Method for manufacturing chips
By forming modified regions and cracks within the workpiece using a laser beam, the method addresses thermal damage and maintains bending strength in chip manufacturing, ensuring reduced thermal impact and enhanced structural integrity.
Patent Information
- Application Number
- JP2023065812
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-10-25
AI Technical Summary
Existing chip manufacturing methods that irradiate the peripheral edge of the chip with a laser beam to chamfer the back side can cause thermal damage and reduce the bending strength of the chip.
A method involving irradiating a workpiece with a laser beam to form modified regions and cracks within the workpiece, allowing for the removal of portions without irradiating the remaining chip, thereby reducing thermal damage and maintaining bending strength.
The method results in chips with reduced thermal damage and suppressed decrease in bending strength by avoiding laser irradiation on the chip's peripheral edge.
Smart Images

Figure 2024151959000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a chip manufacturing method for producing a plurality of chips, each thinner than a workpiece, by removing a first removal portion located around each of the devices and a plurality of second removal portions located on the back side of the devices from a workpiece having a plurality of devices formed on its front side. [Background technology]
[0002] Chips for devices such as ICs (Integrated Circuits) are essential components in various electronic devices such as mobile phones and personal computers. These chips are manufactured, for example, by dividing a workpiece such as a wafer having multiple devices formed on its front surface along the boundaries between the multiple devices.
[0003] Furthermore, for the purpose of miniaturizing various electronic devices that are configured to include many chips, the workpiece and / or the multiple chips manufactured therefrom may be ground. For example, chips may be manufactured by forming grooves on the front side of the workpiece in portions that are located around each of multiple devices, and then grinding the back side of the workpiece until the workpiece is divided at the grooves as boundaries.
[0004] In this case, the back side of each of the multiple chips produced by dividing the workpiece is also slightly ground. In addition, the peripheral portion of the back side of each of the multiple chips may be chipped due to this grinding. If the peripheral portion of the back side of the chip is chipped, the flexural strength of the chip may be reduced.
[0005] In light of this, it has been proposed to irradiate the peripheral portion of the back surface of the chip with a laser beam so that the back surface is chamfered (see, for example, Patent Document 1). This removes the peripheral portion of the back surface where the chip exists from the chip, thereby preventing a decrease in the die strength of the chip. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2004-228218 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, when a laser beam is irradiated onto the peripheral portion of the back surface side of the chip, there is a risk that thermal damage may remain in the chip. In view of this, an object of the present invention is to provide a method for manufacturing a chip that can reduce thermal damage to the chip and suppress a decrease in the flexural strength of the chip. [Means for solving the problem]
[0008] According to the present invention, there is provided a chip manufacturing method for manufacturing a plurality of chips, each of which is thinner than a workpiece, by removing a first removal portion located around each of a plurality of devices formed on the front side of the workpiece and a plurality of second removal portions located on the back side of the plurality of devices, the method including: an internal processing step of irradiating a laser beam having a wavelength that transmits through the workpiece to the first removal portion to form a plurality of modified regions, each of which is located in the first removal portion, and a plurality of cracks extending from the plurality of modified regions so as to reach one of the plurality of second removal portions through one of a plurality of intermediate portions located between the plurality of devices and the plurality of second removal portions; a first removal step of removing the first removal portion after performing the internal processing step; and a second removal step of grinding and removing the plurality of second removal portions and separating each of the back side peripheral portions from the plurality of chips using the plurality of cracks as boundaries after performing the first removal step.
[0009] In addition, in the internal processing step, it is preferable that the laser beam branched to form multiple focal points is irradiated onto the workpiece, and the multiple focal points are formed at different positions in both the thickness direction of the workpiece and the direction perpendicular to the thickness direction.
[0010] Furthermore, it is preferable that the chip manufacturing method of the present invention further comprises a bonding step of bonding the multiple devices to a supporting substrate so that the multiple second removed portions are exposed before performing the internal processing step, after performing the internal processing step and before performing the first removal step, or after performing the first removal step and before performing the second removal step. Effect of the Invention
[0011] In the chip manufacturing method of the present invention, the laser beam is irradiated onto the first removed portions located around each of the multiple devices in the workpiece, but the laser beam is not irradiated onto the portions that remain as the multiple chips. Therefore, this method can provide chips that have reduced thermal damage compared to chips that have been irradiated onto the peripheral edge of their back sides with the laser beam.
[0012] Furthermore, in this method, when grinding and removing the multiple second removed portions located on the back side of the multiple devices of the workpiece, the back side peripheral portions of each of the multiple chips are separated along the boundaries of multiple cracks extending from the multiple modified regions so as to reach one of the multiple second removed portions through one of multiple intermediate portions located between the multiple devices and the multiple second removed portions.
[0013] That is, in this method, even if the peripheral portion of the back surface of each of the chips is chipped during grinding, the portion where the chip exists is removed, and therefore, this method can provide chips with less deterioration in flexural strength compared to chips with chips on the peripheral portion of the back surface. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1(A) is a perspective view showing a schematic example of a workpiece used in manufacturing multiple chips, and FIG. 1(B) is a cross-sectional view showing a schematic example of the workpiece shown in FIG. 1(A). [Diagram 2] FIG. 2 is a flowchart illustrating an example of a chip manufacturing method for producing multiple chips, each of which is thinner than the workpiece, by removing a first removal portion and multiple second removal portions of the workpiece. [Diagram 3] FIG. 3(A) is a perspective view that shows a schematic example of a frame unit including a workpiece, and FIG. 3(B) is a cross-sectional view that shows a schematic example of the frame unit shown in FIG. 3(A). [Figure 4] FIG. 4 is a perspective view that illustrates an example of an internal processing step. [Diagram 5] FIG. 5 is a diagram illustrating an example of the laser beam irradiation unit shown in FIG. 4 and a laser beam irradiated therefrom. [Figure 6] FIG. 6 is a partially enlarged cross-sectional view showing a schematic view of a portion of the frame unit irradiated with a laser beam. [Figure 7] Figure 7(A) is a perspective view showing a frame unit including a workpiece with protective tape peeled off from its surface, and Figure 7(B) is a cross-sectional view showing a frame unit shown in Figure 7(A). [Figure 8] FIG. 8 is a partial cross-sectional side view illustrating an example of the first removal step. [Figure 9] FIG. 9 is a partially enlarged cross-sectional view showing a schematic view of a portion of a frame unit where a groove is formed. [Figure 10] Figure 10(A) is an oblique view showing a schematic of multiple chips with the dicing tape peeled off from their back surfaces and protective tape attached to their front surfaces, and Figure 10(B) is a cross-sectional view showing a schematic of the multiple chips shown in Figure 10(A). [Figure 11]FIG. 11 is a partial cross-sectional side view that illustrates an example of the second removal step. [Figure 12] FIG. 12 is a cross-sectional view showing a schematic diagram of a plurality of chips that have been thinned with their respective surfaces attached to protective tapes. [Figure 13] FIG. 13 is a partial cross-sectional side view illustrating a schematic view of another example of the first removing step. [Figure 14] FIG. 14 is a partially enlarged cross-sectional view showing a schematic view of a portion of a frame unit where a groove is formed. [Figure 15] Figure 15 is a flowchart that illustrates another example of a chip manufacturing method for producing multiple chips, each of which is thinner than the workpiece, by removing a first removal portion and multiple second removal portions of the workpiece. [Figure 16] Figure 16(A) is a cross-sectional view showing a laminate formed by bonding a workpiece to a supporting substrate in a bonding step, Figure 16(B) is a cross-sectional view showing a laminate including a workpiece whose back surface has been ground in a preliminary grinding step, and Figure 16(C) is a cross-sectional view showing a laminate including a workpiece in which multiple cracks have been formed in an internal processing step. [Figure 17] FIG. 17 is a schematic diagram illustrating another example of the first removal step. [Figure 18] FIG. 18(A) is a partially enlarged cross-sectional view showing a schematic representation of a portion of a laminate where a groove is formed, and FIG. 18(B) is a cross-sectional view showing a schematic representation of a laminate including a plurality of chips. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] The present invention will be described with reference to the accompanying drawings, in which: Fig. 1(A) is a perspective view showing an example of a workpiece used in manufacturing a plurality of chips, and Fig. 1(B) is a cross-sectional view showing the workpiece shown in Fig. 1(A).
[0016] 1(A) and 1(B) is, for example, a disk-shaped wafer including a front surface 11a and a back surface 11b that are generally parallel to each other and made of a semiconductor material such as single crystal silicon. A notch 11c is formed on the side of the workpiece 11 to indicate a specific crystal orientation of the semiconductor material.
[0017] Furthermore, a plurality of devices 13 are formed on the front surface 11a side of the workpiece 11. The plurality of devices 13 are arranged in a matrix. That is, the boundaries between the plurality of devices 13 extend in a lattice pattern. Then, by partially removing the workpiece 11, a plurality of chips, each of which is thinner than the workpiece 11, are manufactured.
[0018] Specifically, multiple chips are manufactured by removing first removal portions 11d located around each of multiple devices 13 in the workpiece 11 and multiple second removal portions 11e located on the back side of the multiple devices 13.
[0019] The first portion to be removed 11d extends in a lattice pattern and includes boundaries between the multiple devices 13. Each of the multiple straight line portions included in the first portion to be removed 11d is also called a division line.
[0020] The plurality of second portions to be removed 11e are present in a matrix pattern, similar to the plurality of devices 13. Furthermore, between the plurality of second portions to be removed 11e and the plurality of devices 13, there are a plurality of intermediate portions 11f.
[0021] FIG. 2 is a flowchart illustrating an example of a chip manufacturing method for producing multiple chips, each of which is thinner than workpiece 11, by removing a first removed portion 11d and multiple second removed portions 11e of workpiece 11.
[0022] In this method, first, a plurality of modified regions are formed, each located in the first removed portion 11d, and a plurality of cracks are formed, each extending from the plurality of modified regions so as to pass through one of a plurality of intermediate portions 11f located between the plurality of devices 13 and the plurality of second removed portions 11e and reach one of the plurality of second removed portions 11e (internal processing step S1).
[0023] This internal processing step S1 is performed, for example, in a laser processing device by irradiating a laser beam onto a frame unit including the workpiece 11. Fig. 3(A) is a perspective view that shows a schematic example of a frame unit including the workpiece 11, and Fig. 3(B) is a cross-sectional view that shows a schematic example of the frame unit shown in Fig. 3(A).
[0024] 3(A) and 3(B) has an annular frame 15 in which a circular opening 15a is formed. The frame 15 is made of a metal such as aluminum (Al), and has attached to one surface thereof an outer peripheral region of a disk-shaped dicing tape 17 having a diameter larger than that of the opening 15a.
[0025] The dicing tape 17 has, for example, a flexible film-like base layer and an adhesive layer (glue layer) provided on one surface (the surface on the frame 15 side) of the base layer. Specifically, the base layer is made of polyolefin (PO), polypropylene (PP), polyethylene terephthalate (PET), polyvinyl chloride (PVC), polystyrene (PS), or the like. The adhesive layer is made of ultraviolet-curing silicone rubber, an acrylic material, an epoxy material, or the like.
[0026] Then, the back surface 11b of the workpiece 11, that is, the multiple second portions to be removed 11e, are attached to the central region of the dicing tape 17 so as to position the workpiece 11 in the opening 15a.
[0027] Furthermore, a disk-shaped protective tape 19 having a diameter roughly equal to that of the workpiece 11 and for protecting the devices 13 is attached to the surface 11a of the workpiece 11, i.e., to the multiple devices 13. This protective tape 19 has a structure similar to that of the dicing tape 17, for example.
[0028] In the frame unit 1, the dicing tape 17 may be replaced with a sheet that does not include an adhesive layer. This sheet is made of, for example, the same material as the base layer of the dicing tape 17, and is thermocompression bonded to the back surface 11b of the workpiece, i.e., the multiple second removed portions 11e, and one surface of the frame 15.
[0029] Fig. 4 is a perspective view showing an example of the internal processing step S1. Note that the X-axis direction and the Y-axis direction shown in Fig. 4 are directions perpendicular to each other on a horizontal plane, and the Z-axis direction is a direction perpendicular to the X-axis direction and the Y-axis direction (vertical direction).
[0030] The laser processing apparatus 2 shown in Fig. 4 has a chuck table 4. This chuck table 4 has a disk-shaped frame whose diameter is larger than the diameter of the workpiece 11. This frame has a disk-shaped bottom wall and a cylindrical side wall standing upright from the outer periphery of the bottom wall.
[0031] That is, a disk-shaped recess defined by a bottom wall and a side wall is formed on the upper surface of the frame. A disk-shaped porous plate is fixed to the recess. A flow path is formed in the bottom wall of the frame, the flow path opening at the bottom surface of the recess and penetrating the bottom wall. Furthermore, the porous plate communicates with a suction source such as an ejector through the flow path.
[0032] When the suction source is operated, a suction force acts on the space near the upper surface of the porous plate via the porous plate. Therefore, for example, when the frame unit 1 is carried onto the chuck table 4 so that the workpiece 11 is placed on the chuck table 4 via the protective tape 19, the frame unit 1 is held on the upper surface (holding surface) of the chuck table 4 by operating the suction source.
[0033] Furthermore, the chuck table 4 is connected to a rotation mechanism including, for example, a pulley and a motor, etc. When this rotation mechanism is operated, the chuck table 4 rotates about a rotation axis that passes through the center of the holding surface of the chuck table 4 and is aligned in the Z-axis direction.
[0034] Furthermore, the chuck table 4 is connected to a horizontal movement mechanism including, for example, a ball screw, a motor, etc. When this horizontal movement mechanism is operated, the chuck table 4 moves along the X-axis and / or Y-axis directions.
[0035] A laser beam irradiation unit 6 is provided above the chuck table 4. Fig. 5 is a diagram showing an example of the laser beam irradiation unit 6 and the laser beam emitted therefrom. The laser beam irradiation unit 6 has a laser oscillator 8.
[0036] The laser oscillator 8 has, for example, Nd:YAG as a laser medium, and irradiates the workpiece 11 with a pulsed laser beam LB (for example, with a frequency of 60 kHz) having a wavelength (for example, 1064 nm or 1342 nm) that transmits through the material of the workpiece 11.
[0037] The output (power) of this laser beam LB is adjusted by an attenuator 10, and then the laser beam LB is supplied to a branching unit 12. This branching unit 12 has, for example, a spatial light modulator including a liquid crystal phase control element called LCoS (Liquid Crystal on Silicon) and / or a diffractive optical element (DOE).
[0038] Then, the branching unit 12 branches the laser beam LB so that the laser beam LB irradiated from the head 16 described below to the holding surface side of the chuck table 4 forms a plurality of focusing points. For example, the branching unit 12 branches the laser beam LB so as to satisfy the following conditions in the internal processing step S1.
[0039] An even number of focal points (eight here, four or more) are formed. Except for the distance in the Y-axis direction between a pair of focal points located in the center, the distance in the Y-axis direction between adjacent pairs of focal points is approximately equal. The distance between the pair of focal points located in the center is greater than the distance between the other pairs of adjacent focal points. The positions (heights) in the Z-axis direction of the pair of focal points located in the center are approximately equal. The height of the pair of focal points located in the center is lower than the heights of the other focal points.
[0040] From one of the pair of focusing points located on the central side among the eight focusing points to the focusing point located at one end in the Y-axis direction, i.e., the four focusing points on one side, are arranged at equal intervals in the Z-axis direction. Similarly, from the other of the pair of focusing points located on the central side among the eight focusing points to the focusing point located at the other end in the Y-axis direction, i.e., the four focusing points on the other side, are arranged at equal intervals in the Z-axis direction.
[0041] The distance in the Z-axis direction between a pair of adjacent focusing points among the four focusing points on one side is approximately equal to the distance in the Z-axis direction between a pair of adjacent focusing points among the four focusing points on the other side. The distance in the Y-axis direction between the focusing points located at one end and the focusing points located at the other end is slightly smaller than the width of a region of the first removed portion 11d included in the workpiece 11 that is located between a pair of adjacent devices 13.
[0042] The laser beam LB branched by the branching unit 12 is reflected by a mirror 14 and guided to a head 16. A condenser lens (not shown) for condensing the laser beam LB is housed in the head 16. The laser beam LB condensed by the condenser lens is irradiated onto the holding surface side of the chuck table 4, more simply, directly below.
[0043] Furthermore, the head 16 of the laser beam irradiation unit 6 and an optical system (e.g., mirror 14) for directing the laser beam LB to the head 16 are connected to a vertical movement mechanism including a ball screw, a motor, etc. When this vertical movement mechanism is operated, the head 16 and the like move along the Z-axis direction.
[0044] In addition, as shown in FIG. 4, an imaging unit 18 is provided on the side of the head 16 to capture images using light of a wavelength that passes through the material constituting the dicing tape 17 and the material of the workpiece 11, such as infrared light.
[0045] This imaging unit 18 includes, for example, a light source such as an LED (Light Emitting Diode) that emits infrared rays, an objective lens, and an imaging element such as a CCD (Charge Coupled Device) image sensor or a CMOS (Complementary Metal Oxide Semiconductor) image sensor, and captures an image of the holding surface side of the chuck table 4.
[0046] When performing the internal processing step S1 in the laser processing device 2, first, the frame unit 1 is carried into the laser processing device 2 so that the workpiece 11 is placed on the chuck table 4 via the protective tape 19. Next, the suction source communicating with the porous plate of the chuck table 4 is operated. As a result, the frame unit 1 is held by the chuck table 4 with the dicing tape 17 facing upward.
[0047] Next, the imaging unit 18 captures an image of the front surface 11a side of the workpiece 11. This forms an image that allows recognition of the arrangement of the multiple devices 13 on the front surface 11a side of the workpiece 11. Next, with reference to this image, the chuck table 4 is rotated so that a specific planned dividing line included in the first removed portion 11d of the workpiece 11 becomes parallel to the X-axis direction.
[0048] Next, in a plan view, the chuck table 4 is moved along the X-axis direction and / or the Y-axis direction so that the specific planned division line is positioned in the X-axis direction as seen from the head 16. Next, the head 16 etc. are raised and lowered so that a pair of central focusing points among eight focusing points formed when the laser beam LB is irradiated directly downward from the head 16 are positioned slightly higher than the position of the surface of the first removed portion 11d.
[0049] Next, the laser beam irradiation unit 6 is operated so that the laser beam LB is irradiated directly downward from the head 16. Next, the chuck table 4 is moved along the X-axis direction so that the laser beam LB passes over the workpiece 11 from one end to the other end in the X-axis direction.
[0050] As a result, a modified region 21 in which the crystal structure of the material of the workpiece 11 is disturbed is formed inside the first removed portion 11d, centered on the focal point where the laser beam LB is focused (see FIG. 6). Note that FIG. 6 is a partially enlarged cross-sectional view that typically shows a portion of the frame unit 1 irradiated with the laser beam LB.
[0051] The laser beam LB is branched by the branching unit 12 so as to satisfy the above-mentioned conditions, so that eight modified regions 21 are formed inside the first removed portion 11d.
[0052] The eight modified regions 21 are broadly divided into four modified regions 21 located between the center and one end in the Y-axis direction, i.e., the four modified regions 21 on one side, and four modified regions 21 located between the center and the other end in the Y-axis direction, i.e., the four modified regions 21 on the other side.
[0053] Moreover, the four modified regions 21 on one side and the four modified regions 21 on the other side are linearly aligned so as to be inclined at a predetermined angle with respect to the thickness direction of the workpiece 11 so that the positions of the modified regions 21 located on the outside are higher than the positions of the modified regions 21 located on the inside. Furthermore, the four modified regions 21 on one side and the four modified regions 21 on the other side are plane-symmetrical with respect to a plane that passes through the center of both modified regions in the Y-axis direction and is parallel to the X-axis direction and Z-axis direction.
[0054] Furthermore, when the eight modified regions 21 are formed inside the first removal portion 11d, the volume of the workpiece 11 expands, causing internal stress in the workpiece 11. This internal stress is then alleviated by the extension of cracks 23 from each of the eight modified regions 21.
[0055] Here, crack 23 tends to extend toward the adjacent modified region 21. That is, crack 23 tends to extend so as to be inclined at the predetermined angle with respect to the thickness direction of workpiece 11. As a result, crack 23 reaches the surface of first portion to be removed 11d, and also reaches second portion to be removed 11e through intermediate portion 11f.
[0056] Furthermore, the movement of the chuck table 4 and the operation of the laser beam irradiation unit 6 are repeated so that the modified regions 21 and the cracks 23 are formed in the entire first removed portion 11d of the workpiece 11. This completes the internal processing step S1.
[0057] It should be noted that the cracks 23 formed in the internal processing step S1 do not have to reach the surface of the first removed portion 11d. For example, when the four modified regions 21 on one side and the four modified regions 21 on the other side are formed so that the above-mentioned predetermined angle is 60° or more, the cracks 23 do not have to reach the surface of the first removed portion 11d.
[0058] This is preferable because it is easy to increase the size of the rear surface side peripheral portion separated from each of the multiple chips manufactured from the workpiece 11. However, in this case, the crack 23 is likely to extend to the device 13. In contrast, if the crack 23 is formed to reach the surface of the first portion to be removed 11d, this is preferable because it is possible to suppress the extension of the crack 23 to the device 13.
[0059] After the internal processing step S1 is performed, the first removed portion 11d is removed (first removing step S2). This first removing step S2 is performed, for example, by cutting the frame unit 1 including the workpiece 11 from which the protective tape 19 has been peeled off from the surface 11a in a cutting device.
[0060] Figure 7(A) is an oblique view showing a frame unit 1 including a workpiece 11 with protective tape 19 peeled off from its surface 11a, and Figure 7(B) is a cross-sectional view showing a frame unit 1 shown in Figure 7(A).
[0061] 7(A) and 7(B), a crack 23 is formed on the front surface 11a side along the first portion 11d to be removed of the workpiece 11. Moreover, this crack 23 extends inside the workpiece 11 so as to be inclined with respect to the thickness direction of the workpiece 11.
[0062] Fig. 8 is a partial cross-sectional side view showing an example of the first removal step S2. Note that the U-axis direction and the V-axis direction shown in Fig. 8 are directions perpendicular to each other on a horizontal plane, and the W-axis direction is a direction perpendicular to the U-axis direction and the V-axis direction (vertical direction).
[0063] The cutting device 20 shown in Fig. 8 has a chuck table 22. This chuck table 22 has a structure similar to that of the chuck table 4 shown in Fig. 4. In addition, a plurality of clamps (not shown) are provided around the chuck table 22.
[0064] These clamps are provided at approximately equal angular intervals along the circumferential direction of the chuck table 22. When the frame unit 1 is held on the chuck table 22, the multiple clamps grip the frame 15 at a position lower than the holding surface of the chuck table 22.
[0065] In addition, the chuck table 22 and the multiple clamps are connected to a rotation mechanism including, for example, a pulley and a motor, etc. When this rotation mechanism is operated, the chuck table 22 rotates about a rotation axis that passes through the center of the holding surface of the chuck table 22 and is aligned along the W-axis direction.
[0066] Furthermore, the chuck table 22 is connected to a U-axis direction moving mechanism including, for example, a ball screw, a motor, etc. When this U-axis direction moving mechanism is operated, the chuck table 22 moves along the U-axis direction.
[0067] A cutting unit 24 is provided above the chuck table 22. The cutting unit 24 has a cylindrical spindle 26 extending along the V-axis direction. A base end of the spindle 26 is connected to a rotation drive source (not shown) such as a motor, and an annular cutting blade 28 is attached to the tip end of the spindle 26.
[0068] When the rotary drive source is operated, the cutting blade 28 rotates together with the spindle 26 around a straight line along the V-axis direction as a rotation axis. The cutting blade 28 is attached to the spindle 26 so that the straight line that serves as the rotation axis of the spindle 26 passes through the center of the cutting blade 28.
[0069] The cutting unit 24 is connected to a V-axis direction moving mechanism and a W-axis direction moving mechanism, each of which includes a ball screw, a motor, etc. When the V-axis direction moving mechanism is operated, the cutting unit 24 moves along the V-axis direction, and when the W-axis direction moving mechanism is operated, the cutting unit 24 moves along the W-axis direction.
[0070] When the first removing step S2 is performed in the cutting device 20, first, the frame unit 1 is carried into the cutting device 20 so that the workpiece 11 is placed on the chuck table 22 with the dicing tape 17 interposed therebetween.
[0071] Next, a suction source communicating with the porous plate of the chuck table 22 is operated, and the frame 15 is gripped by the multiple clamps. As a result, the frame unit 1 is held by the chuck table 22 in a state where the surface 11a of the workpiece 11, i.e., the multiple devices 13 and the first removed portion 11d, are exposed.
[0072] Next, the chuck table 22 is rotated so that a specific planned division line included in the first removed portion 11d is parallel to the U-axis direction. Next, the chuck table 22 is moved along the U-axis direction and / or the cutting unit 24 is moved along the V-axis direction so that the specific planned division line is positioned in the U-axis direction when viewed from the cutting blade 28 in a plan view.
[0073] Next, the cutting unit 24 is raised and lowered so that the lower end of the cutting blade 28 is positioned inside the dicing tape 17, i.e., above the holding surface of the chuck table 22 and below the back surface 11b of the workpiece 11. Next, the rotation drive source connected to the spindle 26 is operated to rotate the cutting blade 28.
[0074] Next, the chuck table 22 is moved along the U-axis direction so that the cutting blade 28 passes over the workpiece 11 from one end to the other end in the U-axis direction. As a result, a linear groove 25 is formed in the frame unit 1, penetrating the workpiece 11 and with its bottom surface positioned on the dicing tape 17 (see FIG. 9). Note that FIG. 9 is a partially enlarged cross-sectional view that typically shows a portion of the frame unit 1 where the groove 25 is formed.
[0075] Additionally, a linear region along the specific planned division line in the first portion to be removed 11d is removed together with the multiple modified regions 21 and multiple cracks 23 contained in this region. However, the portions of the multiple cracks 23 that extend from this region and are formed in the intermediate portion 11f and the multiple second portions to be removed 11e remain.
[0076] Furthermore, the relative movement of the chuck table 22 and the cutting unit 24 and the rotation of the cutting blade 28 are repeated so that the first removed portion 11d of the workpiece 11 is removed together with the multiple modified regions 21 and multiple cracks 23 contained therein. As a result, the workpiece 11 is divided to produce multiple chips, each of which has approximately the same thickness as the workpiece 11. This completes the first removal step S2.
[0077] After the first removing step S2 is performed, the second removed portions 11e are ground and removed, and the back surface side peripheral portions of each are separated from the chips along the cracks 23 (second removing step S3). This second removing step S3 is performed, for example, by grinding the back surfaces of each of the chips, i.e., the second removed portions 11e, from which the dicing tape 17 has been peeled off, in a grinding device.
[0078] Fig. 10(A) is a perspective view showing such a plurality of chips, and Fig. 10(B) is a cross-sectional view showing the plurality of chips shown in Fig. 10(A). A disk-shaped protective tape 29 is attached to the surface of each of the plurality of chips 27 shown in Fig. 10(A) and Fig. 10(B), i.e., to the plurality of devices 13. This protective tape 29 has a structure similar to that of the dicing tape 17, for example.
[0079] In the second removal step S3, the chips 27 included in the frame unit may be ground. The frame unit has, for example, a disk-shaped protective tape having a central region attached to each surface, i.e., the device 13, and an annular frame attached to the outer peripheral region of the protective tape.
[0080] The protective tape and frame included in this frame unit have, for example, the same structures as the dicing tape 17 and the frame 15, respectively. When the multiple chips 27 included in the frame unit are ground in the second removal step S3, this is preferable in that it makes it easier to handle the multiple chips 27, for example, to carry the multiple chips 27 into or out of a grinding device.
[0081] In this case, however, it is necessary to hold the frame with, for example, a plurality of clamps so that the frame is not ground together with the plurality of chips 27. In contrast, when the plurality of chips 27 shown in Figures 10(A) and 10(B) are ground in the second removal step S3, this is preferable because the second removal step S3 can be carried out even with a grinding device that does not have a plurality of clamps.
[0082] Fig. 11 is a partially sectional side view showing an example of the second removing step S3. The grinding apparatus 30 shown in Fig. 11 has a chuck table 32. This chuck table 32 has a structure similar to that of the chuck table 4 shown in Fig. 4. However, the holding surface of the chuck table 32 may have a shape corresponding to the side surface of a cone whose center protrudes slightly beyond the outer periphery.
[0083] Furthermore, the chuck table 32 is connected to a rotation mechanism including, for example, a pulley and a motor, etc. When this rotation mechanism is operated, the chuck table 32 rotates in the circumferential direction around a straight line passing through the center of the holding surface of the chuck table 32 as a rotation axis.
[0084] Furthermore, the chuck table 32 is connected to a rotation mechanism including, for example, a turntable, a motor, etc. When this rotation mechanism is operated, the chuck table 32 rotates on a horizontal plane.
[0085] A grinding unit 34 is provided above the chuck table 32. The grinding unit 34 has a spindle 36 that extends in a direction generally parallel to the vertical direction. The top surface of a disk-shaped wheel mount 38 made of stainless steel or the like is fixed to the tip (lower end) of the spindle 36.
[0086] Further, an annular grinding wheel 40 whose outer diameter is approximately equal to the diameter of the wheel mount 38 is attached to the underside of the wheel mount 38. The grinding wheel 40 has an annular wheel base 40a. This wheel base 40a is made of, for example, stainless steel, and on the underside thereof, a plurality of grinding stones 40b are arranged at approximately equal angular intervals along the circumferential direction of the wheel base 40a.
[0087] In addition, the base end (upper end) of the spindle 36 is connected to a rotary drive source such as a motor. When the rotary drive source operates, the wheel mount 38 and the grinding wheel 40 rotate together with the spindle 36.
[0088] Further, the grinding unit 34 is connected to a vertical movement mechanism including, for example, a ball screw, a motor, etc. When the vertical movement mechanism is operated, the grinding unit 34 moves in the vertical direction.
[0089] When the second removal step S3 is performed in the grinding device 30, first, the multiple chips 27 are carried into the grinding device 30 so that the multiple chips 27 are placed on the chuck table 32 via the protective tape 29. Next, the suction source communicating with the porous plate of the chuck table 32 is operated. As a result, the multiple chips 27 are held by the chuck table 32 with the multiple second removed portions 11e facing upward.
[0090] Next, the turning mechanism connected to the chuck table 32 is operated so that the trajectories of the multiple grinding stones 40b when the grinding wheel 40 is rotated are positioned directly above the center of the protective tape 29. Next, the rotary drive source connected to the spindle 36 is operated to rotate the grinding wheel 40, and the rotating mechanism connected to the chuck table 32 is operated to rotate the chuck table 32.
[0091] Next, while rotating both the grinding wheel 40 and the chuck table 32, the grinding unit 34 is lowered so that the lower surfaces of the grinding stones 40b come into contact with the back surfaces of the chips 27, i.e., the second removed portions 11e. This starts grinding the back surfaces of the chips 27, and the second removed portions 11e are gradually removed.
[0092] Furthermore, the back surfaces of the chips 27 are ground until all of the second portions to be removed 11e are removed. As a result, the chips 27 are manufactured, each of which is thinned (see FIG. 12). FIG. 12 is a cross-sectional view that shows the chips 27 that are thinned with their front surfaces attached to protective tape 29.
[0093] Here, when the second removed portions 11e are ground until the cracks 23 are exposed on the respective back surfaces, the chips 27 are cleaved with the cracks 23 as boundaries. In other words, the peripheral portion on the back surface side of each of the chips 27 is separated from each chip 27 during this grinding. This completes the second removal step S3.
[0094] 2, the laser beam LB is irradiated onto first removed portions 11d located around each of the plurality of devices 13 in the workpiece 11, but the laser beam LB is not irradiated onto portions remaining as the plurality of chips 27. Therefore, this method can provide chips 27 with reduced thermal damage compared to chips whose rear surface side peripheral portion is irradiated with the laser beam LB.
[0095] Furthermore, in this method, when grinding and removing the multiple second removed portions 11e located on the back surface 11b side of the multiple devices 13 of the workpiece 11, the back surface side peripheral portions of each of the multiple chips 27 are separated along the boundaries of the multiple cracks 23 extending from the multiple modified regions 21 so as to pass through one of the multiple intermediate portions 11f located between the multiple devices 13 and the multiple second removed portions 11e and reach one of the multiple second removed portions 11e.
[0096] That is, in this method, even if the peripheral edge of the back side of each of the plurality of chips 27 is chipped during grinding, the portion where the chip exists is removed. Therefore, this method can provide chips 27 with less deterioration in flexural strength compared to chips with chips on the peripheral edge of the back side.
[0097] The above-mentioned content is one aspect of the present invention, and the content of the present invention is not limited to the above-mentioned content. For example, in the internal processing step S1 of the present invention, a plurality of modified regions 21 and a plurality of cracks 23 may be formed by irradiating a laser beam LB from the surface 11a side of the workpiece 11.
[0098] In this case, in the internal processing step S1, it is not necessary to perform imaging using infrared rays to check the arrangement of the multiple devices 13, i.e., the orientation of a specific planned division line included in the first removed portion 11d. Therefore, in this case, it is preferable in that the internal processing step S1 can be performed using an inexpensive laser processing device that does not include an imaging unit 18 that performs imaging using infrared rays.
[0099] However, a TEG (Test Elementary Group) or the like for evaluating the performance of the device 13 may be formed on the surface of the first removed portion 11d. In this case, it may be difficult to form a plurality of modified regions 21 and a plurality of cracks 23 at desired locations.
[0100] In contrast, when multiple modified areas 21 and multiple cracks 23 are formed by irradiating a laser beam LB from the back surface 11b side of the workpiece 11, this is preferable in that it is easy to form multiple modified areas 21 and multiple cracks 23 at desired locations even when TEG or the like is formed on the surface of the first removed portion 11d.
[0101] In the internal processing step S1 of the present invention, the multiple (e.g., eight in FIG. 6) modified regions 21 included in the linear region along a specific planned division line in the first removed portion 11d may not be formed simultaneously. Specifically, some of the multiple modified regions 21, for example, the four modified regions 21 on one side, may be formed first, and then the remaining portions, for example, the four modified regions 21 on the other side, may be formed.
[0102] In other words, in the internal processing step S1 of the present invention, a laser beam LB branched to form a portion of the multiple modified regions 21 may be irradiated onto the linear region, and then a laser beam LB branched to form the remainder may be irradiated onto the linear region.
[0103] In the internal processing step S1 of the present invention, the linear region may be irradiated with a laser beam again after the modified regions 21 and the cracks 23 are formed in the linear region, thereby making it possible to enlarge each of the modified regions 21 and / or further extend each of the cracks 23.
[0104] In the first removing step S2 of the present invention, the first removed portion 11d may be removed by cutting the cutting blade 28 from the back surface 11b side of the workpiece 11. In this case, the front surface 11a of the workpiece 11, i.e., the multiple devices 13, are attached to a dicing tape 17 prior to the internal processing step S1.
[0105] In this case, it is not necessary to adhere protective tape 19 to back surface 11b of workpiece 11, i.e., to the second portions 11e to be removed, prior to internal processing step S1. Therefore, this is preferable in that it saves the trouble of adhering protective tape 19 to the second portions 11e to be removed and peeling it off.
[0106] In this case, however, it is necessary to perform imaging using infrared rays in order to grasp the planned dividing line included in the first removed portion 11d of the workpiece 11 in the first removal step S2. Therefore, in this case, it is necessary to perform the first removal step S2 using an expensive cutting device equipped with an imaging unit similar to the imaging unit 18.
[0107] In contrast, when the first removed portion 11d is removed by cutting the cutting blade 28 from the surface 11a side of the workpiece 11, this is preferable in that the first removal step S2 can be carried out using an inexpensive cutting device that does not have an imaging unit similar to the imaging unit 18, such as cutting device 20.
[0108] In the first removal step S2 of the present invention, a groove may be formed in the frame unit 1 so as not to penetrate the workpiece 11, but with its bottom surface located in the workpiece 11. Fig. 13 is a partially sectional side view showing a schematic view of an example of the first removal step S2 thus performed.
[0109] This first removal step S2 is performed, for example, by cutting the frame unit 1 shown in Figures 7(A) and 7(B) in the above-mentioned cutting device 20. Specifically, when performing the first removal step S2 in this manner, first, the frame unit 1 is held by the chuck table 22 as described above.
[0110] Next, as described above, in plan view, the planned division line included in the first removed portion 11d is positioned in the U-axis direction as seen from the cutting blade 28. Next, the cutting unit 24 is raised and lowered so that the lower end of the cutting blade 28 is positioned inside the workpiece 11, specifically, above the dicing tape 17 and below the multiple first removed portions 11d of the workpiece 11.
[0111] Next, as described above, the relative movement of the chuck table 22 and the cutting unit 24 and the rotation of the cutting blade 28 are repeated. As a result, lattice-shaped grooves 31, which do not penetrate the workpiece 11 but have their bottom surfaces located on the workpiece 11, are formed in the frame unit 1 (see FIG. 14). Note that FIG. 14 is a partially enlarged cross-sectional view that shows a schematic view of the portion of the frame unit 1 where the grooves 31 are formed.
[0112] In this first removal step S2, the workpiece 11 is not divided, that is, a plurality of chips 27 are not produced. In this case, in the second removal step S3, the back surface 11b side of the workpiece 11 is ground until the workpiece 11 is divided along the boundary of the groove 31, thereby producing a plurality of chips 27.
[0113] The first removal step S2 of the present invention may be performed in a dry etching apparatus by plasma etching the workpiece 11 having a mask provided thereon so as to cover the plurality of devices 13. An example of a dry etching apparatus for performing such plasma etching will be described later.
[0114] The second removal step S3 of the present invention may also be performed by grinding the respective surfaces, i.e., the devices 13, of a plurality of chips bonded to a support substrate rather than to the protective tape 29. The support substrate may be, for example, a wafer having approximately the same shape as the workpiece 11.
[0115] Furthermore, the bonding of the multiple devices 13 to the support substrate may be performed before performing the internal processing step S1, after performing the internal processing step S1 and before performing the first removal step S2, or after performing the first removal step S2 and before performing the second removal step S3. That is, in the present invention, the multiple chips 27 may be bonded to the support substrate, or the workpiece 11 before being divided into the multiple chips 27 may be bonded to the support substrate.
[0116] In addition, when multiple chips 27 are bonded to a support substrate, it is preferable in that only chips 27 having good processing quality can be extracted and bonded. On the other hand, when the workpiece 11 is bonded to a support substrate, the operation is simplified, so that it is preferable in that it is possible to suppress the intrusion of impurities into the chips and / or improve the throughput.
[0117] In the present invention, prior to the internal processing step S1, the back surface 11b side of the workpiece 11 may be ground so as to thin the second removed portions 11e. This grinding is performed, for example, in a grinding device 30.
[0118] The method for producing a chip of the present invention may be implemented by appropriately combining the above-mentioned contents. Fig. 15 is a flow chart showing an example of such a method for producing a chip.
[0119] In this method, first, the workpiece 11 is bonded to a support substrate (bonding step S4). Fig. 16(A) is a cross-sectional view that shows a schematic diagram of a laminate formed by bonding the workpiece 11 to the support substrate in this bonding step S4.
[0120] The support substrate 33 bonded to the workpiece 11 has, for example, the same shape as the workpiece 11. Similarly to the workpiece 11, a plurality of devices may be formed on the front surface 33a side of the support substrate 33.
[0121] Then, in a bonding step S4, the surface 11a of the workpiece 11, i.e., the multiple devices 13, are bonded to the surface 33a of the support substrate 33. Specifically, in this bonding step S4, first, an adhesive containing an acrylic adhesive or an epoxy adhesive is provided on the surface 33a of the support substrate 33.
[0122] Next, with the back surface 33b of the support substrate 33 supported, the front surface 11a of the workpiece 11 is pressed against the front surface 33a of the support substrate 33 via the adhesive. This forms a layered body 35 including the workpiece 11 bonded to the support substrate 33 so that the back surface 11b is exposed. This completes the bonding step S4.
[0123] After performing the joining step S4, the back surface 11b side of the workpiece 11 is ground (pre-grinding step S5). Fig. 16(B) is a cross-sectional view that shows a schematic diagram of a laminate 35 including the workpiece 11 whose back surface 11b side has been ground in this pre-grinding step S5.
[0124] This preliminary grinding step S5 is performed, for example, by grinding the back surface 11b side of the workpiece 11 in a grinding device 30 until the thickness of the plurality of second removed portions 11e shown in Fig. 1(B) etc. becomes 1 / 3 to 2 / 3 times, typically 1 / 2. Note that this grinding is performed in the same manner as the above-mentioned second removal step S3, and therefore a detailed description thereof will be omitted.
[0125] After the preliminary grinding step S5 is performed, the internal processing step S1 is performed. Fig. 16(C) is a cross-sectional view that shows a schematic diagram of a laminate 35 including a workpiece 11 in which a plurality of cracks 23 are formed in the internal processing step S1.
[0126] This internal processing step S1 is performed, for example, by irradiating a laser beam LB to the laminate 35 including the workpiece 11 whose back surface 11b side has been ground in a laser processing device 2. Note that the irradiation of this laser beam LB is performed in the same manner as in the above-mentioned internal processing step S1, and therefore a detailed description thereof will be omitted.
[0127] After the internal processing step S1 is performed, a first removal step S2 is performed, for example, by plasma etching the laminate 35 including the workpiece 11 having the plurality of cracks 23 formed therein in a dry etching device.
[0128] Fig. 17 is a diagram showing an example of the first removal step S2. The dry etching apparatus 42 shown in Fig. 17 has a chamber 44 made of a conductive material and grounded. The chamber 44 has an inlet / outlet 44a for carrying the laminate 35 in and carrying the laminate 35 out of the chamber 44.
[0129] The loading / unloading port 44a is provided with a gate valve 46 that can isolate or connect the internal space of the chamber 44 to the external space. The chamber 44 is also formed with an exhaust port 44b for exhausting the internal space.
[0130] The exhaust port 44b communicates with an exhaust device 50 such as a vacuum pump via a pipe 48. A support member 52 is provided on the inner surface of the chamber 44, and the support member 52 supports a table .
[0131] An electrostatic chuck (not shown) is provided on the upper part of the table 54. A disk-shaped electrode 54a located below the electrostatic chuck is provided inside the table 54. The electrode 54a is connected to a high-frequency power supply 58 via a matching unit 56.
[0132] A disk-shaped opening is formed in the chamber 44 at a position facing the upper surface of the table 54, and a gas ejection head 62 supported by the chamber 44 via a bearing 60 is provided in this opening. The gas ejection head 62 is made of a conductive material, and is connected to a high-frequency power source 66 via a matching unit 64.
[0133] A cavity (gas diffusion space) 62a is formed inside the gas ejection head 62. A plurality of gas discharge ports 62b that communicate the gas diffusion space 62a with the internal space of the chamber 44 are formed in an inner portion (e.g., a lower portion) of the gas ejection head 62. Two gas supply ports 62c and 62d for supplying a predetermined gas to the gas diffusion space 62a are formed in an outer portion (e.g., an upper portion) of the gas ejection head 62.
[0134] The gas supply port 62c communicates with a gas supply source 70a that supplies, for example, a fluorocarbon gas such as C4F8 and / or a fluorosulfur gas such as SF6 via a pipe 68a, etc. The gas supply port 62d communicates with a gas supply source 70b that supplies, for example, an inert gas such as Ar and O2 gas via a pipe 68b, etc.
[0135] When the first removal step S2 is performed in the dry etching apparatus 42, for example, a so-called Bosch process is performed. Specifically, in the first removal step S2, first, the laminate 35 having the mask 37 provided so as to cover the multiple devices 13 is carried into the internal space of the chamber 44 via the carry-in / out port 44a, and placed on the table 54 with the support substrate 33 facing down.
[0136] Next, the internal space of the chamber 44 is isolated from the external space by the gate valve 46, and the laminate 35 is held by the electrostatic chuck of the table 54. Next, the internal space of the chamber 44 is evacuated by the exhaust device 50 to create a vacuum state.
[0137] Next, while a gas containing SF6 is supplied from the gas supply source 70a to the internal space of the chamber 44 and Ar gas is supplied from the gas supply source 70b, high frequency power is supplied from the high frequency power supply 66 to the gas ejection head 62. As a result, the exposed portion of the workpiece 11 that is not covered by the mask 37 is isotropically etched by F-based radicals and the like generated in the internal space of the chamber 44.
[0138] Next, a gas containing C4F8 is supplied from the gas supply source 70a to the internal space of the chamber 44 for a predetermined period of time, and while Ar gas is being supplied from the gas supply source 70b, high frequency power is supplied from the high frequency power supply 66 to the gas ejection head 62. As a result, CF radicals are deposited on the etched portion of the workpiece 11, forming a protective film containing fluorocarbon.
[0139] Next, while a gas containing SF6 is supplied from the gas supply source 70a to the internal space of the chamber 44 and Ar gas is supplied from the gas supply source 70b for a predetermined period of time, high frequency power is supplied from the high frequency power source 58 to the electrode 54a provided inside the table 54 and high frequency power is supplied from the high frequency power source 66 to the gas ejection head 62. As a result, F-based ions and the like generated in the internal space of the chamber 44 are accelerated toward the table 54, and the protective film is anisotropically etched. In addition, with this etching, the portion of the workpiece 11 not covered by the mask 37 is exposed again and further etched.
[0140] Furthermore, in the first removal step S2, the above-mentioned isotropic etching, formation of a protective film, and anisotropic etching are repeated until lattice-shaped grooves that penetrate the workpiece 11 and have their bottom surfaces located on the support substrate 33 are formed in the laminate 35 (see FIG. 18(A)). Note that FIG. 18(A) is a partially enlarged cross-sectional view that typically shows the locations of the laminate 35 where the grooves have been formed.
[0141] In addition, the first portion to be removed 11d is removed together with the multiple modified regions 21 and multiple cracks 23 contained therein. However, among the multiple cracks 23, the portions that extend from the first portion to be removed 11d and are formed in the intermediate portion 11f and the multiple second portions to be removed 11e remain. With the above, the first removal step S2 is completed.
[0142] After the first removal step S2 is performed, a second removal step S3 is performed. Fig. 18(B) is a cross-sectional view showing a schematic diagram of a stack 35 including a plurality of chips 41 manufactured in the second removal step S3.
[0143] This second removal step S3 is performed, for example, by grinding the back sides of the chips 41 until the second removed portions 11e are removed in the grinding device 30. Note that this grinding is performed in the same manner as the above-mentioned second removal step S3, and therefore a detailed description thereof will be omitted.
[0144] Here, when the backsides of the chips 41 are ground until the cracks 23 are exposed on each backside, the chips 41 are cleaved with the cracks 23 as boundaries. In other words, the peripheral edge of the backside of each of the chips 41 is separated from each chip 41 during this grinding. This completes the second removal step S3.
[0145] In addition, the structures and methods according to the above-described embodiments can be modified as appropriate without departing from the scope of the present invention. [Explanation of symbols]
[0146] 1: Frame unit 2: Laser processing equipment 4: Chuck table 6: Laser beam irradiation unit 8: Laser oscillator 10: Attenuator 11: Workpiece (11a: front side, 11b: back side, 11c: notch) (11d: 1st removed part, 11e: 2nd removed part, 11f: intermediate part) 12: Branch unit 13: Device 14: Mirror 15: Frame (15a: Opening) 16: Head 17: Dicing tape 18: Imaging unit 19: Protective tape 20: Cutting equipment 21: Modification area 22: Chuck table 23: Crack 24: Cutting unit 25: Groove 26: Spindle 27: Tip 28:Cutting blade 29: Protective tape 30: Grinding equipment 31: Groove 32: Chuck table 33: Support substrate (33a: front side, 33b: back side) 34: Grinding unit 35: Laminate 36: Spindle 37: Mask 38: Wheel mount 39: Groove 40: Grinding wheel (40a: wheel base, 40b: grinding stone) 41: Tip 42: Dry etching equipment 44: chamber (44a: loading / unloading port, 44b: exhaust port) 46: Gate valve 48:Plumbing 50: Exhaust system 52: Support member 54: table (54a: electrode) 56: Matching box 58: High frequency power supply 60: Bearing 62: Gas ejection head (62a: gas diffusion space, 62b: gas outlet, 62c, 62d: gas supply port) 64: Matching box 66:High frequency power supply 68a, 68b: Piping 70a, 70b: Gas supply source
Claims
1. A method for manufacturing a chip, comprising the steps of: manufacturing a plurality of chips, each of which is thinner than a workpiece having a plurality of devices formed on a front side thereof, by removing a first removal portion located around each of the plurality of devices and a plurality of second removal portions located on a back side of the plurality of devices, the method comprising the steps of: an internal processing step of irradiating the first removed portion with a laser beam having a wavelength that transmits through the workpiece to form a plurality of modified regions each located in the first removed portion and a plurality of cracks each extending from the plurality of modified regions so as to reach one of the plurality of second removed portions through one of a plurality of intermediate portions located between the plurality of devices and the plurality of second removed portions; a first removing step of removing the first removed portion after performing the internal processing step; a second removing step of, after carrying out the first removing step, grinding and removing the second removed portions and separating the respective rear surface side peripheral portions from the chips at the cracks as boundaries; A method for manufacturing a chip comprising the steps of:
2. In the internal processing step, the laser beam is irradiated onto the workpiece so as to form a plurality of focal points; 2. The method for manufacturing a chip according to claim 1, wherein the plurality of focal points are formed at different positions in both the thickness direction of the workpiece and the direction perpendicular to the thickness direction.
3. The method for manufacturing a chip as described in claim 1 or 2, further comprising a bonding step of bonding the multiple devices to a supporting substrate so that the multiple second removed portions are exposed before performing the internal processing step, after performing the internal processing step and before performing the first removal step, or after performing the first removal step and before performing the second removal step.