Iridium-manganese oxide composite electrode and production method thereof
The iridium-manganese oxide composite electrode addresses the scarcity and cost of iridium by providing a cost-effective and efficient oxygen-generating catalyst for water electrolysis, enhancing durability and enabling the production of hydrogen and hydrocarbon compounds.
Patent Information
- Application Number
- JP2023066489
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2024-10-25
AI Technical Summary
The scarcity and high cost of iridium, a highly active oxygen-generating electrode catalyst, limit its availability for widespread use in water electrolysis, necessitating the development of a more affordable and efficient alternative with comparable catalytic activity.
A composite electrode composed of iridium-manganese oxide coated on a conductive base material, particularly a platinum-coated titanium powder sintered body, enhances oxygen-generating electrocatalytic activity and durability, suitable for alkaline, neutral, or acidic conditions, and solid polymer membrane (PEM) type electrolyzers.
The iridium-manganese oxide composite electrode exhibits high oxygen-generating activity and durability, reducing production costs while maintaining performance in industrial water electrolysis, and can also reduce carbon dioxide to produce hydrocarbon compounds.
Smart Images

Figure 2024152347000003 
Figure 2024152347000004 
Figure 2024152347000005
Abstract
Description
[Technical field]
[0001] The present invention relates to an iridium-manganese oxide composite electrode and a method for producing the same, and more particularly to an iridium-manganese oxide composite electrode used as an anode catalyst for oxygen evolution in industrial water electrolysis carried out under alkaline, neutral or acidic conditions or in water electrolysis using a polymer electrolyte membrane (PEM) type electrolytic cell, and a method for producing the same. [Background technology]
[0002] Due to the problems of fossil fuel depletion and environmental pollution, attention has been focused on the use of hydrogen as a clean energy source and methods for producing it. Water electrolysis is one of the effective means of electrolyzing water to produce high-purity hydrogen gas from the cathode, but is characterized by the fact that oxygen is simultaneously generated from the counter anode. In order to efficiently proceed with the water splitting reaction in water electrolysis, it is necessary to use an electrode catalyst with low hydrogen overvoltage at the cathode and an electrode catalyst with low oxygen overvoltage at the anode, and to electrolyze the water while keeping the electrolysis voltage low. Among these, rare platinum group metals such as platinum (Pt), iridium (Ir), and ruthenium (Ru), as well as compounds including oxides containing these elements, have been proposed as electrode catalyst materials with excellent low oxygen overvoltage at the anode (Patent Documents 1 and 2, Non-Patent Documents 1 to 3).
[0003] Among these, iridium (Ir) is widely known as an extremely active oxygen-evolving electrode catalyst; however, compared to other precious metals, its reserves are extremely small, and due to its uneven distribution in specific regions, its global production is also very small. As a result, there are fears that even if water electrolysis technology becomes widespread in the future, there will not be enough catalysts to meet the demand (Non-Patent Document 4). Since such platinum group metal-based electrode catalysts are very expensive, development of alternative electrode catalysts using inexpensive transition metals has been promoted. For example, transition metal materials composed of manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), etc. have been proposed in recent years (Patent Documents 3 to 5, Non-Patent Documents 5 to 8).
[0004] Until recently, no oxygen evolution electrode catalyst material had been developed that was composed of inexpensive transition metals and had high catalytic activity comparable to that of platinum group metals such as Pt and Ir. In response to this issue, however, an electrode catalyst was discovered that combines low cost with catalytic activity comparable to that of platinum group metals by introducing a small amount of Ir into manganese oxide (Patent Document 6). However, in order to put it into practical use, there is a need to develop electrodes that enable operation at even higher current densities. Therefore, there has been a need to develop electrodes that can show high current densities at low electrolysis voltages, even if the catalyst material is mainly made of transition metals. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 8-269761 [Patent Document 2] Special Publication No. 2007-514520 [Patent Document 3] JP 2015-192993 A [Patent Document 4] International Publication (WO) 2009 / 154753 [Patent Document 5] International Publication (WO) 2019 / 117199 [Patent Document 6] International Publication (WO) 2022 / 264960 [Non-patent literature]
[0006] [Non-Patent Document 1] S. Trasatti, G. Buzzanca, J. Electroanal. Chem., 1971, 29, A1. [Non-Patent Document 2] A. Harriman, IJPickering, JMThomas, PA Christensen, J. Chem. Soc., Faraday Trans. 1, 1988, 84, 2795. [Non-Patent Document 3] Y. Zhao,NMVargas-Barbosa,EAHernandez-Pagan,TEMallouk,Small,2011,7,2087. [Non-Patent Document 4] F. Birol, World Energy Outlook 2016, International Energy Agency (IEA), Paris, 2016. [Non-Patent Document 5] MMNajafpour, G. Renger, M. Holynska, ANMoghaddam, E.-M. Aro, R. Carpentier, H. Nishihara, JJ Eaton-Rye, J.-R. Shen, SIAllakhverdiev, Chem.Rev.,2016,116,2886. [Non-Patent Document 6] T. Takashima, K. Ishikawa, H. Irie, J. Phys. Chem. C, 2016, 120, 24827. [Non-Patent Document 7] JBGerken,JGMcAlpin,JYCChen,MLRigsby,WHCasey,RDBritt,SSStahl,J.Am.Chem.Soc.,2011,133,14431. [Non-Patent Document 8] M.Dinca,Y.Surendranath,DGNocera,Proc.Natl.Acad.Sci.USA,2010,107,10337. Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide an electrode comprising an iridium-manganese oxide composite material and a conductive substrate, and a method for producing the same. More specifically, the present invention relates to an iridium-manganese oxide composite electrode obtained using an iridium-manganese oxide composite material (hereinafter sometimes referred to as iridium-manganese oxide) for water splitting catalyst, which is an electrode for oxygen evolution in industrial water electrolysis performed under alkaline, neutral or acidic conditions or in water electrolysis using a polymer electrolyte membrane (PEM) type electrolytic cell, and which is less expensive than current iridium catalyst systems and has high oxygen evolution electrode catalytic activity, and to a method for producing the same. [Means for solving the problem]
[0008] The present inventors have discovered that an iridium-manganese oxide composite electrode in which a conductive base material made of a sintered powder is at least partially coated exhibits particularly high oxygen evolution electrode catalytic activity and durability, leading to the completion of the present invention. That is, the present invention is as defined in the claims and its gist is as follows.
[0009] [1] An iridium-manganese oxide composite electrode in which an iridium-manganese oxide composite material covers at least a portion of a conductive substrate made of a sintered powder body. [2] The iridium-manganese oxide composite material has a concentration of 0.1 mg / cm per geometric area of the conductive substrate. 2 More than 25mg / cm 2 The iridium-manganese oxide composite electrode [1] above is coated with the following: [3] The iridium-manganese oxide composite electrode according to the above [1] or [2], wherein the conductive substrate is a platinum-coated titanium powder sintered body. [4] A membrane / electrode assembly comprising the iridium-manganese oxide composite electrode according to any one of the above [1] to [3] and a polymer electrolyte membrane. [5] A water electrolysis device having any one of the iridium-manganese oxide composite electrodes [1] to [3] above. [6] A water electrolysis device comprising the membrane / electrode assembly according to [4] above. [7] A method for producing hydrogen by electrolysis of water using the iridium-manganese oxide composite electrode according to any one of [1] to [3] above. [8] A method for producing hydrogen by electrolysis of water using the membrane / electrode assembly described above in [4]. Effect of the Invention
[0010] The iridium-manganese oxide composite electrode of the present invention exhibits high activity and durability in industrial water electrolysis performed under alkaline, neutral, or acidic conditions, or in water electrolysis using a PEM-type electrolytic cell, and functions as an inexpensive and excellent electrode for oxygen generation. Furthermore, by adding carbon dioxide to the electrolysis system using the iridium-manganese oxide composite electrode of the present invention, the carbon dioxide or the like can be reduced at the cathode to produce hydrocarbon compounds (formic acid, formaldehyde, methanol, methane, ethane, propane, etc.). [Brief description of the drawings]
[0011] [Figure 1] 1 is a cross-sectional SEM photograph of a composite electrode made of an iridium-manganese oxide and a sintered body of platinum-coated titanium powder in Example 1. [Diagram 2] 1 is a linear sweep voltammogram showing the relationship between current and potential (voltage) measured using a PEM water electrolysis cell during oxygen generation (water electrolysis) in Example 1 and Comparative Example 1. [Diagram 3] 1 shows data showing time progression of electrolysis voltage measured at a temperature of 80° C. and a current density of 2 A cm −2 using a PEM water electrolytic cell during oxygen generation (during water electrolysis) in Example 1 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will now be described in further detail. First, we will explain the decomposition of water by electrolysis by taking as an example a reaction in which the reaction field is in an acidic environment, such as PEM-type water electrolysis. On the cathode catalyst, hydrogen is produced by the reaction of two protons and two electrons, as shown in formula 1. 2H + + 2e - → H2… Equation 1 Meanwhile, on the anode catalyst, oxygen is produced from two water molecules along with four electrons and four protons, as shown in Equation 2. 2H2O → O2+ 4H + + 4e - … Formula 2 Overall, the reaction produces two hydrogen molecules and one oxygen molecule from two water molecules, as shown in equation 3. 2H2O → 2H2+ O2… Equation 3 The oxygen evolution reaction in the above formula 2 is generally considered to be the rate-limiting step of the entire reaction, and the development of a catalyst that can drive this reaction with minimal energy is of great importance in this technical field. The present invention provides an oxygen evolution electrode catalyst that has high water oxidation catalytic activity.
[0013] The iridium-manganese oxide composite electrode of the present invention is an iridium-manganese oxide composite material that covers at least a part of a conductive substrate made of a powder sintered body. The amount of the iridium-manganese oxide composite material coated is 0.1 mg / cm per geometric area of the conductive substrate. 2 More than 25mg / cm 2 The following is preferred: Here, the geometric area corresponds to the projected area of the conductive substrate, and the thickness of the substrate is not taken into consideration. When the coating amount of the iridium-manganese oxide composite material is within the above range, the iridium-manganese oxide composite material coats the sintered powder compact in an island-like manner or in a form that completely covers the outer surface, although this also depends on the porosity of the sintered powder compact that constitutes the conductive base material, and the average coating thickness can be 25 μm or less. Note that the iridium-manganese oxide composite material that coats the sintered powder compact is composed of secondary particles, so the average coating thickness and the iridium The average secondary particle size of the titanium-manganese oxide composite material is consistent with that of the titanium-manganese oxide composite material.
[0014] In the iridium-manganese oxide composite electrode of the present invention, the average thickness of the iridium-manganese oxide composite material coating the surface of the conductive substrate increases depending on the amount of coating iridium-manganese oxide composite material. In the iridium-manganese oxide composite electrode of the present invention, the conductive base material is composed of a powder sintered body. By the conductive base material being composed of a powder sintered body, the specific surface area is increased, and an iridium-manganese oxide composite electrode exhibiting high oxygen evolution electrode catalytic activity and durability can be obtained. Examples of the powder sintered body include at least one conductive powder selected from the group consisting of bronze, iron, aluminum, copper, nickel, Inconel, titanium metal, stainless steel, titanium oxide, molybdenum, tungsten, tantalum, zirconium boride, and platinum-coated titanium, and preferably titanium metal, titanium oxide, copper, stainless steel, platinum-coated titanium powder sintered body, etc. Among these, from the viewpoint of oxidation resistance, it is preferable that the conductive base material is composed of a platinum-coated titanium powder sintered body. The conductive substrate has a thickness of preferably 1 mm or less, more preferably 0.5 mm or less, and a flat shape. By controlling the thickness within this range, it is expected that the durability and the specific surface area will be improved. The conductive substrate has a porosity of preferably 20% or more, more preferably 30% or more and 60% or less.
[0015] The iridium-manganese oxide composite electrode of the present invention can impart catalytic ability in a water splitting reaction to an oxygen generating electrode by supporting an iridium-manganese oxide composite material as a catalytic material on a conductive substrate. A membrane-electrode assembly is formed by stacking an oxygen generating electrode containing this oxygen generating electrode active material, a polymer electrolyte membrane, and an electrode to which a hydrogen generating catalyst has been imparted. Here, the polymer electrolyte membrane refers to, for example, a fluorine resin-based cation exchange membrane, and the hydrogen generating catalyst refers to, for example, platinum fine particles. In the present invention, by having this oxygen generating electrode, the device becomes a water electrolysis device, and hydrogen can be produced by water electrolysis using this oxygen generating electrode.
[0016] In the iridium-manganese oxide composite material in the iridium-manganese oxide composite electrode of the present invention, the manganese oxide preferably has a manganese metal valence of 3.5 or more and 4.0 or less in order to stably disperse and allocate iridium. In the case of manganese oxide with a metal valence within this range, the chemical stability of the catalyst material is high, and particularly when used under acidic conditions such as PEM, elution as divalent manganese ions can be suppressed. The manganese oxide more preferably has a manganese metal valence of 3.6 or more and 4.0 or less, and even more preferably 3.7 or more and 4.0 or less.
[0017] The manganese oxide in the iridium-manganese oxide composite material may be, for example, electrolytic manganese dioxide obtained by an electrolytic method, or manganese dioxide obtained by a chemical method, with electrolytic manganese dioxide being preferred. Furthermore, the manganese oxide in the iridium-manganese oxide composite material may be a crystalline phase having a basic crystal structure of any of γ-type, β-type, ε-type, or α-type, or may be a mixed crystal manganese dioxide in which these crystal structures are mixed.
[0018] A method for producing an iridium-manganese oxide composite material is described below. An iridium-manganese oxide composite material can be obtained, for example, by electrolytically depositing manganese oxide onto an electrode substrate such as a pure titanium plate using a mixed solution containing sulfuric acid and manganese sulfate as an electrolyte, immersing the electrode in or contacting the electrode with an iridium salt solution, and then annealing the electrode. Manganese oxide may be electrolytically deposited using a mixed solution containing sulfuric acid and manganese sulfate, and then peeled off from the electrode substrate and crushed into a powder form. Regarding the concentration of each component in the mixed solution containing sulfuric acid and manganese sulfate, the sulfuric acid concentration is preferably controlled in the range of 5 g / L to 65 g / L, more preferably 20 g / L to 60 g / L. The concentration of manganese (manganese ion of manganese sulfate) in the mixed solution is not particularly limited as long as it is below the solubility, but is preferably 5 g / L or more and 50 g / L or less, and more preferably 10 g / L or more and 40 g / L or less.
[0019] In order to maintain the component concentrations of the above mixed solution, it is effective to appropriately add manganese sulfate equivalent to the manganese consumed in the electrolytic oxidation, or to continuously supply a manganese sulfate solution. The sulfuric acid concentration in the above-mentioned sulfuric acid-manganese sulfate mixed solution is a value excluding the divalent anion (sulfate ion) of manganese sulfate. In the electrolytic deposition method of manganese oxide for the iridium-manganese oxide composite material, the electrolytic current density is not particularly limited, but is preferably 0.3 mA / cm 2 More than 20mA / cm 2 It is preferable that the electrolytic current density is 1 mA / cm or less. This allows efficient and stable electrolytic deposition of manganese oxide. In order to obtain an iridium-manganese oxide composite material more stably, the electrolytic current density is 1 mA / cm or less. 2 More than 10mA / cm 2 Less than 3mA / cm is more preferable. 2 More than 8mA / cm 2 The following is even more preferred: The electrolysis temperature can be, for example, 93° C. or higher and 98° C. or lower. Since the higher the electrolysis temperature, the higher the efficiency of electrolytic production of precipitated manganese oxide, the electrolysis temperature is preferably at least 94° C. or higher.
[0020] Manganese oxide electrolytically deposited on an electrode substrate such as a pure titanium plate is peeled off from the electrode substrate, and then crushed and adjusted as a single manganese oxide to a predetermined average secondary particle size using a roller mill, vertical mill, Roche mill, jet mill, or the like. The produced manganese oxide is then washed and neutralized to remove residual electrolyte, and then dried using a flash dryer or the like. During this flash drying, fine powder of submicron-order manganese oxide produced as a by-product due to over-pulverization in the crushing process can be collected and separated using a dust collector bag filter, or the like. In some cases, a firing process at 200°C to 500°C is further performed to obtain manganese oxide.
[0021] The oxides of manganese are then immersed in a container containing the iridium salt solution or are brought into contact with the oxides of manganese and the iridium salt solution. The type of iridium salt in the iridium salt solution is exemplified by potassium hexachloroiridate (K2IrCl6) or hexachloroiridate (H2IrCl6). The iridium concentration of the iridium salt solution is not particularly limited as long as it is equal to or lower than the solubility, but is preferably 0.001 g / L or more and 10 g / L or less, and more preferably 0.003 g / L or more and 5 g / L or less. The conditions for immersing manganese oxide in an iridium salt solution or contacting manganese oxide with an iridium salt solution are not particularly limited, but examples include immersion or contact for 30 minutes to 24 hours at a temperature of 20° C. to 100° C. By keeping the immersion or contact time within the above range, the amount of iridium adsorbed onto the manganese oxide can be controlled.
[0022] Next, annealing is performed. The annealing temperature conditions are not particularly limited, but examples thereof include a temperature of more than 100°C and not more than 600°C under air or nitrogen flow, and an annealing time of 10 minutes to 24 hours. The annealing temperature is preferably 300°C to 550°C, and more preferably 350°C to 500°C. The annealing time is preferably 1 hour to 16 hours, and more preferably 2 hours to 8 hours. Although the effect of this annealing is not clear, it is possible to improve the annealing efficiency by selecting the annealing conditions. It is presumed that the interaction with gun oxide is enhanced, making it possible to control the metal valence of iridium in a more desirable range.
[0023] The iridium-manganese oxide composite electrode of the present invention is obtained by electrolyzing a mixed solution containing sulfuric acid and manganese sulfate using a conductive base material composed of a powder sintered body, electrodepositing manganese oxide on at least a part of the conductive base material composed of a powder sintered body, and then immersing or contacting it with an iridium salt solution to uniformly disperse and adsorb iridium at least on the surface of the manganese oxide, and then performing an annealing treatment. In this case, it is preferable that the iridium-manganese oxide composite electrode is prepared so that the coating amount of the iridium-manganese oxide composite material per geometric area of the conductive base material is within the above-mentioned preferred range. In addition, when producing the iridium-manganese oxide composite electrode of the present invention, the manganese oxide obtained by electrolysis of a mixed solution containing sulfuric acid and manganese sulfate is immersed or contacted with an iridium salt solution, and then annealing treatment is performed, and the iridium-manganese oxide composite material is precipitated on the conductive base material, and an iridium-manganese oxide composite material is obtained.
[0024] Regarding the concentration of each component in the mixed solution containing sulfuric acid and manganese sulfate used in the production of the iridium-manganese oxide composite electrode of the present invention, the sulfuric acid concentration is preferably 5 g / L or more and 65 g / L or less, and more preferably 20 g / L or more and 60 g / L or less. The concentration of manganese (manganese ion of manganese sulfate) in the mixed solution is not particularly limited as long as it is below the solubility, but is preferably 5 g / L or more and 50 g / L or less, and more preferably 10 g / L or more and 40 g / L or less.
[0025] In order to maintain the component concentrations of the above mixed solution, it is effective to appropriately add manganese sulfate equivalent to the manganese consumed in the electrolytic oxidation, or to continuously supply a manganese sulfate solution. The sulfuric acid concentration in the above-mentioned sulfuric acid-manganese sulfate mixed solution is a value excluding the divalent anion (sulfate ion) of manganese sulfate.
[0026] In the method for electrolytic deposition of manganese oxide from an iridium-manganese oxide composite electrode of the present invention, the electrolytic current density is not particularly limited, but is preferably 0.3 mA / cm 2 More than 20mA / cm 2 It is preferable that the electrolytic current density is 1 mA / cm or less. This allows efficient and stable electrolytic deposition of manganese oxide. In order to obtain the iridium-manganese oxide composite electrode of the present invention more stably, the electrolytic current density is 1 mA / cm or less. 2 More than 10mA / cm 2 Less than 3mA / cm is more preferable. 2 More than 8mA / cm 2 The following is even more preferred:
[0027] The electrolysis temperature can be, for example, 93° C. or higher and 98° C. or lower. Since the higher the electrolysis temperature, the higher the efficiency of electrolytic production of precipitated manganese oxide, the electrolysis temperature is preferably higher than 94° C. The type of iridium salt in the iridium salt solution is exemplified by potassium hexachloroiridate (K2IrCl6) or hexachloroiridate (H2IrCl6). The iridium concentration of the iridium salt solution is not particularly limited as long as it is equal to or less than the solubility, but is preferably 0.000.1 g / L or more and 10 g / L or less, and more preferably 0.003 g / L or more and 5 g / L or less.
[0028] It is also effective to treat the conductive substrate with hydrochloric acid, sulfuric acid, nitric acid, oxalic acid, or the like before electrolytic deposition of manganese oxide, thereby removing the passive film on the substrate surface and making it hydrophilic. On the other hand, it is also effective to immerse the conductive substrate in a dispersion liquid of a fluorine-based resin or the like to make it water-repellent, for the purpose of controlling the electrodeposition position of manganese oxide in the conductive substrate or imparting gas diffusion properties, which are important when actually using the substrate as an electrode for water electrolysis.
[0029] Electrolytic deposition of manganese oxide for iridium-manganese oxide composites onto conductive substrates As conditions, for example, the sulfuric acid concentration, manganese concentration, electrolysis current density, electrolysis temperature, etc. of the mixed solution of sulfuric acid and manganese sulfate as described above are selected, and electrolysis time is set to a range of 5 to 120 minutes. After electrolytic deposition of manganese oxide on the conductive substrate, the substrate is washed with water and dried, and then the conductive substrate on which manganese oxide has been electrolytically deposited is immersed in a container containing an iridium salt solution, or the conductive substrate on which manganese oxide has been electrolytically deposited is brought into contact with an iridium salt solution, thereby adsorbing iridium onto at least the surface of the manganese oxide, and finally, annealing is performed in an air or nitrogen atmosphere at a temperature of more than 100°C and not more than 600°C for more than 10 minutes and not more than 24 hours, thereby forming the iridium-manganese oxide composite electrode of the present invention.
[0030] The conditions for immersing the manganese oxide electrodeposited on at least a part of the conductive base material composed of a powder sintered body in the iridium salt solution are not particularly limited, but examples include immersion for 30 minutes to 24 hours at a temperature of 20° C. to 100° C. The amount of iridium adsorbed onto the manganese oxide can be controlled by the contact time. The annealing temperature is preferably from 300° C. to 550° C., and more preferably from 350° C. to 500° C. The annealing time is preferably from 1 hour to 16 hours, and more preferably from 2 hours to 8 hours.
[0031] In the iridium-manganese oxide composite electrode of the present invention, if one side of the conductive substrate is shielded with a resin film or the like during electrolytic deposition of manganese oxide, the iridium-manganese oxide composite material can be preferentially coated on only one side, while the other side is hardly covered with the iridium-manganese oxide composite material, so that the iridium-manganese oxide composite material can be intentionally unevenly coated. Furthermore, in the iridium-manganese oxide composite electrode of the present invention, it is presumed that during annealing treatment, the interaction between iridium and manganese oxide is enhanced, making it possible to control the metal valence of iridium within a desirable range, and that other favorable effects are also achieved, such as improving the adhesion between the iridium-manganese oxide composite material and the conductive powder sintered compact, or increasing the crystallinity of the iridium-manganese oxide composite material.
[0032] A membrane electrode assembly (MEA) is formed by stacking the iridium-manganese oxide composite electrode of the present invention, a polymer electrolyte membrane, and an electrode provided with a hydrogen generation catalyst. In the present invention, by having the iridium-manganese oxide composite electrode of the present invention, a water electrolysis device is formed, and hydrogen can be produced by water electrolysis using this iridium-manganese oxide composite electrode. EXAMPLES
[0033] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0034] <SEM observation of the surface of iridium-manganese oxide composite electrode> An elemental analysis of the cross section of the composite electrode was performed using a SEM-instrument (Hoskin Scientific JSF-7800F). When performing elemental analysis of the cross section, tailing was prevented by using conductive carbon tape. <Calculation of the amount of iridium-manganese oxide electrodeposited> The amount of iridium-manganese oxide electrodeposited was calculated according to the following method. From the set electrodeposition time and current density, the quantity of electricity (C) passed through the substrate is calculated using the following formula. (Electrodeposition time (seconds)) × current density (A / cm 2 )...Equation 4 Assuming that the entire amount of current was used for the precipitation of manganese oxide, the amount of current electricity calculated from Equation 4 and the amount of electrons involved in the reaction can be calculated from Equation 5. The amount of manganese oxide electrodeposited was determined. Amount of electricity passing (C) ÷ 96485 ÷ 2 × 86.94 Equation 5
[0035] <Construction of a PEM-type electrolytic cell for evaluating the properties of oxygen evolution electrode catalysts> A PEM-type electrolytic cell using an electrode made of a conductive substrate coated with an iridium-manganese oxide composite material was constructed as follows. The electrode (flat powder sintered body: 2.25 cm × 2.25 cm) was used as the working electrode, and a 20 wt% platinum-supported carbon catalyst (20% Platinum on Vulcan XC-72, Sigma-Aldrich) was used as the catalyst for the counter electrode. A conductive catalyst ink was prepared, applied to carbon paper, and air-dried to prepare a counter electrode. A Nafion membrane (Nafion 115, Sigma-Aldrich) was used as the electrolyte membrane. The electrolyte membrane was washed and protonated (pretreated) by boiling in 3% hydrogen peroxide, pure water, 1M sulfuric acid aqueous solution, and then pure water for 1 hour each. Next, the electrolyte membrane was sandwiched between the catalyst-coated surfaces of the working electrode and counter electrode, and heated at 135°C and a clamping force of 400 kg / cm using a hot press machine (SA-302, Tester Sangyo Co., Ltd.). 2 The MEA was fabricated by hot pressing for 3 minutes at 400 K for 30 minutes. The MEA was attached to the housing of a PEM electrolytic cell (WE-4S-RICW, manufactured by FC Development Co., Ltd.) with carbon paper (TGP-H-060) on the cathode side and platinum-coated titanium powder sintered body (manufactured by Tanaka Kikinzoku Kogyo Co., Ltd.) on the anode side to improve adhesion even during electrolysis operation.
[0036] <Electrochemical measurement 1: Measurement of current-voltage curve> In order to evaluate the water oxidation catalytic activity in an actual device, a PEM electrolytic cell constructed using electrodes made of a conductive substrate coated with an iridium-manganese oxide composite material was used to measure the current-voltage curve at an operating temperature of 80°C. In this measurement, a two-electrode system consisting of only a working electrode and a counter electrode was used, and the current-voltage curve was measured by gradually increasing the applied voltage. Pure water was supplied to the PEM electrolytic cell. The voltage increase rate was set to 10 mV / s so that the voltage at which the current started to rise could be easily identified.
[0037] <Electrochemical measurement 2: Measurement of electrolytic voltage stability> To evaluate the stability of the water oxidation catalytic activity in an actual device, a PEM-type electrolytic cell was constructed using electrodes made of a conductive substrate coated with an iridium-manganese oxide composite material, and electrolysis voltage was measured at an operating temperature of 80°C. In this measurement, a two-electrode system consisting of only a working electrode and a counter electrode was used, and the current density applied between the two electrodes was set to 2 A / cm. 2 The time change in electrolysis voltage was measured while maintaining the temperature at 100°C. Pure water was supplied to the PEM electrolytic cell.
[0038] Example 1 Electrolysis was performed in an electrolytic cell containing a sulfuric acid-manganese sulfate mixed solution with a concentration of 35 g / L of sulfuric acid and 45 g / L of manganese sulfate, and manganese oxide was electrolytically deposited on a conductive substrate of platinum-coated titanium powder sintered body (thickness 0.25 mm, platinum coating thickness 0.3 μm, porosity 50%, manufactured by Tanaka Kikinzoku Kogyo Co., Ltd.). The deposited manganese oxide layer was 5 μm thick, as seen in the cross-sectional SEM image of FIG. 1. The weight of the deposited manganese oxide layer was 0.95 mg. Next, the conductive substrate on which the manganese oxide was electrodeposited was immersed in an iridium salt solution tank containing 1.0 g / L of potassium hexachloroiridate (K2IrCl6) and 1.0 g / L of sulfuric acid at 94°C for 12 hours, allowing iridium to be adsorbed onto the surface of the manganese oxide. The liquid in the iridium salt solution tank before and after the iridium was adsorbed was measured using a UV-Vis spectrometer (Shimadzu UV-2550) to confirm that all the iridium was adsorbed by the manganese oxide and that none remained in the iridium salt solution tank. Next, an annealing treatment was performed in air at 450°C for 5 hours to produce an iridium-manganese oxide composite electrode in which an iridium-manganese oxide composite material was precipitated on the conductive substrate. The synthesis conditions are shown in Table 1.
[0039] [Table 1]
[0040] A SEM photograph of the cross section of this electrode is shown in Figure 1. It can be seen from Figure 1 that the iridium-manganese oxide composite electrode is in a state in which an iridium-manganese oxide composite catalyst is deposited on a platinum-coated titanium powder sintered body. This iridium-manganese oxide composite electrode was cut to a size of 2.25 cm x 2.25 cm, and a PEM-type electrolytic cell was constructed according to the method in <Construction of a PEM-type electrolytic cell for evaluation of oxygen evolution electrode catalytic properties>, and the oxygen evolution electrode catalytic properties were evaluated according to <Electrochemical measurement 1: Measurement of current-voltage curve>. The results are shown in Figure 2. In the measurement results of the current-voltage curve, the higher the current at the same voltage, the higher the oxygen evolution electrode catalytic activity. In addition, the time change in electrolysis voltage was measured according to <Electrochemical Measurement 2: Measurement of current-voltage curve>. The results are shown in Figure 3. The smaller the increase in electrolysis voltage over time (i.e., the lower the rate of voltage increase per unit time), the higher the durability. The evaluation results are shown in Table 2.
[0041] [Table 2]
[0042] Comparative Example 1 An iridium-manganese oxide composite electrode was produced according to the preparation conditions of Example 1, except that a platinum-coated titanium mesh (manufactured by Tanaka Kikinzoku Kogyo Co., Ltd.) was used as the conductive substrate. These synthesis conditions are shown in Table 1. Furthermore, the results of the oxygen evolution electrode catalyst characteristic evaluation are shown in FIG. 2, and the results of the measurement of the time change in electrolysis voltage are shown in FIG. 3. These evaluation results are shown in Table 2.
[0043] As shown in Figures 2 and 3, it has become clear that the iridium-manganese oxide composite electrode of the present invention exhibits extremely good oxygen evolution electrode catalytic activity and durability compared to conventional iridium-manganese oxide composite electrodes in PEM-type electrolytic cells, where a non-noble metal catalyst is desired. [Industrial Applicability]
[0044] The iridium-manganese oxide composite electrode of the present invention has a current density of 2.0 Acm compared to conventional iridium-based catalysts. -2 Because this material exhibits high durability in electrolysis operations under the above-mentioned high current density conditions, its use as an anode catalyst for oxygen evolution in industrial water electrolysis performed under alkaline or neutral conditions, or in water electrolysis using a PEM-type electrolytic cell, makes it possible to obtain hydrogen and oxygen at extremely low production costs. Furthermore, by making carbon dioxide present in a reaction system such as the water electrolysis, the carbon dioxide or the like can be reduced at the cathode to produce hydrocarbon compounds (formic acid, formaldehyde, methanol, methane, ethane, propane, etc.).
Claims
1. An iridium-manganese oxide composite electrode, in which an iridium-manganese oxide composite material covers at least a portion of a conductive substrate made of a sintered powder body.
2. The iridium-manganese oxide composite material is present in an amount of 0.1 mg / cm per geometric area of the conductive substrate. 2 25mg / cm or more 2 2. The iridium-manganese oxide composite electrode according to claim 1, further comprising:
3. 3. The iridium-manganese oxide composite electrode according to claim 1, wherein the conductive substrate is a platinum-coated titanium powder sintered body.
4. A membrane / electrode assembly comprising the iridium-manganese oxide composite electrode according to claim 1 or 2 and a polymer electrolyte membrane.
5. A water electrolysis device comprising the iridium-manganese oxide composite electrode according to claim 1 or 2.
6. A water electrolysis device comprising the membrane / electrode assembly according to claim 4.
7. A method for producing hydrogen, comprising electrolyzing water using the iridium-manganese oxide composite electrode according to claim 1 or 2.
8. A method for producing hydrogen, comprising electrolyzing water using the membrane / electrode assembly according to claim 4.
Citation Information
Patent Citations
JP192993A
Water electrolytic cell and its production
JP1996269761A
Noble metal oxide catalyst for water electrolysis
JP2007514520A
Catalytic materials, electrodes, and systems for water electrolysis and other electrochemical techniques
WO2009154753A2
Manganese oxide for water decomposition catalysts, manganese oxide-carbon mixture, manganese oxide composite electrode material, and respective methods for producing these materials
WO2019117199A1