Rubber composition for paper feeding roller and paper feeding roller

Incorporating low-density polyethylene into the rubber composition for paper feed rollers improves moldability by enhancing fluidity and uniform mixing, addressing moldability issues and reducing defects in large-diameter rollers.

JP2024151056AInactive Publication Date: 2024-10-24SUMITOMO RUBBER INDUSTRIES LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023064175
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-11
Publication Date
2024-10-24
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional rubber compositions for paper feed rollers face challenges in moldability when forming rollers with large outer diameters, leading to molding defects such as insufficient filling, rubber cracking, and welding, due to limitations in increasing the amount of plasticizers like oil or wax to prevent surface bleeding.

Method used

Incorporating low-density polyethylene with a density of 0.910 g/cm³ to 0.930 g/cm³ into the rubber composition, which improves fluidity during molding, ensuring uniform mixing post-curing without affecting performance, thereby enhancing moldability and reducing defects.

Benefits of technology

The rubber composition achieves high moldability, suppressing molding defects, and maintains performance by using low-density polyethylene, which solidifies uniformly with the base rubber, preventing blooming and maintaining the integrity of the paper feed roller.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024151056000001_ABST
    Figure 2024151056000001_ABST
Patent Text Reader

Abstract

To provide a rubber composition for a paper feeding roller which has high moldability.SOLUTION: The rubber composition for a paper feeding roller contains a base rubber, a crosslinking agent, and a low-density polyethylene (excluding a linear low-density polyethylene). The density of the low-density polyethylene is 0.910-0.930 g / cm3. The content of the low-density polyethylene is 3-35 pts.mass based on 100 pts.mass of the base rubber.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rubber composition used in forming a paper feed roller. [Background technology]

[0002] Various paper feed rollers are incorporated into the paper feed mechanisms of devices such as electrostatic copiers, laser printers, plain paper facsimile machines, and all-in-one machines thereof, image forming devices such as inkjet printers, and automated teller machines (ATMs), etc. The paper feed rollers rotate while in contact with a sheet such as paper or plastic film, transporting the sheet by friction.

[0003] Paper feed rollers are often made of ethylene-propylene-diene rubber (EPDM). For example, Patent Document 1 describes a paper feed roller made of a crosslinked rubber composition containing a base rubber and 5 to 50 parts of ultra-high molecular weight polyethylene per 100 parts of the base rubber (see Patent Document 1 (Claim 1, paragraphs 0019 to 0021)). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2002-179263 A Summary of the Invention [Problem to be solved by the invention]

[0005] It is preferable that the outer diameter of the paper feed roller is large in order to increase the contact pressure area, but since it is difficult to mold a roller having such a large outer diameter, the rubber composition for the paper feed roller is required to have good moldability. Here, the moldability of the rubber composition can be improved by increasing the blending amount of a plasticizer such as oil, wax, etc. However, in the rubber composition for a paper-feed roller, the blending amount of a plasticizer such as oil, wax, etc. cannot be increased from the viewpoint of preventing bleeding onto the roller surface after molding and paper staining.

[0006] Therefore, when a conventional rubber composition for a paper-feed roller is used to mold a roller having a large outer diameter, molding defects (insufficient filling, rubber cracks, welds, etc.) tend to occur easily. The present invention has been made in view of the above circumstances, and has an object to provide a rubber composition for a paper-feed roller having high moldability. [Means for solving the problem]

[0007] The rubber composition for a paper-feed roller of the present invention, which has been able to solve the above problems, contains a base rubber, a crosslinking agent, and a low-density polyethylene (excluding linear low-density polyethylene), and the density of the low-density polyethylene is 0.910 g / cm 3 ~0.930g / cm 3 The content of the low-density polyethylene is 3 parts by mass to 35 parts by mass per 100 parts by mass of the base rubber.

[0008] By blending a predetermined amount of low-density polyethylene into the rubber composition, the flowability of the rubber composition during molding is improved, and moldability is improved. Therefore, even when molding a roller with a large outer diameter, molding defects can be suppressed. In addition, after the rubber is hardened, the low-density polyethylene solidifies in a state where it is uniformly mixed with the base rubber. Therefore, blooming does not occur, and the effect on the performance of the base rubber is small, and the moldability of the rubber composition can be improved without impairing the performance of the paper feed roller. Effect of the Invention

[0009] According to the present invention, a rubber composition for a paper-feed roller having high moldability can be obtained. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a perspective view showing an example of a paper feed roller of the present invention. [Diagram 2] FIG. 2 is a schematic diagram illustrating a method for measuring a friction coefficient. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] <Rubber composition for paper feed roller> The rubber composition for a paper-feed roller (hereinafter sometimes simply referred to as "rubber composition") contains a base rubber, a crosslinking agent, and a low-density polyethylene (however, linear low-density polyethylene is excluded).

[0012] (Base rubber) Examples of the base rubber include ethylene-α-olefin copolymer, natural rubber (NR), isoprene rubber (IR), butadiene rubber (BR), styrene butadiene rubber (SBR), acrylonitrile butadiene rubber (NBR), chloroprene rubber (CR), epichlorohydrin rubber, acrylic rubber, butyl rubber, silicone rubber, etc. These base rubbers may be used alone or in combination of two or more.

[0013] The base rubber preferably contains an ethylene-α-olefin copolymer. The ethylene-α-olefin copolymer is a copolymer containing at least ethylene and an α-olefin as constituent components. The ethylene-α-olefin copolymer also includes an ethylene-α-olefin-diene copolymer in which a double bond is introduced into the main chain by adding a small amount of a diene component to ethylene and an α-olefin. The ethylene-α-olefin copolymer may be used alone or in combination of two or more kinds.

[0014] Examples of the α-olefin include propylene, 1-butene, 1-hexene, and 1-octene. Examples of the diene component include ethylidene norbornene (ENB), 1,4-hexadiene (1,4-HD), dicyclopentadiene (DCP), and the like, with ethylidene norbornene being preferred.

[0015] Examples of the ethylene-α-olefin copolymer include ethylene-propylene copolymer (EPM), ethylene-butene copolymer (EBR), ethylene-propylene-butene copolymer (EPBR), ethylene-octene copolymer (EOR), etc. Examples of the ethylene-α-olefin-diene copolymer include ethylene-propylene-diene copolymer (EPDM), ethylene-butene-diene copolymer (EBDM), ethylene-propylene-butene-diene copolymer (EPBDM), etc. Examples of the ethylene-α-olefin copolymer include ethylene-propylene-diene copolymer (EPDM). As the ethylene-α-olefin copolymer, ethylene-propylene-diene copolymer (EPDM) is preferred.

[0016] The ethylene content of the ethylene-α-olefin copolymer is preferably 40% by mass or more, more preferably 45% by mass or more, and even more preferably 50% by mass or more, and is preferably 80% by mass or less, more preferably 75% by mass or less, and even more preferably 72% by mass or less. If the ethylene content is within the above range, it is easy to obtain commercially, is easy to mold into a paper feed roller, and a rubber more suitable for a paper feed roller can be obtained.

[0017] When the ethylene-α-olefin-diene copolymer is used as the ethylene-α-olefin copolymer, the content of the diene component is preferably 0.5% by mass or more, more preferably 1.0% by mass or more, and even more preferably 2.0% by mass or more, and is preferably 15% by mass or less, more preferably 13% by mass or less, and even more preferably 10% by mass or less. If the content of the diene component is within the above range, it is easy to obtain commercially, is easy to mold into a paper feed roller, and a rubber more suitable for a paper feed roller can be obtained.

[0018] The content of the ethylene-α-olefin copolymer in the base rubber is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 90% by mass or more, and even more preferably 100% by mass. If the content of the ethylene-α-olefin copolymer in the base rubber is 50% by mass or more, the ozone resistance of the obtained roller body is improved.

[0019] The ethylene-α-olefin copolymer may be of an oil-extended type, in which flexibility is adjusted by adding an extender oil, or of a non-oil-extended type, in which no extender oil is added, and either may be used. In the case of the oil-extended type, the mass of the extender oil added is treated as a processing aid.

[0020] When the rubber composition for paper feed rollers is used as a rubber composition for paper feed rollers forming paper feed rollers such as pick rollers, feed rollers, and retard rollers arranged around a paper feed tray, the base rubber preferably contains non-oil-extended EPDM and oil-extended EPDM. In this case, by blending oil-extended EPDM in which the extender oil is uniformly dissolved in the base rubber, the kneading time can be shortened and the workability of the kneading can be improved. In addition, the extender oil contained in the oil-extended EPDM is unlikely to bleed onto the outer peripheral surface of the roller body after molding, so that the moldability of the rubber composition can be improved while suppressing paper staining and the like.

[0021] Mooney viscosity ML of the non-oil-extended EPDM 1+4 (125°C) is preferably 38 or more and 120 or less, and more preferably 100 or less. Mooney viscosity ML of non-oil-extended EPDM 1+4 If the Mooney viscosity (ML 1+4 (125°C) is the value measured in accordance with JIS K6300-1 (2013) using an L rotor with a preheating time of 1 minute, rotor rotation time of 4 minutes, and at 125°C.

[0022] The oil-extended EPDM may be EPDM extended with any extender oil at any ratio. Examples of the extender oil include paraffin oil. The amount of the extender oil is preferably 70 parts by mass or more, more preferably 80 parts by mass or more, and preferably 150 parts by mass or less, more preferably 120 parts by mass or less, based on 100 parts by mass of EPDM.

[0023] In the rubber composition, the content of the extender oil in the oil-extended EPDM relative to 100 parts by mass of the total of EPDM and non-oil-extended EPDM in the oil-extended EPDM is preferably 10 parts by mass or more, and more preferably 15 parts by mass or more, and is preferably 100 parts by mass or less, and more preferably 90 parts by mass or less.

[0024] (Crosslinking agent) The rubber composition contains a crosslinking agent. Examples of the crosslinking agent include organic peroxides and sulfur-based crosslinking agents. When the rubber composition contains a crosslinking agent, the wear resistance of the resulting paper feed roller is further improved. The crosslinking agent may be used alone or in combination of two or more.

[0025] Examples of the organic peroxide include dicumyl peroxide, α,α'-bis(t-butylperoxy-m-diisopropyl)benzene, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, and 1,1-bis(t-butylperoxy)3,3,5-trimethylcyclohexane.

[0026] The sulfur-based crosslinking agent may be, for example, elemental sulfur or a sulfur donor compound. The elemental sulfur may be, for example, powdered sulfur, precipitated sulfur, colloidal sulfur, or insoluble sulfur. The sulfur donor compound may be, for example, 4,4'-dithiobismorpholine.

[0027] The content of the crosslinking agent is preferably 1.5 parts by mass or more, more preferably 2.0 parts by mass or more, and even more preferably 2.5 parts by mass or more, and is preferably 5.0 parts by mass or less, more preferably 4.0 parts by mass or less, and even more preferably 3.5 parts by mass or less, based on 100 parts by mass of the base rubber. If the content of the vulcanizing agent is 1.5 parts by mass or more, the wear resistance of the formed roller is further improved, and if it is 5.0 parts by mass or less, the hardness of the formed roller is not too high, and the friction coefficient is better.

[0028] (Low Density Polyethylene) The rubber composition contains low-density polyethylene (LDPE). Low-density polyethylene is a homopolymer of ethylene, has a randomly branched structure in the molecular chain, and has a density of 0.910 g / cm 3 ~0.930g / cm 3 The low-density polyethylene has a melting point of about 100°C to 120°C, and melts at the molding temperature of the rubber composition. This increases the fluidity of the rubber composition during molding, improving moldability. After the rubber is cured, the low-density polyethylene solidifies in a state where it is uniformly mixed with the base rubber, so blooming does not occur, and the effect on the performance of the base rubber is small.

[0029] The melt mass flow rate (190°C, 2.16 kg) of the low-density polyethylene is preferably 1 g / 10 min or more, more preferably 5 g / 10 min or more, and even more preferably 10 g / 10 min or more. If the melt mass flow rate is 1 g / 10 min or more, the low-density polyethylene has a low molecular weight, good fluidity, and is more easily mixed during rubber kneading. The upper limit of the melt mass flow rate (190°C, 2.16 kg) of the low-density polyethylene is not particularly limited, but is usually about 100 g / 10 min. The melt mass flow rate of the low-density polyethylene is measured according to JIS K7210-1 (2014).

[0030] The melting point of the low-density polyethylene is preferably 115° C. or lower, more preferably 110° C. or lower. If the melting point is 115° C. or lower, the molecular structure is randomly branched, the flowability is good, and the mixture is more easily mixed during rubber kneading. The lower limit of the melting point of the low-density polyethylene is not particularly limited, but is usually about 100° C. The melting point of the low-density polyethylene is measured according to JIS K7121 (1987).

[0031] The content of the low-density polyethylene is at least 3 parts by mass, preferably at least 5 parts by mass, more preferably at least 10 parts by mass, and at most 35 parts by mass, preferably at most 30 parts by mass, and even more preferably at most 20 parts by mass, per 100 parts by mass of the base rubber. When the content of the low-density polyethylene is within the above range, the moldability of the rubber composition can be improved while suppressing a decrease in the friction coefficient of a paper feed roller.

[0032] The low-density polyethylene blended in the rubber composition is preferably a powder having a volume-based median diameter (50% diameter) (particle diameter corresponding to cumulative 50% in a volume cumulative distribution in which the small diameter side is 0%) of 100 μm or less. Blending powdered low-density polyethylene in the rubber composition allows for more homogeneous mixing during rubber kneading. The volume-based median diameter of the low-density polyethylene powder is preferably 100 μm or less, more preferably 60 μm or less, and even more preferably 30 μm or less. The lower limit of the volume-based median diameter of the low-density polyethylene powder is not particularly limited, but is usually about 1 μm. The volume-based median diameter is measured by a laser diffraction method.

[0033] The linear low density polyethylene is a copolymer of ethylene and an α-olefin having 3 to 20 carbon atoms. Examples of the α-olefin having 3 to 20 carbon atoms include 1-butene, 1-hexene, 1-octene, and 4-methyl-1-pentene. The low density polyethylene does not include linear low density polyethylene (LLDPE). The linear low density polyethylene does not improve the rubber flowability during rubber molding, and therefore does not provide an effect of improving the moldability of the rubber composition.

[0034] (Other Ingredients) The rubber composition may contain compounding agents that are generally used as compounding agents for rubber, such as fillers, crosslinking accelerators, antioxidants, hinderers, and pigments, within the scope of the present invention.

[0035] (filling material) As the filler, those generally used as compounding agents for rubber can be used, for example, carbon black, silica, calcium carbonate, talc, clay, magnesium carbonate, aluminum oxide, etc., with carbon black and calcium carbonate being preferred. By compounding a filler, the mechanical strength, etc. of the obtained roller can be improved.

[0036] The amount of the filler is preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and is preferably 80 parts by mass or less, more preferably 60 parts by mass or less, based on 100 parts by mass of the base rubber. If the amount of the filler is within the above range, the flexibility and durability of the obtained paper feed roller will be good.

[0037] When the rubber composition for paper feed rollers is used as a rubber composition for paper feed rollers, the content of the filler is preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and preferably 30 parts by mass or less, more preferably 20 parts by mass or less, based on 100 parts by mass of the base rubber. If the content of the filler is within the above range, the flexibility of the obtained paper feed roller will be further improved. When the rubber composition for paper feed rollers is used as a rubber composition for transport rollers, the content of the filler is preferably 20 parts by mass or more, more preferably 30 parts by mass or more, and preferably 80 parts by mass or less, more preferably 60 parts by mass or less, based on 100 parts by mass of the base rubber. If the content of the filler is within the above range, the durability of the resulting transport roller will be further improved.

[0038] (Crosslinking promoter) The rubber composition may contain a crosslinking promoter. An example of the crosslinking promoter is zinc oxide. The amount of the crosslinking promoter used is preferably 1 part by mass or more and 10 parts by mass or less per 100 parts by mass of the base rubber.

[0039] (Anti-aging agent) Examples of the antioxidant include nickel diethyldithiocarbamate and nickel dibutyldithiocarbamate.

[0040] (Rubber composition) The rubber composition for paper feed rollers can be prepared by blending the base rubber, the crosslinking agent, and the low-density polyethylene, and other raw materials as necessary, and kneading the mixture with a kneader, a Banbury mixer, an open roll, etc. The kneading method and conditions are appropriately selected depending on the production scale.

[0041] <Paper feed roller> The paper-feeding roller of the present invention is formed from the rubber composition for a paper-feeding roller. Methods for molding the paper feed roller include transfer molding, extrusion molding, compression molding, etc. The rubber composition for the paper feed roller has high fluidity and is easily pressed into a mold, so it is particularly suitable for transfer molding.

[0042] The shape of the paper feed roller may be cylindrical, columnar, polygonal tubular, or polygonal columnar. When the paper feed roller is cylindrical or polygonal tubular, it is preferable that the paper feed roller has a shaft. The material of the shaft is not particularly limited, and may be metal, ceramic, resin, or the like.

[0043] When the paper feed roller is a paper feed roller, the type A durometer hardness of the roller body is preferably 30 or more, more preferably 35 or more, even more preferably 40 or more, and is preferably 60 or less, more preferably 55 or less, even more preferably 50 or less. If the type A durometer hardness of the roller body of the paper feed roller is 30 or more, the wear resistance of the roller body will be improved and the product life will be longer, and if it is 60 or less, the flexibility of the roller body will be improved and the coefficient of friction with paper will be improved.

[0044] When the paper feed roller is a transport roller, the type A durometer hardness of the roller body is preferably 50 or more, more preferably 60 or more, and is preferably 85 or less, more preferably 80 or less. If the type A durometer hardness of the roller body of the transport roller is 50 or more, the product life at high speed paper feed will be longer, and if it is 85 or less, the coefficient of friction will be better maintained even when paper is fed at high speed.

[0045] An example of a paper feed roller is shown in Figure 1. The paper feed roller 1 shown in Figure 1 is equipped with a roller body 2 formed into a cylindrical shape from the above-mentioned rubber composition of the present invention. A through hole 3 having a circular cross section is provided in the center of the roller body 2, and a cylindrical shaft 4 connected to a drive system (not shown) is inserted and fixed into the through hole 3. The outer circumferential surface of the roller body 2 is formed into a cylindrical shape concentric with the through hole 3 and the shaft 4.

[0046] The roller body 2 and the shaft 4 are fixed to each other so as not to slip, for example, by press-fitting the shaft 4, whose outer diameter is larger than the inner diameter of the through hole 3, into the through hole 3 of the roller body 2. In other words, a certain amount of slip torque (the limit torque at which slip does not occur) is ensured between the two by the tightening margin based on the diameter difference between the two.

[0047] The shaft 4 is made of, for example, metal, ceramic, hard resin, etc. A plurality of roller bodies 2 may be fixed to a single shaft 4 at a plurality of positions, if necessary. Methods for manufacturing the roller body 2 include a method in which a rubber composition is molded into a cylindrical shape by extrusion molding or the like, and then crosslinked by a press crosslinking method or the like; and a method in which a rubber composition is molded into a cylindrical shape and crosslinked at the same time by transfer molding or the like.

[0048] At any point in the above manufacturing process, the outer circumferential surface of the roller body 2 may be polished to a predetermined surface roughness, knurled, embossed, or the like, as necessary. In addition, both ends of the roller body 2 may be cut so that the outer circumferential surface has a predetermined width. The outer circumferential surface of the roller body 2 may be covered with any coating layer.

[0049] The roller body 2 may be formed in a two-layer structure with an outer layer on the outer peripheral surface side and an inner layer on the through hole 3 side. In that case, it is preferable that at least the outer layer is formed from the rubber composition of the present invention. However, in consideration of simplifying the structure, improving productivity, and reducing manufacturing costs, it is preferable that the roller body 2 has a single-layer structure as shown in FIG.

[0050] The roller body 2 may have a porous structure. However, in order to improve wear resistance and reduce compression set, thereby making it difficult for dents to form due to deformation even if contact at one point continues for a relatively long period of time, it is preferable that the roller body 2 has a substantially non-porous structure.

[0051] Depending on the application of the paper feed roller 1, the through hole 3 may be provided at a position eccentric to the center of the roller body 2. Also, the outer circumferential surface of the roller body 2 may not be cylindrical but may be irregularly shaped, for example, a part of the cylindrical outer circumferential surface may be cut out in a flat shape. To manufacture a paper feed roller 1 having a roller body 2 of such an irregular shape, the roller body 2 of the irregular shape may be directly molded by the manufacturing method described above and then crosslinked, or the roller body 2 molded into a cylindrical shape may be post-processed to have the irregular shape.

[0052] Alternatively, the roller body 2 may be deformed into the irregular shape by press-fitting the shaft 4 having a deformed shape corresponding to the irregular shape of the roller body 2 formed into a cylindrical shape into the through hole 3 of the roller body 2 . In this case, polishing, knurling, texturing, etc. of the outer peripheral surface 5 can be performed on the cylindrical outer peripheral surface 5 before deformation, so that workability can be improved.

[0053] <Image forming device> The paper feed roller of the present invention can be incorporated in various image forming apparatuses that utilize electrophotography, such as laser printers, electrostatic copying machines, plain paper facsimile machines, or combination machines of these, etc. The paper feed roller of the present invention can also be incorporated in inkjet printers, ATMs, etc.

[0054] The paper feed roller of the present invention rotates while in contact with a sheet, and feeds or transports the sheet by friction. Examples of the sheet include individual sheets such as paper sheets and continuous sheets such as continuous paper. The paper feed roller can be used as a paper feed roller such as a pick roller, feed roller, or retard roller arranged around a paper feed tray, or as a transport roller such as a registration roller, platen roller, or paper discharge roller. EXAMPLES

[0055] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the following examples, and all modifications and embodiments that do not deviate from the spirit of the present invention are included within the scope of the present invention.

[0056] [Evaluation method] (1)Hardness The hardness of the roller body was measured on the surface of the roller body with the shaft pressed in using a micro rubber hardness tester ("MD-1" manufactured by Kobunshi Keiki Co., Ltd.) The measurement was carried out in an environment of 23°C temperature and 55% relative humidity, and a type A indenter was used to pierce the measurement sample, and the value was recorded 3 seconds after the needle was inserted.

[0057] (2) Friction coefficient measurement As shown in Figure 2, plain paper 11 (P paper (width 60 mm, length 210 mm) manufactured by Fujifilm Business Innovation) was placed on a horizontally placed polytetrafluoroethylene (PTFE) plate 10. The roller body 2 of the paper feed roller 1 was placed on this paper 11, and a vertical load W1 (=300 gf) was applied to the shaft 4 to press it against the plate 10. Next, in an environment of a temperature of 23°C and a relative humidity of 55%, the roller body 2 was rotated at 200 rpm in the direction indicated by the dashed arrow R1, and the conveying force F (gf) applied to the load cell 12 connected to one end of the paper 11 was measured. The initial friction coefficient μ was calculated from the measured conveying force F and the vertical load W1 (=300 gf) using formula (1). μ = F(gf) / W1(gf) (1)

[0058] (3) Forced wear test As shown in Figure 2, plain paper 11 (P paper, manufactured by Fujifilm Business Innovation) was placed on a horizontally placed polytetrafluoroethylene (PTFE) plate 10. The roller body 2 of the paper feed roller 1 was placed on this paper 11, and a vertical load W1 (= 500 gf) was applied to the shaft 4 to press it against the plate 10. Next, the roller body 2 was rotated continuously for 10 minutes at 200 rpm in the direction indicated by the dashed arrow R1 in an environment of a temperature of 23° C. and a relative humidity of 55%. 0 (g) and the mass W of the roller body 2 after rotation 1 The abrasion weight loss rate ΔM (%) was calculated from (g) using the following formula (2). ΔM(%)=100×(W 0 -W 1 ) / W 0 (2)

[0059] [Preparation of rubber composition for paper feed roller] The raw materials were mixed to obtain the composition shown in Table 1, and a rubber composition for a paper feed roller was prepared. Specifically, the raw materials other than the crosslinking agent were first mixed using a kneader to prepare a mixture. At this time, the mixture was mixed for 2 minutes or more at a temperature in the kneader tank (temperature inside the tank) of 80°C to 130°C. Next, the obtained mixture was cooled, and the mixture and the crosslinking agent were mixed using an open roll with a surface temperature controlled at 50°C, to prepare a rubber composition.

[0060] [Table 1]

[0061] The raw materials used in Table 1 are as follows: Oil-extended EPDM: Sumitomo Chemical's "Esprene (registered trademark) 670F" (oil-extended EPDM) (ethylene content 66% by mass, diene content 4.0% by mass, oil added amount 100 parts by mass per 100 parts by mass of EPDM) Non-oil-extended EPDM: Sumitomo Chemical's "Esprene (registered trademark) 586" (non-oil-extended EPDM) (ethylene-propylene-ethylidene norbornene copolymer, ethylene content 66% by mass, diene content 12.5% ​​by mass, Mooney viscosity (M 1+4 (125℃))60) LDPE: Sumitomo Seika Chemicals' "Flothane (registered trademark) UF20" (low density polyethylene, density 0.919 cm 3 / g, melt mass flow rate (190℃, 2.16kg) 20g / 10min, melting point 106℃, volumetric median diameter 20μm) UHMWPE: Mitsui Chemicals' "Mipelon (registered trademark) XM220" (ultra-high molecular weight polyethylene, density 0.94 cm 3 / g) LLDPE: Prime Polymer's "Ultsex (registered trademark) 25100J" (linear low-density polyethylene, density 0.923 cm 3 / g) Organic peroxide: NOF Corp.'s "Percumyl (registered trademark) D" (dicumyl peroxide) Carbon black: Tokai Carbon Co., Ltd., Seast (registered trademark) 3

[0062] [Manufacturing of paper feed rollers] The paper feed roller was produced by transfer molding using the rubber composition for paper feed roller prepared above. A mold having 100 cylindrical cavities (outer diameter 21 mm, inner diameter 11 mm, depth 70 mm) (10 vertical rows, 10 horizontal rows) was used as the mold. A pot mold having a gate to each cavity was placed on top of the mold, 2500 g of the rubber composition was poured into the pot mold, and a pot lid was placed on top of it. After the rubber composition was heated to about 80°C to 100°C in the pot, the pot lid was pushed in and the rubber composition was pressed into each cavity. The pressing conditions were 10 MPa and 1 minute. Subsequently, air was removed and bumping was performed, and then heat treatment was performed at 170°C for 20 minutes to perform crosslinking.

[0063] After cooling, the cured rubber was taken out and checked for molding defects (filling defects) and rated according to the following criteria. ◎: No defective hardened products Good: 1 to 5 pieces of hardened material with molding defects ×: 6 or more pieces of hardened products with molding defects

[0064] The cylindrical cured rubber product obtained above was polished to an outer diameter of 20 mm, and then cut to a length of 24 mm to produce a roller body. A shaft (diameter 12 mm) was inserted into the through hole of this roller body to produce a paper feed roller. The obtained paper feed roller was evaluated, and the results are shown in Table 1. The initial friction coefficient μ and wear loss rate ΔM (%) of the paper feed roller were evaluated according to the following criteria. <Friction coefficient μ> ◎: 1.65≦μ≦2.05 ○: 1.55≦μ<1.65, or 2.05<μ≦2.15 ×: μ<1.55 or 2.15<μ <Abrasion loss rate ΔM (%)> ◎:ΔM≦0.06 ○: 0.06<ΔM≦0.08 △:0.08<ΔM≦0.10 ×:0.10<ΔM

[0065] Rubber composition No. 1 does not contain low density polyethylene. This rubber composition No. 1 had poor moldability and many molding defects. The wear resistance of the resulting paper feed roller was also poor.

[0066] Rubber compositions No. 2 to 6 have a density of 0.910 g / cm 3 ~0.930g / cm 3 The rubber compositions Nos. 2 to 6 contained 3 to 35 parts by mass of low-density polyethylene relative to 100 parts by mass of the base rubber. These rubber compositions had good moldability and reduced molding defects. In particular, when the content of low-density polyethylene was 10 to 30 parts by mass relative to 100 parts by mass of the base rubber, no molding defects occurred. Furthermore, the paper feed rollers obtained from these rubber compositions also had good friction coefficients and wear resistance.

[0067] Rubber composition No. 7 has a density of 0.910 g / cm 3 ~0.930g / cm 3 The rubber composition No. 7 contained 40 parts by mass of low-density polyethylene based on 100 parts by mass of the base rubber. The flowability of the rubber composition No. 7 was too high, resulting in molding defects. In addition, the friction coefficient of the resulting paper feed roller was poor.

[0068] Rubber compositions No. 8 and 9 have a density of 0.940 g / cm 3 (0.930g / cm 3 These rubber compositions No. 8 and No. 9 had poor moldability and produced many molding defects.

[0069] Rubber compositions Nos. 10 and 11 contain linear low density polyethylene. These rubber compositions Nos. 10 and 11 had poor moldability and resulted in many molding defects.

[0070] [Preparation of rubber composition for conveyor roller] The raw materials were mixed to obtain the composition shown in Table 2, and a rubber composition for a conveying roller was prepared. Specifically, the raw materials other than the crosslinking agent were first mixed using a kneader to prepare a mixture. At this time, the mixture was mixed for 2 minutes or more at a temperature in the kneader tank (temperature inside the tank) of 80°C to 130°C. Next, the obtained mixture was cooled, and the mixture and the crosslinking agent were mixed using an open roll with a surface temperature controlled to 50°C, to prepare a rubber composition.

[0071] [Table 2]

[0072] The raw materials used in Table 2 are as follows: Non-oil-extended EPDM: "Esprene (registered trademark) 505A" (non-oil-extended EPDM) manufactured by Sumitomo Chemical (ethylene-propylene-ethylidene norbornene copolymer, ethylene content 50% by mass, diene content 9.5% by mass, Mooney viscosity (M 1+4 (100℃))47) LDPE: Sumitomo Seika Chemicals' "Flothane (registered trademark) UF20" (low density polyethylene, density 0.919 cm 3 / g, melt mass flow rate (190℃, 2.16kg) 20g / 10min, melting point 106℃, volumetric median diameter 20μm) UHMWPE: Mitsui Chemicals' "Mipelon (registered trademark) XM220" (ultra-high molecular weight polyethylene, density 0.94 cm 3 / g) LLDPE: Prime Polymer's "Ultsex (registered trademark) 25100J" (linear low-density polyethylene, density 0.923 cm 3 / g) Organic peroxide: NOF Corp.'s "Percumyl (registered trademark) D" (dicumyl peroxide) Carbon black: Tokai Carbon Co., Ltd., Seast (registered trademark) 3 Calcium carbonate: Shiraishi Calcium Co., Ltd., Hakuenka Process oil: Idemitsu Kosan Co., Ltd., Diana Process Oil PW380

[0073] [Manufacturing of conveyor rollers] The transport roller was produced by transfer molding using the rubber composition for the transport roller prepared above. A mold having 100 cylindrical cavities (outer diameter 13 mm, inner diameter 5.5 mm, depth 70 mm) (10 vertical rows, 10 horizontal rows) was used as the mold. A pot mold having a gate to each cavity was placed on top of the mold, 1500 g of the rubber composition was poured into the pot mold, and a pot lid was placed on top of it. After the rubber composition was heated to about 80°C to 100°C in the pot, the pot lid was pushed in and the rubber composition was pressed into each cavity. The pressing conditions were 10 MPa and 1 minute. Subsequently, air was removed and bumping was performed, and then heat treatment was performed at 170°C for 20 minutes to perform crosslinking.

[0074] After cooling, the cured rubber was taken out and checked for molding defects (filling defects) and rated according to the following criteria. ◎: No defective hardened products Good: 1 to 5 pieces of hardened material with molding defects ×: 6 or more pieces of hardened products with molding defects

[0075] The cylindrical cured rubber product obtained above was polished to an outer diameter of 12 mm, and then cut to a length of 10 mm to produce a roller body. A shaft (diameter 6 mm) was inserted into the through hole of this roller body to produce a conveying roller. The resulting conveying roller was evaluated, and the results are shown in Table 2. The initial friction coefficient μ and wear loss rate ΔM (%) of the conveying roller were evaluated according to the following criteria. <Friction coefficient μ> ◎: 1.33≦μ≦1.73 ○: 1.23≦μ<1.33, or 1.73<μ≦1.83 ×: μ<1.23, 1.83<μ <Abrasion loss rate ΔM (%)> ◎:ΔM≦0.08 ○: 0.08<ΔM≦0.10 △:0.10<ΔM≦0.12 ×:0.12<ΔM

[0076] Rubber compositions No. 12 to 16 have a density of 0.910 g / cm 3 ~0.930g / cm 3 The rubber compositions Nos. 12 to 16 contained 3 to 35 parts by mass of low-density polyethylene relative to 100 parts by mass of the base rubber. These rubber compositions had good moldability and reduced molding defects. In particular, when the content of low-density polyethylene was 10 to 30 parts by mass relative to 100 parts by mass of the base rubber, no molding defects occurred. Furthermore, in particular, when the content of low-density polyethylene was 15 to 30 parts by mass relative to 100 parts by mass of the base rubber, the conveying rollers obtained from these rubber compositions had good friction coefficients and wear resistance.

[0077] Rubber compositions No. 17 and 18 have a density of 0.940 g / cm 3 (0.930g / cm 3 These rubber compositions No. 17 and No. 18 had poor moldability and resulted in many molding defects.

[0078] Rubber compositions Nos. 19 and 20 contain linear low density polyethylene. These rubber compositions Nos. 19 and 20 had poor moldability and resulted in many molding defects.

[0079] The present invention (1) comprises a base rubber, a crosslinking agent, and a low-density polyethylene (excluding linear low-density polyethylene), and the density of the low-density polyethylene is 0.910 g / cm 3 ~0.930g / cm 3 and the content of the low-density polyethylene is 3 parts by mass to 35 parts by mass per 100 parts by mass of the base rubber.

[0080] The present invention (2) is the rubber composition for a paper-feeding roller according to the present invention (1), wherein the low-density polyethylene is a powder having a volume-based median diameter of 100 μm or less.

[0081] The present invention (3) relates to the rubber composition for a paper-feeding roller according to the present invention (1) or (2), wherein the base rubber contains an ethylene-propylene-diene copolymer.

[0082] The present invention (4) is a paper-feeding roller characterized in that a roller body is molded from the rubber composition for a paper-feeding roller according to any one of the present inventions (1) to (3). [Explanation of symbols]

[0083] 1: paper feed roller, 2: roller body, 3: through hole, 4: shaft, 10: plate, 11: paper, 12: load cell

Claims

1. Contains a base rubber, a crosslinking agent, and low-density polyethylene (excluding linear low-density polyethylene), The density of the low density polyethylene is 0.910 g / cm 3 ~0.930g / cm 3 and A rubber composition for a paper-feed roller, comprising: a low-density polyethylene having a content of 3 to 35 parts by mass relative to 100 parts by mass of the base rubber.

2. 2. The rubber composition for a paper-feeding roller according to claim 1, wherein the low-density polyethylene is in the form of a powder having a volume-based median diameter of 100 μm or less.

3. 2. The rubber composition for a paper-feeding roller according to claim 1, wherein the base rubber contains an ethylene-propylene-diene copolymer.

4. A paper-feeding roller, the roller body being formed from the rubber composition for paper-feeding rollers according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Paper feed roller

    JP2002179263A