Method for operating copper smelting
By adding a sulfur source to the matte in copper smelting to sulfurize excess metallic Cu, the coexistence of slag, matte, and metal phases is minimized, stabilizing furnace operation and preventing brick damage.
Patent Information
- Application Number
- JP2023064892
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-04-12
AI Technical Summary
The increasing use of recycled raw materials in copper smelting leads to an increase in metallic Cu, which exceeds its solubility in matte, causing the coexistence of slag, matte, and metal phases, resulting in impurity concentration, brick damage, and operational risks.
Adding a sulfur source (S source) to the matte when metallic Cu exceeds solubility limits, using FeS minerals or pyrite, pyrrhotite, or chalcopyrite, and adjusting the specific surface area and specific gravity to ensure complete sulfurization of metallic Cu into matte.
Reduces the generation of metallic Cu phase, preventing impurity concentration and brick damage, ensuring stable furnace operation.
Smart Images

Figure 2024151511000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a copper smelting operation. [Background technology]
[0002] In the reaction shaft of a copper smelting flash furnace, a reaction gas is fed from a concentrate burner together with smelting raw materials such as copper concentrate and solvent. The copper concentrate undergoes an oxidation reaction due to the reaction gas, producing matte and slag at the bottom of the reaction shaft (see, for example, Patent Documents 1 to 3). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2002-363659 A [Patent Document 2] Japanese Patent Application Publication No. 11-140554 [Patent Document 3] Special Publication No. 01-036539 Summary of the Invention [Problem to be solved by the invention]
[0004] In recent years, the ratio of recycled raw materials as smelting raw materials has been increasing. However, recycled raw materials may contain metallic Cu. As the amount of recycled raw materials processed increases, the ratio of metallic Cu supplied to copper smelting furnaces increases. When the amount of metallic Cu supplied to a matte smelting furnace (a flash smelting furnace) increases and exceeds the solubility of metallic Cu in matte, three phases, slag, matte, and metal, coexist in the furnace. When metal accumulates at the bottom of a flash smelting furnace, it promotes the concentration of impurity elements in the metal phase, the penetration of low-melting-point metal into the joints of the hearth bricks, and the impregnation of the bricks themselves, increasing the risk of molten metal leaking from the bottom of the hearth. In addition, when the amount of metal exceeds a certain amount and reaches the matte tap hole level, metal is suddenly discharged from the matte hole, which may cause the risk of melting the metal matte trough, and may also cause operations to be disrupted by the supply of high-impurity metal to the converter.
[0005] The present invention has been made in consideration of the above problems, and has an object to provide a copper smelting operation method capable of reducing the formation of metallic Cu phase. [Means for solving the problem]
[0006] The copper smelting operation method according to the present invention is characterized in that, in matte produced by reacting a smelting raw material containing copper concentrate and a raw material containing metallic Cu with a reaction gas in a reaction shaft of a flash smelting furnace, an S source is added to the matte when a metal phase of the metallic Cu is produced. The S source may be added to the matte when the metallic Cu is contained in the smelting raw material in an amount exceeding the solubility in the matte. The S source may be added to the matte when a metal phase of the metallic Cu is confirmed in the matte by sampling the matte. The S source may be added to the matte by mixing the S source with the smelting raw material. The S source may be added to the matte by injecting the S source together with an inert gas from an injection nozzle toward the matte. The S source in a briquette form may be added to the matte. The S source may be mixed with other smelting raw materials to form briquettes, and the briquettes may be added to the matte. The specific gravity of the briquettes may be adjusted when the S source is mixed with other smelting raw materials to form briquettes. The S source may be mixed with recycled materials or other smelting materials to form agglomerates, thereby increasing the throughput of the recycled materials. The specific surface area of the S source is 20 mm 2 / g or more. The S source may be supplied to the matte in an amount sufficient to matte the entire amount of the metallic Cu. Assuming that 90 mass% of S contributes to matting the metallic Cu when the total S contained in the S source is 100 mass%, the S source may be supplied to the matte in an amount sufficient to matte the entire amount of the metallic Cu. The S source may contain elemental sulfur or a sulfide. The S source may further contain Fe. The S source containing Fe may be chalcopyrite, pyrite, or pyrrhotite. Effect of the Invention
[0007] According to the present invention, it is possible to provide a copper smelting operation method capable of reducing the formation of metallic Cu phase. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a diagram illustrating a schematic configuration of a flash furnace for copper smelting according to an embodiment. [Diagram 2] FIG. 2 is a diagram illustrating the details of a concentrate burner 4. [Diagram 3] FIG. 2 is a phase diagram showing the solubility of Cu in the matte. [Figure 4] FIG. 2 is a diagram illustrating an injection nozzle. [Diagram 5] FIG. 1 illustrates an experimental setup. [Figure 6] 1A is a photograph showing the results of a comparative example, and FIG. 1B is a photograph showing the results of Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] (Embodiment) FIG. 1 is a diagram showing a schematic configuration of a flash smelting furnace 100 for copper smelting according to an embodiment. As shown in FIG. 1, the flash smelting furnace 100 includes a reaction shaft 1 in which concentrate and reaction gas are mixed, a settler 2, and an uptake 3. A concentrate burner 4 is provided on the ceiling of the reaction shaft 1. The concentrate burner 4 supplies a reaction main blast gas, a reaction auxiliary gas, and a dispersion gas (which also contributes to the reaction) into the reaction shaft 1 together with copper concentrate, solvent, recycled raw materials, etc. (hereinafter, these solid raw materials are referred to as smelting raw materials). For example, the reaction main blast gas and the reaction auxiliary gas are oxygen-enriched air, and the dispersion gas is air or oxygen-enriched air.
[0010] FIG. 2 is a diagram illustrating the details of the concentrate burner 4, and is an explanatory diagram showing the input section 10 that inputs the smelting raw material, the main reaction blast gas, the auxiliary reaction gas, and the dispersion gas into the reaction shaft 1.
[0011] The input section 10 of the concentrate burner 4 is provided with a lance 16, and a first passage 11 through which the dispersion gas passes and a fourth passage 14 through which the reaction auxiliary gas passes are formed in the lance 16. The fourth passage 14 is provided in the center of the lance 16, and the first passage 11 is provided around the fourth passage 14. The input section 10 is also provided with a second passage 12 as a raw material flow path provided on the outside of the lance 16, more specifically on the outer periphery of the lance 16. The input section 10 further includes a third passage 13 provided on the outside of the second passage 12, more specifically on the outer periphery of the second passage 12, through which the reaction main blast gas passes. The third passage 13 is formed by a tubular portion provided so as to surround the second passage 12, and communicates with a funnel-shaped air chamber 17 provided above it. The second passage 12 and the third passage 13 are separated by a cylindrical partition wall 21.
[0012] The first passage 11 supplies the dispersion gas into the reaction shaft 1. The second passage 12 supplies the concentrate into the reaction shaft 1. The third passage 13 supplies the main reaction blast gas from the air chamber 17 into the reaction shaft 1. The fourth passage 14 supplies the auxiliary reaction gas into the reaction shaft 1.
[0013] A hollow truncated cone-shaped dispersion cone 15 is formed at the tip (lower end) of the lance 16. A plurality of supply holes 152 are formed in a lower side portion 151 of the dispersion cone 15 to discharge the dispersion gas that has passed through the first passage 11 into the reaction shaft 1. The supply holes 152 are provided so that the gas is discharged in the normal direction to the bottom circle of the dispersion cone 15.
[0014] When the smelting raw materials are fed into the reaction shaft 1 from the concentrate burner 4, the copper concentrate containing sulfides undergoes an oxidation reaction according to the following reaction formula (1) and separates into matte 5 and slag 6 at the bottom of the reaction shaft 1, as shown in Figure 1. In the following reaction formula (1), Cu2S·FeS corresponds to the main component of matte 5, and FeO·SiO2 corresponds to the main component of slag 6. Silica ore is used as the solvent. CuFeS2+SiO2+O2→Cu2S·FeS+FeO·SiO2+SO2+ Reaction heat (1)
[0015] The recycled raw material may contain metallic Cu. If the amount of metallic Cu is small, the metallic Cu is sulfidized and becomes matte 5 during the process of falling from the concentrate burner 4. Therefore, no metal phase is generated.
[0016] However, as the amount of recycled raw materials processed increases, the proportion of metallic Cu in the smelting raw materials tends to increase. In recent years, the proportion of metallic Cu in the Cu component of the smelting raw materials may be 6.0 mass% or more and 28.0 mass% or less, or 9.0 mass% or more and 18.0 mass% or less, or 9.0 mass% or more and 12.0 mass% or less.
[0017] When the ratio of metallic Cu in the smelting raw material becomes high, metallic Cu is not completely sulfidized during the process of falling from the concentrate burner 4 and falls as metallic Cu. Although metallic Cu dissolves in matte 5 to a certain extent, there is a solubility limit. Figure 3 is a phase diagram showing the solubility of Cu in matte at 1250°C. In Figure 3, "matte(l)" indicates the range in which metallic Cu can dissolve in matte. "matte(l)+Cu(l)" indicates the range in which metallic Cu cannot dissolve in matte and a metal phase is generated. The phase diagram in Figure 3 is taken from "Takazaietsu, Yazawa Akira, 1983, Senkeniho."
[0018] In this embodiment, when the amount of metallic Cu supplied into the flash smelting furnace 100 exceeds the solubility in matte 5, a raw material containing Fe and S (hereinafter referred to as "S source") is supplied as a matte source for metallic Cu. For example, based on the phase diagram of FIG. 3, an S source is supplied in an amount equal to or greater than the amount of metallic Cu that mattes the entire amount of metallic Cu. Thereby, metallic Cu becomes a sulfide containing Fe and S, mattes, and dissolves in matte 5. As a result, the generation of metallic Cu phase at the hearth of the flash smelting furnace 100 can be suppressed.
[0019] Whether or not the supply amount of metallic Cu exceeds the solubility in matte 5 can be determined by sampling the smelting raw material and measuring the composition ratio. Alternatively, it may be determined that the supply amount of metallic Cu exceeds the solubility in matte 5 when a metal phase is confirmed by sampling the matte 5 of the reaction shaft 1.
[0020] As the S source, FeS minerals (pyrrhotite), FeS2 minerals (pyrite), CuFeS2 minerals (chalcopyrite), minerals containing FeS·FeS2, copper concentrate containing S, etc. can be used. When comparing FeS minerals and FeS2 minerals, it is preferable to use FeS2 minerals, which are said to contain more sulfur necessary for matte formation. Alternatively, as the S source, waste slag containing S generated in the ore-dressing process of non-ferrous metal raw materials can be used. For example, tailings generated in the flotation process are an example of waste slag containing S.
[0021] When the total S contained in the S source is 100 mass%, there is a risk that the 100 mass% S does not contribute to the matting of metallic Cu. Therefore, it is preferable to charge an excess amount of S source into the furnace. For example, when the total S contained in the S source is 100 mass%, it is preferable to supply an S source in an amount greater than or equal to the amount of matting of the entire metallic Cu, based on the phase diagram of FIG. 3, when it is assumed that 90 mass% of S contributes to the matting of metallic Cu, based on the phase diagram of FIG. 3, when it is assumed that 80 mass% of S contributes to the matting of metallic Cu, based on the phase diagram of FIG. 3, it is preferable to supply an S source in an amount greater than or equal to the amount of matting of the entire metallic Cu, based on the phase diagram of FIG. When the total S contained in the S source is 100 mass%, it is preferable to supply an S source in an amount greater than or equal to the amount of matting of the entire metallic Cu, based on the phase diagram of FIG. When it is assumed that 70 mass% of S contributes to the matting of metallic Cu, based on the phase diagram of FIG. 3, when it is assumed that 100 mass% of S contributes to the matting of metallic Cu, based on the phase diagram of FIG.
[0022] If a powdered raw material with a large specific surface area is used as the S source, the S source may be oxidized before reacting with metallic Cu due to the oxidizing power of the reaction gas in the reaction shaft 1. Therefore, it is preferable to use a lump-shaped S source. If the S source has a lump shape with a small specific surface area, the oxidation loss during the time it passes through the reaction shaft 1 can be suppressed, and it will arrive directly at the molten metal drop area directly below the reaction shaft 1, come into contact with the matte 5 and metallic Cu, and react. As the S source having a lump shape, a pelletized powdered raw material containing S, a natural mineral, or a melt-formed material can be used.
[0023] On the other hand, if the specific surface area is too small, there is a risk that the S source will remain unreacted in the matte 5 when it is removed from the flash smelting furnace. Since it is unreacted, it cannot contribute to matte formation, and as a result, there is a risk that a metal phase will be formed on the floor of the settler 2. For this reason, specifically, the specific surface area of the S source is set to be 20 mm 2 It is preferable that the molecular weight is 1 / g or more.
[0024] The S source may be added by mixing it with the smelting raw material. Alternatively, the S source may be introduced into the reaction shaft 1 using an inert gas as a carrier. By using an inert gas, the S source can be brought into contact with the matte 5 and metallic Cu while suppressing oxidation of the S source. For example, as illustrated in FIG. 4, an injection nozzle 40 may be provided in the reaction shaft 1, and the S source can be introduced into the reaction shaft 1 from the injection nozzle 40. Alternatively, a briquetted S source or a lump-shaped S source may be added toward the settling bath directly below the reaction shaft 1. For example, molten droplets mainly composed of slag and matte generated in the reaction shaft 1 rain down on the settling bath surface like a shower from above, and when the briquetted S source or a lump-shaped S source is supplied to the molten bath surface part where the molten droplets rain down, the S source comes into contact with the matte 5 and S is supplied to the matte 5. In order to reduce the oxidation of the S source in the gas phase as much as possible, it is effective to use a briquetted or lump-shaped S source having a small specific surface area. In addition, instead of briquetting only the S source, by adjusting the specific gravity by mixing and briquetting with other smelting raw materials, it becomes possible to supply S to the matte 5 more efficiently. For example, by mixing the S source with a powdered recycled raw material mainly composed of Cu, it is possible to form a briquette having a higher specific gravity than that of slag, making it easier for the briquette to reach the matte 5. For example, when only copper concentrate is briquetteed as the S source, the specific gravity varies depending on the pressure conditions, and is 1.4 to 3.8 g / cm. 3 However, by mixing copper concentrate with Cu-based recycled materials in a weight ratio of 5:3 and forming them into agglomerates, the specific gravity can be reduced to 2.1 to 4.8 g / cm3. 3The mixed recycled raw materials are not only used to increase the specific gravity of the briquettes, but are also matted within the matte, making it an efficient method of increasing the amount of recycled raw materials processed in the flash smelting furnace. The briquetted raw materials may be fed into the furnace through a concentrate burner or from the ceiling of the settler 2, but it is preferable to feed them so that they land in the area directly below the reaction shaft 1 where the generated droplets fall in a shower. In addition, in order to increase the stability of the briquetted raw materials, binders may be added or the moisture content may be adjusted, and the particle size distribution and ratio of the S source and the recycled raw materials may be adjusted. As binders, fine powder raw materials processed in the flash smelting furnace or by-products such as powders and liquids generated in each process of the smelter may be used. In addition, in order to increase the stability of the briquetted raw materials, processes such as high-temperature treatment in an inert atmosphere and sintering may be included. EXAMPLES
[0025] Example 1 As shown in FIG. 5, matte 52 was filled in a quartz Tammann tube 51 in advance, and the quartz Tammann tube 51 was fixed to an alumina crucible. Next, the alumina crucible was set in an electric furnace, and the temperature of the molten metal was raised to 1250°C. Next, metallic Cu 53 was added to the molten matte 52 in an amount that exceeded the solubility on the phase diagram, and the mixture was held for 2 minutes. As the metallic Cu 53, spherical Cu with a diameter of 5 mm (100% purity) was used. At this time, the solution in the quartz Tammann tube 51 had a two-liquid phase coexistence composition of matte and Cu.
[0026] Next, in order to matte the Cu that coexists in the solution, a sulfur source with a specific surface area of 300 to 500 mm2 was used. 2 The FeS2 reagent 54, which had been pressurized to a concentration of about 1000 ppm by mass, was added to the quartz Tammann tube 51 together with argon gas and held for 10 minutes. The FeS2 concentration in the FeS2 reagent 54 used was 87.9 mass%. Next, in order to prevent Cu precipitation during the cooling process, the alumina crucible was removed from the electric furnace and immersed together with the quartz Tammann tube 51 in ice water for rapid cooling.
[0027] (Comparative Example) In the comparative example, no S source was added. The other conditions were the same as in Example 1.
[0028] (analysis) For Example 1 and Comparative Example, the presence or absence of a residual Cu phase (metallic Cu) in the samples after quenching was confirmed. The residual Cu phase was evaluated by CT scanning and microscopic observation of the sample cross section. The observation of the sample cross section was performed by polishing a cylindrical sample with a diameter of 17.0 mm in 0.5 mm increments and repeating the observation to confirm the presence or absence of a Cu phase. The evaluation accuracy was improved by using CT in combination.
[0029] The compositions of matte 52, metallic Cu 53, and FeS2 reagent 54 used in the test are shown in Table 1. Table 2 shows the matte grade (copper grade) of matte 52 packed in quartz Tammann tube 51, the amount of matte 52 packed in quartz Tammann tube 51, the amount of metallic Cu 53 added to quartz Tammann tube 51, the amount of FeS2 reagent 54 added to quartz Tammann tube 51, and the average composition of each component in the quenched sample. [Table 1] [Table 2]
[0030] FIG. 6(a) is a photograph showing the results of the comparative example. FIG. 6(b) is a photograph showing the results of the example 1. As shown in FIG. 6(a), a Cu phase was confirmed in the sample of the comparative example, but as shown in FIG. 6(b), a Cu phase was not confirmed in the sample of the example 1. In FIG. 6(a), the small circle below the black circle is the Cu phase. In FIG. 6(b), it can be seen that the Cu phase is matted. From this result, it was confirmed that even if metallic Cu exists in an amount exceeding the solubility on the phase diagram, it can be matted by adding a S source.
[0031] The solubility of metallic Cu in the matte phase was confirmed using the comparative sample, and it was confirmed that the measured solubility generally coincided with the phase diagram.
[0032] (Examples 2 and 3) Next, the contribution of the FeS2 reagent 54 was examined. Example 2 is an example in which the FeS2 reagent 54 was supplied in an amount greater than or equal to the amount of FeS2 reagent 54 that would matt the entire amount of metallic Cu, assuming that 70 mass% of S contributes to matting the metallic Cu when the total S contained in the FeS2 reagent 54 is 100 mass%. Example 3 is an example in which the FeS2 reagent 54 was supplied in an amount greater than or equal to the amount of FeS2 reagent 54 that would matt the entire amount of metallic Cu, assuming that 90 mass% of S contributes to matting the metallic Cu when the total S contained in the FeS2 reagent 54 is 100 mass%.
[0033] Table 3 shows the matte grade (copper grade) of the matte 52 filled in the quartz Tammann tube 51, the amount of the matte 52 filled in the quartz Tammann tube 51, the amount of metallic Cu 53 added to the quartz Tammann tube 51, the amount of FeS2 reagent 54 added to the quartz Tammann tube 51, and the average composition of each component in the quenched sample. [Table 3]
[0034] In Example 3, the amount of Cu phase was smaller than that in the comparative example. From this result, it was confirmed that, assuming that 90 mass% of S contributes to matting metallic Cu when the total S contained in the FeS2 reagent 54 is 100 mass%, the generation of metallic Cu is suppressed by adding FeS2 in an amount greater than or equal to the amount that matts the entire metallic Cu phase. In Example 2, no Cu phase was confirmed. From this result, it was confirmed that, assuming that 70 mass% of S contributes to matting metallic Cu when the total S contained in the FeS2 reagent 54 is 100 mass%, it is preferable to supply FeS2 reagent 54 in an amount greater than or equal to the amount that matts the entire metallic Cu.
[0035] The above-described embodiment is a preferred example of the present invention, but the present invention is not limited to this embodiment and can be modified in various ways without departing from the scope of the present invention. [Explanation of symbols]
[0036] 1 Reaction shaft 2 Setra 3. Uptake 4 Concentrate burner 5. Matt 6. Slug 10 Input section 11 1st aisle 12 2nd aisle 13 3rd aisle 14 4th aisle 16. Lance 40 Injection Nozzle 51 Quartz Tammann tube 52 Matt 53 Metallic Cu 54 FeS2 Reagent 100 Flash furnace
Claims
1. A method for operating copper smelting, comprising the steps of: adding a S source to matte produced by reacting a smelting raw material, which raw material contains copper concentrate and metallic Cu, with a reaction gas in a reaction shaft of a flash smelting furnace, when a metal phase of the metallic Cu is produced in the matte.
2. 2. The copper smelting method according to claim 1, wherein the S source is added to the matte when the metallic Cu is contained in the smelting raw material in an amount exceeding the solubility of the metallic Cu in the matte.
3. 2. The copper smelting operation method according to claim 1, further comprising the step of adding the S source to the matte when a metal phase of the metallic Cu is confirmed in the matte by sampling the matte.
4. 2. The method of claim 1, wherein the S source is added to the matte by mixing the S source with the smelting feedstock.
5. 2. The copper smelting operation method according to claim 1, wherein the S source is added to the matte by injecting the S source together with an inert gas from an injection nozzle toward the matte.
6. 2. The method of claim 1, further comprising adding said briquetted sulfur source to said matte.
7. 2. The method for operating a copper smelter according to claim 1, wherein the S source is mixed with other smelting raw materials to form briquettes, and the briquettes are added to the matte.
8. 8. The copper smelting operation method according to claim 7, characterized in that the specific gravity of the briquettes is adjusted when the S source is mixed with other smelting raw materials to form briquettes.
9. 2. The copper smelting method according to claim 1, wherein the S source is mixed with recycled materials or other smelting materials to form briquettes, thereby increasing the throughput of the recycled materials.
10. The specific surface area of the S source is 20 mm 2 2. The method for operating a copper smelter according to claim 1, wherein the copper content is 1 / g or more.
11. 2. The copper smelting method according to claim 1, wherein the S source is supplied to the matte in an amount equal to or greater than the total amount of the metallic Cu required to form the matte.
12. 2. The copper smelting operation method according to claim 1, characterized in that, assuming that total S contained in the S source is 100 mass%, and that 90 mass% of S contributes to matte formation of the metallic Cu, the S source is supplied to the matte in an amount equal to or greater than the amount by which the entire amount of the metallic Cu is matte-formed.
13. 2. The method of claim 1, wherein the S source comprises elemental sulfur or a sulfide.
14. 2. The copper smelting method according to claim 1, wherein the S source further contains Fe.
15. 15. The copper smelting method according to claim 14, wherein the Fe-containing S source is chalcopyrite, pyrite, or pyrrhotite.
Citation Information
Patent Citations
Treatment of slag concentrate of copper converter
JP1988042335A
Method for smelting copper
JP2009293054A
Noble metal recovery method
JP2020070475A
Integrated hydrometallurgical and pyrometallurgical method for processing ore
US20190218641A1
Concentrate burner of copper smelting furnace and copper smelting furnace operation method
WO2019038866A1