Method of producing molded body of tobermorite-containing calcium silicate, and molded body of tobermorite-containing calcium silicate
By using a slurry with specific aluminum and sulfur molar ratios to form ettringite, the method addresses the challenge of maintaining bending strength and reducing production costs in calcium silicate molded bodies, achieving efficient tobermorite crystal formation at lower temperatures and pressures.
Patent Information
- Application Number
- JP2023065489
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-10-25
AI Technical Summary
Existing methods for producing calcium silicate molded bodies with high industrial waste content face challenges in maintaining bending strength and require high heat treatment temperatures and pressures, leading to increased production costs.
A method involving an aqueous slurry of silicic, calcareous, and aluminum-containing compounds that form ettringite at room temperature, with specific molar ratios of aluminum and sulfur components, allowing for the production of tobermorite-containing calcium silicate molded bodies at reduced heating temperatures and pressures without extending heat treatment time.
The method enables the production of calcium silicate molded bodies with improved bending strength and reduced energy costs by generating tobermorite crystals at lower temperatures and pressures, utilizing industrial waste effectively.
Smart Images

Figure 2024151785000001 
Figure 2024151785000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a tobermorite-containing calcium silicate shaped body and a tobermorite-containing calcium silicate shaped body. [Background technology]
[0002] Tobermorite (5CaO·6SiO2·5H2O) is a type of calcium silicate hydrate that has excellent dimensional stability and heat resistance and is therefore widely used as a constituent material for calcium silicate molded bodies such as calcium silicate boards.
[0003] As disclosed in Patent Document 1 (JP Patent Publication 7-17708 A) and the like, tobermorite (5CaO 6SiO2 5H2O) is generally produced by hydrothermal synthesis by heating a mixture of a siliceous raw material with low melting property, such as quartz or silica stone, and a calcareous raw material, such as slaked lime, in an autoclave in the presence of water. In the initial stage of the reaction in the autoclave, silicate ions eluted from the siliceous raw material react with calcium ions eluted from the calcareous raw material to produce calcium silicate hydrate, an amorphous intermediate product, i.e., Ca-SiO2-H2O gel (hereinafter simply referred to as "CSH gel"). As the reaction proceeds further, the CSH gel crystallizes to produce tobermorite crystals.
[0004] On the other hand, in recent years, it has been proposed to use industrial waste such as paper sludge as the raw material for calcium silicate molded bodies in order to reduce costs. However, when the content of industrial waste is increased in the raw material mixture for calcium silicate molded bodies, particularly when unburned paper sludge is used as the industrial waste, there is a technical problem that the bending strength of the calcium silicate molded bodies after production decreases.
[0005] As a method for producing calcium silicate shaped bodies that solves the above-mentioned technical problems, the applicant has previously proposed a method for producing calcium silicate shaped bodies by dehydrating and molding a mixed slurry obtained by mixing raw materials for calcium silicate shaped bodies, which raw materials include a siliceous raw material, a calcareous raw material, papermaking sludge ash and reinforcing fibers, with water, and subjecting the obtained molded body to a hydrothermal reaction, in which the molar ratio of aluminum (Al) components to silicon (Si) components in the raw materials is Al / (Al+Si)=7-15%, the raw materials contain 6-14% by weight of the papermaking sludge ash, the raw materials further contain exhausted gypsum, and the total amount of the exhausted gypsum and the papermaking sludge ash is 50% by weight or more (see Patent Document 2). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 7-17708 [Patent Document 2] Patent No. 4646310 specification Summary of the Invention [Problem to be solved by the invention]
[0007] According to the manufacturing method described in Patent Document 2, even when the ratio of industrial waste in the raw materials is increased, it is possible to provide a calcium silicate molded body that maintains a high bending strength.
[0008] On the other hand, according to the investigations of the present inventors, in the manufacturing method described in Patent Document 2, water is added to the raw material mixture to form a mixed slurry, which is then dehydrated and molded to obtain a green sheet. The green sheet obtained is then loaded into an autoclave and heat-treated under processing conditions, for example, a temperature of 180°C and a pressure of 0.9 MPa to perform hydrothermal synthesis, thereby obtaining a calcium silicate molded body mainly via the intermediate calcium silicate hydrate (CSH gel). However, when firing the material in the autoclave, it is difficult to reduce the heating treatment time, or to reduce the temperature and pressure without increasing the heating treatment time, and it has been found that this method is likely to lead to increases in costs, such as production equipment costs and energy costs during production, in industrial production.
[0009] As a result of further investigation by the present inventors into this point, it was found that the solubility of siliceous raw materials such as silica stone is lower than that of calcareous raw materials such as slaked lime, and that calcium silicate hydrate (CSH gel) is generated in the early stages of the reaction so as to surround the unreacted siliceous raw material particles, further reducing the solubility of the siliceous raw material. For this reason, it was found that in order to crystallize the raw material mixture into tobermorite, it is necessary to sufficiently raise the temperature inside the autoclave and increase the vapor pressure to improve the solubility of the siliceous raw material. If the temperature inside the autoclave is low, the dissolution of the silica stone does not proceed easily and the processing time required to obtain the desired physical properties increases. Therefore, in order to improve the industrial productivity of calcium silicate molded bodies, it is difficult to reduce the temperature and pressure during the heat treatment in the autoclave.
[0010] Therefore, an object of the present invention is to provide a method for producing a tobermorite-containing calcium silicate molded body while reducing the heating temperature and pressure without reducing the heat treatment time during hydrothermal synthesis or increasing the heat treatment time during hydrothermal synthesis, and to provide a tobermorite-containing calcium silicate molded body. [Means for solving the problem]
[0011] In order to achieve the above-mentioned object, the present inventors have conducted intensive research and have found that the above-mentioned technical problems can be solved by a method for producing a tobermorite-containing calcium silicate shaped body, which comprises dehydrating and molding an aqueous slurry of a mixed raw material containing a siliceous raw material, a calcareous raw material, gypsum, and an aluminum-containing compound that reacts with the gypsum at room temperature to form ettringite, and heat-treating the obtained molded body, wherein the content of the aluminum (Al) component relative to the total amount of the aluminum (Al) component and the silicon (Si) component in the aqueous slurry is more than 15 mol % and not more than 25 mol %, and the content ratio of the aluminum (Al) component to the sulfur (S) component in the aqueous slurry is 0.40 to 1.05 in terms of molar ratio, and the present invention has been completed based on this finding.
[0012] That is, the present invention provides (1) A method for producing a tobermorite-containing calcium silicate molded body, comprising the steps of: dehydrating and molding an aqueous slurry of a mixed raw material containing a siliceous raw material, a calcareous raw material, gypsum, and an aluminum-containing compound that reacts with the gypsum at room temperature to form ettringite; and heat-treating the resulting molded body, The content ratio of the aluminum (Al) component to the total amount of the aluminum (Al) component and the silicon (Si) component in the aqueous slurry is more than 15 mol% and 25 mol% or less; The content ratio of the aluminum (Al) component to the sulfur (S) component in the aqueous slurry is 0.40 to 1.05 in terms of molar ratio. A method for producing a tobermorite-containing calcium silicate shaped body, (2) The method for producing a tobermorite-containing calcium silicate molded product according to (1) above, wherein the gypsum is at least one selected from the group consisting of natural gypsum, desalted gypsum, neutralized gypsum, phosphate gypsum, sulphate gypsum and pulverized powder of waste gypsum board. (3) A method for producing a tobermorite-containing calcium silicate shaped body according to the above (1), wherein the aluminum-containing compound which reacts with gypsum at room temperature to produce ettringite is a compound containing one or more compounds selected from mayenite, tricalcium aluminate, tricalcium aluminate, tetracalcium aluminate ferroferrate, and tetracalcium aluminate ferroferrate. (4) The method for producing a tobermorite-containing calcium silicate molded product according to (1) above, wherein the aluminum-containing compound that reacts with gypsum at room temperature to produce ettringite is papermaking sludge ash. (5) The method for producing a tobermorite-containing calcium silicate shaped product according to the above (4), wherein the aqueous slurry contains 10 to 50 mass % of the papermaking sludge ash in terms of solid content, and the total amount of the papermaking sludge ash and the gypsum in the aqueous slurry is 50 mass % or more in terms of solid content. (6) The method for producing a tobermorite-containing calcium silicate shaped body according to the above (1), wherein the aqueous slurry further contains reinforcing fibers. (7) The method for producing a tobermorite-containing calcium silicate shaped body according to (1) above, wherein the heat treatment is carried out at a temperature of 120° C. or higher and lower than 200° C. (8) The resulting tobermorite-containing calcium silicate molded body has a bulk density of 0.40 g / cm 3 ~1.20g / cm 3 , bending strength 5.00N / mm 2 The method for producing a tobermorite-containing calcium silicate molded product according to the above (1), which has a water absorption dimensional change rate of 0.15% or less and a 1000°C heating shrinkage rate of 7.0% or less; (9) A tobermorite-containing calcium silicate shaped body comprising a heat-treated aqueous slurry containing a siliceous raw material, a calcareous raw material, gypsum, and an aluminum-containing compound that reacts with the gypsum at room temperature to form ettringite, The content ratio of the aluminum (Al) component to the total amount of the aluminum (Al) component and the silicon (Si) component in the aqueous slurry is more than 15 mol% and 25 mol% or less; The content ratio of the aluminum (Al) component to the sulfur (S) component in the aqueous slurry is 0.40 to 1.05 in terms of molar ratio. A tobermorite-containing calcium silicate shaped body, This provides: Effect of the Invention
[0013] The present invention differs from the method for producing calcium silicate molded bodies described in Patent Document 2 in that the content (mol%) of aluminum (Al) relative to the total amount of aluminum (Al) and silicon (Si) in the raw material is high, and aluminum (Al) is contained at a constant ratio relative to sulfur (S) in the raw material. Therefore, it is considered that hydroxylerestadite (3.5CaO·1.5SiO2·1.5CaSO4·0.5H2O) is further generated in the aqueous slurry using ettringite (3CaO·Al2O3·3CaSO4·32H2O) as a precursor instead of calcium silicate hydrate (CSH gel), and that the decrease in the solubility of the siliceous raw material caused by the formation of calcium silicate hydrate around the particles of the siliceous raw material such as silica stone can be suppressed. Furthermore, compared to producing tobermorite crystals via calcium silicate hydrate (CSH gel) as in the manufacturing method described in Patent Document 2, producing tobermorite crystals via hydroxylerestadite, which uses ettringite (3CaO·Al2O3·3CaSO4·32H2O) as a precursor, makes it possible to produce tobermorite crystals while reducing the heat treatment time during hydrothermal synthesis, or to produce tobermorite crystals at low temperature and low pressure without increasing the heat treatment time during hydrothermal synthesis. Therefore, according to the present invention, it is possible to provide a method for producing a tobermorite-containing calcium silicate molded body while reducing the heating temperature and pressure without reducing the heating treatment time during hydrothermal synthesis or increasing the heating treatment time during hydrothermal synthesis, and a tobermorite-containing calcium silicate molded body. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] First, a method for producing a tobermorite-containing calcium silicate molded body according to the present invention will be described. The method for producing a tobermorite-containing calcium silicate molded body according to the present invention comprises the steps of: A method for producing a tobermorite-containing calcium silicate molded body, comprising the steps of dehydrating and molding an aqueous slurry of a mixed raw material containing a siliceous raw material, a calcareous raw material, gypsum, and an aluminum-containing compound which reacts with the gypsum at room temperature to form ettringite, and heat-treating the molded product obtained, The content ratio of the aluminum (Al) component to the total amount of the aluminum (Al) component and the silicon (Si) component in the aqueous slurry is more than 15 mol% and 25 mol% or less; The content ratio of the aluminum (Al) component to the sulfur (S) component in the aqueous slurry is 0.40 to 1.05 in terms of molar ratio. It is characterized by the above.
[0015] In the method for producing a tobermorite-containing calcium silicate molded body according to the present invention, an aqueous slurry of a mixed raw material containing a siliceous raw material, a calcareous raw material, gypsum, and an aluminum-containing compound that reacts with the gypsum at room temperature to form ettringite is dehydrated and molded, and the obtained molded body is heat-treated.
[0016] In the method for producing a tobermorite-containing calcium silicate shaped body according to the present invention, the siliceous raw material may be at least one selected from the group consisting of silica stone, diatomaceous earth, microsilica, silica fume, silica flower, and the like.
[0017] In the method for producing a tobermorite-containing calcium silicate molded body according to the present invention, the aqueous slurry preferably contains, in terms of solid content, 10 to 60 mass % of siliceous raw material, more preferably 12 to 55 mass %, even more preferably 15 to 50 mass %, even more preferably 25 to 50 mass %, and even more preferably 38 to 40 mass %.
[0018] In the method for producing a tobermorite-containing calcium silicate shaped body according to the present invention, by containing the siliceous raw material in the aqueous slurry in the above-mentioned ratio calculated as solid content, the proportion of the siliceous raw material used can be relatively reduced, and the proportion of an aluminum-containing compound, which will be described later, that reacts with gypsum at room temperature to produce ettringite can be increased, making it possible to easily control the content ratio of the aluminum (Al) component relative to the total amount of the aluminum (Al) component and the silicon (Si) component in the mixed raw material within a desired range.
[0019] In the method for producing a tobermorite-containing calcium silicate shaped body according to the present invention, the calcareous raw material may be one or more selected from cement, slaked lime, quicklime, and the like.
[0020] In the method for producing a tobermorite-containing calcium silicate molded body according to the present invention, the aqueous slurry preferably contains, in terms of solid content, 3 to 50 mass % of calcareous raw material, more preferably 4 to 50 mass %, even more preferably 10 to 50 mass %, even more preferably 15 to 45 mass %, and even more preferably 31 to 39 mass %.
[0021] In the method for producing tobermorite-containing calcium silicate molded bodies according to the present invention, by containing the calcareous raw material in the aqueous slurry in the above-mentioned ratio calculated as solid content, the proportion of the siliceous raw material used can be relatively reduced, and the content ratios of aluminum (Al) and silicon (Si) components in the mixed raw material described below can be easily controlled within the desired range.
[0022] In the method for producing a tobermorite-containing calcium silicate molded body according to the present invention, the gypsum can be at least one selected from natural gypsum, desalted gypsum, neutralized gypsum, phosphate gypsum, sulphate gypsum and pulverized powder of waste gypsum board.
[0023] In the method for producing a tobermorite-containing calcium silicate molded body according to the present invention, the removed gypsum, neutralized gypsum, phosphogypsum and sulphate gypsum are called chemical gypsum and are produced as by-products in various chemical industries.
[0024] Of the above-mentioned gypsum, for example, flue gas desulfurization gypsum is also called flue gas desulfurization gypsum, and refers to CaSO4·2H2O (gypsum dihydrate) that is made by recovering SO2 gas in a flue gas desulfurization device and converting it into gypsum. In the method for producing a tobermorite-containing calcium silicate shaped body according to the present invention, when waste gypsum, which is an industrial waste, is used as the gypsum, the production cost can be easily reduced.
[0025] Among the above-mentioned gypsum, for example, neutralized gypsum means calcium carbonate neutralized with sulfuric acid such as waste sulfuric acid generated during copper refining. In the method for producing a tobermorite-containing calcium silicate molded body according to the present invention, even when neutralized gypsum is used as the gypsum, waste sulfuric acid, which is an industrial waste, can be utilized, so that the production cost can be easily reduced while effectively utilizing the industrial waste.
[0026] In the method for producing a tobermorite-containing calcium silicate molded body according to the present invention, the aqueous slurry preferably contains gypsum in an amount, calculated as solid content, of more than 0 mass % and not more than 50 mass %, more preferably 5 to 40 mass %, and even more preferably 10 to 25 mass %.
[0027] In the method for producing a tobermorite-containing calcium silicate molded body according to the present invention, by containing gypsum in the aqueous slurry in the above-mentioned ratio calculated as solid content, the content ratio of aluminum (Al) component to sulfur (S) component in the aqueous slurry can be easily controlled to a desired ratio.
[0028] In the method for producing a tobermorite-containing calcium silicate shaped body according to the present invention, examples of the aluminum-containing compound that reacts with gypsum at room temperature to produce ettringite include compounds containing one or more compounds selected from mayenite (C12A7; 12CaO 7Al2O3), tricalcium aluminate, tricalcium aluminate (C3A; 3CaO Al2O3), tetracalcium aluminate and tetracalcium aluminate (C4AF; 4CaO Al2O3 Fe2O3), and compounds containing one or more compounds selected from mayenite, tricalcium aluminate, tricalcium aluminate, and tetracalcium aluminate are preferred. In the method for producing a tobermorite-containing calcium silicate molded body according to the present invention, a specific example of the aluminum-containing compound that reacts with gypsum at room temperature to form ettringite is paper sludge ash.
[0029] In the method for producing a tobermorite-containing calcium silicate molded body according to the present invention, papermaking sludge ash means papermaking sludge, i.e., non-reusable pulp fibers generated in papermaking processes such as the pulp production process, paper production process, and waste paper processing process, short fibers unsuitable for use in paper after the raw pulp fibers are extracted from waste paper, and factory wastewater containing clay (mainly kaolin) or calcium carbonate, which is coagulated and precipitated using a coagulant such as polyaluminum chloride, and then incinerated to obtain incinerated ash (papermaking sludge incineration ash). In the method for producing a tobermorite-containing calcium silicate molded body according to the present invention, the production cost can be easily reduced by using paper sludge ash, which is an industrial waste, as an aluminum-containing compound that reacts with gypsum at room temperature to produce ettringite.
[0030] Paper sludge ash contains Al2O3, SiO2 and CaO as its main components. The papermaking sludge ash preferably contains 5 to 30 mass % of Al2O3, more preferably 10 to 25 mass %, and even more preferably 12 to 18 mass %. The papermaking sludge ash preferably contains 5 to 40 mass % of SiO2, more preferably 5 to 30 mass %, and even more preferably 10 to 20 mass %. The papermaking sludge ash preferably contains 30 to 70 mass % of CaO, more preferably 40 to 70 mass %, and even more preferably 50 to 70 mass %.
[0031] Because the papermaking sludge ash contains Al2O3, SiO2, and CaO in the above-mentioned proportions, the amounts of siliceous and calcareous raw materials that have traditionally been used as raw materials for tobermorite can be reduced, and the proportion of industrial waste in the mixed raw material can be increased and effectively utilized, while the content (mol %) of the aluminum (Al) component relative to the total amount of the aluminum (Al) component and the silicon (Si) component in the mixed raw material and the content (mol ratio) of the aluminum (Al) component relative to the sulfur (S) component in the mixed raw material can be easily controlled within desired ranges.
[0032] In addition, in the present application, the content ratios of Al2O3, SiO2 and CaO in the papermaking sludge ash refer to values measured using a wavelength dispersive fluorescent X-ray spectrometer ZSX Primus II manufactured by Rigaku Corporation.
[0033] In the method for producing a tobermorite-containing calcium silicate molded body according to the present invention, the aqueous slurry contains, in terms of solid content, preferably 10 to 50 mass %, more preferably 12 to 45 mass %, even more preferably 15 to 45 mass %, still more preferably 15 to 40 mass %, even more preferably 15 to 30 mass %, and particularly preferably 18 to 30 mass % of an aluminum-containing compound that reacts with gypsum at room temperature to produce ettringite.
[0034] In the method for producing a tobermorite-containing calcium silicate molded body according to the present invention, the aqueous slurry contains, in the above-mentioned ratio, an aluminum-containing compound that reacts with gypsum at room temperature, calculated as a solid content, to produce ettringite. This makes it possible to easily control, within desired ranges, the content ratio of the aluminum (Al) component relative to the total amount of the aluminum (Al) component and the silicon (Si) component in the mixed raw material, and the content ratio (molar ratio) of the aluminum (Al) component relative to the sulfur (S) component.
[0035] In the method for producing a tobermorite-containing calcium silicate molded body according to the present invention, the aqueous slurry preferably contains, in terms of solid content, gypsum and an aluminum-containing compound that reacts with gypsum at room temperature to produce ettringite in total at 50 mass% or more, more preferably 50 to 60 mass%, and even more preferably 50 to 55 mass%.
[0036] In the method for producing tobermorite-containing calcium silicate shaped bodies according to the present invention, the aqueous slurry contains the above-mentioned total amount, calculated as solid content, of gypsum and an aluminum-containing compound that reacts with gypsum at room temperature to produce ettringite. This makes it possible to easily produce calcium silicate shaped bodies containing tobermorite crystals at low temperatures and under low pressures, as compared with the case where a siliceous raw material or a calcareous raw material is used as the main raw material.
[0037] In the method for producing a tobermorite-containing calcium silicate molded body according to the present invention, the aqueous slurry preferably contains, in terms of solid content, 79 to 89 mass% in total of the siliceous raw material, the calcareous raw material, gypsum, and the aluminum-containing compound that reacts with the gypsum at room temperature to produce ettringite, more preferably 81 to 88 mass%, and even more preferably 83 to 87 mass%.
[0038] In the method for producing tobermorite-containing calcium silicate molded bodies according to the present invention, by containing in the aqueous slurry the above-mentioned total amounts, calculated on solid content basis, of the siliceous raw material, the calcareous raw material, gypsum, and the aluminum-containing compound that reacts with the gypsum at room temperature to produce ettringite, it is possible to reduce the heat treatment time during hydrothermal synthesis, or to easily produce tobermorite-containing calcium silicate molded bodies while reducing the heating temperature and pressure without increasing the heat treatment time during hydrothermal synthesis.
[0039] In the method for producing a tobermorite-containing calcium silicate molded body according to the present invention, the content ratio of the aluminum (Al) component to the total amount of the aluminum (Al) component and the silicon (Si) component in the aqueous slurry, i.e., {Aluminum (Al) component content (molar amount) in the aqueous slurry / (Total aluminum (Al) component and silicon (Si) component content (molar amount) in the aqueous slurry)}×100 The content (mol %) represented by the above formula is more than 15 mol % and 25 mol % or less, preferably 16 to 23 mol %, and more preferably 17 to 21 mol %.
[0040] In the method for producing a tobermorite-containing calcium silicate shaped body according to the present invention, the content ratio of aluminum (Al) component to sulfur (S) component in the aqueous slurry, i.e., (Aluminum (Al) component content (molar amount) in the aqueous slurry / (Sulfur (S) component content (molar amount) in the aqueous slurry) The ratio (molar ratio) represented by the above formula is from 0.40 to 1.05, preferably from 0.41 to 1.04, more preferably from 0.42 to 1.02, even more preferably from 0.44 to 1.02, and still more preferably from 0.46 to 1.02.
[0041] In the method for producing a tobermorite-containing calcium silicate molded body according to the present invention, the contents of the aluminum (Al) component, silicon (Si) component and sulfur (S) component used in determining the content ratio of the aluminum (Al) component to the total amount of the aluminum (Al) component and silicon (Si) component in the aqueous slurry and the content ratio of the aluminum (Al) component to the sulfur (S) component in the aqueous slurry refer to the contents of the aluminum (Al) component, silicon (Si) component and sulfur (S) component which are the sources of tobermorite production. That is, in the method for producing a tobermorite-containing calcium silicate molded body according to the present invention, it means the total content of each of the aluminum (Al) component, silicon (Si) component and sulfur (S) component which constitute the raw materials such as the siliceous raw material, the calcareous raw material, gypsum and the aluminum-containing compound which reacts with the gypsum at room temperature to produce ettringite, which are the sources of tobermorite production.
[0042] In this application, the molar amounts of aluminum (Al) components, silicon (Si) components, and sulfur (S) components in the aqueous slurry refer to the amounts (mass%) of each component measured using a wavelength dispersive fluorescent X-ray analyzer ZSX Primus II manufactured by Rigaku Corporation, divided by the molecular weight of each component. Specifically, the molar amounts of the aluminum (Al) component, silicon (Si) component, and sulfur (S) component in the aqueous slurry are calculated by the following method. (1) The amounts (mass%) of aluminum (Al), silicon (Si), and sulfur (S) components constituting the tobermorite-forming raw materials, such as siliceous raw materials, calcareous raw materials, gypsum, and aluminum-containing compounds that react with the gypsum at room temperature to form ettringite, are determined using a wavelength-dispersive X-ray fluorescence spectrometer ZSX Primus II manufactured by Rigaku Corporation. (2) The total content (mass%) of the aluminum (Al) component, silicon (Si) component, and sulfur (S) component in the aqueous slurry, calculated as solid content, is calculated from the amounts (mass%) of the aluminum (Al) component, silicon (Si) component, and sulfur (S) component constituting the tobermorite-forming components, such as the siliceous raw material, calcareous raw material, gypsum, and aluminum-containing compounds that react with the gypsum at room temperature to form ettringite, which are added to the aqueous slurry, and the blending ratio (solid content ratio) of each reactive component, such as the siliceous raw material, calcareous raw material, gypsum, and aluminum-containing compounds that react with the gypsum at room temperature to form ettringite. (3) The total content (% by mass) of the aluminum (Al) component, silicon (Si) component, and sulfur (S) component in the aqueous slurry is divided by the molecular weight of the aluminum (Al) component, silicon (Si) component, and sulfur (S) component, respectively, to convert the total amount of each component from mass% to mole%. (4) The total contents (mol %) of the aluminum (Al) component, silicon (Si) component and sulfur (S) component are defined as the molar amounts of each.
[0043] In the method for producing a tobermorite-containing calcium silicate shaped body according to the present invention, the content ratio of the aluminum (Al) component to the total amount of the aluminum (Al) component and the silicon (Si) component in the aqueous slurry and the content ratio of the aluminum (Al) component to the sulfur (S) component in the aqueous slurry are within the above-mentioned ranges, so that hydroxylerestadite (3.5CaO·1.5SiO2·1.5CaSO4·0.5H2O) is further produced in the aqueous slurry using ettringite (3CaO·Al2O3·3CaSO4·32H2O) as a precursor instead of calcium silicate hydrate (CSH gel), and it is possible to suppress a decrease in the solubility of the siliceous raw material due to the production of calcium silicate hydrate around the particles of the siliceous raw material such as silica stone. In addition, compared to generating tobermorite crystals via calcium silicate hydrate (CSH gel), generating tobermorite crystals via hydroxylerestadite, which uses ettringite (3CaO·Al2O3·3CaSO4·32H2O) as a precursor, enables the generation of tobermorite crystals at low temperatures and under low pressures.
[0044] In the method for producing a tobermorite-containing calcium silicate shaped body according to the present invention, the reinforcing fibers can be one or more selected from inorganic fibers such as wollastonite, carbon fibers, and glass fibers, and organic fibers such as pulp. In addition, in the manufacturing method of the tobermorite-containing calcium silicate molded body of the present invention, inorganic fibers such as the above-mentioned wollastonite generally do not change when heated to below 1000°C, so they are treated as reinforcing fibers rather than as tobermorite-forming components.
[0045] The method for producing a tobermorite-containing calcium silicate shaped article according to the present invention uses reinforcing fibers as a raw material, and therefore the tobermorite-containing calcium silicate shaped article obtained can be easily given a desired strength.
[0046] In the method for producing a tobermorite-containing calcium silicate molded body according to the present invention, the aqueous slurry preferably contains 6 to 16 mass % of reinforcing fibers, calculated as solid content, more preferably 8 to 14 mass %, and even more preferably 10 to 12 mass %.
[0047] In the method for producing a tobermorite-containing calcium silicate molded body according to the present invention, the aqueous slurry contains reinforcing fibers in the above-mentioned ratio calculated on solid content basis, so that the obtained tobermorite-containing calcium silicate molded body can be easily imparted with the desired strength.
[0048] In the method for producing a tobermorite-containing calcium silicate molded body according to the present invention, the aqueous slurry preferably contains, in terms of solid content, 85 to 100 mass% in total of the siliceous raw material, the calcareous raw material, gypsum, the aluminum-containing compound that reacts with the gypsum at room temperature to form ettringite, and the reinforcing fibers, more preferably 86 to 96 mass% or more, even more preferably 88 to 95 mass%, and even more preferably 90 to 94 mass%.
[0049] In the method for producing tobermorite-containing calcium silicate shaped bodies according to the present invention, by containing in the aqueous slurry the above-mentioned total amounts, calculated on solid content basis, of the siliceous raw material, the calcareous raw material, the gypsum, the aluminum-containing compound that reacts with the gypsum at room temperature to produce ettringite, and the reinforcing fibers, the heat treatment time during hydrothermal synthesis can be reduced, or the tobermorite-containing calcium silicate shaped bodies can be produced more easily while reducing the heating temperature and pressure without increasing the heat treatment time during hydrothermal synthesis.
[0050] In the method for producing a tobermorite-containing calcium silicate shaped body according to the present invention, the aqueous medium constituting the aqueous slurry may be water or a mixture of water and a water-miscible solvent. Specific examples of the water-miscible solvent include one or more selected from lower alcohols such as ethanol and propanol, polyhydric alcohols such as glycerin, (poly)alkylene glycols such as (poly)ethylene glycol and (poly)propylene glycol, and alkyl ethers thereof.
[0051] In the method for producing a tobermorite-containing calcium silicate shaped body according to the present invention, the solid content concentration in the aqueous slurry is preferably 5 to 30 mass %, more preferably 5 to 20 mass %, and even more preferably 5 to 10 mass %.
[0052] In the method for producing a tobermorite-containing calcium silicate molded body according to the present invention, an aqueous slurry of a mixed raw material containing a siliceous raw material, a calcareous raw material, gypsum, and an aluminum-containing compound that reacts with the gypsum at room temperature to produce an entrigaite is dehydrated and molded, and the resulting molded body is heat-treated.
[0053] Examples of the method for dehydrating and molding the aqueous slurry include a suction dehydration molding method, a pressure dehydration molding method, and a papermaking method.
[0054] The compact (wet compact) obtained by dehydrating and molding the aqueous slurry has a bulk density of 1.2 to 1.7 g / cm. 3 Preferably, the density is 1.3 to 1.6 g / cm 3 More preferably, it is 1.4 to 1.5 g / cm 3 It is even more preferred that:
[0055] In the method for producing a tobermorite-containing calcium silicate molded body according to the present invention, the molded body (wet molded body) obtained by dehydrating and molding the above-mentioned aqueous slurry is heat-treated, whereby hydrothermal synthesis proceeds and crystals containing tobermorite can be easily formed.
[0056] In the method for producing a tobermorite-containing calcium silicate molded body according to the present invention, the heat treatment of the molded body (wet molded body) obtained by dehydrating and molding the hydrothermal slurry is preferably carried out in an autoclave.
[0057] In the tobermorite-containing calcium silicate molded body according to the present invention, the treatment temperature during the heat treatment of the molded body (wet molded body) obtained by dehydrating and molding the aqueous slurry is preferably 120°C or higher and lower than 200°C, more preferably 130 to 180°C, and even more preferably 140 to 160°C.
[0058] In the method for producing a tobermorite-containing calcium silicate molded body according to the present invention, the treatment pressure during the heat treatment of the molded body (wet molded body) obtained by dehydrating and molding the aqueous slurry is preferably 1.4 MPa or less, more preferably 0.1 to 0.9 MPa, and even more preferably 0.2 to 0.5 MPa.
[0059] In the tobermorite-containing calcium silicate molded body according to the present invention, the treatment time for the heat treatment of the molded body (wet molded body) obtained by dehydrating and molding the aqueous slurry is preferably 2 to 16 hours, more preferably 4 to 14 hours, and even more preferably 6 to 12 hours.
[0060] According to the method for producing a tobermorite-containing calcium silicate molded body of the present invention, the molded body is produced by heat-treating a dehydrated molded product of an aqueous slurry containing specific raw materials in specific ratios. This makes it possible to reduce the heat treatment time during hydrothermal synthesis, or to obtain the desired tobermorite-containing calcium silicate molded body while reducing the heating temperature and pressure without increasing the heat treatment time during hydrothermal synthesis.
[0061] The tobermorite-containing calcium silicate molded body obtained by the manufacturing method according to the present invention has a bulk density of 0.40 g / cm 3 ~1.20g / cm 3 Preferably, the density is 0.6 to 1.0 g / cm 3 More preferably, it is 0.7 to 0.9 g / cm 3 It is even more preferred that:
[0062] In the present application, the bulk density refers to a value measured according to JIS A5430 (calcium silicate board type 2) 6.3.
[0063] The tobermorite-containing calcium silicate molded body obtained by the manufacturing method according to the present invention has a bending strength (bending strength in the fiber orientation direction) of 5.00 N / mm 2 More preferably, it is 6.00 to 7.50 N / mm 2 More preferably, it is 6.50 to 8.00 N / mm 2 It is even more preferred that:
[0064] In the present application, the bending strength refers to a value measured according to JIS A5430 (calcium silicate board type 2) 6.4.
[0065] The tobermorite-containing calcium silicate shaped body obtained by the production method according to the present invention preferably has a water absorption dimensional change rate of 0.15% or less, more preferably 0.14 to 0.15%, and even more preferably 0.11 to 0.13%.
[0066] In the present application, the water absorption dimensional change rate refers to a value measured according to JIS A5430 (calcium silicate board type 2) 6.7.
[0067] The tobermorite-containing calcium silicate molded body obtained by the manufacturing method of the present invention preferably has a heat shrinkage rate of 7.0% or less (0.0 to 7.0%) at 1000°C, more preferably 5.0% or less (0.0 to 5.0%), and even more preferably 3.0% or less (0.0 to 3.0%).
[0068] In the present application, the 1000°C heat shrinkage rate is calculated by cutting the obtained molded body into a cube of 5 cm square, measuring the length of each side of the obtained sample, placing the sample in a firing furnace with an atmospheric temperature of 200°C or less, heating it to 1000°C at a heating rate of 400°C per hour and holding it at that temperature for 3 hours, then lowering the temperature to 200°C at a heating rate of 180°C per hour, and then measuring the length of each side of the test piece taken out of the firing furnace, and calculating the shrinkage rate of each side according to the following formula: {(side length before firing (cm) - side length after firing (cm)) / side length before firing (cm)} x 100 It means the arithmetic mean value calculated by the above.
[0069] The method for producing a tobermorite-containing calcium silicate molded body according to the present invention differs from conventional production methods in that the content (mol %) of the aluminum (Al) component relative to the total amount of the aluminum (Al) component and the silicon (Si) component in the mixed raw material is high, and the content (mol ratio) of the aluminum (Al) component relative to the sulfur (S) component falls within a specific range. For this reason, it is believed that by generating hydroxylesterodite (3.5CaO·1.5SiO2·1.5CaSO4·0.5H2O) as an intermediate using ettringite (3CaO·Al2O3·3CaSO4·32H2O) as a precursor rather than calcium silicate hydrate (CSH gel), it is possible to reduce the inhibition of dissolution of siliceous raw materials caused by the formation of calcium silicate hydrate (CSH gel) around siliceous raw material particles such as silica stone. Furthermore, compared to using calcium silicate hydrate (CSH gel) as an intermediate, by performing a hydrothermal synthesis reaction using hydroxylerestadite, which has ettringite as a precursor, as an intermediate, it is possible to reduce the heat treatment time during hydrothermal synthesis, or to produce tobermorite crystals while reducing the heating temperature and pressure without increasing the heat treatment time during hydrothermal synthesis.
[0070] Therefore, according to the present invention, a method can be provided for simply producing a tobermorite-containing calcium silicate molded body (a molded body containing tobermorite-type calcium silicate) while reducing the heating temperature and pressure without reducing the heating treatment time during hydrothermal synthesis or increasing the heating treatment time during hydrothermal synthesis.
[0071] In the present invention, whether or not the calcium silicate shaped body contains tobermorite crystals is confirmed by the following method. <How to confirm tobermorite crystals> When analyzed using an X-ray powder diffractometer (NEW8ADVANCE manufactured by Bruker), if a peak is observed near 2θ=7.8, d value=11.8, which is the second peak of Tobermorite-1.1 nm in the International Center for Diffraction Data (ICD) database, it is determined that tobermorite crystals are contained, and if this peak is not observed, it is determined that tobermorite crystals are not contained.
[0072] The method for producing a tobermorite-containing calcium silicate shaped body according to the present invention makes it possible to effectively produce a tobermorite-containing calcium silicate shaped body according to the present invention, which will be described below.
[0073] Next, the tobermorite-containing calcium silicate shaped body according to the present invention will be described. The tobermorite-containing calcium silicate shaped body according to the present invention is a tobermorite-containing calcium silicate shaped body comprising a heat-treated aqueous slurry containing a siliceous raw material, a calcareous raw material, gypsum, and an aluminum-containing compound that reacts with the gypsum at room temperature to form ettringite, The content ratio of the aluminum (Al) component to the total amount of the aluminum (Al) component and the silicon (Si) component in the aqueous slurry is more than 15 mol% and 25 mol% or less; The content ratio of the aluminum (Al) component to the sulfur (S) component in the aqueous slurry is 0.40 to 1.05 in terms of molar ratio. It is characterized by the above.
[0074] In the tobermorite-containing calcium silicate shaped body of the present invention, details of the siliceous raw material, the calcareous raw material, the gypsum, and the aluminum-containing compound that reacts with the gypsum at room temperature to produce ettringite, details of the reinforcing fibers that are further used as desired, and details of the aqueous slurry containing these are as described in the explanation of the method for producing the tobermorite-containing calcium silicate shaped body of the present invention. Details of the method for obtaining a heat-treated product by heat-treating the aqueous slurry using the above-mentioned aqueous slurry are also as described in the explanation of the method for producing the tobermorite-containing calcium silicate shaped body of the present invention. Further, the detailed physical properties of the tobermorite-containing calcium silicate shaped body according to the present invention are similar to those of the tobermorite-containing calcium silicate shaped body obtained by the production method according to the present invention.
[0075] As described above, conventionally known calcium silicate molded bodies consist of tobermorite crystals obtained by the hydrothermal synthesis reaction of calcium silicate hydrate (Ca-SiO-H2O gel (CSH gel)), which is obtained by the reaction of silicate ions eluted from a siliceous raw material with calcium ions eluted from a calcareous raw material. In contrast, the tobermorite-containing calcium silicate molded body of the present invention is obtained by hydrothermal synthesis at relatively low temperature and pressure using hydroxylesterdaite (3.5CaO·1.5SiO2·1.5CaSO4·0.5H2O) as an intermediate, which is made from ettringite (3CaO·Al2O3·3CaSO4·32H2O) as a precursor, and contains anhydrous gypsum in addition to tobermorite. The tobermorite-containing calcium silicate shaped body according to the present invention contains tobermorite which is produced as an intermediate, katoite (3CaO·Al2O3·(3-x)SiO2·(4-x)H2O).
[0076] Therefore, according to the present invention, it is possible to provide a tobermorite-containing calcium silicate molded body that can be produced by reducing the heating treatment time during hydrothermal synthesis or by reducing the heating temperature and pressure without increasing the heating treatment time during hydrothermal synthesis.
[0077] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples in any way.
[0078] (Examples 1 to 3, Comparative Examples 1 to 5) (1) Raw materials The following raw materials were prepared as raw materials for the calcium silicate molded body. · Siliceous raw material: Silica (SiO2 content is 97% by mass) Calcareous raw material: Cement (SiO2 content 22% by mass, Al2O3 content 1% by mass) Gypsum: Desulfurized gypsum (SO4 content 57% by mass, CaO content 41% by mass) Aluminum-containing compound that reacts with gypsum at room temperature to form ettringite: Paper sludge ash (Al2O3 content 14 mass%, SiO2 content 12 mass%, CaO content 50 mass%, MgO content 2 mass%, TiO2 content 1 mass%) Reinforcing fiber 1: Wollastonite Reinforcing fiber 2: Pulp
[0079] (2) Preparation of water slurry The above raw materials were mixed in the ratios shown in Table 1, and water was added to prepare aqueous slurries with solid concentrations of 10% by mass. The content ratio of the aluminum (Al) component to the total amount of the aluminum (Al) component and the silicon (Si) component in the water slurry, that is, the ... silicon (Si) component in the water slurry, {Al / (Al+Si)}×100 (where Al is the amount (molar amount) of aluminum contained in the water slurry, and Si is the amount (molar amount) of silicon contained in the water slurry) The content ratio of aluminum (Al) component to the total amount of aluminum (Al) component and silicon (Si) component contained in each water slurry (Al / (Al+Si) (mol %)) is also shown in Table 1. In addition, the content ratio of aluminum (Al) component to sulfur (S) component in the water slurry, that is, the content ratio of aluminum (Al) component to sulfur (S) component in the water slurry is expressed by the following formula: Al / S (where S is the molar amount of sulfur contained in the water slurry, and Al is the molar amount of aluminum contained in the water slurry) The content ratio of sulfur (S) to aluminum (Al) contained in each water slurry (Al / S (molar ratio)) is calculated based on the above formula.
[0080] [Table 1]
[0081] (3) Dehydration and heat treatment The water slurries obtained in (2) were each dehydrated and molded to obtain wet-formed bodies (green sheets) having a thickness of 10 mm. The obtained wet molded bodies (green sheets) were each placed in an autoclave and heat-treated under the heating conditions shown in Table 2 to carry out hydrothermal synthesis, thereby obtaining each calcium silicate molded board. However, in Comparative Examples 4 and 5, the hydrothermal synthesis did not proceed, and a calcium silicate molded board could not be obtained. The presence or absence of tobermorite crystal formation was confirmed for each of the obtained calcium silicate molded bodies, and various physical properties (bulk density (g / cm 3 ), bending strength (N / mm 2 The results are shown in Table 2. In the present examples and comparative examples, the density means a value measured according to JIS A5430 (calcium silicate board type 2) 6.3, the bending strength means a value measured according to JIS A5430 (calcium silicate board type 2) 6.4, and the dimensional change rate due to water absorption means a value measured according to JIS A5430 (calcium silicate board type 2) 6.7.
[0082] [Table 2]
[0083] As can be seen from Tables 1 and 2, in Examples 1 to 3, the hydrothermal synthesis reaction is carried out using an aqueous slurry of a mixed raw material containing a siliceous raw material, a calcareous raw material, gypsum, and an aluminum-containing compound that reacts with the gypsum at room temperature to produce ettringite in a manner that satisfies predetermined regulations. As a result, it is possible to produce a tobermorite-containing calcium silicate molded board having excellent physical properties such as bending strength and water absorption dimensional change rate at low temperature and low pressure (Example 1 and Example 2) without increasing the heat treatment time during hydrothermal synthesis compared to Comparative Example 2, by reducing the heat treatment time during hydrothermal synthesis (Example 3) compared to Comparative Example 2.
[0084] On the other hand, from Tables 1 and 2, in Comparative Examples 1 to 4, the content of the aluminum (Al) component relative to the total amount of the aluminum (Al) component and the silicon (Si) component in the aqueous slurry is greater than 15 mol % and outside the range of 25 mol %, and in Comparative Examples 1 to 3 and 5, the content ratio of the sulfur (S) component relative to the aluminum (Al) component in the aqueous slurry is outside the range of 0.40 to 1.05 in terms of molar ratio. For this reason, it is understood that the obtained calcium silicate molded bodies do not contain tobermorite and have inferior bending strength (Comparative Example 1, Comparative Example 3), require treatment at a higher temperature (150°C to 180°C) and a higher pressure (0.4 MPa to 0.9 MPa) than in Examples 1 and 2, and require a longer heat treatment time (2 hours to 8 hours) than in Example 3 (Comparative Example 2).It is also understood that no calcium silicate molded bodies are obtained (Comparative Examples 4 and 5). [Industrial Applicability]
[0085] According to the present invention, it is possible to provide a method for producing a tobermorite-containing calcium silicate molded body while reducing the heating temperature and pressure without reducing the heat treatment time during hydrothermal synthesis or increasing the heat treatment time during hydrothermal synthesis, and a tobermorite-containing calcium silicate molded body.
Claims
1. A method for producing a tobermorite-containing calcium silicate molded body, comprising the steps of dehydrating and molding an aqueous slurry of a mixed raw material containing a siliceous raw material, a calcareous raw material, gypsum, and an aluminum-containing compound which reacts with the gypsum at room temperature to form ettringite, and heat-treating the molded product obtained, The content ratio of the aluminum (Al) component to the total amount of the aluminum (Al) component and the silicon (Si) component in the aqueous slurry is more than 15 mol % and is 25 mol % or less; The content ratio of aluminum (Al) component to sulfur (S) component in the aqueous slurry is 0.40 to 1.05 in terms of molar ratio.
2. The method for producing a tobermorite-containing calcium silicate molded body comprising the steps of:
2. 2. The method for producing a tobermorite-containing calcium silicate molded product according to claim 1, wherein the gypsum is at least one selected from the group consisting of natural gypsum, desalted gypsum, neutralized gypsum, phosphate gypsum, sulphate gypsum and pulverized powder of waste gypsum board.
3. 2. The method for producing a tobermorite-containing calcium silicate molded body according to claim 1, wherein the aluminum-containing compound that reacts with gypsum at room temperature to produce ettringite is a compound containing one or more compounds selected from mayenite, tricalcium aluminate, tricalcium aluminate, tetracalcium aluminate ferroferrate, and tetracalcium aluminate ferroferrate.
4. 2. The method for producing a tobermorite-containing calcium silicate molded product according to claim 1, wherein the aluminum-containing compound which reacts with gypsum at room temperature to produce ettringite is paper sludge ash.
5. 5. The method for producing a tobermorite-containing calcium silicate molded body according to claim 4, wherein the aqueous slurry contains 10 to 50 mass% of the papermaking sludge ash in terms of solid content, and the total amount of the papermaking sludge ash and the gypsum in the aqueous slurry is 50 mass% or more in terms of solid content.
6. The method for producing a tobermorite-containing calcium silicate shaped body according to claim 1, wherein the aqueous slurry further contains reinforcing fibers.
7. The method for producing a tobermorite-containing calcium silicate molded body according to claim 1, wherein the heat treatment is carried out at a temperature of 120°C or higher and lower than 200°C.
8. The resulting tobermorite-containing calcium silicate molded body has a bulk density of 0.40 g / cm 3 ~1.20g / cm 3 , bending strength 5.00N / mm 2 2. The method for producing a tobermorite-containing calcium silicate molded article according to claim 1, wherein the water absorption dimensional change rate is 0.15% or less and the heat shrinkage rate at 1000° C. is 7.0% or less.
9. A tobermorite-containing calcium silicate shaped body comprising a heat-treated aqueous slurry containing a siliceous raw material, a calcareous raw material, gypsum, and an aluminum-containing compound that reacts with the gypsum at room temperature to form ettringite, The content ratio of the aluminum (Al) component to the total amount of the aluminum (Al) component and the silicon (Si) component in the aqueous slurry is more than 15 mol % and is 25 mol % or less; The content ratio of aluminum (Al) component to sulfur (S) component in the aqueous slurry is 0.40 to 1.05 in terms of molar ratio. A tobermorite-containing calcium silicate shaped body.
Citation Information
Patent Citations
Calcium silicate board with paper mill sludge ash and preparation method thereof
CN105016663A
Method for preparing calcium silicate board
CN105601184A
Gas concrete and its manufacture
JP1978063426A
Aqueous slurry for calcium silicate hydrate and calcium silicate molded article made from slurry
JP1989119554A
Calcium silicate plate and its production
JP1996325074A