of the substrate. In the present embodiment, the positive electrode slurry may be applied to the surface of the substrate by any coating device.

[0042] Drying (G) may include, for example, heating and drying the coating film with a hot air dryer or the like to form a dried coating film. Compression (H) may include compressing the dried coating film using any compression device to form a positive electrode active material layer 12. The dried coating film is compressed to form the positive electrode active material layer 12, and the positive electrode plate 10 is completed. The positive electrode plate 10 may be cut to a predetermined planar size according to the specifications of the battery. The positive electrode plate 10 may be cut to have, for example, a band-like planar shape. The positive electrode plate 10 may be cut to have, for example, a rectangular planar shape.

[0043] <Battery> The battery in this embodiment may be a lithium ion battery. FIG. 5 is a schematic diagram showing an example of the battery in this embodiment. The battery 100 shown in FIG. 5 may be a lithium ion battery used, for example, as a main power source for an electric vehicle or a power source for power assist. The battery 100 includes an exterior body 90. The exterior body 90 houses an electrode body 50 and a non-aqueous electrolyte (not shown). The electrode body 50 is connected to a positive terminal 91 by a positive current collector 81. The electrode body 50 is connected to a negative terminal 92 by a negative current collector 82. FIG. 6 is a schematic diagram showing an example of the electrode body in this embodiment. The electrode body 50 is a wound type. The electrode body 50 includes a positive electrode plate 10, a separator 70, and a negative electrode plate 60. That is, the battery 100 includes a positive electrode plate 10. The positive electrode plate 10 includes a positive electrode active material layer 12 and a positive electrode substrate 11. The negative electrode plate 60 includes a negative electrode active material layer 62 and a negative electrode substrate 61 . EXAMPLES

[0044] The present disclosure will be described in more detail below with reference to examples. In the examples, "%" and "parts" are by mass % and parts by mass unless otherwise specified.

[0045] <Evaluation method for storage characteristics> [How to make the positive electrode plate] The first positive electrode active material and the second positive electrode active material [LiOH and Ni 0.83 Co 0.09 Mn 0.08 A transition metal compound synthesized from (OH)2. Particle size: 15-18μm, average particle size: 16μm, specific surface area: 0.20m 2 97.5 parts by mass of a mixture of 5:5 weight ratio of [polycrystalline particles of 1.5g / g], 1.5 parts by mass of carbon black as a conductive additive, and 1.0 parts by mass of polyvinylidene fluoride (PVdF) as a binder were mixed, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) was added to prepare a positive electrode slurry. This positive electrode slurry was applied to a current collector made of aluminum foil to form a positive electrode active material layer. It was then dried and compressed with a compression roller to a density of 3.55g / cm. 3 The mixture was compressed so that the thickness became 100 mm, cut into a predetermined size, and an aluminum tab was attached to form a positive electrode plate.

[0046] [How to make the negative electrode plate] The negative electrode active material, carboxymethyl cellulose (CMC) as a thickener, and styrene butadiene rubber (SBR) as a binder were weighed out in a mass ratio of 98:1:1, and dispersed in water to prepare a negative electrode slurry. The negative electrode slurry was applied to a current collector made of copper foil to form a negative electrode active material layer. The negative electrode active material layer was then dried, rolled to a predetermined thickness using a rolling roller, cut to a predetermined size, and attached with a nickel tab to form a negative electrode.

[0047] [Method of preparing non-aqueous electrolyte] Ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 30:30:40. Lithium hexafluorophosphate (LiPF6) was added to the mixed solvent to a concentration of 1.15 mol / L. Furthermore, vinylene carbonate (VC) was added to the mixed solvent at a concentration of 1.0 mass% relative to the total mass of the mixed solvent to prepare a non-aqueous electrolyte.

[0048] [How to prepare the test cell] The positive electrode plate and the negative electrode plate were laminated with a polyolefin separator interposed therebetween to prepare a laminated electrode assembly, which was then housed in an exterior body made of an aluminum laminate sheet, and the nonaqueous electrolyte was poured into the exterior body, and the opening of the exterior body was sealed to obtain a test cell.

[0049] [Evaluation of stored gas volume] The gas amount in the test cell in the above discharged state was determined as the gas amount before storage. After that, under the temperature condition of 25°C, the gas amount was 0.2 mA / cm 2 The battery was charged at a constant current density of 0.04 mA / cm until the voltage reached 4.25 V. 2 After charging at a constant voltage until the current reached 0.2 mA / cm, the battery was stored in a thermostatic chamber at 60°C for 60 days. 2 After constant current discharge at a current density of 0.60 cc or less until the voltage reached 3.0 V, the amount of gas was measured to obtain the amount of gas generated after storage. The amount of gas generated during storage was measured by subtracting the amount of gas generated before storage from the amount of gas generated after storage. If the amount of gas generated during storage is 0.60 cc or less, the storage characteristics are deemed to be good.

[0050] <Thermal mass spectrometry> [How to make the positive electrode plate] 97.5 parts by mass of the first positive electrode active material, 1.5 parts by mass of carbon black as a conductive material, and 1.0 parts by mass of polyvinylidene fluoride (PVdF) as a binder were mixed, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) was further added to prepare a positive electrode slurry. This positive electrode slurry was applied to a current collector made of aluminum foil to form a positive electrode mixture layer. Thereafter, the positive electrode was dried, rolled to a predetermined thickness using a rolling roller, cut to a predetermined size, and an aluminum tab was attached to form a positive electrode.

[0051] [Method of preparing non-aqueous electrolyte] Ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 30:30:40. Lithium hexafluorophosphate (LiPF6) was added to the mixed solvent to a concentration of 1.15 mol / L. Furthermore, vinylene carbonate (VC) was added to the mixed solvent at a concentration of 1.0 mass% relative to the total mass of the mixed solvent to prepare a non-aqueous electrolyte.

[0052] [How to prepare the test cell] A positive electrode plate and a metallic lithium sheet were wound with a polyolefin separator interposed therebetween to prepare a wound electrode assembly, which was then housed in an exterior body made of an aluminum laminate sheet, and the nonaqueous electrolyte was poured into the exterior body, and the opening of the exterior body was sealed to obtain a test cell.

[0053] [Sampling method for thermogravimetric analysis] The test cell was placed under a temperature condition of 25°C and discharged 0.2mA / cm 2 The battery was charged at a constant current density of 0.04 mA / cm until the voltage reached 4.35 V. 2 The charged cell was then disassembled in a glove box, the positive electrode plate was removed, washed with DMC, and dried in vacuum. The positive electrode mixture layer was scraped off from the core of the positive electrode plate to prepare a sample for thermogravimetric analysis.

[0054] [How to calculate mass reduction rate] 20 mg of the above sample was weighed out on a TG pan and set in a thermal analysis measuring device (Shimadzu DTG-60AH). Measurements were performed in an Ar atmosphere at a heating rate of 5°C / min and an upper limit temperature of 600°C. The mass loss from 100°C to 600°C and the mass loss rate per minute were calculated.

[0055] <Example 1> LiOH and Ni 0.83 Co 0.09 Mn 0.08The above-mentioned thermogravimetric analysis was carried out on single crystal particles made of a transition metal compound synthesized with (OH)2, and the mass loss rate at a temperature of 100 to 600°C and a heating rate of 5°C / min was 0.99% / min. Using these single crystal particles as the first positive electrode active material, the storage gas amount was measured according to the above-mentioned evaluation method for storage characteristics. The results are shown in Table 1 together with the average particle diameter (D50) and specific surface area of ​​the single crystal particles.

[0056] <Examples 2 and 3 and Comparative Examples 1 to 4> Single crystal particles [LiOH and Ni 0.83 Co 0.09 Mn 0.08 (OH)2 was synthesized to prepare single crystal particles of a transition metal compound, and the mass reduction rate was measured. The amount of gas stored in these single crystal particles was measured in the same manner as in Example 1. The results are shown in Table 1.

[0057] [Table 1]

[0058] As shown in Table 1, in Examples 1 to 3 in which the mass reduction rate was 1.10% / min or less, the amount of storage gas was 0.60cc or less, and the storage characteristics were good. In contrast, in Comparative Examples 1 to 4 in which the mass reduction rate was more than 1.10% / min, the amount of storage gas was more than 0.60cc, and sufficient storage characteristics were not obtained. In addition, it can be seen from Table 1 that the amount of storage gas generated is poorly correlated with both the average particle size and the specific surface area. Therefore, it can be seen that the selection method for a nickel-cobalt-manganese-based positive electrode active material of the present disclosure can select a nickel-cobalt-manganese-based positive electrode active material having good storage characteristics. [Explanation of symbols]

[0059] 10 positive electrode plate, 11 positive electrode substrate, 12 positive electrode active material layer, 22, 23 active material particles, 50 electrode body, 60 negative electrode plate, 61 negative electrode substrate, 62 negative electrode active material layer, 70 separator, 81 positive electrode current collector, 82 negative electrode current collector, 90 exterior body, 91 positive electrode terminal, 92 negative electrode terminal, 200 battery.

Claims

1. A method for selecting a nickel-cobalt-manganese based active material for a positive electrode, comprising: A thermogravimetric analysis step of determining the mass loss rate (mass% / min) of the nickel-cobalt-manganese active material at a temperature of 100 to 600° C. and a heating rate of 5° C. / min by thermogravimetric analysis; and When the mass reduction rate (mass% / min) is Wd, the nickel-cobalt-manganese-based active material has a mass reduction rate (mass% / min) satisfying the following formula: (1) Wd≦1.10 A determination step for determining whether the above condition is satisfied. The method for selecting a nickel-cobalt-manganese-based active material for a positive electrode includes the steps of:

2. 2. The method for selecting a nickel-cobalt-manganese-based active material for a positive electrode according to claim 1, wherein the thermogravimetric analysis step includes a sampling step of collecting a nickel-cobalt-manganese-based active material for thermogravimetric analysis from a charged battery.

3. 2. The method for selecting a nickel-cobalt-manganese based active material for a positive electrode according to claim 1, wherein the nickel-cobalt-manganese based active material has a nickel content of 70 mol % or more.

4. The method for selecting a nickel-cobalt-manganese based active material for a positive electrode according to claim 1 , wherein the nickel-cobalt-manganese based active material includes single crystal particles.

5. A method for producing a nickel-cobalt-manganese based positive electrode active material, comprising a selection step of carrying out the method for selecting a nickel-cobalt-manganese based positive electrode active material according to claim 1.

6. A nickel-cobalt-manganese-based active material for a positive electrode, which has a mass loss rate per minute of 1.10 mass % / min or less in thermogravimetric analysis at 100 to 600° C. and a heating rate of 5° C. / min.

7. 7. The nickel-cobalt-manganese-based active material for positive electrodes according to claim 6, having a nickel content of 70% or more.

8. 7. The nickel-cobalt-manganese based positive electrode active material of claim 6, comprising single crystal particles.

9. A mixture of nickel-cobalt-manganese-based positive electrode active materials comprising the nickel-cobalt-manganese-based positive electrode active material according to claim 6 and a nickel-cobalt-manganese-based positive electrode active material different from the nickel-cobalt-manganese-based positive electrode active material.

10. 10. The nickel-cobalt-manganese-based active material for the positive electrode according to claim 9, wherein the nickel-cobalt-manganese-based active material for the positive electrode comprises single crystal particles, and the nickel-cobalt-manganese-based active material different from the nickel-cobalt-manganese-based active material for the positive electrode comprises polycrystalline particles.

11. A positive electrode plate having a positive electrode active material layer containing the nickel-cobalt-manganese based positive electrode active material according to claim 6.

12. A non-aqueous electrolyte secondary battery comprising the positive electrode plate according to claim 11.

Citation Information

Patent Citations

  • Positive electrode composite material for lithium supplement purpose, lithium supplement charging and discharging method and application thereof

    CN114975900A

  • Positive electrode active material for lithium ion secondary battery and method of producing the same

    JP2012156046A

  • Spherical or pseudo-spherical positive electrode material of lithium ion battery, and manufacturing method and application thereof

    JP2018045998A

  • Positive electrode active material for secondary battery, method for producing the same, and lithium secondary battery including the same

    JP2020537298A

  • Positive electrode active material and lithium secondary battery using the same

    JP2022159119A