Glass interposer and method for manufacturing glass interposer
The glass interposer addresses the challenges of moisture absorption and thermal expansion in conventional interposers by using laminated glass substrates with conductive resin paste, ensuring easy manufacturing and effective conductivity.
Patent Information
- Application Number
- JP2023064403
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-11
- Publication Date
- 2024-10-24
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional interposers using organic resin materials face issues with moisture absorption and thermal expansion, leading to difficulty in fine interconnection formation and potential deformation due to differing thermal expansion coefficients, while glass interposers with non-glass materials are costly and challenging to miniaturize.
A glass interposer formed by laminating glass substrates with integrated wiring recesses and through-holes, using conductive resin paste for conductivity, and bonded under vacuum to eliminate non-glass materials, ensuring smooth bonding and reduced thermal expansion.
The glass interposer achieves easy manufacturing, good conductivity, and reduced deformation risks, while maintaining fine wiring integrity and cost-effectiveness.
Smart Images

Figure 2024151193000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a glass interposer and a manufacturing method thereof, and more particularly to a glass interposer that is easy to manufacture and has good electrical conductivity, and a manufacturing method thereof. [Background technology]
[0002] Semiconductor elements such as various memories, CPUs, and GPUs mounted on a circuit board have terminals for electrical connection. The pitch of the connection terminals and the pitch of the connection parts of the circuit board that are electrically connected to the semiconductor elements usually differ by several to several tens of times. Therefore, an intermediate board for connection called an interposer is used to electrically connect the semiconductor elements and the circuit board. The semiconductor elements are mounted on one side of the interposer, and the circuit board is connected to the other side.
[0003] Organic resin materials have been used as materials for interposers. However, in order to improve the processing power of semiconductor elements and respond to high integration, there is a demand for fine wiring formation in interposers. However, with interposers that use conventional organic resin materials, the resin absorbs moisture and expands and contracts greatly depending on the temperature, making it difficult to handle fine wiring.
[0004] Therefore, currently, to address the issues with organic resin materials, interposers using silicon and glass as base materials are being developed. These inorganic materials are less susceptible to moisture absorption, and their thermal expansion coefficients are similar to those of semiconductor elements, reducing the effects of expansion and contraction due to temperature.
[0005] However, interposers using silicon as a base material require surface protection, and the materials, processing costs, etc. are expensive. For this reason, glass interposers are currently in vogue (see Patent Documents 1 and 2, etc.).
[0006] However, conventional glass interposers have layers of materials other than glass, making it difficult to miniaturize wiring, and there is a risk of deformation defects such as warping due to the difference in thermal expansion coefficient between glass and other materials. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2016-046361 A [Patent Document 2] JP 2019-044212 A Summary of the Invention [Problem to be solved by the invention]
[0008] After that, the inventors conducted extensive research and eventually developed a glass interposer that uses no materials other than the glass substrate and the conductive material of the wiring portion.
[0009] The present invention has been made in consideration of the above-mentioned points, and provides a glass interposer and a manufacturing method thereof that is easy to manufacture and has good conductivity, without using any materials other than the glass material that forms the substrate and the conductive material for the wiring portion in the configuration of the glass interposer. [Means for solving the problem]
[0010] That is, the glass interposer of the embodiment is formed by stacking and bonding a plurality of glass substrates, the glass substrate has a plurality of wiring recesses formed at predetermined positions on the main surface of the glass substrate, a plurality of fine through holes formed in the wiring recesses and penetrating the glass substrate, and a wiring portion made of a conductive material that is disposed in the wiring recesses and the fine through holes, each of the fine through holes is composed of two hemispherical depressions and has a shape in which hemispherical curved portions are bonded together, the upper surface portion of the wiring portion that is disposed in the wiring recesses is positioned 1 to 50 μm lower than the main surface of the glass substrate, and the glass substrates are bonded together in a vacuum.
[0011] Furthermore, in the glass interposer, the glass substrate may have a thickness of 10 to 100 μm.
[0012] Furthermore, in the glass interposer, the radius of the hemispherical recess of the fine through-hole may be 2 / 3 to 3 / 4 of the thickness of the glass substrate.
[0013] Furthermore, in the glass interposer, the conductive material may be a conductive resin paste containing fine metal particles.
[0014] That is, the manufacturing method of the glass interposer of the embodiment is characterized in that, when arranging the wiring portion, a conductive material is filled into the wiring recess and the fine through-hole formed in the glass substrate by a micro-dispenser.
[0015] Furthermore, in the method for manufacturing a glass interposer, when bonding the glass substrates together in a vacuum, the glass substrates may be bonded together at room temperature, or the glass substrates may be bonded together under heating at room temperature or 200°C. Effect of the Invention
[0016] According to the glass interposer of the present invention, a plurality of glass substrates are laminated and bonded together, and the glass substrate has a plurality of wiring recesses formed at predetermined positions on the main surface of the glass substrate, a plurality of fine through holes formed in the wiring recesses and penetrating the glass substrate, and a wiring portion made of a conductive material that is disposed in the wiring recesses and the fine through holes, and each of the fine through holes is composed of two hemispherical depressions and has a shape in which hemispherical curved portions are bonded together, and the upper surface portion of the wiring portion that is disposed in the wiring recess is disposed at a position 1 to 50 μm lower than the main surface of the glass substrate, and since the glass substrates are bonded together in a vacuum, no materials are used other than the glass material that forms the substrate and the conductive material of the wiring portion, and a glass interposer that is easy to manufacture and has good conductivity can be obtained.
[0017] Furthermore, according to the manufacturing method of the glass interposer of the present invention, when arranging the wiring portion, a conductive material is filled into the wiring recesses and the fine through holes formed in the glass substrate by a micro-dispenser, making the manufacturing process simple and inexpensive. [Brief description of the drawings]
[0018] [Figure 1] 1 is a schematic cross-sectional view showing a mounted state of a glass interposer according to an embodiment. [Diagram 2] FIG. 2A is a schematic cross-sectional view of a fine through-hole and FIG. 2B is a schematic cross-sectional view of a wiring portion of a glass substrate to be laminated as a glass interposer. [Diagram 3] 1A is a schematic cross-sectional view of a fine through-hole, and FIG. 1B is a schematic cross-sectional view of a wiring portion of a glass substrate in another form to be laminated as a glass interposer. [Figure 4] 1A is a first schematic cross-sectional view, FIG. 1B is a second schematic cross-sectional view, and FIG. 1C is a third schematic cross-sectional view showing a manufacturing process of a glass substrate. [Diagram 5] 3A is a fourth schematic cross-sectional view, FIG. 3B is a fifth schematic cross-sectional view, and FIG. 3C is a sixth schematic cross-sectional view showing a manufacturing process of a glass substrate. [Figure 6] FIG. 2A is a first schematic diagram and FIG. 2B is a second schematic diagram showing the formation of a wiring portion on a glass substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The glass interposer of the embodiment is a member that serves as a relay substrate for electrically connecting semiconductor elements such as various memories, CPUs, and GPUs mounted on a circuit board to the circuit board via wiring. In particular, the glass interposer itself is formed only from glass and conductive materials for wiring, and does not include materials with different thermal expansion coefficients such as resins, thereby reducing deformation due to heat exposure during use.
[0020] 1 is a schematic cross-sectional view showing a mounting state of a glass interposer 1 according to an embodiment. The glass interposer 1 is formed by laminating a plurality of glass substrates 2 (glass wiring substrates for lamination) and bonding them together to form an integrated structure. In the figure, a base substrate 3 is disposed directly below the glass interposer 1, and base substrate side wiring 4 and connection pads 5 are provided on the base substrate 3. A circuit board, a printed circuit board, etc. (not shown) of an electronic device are disposed on the base substrate 3 and are electrically connected. In addition, semiconductor elements (not shown) such as various memories, CPUs, and GPUs are mounted directly above the glass interposer 1.
[0021] Each glass substrate 2 of the glass interposer 1 has a plurality of wiring portions 8 arranged thereon, penetrating the glass substrate 2 in the thickness direction. When the glass substrates 2 are stacked, the wiring portions 8 of the glass substrates 2 can be joined along the stacking direction. As a result, an electrical connection is established between the circuit board of the electronic device and the semiconductor element mounted on the glass interposer 1.
[0022] The glass substrate 2 constituting the glass interposer 1 is made of glass materials such as soda lime glass, borosilicate glass, aluminosilicate glass, and quartz glass, and is manufactured as a thin plate by a float method or the like. The thickness of the glass substrate 2 is preferably in the range of 10 to 100 μm. If the thickness of the glass substrate 2 increases, the conductivity of the glass interposer 1 itself decreases. In addition, when the fine through-holes 6 are formed by the etching process described below, the areas above and below the fine through-holes 6 increase. Therefore, the area for wiring that can be developed on the surface of the glass substrate 2 decreases. Then, the area of the glass interposer 1 must be increased, and the circuit design must be enlarged. Therefore, a thin glass plate (glass sheet) is used for the glass substrate 2 from the viewpoints of miniaturization of the circuit design and conductivity.
[0023] In the glass interposer 1, the glass substrates 2 are stacked and bonded together, so it is desirable that the surfaces of the glass substrates 2 are as smooth as possible. As mentioned above, the glass plates are manufactured by the float method, so the surface smoothness (degree of unevenness) is about 10 to 100 nm. Note that surface polishing can be performed separately to adjust the surface smoothness. For polishing, a cerium oxide abrasive (fine particles) is usually used.
[0024] FIG. 2 is a partially enlarged schematic cross-sectional view of one of the glass substrates 2 constituting the glass interposer 1. A plurality of wiring recesses 7 are formed at predetermined positions on the main surface 11 (first surface) of the glass substrate 2. At the same time, a plurality of wiring recesses 7 are formed at predetermined positions on the secondary surface 12 (second surface) opposite to the main surface 11 (first surface) of the glass substrate 2. The predetermined positions here refer to positions where wiring is to be formed on the glass substrate 2. A plurality of fine through holes 6 are formed in the glass substrate 2. Each fine through hole 6 connects the wiring recess 7 on the main surface 11 (first surface) to the wiring recess 7 on the secondary surface 12 (second surface), and each fine through hole 6 penetrates the glass substrate 2 from the main surface 11 to the secondary surface 12. FIG. 2(A) is a schematic cross-sectional view of the glass substrate 2 with the fine through holes 6 formed therein. For convenience of illustration, only one fine through hole 6 is shown.
[0025] A conductive material 9 is disposed (filled) in the wiring recesses 7 and the fine through holes 6 of the main surface 11 and the secondary surface 12. Thus, in the wiring portion 8, the conductivity between the main surface 11 (first surface) and the secondary surface 12 (second surface) of the glass substrate 2 is ensured. FIG. 2(B) is a schematic cross-sectional view showing an enlarged view of the wiring portion 8 and its vicinity. For convenience of illustration, only one fine through hole 6 and wiring portion 8 are shown. Then, when the main surface 11 of the second glass substrate 2 is laminated and bonded to the secondary surface 12 of the first glass substrate 2, the wiring recesses 7 of the main surface 11 of the second glass substrate 2 are bonded to the wiring recesses 7 of the secondary surface 12 of the first glass substrate 2, and the conductivity of the multiple glass substrates 2 is ensured (see FIG. 1).
[0026] Each of the micro through holes 6 formed in the glass substrate 2 is formed by combining two hemispherical recesses 6k, and is formed in a shape in which the curved portions of the hemispherical recesses 6k are joined together. The micro through holes 6 are shaped approximately like the number "8" in a vertical cross-sectional view. A recess 7 for wiring is formed on the opening 6p side of the hemispherical recess 6k. The recess 7 for wiring is sized to ensure conductivity when stacked with another glass substrate 2, that is, to allow the recesses 7 for wiring to come into contact with each other.
[0027] The conductive material 9 used in the wiring portion 8 is preferably a conductive resin paste containing fine particles of metal such as copper, silver, gold, platinum, nickel, and lead. The conductive resin paste is based on acrylic resin, urethane resin, and various organic solvents, and fine metal particles are dispersed in the base material at a ratio of 60 to 90% by weight. This conductive resin paste contains a conductive resin ink. When forming the wiring portion 8, a method of applying a resin coating material is used, as will be understood from the description of the manufacturing method described later. Of course, a conventional method of plating metal may also be adopted. Therefore, as the conductive material 9, a coating material containing fine metal particles is injected into the wiring recess 7 and the fine through hole 6. The wiring recess 7 and the fine through hole 6 are filled with a coating material containing fine metal particles, and the fine metal particles act as a conductive material.
[0028] Here, the upper surface 15 of the wiring portion 8 disposed in the recess 7 for wiring is disposed at a position 1 to 50 μm lower than the main surface 11 (and the secondary surface 12) of the glass substrate 2. As described above, the wiring portion 8 is formed of the conductive material 9. It is considered that the resin component and metal particles of the conductive material 9 thermally expand due to heat generation in the usage environment of the glass interposer 1.
[0029] If the upper surface 15 of the wiring portion 8 where the conductive material 9 is placed in the recess 7 for wiring is made to be at the same height as the main surface 11 (and the secondary surface 12) of the glass substrate 2, the conductive material 9 may leak from the recess 7 for wiring or the fine through-hole 6 due to thermal expansion. Furthermore, the leaked conductive material 9 may penetrate into the gaps between the glass substrates 2 and reduce the adhesion between the glass substrates 2. For this reason, the upper surface 15 of the wiring portion 8 which is intentionally placed in the recess 7 for wiring is made to be lower than the main surface 11 (and the secondary surface 12) of the glass substrate 2, and the amount of the conductive material 9 is adjusted so that they are just bonded to each other when the glass interposer 1 is assembled.
[0030] Here, in the hemispherical recess 6k of the micro through hole 6 of the glass substrate 2, the radius R of the recess 6k when the recess 6k is regarded as a sphere is set to a range of 2 / 3 to 3 / 4 of the thickness of the glass substrate 2. In the embodiment disclosed in FIG. 2, the center of the recess 6k when the recess 6k is regarded as a sphere is present in the glass substrate 2. When the radius R of the recess 6k is about half the thickness T of the glass substrate 2, the recesses 6k formed on the main surface 11 and the secondary surface 12 of the glass substrate 2 do not contact each other, and the micro through hole 6 is meaningless. In addition, if the radius R of the recess 6k is too large, it takes time to form the micro through hole 6, and the productivity decreases. In other words, it is sufficient that the hemispherical curved surface parts of the recess 6k are in moderate contact with each other and communicate with each other, and the filled conductive material 9 can penetrate from the main surface 11 to the secondary surface 12.
[0031] 3 is a schematic cross-sectional view of another type of glass substrate 2 laminated as a glass interposer. As shown in FIG. 3(A), in the illustrated glass substrate 2, when the recess 6k is regarded as a sphere, the center of the hemispherical recess 6k is present outside the glass substrate 2. As can be seen from the drawing, the shape of the recess 6k of the fine through-hole 6 is relatively free and does not necessarily have to be strict. Even with the glass substrate 2 of this type, it is possible to arrange the wiring portion 8 in the fine through-hole 6 as shown in FIG. 3(B). Of course, the radius R of the recess 6k is defined to be in the range of 2 / 3 to 3 / 4 of the thickness of the glass substrate 2, as in the case of FIG. 2.
[0032] In the glass interposer 1 of FIG. 1, the bonding of the individual glass substrates 2 is performed under vacuum. It is empirically known that glass is easily bonded when the same type of glass is in surface contact. Therefore, when manufacturing the glass interposer 1, the individual glass substrates 2 are carried into a vacuum chamber (not shown), and the individual glass substrates 2 are stacked on top of each other in the vacuum chamber. The degree of vacuum is adjusted to a value taking into consideration actual production. In a vacuum state, the amount of molecules such as nitrogen and oxygen near the main surface 11 and the secondary surface 12 of the glass substrate 2 is reduced, and the glass material of the glass substrate 2 itself is exposed, making bonding easier than in air. In particular, even if the smoothness (degree of unevenness) of the surface of the glass substrate 2 is 10 to 100 nm, the vacuum state improves the adhesion between the glass substrates 2, making the bonding stronger.
[0033] Furthermore, when bonding in a vacuum, the glass substrates 2 may be bonded together at room temperature, or the glass substrates 2 may be bonded together under heating at room temperature or 200°C. By heating, the reactivity between the surfaces of the glass substrates 2 can be increased, albeit slightly. Note that since the heating is not intended to melt the glass material, the temperature is milder than that for glass transition, etc.
[0034] 4 to 6, a method for manufacturing the individual glass substrates 2 that constitute the glass interposer 1 will be described. The illustrated manufacturing method is an example, and is not necessarily limited to the illustrated example.
[0035] As shown in FIG. 4(A), a thin glass plate (glass sheet) that will become the glass substrate 2 is prepared, and as shown in FIG. 4(B), a protective portion 20 such as a photoresist or a chrome mask is formed in the area other than the area where the wiring is to be formed. The area where the wiring is to be formed is an exposed area 21. Then, as shown in FIG. 4(C), etching is performed on the area not treated with the photoresist, that is, the exposed area 21 where the wiring is to be formed. In the etching, the glass substrate 2 comes into contact with a mixed acid solution of, for example, hydrofluoric acid and hydrochloric acid, and the glass of the glass substrate 2 that is directly exposed to the mixed acid solution corrodes and dissolves. The glass of the glass substrate 2 is locally dissolved by the etching, and a removed portion 22 of a predetermined depth is formed. This removed portion 22 becomes the recess 7 for wiring.
[0036] In Fig. 5(A), etching continues on the removed portion 22, and dissolution of the glass of the glass substrate 2 progresses. As shown in Fig. 5(B), corrosion penetrates further from the removed portion 22 into the inside of the glass substrate 2, forming a hemispherical depression 6k. The depressions 6k formed on the main surface 11 and the secondary surface 12 of the glass substrate 2 contact each other at the center in the thickness direction of the glass substrate 2, and penetrate from the main surface 11 to the secondary surface 12, forming a fine through hole 6. In Fig. 5(C), the protective portion 20 such as a photoresist or a chrome mask is removed, decomposed, and cleaned by laser irradiation or the like, and the original main surface 11 and secondary surface 12 of the glass substrate 2 are exposed.
[0037] When a laser is used to drill the glass substrate 2, it is possible to form the fine through-holes 6 at high density by controlling the irradiation position. In contrast, according to the formation of the fine through-holes 6 in the glass substrate 2 of FIG. 4 and FIG. 5, it is possible to form the fine through-holes 6 only by etching the glass material without using processing equipment such as a carbon dioxide gas laser. As a result, it is possible to suppress the capital investment of the equipment required for manufacturing. In addition, since the fine through-holes 6 are formed by joining the recesses 6k formed by etching, the fine through-holes 6 can be formed almost straight from the main surface 11 to the secondary surface 12 of the glass substrate 2. Therefore, it is possible to form the fine through-holes 6 at the same density as the drilling of the glass substrate 2 by the laser.
[0038] 6 is a schematic diagram showing how a conductive material 9, specifically a conductive resin paste, is filled into a fine through hole 6 formed in a glass substrate 2. In this embodiment, when arranging a wiring portion 8, the conductive material 9 is filled into the wiring recess 7 formed in the glass substrate 2 and the fine through hole 6 by a micro-dispenser 30.
[0039] 6(A), a microsyringe 31 is used as the micro-dispenser 30, and the conductive resin paste is stored in the microsyringe 31 and dispensed from the microsyringe 31 in a predetermined amount into the wiring recess 7 and the fine through-hole 6. In the figure, the microsyringe 31 is disposed on the main surface 11 side of the glass substrate 2. In addition, microsyringes may be disposed on both the main surface 11 side and the secondary surface 12 side of the glass substrate 2, and the conductive resin paste may be dispensed from both microsyringes.
[0040] 6(B), a sprayer 36 (inkjet mechanism) used in a printing machine such as an inkjet printer is used. A predetermined amount of conductive resin paste stored in an ink tank or the like (not shown) is discharged from the sprayer 36 and sprayed onto the wiring recess 7 and the fine through-hole 6. Of course, the sprayer 36 may be disposed on both the main surface 11 side and the secondary surface 12 side of the glass substrate 2.
[0041] Since the viscosity and fluidity of the conductive resin paste can be adjusted according to the amount of solvent, it can be discharged from the micro-dispenser 30 even if it contains metal particles. Furthermore, since the fine through-holes 6 have a shape in which hemispherical depressions 6k are stacked, the inner surface area of the fine through-holes 6 is larger than that of a cylinder formed by drilling with a laser. Therefore, it is considered that the conductive resin paste easily spreads inside the fine through-holes 6 due to the surface tension of the conductive resin paste.
[0042] Furthermore, since no known plating technique such as electrolytic plating is used when arranging the wiring portion 8 in the fine through-hole 6, there is no need to install and peel off a protective film on the portion not to be plated. In addition, the burden of waste liquid treatment such as plating solution is reduced.
[0043] Thereafter, the multiple glass substrates 2 with the wiring portions 8 arranged in the micro through holes 6 and the recessed portion for wiring 7 are accurately laminated while checking the position of the recessed portion for wiring 7. The multiple glass substrates 2 are laminated together under vacuum such as in a vacuum chamber. The lamination may be performed at room temperature or under heating from room temperature to 200°C. The multiple glass substrates 2 are bonded together in close contact with each other through the lamination under vacuum. [Explanation of symbols]
[0044] 1 Glass Interposer 2. Glass substrate 3 Base Board 4 Base board side wiring 5 Connection Pads 6 Micro through holes 6k depression 7 Wiring recess 8 Wiring section 9. Conductive Materials 11 Main surface (first surface) 12 Second Face 15 Top part 20 Protection part 21 Exposed part 22 Removal part 30 Micro-dispensing machine 31 Micro Syringe 36 Squirt machine R Radius of the recess T Glass substrate thickness
Claims
1. A glass interposer formed by laminating and bonding a plurality of glass substrates, The glass substrate is A plurality of recesses for wiring formed at predetermined positions on a main surface of the glass substrate; a plurality of fine through holes formed in the wiring recess and penetrating the glass substrate; a wiring portion made of a conductive material and disposed in the wiring recess and the fine through hole, Each of the micro through holes is composed of two hemispherical recesses and has a shape in which the hemispherical curved portions are joined together, an upper surface of the wiring portion disposed in the recess for wiring is disposed at a position 1 to 50 μm lower than a main surface of the glass substrate; The glass substrates are bonded together in a vacuum. A glass interposer comprising:
2. 2. The glass interposer according to claim 1, wherein the glass substrate has a thickness of 10 to 100 μm.
3. 2. The glass interposer according to claim 1, wherein the radius of the hemispherical recess of the fine through-hole is 2 / 3 to 3 / 4 of the thickness of the glass substrate.
4. 2. The glass interposer according to claim 1, wherein the conductive material is a conductive resin paste containing fine metal particles.
5. A method for manufacturing the glass interposer according to claim 1, comprising the steps of: When arranging the wiring portion, the conductive material is filled into the wiring recess and the fine through hole formed in the glass substrate by a micro-dispenser. A method for manufacturing a glass interposer comprising the steps of:
6. 5. The method for manufacturing a glass interposer according to claim 4, wherein, when the glass substrates are bonded to each other under vacuum, the glass substrates are bonded to each other under room temperature, or the glass substrates are bonded to each other under heating at room temperature or 200°C.
Citation Information
Patent Citations
Glass interposer
JP2016046361A
Plating method to glass substrate and production method of glass interposer
JP2019044212A