Method for producing calcium carbonate

By extracting calcium ions from a calcium-containing substance with a strong acid and weak base solution and mixing with carbon dioxide at a specific ratio, the method produces vaterite-rich calcium carbonate, addressing the strength issues of calcite and enhancing concrete properties.

JP2024152191APending Publication Date: 2024-10-25TAIHEIYO CEMENT CORP +1

Patent Information

Application Number
JP2023066234
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-14
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Conventional methods for producing calcium carbonate result in the stable calcite form, which decreases the strength of concrete when used as a mixture or admixture, while vaterite, the least stable form, is desirable for improved concrete properties.

Method used

A method involving the extraction of calcium ions from a calcium-containing substance using an aqueous solution of a strong acid and weak base, followed by mixing with carbon dioxide gas at a specific molar ratio (0.5 to 9) to produce vaterite-rich calcium carbonate.

Benefits of technology

The method allows for the production of vaterite-rich calcium carbonate with enhanced kneading properties, preventing a decrease in concrete strength and enabling its use in various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152191000002
    Figure 2024152191000002
  • Figure 2024152191000003
    Figure 2024152191000003
  • Figure 2024152191000004
    Figure 2024152191000004
Patent Text Reader

Abstract

To provide a method for producing calcium carbonate rich in vaterite.SOLUTION: A method for producing calcium carbonate rich in vaterite comprises the steps of: extracting calcium ions from a calcium-containing substance by bringing an aqueous solution containing a strong acid and a salt of a weak base into contact with the calcium-containing substance; and producing calcium carbonate by bringing a calcium ion extraction liquid into contact with a gas containing carbon dioxide gas at a ratio of the molar ratio of carbon dioxide gas to calcium ions (CO2 / Ca2+) of 0.5 to 9.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing calcium carbonate from a calcium-containing material. [Background technology]

[0002] Methods for immobilizing carbon dioxide include, for example, (1) chemical immobilization, (2) biological immobilization, and (3) isolation and storage. In order to put carbon dioxide immobilization into practical use, it is important that it is simple and low-cost, that it can be immobilized as a chemically stable substance, and that the substance obtained by immobilization can be effectively used. From this perspective, chemical immobilization methods, particularly the method of contacting alkaline earth metals with carbon dioxide to immobilize it as a carbonate, are considered to be promising methods because the carbonates produced are stable and harmless.

[0003] A method has been proposed in the past in which, for example, an alkaline earth metal-containing substance is brought into contact with an aqueous solution obtained from a salt of a weak base and a strong acid to transfer the alkaline earth metal into the aqueous solution, and then this aqueous solution is brought into contact with a gas containing carbon dioxide to produce carbonates such as calcium carbonate (Patent Document 1). Also proposed is a method in which calcium-containing waste is finely divided, the finely divided waste is added to water under a predetermined carbon dioxide partial pressure to extract calcium ions, a liquid containing calcium ions is separated from the residue, the separated liquid is mixed with calcium carbonate seed crystals, and calcium carbonate is precipitated from the mixed liquid under a predetermined carbon dioxide partial pressure (Patent Document 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2005-97072 A [Patent Document 2] JP 2006-69860 A Summary of the Invention [Problem to be solved by the invention]

[0005] Calcium carbonate exists in three crystal polymorphs: calcite, which is a rhombohedral crystal, aragonite, which is a rod-shaped crystal, and vaterite, which is a spherical crystal. At room temperature and pressure, calcite is the stable phase, and vaterite is known to be the most unstable of the three. The calcium carbonate produced by the above-mentioned conventional chemical fixation methods is stable calcite, but the present inventors have found that there is a problem in that the strength of concrete decreases when calcite is used in a large amount as a mixing material or admixture for concrete. An object of the present invention is to provide a method for producing vaterite-rich calcium carbonate. [Means for solving the problem]

[0006] The present inventors contacted a calcium-containing substance with an aqueous solution containing a salt of a strong acid and a weak base to extract calcium ions from the calcium-containing substance, and then mixed the calcium ion extract with a gas containing carbon dioxide at a molar ratio of calcium ions to carbon dioxide (CO2 / Ca 2+ ) in a specific range, it has been unexpectedly found that a stable calcium carbonate rich in vaterite is produced.

[0007] That is, the present invention provides the following [1] to [5]. [1] A step of contacting a calcium-containing substance with an aqueous solution containing a salt of a strong acid and a weak base to extract calcium ions from the calcium-containing substance; The calcium ion extract and the gas containing carbon dioxide were mixed at a molar ratio of calcium ion to carbon dioxide (CO2 / Ca 2+ ) is 0.5 to 9 to produce calcium carbonate A method for producing vaterite-rich calcium carbonate, comprising: [2] The manufacturing method according to [1] above, wherein the calcium-containing material comprises waste concrete, ready-mix concrete sludge, kiln dust, fly ash, incineration ash, or rocks mainly composed of one or more selected from calcium silicate, calcium phosphate, and calcium aluminate. [3] The method according to [1] or [2] above, wherein the salt of a strong acid and a weak base comprises a salt of an inorganic strong acid and one or more weak bases selected from ammonia and organic amines. [4] The method for producing a carbon dioxide gas according to any one of [1] to [3] above, wherein the gas containing carbon dioxide gas includes an exhaust gas discharged from a production facility. [5] The method according to any one of [1] to [4] above, wherein the calcium carbonate contains 30% or more of vaterite. Effect of the Invention

[0008] According to the present invention, vaterite-rich calcium carbonate can be produced by a simple operation. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a diagram showing diffraction patterns measured by X-ray diffraction for calcium carbonate obtained in Examples 1 to 4 and Comparative Example 1. [Diagram 2] FIG. 1 is a diagram showing an electron microscope image of calcium carbonate obtained in Example 3. [Diagram 3] FIG. 2 is a diagram showing an electron microscope image of calcium carbonate obtained in Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The method for producing calcium carbonate according to the present invention is characterized by comprising a calcium ion extraction step and a calcium carbonate production step. Each step will be described in detail below.

[0011] [Calcium ion extraction process] This step is a step of extracting calcium ions from a calcium-containing substance by contacting the calcium-containing substance with an aqueous solution containing a salt of a strong acid and a weak base, thereby enabling efficient extraction of calcium ions from the calcium-containing substance.

[0012] An aqueous solution containing a salt of a strong acid and a weak base (hereinafter also simply referred to as an "aqueous solution") may be prepared by dissolving a strong acid and a weak base in water, or by dissolving a salt formed from a strong acid and a weak base in water. Examples of water include pure water, tap water as specified in JIS A 5303 Appendix C, and water other than tap water (e.g., river water, lake water, well water, groundwater, industrial water). In addition, the water may be any of cooling water, room temperature water, and hot water, and is not particularly limited.

[0013] The strong acid may be, for example, an inorganic strong acid or an organic strong acid. One or more kinds of strong acids may be used. Examples of strong inorganic acids include hydrochloric acid, sulfuric acid, nitric acid, chromic acid, permanganic acid, hydroiodic acid, hydrobromic acid, perchloric acid, chloric acid, iodic acid, and bromic acid. Examples of the strong organic acid include metasulfonic acid, trifluoromethasulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, and camphorsulfonic acid. Among these, strong inorganic acids are preferred, and hydrochloric acid, sulfuric acid, and nitric acid are more preferred.

[0014] Examples of the weak base include ammonia, metal hydroxides, hydrazine derivatives, and organic amines. One or more types of weak bases can be used. Examples of metal hydroxides include magnesium hydroxide, iron hydroxide, copper hydroxide, and zinc hydroxide. Examples of the hydrazine derivative include hydrazine, methylhydrazine, and ethylhydrazine.

[0015] In this specification, the term "organic amine" is a general term for aliphatic amines, alicyclic amines, heterocyclic amines, and aromatic amines. Examples of the aliphatic amine include alkylamines and alkyl alcoholamines. The number of carbon atoms in the alkyl group is preferably 1 to 10, and more preferably 1 to 5. Specific examples include monoalkylamines such as methylamine, ethylamine, isopropylamine, n-butylamine, and n-hexylamine; dialkylamines such as diethylamine, di-n-propylamine, and di-n-heptylamine; trialkylamines such as trimethylamine, triethylamine, and tri-n-propylamine; and alkyl alcoholamines such as diethanolamine, triethanolamine, diisopropanolamine, and triisopropanolamine. Other examples include tris(2-methoxymethoxyethyl)amine, tris[2-{2-(2-hydroxyethoxy)ethoxy}ethyl]amine, and triethanolamine triacetate. The alicyclic amine may be an aliphatic monocyclic amine or an aliphatic polycyclic amine. Specific examples include aliphatic monocyclic amines such as bis(aminomethyl)cyclohexane and isophoronediamine, and aliphatic polycyclic amines such as dicyclohexyldiamine and methylenebis(aminocyclohexane). Examples of heterocyclic amines include morpholine, piperazine, and piperidine. These may be substituted with an alkyl group, and the number of carbon atoms in the alkyl group is preferably 1 to 10, and more preferably 1 to 5. Examples of aromatic amines include aniline, benzylamine, toluidine, diaminotoluene, benzidine, and phenylenediamine. The aromatic amine may be a heterocyclic aromatic amine, and examples of the heterocyclic aromatic amine include pyridine, pyrimidine, quinoline, and benzimidazole.

[0016] Among them, the weak base is preferably one or more selected from ammonia and organic amines, and more preferably an organic amine.

[0017] Suitable salts formed from strong acids and weak bases include, for example, Cl - , SO4 2- , NO3 - and HSO4 - and one or more cations selected from ammonium ions, primary aminium cations, secondary aminium cations, and tertiary aminium cations. Specific examples include ammonium chloride, methylamine hydrochloride, ethanolamine hydrochloride, diethanolamine hydrochloride, and triethanolamine hydrochloride.

[0018] The amounts of the strong acid and the weak base used may be any amounts that satisfy the stoichiometric composition of the salt formed by the strong acid and the weak hydrochloric acid. From the viewpoint of calcium extraction efficiency, the salt concentration in the aqueous solution is preferably 0.01 mol / L or more, more preferably 0.1 mol / L or more, even more preferably 0.5 mol / L or more, and preferably 5 mol / L or less, more preferably 3 mol / L or less, even more preferably 2 mol / L or less.

[0019] The calcium-containing substance is not particularly limited as long as it contains calcium, but examples thereof include waste materials, by-products discharged in manufacturing processes, and natural minerals. One or more calcium-containing substances can be used. Examples of waste materials include waste concrete and ready-mixed concrete sludge. Examples of waste concrete include dismantled concrete generated during civil engineering works or the demolition of structures, and surplus concrete generated during the construction of buildings, etc. The waste concrete also includes concrete from which the cement components have been separated and recovered. The ready-mixed concrete sludge may be, for example, concrete sludge water discharged from washing a concrete mixer in a concrete or concrete product factory, or from washing a ready-mixed concrete transport vehicle. The ready-mixed concrete sludge may have an adjusted solid-liquid ratio, which is, for example, preferably 0.001 to 5 mass%, more preferably 0.01 to 2 mass%, and even more preferably 0.01 to 0.2 mass%. The "solid-liquid ratio" here refers to the ratio of the solid content to the mass of the liquid content.

[0020] Examples of by-products discharged in the manufacturing process include kiln dust, fly ash, and incineration ash. Examples of kiln dust include gas discharged from the bottom of a cement kiln, or dust collected by a bag filter or the like from combustion gas discharged from a cyclone at the top of a cement manufacturing facility. Examples of fly ash include coal ash generated by the combustion of pulverized coal at a thermal power plant or the like and collected by an electric dust collector or the like. In addition, clinker ash and biomass ash generated by the combustion of pulverized coal or biomass at a thermal power plant or the like can also be used. Examples of incineration ash include incineration ash of urban waste, sludge (e.g., urban underground sludge, water purification plant sludge), and paper sludge incineration ash.

[0021] Examples of natural minerals include rocks mainly composed of one or more selected from calcium silicate, calcium phosphate, and calcium aluminate. Specific examples include wollastonite, olivine, serpentine, anorthite, anorthite, augite, and diopside.

[0022] Among these, the calcium-containing substance preferably includes waste concrete, ready-mixed concrete sludge, kiln dust, fly ash, incineration ash, or rocks mainly composed of one or more selected from calcium silicate, calcium phosphate, and calcium aluminate, more preferably includes waste concrete, ready-mixed concrete sludge, kiln dust, fly ash, or incineration ash, and even more preferably includes waste concrete, ready-mixed concrete sludge, kiln dust, or fly ash.

[0023] From the viewpoint of calcium ion extraction efficiency and impurity removal, the calcium-containing substance preferably has a small particle size. In order to adjust the calcium-containing substance to a desired particle size, one or more selected from crushing, grinding, and sieving can be performed. A known crusher can be used for crushing, and a screen can be attached to the crusher to adjust to a desired particle size. In addition, a known crusher can be used for crushing, and a known sieve separator can be used for sieving. When waste concrete or ready-mixed concrete sludge is used as the calcium-containing substance, aggregate can also be removed by performing such a process.

[0024] The size of the calcium-containing substance after particle size adjustment can be appropriately selected, but from the viewpoint of calcium ion extraction efficiency and impurity removal, the maximum particle size is preferably less than 2 mm, more preferably less than 1 mm, and even more preferably less than 0.5 mm. The "maximum particle size" here refers to the particle size represented by the smallest mesh size of a sieve through which the entire sample passes.

[0025] The calcium-containing substance may be contacted with the aqueous solution by immersing the calcium-containing substance in the aqueous solution, or may be stirred to promote extraction of calcium ions. When stirring, the stirring speed can be appropriately set, but is usually 50 to 2000 rpm, and preferably 100 to 1000 rpm. The order of adding the calcium-containing substance and the aqueous solution containing a salt is not particularly limited.

[0026] From the viewpoint of extraction efficiency of calcium ions, the mixing ratio of the calcium-containing substance to the aqueous solution containing a salt is preferably 1 or more, more preferably 2 or more, even more preferably 4 or more, and preferably 10 or less, more preferably 8 or less, even more preferably 5 or less, in terms of the molar ratio (salt / calcium) of calcium in the calcium-containing substance to salt in the aqueous solution.

[0027] The contact temperature is preferably from room temperature to 100°C, more preferably from 20 to 90°C, and further preferably from 30 to 85°C, from the viewpoints of calcium ion extraction efficiency and energy efficiency. From the viewpoint of calcium ion extraction efficiency, the contact time is preferably 5 minutes or more, more preferably 10 minutes or more, and even more preferably 15 minutes or more, and from the viewpoint of production efficiency, the contact time is preferably 120 minutes or less, more preferably 60 minutes or less, and even more preferably 40 minutes or less. The calcium-containing substance may be contacted with the aqueous solution at normal pressure, and there is no need to apply pressure or reduce pressure.

[0028] After the completion of this step, and before the calcium carbonate production step, the aqueous solution after this step may be subjected to solid-liquid separation to remove water-insoluble matters (solid matters not dissolved in the aqueous solution). This can increase the purity of calcium carbonate produced in the next step. For solid-liquid separation, a known method can be adopted, and examples thereof include filtration, centrifugation, and decantation.

[0029] [Calcium carbonate production process] In this step, the calcium ion extract obtained in the calcium ion extraction step and a gas containing carbon dioxide are mixed at a molar ratio of calcium ion to carbon dioxide (CO2 / Ca 2+ ) is 0.5 to 9 to produce calcium carbonate.

[0030] The inventors have 2+It was found that the molar ratio of CO2 / Ca is closely related to the crystal polymorphism of the calcium carbonate produced. 2+ It was found that when the molar ratio of CO2 / Ca is within a specific range of 0.5 to 9, the formation of vaterite is promoted and the stability is excellent even if the vaterite is abundant. 2+ If the molar ratio of calcium ions to carbon dioxide (CO2 / Ca) exceeds 9, calcite is specifically formed, while if it is less than 0.5, the amount of calcium carbonate produced and the amount of vaterite produced are insufficient. 2+ ) is preferably 0.5 or more, more preferably 1 or more, and even more preferably 1.5 or more from the viewpoint of promoting the production of vaterite, and is preferably 9 or less, more preferably 7 or less, and even more preferably 6 or less from the viewpoint of suppressing the production of calcite.

[0031] The gas containing carbon dioxide is not limited to high-purity carbon dioxide, and any gas containing carbon dioxide can be used. Examples of the gas include the breath of living organisms, carbon dioxide in the atmosphere, exhaust gas from automobiles, and exhaust gas discharged from manufacturing facilities. Examples of manufacturing facilities include plants (e.g., steel plants and cement plants) and thermal power plants. When exhaust gas discharged from manufacturing facilities is used as the gas containing carbon dioxide, the exhaust gas may be passed through an adsorption filter or the like to remove dust and the like before contact. Gases containing carbon dioxide also include gases other than carbon dioxide, such as SO x , NO x It is okay if it contains:

[0032] The method of contacting the calcium ion extract with the gas containing carbon dioxide is not particularly limited, but examples include a method of bubbling (blowing) the gas containing carbon dioxide into the calcium ion extract, and a method of sealing the calcium ion extract and the gas containing carbon dioxide in the same container and shaking the container.

[0033] From the viewpoint of promoting the production of vaterite, the contact temperature is preferably from room temperature to 80°C, more preferably from 20 to 60°C, and further preferably from 20 to 50°C. The contact time is the time required to separate the carbon dioxide-containing gas into the desired CO2 / Ca 2+ There is no particular limitation as long as the components can be supplied in this molar ratio. When bubbling a gas containing carbon dioxide into the calcium ion extract, the supply rate of the gas containing carbon dioxide can be appropriately set. From the viewpoint of production efficiency, however, it is preferable to set the supply rate of the gas containing carbon dioxide to 0.01 (CO2 / Ca 2+ ) / min or more, and more preferably 0.05(CO2 / Ca 2+ ) / min or more, and more preferably 0.08(CO2 / Ca 2+ ) / min or more, and preferably 5(CO2 / Ca 2+ ) / min or less, and more preferably 1(CO2 / Ca 2+ ) / min or less, and more preferably 0.5(CO2 / Ca 2+ ) / min or less.

[0034] After the contact with the gas containing carbon dioxide is stopped, the reaction liquid is subjected to solid-liquid separation, and vaterite-rich calcium carbonate can be recovered. For solid-liquid separation, a known method can be adopted, and examples thereof include filtration, centrifugation, and decantation.

[0035] The calcium carbonate produced by the chemical immobilization method of the present invention is rich in vaterite. Specifically, the ratio of vaterite in calcium carbonate is usually 30% or more, preferably 35% or more, more preferably 50% or more, even more preferably 60% or more, and even more preferably 70% or more. The upper limit of the ratio of vaterite in calcium carbonate is not particularly limited, and may be 100%. Here, in this specification, the "ratio of vaterite in calcium carbonate" is analyzed by the method described in the Examples below.

[0036] Calcium carbonate produced by the conventional chemical fixation method has a calcite crystal structure and has a pointed shape as shown in Figure 3, so that it has poor kneadability when used as a concrete admixture or mineral admixture. Therefore, if calcite is used in large amounts as a concrete admixture or mineral admixture, the concrete strength decreases. In contrast, calcium carbonate produced by the chemical fixation method of the present invention is a spherical buterite as shown in Figure 2, so that it has excellent kneadability when used as a concrete admixture or mineral admixture, and can suppress the decrease in concrete strength. Therefore, calcium carbonate produced by the chemical fixation method of the present invention is a harmless and stable substance with excellent kneadability, and can be used in various applications, such as cement raw material, steelmaking auxiliary material, refractory raw material, papermaking filler, soil improvement material, fertilizer, essential raw material used in various environmental purification processes, filler for rubber, plastic, paper, etc., and various industrial raw materials. EXAMPLES

[0037] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the following examples.

[0038] 1. Identification of the crystal phase of calcium carbonate Measurements were performed using an X-ray diffraction measurement device (Bruker D8 advance, manufactured by Bruker AXS Co., Ltd.) in accordance with powder X-ray diffraction measurement methods, and the crystalline phases were identified from the diffraction patterns.

[0039] 2. Proportion of vaterite in calcium carbonate The proportion of vaterite was calculated from the following formula based on the diffraction line intensity shown on the vertical axis of a diffraction chart obtained by powder X-ray diffraction measurement.

[0040] Percentage of vaterite (%) = (I 110(V) +I 112(V) +I 114(V) )÷(I 110(V)+I 112(V) +I 104(C) +I 114(V) ) x 100 [In the formula, I 110(V) indicates the diffraction intensity of the vaterite 110 plane, and I 112(V) indicates the diffraction intensity of the vaterite 112 plane, and I 114(V) indicates the diffraction intensity of the vaterite 114 plane, and I 104(C) indicates the diffraction intensity of the calcite 104 plane.

[0041] Examples 1 to 4 and Comparative Example 1 (1) Preparation of an aqueous solution containing a salt of a strong acid and a weak base 90 mL of commercially available hydrochloric acid (35 wt%) and 107.21 g of diethanolamine were placed in a 1 L measuring flask and diluted with pure water. The molar ratio of hydrochloric acid to amine (hydrochloric acid / amine) was 1.0. (2) Calcium ion extraction process 120 mL of the aqueous solution prepared in (1) and 14.0 g of concrete powder (grain size less than 1 mm) were added to a 300 mL flask and stirred to form a slurry. The mixture was then stirred at 500 rpm for 30 minutes in a water bath at 80°C. After stirring, solid-liquid separation was performed by suction filtration to obtain a calcium ion extract. (3) Calcium carbonate production process 85 mL of the calcium ion extract obtained in (2) was added to the flask, and carbon dioxide gas (concentration: 100%) was supplied by bubbling at a flow rate of 90 mL / min at a temperature of 40°C for the time shown in Table 1. 2+ The molar ratios of are shown in Table 1. After bubbling was completed, the precipitate was subjected to solid-liquid separation. The obtained solid was dried overnight in a vacuum, and then the crystal phase was identified using a powder X-ray diffractometer, and the proportion of vaterite was calculated. The results are shown in Table 1. The X-ray diffraction patterns of the solids obtained in each Example and Comparative Example are shown in FIG. 1. In addition, the particle shapes of the solids obtained in Example 3 and Comparative Example 1 were observed using an electron microscope. The results of Example 3 are shown in FIG. 2, and the results of Comparative Example 1 are shown in FIG. 3.

[0042] [Table 1]

[0043] Calcium ion extract, CO2 / Ca 2+ It can be seen that by blowing in carbon dioxide gas at a molar ratio of 0.5 to 9, calcium carbonate rich in the vaterite phase can be specifically obtained. The calcium carbonate obtained in Examples 1 to 4 were all aggregates composed of spherical primary particles having a particle size of 100 nm or less, whereas the calcium carbonate obtained in Comparative Example 1 was an aggregate composed of pointed primary particles having a particle size of 2 to 5 μm.

Claims

1. a step of contacting a calcium-containing substance with an aqueous solution containing a salt of a strong acid and a weak base to extract calcium ions from the calcium-containing substance; The calcium ion extract and the gas containing carbon dioxide were mixed at a molar ratio of calcium ion to carbon dioxide (CO 2 / Ca 2+ ) in a ratio of 0.5 to 9 to produce calcium carbonate. A method for producing vaterite-rich calcium carbonate, comprising:

2. 2. The method according to claim 1, wherein the calcium-containing material comprises waste concrete, ready-mix concrete sludge, kiln dust, fly ash, incineration ash, or rocks mainly composed of one or more selected from calcium silicate, calcium phosphate, and calcium aluminate.

3. The method according to claim 1, wherein the salt of a strong acid and a weak base comprises a salt of a strong inorganic acid and one or more weak bases selected from ammonia and organic amines.

4. The method according to claim 1, wherein the gas containing carbon dioxide gas includes exhaust gas discharged from a production facility.

5. The method according to any one of claims 1 to 4, wherein the calcium carbonate contains 30% or more of vaterite.

Citation Information

Patent Citations

  • Method for fixing carbon dioxide

    JP2005097072A

  • Method for producing high purity calcium carbonate from calcium-containing waste

    JP2006069860A

Cited By

  • Vinyl-chloride-based resin mixture containing calcium carbonate, and production method therefor

    WO2026221104A1